Joint and power module
Patent Information
- Application Number
- JP2024516525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-25
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Electronic components such as power modules require higher insulation performance at high temperatures due to the use of wide gap semiconductors, which generate thermal stress and increase the risk of dielectric breakdown.
A ceramic sintered body with a ceramic plate, metal plate, and brazing material layer, where the average pore area ratio within 200 μm from the ceramic plate surface is 2.0% or less, and the equivalent circular diameter of pores is 10 μm or less, reducing thermal stress and dielectric breakdown.
The solution provides a joined body with excellent insulation reliability at high temperatures, enhancing the reliability of power modules by suppressing dielectric breakdown and improving thermal stress management.
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a joint and a power module. [Background technology]
[0002] In recent years, power modules for controlling large power are used in industrial equipment such as motors and products such as electric vehicles. In such power modules, a circuit board having a ceramic plate and a circuit pattern is used to efficiently diffuse heat generated from a semiconductor device and suppress leakage current. For example, Patent Document 1 proposes reducing the bonding void ratio in a brazing material layer that bonds a ceramic plate and a circuit pattern to a predetermined value or less.
[0003] It has been proposed to use wide-gap semiconductors in semiconductor devices (for example, Patent Document 2). A semiconductor device using a wide-gap semiconductor has better pressure resistance and heat resistance than a semiconductor device including a Si semiconductor. Such a wide-gap semiconductor has excellent pressure resistance and is capable of high-temperature operation. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2019 / 022133 [Patent Document 2] JP 2018-200918 A Summary of the Invention [Problem to be solved by the invention]
[0005] Electronic components such as power modules are becoming more and more compact and high performance. Accordingly, the reliability of various products used in the electronic components is becoming increasingly higher. For example, a bonded body such as a circuit board on which a semiconductor element using a wide gap semiconductor is mounted is required to have higher insulation performance than ever before at high temperatures.
[0006] In view of this, the present disclosure provides a bonded body having excellent insulation reliability at high temperatures, and also provides a power module having excellent reliability by including such a bonded body. [Means for solving the problem]
[0007] One aspect of the present disclosure provides the following ceramic sintered body.
[0008] [1] A joint comprising a ceramic plate, a metal plate, and a brazing filler layer joining a main surface of the ceramic plate and a main surface of the metal plate, wherein, in a cut surface obtained by cutting the ceramic plate along the thickness direction of the ceramic plate, the average area ratio of pores in a region including directly below the outer edge of the side of the metal plate and extending to a depth of 200 μm from the main surface of the ceramic plate is 2.0% or less.
[0009] When a semiconductor element or the like is mounted on the bonded body, the temperature fluctuates with the heat generation of the semiconductor element. Here, since the ceramic plate and the metal plate have different thermal expansion coefficients, thermal stress occurs in the ceramic plate with the temperature change of the bonded body. This thermal stress is greatest in the ceramic plate near the end of the metal plate. Therefore, when a high voltage is applied to the metal plate of such a bonded body, dielectric breakdown is likely to occur in the ceramic plate near the end of the metal plate with the rise in temperature of the bonded body. In the bonded body of [1] above, the average value of the area ratio of pores in the region including just below the outer edge of the metal plate and extending to a depth of 200 μm from the main surface of the ceramic plate, which corresponds to the portion where large thermal stress occurs, is sufficiently low. Therefore, dielectric breakdown of the bonded body at high temperatures can be sufficiently suppressed. Therefore, the bonded body has excellent insulation reliability at high temperatures.
[0010] The bonded body of the above [1] may be any one of the following [2] to [5].
[0011] [2] The bonded body according to the above-mentioned [1], wherein the maximum value of the equivalent circle diameter of the pores included in the region of the cut surface is 10 μm or less. [3] The joined body according to [1] or [2], wherein the ceramic plate has a thickness of 0.2 mm or more. [4] The joined body according to any one of [1] to [3], wherein the metal plates have a thickness of 0.5 mm or less. [5] The bonded structure according to any one of [1] to [4], which is a circuit board on which a semiconductor element made of a semiconductor material having a band gap exceeding 1.12 eV is mounted.
[0012] In the bonded body of [2], the maximum value of the circle equivalent diameter of the pores in the region of the ceramic plate is 10 μm or less. If there are large pores, insulation breakdown is likely to occur from those pores. By reducing the maximum value of the circle equivalent diameter of the pores, the variation in insulation reliability can be sufficiently reduced. Therefore, the bonded body of [2] has even better insulation reliability at high temperatures. Since the ceramic plate in the bonded body of [3] has a sufficient thickness, the durability of insulation at high temperatures can be improved. In the bonded body of [4], the thickness of the metal plate is 0.5 mm or less, so that the thermal stress generated in the ceramic plate can be reduced. Therefore, the insulation reliability at high temperatures can be further improved. In the bonded body of [5], a power module capable of operating at high frequencies can be obtained by using the bonded body having excellent insulation performance at high temperatures as a circuit board on which a semiconductor element made of a semiconductor material having a band gap exceeding 1.12 eV is mounted.
[0013] One aspect of the present disclosure provides the following power module.
[0014] [6] A power module comprising: the bonded body according to any one of the above [1] to [5]; and a semiconductor element electrically connected to the metal plate of the bonded body.
[0015] The power module includes the semiconductor element and the bonded body having excellent insulation performance at high temperatures, and therefore has excellent reliability.
[0016] The power module of the above [6] may be any one of the following [7] to [9].
[0017] [7] The power module according to [6], wherein the band gap of the semiconductor material constituting the semiconductor element exceeds 1.12 eV. [8] The power module according to [6] or [7], wherein the ceramic plate has a thickness of 0.35 mm or less. [9] The power module according to any one of [6] to [8], wherein the metal plates in the bonded body have a thickness of 0.3 mm or more.
