Electrode binders, electrode composites, electrodes, and batteries

A modified vinylidene fluoride copolymer with controlled molecular weight and adsorption rate addresses the viscosity and adhesion issues in electrode binders, enhancing the adhesion and handling of active materials in electrodes.

KR1020260161602APending Publication Date: 2026-11-09KUREHA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267033255
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-29
Filing Date
2025-03-26
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

Existing electrode binders face issues with high viscosity and poor handling ability when used with active materials that have undergone carbon coating treatment or micronization, leading to reduced adhesion to current collectors.

Method used

A vinylidene fluoride copolymer modified with 1-bromomethylpyrene, with specified weight average molecular weight and adsorption rate, is used to form an electrode binder that maintains adhesion while preventing slurry thickening.

Benefits of technology

The electrode binder exhibits excellent adhesion to current collectors and prevents excessive thickening of the electrode composite, improving handling and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00001
    Figure PCT00001
  • Figure PCT00002
    Figure PCT00002
  • Figure PCT00003
    Figure PCT00003
Patent Text Reader

Abstract

The present invention aims to provide an electrode binder comprising a vinylidene fluoride copolymer that has excellent adhesion to a current collector and is difficult to thicken even when lithium iron phosphate is used as the electrode active material. The electrode binder solving the above problem contains a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group. When the vinylidene fluoride copolymer is modified with a labeling material consisting of 1-bromomethylpyrene and the weight-average molecular weight of the carboxyl-containing vinylidene fluoride copolymer that absorbs light of a wavelength of 345 nm is determined, the weight-average molecular weight is 1.3 million or less. The adsorption rate obtained by a predetermined method is greater than 0% and less than or equal to 30%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrode binder, an electrode composite, an electrode, and a battery. Background Technology

[0002] Vinylidene fluoride polymers are mainly used as binders in electrodes of non-aqueous electrolyte secondary batteries. High adhesion is required for binders because they play a role in adhering active materials to current collectors. For example, Patent Document 1 describes introducing functional groups such as carboxyl groups into a fluorine-based resin to improve adhesion to current collectors or improve solubility in solvents. Patent Document 2 describes a binder composition comprising vinylidene fluoride and a copolymer of a compound of a specific structure (vinylidene fluoride copolymer), and describes that the vinylidene fluoride copolymer exhibits high adhesion to current collectors.

[0003] Meanwhile, electrodes using active materials that have undergone carbon coating treatment or micronization are being considered for the purpose of improving battery characteristics, such as improving rate characteristics or reducing internal resistance. Prior art literature

[0004] Patent Document 1: Japanese Published Patent Application No. (Hei) 6-172452 Patent Document 2: Japanese Patent Application No. 5797206 The problem to be solved

[0005] In order to increase adhesion to the current collector, etc., it is conceivable to use the vinylidene fluoride copolymer described in Patent Document 1 or Patent Document 2 as an electrode binder in active materials that have undergone carbon coating treatment or micronization as described above. However, as the inventors have carefully investigated, when an active material having a plurality of surface functional groups through carbon coating treatment is mixed with a vinylidene fluoride copolymer having carboxyl groups, the carboxyl groups of the vinylidene fluoride copolymer interact with the functional groups on the surface of the active material to form a robust network. Furthermore, when using an active material with a small particle diameter, the viscosity of the slurry tends to increase. That is, there was a problem in that the viscosity of the slurry tends to become very high as they stack up, and its handling ability is low.

[0006] The present invention has been made in consideration of the above-mentioned problem. The present invention aims to provide an electrode binder comprising a vinylidene fluoride copolymer that exhibits excellent adhesion to a current collector and is resistant to thickening of the electrode composite even when using an electrode active material with many surface functional groups. Furthermore, the present invention also aims to provide an electrode composite, an electrode, and a battery comprising said electrode binder. means of solving the problem

[0007] [1] The present invention provides an electrode binder containing a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, wherein the vinylidene fluoride copolymer is modified with a labeling material consisting of 1-bromomethylpyrene, and when the weight average molecular weight of the carboxyl group-containing vinylidene fluoride copolymer that absorbs light of wavelength 345 nm is specified, the weight average molecular weight is 1.3 million or less, and the adsorption rate obtained by the following method is greater than 0% and less than 30%.

[0008] (Method for determining adsorption rate)

[0009] (i) Prepare an N,N-dimethylacetamide (DMAc) solution with a vinylidene fluoride copolymer concentration of 1 g / L.

[0010] (ii) Gel penetration chromatography (GPC) is performed on the DMAc solution, and the peak area AR1 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0011] (iii) 5 g of the above DMAc solution, with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 Add 0.8 g of aluminum oxide with a concentration of 1 g or less, stir for 2 hours, and then let stand for 16 hours.

[0012] (iv) After settling, the supernatant of the above DMAc solution is collected, and solid-liquid separation is performed by centrifugation.

[0013] (v) GPC is performed on the separated solution, and the peak area AR2 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0014] (vi) The adsorption rate is calculated based on the following equation (I). This is done three times, and the average value is taken as the adsorption rate.

[0015] Adsorption rate = (AR1 - AR2) / AR1 × 100 (I)

[0016] [2] The present invention provides an electrode binder described in [1] having an adsorption rate of 1% or more and 20% or less.

[0017] [3] The present invention relates to an electrode binder comprising a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, wherein the adsorption rate obtained by the following method is greater than 0% and less than or equal to 60%, and

[0018] The above vinylidene fluoride copolymer is modified with a labeling material composed of 1-bromomethylpyrene to specify the weight average molecular weight Mwc of the carboxyl group-containing vinylidene fluoride copolymer that absorbs light of wavelength 345 nm, wherein the Mwc is less than 3.4 relative to the weight average molecular weight Mwa of the vinylidene fluoride copolymer, and the Mwc, Mwa, and the adsorption rate satisfy the following formula (II).

[0019] Mwc / Mwa<0.30 / adsorption rate (II)

[0020] (Method for determining adsorption rate)

[0021] (i) Prepare an N,N-dimethylacetamide solution with a concentration of 1 g / L of vinylidene fluoride copolymer.

[0022] (ii) Gel penetration chromatography is performed on the above N,N-dimethylacetamide solution, and the peak area AR1 derived from the above vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0023] (iii) 5 g of the above N,N-dimethylacetamide solution, with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 Add 0.8 g of aluminum oxide with a concentration of 1 g or less, stir for 2 hours, and then let stand for 16 hours.

[0024] (iv) After settling, the supernatant of the above N,N-dimethylacetamide solution is collected, and solid-liquid separation is performed by centrifugation.

[0025] (v) Gel penetration chromatography is performed on the separated solution, and the peak area AR2 derived from the vinylidene fluoride copolymer is calculated by detecting the differential refractive index.

[0026] (vi) The adsorption rate is calculated based on the following equation (I). This is done three times, and the average value is taken as the adsorption rate.

[0027] Adsorption rate = (AR1 - AR2) / AR1 × 100 (I)

[0028] [4] The present invention provides an electrode binder described in any one of [1] to [3], wherein, for every 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer, the amount of constituent units derived from vinylidene fluoride is 90.0 mol% or more, and the amount of constituent units derived from vinyl compounds is 0.01 mol% or more and 0.80 mol% or less.

[0029] [5] The present invention provides an electrode binder described in any one of [1] to [5], wherein the vinyl compound is a compound represented by the following general formula (1).

[0030] [Painting 1]

[0031]

[0032] (In general formula (1), R 1 , R 2 , R 3 Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents an atomic group))

[0033] [6] The present invention provides an electrode binder described in [1] to [5], wherein the vinyl compound is a compound represented by the following general formula (1).

[0034] [Painting 2]

[0035]

[0036] (In general formula (1), R 1 , R 2 , R 3 Each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents a divalent atomic group having a molecular weight of 500 or less, containing either an oxygen atom or a nitrogen atom and having 1 to 10 atoms in the main chain).

[0037] [7] The present invention provides an electrode composite comprising an electrode binder and an electrode active material as described in any one of [1] to [6].

[0038] [8] The present invention provides an electrode comprising a solid component of an electrode binder described in any one of [1] to [6].

[0039] [9] The present invention provides a battery comprising the electrode described in [8] above. Effects of the invention

[0040] According to the present invention, an electrode binder comprising a vinylidene fluoride copolymer is provided, which has excellent adhesion to a current collector and is difficult to thicken in an electrode composite even when an electrode active material with many surface functional groups is used. Additionally, an electrode composite, an electrode, and a battery comprising said electrode binder are also provided. Specific details for implementing the invention

[0041] 1. Electrode binder

[0042] The electrode binder of the present invention may contain a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group. The electrode binder may be in a solid state, such as a powder, for example, or in a liquid state. Furthermore, the electrode binder may be composed solely of a vinylidene fluoride copolymer, or, if necessary, may contain a solvent. When the electrode binder contains a solvent, the vinylidene fluoride copolymer may be dissolved in the solvent or dispersed in the solvent. The present invention has the following two embodiments. Each of them will be described below.

[0043] (1) First embodiment

[0044] Conventionally, when an electrode mixture (slurry) is prepared by mixing a vinylidene fluoride copolymer having carboxyl groups with an active material having a small particle size and having multiple functional groups on its surface, such as LFP (lithium iron phosphate), the viscosity tends to become very high. In contrast, the electrode binder according to one embodiment of the present invention is unlikely to increase in slurry viscosity even when mixed with an active material having a small particle size and having multiple functional groups, such as LFP. The reason for this is considered as follows.

