Back sealing of a semiconductor substrate
A single-chamber, single-temperature process using PECVD forms a SiO2 and amorphous silicon stack on semiconductor substrates, addressing inefficiencies in conventional auto-doping mitigation methods by enhancing back sealing and reducing complexity and cost.
Patent Information
- Application Number
- KR1020267033742
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-13
- Filing Date
- 2025-03-07
- Publication Date
- 2026-11-09
AI Technical Summary
Conventional methods for mitigating auto-doping in semiconductor substrates during epitaxial deposition processes are complex, costly, and inefficient, requiring multiple temperature changes and substrate repositioning, leading to high costs and low efficiency.
A method and apparatus for depositing a back sealing layer on semiconductor substrates using a single process chamber and temperature, employing PECVD to form a stack of SiO2 and amorphous silicon layers without flipping the substrate, followed by optional annealing to crystallize the amorphous silicon, thereby forming a polycrystalline silicon layer.
This approach reduces complexity and cost, increases efficiency, and ensures excellent adhesion and smoothness of the back sealing layer, preventing dopant diffusion and migration, while allowing for simultaneous processing of multiple substrates.
Smart Images

Figure PCT00007_ABST
Abstract
Description
Background Technology
[0001] In semiconductor processing, auto-doping is a serious problem that occurs in epitaxial deposition processes. During this process, doped heteroatoms may diffuse from the back side of the substrate or migrate around the edges of the substrate, causing unintended over-doping on the edges and front side of the substrate. Current solutions for mitigating auto-doping involve extensive procedures involving various temperatures, processes, and substrate positions, and entail complex procedures requiring repositioning (including flipping), resulting in high costs and low efficiency. A new solution using a tool for mitigating auto-doping would be desirable, as it eliminates much of the complexity and even improves other modes of tool usage.
[0002] The description of the background art provided in this specification is intended for the purpose of generally presenting the context of the disclosure. The work of the inventors named in this specification to the extent described in this background art section, as well as aspects of the technology that may not otherwise be recognized as prior art at the time of filing, are not explicitly or implicitly recognized as prior art to the disclosure.
[0003] Citation as a reference
[0004] The PCT application form has been filed concurrently with this specification as part of this application. Each application claiming priority or the benefit of priority, as identified in the PCT application form filed concurrently with this application, is incorporated herein by reference in its entirety for all purposes.
[0005] In one aspect of the present disclosure, an apparatus configured for back sealing of a semiconductor substrate is disclosed. In some embodiments, the apparatus comprises: one or more process chambers; a showerhead configured to deliver one or more process gases to the back surface of at least one semiconductor substrate among the one or more process chambers; and a first set of one or more process gases coupled to the showerhead and one or more process chambers and causing delivery to a first process chamber having a semiconductor substrate; applying a first process temperature of 200 to 400 °C in the presence of plasma to form a silicon oxide (SiO2) layer on the back surface of the semiconductor substrate; and causing delivery to a second set of one or more process gases to the first process chamber; The controller may also be configured to apply a first process temperature of 200 to 400 °C in the presence of plasma to form an amorphous silicon layer on a SiO2 layer on the back surface of a semiconductor substrate to collectively form a stack of materials that seal the back surface of the semiconductor substrate and mitigate the diffusion of dopants from the semiconductor substrate. In some embodiments, the controller may be further configured to apply a second process temperature of at least 700 °C to cause an annealing process to occur following the formation of the amorphous silicon layer, and the annealing process includes a step of inducing crystallization of the amorphous silicon layer to form a polycrystalline silicon layer to collectively form a stack of materials that seal the back surface of the semiconductor substrate.
[0006] In another aspect of the present disclosure, an apparatus is disclosed. In some embodiments, the apparatus may include: a first process chamber configured to receive a semiconductor substrate; a showerhead configured to deliver one or more process gases to the back surface of the semiconductor substrate of the first process chamber; and a controller coupled to at least the showerhead and one or more process chambers and configured to induce the delivery of one or more first sets of process gases to the first process chamber having the semiconductor substrate; to apply a first process temperature of 200 to 400 °C in the presence of plasma to form an amorphous silicon layer on the back surface of the semiconductor substrate; to induce the delivery of one or more second sets of process gases to the first process chamber; and to apply a first process temperature of 200 to 400 °C in the presence of plasma to form a silicon oxide (SiO2) layer on the amorphous silicon layer on the back surface of the semiconductor substrate to collectively form a stack of materials that seal the back surface of the semiconductor substrate and mitigate the diffusion of dopants from the semiconductor substrate. In some embodiments, the controller may be further configured to apply a second process temperature of at least 700°C to cause an annealing process to occur following the formation of the SiO2 layer, and the annealing process includes the step of causing crystallization of an amorphous silicon layer to form a polycrystalline silicon layer to collectively form a stack of materials sealing the back surface of the semiconductor substrate.
[0007] In another aspect of the present disclosure, a method for sealing the back surface of a semiconductor substrate is disclosed. In some embodiments, the method may include the step of causing the delivery of one or more process gases of a first set to a first process chamber of a deposition apparatus, wherein the first process chamber has a semiconductor substrate disposed therein; the step of applying a first process temperature in the presence of plasma to form a first material layer on the back surface of the semiconductor substrate; the step of causing the delivery of one or more process gases of a second set to the first process chamber; and the step of applying a first process temperature in the presence of plasma to form a second material layer on the first material layer on the back surface of the semiconductor substrate to collectively form a stack of materials that seal the back surface of the semiconductor substrate and mitigate the diffusion of dopants from the semiconductor substrate. In some embodiments, the method may further include the step of applying a second process temperature to cause an annealing process to occur following the formation of a second material layer, and the annealing process includes causing crystallization of the first material layer or the second material layer to collectively form a stack of materials sealing the back surface of the semiconductor substrate.
[0008] These features and other features of the disclosed embodiments will be described in detail below with reference to the associated drawings. Brief explanation of the drawing
[0009] Figures 1a and 1b illustrate exemplary doping profiles in which an epitaxial process is applied to a semiconductor substrate to induce epitaxial growth of a film. Figure 2 illustrates an exemplary process flow of a conventional approach to depositing a back sealing layer without back deposition. FIG. 3 illustrates an exemplary process flow of an approach to depositing a back sealing layer using back deposition according to some embodiments. FIG. 4 illustrates an example of an enhanced back sealing layer formed on the surface of a semiconductor substrate according to some embodiments. FIG. 5 illustrates another exemplary process flow of an approach to depositing a back sealing layer using back deposition according to some embodiments. FIG. 6 is a flowchart of an example of a back sealing method for a semiconductor substrate according to some embodiments. FIGS. 7 and 8 illustrate block diagrams of exemplary substrate processing systems according to some embodiments of the present specification. FIG. 9a illustrates an exemplary cross-sectional view of the edge of a shower-pedestal. FIG. 9b illustrates a plan view of an exemplary carrier ring. FIG. 10 is a cross-sectional view of a processing system for depositing a film on the back surface of a semiconductor substrate according to some embodiments of the present specification. FIG. 11 illustrates a schematic diagram of an exemplary process system that may be used to perform the methods described herein. Specific details for implementing the invention
[0010] The following terms are used throughout this specification:
[0011] The terms "semiconductor wafer," "wafer," "substrate," "wafer substrate," and "partially fabricated integrated circuit" may be used interchangeably. Those skilled in the art understand that the term "partially fabricated integrated circuit" may refer to a semiconductor wafer during any of the many stages of integrated circuit fabrication. Wafers or substrates used in the semiconductor device industry typically have a diameter of 200 mm, 300 mm, or 450 mm. Examples of wafer materials include silicon (Si), gallium arsenide (GaAs), and silicon germanium (SiGe). In addition to semiconductor wafers, other workpieces that may take advantage of the disclosed embodiments include various articles such as printed circuit boards, magnetic recording media, magnetic recording sensors, mirrors, optical elements, display devices or components such as backplanes for pixelated display devices, flat panel displays, micro-mechanical devices, etc. The workpieces may be of various shapes, sizes, and materials.
[0012] As used herein, “semiconductor device manufacturing operation” refers to an operation performed during the manufacturing of semiconductor devices. Typically, the entire manufacturing process comprises a plurality of semiconductor device manufacturing operations, each performed in its own semiconductor manufacturing tool, such as a plasma reactor, an electroplating cell, a chemical mechanical planarization tool, a wet etching tool, etc. Categories of semiconductor device manufacturing operations include subtractive processes, such as etching processes and planarization processes, and material additive processes, such as deposition processes (e.g., physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), electrochemical deposition, electroless deposition). In the context of etching processes, substrate etching processes include processes for etching a mask layer, or more generally, processes for etching any layer of material previously deposited and / or otherwise existing on a substrate surface. This etching process can also etch a stack of layers on the substrate.