[0018] The power module described in [7] above has a semiconductor element made of a semiconductor material with a large band gap, and therefore can be driven at high frequencies to improve control performance. When such a semiconductor with a large band gap is used, the amount of heat generated by the semiconductor element increases. Therefore, by reducing the thickness of the ceramic plate as described in [8] above, the joint can be made smaller and heat dissipation can be improved. Also, by increasing the thickness of the metal plate as described in [9] above, heat dissipation can be improved, further increasing reliability. Effect of the Invention
[0019] The present disclosure can provide a joined body having excellent insulation reliability at high temperatures, and can also provide a power module having excellent reliability by including such a joined body. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a plan view of the bonded assembly. [Diagram 2] FIG. 2 is a cross-sectional view of the bonded body taken along the thickness direction. [Diagram 3]FIG. 3 is an enlarged cross-sectional view showing a schematic view of a cross section obtained by cutting the ceramic plate along the thickness direction, the cross section including a region just below the outer edge of the side of the metal plate and extending to a depth of 200 μm from the main surface of the ceramic plate. [Figure 4] FIG. 4 is a cross-sectional view of the power module. [Diagram 5] FIG. 5 is a diagram showing an example of the volume-based particle size distribution of the sintering additive powder obtained by the laser diffraction / scattering method. [Figure 6] FIG. 6 is a diagram showing an example of an image of grain growth as sintering progresses in an example of a manufacturing method. [Figure 7] FIG. 7 is a diagram showing a schematic diagram of an example of an inspection device for performing a Vt test. [Figure 8] FIG. 8(A) is a photograph (500x) showing an image of the cut surface of the ceramic plate of Example 1 taken by a scanning electron microscope, and FIG. 8(B) is a diagram showing the image after being binarized. [Figure 9] FIG. 9 is a diagram showing an image of grain growth as sintering progresses in a conventional manufacturing method. [Figure 10] FIG. 10 is a photograph taken by a scanning electron microscope (200x) of a cut surface of a conventional molded body (ceramic green sheet) and of aggregates of sintering additive powder contained in the cut surface. [Figure 11] FIG. 11(A) is a photograph (500x) showing an image of the cut surface of the ceramic plate of Comparative Example 1 taken with a scanning electron microscope, and FIG. 11(B) is a diagram showing the photograph after being binarized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present disclosure will be described with reference to the drawings in some cases. However, the following embodiments are examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. The numerical range indicated by the symbol "~" includes the lower limit and the upper limit. That is, the numerical range indicated by "A~B" means A or more and B or less. The present disclosure also includes a numerical range that combines a numerical range having only an upper limit and a numerical range having only a lower limit. The present disclosure also includes a numerical range in which the upper limit or lower limit of each numerical range is replaced with the numerical value of any of the examples. When multiple materials are exemplified, one of them may be used alone, or multiple materials may be used in combination.
[0022] A joined body according to one embodiment includes a ceramic plate, a metal plate, and a brazing material layer joining a main surface of the ceramic plate and a main surface of the metal plate. The ceramic plate is made of a ceramic sintered body including ceramic particles.
[0023] The ceramic particles constituting the ceramic sintered body may contain at least one selected from the group consisting of silicon nitride particles, aluminum nitride particles, and alumina particles. The ceramic plate may contain pores. Examples of the ceramic plate include a silicon nitride plate containing silicon nitride particles as a main component, an aluminum nitride plate containing aluminum nitride particles as a main component, and an alumina plate containing alumina particles as a main component. The ceramic plate may also be composed of a composite sintered body containing multiple types of ceramic particles.
[0024] In the bonded body of the present embodiment, the average area ratio of pores in a region including just below the outer edge of the side of the metal plate and extending to a depth of 200 μm from the main surface of the ceramic plate in a cut surface obtained by cutting the ceramic plate along the thickness direction of the ceramic plate is 2.0% or less. The average area ratio in the region may be 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, or 1.3% or less. A bonded body including a ceramic plate having such a small average area ratio in the region has sufficiently excellent insulation reliability at high temperatures. The average area ratio in the region may be 0.1% or more, 0.3% or more, 0.5% or more, or 0.8% or more. An example of the average area ratio range in the region is 0.1 to 1.9%.
[0025] The side surface of the metal plate may be inclined so as to widen toward the ceramic plate. In this case, the "outer edge of the side of the metal plate" is the outer edge of the main surface of the metal plate facing the ceramic plate. The brazing material may creep up onto the side surface of the metal plate and be covered with the brazing material. If the side surface of the metal plate is covered with a coating layer containing a brazing material component, the "outer edge of the side of the metal plate" is the outer edge of the coating layer covering the side surface of the metal plate.
[0026] In this specification, the insulation reliability at high temperatures refers to insulation reliability in an environment of, for example, 80 to 100°C. When the bonded body is used as a part of a power module, it will be exposed to such a temperature environment for a long time. In particular, since a power module using a wide-gap semiconductor generates a large amount of heat because it is driven at high frequency, the bonded body (circuit board) built into the power module will be frequently exposed to such high temperatures. In the bonded body of this embodiment, the average value of the area ratio of pores in the region including just below the outer edge of the metal plate and up to a depth of 200 μm from the main surface of the ceramic plate, which corresponds to the portion where thermal stress increases at high temperatures, is sufficiently low. Therefore, the dielectric breakdown of the bonded body of this embodiment at high temperatures can be sufficiently suppressed. Therefore, the bonded body of this embodiment has excellent insulation reliability at high temperatures.
[0027] The junction may be a circuit board on which a semiconductor element made of a semiconductor material having a band gap of more than 1.12 eV, 2.0 eV or more, 2.5 eV or more, or 3.0 eV or more is mounted. The semiconductor element may be a wide-gap semiconductor element. That is, examples of wide-gap semiconductor materials constituting the semiconductor element include silicon carbide, diamond, gallium oxide, and gallium nitride. Also, the semiconductor may be one doped with impurities. In this specification, the wide-gap semiconductor (wide-gap semiconductor material) refers to one having a band gap of 2.2 eV or more.
[0028] The average value of the area ratio in the region is the arithmetic mean value of the area ratio in at least five regions. The at least five regions are different from one another and are selected so that the regions do not overlap. The area of each region is, for example, 0.05 mm 2 The maximum value of the equivalent circle diameter of the pores in at least five regions is 10 μm or less, 9 μm or less, 8 μm or less, or 7 μm or less. By reducing the maximum value of the equivalent circle diameter of the pores in this manner, it is possible to sufficiently reduce the variation in insulation reliability. The area of the pores in the region and the maximum value of the equivalent circle diameter can be determined from an image magnified 500 times by a scanning electron microscope.