[0045] The vinylidene fluoride polymer included in the electrode binder of the present embodiment is a copolymer of at least vinylidene fluoride and a vinyl compound having a carboxyl group, and is an aggregate of multiple polymers. The vinylidene fluoride copolymer (an aggregate of multiple polymers) includes a polymer comprising a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound (referred to herein as "carboxyl group-containing vinylidene fluoride copolymer" or "carboxyl group-containing copolymer") and a polymer mainly composed of a constituent unit derived from vinylidene fluoride and not comprising a constituent unit derived from a vinyl compound having a carboxyl group.

[0046] Furthermore, in the vinylidene fluoride copolymer included in the electrode binder according to the present embodiment, the weight average molecular weight (Mwc) of the carboxyl group-containing copolymer, specified by the method described below, is 1.3 million or less. As described above, when a general vinylidene fluoride copolymer having carboxyl groups is mixed with an active material, the functional groups present on the surface of the active material interact with the functional groups contained in the vinylidene fluoride copolymer. As a result, a robust network is formed based on the active material, and the viscosity of the slurry increases. In contrast, in the vinylidene fluoride copolymer included in the electrode binder of the present embodiment, the polymerization average molecular weight of the carboxyl group-containing copolymer interacting with the active material is relatively small. Therefore, even if the carboxyl group-containing copolymer interacts with the active material, it is difficult to form a robust network, and thus it is difficult for the viscosity of the slurry to increase excessively.

[0047] In addition, the vinylidene fluoride copolymer included in the electrode binder of the present embodiment has an adsorption rate for aluminum oxide measured by the method described below that is greater than 0% and less than or equal to 30%. The said adsorption rate represents the ratio of the polymer capable of adsorbing aluminum oxide within the vinylidene fluoride copolymer (an aggregate of multiple polymers). That is, the said adsorption rate corresponds to the ratio of the carboxyl group-containing copolymer within the vinylidene fluoride copolymer. Furthermore, since the said adsorption rate is 30% or less, when the vinylidene fluoride copolymer is mixed with an active material, it is difficult to form the aforementioned network, and consequently, it is difficult for excessive thickening of the slurry to occur. Below, the vinylidene fluoride copolymer included in the electrode binder according to the present embodiment, its physical properties, and additionally the solvent, etc., will be described in detail.

[0048] (Vinylidene fluoride copolymer)

[0049] As described above, the vinylidene fluoride copolymer is a copolymer formed by copolymerizing at least vinylidene fluoride with a vinyl compound having a carboxyl group. The amount of constituent units derived from vinylidene fluoride in the vinylidene fluoride copolymer is preferably 90.0 mol% or more and 95.00 mol% or more and 99.98 mol% or less with respect to 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer. If the amount of constituent units derived from vinylidene fluoride is 90.0 mol% or more, it becomes easier to obtain physical properties characteristic of vinylidene fluoride. This value can be calculated, for example, by specifying the amount of constituent units derived from compounds other than vinylidene fluoride contained in the vinylidene fluoride copolymer.

[0050] Meanwhile, the amount of constituent units derived from vinyl compounds having carboxyl groups in the vinylidene fluoride copolymer is preferably 0.01 mol% or more and 0.80 mol% or less, and preferably 0.02 mol% or more and 0.50 mol% or less, based on 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer. If the amount of the constituent units derived from vinyl compounds is 0.01 mol% or more, the adhesion of the vinylidene fluoride copolymer to the current collector is more likely to increase when an electrode is formed using an electrode binder. On the other hand, if the amount of the constituent units derived from vinyl compounds is 0.80 mol% or less, it becomes more easy to suppress the increase in slurry viscosity when the electrode binder is mixed with the active material. The amount of the constituent units derived from vinyl compounds is neutralized titrated or 1 It can be obtained from H-NMR spectra, etc.

[0051] Here, the structure of the vinyl compound is not particularly limited, and any compound having a vinyl group capable of polymerizing with vinylidene fluoride and having a carboxyl group is acceptable. Additionally, the number of carboxyl groups included in the vinyl compound may be one or two or more. Furthermore, in this specification, an acid anhydride structure composed of two carboxyl groups is also treated as a type of carboxyl group. The vinylidene fluoride copolymer may include only one type of constituent unit derived from the vinyl compound or two or more types. Examples of preferred vinyl compounds include compounds represented by the following general formula (1).

[0052] [Tuesday 3]

[0053]

[0054] In general formula (1), R 1 , R 2 , R 3 Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms. Examples of alkyl groups having 1 to 5 carbon atoms include straight-chain or branched-chain alkyl groups, and specific examples thereof include methyl groups, ethyl groups, propyl groups, isopropyl groups, n-butyl groups, sec-butyl groups, isobutyl groups, t-butyl groups, pentyl groups, etc. Among these, methyl groups, ethyl groups, or butyl groups are preferred from the perspective of ease of availability. Furthermore, particularly from the perspective that steric hindrance is unlikely to occur during polymerization with vinylidene fluoride, R 1 , R 2 and R 3 It is more preferable that each be an independent hydrogen atom or a methyl group.

[0055] In addition, in the above general formula (1), X is a hydroxyl group or a group represented by -Y-COOH. Here, Y represents an atomic group, and it is preferable that Y is an atomic group containing either an oxygen atom or a nitrogen atom, more preferable that Y is an atomic group containing either an oxygen atom or a nitrogen atom and also having a main chain with 1 or more and 10 or fewer atoms, and more preferable that Y is a divalent atomic group containing either an oxygen atom or a nitrogen atom and also having a main chain with 1 or more and 10 or fewer atoms and a molecular weight of 500 or less.

[0056] The atomic group (Y) may be linear, branched, cyclic, or a combination thereof. Among these, it is preferable that the atomic group (Y) be linear or branched from the perspective that steric hindrance is unlikely to occur during polymerization with vinylidene fluoride.

[0057] The number of atoms in the main chain of the atomic group (Y) may be 1 or more and 10 or less, and 2 or more and 8 or less is preferred. In this specification, the main chain of the atomic group (Y) refers to the longest chain among the chains connecting the carbonyl group of general formula (1) and the carboxyl group of -Y-COOH.

[0058] Here, the atomic group (Y) includes either or both of oxygen atoms and nitrogen atoms (hereinafter collectively referred to as "hetero atoms"). The number of hetero atoms in the atomic group (Y) is preferably 1 to 10, and more preferably 1 to 5. When the atomic group (Y) includes two or more hetero atoms, they may be atoms of the same type or atoms of different types. The hetero atoms may be included in a structure (functional group) or may exist at any position within the atomic group (Y). Examples of structures (functional groups) containing these hetero atoms include ether bonds, ester bonds, carbonyl groups, carboxyl groups, amide groups, hydroxyl groups, etc. Among these, ether bonds, ester groups, carbonyl groups, carboxyl groups, amide groups, and hydroxyl groups are preferred.

[0059] The structure of the atomic group (Y) is not particularly limited and, for example, can be a structure in which a hydrocarbon group such as an alkylene group or an alkyl group is combined with a structure (functional group) containing the above heteroatom. In addition, the molecular weight of the atomic group (Y) may be 500 or less, and from the perspective of polymerization reactivity, it is preferable to be 30 or more and 200 or less.

[0060] Specific examples of the compound represented by the above general formula (1) include (meth)acrylic acid, (meth)acryloyloxyethyl succinic acid, (meth)acryloyloxypropyl succinic acid, 2-carboxyethyl (meth)acrylate, 2-carboxymethyl (meth)acrylate, (meth)acryloyloxyethyl phthalic acid, N-carboxyethyl (meth)acrylamide, and other (meth)acrylamide compounds. Additionally, in this specification, (meth)acrylic refers to methacrylate, acrylate, or a mixture thereof, (meth)acrylate refers to methacrylate, acrylate, or a mixture thereof, and (meth)acryloyl refers to methacryloyl, acryloyl, or a mixture thereof.

[0061] The compounds represented by the above general formula (1) are more preferably acrylic acid, acryloyloxyethyl succinic acid, acryloyloxypropyl succinic acid, 2-carboxyethyl acrylate, and 2-carboxymethyl acrylate in terms of ease of availability and reactivity with vinylidene fluoride.

[0062] However, the vinyl compound having the above-mentioned carboxyl group is not limited to the compound represented by the general formula (1). Examples of vinyl compounds other than the compound represented by the general formula (1) include unsaturated dibasic acids such as maleic acid, fumaric acid, and itaconic acid; unsaturated dibasic acid anhydrides such as maleic anhydride and itaconic anhydride; and unsaturated dibasic acid monoesters such as monomethyl fumarate, monoethyl fumarate, monomethyl maleate, monoethyl maleate, monomethyl citraconic acid, monoethyl citraconic acid, monomethyl phthalate, monoethyl phthalate, monomethyl itaconic acid, and monoethyl itaconic acid.

[0063] In addition, the vinylidene fluoride copolymer may partially contain constituent units derived from compounds other than vinylidene fluoride and vinyl compounds having said carboxyl groups (other compounds), to the extent that the purpose and effect of the present embodiment are not impaired. The vinylidene fluoride copolymer may contain only one type of constituent unit derived from other compounds, or it may contain two or more types. However, the total amount of constituent units derived from other compounds relative to 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer is preferably 10.0 mol% or less, and more preferably 5.0 mol% or less. The amounts thereof 19 F-NMR spectrum and 1 It is determined from H-NMR spectra, etc.