[0013] In the context of the present disclosure, “epitaxy” or “epitaxial” may refer to an approach to manufacturing for creating crystalline layers for constructing semiconductor devices. “Epitaxial process,” “epitaxial deposition process,” or “epitaxial growth process” may refer to a process comprising forming layers of material (e.g., films) under high temperature, and may be an example of the aforementioned semiconductor device manufacturing operation.
[0014] "Fabrication equipment" refers to equipment where the fabrication process takes place. Fabrication equipment often has a process chamber where the workpiece is located during processing. Typically, when in use, fabrication equipment performs one or more semiconductor device manufacturing operations. Examples of fabrication equipment for semiconductor device manufacturing include deposition reactors such as electroplating cells, physical vapor deposition reactors, chemical vapor deposition reactors, and atomic layer deposition reactors, and subtractive process reactors such as dry etching reactors (e.g., chemical etching reactors and / or physical etching reactors), wet etching reactors, and ashers.
[0015] "Silicon oxide" includes integer values of x and y and non-integer values of x and y, Si x O y It is referred to herein as including any and all stoichiometric possibilities for. For example, "silicon oxide" is defined by the chemical formula SiO₂. n Compounds having, wherein 1 < n < It is 2, where n can be an integer or a non-integer value. "Silicon oxide" is SiO 1.8 It may include sub-stoichiometric compounds such as. "Silicon oxide" also includes silicon dioxide (SiO2) and silicon monooxide (SiO). "Silicon oxide" also includes both natural and synthetic variations, and includes any and all crystalline and molecular structures including tetrahedral coordination of oxygen atoms surrounding a central silicon atom. "Silicon oxide" also includes amorphous silicon oxide and silicates.
[0016] In various approaches, the materials of stacks of layers (e.g., thin films) may be deposited via chemical vapor deposition (CVD) techniques such as plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), atmospheric pressure chemical vapor deposition (APCVD), metal organic CVD (MOCVD), atomic layer deposition (ALD), and plasma enhanced atomic layer deposition (PEALD), or via direct metal deposition (DMD), etc. These examples are not intended to be limiting. Different deposition techniques may be used at different ends. For example, deposition may be useful whenever wafer stress and / or bowing is induced due to the material present on the front surface of the wafer. In particular, different deposition techniques may be associated with or subject to different temperatures, pressures, precursors, or other deposition processes, conditions, or recipes. For example, specific deposition techniques may overlap within the temperature ranges in which they can be used, which may be advantageously used to strategically deposit multiple layers at once or only specific layers.
[0017] Semiconductor substrates may be doped with elements (e.g., phosphorus atoms) to improve the substrate's conductivity. More specifically, in silicon-based wafers, the conductivity of silicon can be increased using these dopants. Many downstream applications or uses of wafers may involve high temperatures, such as forming an epitaxial growth layer on the wafer surface. However, high temperatures can cause dopants to diffuse out of the wafer. This is a problem well known to the semiconductor industry as "auto-doping."
[0018] One way to prevent dopants from being released is to deposit a back sealing layer on the back side of the wafer. Generally, silicon-based films, such as silicon oxide (SiO2), silicon nitride (SiN), or polysilicon films, can be deposited to seal the back side of the wafer. However, conventional processes for achieving the deposition of a back sealing layer are costly, complex, lengthy, and inefficient. In particular, multiple deposition techniques requiring different wafer temperatures and orientations (with the back side of the wafer facing down and up through the processes) increase the complexity and inefficiency.
[0019] To address this problem in conventional approaches, methods and apparatus for depositing an enhanced back sealing layer directly on the back surface of a wafer are described herein. These approaches do not require flipping the wafer between different deposition techniques. In practice, the wafer may remain fixed within the processing environment (e.g., a process chamber or a station of the deposition apparatus). In some embodiments, the enhanced back sealing layer may comprise a stack of SiO2 and amorphous silicon (a-Si), which can be formed in a single process using a deposition apparatus configured for back deposition using PECVD at the same process temperature, as described in more detail herein. This simplified approach advantageously reduces the associated cost and time and increases the efficiency of providing a back sealing layer to the wafer.
[0020] Wafer back sealing
[0021] FIG. 1a illustrates an exemplary doping profile (100) in which an epitaxial process is applied to a semiconductor substrate (102) to induce epitaxial growth of a film (104). In some examples, the semiconductor substrate (102) may be a doped silicon-based wafer, and the film (104) may be formed on the front surface of the semiconductor substrate (102) as a result of an epitaxial deposition process, or may be in the process of being formed. However, during this epitaxial deposition process, dopants (106), such as doped heteroatoms, may diffuse from the back surface of the semiconductor substrate (102) to the opposite surface of the front surface. This diffusion may migrate and affect along the edges and bevels of the semiconductor substrate (102), which also causes unintended overdoping (108) on the wafer edges and front surface, known as self-doping. Therefore, the exemplary doping profile (100) is a harmful doping profile that requires back sealing to mitigate self-doping, which is generally performed before the epitaxial process.
[0022] To this end, in some approaches, a silicon-based film may be deposited on the back surface of a semiconductor substrate (102). Examples of silicon-based films may include silicon oxide (e.g., SiO2), low-temperature oxide (LTO, which may also be referred to as SiO2), silicon nitride (e.g., SiN), or polycrystalline silicon (also referred to as poly-Si, polysilicon, or semicrystalline silicon). In addition, the deposited material may be a combination of different films and may form a stack of layers or materials. An exemplary stack may be a stack of SiO2 and poly-Si. The deposited film or stack may seal the dopants (106) within the semiconductor substrate (102) and prevent excessive diffusion and migration of the dopants (106).
[0023] FIG. 1b illustrates another exemplary doping profile (120) in which an epitaxial process is applied to a semiconductor substrate (102) to induce epitaxial growth of a film (104). In this example, a back sealing layer (124) is deposited on the back surface of the semiconductor substrate (102). A stack of SiO2 and poly-Si films deposited on the back surface of the semiconductor substrate (102) may be an example of the back sealing layer (124). This mitigates the self-doping problem by preventing the diffusion and migration of dopants (106).
[0024] However, current techniques for depositing a back sealing layer (124) are complex, expensive, and inefficient. In one example of such current techniques, illustrated in FIG. 2, a 5-step process flow is required to deposit the back sealing layer (124) on the back.
[0025] FIG. 2 illustrates an exemplary process flow (200) of a conventional approach for depositing a back sealing layer without back deposition. In step (202), the semiconductor substrate (201) may be provided so that its front side faces upward. In step (204), the semiconductor substrate (201) may be flipped so that its front side faces downward. In step (206), the deposition process may be applied to the semiconductor substrate (201) to deposit a silicon oxide layer on the back side of the semiconductor substrate (201) from above (since the front side faces downward).
[0026] Referring again to FIG. 2, an example of a deposition process that may be used in step (206) is APCVD, and a silicon oxide precursor introduced at a uniform rate into an atmospheric pressure processing environment (e.g., a process chamber) and the application of a first process temperature to the environment (e.g., 250 to 400 °C) may cause the deposition of a first layer. Another example of a deposition process that may be used in step (206) is PECVD with the introduction of a silicon oxide precursor. The first layer may be a silicon oxide (SiO2) layer deposited on the back surface of a semiconductor substrate (201), as illustrated in FIG. 2.
[0027] In step (208), another deposition process may occur to deposit a layer on both sides of the semiconductor substrate (201). For example, LPCVD may be used with a silicon-based precursor at a second process temperature (e.g., 600 to 700 °C) to deposit a polysilicon (poly-Si) layer on the front and back sides.
[0028] In step (210), the semiconductor substrate (201) may be flipped back so that the front face again faces upward. In step (212), the front face of the semiconductor substrate (201) may be polished to remove the poly-Si layer from the front face. Thus, the exemplary process flow (200) may produce a wafer having a back sealing layer, wherein the back sealing layer comprises a silicon oxide layer and a poly-Si layer. Having these two layers may improve the sealing ability of the back sealing layer as opposed to having only one of the layers, but having only one of the layers may also be acceptable under some circumstances (e.g., when the epitaxial layer is not thick and fewer dopants diffuse from the back face).
[0029] However, the aforementioned conventional approach has disadvantages. These complex procedures, involving flipping and several steps, require high costs and time, and result in low efficiency. Part of the complexity of the conventional approach is that depositing the two silicon oxide and poly-Si layers requires different process temperatures (e.g., 250 to 400 °C and 600 to 700 °C). Additionally, two different deposition tools are required to deposit the two layers, which increases the complexity of the process flow, as well as the cost and process time. Furthermore, poly-Si layers deposited via LPCVD may undergo excessive crystallization (undergo) during any subsequent epitaxial steps at high process temperatures (e.g., above 1000 °C), resulting in large grain sizes and rough surfaces.