[0029] The thickness of the ceramic plate may be 0.2 mm or more, 0.25 mm or more, or 0.3 mm or more. By increasing the thickness of the ceramic plate in this way, the durability of the insulation at high temperatures can be improved. The thickness of the ceramic plate may be 0.35 mm or less, or 0.31 mm or less. This allows the bonded body to be made smaller, and when the bonded body is mounted on a device that generates a large amount of heat, such as a power module having a wide band gap semiconductor element, the heat dissipation can be improved. Therefore, the reliability of devices such as power modules can be further improved. An example of the thickness range of the ceramic plate may be 0.2 to 0.35 mm from the viewpoint of achieving both of the above-mentioned characteristics.
[0030] The thickness of the metal plate may be 0.5 mm or less, 0.45 mm or less, or 0.4 mm or less. By reducing the thickness of the metal plate in this way, the thermal stress generated in the ceramic plate can be reduced. Therefore, the insulation reliability at high temperatures can be further improved. The thickness of the metal plate may be 0.3 mm or more, or 0.35 mm or more. In this way, when the metal plate is mounted on a device that generates a large amount of heat, such as a power module having a wide band gap semiconductor element, the heat dissipation can be improved and the reliability of the device can be further increased. An example of the thickness range of the metal plate may be 0.3 to 0.5 mm from the viewpoint of achieving both the above-mentioned characteristics. The metal plate may be, for example, a copper plate from the viewpoint of increasing thermal conductivity and electrical conductivity.
[0031] FIG. 1 is a plan view showing an example of a bonded body. FIG. 2 is a cross-sectional view obtained by cutting along line II-II in FIG. 1. The bonded body 100 shown in FIG. 1 and FIG. 2 includes a ceramic plate 10, a metal plate 41 bonded to one main surface 10A of the ceramic plate 10 via a brazing material layer 51, and a metal plate 42 bonded to the other main surface 10B of the ceramic plate 10 via the brazing material layer 51. The metal plate 41 is patterned and functions as, for example, a circuit. In this specification, such a metal circuit pattern is also referred to as a metal plate. The metal plate 42 is not patterned and functions as, for example, a heat sink.
[0032] 2 shows a cut surface along the thickness direction of the ceramic plate 10. In the cut surface thus obtained, the average area ratio of pores in the region RE including directly below the outer edge 44 on the side of the metal plate 41 and extending to a depth of 200 μm from the main surface 10A of the ceramic plate 10 is 2.0% or less. Directly below the outer edge 44 on the side of the metal plate 41 is directly below the outer edge of the side (side surface) of the metal plate 41 when the bonded body 100 is viewed in plan as shown in FIG. 1. As shown in FIG. 1, regions RE1, RE2, RE3, RE4, and RE5 are selected directly below at least five outer edge portions 44a, 44b, 44c, 44d, and 44e of the outer edge 44 on the side of the metal plate 41. Each of the regions RE1, RE2, RE3, RE4, and RE5 includes a region immediately below the outer edge 44 (outer edge portions 44a, 44b, 44c, 44d, and 44e) and is a region from the main surface 10A of the ceramic plate 10 to a depth of 200 μm. Note that the region RE5 including the outer edge portion 44e and the region immediately below it is not shown in FIG. Like the regions RE1, RE2, RE3, and RE4, the region RE5 can be defined by a cut surface obtained by cutting the ceramic plate 10 along the thickness direction so as to pass directly below the outer edge 44 of the metal plate 41.
[0033] Although five regions RE are shown in FIG. 1 (four regions in FIG. 2), six or more regions RE may be selected to obtain the average value of the area ratio of the pores in the regions RE. The positions of cutting the ceramic plate 10 in the thickness direction are not limited to the positions shown in FIG. 1 and FIG. 2. For example, five cut surfaces may be obtained, the regions RE may be determined in each cut surface, and the area ratio of the pores in each region RE may be obtained. The average value of the area ratio of the pores in the bonded body 100 may be calculated by arithmetically averaging the area ratio of the pores obtained in each region RE. The thickness ranges of the ceramic plate 10 and the metal plates 41 and 42 are as described above. The thicknesses of the metal plates 41 and 42 may be the same as each other or different from each other.
[0034] FIG. 3 is a diagram showing an example of an image obtained by observing a part of a cut surface 10C of a ceramic plate 10 with a scanning electron microscope (SEM, magnification: 500 times). As shown in FIG. 3, the region RE in the cut surface 10C of the ceramic plate 10 includes ceramic particles and pores 20. The region RE includes a plurality of pores 20. FIG. 3 shows a schematic enlarged view of one pore 20. Thus, the two-dimensional image of the pores 20 includes pores that are not perfect circles. Note that the region RE usually includes a large number of ceramic particles, but in FIG. 3, the ceramic particles are not shown for convenience. The area of each pore 20 can be obtained using commercially available image processing software (e.g., Image J). The area of each pore 20 may be obtained by binarizing the SEM image.
[0035] The total area of the pores 20 is calculated from the area of each pore 20 included in the region RE shown in FIG. 3. The total area is divided by the area of the region RE to calculate the area ratio of the pores 20 in each region RE. The area of the region RE is, for example, 0.05 mm 2 Using the area ratio of the pores 20 in each region RE, the average value of the area ratio of the pores 20 can be calculated as described above. The average value of the area ratio of the pores 20 is 2.0% or less as described above. Other examples of the numerical range are as described above.
[0036] In the bonded body 100 including such ceramic plates 10, large thermal stress occurs in the region RE with temperature changes. In the region RE, the area ratio of the pores 20 is low, so that the occurrence and progression of cracks can be sufficiently suppressed. Therefore, the bonded body 100 has excellent insulation reliability at high temperatures.
[0037] The circle-equivalent diameter of the pores 20 included in the region RE in Fig. 3 can be obtained using commercially available image processing software (e.g., Image J). When five regions RE1, RE2, RE3, RE4, and RE5 are selected as the region RE, the maximum value of the circle-equivalent diameter of the pores 20 in the five regions is obtained. In other words, the maximum value is obtained from among the five maximum values. The maximum value of the circle-equivalent diameter obtained in this manner is within the above-mentioned range.