[0064] Examples of other compounds include fluorinated vinyl compounds having a vinyl group and a fluorine atom or a fluorine-containing alkyl group in one molecule. Examples of fluorinated vinyl compounds include vinyl fluoride; trifluoroethylene; tetrafluoroethylene; chlorotrifluoroethylene; hexafluoropropylene; and perfluoroalkyl vinyl ethers represented by perfluoromethyl vinyl ether. Additionally, examples of other compounds include compounds having a vinyl group and not containing fluorine. Examples thereof include unsaturated hydrocarbon compounds such as ethylene and propylene.

[0065] Here, among the vinylidene fluoride copolymers (multiple polymers), the weight average molecular weight Mwc of the polymer having a carboxyl group, i.e., the carboxyl group-containing copolymer, may be 1.3 million or less, but it is preferable that it be 25,000 or more and 1.3 million or less, and more preferable that it be 100,000 or more and 1.2 million or less. As described above, if the weight average molecular weight Mwc of the carboxyl group-containing copolymer is 1.3 million or less, it becomes difficult for the slurry viscosity to become excessively high when the vinylidene fluoride copolymer is used in the electrode composite.

[0066] In this specification, the weight average molecular weight Mwc of a carboxyl group-containing copolymer is a value obtained as follows. A vinylidene fluoride copolymer modified with pyrene is obtained by mixing a labeling material (1-bromomethylpyrene) for labeling carboxyl groups with potassium carbonate and performing esterification of the carboxyl groups. Then, GPC is performed using N,N-dimethylacetamide as the eluent, and the polystyrene equivalent value is obtained using an ultraviolet-visible (UV-vis) detector (detection wavelength is 345 nm). Furthermore, the pyrene structure has characteristic absorption in the ultraviolet-visible region and strongly absorbs light of wavelength 345 nm. That is, the polymerization average molecular weight Mwc of the carboxyl group-containing copolymer is determined by esterifying the carboxyl groups with 1-bromomethylpyrene.

[0067] Meanwhile, the weight average molecular weight Mwa of the vinylidene fluoride copolymer (total) is not particularly limited, but is preferably 100,000 or more and 5 million or less, more preferably 200,000 or more and 4 million or less, and particularly preferably 250,000 or more and 3 million or less. If the weight average molecular weight Mwa of the vinylidene fluoride copolymer is 100,000 or more, the adhesion strength of the vinylidene fluoride copolymer with the active material, etc., or the current collector is likely to increase. On the other hand, if the Mwa is 5 million or less, the slurry viscosity does not become too high when the electrode mixture (slurry) is prepared, so workability is particularly likely to be excellent. In this specification, the weight average molecular weight Mwa of the vinylidene fluoride copolymer is a polystyrene equivalent value measured by gel permeation chromatography (GPC). At this time, the eluent is N,N-dimethylacetamide, and the weight average molecular weight is determined by a differential refractive index (RI) detector.

[0068] Here, the weight average molecular weight Mwc of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer is preferably less than 3.4 relative to the weight average molecular weight Mwa of the vinylidene fluoride copolymer, i.e., Mwc / Mwa < 3.4, and Mwc / Mwa is preferably 0.25 or more and 3.0 or less, more preferably 0.25 or more and 2.0 or less, and more preferably 0.25 or more and 1.0 or less. If the ratio is less than 3.4, it becomes difficult for the slurry viscosity to increase further when mixed with an active material to form an electrode mixture (slurry).

[0069] In addition, the above vinylidene fluoride copolymer has an adsorption rate specified by the following method that is greater than 0% and less than 30%, more preferably greater than 1% and less than 20%, and even more preferably greater than 2% and less than 15%.

[0070] (Method for determining adsorption rate)

[0071] The adsorption rate is determined by performing (i) to (vi) below.

[0072] (i) Prepare a dimethylacetamide (DMAc) solution with a concentration of 1 g / L of vinylidene fluoride copolymer.

[0073] (ii) Gel penetration chromatography (GPC) is performed on the DMAc solution prepared in (i), and the peak area AR1 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0074] (iii) 5 g of the DMAc solution prepared in (i), with a BET specific surface area of ​​4 m 2 / g or more than 5 m 2 Add 0.8 g of aluminum oxide with a concentration of 1 g or less, stir for 2 hours, and then let stand for 16 hours.

[0075] (iv) Collect the supernatant of the DMAc solution after settling in (iii), and perform solid-liquid separation by centrifugation.

[0076] (v) GPC is performed on the separation solution obtained in (iv), and the peak area AR2 derived from the vinylidene fluoride copolymer is calculated by differential refractive index detection.

[0077] (vi) From the areas AR1 and AR2 obtained in (ii) and (v) above, the adsorption rate is calculated based on the following equation (I). This is performed three times, and the average value is taken as the adsorption rate.

[0078] Adsorption rate = (AR1 - AR2) / AR1 × 100 (I)

[0079] As described above, the vinylidene fluoride copolymer comprises a carboxyl group-containing copolymer containing constituent units derived from the vinyl compound, and a polymer that does not contain constituent units derived from the vinyl compound and is mainly composed of constituent units of vinylidene fluoride (and other compounds). Furthermore, the adsorption rate corresponds to the amount of the carboxyl group-containing copolymer relative to the total amount of polymers constituting the vinylidene fluoride copolymer. In this embodiment, since the content ratio of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer is 30% or less, it is difficult for the slurry viscosity to increase excessively when the electrode binder is mixed with the active material. Meanwhile, because the vinylidene fluoride copolymer contains the carboxyl group-containing copolymer, when the electrode binder (vinylidene fluoride copolymer) is used in the electrode, the adhesion strength between the vinylidene fluoride copolymer and the current collector, etc., is improved.

[0080] Here, the inherent viscosity of the vinylidene fluoride copolymer is preferably 0.5 dL / g or more and 6.0 dL / g or less, more preferably 0.5 dL / g or more and 5.0 dL / g or less, and even more preferably 0.8 dL / g or more and 4.5 dL / g or less. If the inherent viscosity is 0.5 dL / g or more, the adhesion strength of the vinylidene fluoride copolymer with the active material, etc., or the current collector tends to increase. On the other hand, if the inherent viscosity is 6.0 dL / g or less, the slurry viscosity does not become too high when the electrode mixture (slurry) is prepared, so workability is particularly likely to be excellent. Inherent viscosity (η i ) represents the logarithmic viscosity. First, 80 mg of vinylidene fluoride copolymer is dissolved in 20 ml of N,N-dimethylformamide, and the viscosity is measured using a Ubbelohde viscometer in a constant temperature bath at 30°C. Then, it is calculated based on the following formula from the obtained value.

[0081] η i =(1 / C)·ln(η / η0)

[0082] In the above formula, η is the viscosity of the solution, η0 is the viscosity of the solvent N,N-dimethylformamide alone, and C is the concentration of vinylidene fluoride copolymer in the solution, i.e., 0.4 g / dl.

[0083] In addition, the melting point of the vinylidene fluoride copolymer is preferably 150°C or higher and 180°C or lower, more preferably 155°C or higher and 175°C or lower, and particularly preferably 160°C or higher and 175°C or lower. If the melting point of the vinylidene fluoride copolymer is 150°C or higher, when the electrode binder (vinylidene fluoride copolymer) is used in the electrode, it is difficult to swell due to the electrolyte, and the performance of the resulting battery is likely to be good. On the other hand, if the melting point is 180°C or lower, the flexibility when forming the electrode is likely to be good. The melting point of the vinylidene fluoride copolymer can be determined by calorimetric measurement using differential scanning calorimetry (DSC).

[0084] The above vinylidene fluoride copolymer can be prepared by copolymerizing vinylidene fluoride, the vinyl compound having the carboxyl group, and other compounds as needed. Examples of methods for copolymerizing these include suspension polymerization, emulsion polymerization, and solution polymerization, but suspension polymerization is preferred from the view that it reduces impurities.

[0085] In suspension polymerization using water as a dispersion medium, a suspending agent such as methyl cellulose, propoxylated methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyethylene oxide, or gelatin is added and used in a range of 0.005 to 1.0 parts by mass, preferably 0.01 to 0.4 parts by mass, per 100 parts by mass of the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers).

[0086] As a polymerization initiator, diisopropyl peroxydicarbonate, dinormal propyl peroxydicarbonate, dinormal heptafluoropropyl peroxydicarbonate, isobutyryl peroxide, di(chlorofluoroacyl)peroxide, di(perfluoroacyl)peroxide, t-butyl peroxypivalate, etc. may be used. The amount used is 0.05 to 10 parts by mass, preferably 0.15 to 5 parts by mass, when the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers as needed) are 100 parts by mass.

[0087] In addition, it is also possible to control the degree of polymerization of the obtained vinylidene fluoride copolymer by adding a chain transfer agent such as ethyl acetate, methyl acetate, diethyl carbonate, acetone, ethanol, n-propanol, acetaldehyde, propylaldehyde, ethyl propionate, and carbon tetrachloride. When a chain transfer agent is used, the amount used is typically 0.01 to 5 parts by mass, preferably 0.01 to 3 parts by mass, when the total monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers) are 100 parts by mass.