[0030] While the resulting back sealing layer can mitigate self-doping, it is evident that significant improvements can be made to reduce complexity, lower costs, and decrease process time, thereby increasing efficiency. The techniques and devices described below can address each of these issues. Furthermore, different types of layers can be deposited in different configurations (beyond SiO2 and poly-Si) to prevent some of the aforementioned problems.
[0031] FIG. 3 illustrates an exemplary process flow (300) of an approach to depositing a back sealing layer using back deposition according to some embodiments. In step (302), the semiconductor substrate (401) may be provided such that its front side faces upward.
[0032] In step (304), the deposition process may be applied to the semiconductor substrate (301) without flipping the semiconductor substrate (301). In some embodiments, the deposition process may include PECVD using a back-side deposition device (described below). This eliminates the need to flip or otherwise move the semiconductor substrate (301) because it enables the deposition of one or more layers directly on the back side of the semiconductor substrate (301).
[0033] In some approaches, the deposition process may include two consecutive deposition steps. In the first deposition step, a first layer (312) may be deposited on the back surface of a semiconductor substrate (301) in an environment suitable for PECVD (e.g., a process chamber of a back deposition apparatus). In some examples, the first layer (312) may include a silicon oxide (SiO2) film. This deposition step may involve a lower process temperature (e.g., 200 to 400 °C) compared to the process temperature used in LPCVD, which is applied to a plasma introduced into the environment to form the SiO2 film and a set of first process gases (reactive material gases, e.g., silane gas (SiH4) and nitrous oxide gas (N2O)).
[0034] In the second deposition step, following the deposition of the first layer (312) and while the front side is still facing upward, the second layer (314) may be deposited on the back side of the semiconductor substrate (301) directly above the first layer (312). The second deposition step may occur immediately after or substantially immediately after the first deposition step (e.g., within 5 seconds). This deposition step may involve a process temperature equal to the process temperature of the first deposition step (e.g., 200 to 400 °C), and a carrier gas and plasma introduced into the environment. In some examples, the second layer (314) may comprise a high-quality amorphous silicon (a-Si) film. The SiO2 film and the a-Si film may each have a predetermined thickness. For example, the SiO2 film may have a thickness of 3,000 to 5,000 Å, and the a-Si film may have a thickness of up to 12,000 Å. In some embodiments, one or both of the SiO2 film and the a-Si film may have a thickness of up to 20,000 Å. For the formation of a-Si, the chemical reaction may involve the decomposition of SiH4, and only a carrier gas may be introduced without other process gases or reactant gases. The carrier gas used in the second deposition step may be an inert gas, for example, argon (Ar), nitrogen (N2), or helium (He).
[0035] In some embodiments, the deposition of the second layer (114) may result in an enhanced back sealing layer (320) on the back surface of the semiconductor substrate (301) without any movement of the semiconductor substrate (301) during the formation of the enhanced back sealing layer (320). Thus, the enhanced back sealing layer (320) may include a SiO2+a-Si stack.
[0036] For reference, the first deposition step and the second deposition step have been described above, but it will be understood that these steps are part of a single process for producing two layers or films. That is, the process temperature may be maintained constant (e.g., 200 to 400 °C), the substrate may be maintained in a fixed state, and the only change in process conditions is the switching of the reaction material gases to form two layers on the back surface of the substrate. As described below with respect to FIG. 5, the reaction material gases may be changed to change the order of the layers formed on the back surface of the substrate.
[0037] One prominent advantage of the present disclosure is found in this specification. Two deposition steps for producing a silicon oxide (SiO2) and a-Si bilayer may be performed in the same environment or process chamber and at the same process temperature without breaking the vacuum or transporting or otherwise moving the semiconductor substrate (301). Only a change in process gases is required between the deposition steps. Since the depositions are performed directly on the back of the wafer without any front deposition occurring and without any removal or polishing of the front being required or performed, flipping is not required as in conventional approaches such as the exemplary process flow (200) of FIG. 2. In addition, there is excellent adhesion between the silicon oxide layer and the a-Si layer, which can prevent delamination or flaking of the a-Si film, which may be relatively thicker than the silicon oxide film in some cases.
[0038] Additional advantages and examples of applications include cases where a-Si may be used as a conductive layer to improve wafer chucking, for example, electrostatic chucking. In some cases, the bilayer may serve as an opaque and conductive backing layer for glass wafer processing to implement displays for extended reality (XR) (e.g., augmented reality (AR), virtual reality (VR)), mixed reality (MR)), devices and products including, for example, user devices and wearable devices. Thus, the deposition of a-Si on the semiconductor substrate (301) enables transparent glass wafer processing on wafer processing equipment (including those configured to perform CVD deposition, physical vapor deposition (PVD), or etching), and may be useful for further stabilizing or fixing it, for example, within the environment on the pedestal of the process chamber.
[0039] In some optional approaches, an annealing process may be performed in step (306). Annealing may be optional because the second layer (314) (e.g., a-Si film) alone can provide the desired results, e.g., back sealing and relaxation of self-doping. In some embodiments involving an annealing process, annealing may occur at a temperature different from the temperature used in the deposition steps, e.g., 700 °C or higher (e.g., 700 to 1100 °C). That is, the semiconductor substrate (301) having the first layer (312) and the second layer (314) may be exposed to a high temperature (e.g., 700 to 1100 °C) and may be cooled over time. Annealing may be performed in a different environment or process chamber. By this annealing process, the second layer (314) (e.g., a-Si film) may undergo crystallization and transition to a different material. In some examples, the resulting crystallized layer (316) (e.g., poly-Si film) may be formed on the SiO2 film, or the enhanced back sealing layer (320') may be formed on the back surface of the semiconductor substrate (301) without any movement of the semiconductor substrate (301) during the formation of the enhanced back sealing layer (320'). Thus, the enhanced back sealing layer (320') may comprise a SiO2+poly-Si stack. The poly-Si film may have a smaller particle size and a smoother surface than in conventional approaches such as the exemplary process flow (200) of FIG. 2, which is another advantage of the present disclosure. In wafer processing, it is generally desirable to have a smooth surface rather than a rough surface, otherwise wafer chucking on other tools and downstream processes (including lithography and etching processes) may be affected.
[0040] Accordingly, the double-layer structure of the enhanced back sealing layer (320 or 320') on the semiconductor substrate (301) may comprise (i) a first layer (312) (e.g., SiO2 film) and a second layer (314) (e.g., a-Si film) without any additional annealing process or epitaxial process, or (ii) a first layer (312) (e.g., SiO2 film) and a crystallized layer (316) (e.g., poly-Si film) produced by annealing.
[0041] Referring briefly to FIG. 4, an example of an enhanced back sealing layer (400) formed on the surface of a semiconductor substrate (401) according to some embodiments is illustrated. According to the single-process deposition approach described above for step (304), a first material layer (e.g., a SiO2 film (404)) may be deposited on the surface of the semiconductor substrate (401), and a second material layer (e.g., an a-Si film (406)) may be deposited on the first material layer. The SiO2 film (404) may have a thickness (T1) (e.g., 4500 Å in this example within the parameters mentioned above) smaller than the thickness (T2) of the a-Si (e.g., 10000 Å in this example within the parameters mentioned above). However, among the functions of the SiO2 film (404) is the promotion of the adhesion of a-Si to the semiconductor substrate (401). Thus, a thicker (T2) does not create issues of delamination or flaking of the a-Si film (406). The SiO2 film (404) may further block dopants from escaping or diffusing from the semiconductor substrate (401) and may increase the stability of the a-Si film (406) during high-temperature processes by absorbing hydrogen released from the a-Si. Furthermore, the outer surface (408) of the a-Si film (406) produced according to the disclosed embodiments after annealing is smoother (due to the smaller particle size) compared to poly-Si produced using LPCVD in a conventional approach.
[0042] Additionally, optionally, following the annealing process of step (306), other processes may be performed, such as (i) removing the semiconductor substrate (301) having an enhanced back sealing layer (320), (ii) downstream processes related to the environment (e.g., process chamber), such as process diagnostics, process control, chamber cleaning, hazardous purging, gas purging (e.g., N2 from the process chamber), or (iii) collecting data related to the semiconductor substrate (301) and / or the environment through one or more sensors, such as a spatial sensor (e.g., camera), a spectrum sensor (e.g., optical emission spectrometry (OES) sensor), and / or a transient sensor (e.g., a photodiode).
[0043] In addition, the above process can be performed simultaneously on multiple semiconductor substrates within a single process chamber or multiple process chambers of a multi-chamber deposition apparatus, which is further described below.