[0038] In this example, only a plurality of regions from the main surface 10A to a depth of 200 μm are selected, but in another example, the area ratio of pores may be obtained in a region RE from the main surface of the ceramic plate to a depth of 200 μm, including directly below the outer edge of the side portion of the metal plate 42 in the main surface 10B. For example, three regions RE from the main surface 10A to a depth of 200 μm and two regions RE from the main surface 10B to a depth of 200 μm may be selected.
[0039] The region RE may contain a sintering aid phase in addition to the pores 20 and ceramic particles. The average value of the area ratio of the ceramic particles (ceramic phase) in the region RE may be 70 to 90%, or 75 to 85%. The average value of the area ratio of the sintering aid phase in the region RE may be 10 to 25%, or 14 to 22%. The ceramic plate 10 having the region RE (cut surface 10C) containing the ceramic particles and the sintering aid phase at such an average area ratio has a sufficiently high thermal conductivity. The average value of the area ratio of the ceramic particles and the sintering aid phase is calculated as the arithmetic average value of the area ratios measured in at least five regions RE, similar to the average value of the area ratio of the pores 20.
[0040] 1, 2 and 3 are an example of the bonded body. The shapes of the ceramic plate 10 and the metal plates 41 and 42 are not limited to those shown in FIG. 1 and FIG. 2. In a modified example of the bonded body 100, the metal plate 42 may also have a circuit pattern. In another modified example, both the metal plate 41 and the metal plate 42 may not be patterned. For example, when a circuit pattern is formed by etching a metal plate, both before and after the circuit pattern is formed correspond to the bonded body. In yet another modified example, there may be a plurality of metal plates (circuit patterns) bonded to one main surface of the ceramic plate. A metal plate may be bonded to only one main surface of the ceramic plate.
[0041] The brazing material layers 51, 52 are layers for joining the ceramic plate 10 and the metal plate 41, 42, and contain brazing material components. The brazing material layers 51, 52 may contain, for example, silver derived from the brazing material, or silver and copper. The brazing material layers 51, 52 may further contain one or more metals selected from the group consisting of tin and active metals derived from the brazing material. In the brazing material layers 51, 52, the two or more metals may be alloyed. The active metal may contain one or more metals selected from the group consisting of titanium, hafnium, zirconium, and niobium. The silver and copper contained in the brazing material layers 51, 52 may be contained as an alloy, such as an Ag-Cu eutectic alloy.
[0042] The silver content in the brazing material layers 51, 52 may be 45 to 95 mass % or 50 to 95 mass % in terms of Ag. The total silver and copper content in the brazing material layers 51, 52 may be 65 to 100 mass %, 70 to 99 mass %, or 90 to 98 mass % in terms of Ag and Cu, respectively. The thickness and composition of the brazing material layers 51, 52 may be the same as or different from each other.
[0043] A power module according to an embodiment includes a bonded body (circuit board) and a semiconductor element electrically connected to the metal plate of the bonded body. The bonded body may be the bonded body 100 described above or a modified version thereof. The description of the bonded body and the modified versions applies to the power module of this embodiment. Such a power module includes a bonded body (circuit board) that has excellent insulation reliability at high temperatures. Therefore, even when used in a high-temperature environment, high performance can be maintained. Thus, the power module has excellent reliability.
[0044] FIG. 4 is a cross-sectional view showing an example of a power module. The description of this example is not limited to this example, and is also applied to modified examples of the power module. The power module 200 of FIG. 4 includes a base plate 90 and a joint body 100 joined to one side of the base plate 90 via solder 82. A metal plate 42 (heat sink) on one side of the joint body 100 is joined to the base plate 90 via the solder 82.
[0045] A semiconductor element 80 is attached to a metal plate 41 (circuit pattern) on the other surface side of the bonded body 100 via solder 81. The semiconductor element 80 is connected to a predetermined location of the metal plate 41 by a metal wire 84 such as an aluminum wire. In this manner, the semiconductor element 80 and the metal plate 41 are electrically connected. To electrically connect the outside of the housing 86 to the metal plate 41, a metal plate 41a, which is one of the metal plates 41, is connected to an electrode 83 provided penetrating the housing 86 via solder 85.
[0046] A housing 86 is disposed on one of the main surfaces of the base plate 90, and is integrated with the main surface to accommodate the bonded body 100. A space formed by the one of the main surfaces of the base plate 90 and the housing 86 is filled with a resin 95. The resin 95 seals the bonded body 100 and the semiconductor element 80. The resin may be, for example, a thermosetting resin or a photocurable resin.
[0047] A cooling fin 92 serving as a heat dissipation member is joined to the other main surface of the base plate 90 via grease 94. Screws 93 are attached to the ends of the base plate 90 to fix the cooling fin 92 to the base plate 90. The base plate 90 and the cooling fin 92 may be made of aluminum. The base plate 90 and the cooling fin 92 function well as a heat dissipation section due to their high thermal conductivity.
[0048] The metal plate 41 and the metal plate 42 are electrically insulated by the ceramic plate 10. The metal plate 41 (41a) may form an electric circuit. The metal plate 41 and the metal plate 42 are respectively joined to the main surface 10A and the main surface 10B of the ceramic plate 10 by a brazing material layer (not shown) containing a brazing material component. The power module 200 has excellent reliability because it includes the joined body 100.
[0049] The semiconductor element 80 in the power module 200 may be made of a semiconductor material having a band gap of more than 1.12 eV, 2.0 eV or more, 2.5 eV or more, or more than 3.0 eV. The semiconductor element may be made of a wide-gap semiconductor material. Examples of wide-gap semiconductor materials include silicon carbide, diamond, and gallium nitride. The junction 100 and its variations have excellent insulation reliability at high temperatures, so that the power module 200 including the wide-gap semiconductor element can operate at a high power level. The band gap of the semiconductor material constituting the semiconductor element 80 may be 6.0 eV or less, 5.5 eV or less, or 5.0 eV or less. An example of the range of the band gap of the semiconductor material is more than 1.12 eV and 6.0 eV or less.