[0088] In addition, the total amount of monomers used in copolymerization (vinylidene fluoride, vinyl compounds having carboxyl groups, and other monomers) added is typically 1:1 to 1:10, preferably 1:2 to 1:5, in terms of the mass ratio of total monomers to water.

[0089] The polymerization temperature T is the 10-hour half-life temperature T of the polymerization initiator. 10 It is selected appropriately depending on, and usually T 10 -25℃≤T≤T 10 It is selected within the range of +25℃. For example, T of t-butyl peroxypivalate and diisopropyl peroxydicarbonate 10These are 54.6°C and 40.5°C, respectively (refer to the Nichiyu Corporation product catalog). Accordingly, in polymerization using t-butyl peroxypivalate and diisopropyl peroxydicarbonate as polymerization initiators, the polymerization temperature T is appropriately selected within the ranges of 29.6°C ≤ T ≤ 79.6°C and 15.5°C ≤ T ≤ 65.5°C, respectively. The polymerization time is not particularly limited, but considering productivity, it is preferable to be 100 hours or less. The pressure during polymerization is typically performed under pressure, and is preferably 2.0 to 10.0 MPa-G.

[0090] Here, as a method to set the weight average molecular weight Mwc of the above-mentioned carboxyl group-containing copolymer to 1.3 million or less and the adsorption rate described above to be greater than 0% and less than or equal to 30%, the following two methods may be cited as examples. However, they are not limited to these methods. The first method is a method of mixing the entire amount of vinylidene fluoride (and other compounds) and the vinyl compound having carboxyl groups and then starting polymerization. The second method is a method of polymerizing vinylidene fluoride (and other compounds) to a certain extent, then adding the entire amount of the vinyl compound having carboxyl groups to the reaction system in a short time, and then performing polymerization again. Examples of adding in a short time include setting the addition rate of the vinyl compound having carboxyl groups to 0.2 parts by mass / hour or more when the total monomer used in copolymerization is 100 parts by mass. By doing so, the weight average molecular weight Mwc and the adsorption rate can be set to a desired range.

[0091] (menstruum)

[0092] As described above, the electrode binder may contain a solvent. The solvent may be a non-aqueous solvent or water. Additionally, the non-aqueous solvent may be a polar solvent (polar solvent). Examples of the above polar solvents include amide compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; alcohol compounds such as methanol, ethanol, isopropyl alcohol, 2-ethyl-1-hexanol, 1-nonanol, lauryl alcohol, and tripropylene glycol; amine compounds such as o-toluidine, m-toluidine, and p-toluidine; imide compounds such as 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide; lactone compounds such as γ-butyrolactone and δ-butyrolactone; and sulfoxide-sulfone compounds such as dimethyl sulfoxide and sulfolane. Ether compounds such as tetrahydrofuran, diethyl ether, 1,4-dioxane, and diethylene glycol dimethyl ether; ketone compounds such as acetone, 2-butanone, methyl isobutyl ketone, and cyclohexanone are included. The electrode binder may contain only one of the above solvents, or may contain two or more.

[0093] When the electrode binder contains a solvent, the amount of solvent in the electrode binder is preferably 50 parts by mass or more and 10,000 parts by mass or less per 100 parts by mass of the vinylidene fluoride copolymer, and more preferably 100 parts by mass or more and 5,000 parts by mass or less. If the amount of solvent in the electrode binder is within this range, it is possible to uniformly disperse or dissolve the vinylidene fluoride copolymer in the solvent.

[0094] (etc)

[0095] The electrode binder may additionally include, to the extent that it does not impair the purpose and effect of the present embodiment, other resins such as acrylic resin, fillers such as inorganic fillers, various additives such as dispersants and emulsifiers.

[0096] (2) Second embodiment

[0097] The vinylidene fluoride polymer included in the electrode binder of the present embodiment is also a copolymer of at least vinylidene fluoride and a vinyl compound having a carboxyl group, and is an aggregate of multiple polymers. The vinylidene fluoride copolymer (an aggregate of multiple polymers) includes the carboxyl group-containing copolymer described above and a polymer that is mainly composed of constituent units derived from vinylidene fluoride and does not include constituent units derived from a vinyl compound having a carboxyl group.

[0098] The vinylidene fluoride copolymer included in the electrode binder according to the present embodiment has an adsorption rate for aluminum oxide obtained by the method described in the first embodiment greater than 0% and less than or equal to 60%. In addition, the weight average molecular weight Mwc of the carboxyl group-containing copolymer obtained by the method described above is less than 3.4 relative to the weight average molecular weight Mwa of the vinylidene fluoride copolymer (total), and Mwc, Mwa, and the adsorption rate satisfy the following formula (II).

[0099] Mwc / Mwa<0.30 / adsorption rate (II)

[0100] According to the inventors' careful examination, it has been found that when the vinylidene fluoride copolymer satisfies the specific formula above, excessive thickening of the slurry is unlikely to occur when the vinylidene fluoride copolymer is mixed with an active material. Hereinafter, the vinylidene fluoride copolymer included in the electrode binder according to the present embodiment and its physical properties will be described. The electrode binder of the present embodiment may also additionally include a solvent, but since the solvent is the same as that of the first embodiment, a description thereof is omitted here.

[0101] (Vinylidene fluoride copolymer)

[0102] As described above, the vinylidene fluoride copolymer is a copolymer formed by copolymerizing at least vinylidene fluoride with a vinyl compound having a carboxyl group. The amount of constituent units derived from vinylidene fluoride and the amount of constituent units derived from the vinyl compound having a carboxyl group in the vinylidene fluoride copolymer are the same as the respective amounts in the first embodiment. Furthermore, the structure of the vinyl compound is the same as the structure of the vinyl compound described in the first embodiment.

[0103] In addition, the vinylidene fluoride copolymer may partially contain constituent units derived from compounds other than vinylidene fluoride and vinyl compounds having said carboxyl groups (other compounds), to the extent that the purpose and effect of the present embodiment are not impaired. The vinylidene fluoride copolymer may contain only one type of constituent unit derived from other compounds, or it may contain two or more types. However, the total amount of constituent units derived from other compounds relative to 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer is preferably 10.0 mol% or less, and more preferably 5.0 mol% or less. The amounts thereof 19 F-NMR spectrum and 1 It is identified from H-NMR spectra, etc. Other compounds are the same as the other compounds described in the first embodiment.

[0104] Here, among the vinylidene fluoride copolymers (multiple polymers) of the present embodiment, the weight average molecular weight Mwc of the polymer having a carboxyl group, i.e., the carboxyl group-containing copolymer, is not particularly limited as long as the ratio to Mwa falls within a predetermined range and it is possible to satisfy the formula (II) described above. The weight average molecular weight Mwc is preferably 1.3 million or less, more preferably 25,000 or more and 1.3 million or less, and even more preferably 100,000 or more and 1.2 million or less. If the weight average molecular weight Mwc of the carboxyl group-containing copolymer is 1.3 million or less, it becomes difficult for the slurry viscosity to become excessively high when the vinylidene fluoride copolymer is used in the electrode composition. Mwc is measured by the method described above.

[0105] Meanwhile, the weight-average molecular weight Mwa of the vinylidene fluoride copolymer (total) is not particularly limited as long as the ratio to Mwc falls within a predetermined range and it is possible to satisfy the formula (II) described above. The weight-average molecular weight Mwa is preferably 100,000 or more and 5 million or less, more preferably 200,000 or more and 4 million or less, and particularly preferably 250,000 or more and 3 million or less. If the weight-average molecular weight Mwa of the vinylidene fluoride copolymer is 100,000 or more, the adhesion strength of the vinylidene fluoride copolymer with the active material, etc., or the current collector is likely to increase. On the other hand, if the Mwa is 5 million or less, the slurry viscosity does not become too high when the electrode mixture (slurry) is prepared, and workability is particularly likely to be excellent. Mwa is measured by the method described above.

[0106] Here, the weight average molecular weight Mwc of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer may be less than 3.4 with respect to the weight average molecular weight Mwa of the vinylidene fluoride copolymer (i.e., Mwc / Mwa < 3.4), but Mwc / Mwa is preferably 0.25 or higher and 3.0 or lower, more preferably 0.25 or higher and 2.0 or lower, and more preferably 0.25 or higher and 1.0 or lower.

[0107] In addition, the above-described vinylidene fluoride copolymer may have an adsorption rate of greater than 0% and less than or equal to 60% as specified by the method described above, but it is preferable that it is greater than 0% and less than or equal to 30%, more preferable that it is greater than or equal to 1% and less than or equal to 20%, and even more preferable that it is greater than or equal to 2% and less than or equal to 15%.

[0108] In addition, Mwc, Mwa, and the adsorption rate are adjusted so as to satisfy the following equation (II).

[0109] Mwc / Mwa<0.30 / adsorption rate (II)

[0110] Mwc / Mwa may be less than 0.30 / adsorption rate, but less than 0.25 / adsorption rate is preferable, and less than 0.20 / adsorption rate is more preferable. The method of adjusting Mwc, Mwa, and adsorption rate is not particularly limited, but can be realized by preparing the vinylidene fluoride copolymer by any one of the following two methods.