[0044] However, in some embodiments, the first layer (312) may include a-Si and the second layer (314) may include SiO2. That is, the materials of the first layer (312) and the second layer (314) may be flipped instead of those shown in FIG. 3.
[0045] FIG. 5 illustrates another exemplary process flow (500) of an approach to depositing a back sealing layer using back deposition according to some embodiments. Here, the process begins with step (502), in which the front side of a semiconductor substrate (501) is provided to face upward, similar to step (302).
[0046] In step (504), the deposition process may be applied to the semiconductor substrate (501) without flipping the semiconductor substrate (501). In some embodiments, the deposition process may include PECVD using a back-side deposition device (described below). This eliminates the need to flip or otherwise move the semiconductor substrate (501) because it allows for the deposition of one or more layers directly on the back side of the semiconductor substrate (501).
[0047] In some approaches, the deposition process may include two consecutive deposition steps. In the first deposition step, a first layer (512) may be deposited on the back surface of a semiconductor substrate (501) in an environment suitable for PECVD (e.g., a process chamber of a back deposition apparatus). In some examples, the first layer (512) may include an a-Si film. This deposition step may involve a lower process temperature (e.g., 200 to 400 °C) compared to the process temperature used in LPCVD, which is applied to a plasma introduced into the environment to form the a-Si film and a set of first process gases (e.g., a reactive material gas SiH4).
[0048] In a second deposition step, following the deposition of the first layer (512) and while the front side is still facing upward, a second layer (514) may be deposited on the back side of the semiconductor substrate (501) directly above the first layer (512). The second deposition step may occur immediately after or substantially immediately after the first deposition step (e.g., within 5 seconds). This deposition step may involve a process temperature equal to the process temperature of the first deposition step (e.g., 200 to 400 °C), and a second set of process gases (e.g., reactive material gases SiH4 and N2O) and plasma introduced into the environment. In some examples, the second layer (514) may comprise a SiO2 film. The SiO2 film and the a-Si film may each have a predetermined thickness, for example, up to 12,000 Å for a-Si and up to 5,000 Å for SiO2.
[0049] In some embodiments, the deposition of the second layer (514) may produce an enhanced back sealing layer (520) on the back surface of the semiconductor substrate (501) without any movement of the semiconductor substrate (501) during the formation of the enhanced back sealing layer (520). Thus, the enhanced back sealing layer (5320) may include an a-Si+SiO2 stack.
[0050] Additionally, advantageously, the two deposition steps for producing a double layer of a-Si and SiO2 may be performed in the same environment or process chamber and at the same process temperature without breaking the vacuum or transporting or otherwise moving the semiconductor substrate (501). Only a change of process gases is required between the deposition steps. Since the depositions are performed directly on the back of the wafer without any front deposition occurring and without any removal or polishing of the front being required or performed, flipping is not required as in conventional approaches such as the exemplary process flow (200) of FIG. 2.
[0051] In some selectable approaches, similar to step (306) (which may also be selectable), an annealing process may be performed in step (506). Similar to the bilayer produced according to step (304), the annealing process in step (506) may be selectable because only the first layer (512) (e.g., a-Si film) can provide the desired results, e.g., back sealing and the relaxation of self-doping. In some embodiments, annealing may occur at a temperature different from the temperature used in the deposition steps, e.g., 700 to 1100 °C, within the same environment or process chamber, and is cooled over time. Through this annealing process, the first layer (512) (e.g., a-Si film) may undergo crystallization and a transition to a different material. In some examples, the resulting crystallized layer (516) (e.g., a poly-Si film) may be formed under the SiO2 film, or the enhanced back sealing layer (520') may be formed on the back surface of the semiconductor substrate (501) without any movement of the semiconductor substrate (301) during the formation of the enhanced back sealing layer (520'). Thus, the enhanced back sealing layer (520') may include a poly-Si+SiO2 stack. In an exemplary process flow (500), the surface smoothness of the enhanced back sealing layer (520') is dependent on the surface smoothness of the outer layer, which is the second layer (514) (e.g., a SiO2 film).
[0052] Accordingly, the double-layer structure of the enhanced back sealing layer (520 or 520') on the semiconductor substrate (501) may comprise (i) a first layer (512) (e.g., a-Si film) and a second layer (514) (e.g., SiO2 film) without any additional annealing process or epitaxial process, or (ii) a crystallized layer (516) (e.g., poly-Si film) produced by annealing the second layer (514) (e.g., SiO2 film).
[0053] Optionally, other downstream processes as described may be performed following the annealing process of step (506).
[0054] In addition, the above process can be performed simultaneously on multiple semiconductor substrates within a single process chamber or multiple process chambers of a multi-chamber deposition apparatus, which is further described below.
[0055] Methods
[0056] FIG. 6 is a flowchart of an example of a back sealing method (600) of a semiconductor substrate according to some embodiments. One or more of the functions of the method (600) may be performed by or triggered by a computerized device or system. A structure for performing the functionality illustrated in one or more of the blocks shown in FIG. 6 may be performed by hardware components and / or software components of such a computerized device or system, such as a computer-readable device comprising a storage medium for storing computer-readable and / or computer-executable instructions configured to cause at least one processor device or computerized device to perform operations when executed by, for example, a controller device, a computerized system, or a processor device. A controller may be an example of a computerized device or system. A process chamber may be another example of a computerized device or system. Exemplary components of the device are illustrated in FIG. 7 through 11 and are described in more detail elsewhere in this specification.
[0057] It should also be noted that the operations of FIG. 6 do not necessarily have to be in the order shown in FIG. 6 and may be performed in any suitable order. Additionally, the process shown in FIG. 6 may include additional operations or fewer operations than those shown in FIG. 6.
[0058] In block (610), the method (600) may include the step of causing the delivery of one or more process gases of a first set to a first process chamber of a deposition apparatus, wherein the first process chamber has a semiconductor substrate disposed therein. In some embodiments, the first process chamber may be one of a plurality of process chambers or stations of the deposition apparatus, which are further described below.
[0059] In block (620), the method (600) may include the step of applying a first process temperature in the presence of plasma to form a first material layer on the back surface of a semiconductor substrate.
[0060] In some embodiments, the first material layer may include silicon oxide (SiO2).
[0061] In some embodiments, the first material layer may include amorphous silicon.
[0062] In some embodiments, the first process temperature may include a temperature of 200 to 400 ℃.
[0063] In block (630), the method (600) may include the step of causing the delivery of one or more of a second set of process gases into a first process chamber.
[0064] In some embodiments, one or more of the first set of process gases may include silane (SiH4) and nitrous oxide (N2O), and one or more of the second set of process gases may include a carrier gas. For example, these sets of gases may be used with an exemplary process flow (300).
[0065] In some embodiments, one or more of the first set of process gases may include silane (SiH4), and one or more of the second set of process gases may include SiH4 and nitrous oxide (N2O). For example, these sets of gases may be used with an exemplary process flow (500).
[0066] In block (640), the method (600) may include the step of applying a first process temperature in the presence of plasma to form a second material layer on a first material layer on the back surface of a semiconductor substrate. The first process temperature may be the same as the first process temperature in block (620) (e.g., 200 to 400 °C).
[0067] In some embodiments, the second material layer may comprise amorphous silicon. In some embodiments, the second material layer may comprise silicon oxide (SiO2).
[0068] Optionally, in block (650), the method (600) may include the step of applying a second process temperature to cause an annealing process to occur following the formation of a second material layer, and the annealing process may include causing crystallization of the first material layer or the second material layer to collectively form a stack of materials sealing the back surface of the semiconductor substrate.
[0069] In some embodiments, the first material layer may comprise a silicon oxide (SiO2) layer or film; the second material layer may comprise an amorphous silicon layer or film formed on the SiO2 film; crystallization of the first material layer or the second material layer may comprise crystallization of the amorphous silicon film into a layer or film of polycrystalline silicon; and the polycrystalline silicon film and the SiO2 film may collectively form a stack of materials that seal the back surface of the semiconductor substrate, thereby mitigating the diffusion of dopants from the semiconductor substrate.
[0070] In some embodiments, the first material layer may comprise a layer or film of amorphous silicon; the second material layer may comprise a layer or film of silicon oxide (SiO2) formed on the amorphous silicon film; the crystallization of the first material layer or the second material layer may comprise the crystallization of the amorphous silicon film into a layer or film of polycrystalline silicon; and the polycrystalline silicon film and the SiO2 film may collectively form a stack of materials that seal the back surface of the semiconductor substrate, thereby mitigating the diffusion of dopants from the semiconductor substrate.
[0071] In some embodiments, the silicon oxide layer (SiO2) may have a thickness of up to 5000 Å, and the amorphous silicon layer may have a thickness of up to 12000 Å.
