Separator, secondary battery cell, battery device and power user device
A separator with a coating layer of low-density organic particles addresses the challenge of achieving high energy density and reliability in secondary battery cells by ensuring electrochemical stability and thermal stability, thereby enhancing performance under high voltage conditions.
Patent Information
- Application Number
- KR1020267034090
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-09-30
- Filing Date
- 2025-01-24
- Publication Date
- 2026-11-09
AI Technical Summary
Existing secondary battery cells face challenges in achieving high energy density and reliability, particularly due to the limitations of polyolefin-based separators which have low glass transition temperatures leading to thermal shrinkage and reduced energy density when combined with high-density inorganic fillers like boehmite or alumina.
A separator comprising a porous substrate with a coating layer containing low-density organic particles, such as thermosetting resin polymers or crosslinked polymers, which exhibit excellent electrochemical stability and thermal stability, ensuring no oxidation peaks within a voltage range of 2.50 V to 4.40 V, thereby improving energy density and capacity performance.
The use of low-density organic particles in the separator enhances mass energy density and maintains excellent capacity performance characteristics even under high voltage conditions, while suppressing thermal shrinkage and improving the reliability of secondary battery cells.
Smart Images

Figure PCT00006_ABST
Abstract
Description
Technology Field
[0001] Cross-reference of related applications
[0002] This application claims priority to Chinese patent application 202410946641.X, filed on July 15, 2024, titled “Separator, Battery Cell and Power Usage Device” and Chinese patent application 202411382998.6, filed on September 30, 2024, titled “Separator, Secondary Battery Cell, Battery Device and Power Usage Device”, the entire contents of said applications are incorporated herein by reference.
[0003] Technology field
[0004] The present disclosure relates to a separator, a secondary battery cell, a battery device, and a power usage device. Background Technology
[0005] As the application scope of secondary battery cells becomes increasingly extensive, the demand for their use is growing day by day, and requirements for, for example, energy density and reliability are also rising. Therefore, ensuring high reliability while simultaneously achieving higher energy density in secondary battery cells is a technical challenge that must be urgently addressed.
[0006] The present disclosure provides a separator, a secondary battery cell, a battery device, and a power usage device, wherein the secondary battery cell has excellent capacity performance characteristics at high voltage.
[0007] In a first embodiment, the present disclosure provides a secondary battery cell comprising a positive plate, a negative plate, and a separator. The separator is disposed between the positive plate and the negative plate, and the separator comprises a porous substrate and a coating layer located on at least one side of the porous substrate, wherein the coating layer comprises organic particles, and the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V.
[0008] Since organic particles have low density, secondary battery cells to which they are applied can have a higher mass energy density. The first cycle cyclic voltammetry curve of the organic particles of the separator of the present disclosure does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V, which indicates that the organic particles are stable within a voltage range of 2.50 V to 4.40 V. Therefore, since the organic particles of the present disclosure have excellent electrochemical stability, they can be applied to high-voltage secondary battery cells, and the operating voltage and energy density of the secondary battery cells can be improved, and the secondary battery cells can also have excellent capacity performance characteristics even under high voltage conditions.
[0009] In some embodiments, the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.50 V.
[0010] In some embodiments, the organic particles are at least one of a thermosetting resin polymer or a crosslinked polymer.
[0011] In some embodiments, the organic particles are amorphous polymers.
[0012] In some embodiments, the true density of the organic particles is 1.0 g / cm³ 3 -2.0g / cm 3 and; optionally 1.0 g / cm² 3 -1.8g / cm 3 It could be.
[0013] In some embodiments, the volume distribution particle size Dv50 of the organic particles is less than 1 μm and optionally 50 nm to 840 nm.
[0014] In some embodiments, the organic particles do not have a melting point.
[0015] The organic particles of the present disclosure have no melting point, which indicates that the organic particles have excellent heat resistance and thermal stability. Accordingly, thermal shrinkage of the porous substrate can be suppressed more effectively, thereby improving the heat resistance of the separator and improving the reliability of the secondary battery cell.
[0016] In some embodiments, the organic particles comprise one or more of phenol resin-based organic particles, polymer particles containing triazine ring structure units, cross-linked styrene-based organic particles, and silicon-containing organic resin particles.
[0017] In some embodiments, the phenol resin-based organic particles are thermosetting resist resin polymers.
[0018] In some embodiments, the phenol resin-based organic particles do not have a glass transition temperature of 300°C or lower.