[0111] As a first method, a vinylidene fluoride copolymer is obtained by mixing vinylidene fluoride (and other compounds) with the entire amount of a vinyl compound having a carboxyl group and then initiating polymerization. Additionally, as a second method, a vinylidene fluoride copolymer is obtained by polymerizing vinylidene fluoride (and other compounds) to a certain extent, then adding the entire amount of a vinyl compound having a carboxyl group to the reaction system in a short time, and then performing polymerization again. Examples of adding in a short time include setting the addition rate of the vinyl compound having a carboxyl group to 0.2 parts by mass / hour or more when the total monomer used for copolymerization is 100 parts by mass. By doing so, the weight-average molecular weight Mwc and the adsorption rate can be set to a desired range. Furthermore, the weight-average molecular weight Mwa of the vinylidene fluoride copolymer can be adjusted by the amount of polymerization initiator, the amount of chain transfer agent, the polymerization temperature, etc. In addition, the polymerization initiator, chain transfer agent, polymerization time, etc. used in the preparation of the vinylidene fluoride copolymer can be the same as the method described in the first embodiment.

[0112] The inherent viscosity or melting point of the vinylidene fluoride copolymer of the present embodiment can be made the same as the inherent viscosity or melting point of the vinylidene fluoride copolymer of the first embodiment.

[0113] 2. Electrode composite

[0114] The aforementioned electrode binder and active material (positive active material or negative active material) can be mixed to form an electrode mixture (slurry) for manufacturing electrodes of a non-aqueous electrolyte secondary battery. The electrode mixture may additionally contain a conductive agent, a solvent, or other additives.

[0115] The amount of solid derived from the electrode binder (vinylidene fluoride copolymer) relative to the total amount of solid derived from the electrode binder (total amount excluding volatile components), active material, and conductive aid is preferably 0.2 mass% or more and 20 mass% or less, more preferably 0.2 mass% or more and 10 mass% or less, and even more preferably 0.2 mass% or more and 7 mass% or less.

[0116] In addition, the vinylidene fluoride copolymer included in the aforementioned electrode binder is carbon-coated and has a large number of surface functional groups, and even when mixed with an active material having a small particle diameter (e.g., LFP or LFMP (lithium iron manganese phosphate)), it is difficult for the electrode mixture to thicken or gel. For example, LFP has an average particle diameter of 15 μm or less when measured by measuring particle diameter distribution by laser dilution and scattering with pure water as the dispersion medium, and is typically between 0.1 μm and 15 μm. Even when the aforementioned electrode binder is mixed with such an active material, it is difficult for the electrode mixture to thicken. However, the average particle diameter of the active material is not limited to the above range.

[0117] In the present invention, various materials can be used as the active material of the electrode composite. The active material is not particularly limited, and both known negative electrode active materials (negative electrode active materials) and positive electrode active materials (positive electrode active materials) can be used.

[0118] Examples of negative electrode active materials include carbon materials such as artificial graphite, natural graphite, non-graphitized carbon, digraphitized carbon, activated carbon, or phenolic resin and pitch, etc., which are calcined and carbonized; metal and alloy materials such as Cu, Li, Mg, B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Cd, Ag, Zn, Hf, Zr, and Y; and metal oxides such as GeO, GeO2, SnO, SnO2, PbO, and PbO2. Additionally, the negative electrode active material may be a material coated on the surface of the above carbon materials, metal and alloy materials, metal oxides, etc. Additionally, the negative electrode active material may be a commercially available product.

[0119] Meanwhile, examples of positive electrode active materials include lithium-based positive electrode active materials containing lithium. Examples of lithium-based positive electrode active materials include LiCoO2, LiNiO2, and LiNi x Co y Mn 1-x-y O2(0 <x<1, 0<y<1), LiNi x Co y Al 1-x-y O2(0 <x<1, 0<y<1), LiNi x Co 1-x O2(0 <x≤1) 등의 일반식 LiMY2(M은 Co, Ni, Fe, Mn, Cr, Ti 및 V 등의 전이 금속 중 1종 또는 2종 이상, Y는 O 및 S 등의 칼코겐 원소)로 표시되는 복합 금속 칼코겐 화합물; LiMnO2, LiMn2O4등의 스피넬 구조를 취하는 복합 금속 산화물; LiFePO4나 LiFeMnPO4등의 LiMaPO4(다만, Ma는 Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, Zr로부터 선택되는 1종류 이상의 원소)로 표시되는 올리빈형 리튬 화합물; Li2MnO3-LiMbO2(Mb=Mn, Co, Ni)로 표시되는 Li 과잉계 고용체 양극; 티탄산 리튬(Li4Ti5O 12 ), titanium oxide (TiO2); Li s Ni t Co u Al vO2(0.9 <s<1.3, 0.9<t+u+v<1.1); LiNi x Co y M z O2(M represents Mn or Al, and x, y, and z are each 0 <x<1, 0<y<1, 0<z<1 및 x+y+z=1을 만족한다) 등으로 표시되는 리튬 금속 산화물이 포함된다. 이들 중에서도 특히, 입자 직경이 작고, 또한 탄소 피복 처리에 의해 표면 관능기가 많은 LiFePO4(LFP), LiFeMnPO4(LFMP)가 본 발명의 효과를 향수하기 쉽다는 관점에서 바람직하다. 또한, 양극 활물질은 상기 화합물의 표면에 코팅을 실시한 것일 수도 있다. 또한, 양극 활물질은 시판품일 수도 있다.

[0120] The amount of active material included in the electrode composite is appropriately selected according to the application of the electrode composite, but it is preferable that it be 50 mass% or more and 99.9 mass% or less with respect to the total amount of solids derived from the electrode binder, active material, and conductive additive. If the amount of active material is within this range, for example, sufficient charge / discharge capacity is obtained, and battery performance is likely to be good.

[0121] In addition, the conductive aid included in the electrode composite is not particularly limited as long as it is a compound capable of further enhancing the conductivity between the active materials or between the active materials and the current collector. Examples of conductive aids include acetylene black, ketjen black, carbon black, graphite powder, carbon nanofiber, carbon nanotube, and carbon fiber, etc.

[0122] The amount of conductive additive included in the electrode composite is appropriately selected according to its type, etc. In terms of improving conductivity and increasing the dispersibility of the conductive additive, with respect to the total amount of the solid component derived from the electrode binder, the active material, and the conductive additive, it is preferable to have 0.1 mass% or 15 mass% or less, more preferable to have 0.1 mass% or more and 7 mass% or less, and even more preferable to have 0.1 mass% or more and 5 mass% or less.

[0123] The electrode composite may contain a solvent different from the solvent that the above-mentioned electrode binder may contain. The said solvent may be selected from among the solvents that the binder described above may contain.

[0124] The total amount of solvent in the electrode mixture (including the amount of solvent in the electrode binder) is not particularly limited, but typically, it is preferably 10 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the active material described above.

[0125] The electrode composite may additionally include a dispersant, an adhesion aid, a thickener, etc., and known compounds may be used for these. Examples of the dispersant include polyvinylpyrrolidone, methyl cellulose, propoxylated methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyethylene oxide, polypropylene oxide, gelatin, etc. In addition, examples of the adhesion aid include poly(meth)acrylic acid, metal salts of poly(meth)acrylate such as sodium poly(meth)acrylate, carboxymethyl cellulose, etc. The amounts of these are not particularly limited as long as they are within a range that does not impair the purpose and effects of the present invention, but it is preferable that they be 15 mass% or less with respect to the total amount of solids derived from the electrode binder and the active material.

[0126] In addition, the electrode composite may further include additives such as phosphorus compounds; sulfur compounds; nitrogen compounds such as amine compounds and ammonium compounds; organic acids; organic esters; various silane-based, titanium-based, and aluminum-based coupling agents; vinylidene fluoride polymers other than the vinylidene fluoride copolymer described above; and resins such as polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), and polyacrylonitrile (PAN). These are not particularly limited as long as they do not impair the purpose and effects of the present invention, but it is preferable that they be 15 mass% or less with respect to the total amount of solids derived from the electrode binder and the active material.

[0127] The above electrode mixture may be prepared by mixing all components simultaneously, or by mixing some components first and then mixing the remaining components later.

[0128] The viscosity of the electrode mixture is not particularly limited as long as it is a viscosity that can prevent dripping, uneven coating, and delayed drying after coating when forming a mixture layer by coating the electrode mixture, and provides good workability and applicability during the production of the mixture layer. The said viscosity is a value measured at 25°C using an E-type viscometer, and after a holding period of 60 seconds at 25°C using an E-type viscometer, a shear rate of 1 s -1 This is the value measured 120 seconds after the rotor starts rotating.

[0129] 3. Electrode

[0130] The electrode composite described above can be used to form a composite layer of an electrode of various non-aqueous electrolyte secondary batteries. An electrode of a non-aqueous electrolyte secondary battery comprises, for example, a current collector and a composite layer disposed on said current collector. The electrode composite described above can be used to form said composite layer.

[0131] · Entire house

[0132] The current collector is a terminal for extracting electricity. The material of the current collector is not particularly limited, and may be used as a metal foil or metal mesh such as aluminum, copper, iron, stainless steel, steel, nickel, or titanium, or as a material having a layer containing carbon black formed on its surface. In addition, it may be a material having a layer containing carbon black formed on the surface of another medium, or a material having the above-mentioned metal foil or metal mesh applied thereto.