[0050] An example of a manufacturing method of the ceramic plate 10 provided in the bonded body 100 will be described below. This manufacturing method includes a crushing step of crushing a sintering aid raw material with a crusher to obtain a sintering aid powder having a D50 (median diameter) of 0.5 to 1.1 μm, a mixing step of preparing a mixed raw material containing ceramic powder and sintering aid powder, and a firing step of firing a compact of the mixed raw material.
[0051] The sintering aid powder may contain at least one selected from the group consisting of alkaline earth metal oxides, rare earth oxides, transition metal oxides different from the rare earth oxides, silica, and alumina, and may contain two or more, or three or more.
[0052] The alkaline earth metal oxide has an alkaline earth metal and oxygen as constituent elements. The alkaline earth metal oxide may include at least one selected from the group consisting of magnesium oxide, calcium oxide, and strontium oxide. The rare earth oxide has a rare earth element and oxygen as constituent elements. The rare earth oxide may include at least one selected from the group consisting of yttrium oxide and cerium oxide, for example. The transition metal oxide different from the rare earth oxide has a transition metal different from the rare earth and oxygen as constituent elements. Such a transition metal oxide may include, for example, iron oxide.
[0053] An example of the sintering aid powder contains magnesium oxide, rare earth oxide, and silica. In this case, when the entire sintering aid powder is taken as 100 parts by mass, the content of the rare earth oxide may be 30 to 80 parts by mass, or may be 40 to 70 parts by mass. In this case, the content of the magnesium oxide may be 5 to 40 parts by mass, or may be 10 to 30 parts by mass. In this case, the content of the silica may be 5 to 40 parts by mass, or may be 10 to 30 parts by mass.
[0054] The D50 (median diameter) of the sintering aid powder in the pulverizing step may be adjusted, for example, by pulverizing the sintering aid raw material with a pulverizer. As the pulverizer, a bead mill type pulverizer may be used. The particle size distribution of the sintering aid powder may be adjusted by changing at least one condition selected from the group consisting of the diameter of the beads of the bead mill type pulverizer, the peripheral speed, and the pulverizing time. The diameter of the beads may be 0.1 to 0.3 mm. The peripheral speed of the rotor may be 8 to 12 m / sec. The pulverizing time may be 5 to 20 minutes. Examples of pulverizers other than the bead mill type pulverizer include a ball mill, a vibration mill, and a pot mill.
[0055] When the D50 of the sintering aid powder exceeds 1.1 μm, the number and size of the pores 20 increase, and the average area ratio of the pores 20 in the region RE tends to increase. Also, when the D50 of the sintering aid powder is less than 0.5 μm, the crushed particles tend to aggregate due to the relationship between the input energy applied to the sintering aid raw material from the crusher and the crushing ratio. This is thought to be due to the fact that the frequency of contact between the crushed particles increases as the crushing progresses, and that the potential energy becomes attractive. In this case, too, the average area ratio of the pores 20 in the region RE tends to increase.
[0056] The D50 of the sintering aid powder is determined based on the volume-based particle size distribution measured by a particle size distribution measuring device using a laser diffraction / scattering method. By having the D50 of the sintering aid powder within the above range, the particles contained in the sintering aid powder are sufficiently small, and the particles can be prevented from agglomerating together. This makes it possible to prevent the generation of pores due to the particles and agglomerates of the sintering aid powder when producing a ceramic plate (ceramic sintered body). Therefore, the average value of the area ratio of the pores 20 in the region RE can be reduced, and the maximum value of the circle-equivalent diameter of the pores 20 contained in the region RE can be reduced. In addition, the grain growth of the ceramic particles can be promoted with high uniformity.
[0057] FIG. 5 is a diagram showing an example of a volume-based particle size distribution of a sintering aid powder by a laser diffraction / scattering method. The horizontal axis is the particle size [μm] in logarithmic scale, and the vertical axis is the frequency [volume %]. The particle size distribution in this disclosure is measured in accordance with the method described in JIS Z 8825:2013 "Particle size analysis - Laser diffraction / scattering method". For particle size distribution measurement, LS-13 320 (product name) manufactured by Beckman Coulter, Inc. is used. The measurement conditions are a particle refractive index of 2.2 and a solvent refractive index of 1.33.
[0058] The sintering aid powder may have only one peak in the particle size distribution (frequency %) as shown in FIG. 5. Since such a sintering aid powder is sufficiently inhibited from agglomerating, the size and number of pores in the ceramic sintered body can be sufficiently reduced. The peak in the particle size distribution may be sharp. For example, the D100 of the sintering aid powder may be 5.5 μm or less, or less than 5.0 μm. For example, the ratio of D100 to D50 may be 5 or less. An example of the lower limit of D100 is 2 μm. An example of the lower limit of the ratio of D100 to D50 is 2.
[0059] In the mixing step, the sintering aid powder obtained by pulverization, the ceramic powder, and additives, if necessary, are blended and mixed using, for example, a ball mill. In this way, a mixed raw material containing the sintering aid powder and the ceramic powder is prepared. Examples of additives include binders, plasticizers, dispersion media, and release agents. Examples of binders include methylcellulose-based binders having plasticity or surface activity, and acrylic ester-based binders having excellent thermal decomposition properties. Examples of plasticizers include glycerin. Examples of dispersion media include ion-exchanged water and ethanol.
[0060] As the ceramic powder, for example, silicon nitride powder, aluminum nitride powder, or aluminum oxide powder can be used. The D50 (median diameter) of the ceramic powder may be 0.1 to 6 μm, or may be 0.5 to 4 μm. This allows a sufficiently densified ceramic sintered body to be obtained. The D50 of the ceramic powder is determined in the same manner as the D50 of the sintering aid powder. The number of peaks in the particle size distribution (frequency %) of the ceramic powder may also be one.
[0061] The mass ratio of the sintering aid powder to the ceramic powder may be 0.03 to 0.12, or may be 0.05 to 0.1, which makes it easier to densify the ceramic sintered body and allows the bending strength to be sufficiently high.