[0072] In some embodiments, the semiconductor substrate may be placed in at least one of one or more process chambers (e.g., a first process chamber) such that the back surface of the semiconductor substrate faces downward and the front surface of the semiconductor substrate faces upward during the formation of a first material layer on the back surface of the semiconductor substrate and the formation of a second material layer on the back surface of the semiconductor substrate.
[0073] In some embodiments, movement of the semiconductor substrate does not occur between the application of the first process temperature and the application of the second process temperature. In some embodiments, during the application of the first process temperature, the first material layer and the second material layer may be formed only on the back surface of the semiconductor substrate and may not be formed on the front surface of the semiconductor substrate.
[0074] In some embodiments, the method (600) may further include the step of performing an epitaxial process following the formation of a second material layer. In some embodiments, the stack of materials may mitigate the diffusion of dopants from the semiconductor substrate during the epitaxial process.
[0075] device
[0076] In some embodiments, FIG. 7 is a block diagram illustrating a substrate processing system (700) used to perform processing on a semiconductor substrate (702) (also referred to herein as a wafer) according to some embodiments. As illustrated, the substrate processing system (700) may include a chamber (734). A central column may be configured to support a pedestal when the top surface of the semiconductor substrate (702) is processed, for example, when a film is formed on the top surface of the semiconductor substrate (702) or on the back surface of the semiconductor substrate (702). According to embodiments disclosed herein, the pedestal may be referred to as a showerhead-pedestal ("ShoPed") (706). A showerhead (736) may be placed on the ShoPed (706).
[0077] In some embodiments, the showerhead (736) may be electrically coupled to the power supply (738) via a matching network (740). The power supply (738) may be controlled by a control module (742), for example, a controller. In some embodiments, power may be supplied to the ShoPed (706) instead of the showerhead (736). The control module (742) may be configured to operate the substrate processing system (700) by executing process input and control for specific process recipes. Depending on whether the top surface of the semiconductor substrate (702) accommodates a deposited layer or a layer stack or the bottom surface of the semiconductor substrate (702) accommodates a deposited layer or a layer stack, the controller module (742) may set various operation inputs for the process recipe, such as power levels, timing parameters, process gases, mechanical movement of the semiconductor substrate (702), and / or height of the semiconductor substrate (702) relative to the ShoPed (706).
[0078] In some embodiments, the center column may also include lift pins controlled by lift pin control. These lift pins may be used to raise the semiconductor substrate (702) from the ShoPed (706) to pick the wafer by an end effector (not shown) and to lower the semiconductor substrate (702) after it has been placed by the end effector. The end effector may also place the semiconductor substrate (702) on the spacers (744). As described below, the spacers (744) may be sized to provide a controlled separation of the semiconductor substrate (702) between the bottom surface of the showerhead (736) (facing the wafer) and the top surface of the ShoPed (706) (facing the wafer).
[0079] In some embodiments, the substrate processing system (732) may further include a first gas manifold (746) connected to first gas sources (748), for example, gas chemical supply units from a facility and / or inert gases. Depending on the processing performed on the top surface of the semiconductor substrate (702), the control module (742) may control the delivery of the first gas sources (748) through the first gas manifold (746). The selected gases may then flow into the showerhead (736) and are distributed within a defined spatial volume between the face of the showerhead (736) facing the semiconductor substrate (702) when the wafer rests on the pedestal.
[0080] In some embodiments, the substrate processing system (732) may further include a second gas manifold (750) connected to second gas sources (752), for example, gas chemical supply units from a facility and / or inert gases. Depending on the processing performed on the bottom surface of the semiconductor substrate (702), the control module (742) may control the delivery of the second gas sources (752) through the second gas manifold (750). The selected gases may then flow into the showerhead (736) or be distributed within a defined spatial volume between the surfaces of the ShoPed (706) facing the bottom surface or bottom side (e.g., rear) of the semiconductor substrate (702) when the wafer is placed on the spacers (744). Spacers (744) may provide separation that optimizes deposition to the lower surface of the semiconductor substrate (702) while reducing deposition on the upper surface of the semiconductor substrate (702). In some embodiments, while deposition targets the lower surface of the semiconductor substrate (702), an inert gas may flow over the upper surface of the semiconductor substrate (702) through a showerhead (736), which may push the reactive material gases from the upper surface and direct the reactive material gases provided from the ShoPed (706) toward the lower surface of the semiconductor substrate (702).
[0081] In some embodiments, the showerhead (736) or ShoPed (706) may have a zonal deposition design. For example, a second gas manifold (750) may be fluidically linked to control the transfer of gases to different zones of the wafer. By controlling the flow of gases to different zones, different films may be deposited on the wafer as intended.
[0082] Additionally, the gases may or may not be pre-mixed. Appropriate valve and mass flow control mechanisms may be employed to ensure that the correct gases are delivered during the deposition and plasma treatment phases of the process. Process gases may exit the chamber (734) through an outlet. A vacuum pump (e.g., a one- or two-stage mechanical dry pump and / or turbomolecular pump) may draw out the process gases, and a closed-loop controlled flow limiting device, such as a throttle valve or a pendulum valve, may maintain an appropriately low pressure within the reactor.
[0083] In some embodiments, the carrier ring (754) may encircle the outer region of the ShoPed (706). When the top surface of the semiconductor substrate (702) is processed, for example, when a material is deposited on the top surface, the carrier ring (754) may be configured to sit on a carrier ring support region that is stepped down from the wafer support region at the center of the ShoPed (706). The top surface of the carrier ring (754) is generally coplanar with the top surface of the semiconductor substrate (702). The carrier ring (754) may include an outer edge side of the carrier ring disk structure, for example, an outer radius, and a wafer edge side of the carrier ring disk structure closest to where the semiconductor substrate (702) is placed, for example, an inner radius. The carrier ring (754) may also be associated with an inner diameter (ID). The inner diameter may extend to the inner periphery of the carrier ring and generally surround a substrate (e.g., a semiconductor substrate (702)) within a processing chamber. The wafer edge side of the carrier ring (754) may also include a plurality of contact support structures or "tabs" that may be configured to lift the semiconductor substrate (702) when the carrier ring (754) is held by the spacers (744). The carrier ring (754) may include a plurality of tabs having an amount selected from a range for supporting the semiconductor substrate (702) during processing. Additional details regarding embodiments of the tabs will follow.
[0084] FIG. 8 is a block diagram illustrating another substrate processing system (800) used to perform processing on a semiconductor substrate (802) (also referred to herein as a wafer) according to some embodiments. In some embodiments, spider forks (856) may be used to lift and hold a carrier ring (854) to a process height, for example, to allow deposition on the lower surface (rear side) of the semiconductor substrate (802). Thus, the carrier ring (854) may be lifted together with the semiconductor substrate (802). In some embodiments, the carrier ring (854) may be rotated to another station, for example, in a multi-station system.
[0085] Generally speaking, the embodiments disclosed herein are for systems for depositing PECVD films on selective sides (front and / or back) of a wafer using dynamic control. Some embodiments may include dual gas-flow electrodes to define a capacitively coupled PECVD system. The system may include a gas-flow showerhead (e.g., showerhead (836)) and a ShoPed (806). In some embodiments, a gas-flow pedestal (i.e., ShoPed) is a combination of the showerhead and the pedestal, which enables deposition on the back of the wafer. The electrode geometry combines the features of the showerhead, e.g., a gas mixing plenum, holes, a hole pattern, a gas jet prevention baffle, and the features of the pedestal. Examples of features of the pedestal include an embedded controlled heater, wafer-lift mechanisms, the ability to hold plasma suppression rings, and mobility. This enables the transfer of wafers and the processing of gases with or without using RF power from the pedestal.
[0086] In some embodiments, the system may have a wafer lift mechanism that strictly controls the parallelism of the substrates to the electrodes. In one example, this may be achieved by setting up the lift mechanism parallel to two electrodes and controlling manufacturing tolerances, e.g., spindle or lift pin mechanisms. In another example, the lift may be achieved by raising the wafer lift component. This option may not allow dynamic control of the deposition side.
[0087] In some configurations, the lift mechanism may enable dynamic control of the substrate position during processing (before plasma, during plasma, and after plasma) to control the deposition side, the deposition profile, and the properties of the deposited film. The system may also enable selective enable / disable of the side through which the reactive material flows. One side may flow the reactive material, and the other side may flow inert gases to suppress deposition and plasma.
[0088] In some embodiments, the gap between the sides of the wafer that do not require plasma / dep may be strictly controlled. This distance may be controlled to suppress plasma. By not controlling the distance, the wafer may be sensitive to plasma damage. For example, the system may enable a minimum gap of about 2 mm to about 0.5 mm, and in another embodiment, about 1 mm to about 0.05 mm (limited by the wafer bow), and such a gap may be controlled. The gap may be controlled according to process conditions.