[0133] · Combined layer

[0134] The composite layer is a layer formed by applying the above-described electrode composite onto a current collector and solidifying it. That is, the composite layer comprises at least a vinylidene fluoride-based compound, which is a solid component of the above-described electrode binder, and an active material. The composite layer may be formed on only one side of the current collector or may be disposed on both sides.

[0135] The composite layer comprises at least the components included in the electrode composite described above, namely, a solid derived from the electrode binder (vinylidene fluoride copolymer) and an active material, and additionally includes various additives such as conductivity aids, dispersants, adhesion aids, and thickeners as needed. These are the same as those described in the electrode composite.

[0136] Here, the thickness of the composite layer is not particularly limited, but in one example, it is preferably 1 μm or more and 1,000 μm or less. In addition, the weight per unit area of ​​the composite layer formed on one side of the current collector is not particularly limited and can be any weight per unit area, but in one example, 50 g / m² 2 1000 g / m² or more 2 The following is preferable, and 100 g / m² 2 500 g / m² or more 2 The following is more desirable.

[0137] The above composite layer can be formed by performing a process of applying the above-described electrode composite onto a current collector and a process of solidifying it.

[0138] The method of applying the electrode mixture is not particularly limited, and the doctor blade method, reverse roll method, comma bar method, gravure method, air knife method, die coating method, and dip coating method can be applied.

[0139] In addition, after applying the electrode mixture, the solvent is dried by heating at any temperature. In one example, the drying temperature is preferably 60°C or higher and 500°C or lower, and more preferably 80°C or higher and 200°C or lower. Heating may be performed multiple times at different temperatures. In addition, the solvent in the mixture may be dried under atmospheric pressure, pressurized pressure, or reduced pressure, or it may be dried under an environment such as air, nitrogen, or argon. Additional heat treatment may be performed after drying.

[0140] After applying and drying the above electrode mixture, additional press treatment may be performed. By performing press treatment, the electrode density can be improved. In one example, the press pressure is preferably 1 kPa or more and 10 GPa or less.

[0141] 4. Battery

[0142] The electrode binder or electrode composite described above can be used for electrodes of various non-aqueous electrolyte secondary batteries, as described above, but can also be used to form other layers of non-aqueous electrolyte secondary batteries.

[0143] Examples

[0144] Specific embodiments of the present invention are described below together with comparative examples, but the present invention is not limited to these.

[0145] (Methods for measuring and evaluating physical properties)

[0146] In the examples and comparative examples described below, the amount of a vinyl compound having a carboxyl group in a vinylidene fluoride copolymer is determined by the following method ( 1 H-NMR measurement and neutralization titration), inherent viscosity of vinylidene fluoride copolymer, weight average molecular weight Mwa of vinylidene fluoride copolymer, weight average molecular weight Mwc of carboxyl group-containing copolymer in vinylidene fluoride copolymer, and adsorption rate of vinylidene fluoride copolymer for aluminum oxide were determined. In addition, the slurry viscosity and peel strength of the electrode mixture were determined by the following method.

[0147] · Specification of the amount of vinyl compound having a carboxyl group introduced ( 1 H-NMR measurement)

[0148] 1 From the spectrum obtained by H-NMR, the integrated intensity of the peak originating from vinylidene fluoride and the integrated intensity of the peak originating from vinyl compounds having carboxyl groups were determined, respectively, among the peaks originating from the constituent units of the vinylidene fluoride polymer. Then, the ratio (mol%) of vinyl compounds having carboxyl groups in the total constituent units of the vinylidene fluoride polymer was calculated from the ratio of the integrated intensity of the peak originating from vinyl compounds having carboxyl groups to the total constituent units of the vinylidene fluoride polymer (the sum of the integrated intensity of the peak originating from vinyl compounds and the integrated intensity of the peak originating from vinylidene fluoride). The measurement device used was a nuclear magnetic resonance device (NMR, JEOL product, JNM-ECZ600R / S1, frequency 600 MHz), and DMSO-d6 was used as the solvent.

[0149] · Determination of the amount of vinyl compound containing a carboxyl group introduced (neutralization titration)

[0150] 0.50 g of accurately weighed polymer was added to 100 mL of acetone while stirring. The mixture was heated and stirred at 50°C, and after confirming dissolution, 5 mL of water was slowly added while heating and stirring. Then, about 5 drops of phenolphthalein ethanol solution were added as an indicator. A 0.1 N aqueous sodium hydroxide solution of known concentration was added to the solution to be titrated while stirring using a burette, and the titration was performed. This was repeated three times, and the mole fraction of the vinyl compound containing a carboxyl group was calculated from the average value.

[0151] ·Inherent viscosity

[0152] The inherent viscosity of the vinylidene fluoride copolymer was measured as follows. First, 80 mg of the vinylidene fluoride copolymer was dissolved in 20 ml of N,N-dimethylformamide, and the viscosity was measured using an Ubérode viscometer in a constant temperature bath at 30°C. Then, based on the obtained value, the inherent viscosity (η) of the vinylidene fluoride copolymer was calculated according to the following formula. i ) produced.

[0153] η i =(1 / C)·ln(η / η0)

[0154] In the above formula, η is the viscosity of the solution, η0 is the viscosity of the solvent N,N-dimethylformamide alone, and C is the concentration of the vinylidene fluoride copolymer in the solution, i.e., 0.4 g / dl.

[0155] · Weight average molecular weight Mwa of vinylidene fluoride copolymer

[0156] The weight-average molecular weight (Mwa) of the vinylidene fluoride copolymer prepared in each example and comparative example was measured using a differential refractometer (RI). Specifically, gel penetration (GPC) was performed under the following conditions, and the Mwa was determined using a differential refractive index detector. This was performed three times, and the average value was taken as Mwa.

[0157] Separation Columns: Shodex KD-807, KD-806M

[0158] Detector: JASCO Corporation RI-4030 (Disparity Refractive Index Detector)

[0159] Eluent: 10 mM LiBr-N, N-dimethylacetamide (DMAc) solution

[0160] Eluent flow rate: 0.5 mL / min

[0161] Column temperature: 40℃

[0162] Standard polymer for calibration curve: TSK standard POLY(STYRENE) (Product of TOSOH CORPORATION)

[0163] · Weight average molecular weight Mwc of carboxyl group-containing copolymer

[0164] To 10 mg of DMAc, 10 mg of the vinylidene fluoride copolymer prepared in each example and comparative example, 2 mg of 1-bromomethylpyrene, and 2 mg of potassium carbonate were added, and the dissolution and reaction were carried out for 3 hours while stirring in a constant temperature shaking bath at 50°C, and the potassium carbonate was removed using a 0.45 μm filter. In this way, the carboxyl groups of the carboxyl group-containing copolymer in the vinylidene fluoride copolymer were labeled with 1-bromomethylpyrene.

[0165] The weight-average molecular weight Mwc of a carboxyl group-containing copolymer (a polymer that absorbs light at a wavelength of 345 nm) containing a vinylidene fluoride copolymer labeled with 1-bromomethylpyrene was determined using a UV-vis detector (UV-4075 manufactured by Nihon Bunko Co., Ltd.). Except for the detector, the measurement was performed under the same conditions as the above Mwa. The detection wavelength was set to 345 nm, and the weight-average molecular weight Mwc of the carboxyl group-containing copolymer was determined. This was performed three times, and the average value was taken as Mwc.

[0166] · Measurement of adsorption rate for aluminum oxide

[0167] For the vinylidene fluoride copolymers prepared in each example and comparative example, the adsorption rate for aluminum oxide was determined by the following method. The results are shown in Tables 1 and 2.

[0168] (i) An N, N-dimethylacetamide (DMAc) solution with a vinylidene fluoride copolymer concentration of 1 g / L was prepared.

[0169] (ii) Gel penetration chromatography (GPC) was performed on the DMAc solution prepared in (i), and the peak area AR1 derived from the vinylidene fluoride copolymer was calculated by detecting the differential refractive index (RI). The device configuration and measurement method were carried out under the same conditions as the weight-average molecular weight Mwa of the vinylidene fluoride copolymer.

[0170] (iii) 0.8 g of aluminum oxide (product of SUMITOMO CHEMICAL COMPANY, LIMITED, AKP3000: BET specific surface area 4.4 m²) to 5 g of the DMAc solution prepared in (i) 2 Added ( / g), stirred for 2 hours, and then left to stand for 16 hours.

[0171] (iv) The supernatant of the DMAc solution was collected after settling in (iii), and solid-liquid separation was performed by centrifugation.

[0172] (v) GPC was performed on the separated solution, and the peak area AR2 derived from the vinylidene fluoride copolymer was calculated by differential refractive index detection. The device configuration and measurement method were carried out in the same manner as above.

[0173] (vi) From the areas AR1 and AR2 obtained in (ii) and (v) above, the adsorption rate was calculated based on the following equation (I). This was performed three times, and the average value was taken as the adsorption rate.

[0174] Adsorption rate = (AR1 - AR2) / AR1 × 100 (I)

[0175] ·Slurry viscosity

[0176] As the slurry viscosity of the electrode mixture prepared in the examples and comparative examples, the value immediately after preparation of the electrode mixture was measured for each.