[0062] The mixed raw material obtained in the mixing step is applied to a release film in a predetermined thickness by a doctor blade method, a calendar method, an extrusion method, or the like, dried, and molded to obtain a molded body. The molding pressure may be 3 to 30 MPa. The molded body may be produced by uniaxial pressing or by CIP. It may also be fired while being molded by hot pressing. For example, after producing a ceramic green sheet substrate by the above-mentioned method such as the doctor blade method, the ceramic green sheet substrate may be punched out using a mold equipped with a die and a punch to obtain a molded body.
[0063] The solid content of the ceramic green sheet substrate when punched with a die may be 65 to 85 mass %, or may be 75 to 85 mass %. The solid content may be adjusted by carrying out a drying process of drying the ceramic green sheet substrate before punching with a die.
[0064] Before firing the molded body in the firing step, the molded body may be degreased. The degreasing method is not particularly limited, and may be, for example, performed by heating the molded body in air or a non-oxidizing atmosphere such as nitrogen to 300 to 700° C. The heating time may be, for example, 1 to 10 hours.
[0065] A ceramic plate (plate-shaped ceramic sintered body) can be obtained by firing the molded body. The atmosphere, temperature, time, etc. during firing can be appropriately set depending on the type of ceramic sintered body. When a silicon nitride plate is produced as the ceramic plate, it may be performed in an inert gas atmosphere such as nitrogen gas or argon gas. The pressure during firing may be 0.7 to 1 MPa. The firing temperature may be 1800 to 2100°C, 1800 to 2000°C, or 1800 to 1900°C. The firing time at the firing temperature may be 3 to 20 hours, or 4 to 16 hours.
[0066] When an aluminum nitride plate is produced as the ceramic plate, the sintering temperature may be, for example, 1760 to 1840°C. The holding time in the temperature range of 1760 to 1840°C may be, for example, 1 to 10 hours. The sintering may be carried out under atmospheric pressure. When producing a ceramic plate other than a silicon nitride plate or an aluminum nitride plate (for example, an aluminum oxide plate), the sintering conditions may be appropriately set so that the densification of the sintered body proceeds sufficiently.
[0067] FIG. 6 is a diagram showing an image of grain growth as sintering progresses in the manufacturing method of this example. In this example, as shown in FIG. 6(a), fine sintering aid powder 32 is dispersed in ceramic particles 12 with high uniformity in the molded body. When such a molded body is fired, the liquefied sintering aid phase 32a diffuses to the grain boundaries by capillary action as shown in FIG. 6(b). When the sintering aid phase 32a diffuses, the shrinkage of the molded body (ceramic sintered body) progresses, and the pores 22 disappear as shown in FIG. 6(c). When heating is continued, the ceramic particles 12 melt into the sintering aid phase 32a, and columnar ceramic particles 14 are generated as shown in FIG. 6(d). In this way, as liquid phase sintering progresses, the pores 22 disappear sufficiently with the smooth grain growth of the ceramic particles, so that the pores 20 contained in the ceramic plate 10 can be sufficiently reduced. A part of the sintering aid phase 32a may remain in the ceramic plate.
[0068] FIG. 9 is a diagram showing an image of grain growth as sintering progresses in the conventional manufacturing method. In the conventional manufacturing method, as shown in FIG. 9(a), in the molded body, aggregates 132 of sintering aid powder are contained in ceramic particles 112. A cross-sectional photograph of such a conventional molded body is shown in FIG. 10. When such a molded body is fired, as shown in FIG. 9(b), the liquefied sintering aid phase 132a diffuses from the aggregates 132 to the grain boundaries by capillary action. As diffusion by capillary action progresses, pores 122 are generated in the aggregates 132 because the aggregates 132 are large in size. Since the pores 122 have a large size, they do not disappear even when the molded body shrinks, and the pores 122 remain in the ceramic plate as shown in FIG. 9(c). In this way, the number of large pores contained in the ceramic plate increases.
[0069] In the method for manufacturing the ceramic plate 10 of this embodiment, the particles of the sintering aid powder are sufficiently fine, and the aggregation of the particles is suppressed, compared to the conventional manufacturing method. Therefore, the pores remaining as traces of the sintering aid powder can be reduced. This reduces the number of pores generated during the sintering process and reduces the size of the pores. The average area ratio of the pores 20 in the region RE of the ceramic plate 10 obtained in this manner is sufficiently small. In addition, the maximum value of the circle-equivalent diameter of the pores 20 in the region RE is also sufficiently small. Such a ceramic plate can sufficiently suppress the occurrence and progression of cracks when thermal stress occurs due to temperature change. Therefore, it has excellent insulation reliability at high temperatures.
[0070] 7 is a diagram showing a schematic diagram of an example of an inspection device for performing a Vt test on a bonded body (circuit board). The inspection device 400 includes an AC power source 60 and a voltage resistance tester 50 connected to the AC power source 60. One terminal of the voltage resistance tester 50 is electrically connected to a conductive support part 72a that contacts a metal plate 41 bonded to a ceramic plate 10. The other terminal of the voltage resistance tester 50 is electrically connected to a conductive support part 72b that contacts a metal plate 42 via an electrode 70 arranged in a storage tank 77 that stores insulating oil 76.
[0071] The electrode 70 is disposed along the bottom surface and one side surface of the storage tank 77. As shown in Fig. 7, the electrode 70 has an L-shape when viewed in vertical cross section. The electrode 70 has two insulating supports 74 disposed adjacent to the conductive support 72b. The two insulating supports 74 are in contact with the metal plate 42, respectively, and support the assembly 100 in the insulating oil 76.
[0072] The electrode 70 and the conductive supporting parts 72a, 72b may be made of, for example, oxygen-free copper. The insulating oil 76 may be, for example, a fluorine-based inert liquid. The withstand voltage tester 50 may be a commercially available one. In such an inspection device 400, a voltage of, for example, about 10 to 15 kV is applied between the metal plates 41, 42 sandwiching the ceramic plate 10, and the withstand voltage tester 50 measures the presence or absence of leakage current. By heating the insulating oil 76, the insulating performance of the ceramic plate 10 in the joined body 100 at a high temperature of, for example, 100° C. or higher can be evaluated.