[0089] In some embodiments, the gas-flowing pedestal (i.e., ShoPed) comprises, without limitation: (a) thermal stabilization of the wafer to a processing temperature prior to processing; (b) selective design of hole patterns on the ShoPed to selectively deposit films on different regions of the back surface of the wafer; (c) swappable rings that can be attached to achieve appropriate plasma confinement and hole patterns; (d) stable in-chamber wafer transfer mechanisms for transferring the wafer to another chamber or cassette, such as lift pins, RF-coupling features, and minimum contact arrays; and (e) implementation of gas mixing features, such as an inner plenum, baffles, and manifold line openings. and (f) may also enable the addition of compartments within a gas-flow pedestal (i.e., ShoPed) to enable selective gas flow to different regions on the back of the wafer and to control flow rates through flow controllers and / or multiple plenums.
[0090] In another embodiment, dynamic gap control using a wafer lift mechanism enables the lift mechanism to: (a) control the distance from an intermediate point so that deposition can occur on the side of the wafer where deposition or reaction material is required from the electrode flowing the deposition or reaction material, or on both sides; and (b) dynamically control the distance during the process (before plasma, during plasma, after plasma) to control the deposition side, the profile of the deposition, and the properties of the deposited film. In another embodiment, for a deposition mode used to deposit on the back side of the wafer, film edge exclusion control is highly desirable to prevent lithography-related overlay problems. The lift mechanism used in this system is achieved through a carrier ring (854) having design features for shadowing the deposition on the edge. This specifies edge exclusion control through the design and geometry of the carrier ring.
[0091] FIG. 9a illustrates a cross-sectional view of the edge region of a ShoPed (906) (e.g., 706, 806). This figure provides a cross-sectional view of a carrier ring (954) (e.g., 754, 854) having an inner radius (954a) and an outer radius (954b). In some embodiments, the carrier ring (954) includes supporting extensions (954c) extending below a substantially flat surface of the carrier ring (954).
[0092] The support extensions (954c) are configured to mate and be placed within the support surfaces defined within the top surface of the spacers (944). The support surfaces provide complementary mating surfaces for the support extensions (954c) so as to prevent the carrier ring (954) from sliding or moving when supported by the spacers (944). Although three spacers are shown as spacers (944) in FIG. 9, it is envisioned that any number of spacers may be provided, provided that the carrier ring can be supported substantially parallel to the surface of the ShoPed (906) and the spacing is defined to support the semiconductor substrate (902) in a spaced-away relationship from the top surface of the ShoPed (906).
[0093] It is also shown that the top surface of the ShoPed (906) will include a hole pattern (906a) distributed across the surface to provide even distribution and output of gases during operation. In one embodiment, the hole pattern (906a) is distributed in a plurality of concentric rings extending from the center of the top surface of the ShoPed (906) to the outer periphery of the ShoPed (906). At least one hole pattern (906a) is provided in an edge hole region (907) of the hole pattern, and orifices defined within the edge hole region (907) are preferably inclined to provide gases that are not perpendicular to the surface of the ShoPed (906).
[0094] In one example, the angle or tilting is defined so that the orifices within the edge hole region (907) are tilted or inclined from the center of the ShoPed (906). In one embodiment, the angle is approximately 45° from the horizontal. In other embodiments, the angle can be varied from 20° from the horizontal to approximately 80° from the horizontal. In one embodiment, by providing tilted orifices within the edge hole region (907), additional distribution of process gases can be provided during back deposition of the semiconductor substrate (902). In one embodiment, the remaining orifices (906d) of the hole pattern (906a) are oriented substantially perpendicular to the surface of the ShoPed (906) and directed toward the bottom surface of the semiconductor substrate (902).
[0095] FIG. 9b illustrates that when the semiconductor substrate (902) is held by the carrier ring (954), the edge of the semiconductor substrate (902) will be placed on an edge region closer to the inner radius (954a) of the carrier ring (954). When positioned using spacers (944), the surface of the showerhead (936) facing the top surface of the wafer (902) may be substantially close to prevent deposition during a mode in which deposition is performed on the back surface of the semiconductor substrate (902).
[0096] For example, the distance between the top surface of the semiconductor substrate (902) and the surface of the showerhead (936) is preferably about 2 mm to about 0.5 mm depending on the wafer bow, and about 1 mm to about 0.5 mm in some embodiments. That is, when the wafer is substantially bowed, the separation will be about 0.5 mm or more. If the wafer is not yet substantially bowed, the separation may be less than about 0.5 mm. In one embodiment, it is desirable to minimize the separation to prevent deposition on the top surface of the substrate when the back surface of the substrate is deposited with a layer of material. In some embodiments, the showerhead (936) is configured to supply an inert gas flow over the top surface of the wafer (902) while the back surface of the substrate is being deposited and deposition gases are supplied by the ShoPed (906).
[0097] Any suitable chamber may be used to implement the disclosed embodiments. Exemplary deposition apparatuses are available from various systems, e.g., the ALTUS available from Lam Research Corp., Fremont, California. ® and ALTUS ® Includes Max, or any other various commercially available processing systems.
[0098] FIG. 10 is a cross-sectional view of a processing system (1000) for depositing a film on the back surface of a semiconductor substrate according to some embodiments of the present specification. In some embodiments, the processing system (1000) may include a showerhead (1002), a shower pedestal (ShoPed) (1004), and one or more support structures (1006) (e.g., carrier rings (754, 854, 954) and / or tabs of the carrier rings, or a spider fork (856)). One or more support structures (1006) may be configured to support a semiconductor substrate (1020). In some embodiments, one or more support structures (1006) may be coupled to the ShoPed (1004) and / or other structures associated with the processing system (1000), e.g., the processing chamber wall(s). In some embodiments, electrostatic chucking (e.g., bipolar chucking or monopolar chucking) may be used to further secure the semiconductor substrate (1020) (electrostatic chuck not shown). In some embodiments, as described above, the deposition of SiO2 on the semiconductor substrate (1020) may improve the chucking of the semiconductor substrate (1020).
[0099] In some embodiments, the showerhead (1002) may include an electrode (1010) operable by providing RF power to a plurality of zones. For example, there may be two distinct zones configured to receive different amounts of RF power at different or substantially simultaneous times. In another example, there may be three distinct zones. In other examples, there may be four or more. The RF power provided to two or more zones (or all zones in some cases) may be the same amount.
[0100] In some embodiments, the electrode (1010) may be integrated into or embedded within the showerhead (1002). The electrode (1010) may have zones of a specific configuration depending on the wafer bow and / or other requirements. Examples of zones are discussed above. However, in certain embodiments, the electrode (1010) may be a distinct component that can be replaced without destroying the showerhead (1002) or installed within the showerhead (1002). These interchangeable electrodes may be useful for performing different customized back film depositions of the types discussed in this disclosure. For example, an electrode having three zones may be swapped with an electrode having two zones to compensate for different types of wafer bows.
[0101] In some embodiments, the ShoPed (1004) may have one or more gas inlets (1005) configured to transport and discharge a process gas (1007). Examples of the process gas (1007) may include silane (SiH4), nitrous oxide (N2O), and / or ammonia (NH3). Inert carrier gases (e.g., argon, nitrogen, neon, or helium) may also be transported from the ShoPed (1004) through the ShoPed (1004). In some cases, a mixture of the process gas and the carrier gas may be routed through a showerhead (1002) and discharged from the showerhead. Different types of film materials may be deposited on the semiconductor substrate (1020) based on the type of process gas. The showerhead (1002) may have one or more gas inlets (1003) configured to receive and disperse a purge gas (1008), such as nitrogen. The purge gas (1008) flowing along the top or front of the semiconductor substrate (1020) may be used to prevent process gas (1007) or impurities from the ShoPed (1004) from reaching the top or front of the semiconductor substrate (1020).
[0102] In some embodiments, the semiconductor substrate (1020) may be positioned and supported closer to the showerhead (1002) than to the ShoPed (1004). In an exemplary embodiment, the distance of the gap (1012) between the showerhead (1002) and the semiconductor substrate (1020) may be about 1 mm, while the distance of the gap (1014) between the ShoPed (1004) and the semiconductor substrate (1020) may be about 12 mm. Various distances may be used. However, it is noteworthy and useful that the gap (1012) may be small (e.g., small enough so that plasma is not formed) and much smaller than the gap (1014). This is to prevent plasma (1015) from developing between the semiconductor substrate (1020) and the showerhead (1002) with the front surface of the semiconductor substrate (1020). That is, plasma (1015) is encouraged to form on the back surface (1025) of the semiconductor substrate (1020), where the back surface faces away from the showerhead (1002) and electrode (1010) and faces the ShoPed (1004) and / or support structures (1006). The front surface may have sensitive and high-cost features (transistors, memory cells, wiring, etc.). In some embodiments, flushing purge gas from the holes of the showerhead (1002) may push out any process gas or precursor that may remain or have been transferred to the front surface.