[0177] Specifically, the viscosity of the electrode mixture was measured immediately after preparation. The electrode mixture immediately after preparation was introduced into an E-type viscometer (RE-215R type viscometer manufactured by Toki Sangyo Co., Ltd., rotor 3°×R14). After maintaining a warming period of 60 seconds at 25°C within the device, a shear rate of 1 s -1 The rotor was rotated, and the viscosity 120 seconds after the start of rotor rotation was determined as the slurry viscosity.

[0178] · Peel strength

[0179] The electrode mixtures prepared in the examples and comparative examples were coated onto a 16 μm thick aluminum foil using a bar coater and dried at 110°C for 30 minutes, resulting in a weight per unit area of ​​160 g / cm² 2 A single-sided coated electrode was obtained. The obtained single-sided coated electrode was cut to a length of 70 mm and a width of 20 mm, and the peel strength between the aluminum foil and the composite layer was evaluated. Specifically, the upper surface of the formed composite layer was bonded to a thick plastic plate (made of acrylic resin, thickness 5 mm), and a 90° peel test was performed at a head speed of 10 mm / min using a tensile testing machine (Single-column type material testing machine STA-1150 manufactured by ORIENTEC CORPORATION) in accordance with JIS K6854-1. In addition, the measurement environment was set to a control temperature of 25℃ and a dew point of -20℃.

[0180] (Example 1)

[0181] [Preparation of Vinylidene Fluoride Copolymer (Electrode Binder)]

[0182] 1240 g of ion-exchanged water as a dispersion medium, 0.4 g of METOLOSE SM-100 (manufactured by Shin-Etsu Chemical Co., Ltd.) as a cellulose-based suspending agent, 2.0 g of acryloyloxypropyl succinic acid (APS), 0.6 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 0.72 g of ethyl acetate as a chain transfer agent, and 400 g of vinylidene fluoride were added to an autoclave with a net capacity of 2 liters, and the temperature was raised to 45°C over 2 hours. While maintaining the temperature at 45°C, the reaction was continued until the pressure inside the system was lowered to 1.5 MPaG.

[0183] After the polymerization was completed, the polymer slurry was heat-treated at 95°C for 60 minutes, dehydrated, washed with water, and dried again at 80°C for 20 hours to obtain a powder of a vinylidene fluoride copolymer, which is a copolymer of vinylidene fluoride (VDF) and APS (binder for electrodes).

[0184] The amount of vinyl compound having a carboxyl group introduced 1 Calculated by H-NMR measurement. Table 1 shows the amount of vinyl compound introduced in the vinylidene fluoride copolymer, inherent viscosity, weight average molecular weight Mwa, and the weight average molecular weight Mwc of the carboxyl group-containing copolymer, as well as the adsorption rate for aluminum oxide. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 4 mass% and used as a binder solution.

[0185] [Preparation of Electrode Mixture]

[0186] LFP (carbon coating amount: 1.4%, average particle diameter D50: 4 μm) was used as the electrode active material, carbon nanotubes (CNT: Cnao product LB107-44) were used as the conductivity aid, and NMP was used as the dispersion medium. Then, the above-mentioned vinylidene fluoride copolymer was mixed with LFP and CNT to prepare an electrode composite by adjusting the amount of NMP so that the slurry viscosity was 8,000 to 30,000 mPa·sec at 25°C and a shear rate of 1 / sec using an E-type viscometer. The mass ratio of LFP, CNT, and VDF in the obtained electrode composite was 100:2:2.5, and the solid content concentration was 52.0 mass%. The slurry viscosity at this time is shown in Table 1.

[0187] [Manufacturing of Electrodes]

[0188] The obtained electrode mixture was applied onto a current collector (carbon-coated aluminum foil with a thickness of 16 μm) using a bar coater. This was dried in a constant temperature bath under a nitrogen atmosphere at 110°C for 30 minutes, so that the weight per unit area of ​​the dried mixture was 160 g / m² 2 I fabricated an electrode.

[0189] (Comparative Example 1)

[0190] 1143 g of ion-exchanged water as a dispersion medium, 0.21 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 0.13 g of APS, 2.10 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, and 420 g of vinylidene fluoride were added to an autoclave with a net capacity of 2 liters, and the temperature was raised to 26°C over 55 minutes. While maintaining the temperature at 26°C, 0.92 g of an aqueous solution of APS with a concentration of 5 wt% was added over 4.3 hours starting 2 hours after the start of the temperature increase. From the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the temperature increase, the temperature was raised to 40°C over 120 minutes. The reaction was continued while maintaining the temperature at 40℃ until the pressure in the system dropped to 1.3 MPaG.

[0191] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer was obtained (binder for electrodes).

[0192] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 4 mass% and used as a binder solution.

[0193] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 1. However, the viscosity of the slurry of the electrode mixture using the vinylidene fluoride copolymer was high, and due to poor dispersion, protrusions occurred during electrode fabrication, making it difficult to achieve a uniform coating.

[0194] (Example 2)

[0195] Polymerization and post-polymerization treatment were carried out in the same manner as in Example 1, except that 1.40 g of a diisopropyl peroxydicarbonate-HFE-347pc-f solution with a polymerization initiator concentration of 50 wt% and 0.80 g of ethyl acetate were added, to obtain a powder of vinylidene fluoride copolymer (electrode binder).

[0196] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 5 mass% and used as a binder solution.

[0197] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 1, except that the solid content concentration of the electrode mixture was 55.0 mass%.

[0198] (Comparative Example 2)

[0199] Polymerization and post-polymerization treatment were carried out in the same manner as Comparative Example 1, except that 0.07 g of APS and 3.15 g of a diisopropyl peroxydicarbonate-HFE-347pc-f solution with a polymerization initiator concentration of 50 wt% were added before the start of heating, and 0.77 g of an aqueous APS solution with a concentration of 5 wt% was added over 4.3 hours starting 2 hours after the start of heating, in terms of solute equivalent, to obtain a powder of vinylidene fluoride copolymer (electrode binder).

[0200] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained.

[0201] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 5 mass% and used as a binder solution.

[0202] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 2 above.

[0203] (Example 3)

[0204] Polymerization and post-polymerization treatment were carried out in the same manner as in Example 2, except that the amount of APS added was 2.12 g and the amount of ethyl acetate added was 1.60 g, and a powder of vinylidene fluoride copolymer (electrode binder) was obtained.

[0205] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a mass of 6% and used as a binder solution.

[0206] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 1, except that the solid content concentration of the electrode mixture was 58.5 mass%.

[0207] (Comparative Example 3)

[0208] In an autoclave with a net capacity of 2 liters, 1085 g of ion-exchanged water as a dispersion medium, 0.21 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 0.13 g of APS, 2.12 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 1.70 g of ethyl acetate as a chain transfer agent, and 424 g of vinylidene fluoride were added, and the temperature was raised to 26°C over 55 minutes. While maintaining the temperature at 26°C, 2.12 g of an aqueous solution of APS with a concentration of 5 wt% was added over 12 hours, starting 2 hours after the start of the temperature increase, in terms of solute. From the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the temperature increase, the temperature was raised to 40°C over 180 minutes. The reaction was continued while maintaining the temperature at 40℃ until the pressure in the system dropped to 1.3 MPaG.

[0209] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained. The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 6 mass% and used as a binder solution.

[0210] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 3 above. However, the viscosity of the slurry of the electrode mixture using the vinylidene fluoride copolymer was high, making it impossible to measure the viscosity.

[0211] (Example 4)

[0212] In an autoclave with a net capacity of 2 liters, 1024 g of ion-exchanged water as a dispersion medium, 0.6 g of metolose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 0.04 g of APS, 4.80 g of a dinormal propyl peroxydicarbonate-methanol solution with a polymerization initiator concentration of 50 wt%, 1.96 g of ethyl acetate as a chain transfer agent, and 400 g of vinylidene fluoride were added, and the temperature was raised to 26°C over 55 minutes. The temperature was maintained at 26°C, and from the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the heating process, the temperature was raised to 55°C over 60 minutes. During this time, 3.96 g of an aqueous APS solution with a concentration of 5 wt% was added in terms of solute. The reaction was continued while maintaining the temperature at 55℃ until the pressure in the system dropped to 1.3 MPaG.

[0213] By processing the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained. The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution. Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 1, except that the mass ratio of LFP, CNT, and PVDF in the electrode mixture was 100:2:4 and the solid content concentration was 59.0 mass%.

[0214] (Example 5)

[0215] In an autoclave with a net capacity of 2 liters, 1034 g of ion-exchanged water as a dispersion medium, 0.47 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 6.58 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 15.09 g of ethyl acetate as a chain transfer agent, and 470 g of vinylidene fluoride were added, and the temperature was raised to 26°C over a period of 55 minutes. The temperature was maintained at 26°C, and from the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the heating process, the temperature was raised to 45°C over a period of 127 minutes. During this time, 2.35 g of an aqueous APS solution with a concentration of 5 wt% was added in terms of solute. The reaction was continued while maintaining the temperature at 45°C until the pressure in the system was reduced to 1.3 MPaG. By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (electrode binder) was obtained.

[0216] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution.

[0217] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 4 above.

[0218] (Example 6)

[0219] Polymerization and post-polymerization treatment were carried out in the same manner as in Example 4, except that the amount of acrylic acid (AA) added instead of APS was 1.20 g, the amount of diisopropyl peroxydicarbonate-HFE-347pc-f solution with a polymerization initiator concentration of 50 wt% was 2.48 g, and the amount of ethyl acetate as a chain transfer agent was 2.60 g, thereby obtaining a powder of vinylidene fluoride copolymer (electrode binder).