[0073] The inspection device is not limited to the configuration of FIG. 7, and any inspection device that can perform a Vt test when a voltage is applied between metal plates 41 and 42 at a temperature of, for example, 100° C. or higher can be used without any particular restrictions.
[0074] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments. The contents of the description of the embodiments of the ceramic sintered body are also applicable to the joined body, the power module, and the manufacturing method of the ceramic sintered body. The contents of the description of the embodiments of the manufacturing method of the ceramic sintered body are also applicable to the ceramic sintered body.
[0075] Any combination of the upper and lower limit values of the numerical ranges specifically described in each of the above embodiments is also included in the present disclosure. In addition, the upper and / or lower limit values of the numerical ranges are also included in the present disclosure in which the values of the examples described below are substituted. EXAMPLES
[0076] The present disclosure will be described in more detail with reference to examples, reference examples and comparative examples, but the present disclosure is not limited to the specific examples below.
[0077] (Preparation of sintering aid powder) As raw materials for the sintering aid powder, commercially available yttrium oxide powder, magnesium oxide powder, and silica powder were prepared. 2 O 3 :MgO:SiO 2 The mixture was mixed to a mass ratio of 5:2:2 to obtain a mixed powder. The mixed powder was pulverized using a bead mill pulverizer (manufactured by Ashizawa Finetech Co., Ltd., device name: Star Mill LMZ) to obtain a sintering aid powder. The pulverization conditions (bead diameter, rotor circumferential speed, and pulverization time) using the bead mill pulverizer were changed as shown in Tables 1 and 2 to prepare eight types of sintering aid powders with different pulverization conditions.
[0078] The volumetric particle size distribution of each sintering aid powder was measured using a particle size distribution measuring device (manufactured by Nikkiso Co., Ltd., device name: particle size distribution measuring device MT3000II) using the laser diffraction / scattering method. From the results of these particle size distribution measurements, D50 (median size) and D100 (maximum particle size) were calculated. The results are shown in Tables 1 and 2. Tables 1 and 2 also show the ratio of D100 to D50. The particle size distributions (frequency %) of numbers 5 to 8 all had only one peak. In other words, these particle size distributions had the shape shown in FIG. 5.
[0079] [Table 1]
[0080] [Table 2]
[0081] From the results of Nos. 1 to 3 in Table 1, it was confirmed that the D50 and D100 of the sintering aid can be reduced by reducing the diameter of the beads. Also, from the results of Nos. 3, 4, and 5 in Tables 1 and 2, it was confirmed that the D50 and / or D100 can be reduced by increasing the circumferential speed of the rotor. From the results of Nos. 5 and 6, it was confirmed that the D50 and D100 can be reduced by increasing the grinding time. On the other hand, from the results of Nos. 6, 7, and 8, it was confirmed that the D50 and D100 increase when the grinding time is too long. This is thought to be due to the aggregation of the ground powder.
[0082] Example 1 [Preparation of silicon nitride plate] Commercially available silicon nitride powder (D50: 0.7 μm), sintering aid powder number 6 in Table 2, and additives (solvent-based binder) were mixed in a bead mill to prepare raw material slurry. The compounding ratio of silicon nitride powder and sintering aid powder was silicon nitride powder: sintering aid powder = 91:9. Next, the above-mentioned raw material slurry was applied to a release film by a doctor blade method to prepare a green sheet. The prepared ceramic green sheet was cut to a length x width = 250 mm x 180 mm, and 70 sheets were stacked to obtain a laminate. The above laminate was placed in an electric furnace equipped with a carbon heater and heated in air at 500 ° C for 20 hours to degrease.
[0083] The degreased molded body was placed in a sintering furnace, the pressure in the furnace was reduced to 100 Pa or less, and the temperature was raised to 900°C. Nitrogen gas was then introduced into the sintering furnace, and the temperature was raised to 1500°C under a pressure of about 0.9 MPa and held for 4 hours. After that, the temperature was raised to 1830°C and held at 1830°C for 5 hours. In this way, a silicon nitride plate with a thickness of 3 mm was obtained.
[0084] [Preparation of junction] Ag powder (manufactured by Fukuda Metal Foil & Powder Industry Co., Ltd., product name: Ag-HWQ, average particle size D50: 2.5 μm, specific surface area 0.4 m 2 / g) 89.5 parts by mass, Cu powder (manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name: Cu-HWQ, average particle size D50: 3.0 μm, specific surface area: 0.4 m2 / g,) 9.5 parts by mass, Sn powder (Fukuda Metal Foil Powder Co., Ltd.: Sn-HPN, average particle diameter D50: 3 μm, specific surface area 0.1 m 2 A brazing filler metal was prepared containing 3.5 parts by mass of titanium hydride powder (manufactured by Toho Tech Co., Ltd., product name: TCH-100) for a total of 100 parts by mass of 1.0 part by mass of SiO2 / g. 2 The mixture was applied to both main surfaces of a silicon nitride plate by screen printing so as to give the following composition.
[0085] A copper plate for forming a circuit was placed on the brazing material layer on one of the main surfaces of the silicon nitride plate, and a copper plate for forming a heat sink (both 0.3 mm thick, oxygen-free copper plate of C1020 with a purity of 99.60% by mass) was placed on the brazing material layer on the other main surface to obtain a laminate. -3 A bonded assembly was obtained by heating the bonded copper plates for forming a circuit at 830°C for 30 minutes in a vacuum of 100 Pa or less. An etching resist was printed on the bonded copper plates for forming a circuit, and the copper plates for forming a circuit were etched with a ferric chloride solution to form a circuit pattern as shown in Figure 1. Furthermore, the brazing material layer protruding beyond the side surface of the metal plate was removed with an ammonium fluoride / hydrogen peroxide solution. In this way, a circuit board was produced. Multiple circuit boards were produced for use in the following cross-section observation and Vt test.