[0019] In some embodiments, the volume distribution particle size Dv50 of the phenol resin-based organic particles is 200 nm to 840 nm.
[0020] In some embodiments, the polymer particles containing the triazine ring structure units include a cross-linking structure connecting the triazine ring structure units. Optionally, the cross-linking structure includes one or more combinations of alkylene groups, alkylene ether groups, alkylene amine groups, ester groups, and amide groups.
[0021] In some embodiments, the triazine ring structure unit of the polymer particles containing the triazine ring structure unit also has a substituent, said substituent includes a combination of one or more of an alkyl group, an alkenyl group, a phenyl group, a cycloalkyl group, an amino group, a hydroxyl group, and a halogen.
[0022] In some embodiments, the polymer particles containing triazine ring structure units include melamine aldehyde-based polymers and derivatives thereof.
[0023] In some embodiments, the melamine aldehyde-based polymer and its derivative comprises one or more of melamine formaldehyde, benzoguanamine formaldehyde, melamine-benzoguanamine formaldehyde, melamine-(2,4-diamino-1,3,5-triazine) formaldehyde, melamine-(6-methyl-1,3,5-triazine-2,4-diamine) formaldehyde, melamine-(2,4,6-triethylamino-1,3,5-triazine) formaldehyde, trihydrazino-s-triazine formaldehyde, melamine-(2-amino-4-methylamino-1,3,5-triazine) formaldehyde, and melamine-(2,4-diamino-6-dimethylamino-1,3,5-triazine) formaldehyde.
[0024] In some embodiments, the polymer particles containing the triazine ring structure unit do not have a glass transition temperature of 300°C or lower.
[0025] In some embodiments, the volume distribution particle size Dv50 of the polymer particles containing the triazine ring structure unit is 200 nm to 840 nm.
[0026] In some embodiments, the cross-linked styrene-based organic particles comprise styrene or styrene derivative structural units and cross-linked structural units.
[0027] In some embodiments, the styrene or styrene derivative structural unit comprises one or more of a styrene structural unit, a 1-methyl-1-styrene structural unit, a 4-methylstyrene structural unit, a 2-methylstyrene structural unit, a 2,4-dimethylstyrene structural unit, and a 2,5-dimethylstyrene structural unit.
[0028] In some embodiments, the crosslinking structural unit comprises one or more of a divinylbenzene structural unit, an ethylene glycol dimethacrylate structural unit, a pentaerythritol tetraacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, an N,N-methylenebisacrylamide structural unit, an N,N'-vinylbisacrylamide structural unit, a 1,3,5-triacryloylhexahydro-1,3,5-triazine structural unit, and a trialyl isocyanurate structural unit.
[0029] In some embodiments, the glass transition temperature of the cross-linked styrene-based organic particles T g It is 110℃ to 154℃.
[0030] In some embodiments, the volume distribution particle size Dv50 of the cross-linked styrene-based organic particles is 88 nm to 295 nm.
[0031] In some embodiments, the silicon-containing organic resin particles are silicon-containing organic cross-linked resin particles, and the silicon-containing organic resin particles contain carbon-carbon bonds and a siloxane structure.
[0032] In some embodiments, the silicon-containing organic resin particles are silicon-containing organic cross-linked resin particles, and the silicon-containing organic resin particles have a network structure formed with carbon-carbon bonds as the main chain, and the side chains contain a siloxane structure.
[0033] In some embodiments, the silicon-containing organic crosslinked resin particles include crosslinked structural units.
[0034] Optionally, the crosslinking structural unit is a divinylbenzene structural unit, a diethylene glycol divinyl ether structural unit, a triethylene glycol divinyl ether structural unit, a diallyl maleate structural unit, an ethylene glycol dimethacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, a 2,2,4-trimethyladipoylbis[2-ethylaziridine] structural unit, a 1,1-azellaoilbis[2-methylaziridine] structural unit, a 1,1-(1,3-phenylenedicarbonyl)bis[2-methylaziridine] structural unit, It includes one or more of the trimethylolpropane tri(2-methyl-1-aziridinylpropionate) structural unit, the trimethylolpropane-tri[3-(2-methylaziridinyl)propionate] structural unit, and the pentaerythritol tri(3-aziridinyl)propionate structural unit.
[0035] In some embodiments, the silicon-containing organic resin particles do not have a glass transition temperature of 300°C or lower.
[0036] In some embodiments, the volume distribution particle size Dv50 of the silicon-containing organic resin particles is 88 nm to 295 nm.