[0220] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained.

[0221] In the evaluation of the vinylidene fluoride copolymer, the amount of vinyl compound having a carboxyl group introduced was calculated by neutralization titration measurement, except that the procedure was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution.

[0222] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 4 above.

[0223] (Example 7)

[0224] 1010 g of ion-exchanged water as a dispersion medium, 0.21 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 2.10 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 6.30 g of ethyl acetate as a chain transfer agent, and 420 g of vinylidene fluoride were added to an autoclave with a net capacity of 2 liters, and the temperature was raised to 28°C over 65 minutes. While maintaining the temperature at 28°C, 0.21 g of an aqueous APS solution with a concentration of 1 wt% was added over 2 hours, starting 2 hours after the start of the temperature increase, in terms of solute equivalent. After the addition, the temperature was raised to 40°C over 180 minutes. The reaction was continued while maintaining the temperature at 40℃ until the pressure in the system dropped to 1.3 MPaG.

[0225] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained.

[0226] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution.

[0227] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 4 above.

[0228] (Comparative Example 4)

[0229] In an autoclave with a net capacity of 2 liters, 1085 g of ion-exchanged water as a dispersion medium, 0.21 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) and 0.21 g of APS as cellulose-based suspending agents, 5.09 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 9.33 g of ethyl acetate and 424 g of vinylidene fluoride as chain transfer agents were added, and the temperature was raised to 26°C over 55 minutes. While maintaining the temperature at 26°C, 4.03 g of an aqueous solution of APS with a concentration of 5 wt% was added over 18 hours, starting 2 hours after the start of the temperature increase. From the point when the pressure decreased by 0.2 MPaG from the pressure at the end of the temperature increase, the temperature was raised to 40°C over 180 minutes. The reaction was continued while maintaining the temperature at 40℃ until the pressure in the system dropped to 1.3 MPaG.

[0230] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (binder for electrodes) was obtained.

[0231] The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution.

[0232] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 4 above.

[0233] (Comparative Example 5)

[0234] In an autoclave with a net capacity of 2 liters, 1010 g of ion-exchanged water as a dispersion medium, 0.21 g of metholose SM-100 (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.) as a cellulose-based suspending agent, 2.94 g of a solution of diisopropyl peroxydicarbonate-HFE-347pc-f with a polymerization initiator concentration of 50 wt%, 2.94 g of ethyl acetate as a chain transfer agent, and 420 g of vinylidene fluoride were added, and the temperature was raised to 24°C over 55 minutes. While maintaining the temperature at 24°C, 0.21 g of an aqueous APS solution with a concentration of 1 wt% was added over 2 hours, starting 2 hours after the start of the temperature increase (in terms of solute). After the addition, the temperature was raised to 52°C over 180 minutes. The reaction was continued while maintaining the temperature at 52℃ until the pressure in the system dropped to 2.5 MPaG.

[0235] By treating the obtained polymer slurry in the same manner as in Example 1, a powder of vinylidene fluoride copolymer (electrode binder) was obtained. The evaluation of the vinylidene fluoride copolymer was carried out in the same manner as in Example 1. Then, the vinylidene fluoride copolymer was dissolved in NMP to a concentration of 13 mass% and used as a binder solution.

[0236] Using the vinylidene fluoride copolymer, an electrode mixture and an electrode were prepared in the same manner as in Example 4 above.

[0237] (result)

[0238]

[0239]

[0240] As shown in the table above, when the weight average molecular weight Mwc of the carboxyl group-containing copolymer is 1.3 million or less and the adsorption rate is greater than 0% and less than 30%, the slurry viscosity is lower and the peel strength is at the same level compared to the comparative example under the same conditions as the slurry composition and solid content concentration.

[0241] In addition, if the adsorption rate is greater than 0% and less than or equal to 60%, and Mwc is less than 3.4 relative to Mwa, and Mwc / Mwa < 0.30 / adsorption rate, the slurry viscosity is lower and the peel strength is at the same level compared to a comparative example with the same conditions as the slurry composition and solid content concentration.

[0242] This application claims priority based on Patent Application No. 2024-056522 filed on March 29, 2024. All contents described in the specification of said application are incorporated by reference into this specification.

[0243] Industrial applicability

[0244] According to the present invention, an electrode binder comprising a vinylidene fluoride copolymer is provided, which has excellent adhesion to a current collector and the like, and is also difficult to thicken the electrode composite even when lithium iron phosphate is used as the electrode active material. The electrode binder is very useful in the field of manufacturing various batteries.

Claims

Claim 1 An electrode binder comprising a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, wherein the vinylidene fluoride copolymer is modified with a labeling material composed of 1-bromomethylpyrene, and when the weight-average molecular weight of the carboxyl-containing vinylidene fluoride copolymer absorbing light of a wavelength of 345 nm is specified, the weight-average molecular weight is 1.3 million or less, and the adsorption rate obtained by the following method is greater than 0% and less than or equal to 30%. (Method for specifying the adsorption rate) (i) Prepare an N,N-dimethylacetamide solution having a concentration of vinylidene fluoride copolymer of 1 g / L. (ii) Perform gel permeation chromatography on the N,N-dimethylacetamide solution and calculate the peak area AR1 derived from the vinylidene fluoride copolymer by differential refractive index detection. (iii) The N, 5 g of N-dimethylacetamide solution, with a BET specific surface area of ​​4 m² 2 / g or more than 5 m 2 (iv) Add 0.8 g of aluminum oxide at a concentration of 1 / g or less, stir for 2 hours, and then let stand for 16 hours. (iv) After standing, collect the supernatant of the above N,N-dimethylacetamide solution and perform solid-liquid separation by centrifugation. (v) Perform gel permeation chromatography on the separated solution and calculate the peak area AR2 derived from the above vinylidene fluoride copolymer by differential refractive index detection. (vi) Calculate the adsorption rate based on the following Equation (I). Perform this three times, and the average value is taken as the adsorption rate. Adsorption rate = (AR1 - AR2) / AR1 × 100 (I) Claim 2 An electrode binder according to claim 1, wherein the adsorption rate is 1% or more and 20% or less. Claim 3 An electrode binder comprising a vinylidene fluoride copolymer having a constituent unit derived from vinylidene fluoride and a constituent unit derived from a vinyl compound having a carboxyl group, wherein the adsorption rate obtained by the following method is greater than 0% and less than or equal to 60%, and when the vinylidene fluoride copolymer is modified with a labeling material consisting of 1-bromomethylpyrene to determine the weight average molecular weight Mwc of the carboxyl group-containing vinylidene fluoride copolymer that absorbs light of a wavelength of 345 nm, said Mwc is less than 3.4 relative to the weight average molecular weight Mwa of said vinylidene fluoride copolymer, and said Mwc, said Mwa, and said adsorption rate satisfy the following formula (II), Mwc / Mwa < 0.30 / adsorption rate (II) electrode binder. (Method for determining adsorption rate) (i) Prepare an N,N-dimethylacetamide solution having a concentration of vinylidene fluoride copolymer of 1 g / L. (ii) Gel permeation chromatography is performed on the above N,N-dimethylacetamide solution, and the peak area AR1 derived from the above vinylidene fluoride copolymer is calculated by differential refractive index detection. (iii) 5 g of the above N,N-dimethylacetamide solution, with a BET specific surface area of ​​4 m² 2 / g or more than 5 m 2 (iv) Add 0.8 g of aluminum oxide at a concentration of 1 / g or less, stir for 2 hours, and then let stand for 16 hours. (iv) After standing, collect the supernatant of the N,N-dimethylacetamide solution and perform solid-liquid separation by centrifugation. (v) Perform gel permeation chromatography on the separated solution and calculate the peak area AR2 derived from the vinylidene fluoride copolymer by differential refractive index detection. (vi) Calculate the adsorption rate based on the following equation (I). Perform this three times, and the average value is taken as the adsorption rate. Adsorption rate = (AR1 - AR2) / AR1 × 100 (I) Claim 4 An electrode binder according to any one of claims 1 to 3, wherein, with respect to 100.0 mol% of the total constituent units of the vinylidene fluoride copolymer, the amount of constituent units derived from vinylidene fluoride is 90.0 mol% or more, and the amount of constituent units derived from the vinyl compound is 0.01 mol% or more and 0.80 mol% or less. Claim 5 An electrode binder according to any one of claims 1 to 3, wherein the vinyl compound is a compound represented by the following general formula (1). [Chem 1] (In general formula (1), R 1 , R 2 , R 3 Each represents independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents an atomic group) Claim 6 An electrode binder according to any one of claims 1 to 3, wherein the vinyl compound is a compound represented by the following general formula (1). [Chem 2] (In general formula (1), R 1 , R 2 , R 3 Each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and X represents a hydroxyl group or -Y-COOH (Y represents a divalent atomic group having a molecular weight of 500 or less, containing either an oxygen atom or a nitrogen atom and having 1 to 10 atoms in the main chain). Claim 7 An electrode composite comprising an electrode binder and an electrode active material as described in any one of claims 1 to 3. Claim 8 An electrode comprising a solid portion of an electrode binder described in any one of paragraphs 1 to 3. Claim 9 A battery comprising the electrode described in paragraph 8.