[0103] As already discussed in this specification, by specifying the amount of RF power provided to different zones of the electrode (1010), and at different times in some embodiments, a film material having spatially variable properties across the semiconductor substrate (1020) may be formed. Some examples of film properties include internal stress (e.g., tensile stress or compressive stress) and film thickness.
[0104] FIG. 11 is a schematic diagram of a process system suitable for performing deposition processes, such as front deposition processes according to embodiments. The system (1100) includes a transfer module (1103). The transfer module (1103) provides a clean, pressurized atmosphere to minimize the risk of contamination of substrates to be processed when moved between various reactor modules. A multi-station reactor (1109) capable of performing ALD, processing, and CVD according to various embodiments is mounted on the transfer module (1103). The multi-station reactor (1109) may include a plurality of stations (1111, 1113, 1115, and 1117) capable of performing operations according to the disclosed embodiments sequentially. The stations may include a heated pedestal or substrate support, one or more gas inlets or a showerhead or a dispersion plate.
[0105] One or more single-station modules or multi-station modules (1107) capable of performing plasma or chemical (non-plasma) pre-cleaning, other deposition operations, or etching operations may be mounted on the transfer module (1103). The modules may also be used for various processes, for example, to prepare a substrate for a deposition process. The system (1100) also includes one or more wafer source modules (1101) where wafers are stored before and after processing. An atmospheric robot (not shown) of the atmospheric transfer chamber (1119) may first remove wafers from the wafer source modules (1101) to loadlocks (1121). A wafer transfer device (typically a robot arm unit) of the transfer module (1103) moves wafers from the loadlocks (1121) to the modules mounted on the transfer module (1103) and between the modules.
[0106] In various embodiments, a system controller (1142) is employed to control process conditions during deposition. The system controller (1142) will typically include one or more memory devices and one or more processors. The processor may include a CPU or computer, an analog input / output connection and / or a digital input / output connection, stepper motor controller boards, etc.
[0107] The system controller (1142) may control all activities of the deposition apparatus. The system controller (1142) executes system control software that includes sets of instructions for controlling timing, mixtures of gases, chamber pressure, chamber temperature, wafer temperature, radio frequency (RF) power levels, wafer chuck or pedestal position, and other parameters of a specific process. In some embodiments, other computer programs stored on memory devices associated with the system controller (1142) may be employed.
[0108] The illustrated embodiment includes a user interface associated with a system controller (1142). The user interface may include a display screen, graphic software displays of device and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.
[0109] System control logic may be configured in any suitable manner. Generally, logic may be designed or configured in hardware and / or software. Instructions for controlling the driving network may be hard-coded or provided as software. Instructions may also be provided by "programming." Such programming is understood to include any form of logic, including hard-coded logic on digital signal processors (DSPs), application-specific integrated circuits (ASICs), and other devices having specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions that may be executed on a general-purpose processor. System control software may be coded in any suitable computer-readable programming language.
[0110] Computer program code for controlling processes in a process sequence may be written in any conventional computer-readable programming language, for example, assembly language, C, C++, Pascal, Fortran, or other languages. Compiled object code or scripts are executed by a processor to perform tasks identified in the program. Also, as indicated, the program code may be hardcoded.
[0111] Controller parameters relate to process conditions, such as process gas composition and flow rates, temperature, pressure, cooling gas pressure, substrate temperature, and chamber wall temperature. These parameters may be entered using a user interface or provided to the user in the form of a recipe.
[0112] Signals for monitoring the process may be provided by the analog input connection and / or digital input connection of the system controller (1142). Signals for controlling the process are output on the analog output connection and digital output connection of the system (1100).
[0113] System software may be designed or configured in different ways. For example, various chamber component subroutines or control objects may be written to control the operation of chamber components necessary to perform deposition processes according to the disclosed embodiments. Examples of programs or sections of programs for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.
[0114] In some embodiments, the system controller (1142) is part of the system, which may be part of the examples described above. These systems may include semiconductor processing equipment, including processing tools or tools, chambers or chambers, a platform or platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems may be integrated with an electronic device for controlling their operation before, during, and after processing of a semiconductor wafer or substrate. The electronic device may be referred to as a "controller" that may control the system or various components or sub-parts of the systems. A system controller (1142) may be programmed to control any of the processes disclosed herein, including, depending on the processing requirements and / or type of the system, the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, and wafer transfer into and out of load locks connected to or interfacing with tools and other transfer tools and / or a specific system.
[0115] System controllers
[0116] Generally speaking, a controller may be defined as an electronic device having various integrated circuits, logic, memory, and / or software that receives instructions, issues instructions, controls operations, enables cleaning operations, enables endpoint measurements, etc. Such a controller may be used in any device described herein or in conjunction with any device described herein. Integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application-specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions that communicate with the controller or the system in the form of various individual settings (or program files) that define operation parameters for performing a specific process on or for a semiconductor wafer. In some embodiments, the operation parameters may be part of a recipe defined by process engineers to achieve one or more processing steps during the manufacture of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits and / or wafer dies.
[0117] The system controller may be integrated into the system, coupled to the system, otherwise networked to the system, or coupled to or part of a computer that is a combination of these. For example, the system controller may be all or part of a fab host computer system capable of enabling remote access to wafer processing, or it may be located within the "cloud." The computer may enable remote access to the system to monitor the current progress of manufacturing operations, examine the history of past manufacturing operations, examine trends or performance measurements from multiple manufacturing operations, change parameters of the current processing, set processing steps following the current processing, or start a new process. In some examples, a remote computer (e.g., a server) may provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that enables the input or programming of parameters and / or settings to be subsequently transmitted from the remote computer to the system. In some examples, the controller receives instructions in the form of data that specify parameters for each of the processing steps to be performed during one or more operations. It should be understood that parameters may be specific to the type of tool configured to be controlled or interfaced by the controller and the type of process to be performed. Accordingly, as described above, the controller may be distributed by including one or more individual controllers that are networked and operate together toward a common purpose, such as the processes and controls described herein, for example. An example of a distributed controller for such purposes would be one or more integrated circuits on a chamber that communicate with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) that are combined to control a process on the chamber.
[0118] Without limitation, exemplary systems may include a plasma etching chamber or module, a deposition chamber or module, a spin-rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etching chamber or module, a PVD chamber or module, a CVD chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, and any other semiconductor processing systems that may be used or associated in the manufacture and / or fabrication of semiconductor wafers.
[0119] As noted above, depending on the process steps or steps to be performed by the tool, the controller may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport for moving containers of wafers from and to tool locations and / or load ports of the semiconductor manufacturing plant.
[0120] The system controller may include various programs. A substrate positioning program may include program code for controlling chamber components used to load the substrate onto the pedestal or chuck and to control the gap between the substrate and other parts of the chamber, such as the gas inlet and / or target. A process gas control program may include code for controlling gas composition, flow rates, and pulse times, and optionally for flowing gas into the chamber before deposition to stabilize the pressure within the chamber. A pressure control program may include code for controlling the pressure in the chamber, for example, by adjusting the throttle valve of the chamber's exhaust system. A heater control program may include code for controlling the current to a heating unit used to heat the substrate. Alternatively, a heater control program may control the delivery of a heat transfer gas, such as helium, to the wafer chuck.
[0121] Examples of chamber sensors that may be monitored during deposition include mass flow controllers, pressure sensors such as manometers, and thermocouples located on a pedestal or chuck. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain targeted process conditions.
[0122] The foregoing describes examples of implementations of disclosed embodiments of single or multi-chamber semiconductor processing tools. The apparatus and process described herein may be used in conjunction with lithographic patterning tools or processes for the manufacture or fabrication of, for example, semiconductor devices, displays, LEDs, photoelectric panels, etc. Typically, but not necessarily, these tools / processes will be used or performed together in a common manufacturing facility. Lithographic patterning of a film typically comprises the following steps, each of which is provided with a plurality of possible tools: (1) applying a photoresist onto a workpiece, i.e., a substrate, using a spin-on tool or a spray-on tool; (2) curing the photoresist using a hot plate, a furnace, or a UV curing tool; (3) exposing the photoresist to visible light, UV, or X-ray light using a tool such as a wafer stepper; (4) a step of developing the resist to pattern the resist by selectively removing the resist using a tool such as a wet bench; (5) a step of transferring the resist pattern into a film or workpiece placed underneath by using a dry or plasma-assisted etching tool; and (6) some or all of the step of removing the resist using a tool such as an RF or microwave plasma resist stripper.