[0086] [Cutting surface observation] The silicon nitride plate was cut along the thickness direction of the silicon nitride plate to obtain a cut surface. Cutting was performed at multiple locations to select five regions extending from the main surface of the silicon nitride plate to a depth of 200 μm, including immediately below the outer edge on the side of the circuit pattern. The identified regions RE were observed under a scanning electron microscope (SEM) at a magnification of 500 times. The five regions RE (area of each: 0.05 mm 2 The total area of pores and the maximum equivalent circle diameter of pores in each region were determined. Each region included the area just below the outer edge of the side of the circuit pattern. The size and number of pores were measured using image processing software (ImageJ). The total area of pores was calculated by multiplying the area of the field of view (0.05 mm2). 2) to determine the pore area ratio. The maximum pore circle equivalent diameter and pore area ratio were determined for each of the five regions RE. The arithmetic mean value of the pore area ratio and the maximum pore circle equivalent diameter (maximum value in the five regions RE) are shown in Table 3.
[0087] [Insulation test] Using an inspection device as shown in Fig. 7, a Vt test of the circuit board was performed in accordance with JIS C2110-1:2010. For this inspection, an AC20kV withstand voltage tester (model: 7473) manufactured by Keisoku Gijutsu Kenkyusho Co., Ltd. was used. Silicon oil was used as the insulating oil. An inspection tool manufactured by Onishi Electronics Co., Ltd. was used as the reservoir 77, the electrode 70, the conductive supports 72a and 72b, and the insulating support 74. The electrode 70 was made of oxygen-free copper, and the conductive supports 72a and 72b were made of carbon tool steel (SK material) plated with rhodium.
[0088] The insulating oil of the inspection device was heated to 100° C., the circuit board 100 was fixed in the insulating oil, and a voltage of 10 kV was applied between the circuit pattern 41 and the copper plate 42 to measure the time until dielectric breakdown occurred (maximum: 746 hours). The results are shown in Table 3.
[0089] Example 2 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 5 in Table 2 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0090] Example 3 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 7 in Table 2 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0091] Example 4 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 8 in Table 2 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0092] Comparative Example 1 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 3 in Table 1 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0093] Comparative Example 2 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 1 in Table 1 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0094] Comparative Example 3 A silicon nitride plate and a bonded body were produced and each evaluation was carried out in the same manner as in Example 1, except that the sintering aid powder No. 2 in Table 1 was used instead of the sintering aid powder No. 6 in Table 2. The results are shown in Table 3.
[0095] [Table 3]
[0096] As shown in Table 3, it was confirmed that the area ratio of pores is reduced by using a sintering aid powder with a small D50. In Example 1, which used sintering aid powder No. 6 with the smallest D50 and D100 / D50, the area ratio of pores was the smallest. This Example 1 had the best insulation reliability without any dielectric breakdown. FIG. 8(A) is a photograph showing an SEM image (500x) of one of the above regions selected from the cut surface of the silicon nitride plate of Example 1, and FIG. 8(B) is a diagram showing the SEM image after binarization. FIG. 11(A) is a photograph showing an SEM image (500x) of one of the above regions selected from the cut surface of the silicon nitride plate of Comparative Example 1, and FIG. 11(B) is a diagram showing the SEM image after binarization. Comparing FIG. 8 and FIG. 11, the number of pores was obviously smaller in Example 1 than in Comparative Example 1, and the size of the pores was also smaller.
[0097] From the results shown in Table 3, the average pore area ratio and the maximum pore circle equivalent diameter in the above-mentioned region of the silicon nitride plate were smaller in Examples 1 to 4 than in Comparative Examples 1 to 3. In the Vt test of the circuit board of Example 1, no dielectric breakdown occurred until the end of the test (746 hours). Moreover, it was confirmed that Examples 2 to 4 also took longer to break down than Comparative Examples 1 to 3, and thus had excellent insulation reliability. [Industrial Applicability]
[0098] According to the present disclosure, there is provided a joined body having excellent insulation reliability at high temperatures, and a power module having excellent reliability by including the joined body. [Explanation of symbols]
[0099] 10...ceramic plate, 10A, 10B...main surface, 10C...cut surface, 12, 14...ceramic particles, 20, 22, 122...pores, 32...sintering aid powder, 32a, 132a...sintering aid phase, 41...metal plate (circuit pattern), 42...metal plate (copper plate), 44...outer edge, 44a, 44b, 44c, 44d, 44e...outer edge portion, 50...voltage tester, 51, 52...brazing material layer, 60...AC power source, 70, 83...electrodes, 72a ,72b...conductive support part, 74...insulating support part, 76...insulating oil, 77...reservoir, 80...semiconductor element, 81,82,85...solder, 84...metal wire, 86...housing, 90...base plate, 92...cooling fin, 93...screw, 94...grease, 95...resin, 100...joint (circuit board), 132...aggregate, 200...power module, 400...inspection equipment, RE,RE1,RE2,RE3,RE4,RE5...area.
Claims
1. A method for manufacturing a bonding material for a bonding substrate, comprising: a silicon nitride plate; a metal plate; and a brazing material layer that bonds a main surface of the silicon nitride plate to a main surface of the metal plate; In a cut surface obtained by cutting the silicon nitride plate along the thickness direction of the silicon nitride plate, the average area ratio of pores in a region including directly below the outer edge of the side of the metal plate and extending to a depth of 200 μm from the main surface of the silicon nitride plate is 1.9% or less; A bonded body, wherein the maximum equivalent circle diameter of the pores included in the region of the cut surface is 10 μm or less.
2. 2. The bonded structure according to claim 1, wherein the silicon nitride plate has a thickness of 0.2 mm or more.
3. The joined body according to claim 1 , wherein the metal plate has a thickness of 0.5 mm or less.
4. The bonded structure according to claim 1 , which is a circuit board on which a semiconductor element made of a semiconductor material having a band gap exceeding 1.12 eV is mounted.
5. A power module comprising: the bonded body according to any one of claims 1 to 4; and a semiconductor element electrically connected to the metal plate of the bonded body.
6. 6. The power module according to claim 5, wherein the band gap of the semiconductor material constituting the semiconductor element is greater than 1.12 eV.
7. 6. The power module according to claim 5, wherein the silicon nitride plate has a thickness of 0.35 mm or less.
8. 6. The power module according to claim 5, wherein the metal plates in the joined body have a thickness of 0.3 mm or more.