[0123] conclusion
[0124] Although the foregoing embodiments have been described in some detail for the sake of clarity of understanding, it will be apparent that specific changes and modifications may be made within the scope of the appended claims. The embodiments disclosed herein may be made without some or all of these specific details. In other examples, well-known process operations have not been described in detail so as not to unnecessarily obscure the disclosed embodiments. Furthermore, it will be understood that while the disclosed embodiments will be described together with specific embodiments, specific embodiments are not intended to limit the disclosed embodiments. It should be noted that there are many alternative ways of implementing the processes, systems, and devices of the embodiments. Accordingly, the embodiments are to be considered exemplary and non-limiting, and the embodiments are not to be limited to the details given herein.
Claims
Claim 1 An apparatus configured for back sealing of a semiconductor substrate, comprising: one or more process chambers; a showerhead configured to deliver one or more process gases to the back surface of at least one semiconductor substrate among the one or more process chambers; and a first set of one or more process gases to be coupled to the showerhead and the one or more process chambers and to induce delivery to a first process chamber having the semiconductor substrate; a first process temperature of 200 to 400 °C in the presence of plasma to form a silicon oxide (SiO2) layer on the back surface of the semiconductor substrate; and a second set of one or more process gases to be delivered to the first process chamber. An apparatus configured for back sealing of a semiconductor substrate, comprising a controller configured to apply a first process temperature of 200 to 400 °C in the presence of plasma to form an amorphous silicon layer on the SiO2 layer on the back surface of the semiconductor substrate in order to seal the back surface of the semiconductor substrate and collectively form a stack of materials that mitigate the diffusion of dopants from the semiconductor substrate. Claim 2 An apparatus configured for rear sealing of a semiconductor substrate, wherein, in claim 1, the semiconductor substrate is disposed in at least one of the one or more process chambers such that the rear surface of the semiconductor substrate faces downward and the front surface of the semiconductor substrate faces upward during the formation of the SiO2 layer on the rear surface of the semiconductor substrate and the formation of the amorphous silicon layer on the rear surface of the semiconductor substrate. Claim 3 An apparatus configured for back sealing of a semiconductor substrate, wherein, in claim 1, one or more process gases of the first set comprise silane (SiH4) and nitrous oxide (N2O), and one or more process gases of the second set comprise a carrier gas. Claim 4 An apparatus configured for back sealing of a semiconductor substrate, wherein, in claim 1, the silicon oxide (SiO2) layer comprises a thickness of up to 5000 Å and the amorphous silicon layer comprises a thickness of up to 12000 Å. Claim 5 An apparatus configured for back surface sealing of a semiconductor substrate, wherein, in claim 1, the controller is further configured to apply a second process temperature of at least 700°C to cause an annealing process to occur following the formation of the amorphous silicon layer, and the annealing process includes the step of inducing crystallization of the amorphous silicon layer to form a polycrystalline silicon layer to collectively form a stack of materials sealing the back surface of the semiconductor substrate. Claim 6 In claim 5, the controller is further configured to perform an epitaxial process following the formation of the amorphous silicon layer; and the stack of materials is configured for back sealing of a semiconductor substrate, which mitigates the diffusion of dopants from the semiconductor substrate during the epitaxial process. Claim 7 An apparatus configured for back sealing of a semiconductor substrate, wherein, in claim 5, movement of the semiconductor substrate does not occur between the application of the first process temperature and the application of the second process temperature. Claim 8 An apparatus configured for back sealing of a semiconductor substrate, wherein, during the application of the first process temperature, the amorphous silicon and the polycrystalline silicon are formed only on the back surface of the semiconductor substrate and not on the front surface of the semiconductor substrate. Claim 9 A first process chamber configured to accommodate a semiconductor substrate; a showerhead configured to deliver one or more process gases to the rear surface of the semiconductor substrate within the first process chamber; and a controller coupled to at least the showerhead and the first process chamber, and inducing the delivery of a first set of one or more process gases to the first process chamber having the semiconductor substrate; applying a first process temperature of 200 to 400 °C in the presence of plasma to form an amorphous silicon layer on the rear surface of the semiconductor substrate; and inducing the delivery of a second set of one or more process gases to the first process chamber; An apparatus comprising a controller configured to apply a first process temperature of 200 to 400°C in the presence of plasma to form a silicon oxide (SiO2) layer on the amorphous silicon layer on the back surface of the semiconductor substrate in order to seal the back surface of the semiconductor substrate and collectively form a stack of materials that mitigate the diffusion of dopants from the semiconductor substrate. Claim 10 An apparatus according to claim 9, wherein one or more of the first set of process gases comprises silane (SiH4), and one or more of the second set of process gases comprises SiH4 and nitrous oxide (N2O). Claim 11 In claim 9, the apparatus is further configured such that the controller is configured to apply a second process temperature of at least 700°C to cause an annealing process to occur following the formation of the SiO2 layer, and the annealing process comprises the step of inducing crystallization of the amorphous silicon layer to form a polycrystalline silicon layer to collectively form a stack of the materials sealing the back surface of the semiconductor substrate. Claim 12 A method for back sealing of a semiconductor substrate, comprising: a step of inducing the delivery of one or more process gases of a first set to a first process chamber of a deposition apparatus, wherein the first process chamber has a semiconductor substrate disposed therein; a step of applying a first process temperature in the presence of plasma to form a first material layer on the back surface of the semiconductor substrate; a step of inducing the delivery of one or more process gases of a second set to the first process chamber; and a step of applying the first process temperature in the presence of plasma to form a second material layer on the first material layer on the back surface of the semiconductor substrate to collectively form a stack of materials that seal the back surface of the semiconductor substrate and mitigate the diffusion of dopants from the semiconductor substrate. Claim 13 A method for back sealing of a semiconductor substrate according to claim 12, wherein the first material layer comprises silicon oxide (SiO2). Claim 14 A method for back sealing of a semiconductor substrate according to claim 12, wherein the first material layer comprises amorphous silicon. Claim 15 A method for back sealing of a semiconductor substrate according to claim 12, wherein the second material layer comprises amorphous silicon. Claim 16 A method for back sealing of a semiconductor substrate according to claim 12, wherein the second material layer comprises silicon oxide (SiO2). Claim 17 A method for back sealing of a semiconductor substrate according to claim 12, wherein the first process temperature includes a temperature of 200 to 400 ℃. Claim 18 A method for back sealing of a semiconductor substrate according to claim 12, wherein one or more process gases of the first set comprise silane (SiH4) and nitrous oxide (N2O), and one or more process gases of the second set comprise a carrier gas. Claim 19 A method for back sealing of a semiconductor substrate according to claim 12, wherein one or more process gases of the first set comprise silane (SiH4), and one or more process gases of the second set comprise SiH4 and nitrous oxide (N2O). Claim 20 A method for sealing the back surface of a semiconductor substrate according to claim 12, further comprising the step of applying a second process temperature to cause an annealing process to occur following the formation of the second material layer, wherein the annealing process comprises inducing crystallization of the first material layer or the second material layer to collectively form a stack of materials sealing the back surface of the semiconductor substrate. Claim 21 A method for sealing the back surface of a semiconductor substrate according to claim 20, wherein the first material layer comprises a silicon oxide (SiO2) film; the second material layer comprises an amorphous silicon film formed on the SiO2 film; the crystallization of the first material layer or the second material layer comprises crystallization of the amorphous silicon film into a polycrystalline silicon film; and the polycrystalline silicon film and the SiO2 film collectively form a stack of the materials that seal the back surface of the semiconductor substrate, thereby mitigating the diffusion of dopants from the semiconductor substrate. Claim 22 A method for sealing the back surface of a semiconductor substrate according to claim 20, wherein the first material layer comprises an amorphous silicon film; the second material layer comprises a silicon oxide (SiO2) film formed on the amorphous silicon film; the crystallization of the first material layer or the second material layer comprises crystallization of the amorphous silicon film into a polycrystalline silicon film; and the polycrystalline silicon film and the SiO2 film collectively form a stack of the materials that seal the back surface of the semiconductor substrate, thereby mitigating the diffusion of dopants from the semiconductor substrate. Claim 23 A method for back sealing of a semiconductor substrate according to claim 20, further comprising the step of performing an epitaxial process following the formation of the second material layer; wherein the stack of the materials mitigates the diffusion of dopants from the semiconductor substrate during the epitaxial process. Claim 24 A method for back sealing of a semiconductor substrate according to claim 20, wherein movement of the semiconductor substrate does not occur between the application of the first process temperature and the application of the second process temperature. Claim 25 A method for back sealing of a semiconductor substrate according to claim 12, wherein, during the application of the first process temperature, the first material layer and the second material layer are formed only on the back surface of the semiconductor substrate and not on the front surface of the semiconductor substrate.