[0037] In some embodiments, the ratio of the volume distribution particle size Dv50 of the organic particles to the average pore diameter of the porous substrate is 1.2 or greater.
[0038] In some embodiments, the coating layer further includes a binder.
[0039] In some embodiments, based on the total mass of the coating layer, the mass content of organic particles in the coating layer is 50%-99%.
[0040] In some embodiments, the thickness of the coating layer is 0.5μm to 5μm.
[0041] In some embodiments, the areal density of the coating layer is 0.45 g / m² 2 -5g / m 2 am.
[0042] In a second aspect, the present disclosure provides a battery device comprising a plurality of secondary battery cells of the first aspect of the present disclosure.
[0043] In a third embodiment, the present disclosure provides a power-using device comprising a secondary battery cell of the first embodiment of the present disclosure or a battery device of the second embodiment of the present disclosure.
[0044] In a fourth embodiment, the present disclosure provides a separator comprising a porous substrate and a coating layer located on at least one side of the porous substrate, wherein the coating layer comprises organic particles, and the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V.
[0045] In some embodiments, the organic particles are at least one of a thermosetting resin polymer or a crosslinked polymer.
[0046] In some embodiments, the organic particles are amorphous polymers.
[0047] In some embodiments, the true density of the organic particles is 1.0 g / cm³ 3 -2.0g / cm 3 and; optionally 1.0 g / cm² 3 -1.8g / cm 3 It could be.
[0048] In some embodiments, the volume distribution particle size Dv50 of the organic particles is less than 1 μm and optionally 50 nm to 840 nm.
[0049] In some embodiments, the organic particles do not have a melting point.
[0050] In some embodiments, the organic particles comprise one or more of phenol resin-based organic particles, polymer particles containing triazine ring structure units, cross-linked styrene-based organic particles, and silicon-containing organic resin particles. Brief explanation of the drawing
[0051] To more clearly explain the technical methods of the embodiments of the present disclosure, the drawings used in the embodiments of the present disclosure are briefly introduced below. The drawings described below are merely partial embodiments of the present disclosure, and it is obvious to those skilled in the art that other drawings may be obtained based on the drawings without making any inventive efforts. FIG. 1 illustrates a schematic diagram of a secondary battery cell provided in some embodiments of the present disclosure. FIG. 2 illustrates a schematic diagram of a power-using device provided in some embodiments of the present disclosure. In drawings, the drawing may not necessarily be drawn according to actual proportions. Specific details for implementing the invention
[0052] Hereinafter, embodiments of the separator, secondary battery cell, battery device, and power user device of the present disclosure are described in detail with appropriate reference to the drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of substantially identical structures may be omitted. This is to prevent the following description from becoming unnecessarily long and to aid the understanding of those skilled in the art. Furthermore, the drawings and the following description are intended only to provide those skilled in the art with a sufficient understanding of the present disclosure and are not intended to limit the subject matter described in the claims.
[0053] The “range” disclosed in this disclosure is limited in the form of lower and upper limits, and a given range is limited by selecting one lower limit and one upper limit, and the selected lower limit and upper limit define the boundaries of a specific range. A range limited in this way may or may not include a final value and may be arbitrarily combined, that is, all lower limit values may be combined with all upper limit values to form a single range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, ranges of 60-110 and 80-120 are also considered to be expected. Additionally, if minimum range values 1 and 2 are listed and maximum range values 3, 4 and 5 are listed, ranges of 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 may all be considered. In the present disclosure, unless otherwise specified, the numeric range “ab” is an abbreviated expression for any combination of numbers between a and b, where a and b are both real numbers. For example, the numeric range “0-5” indicates that all real numbers between “0-5” have already been listed in the text, and “0-5” is merely an abbreviated expression for such combination of numbers. Also, if a particular parameter is expressed as an integer ≥2, this is equivalent to disclosing that the parameter is an integer such as, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0054] Unless otherwise specifically described, all embodiments and optional embodiments of the present disclosure may be combined with each other to form a new technical solution.
[0055] Unless otherwise specifically stated, all technical features and optional technical features of the present disclosure may be combined to form a new technical solution, and such technical solution shall also be deemed to be included in the disclosed content of the present disclosure.
[0056] Unless otherwise specifically described, all steps of the present disclosure may be performed sequentially or randomly, preferably sequentially. For example, the method comprises steps (a) and (b), which means that the method may perform steps (a) and (b) sequentially, or steps (b) and (a) sequentially. For example, the fact that the said method may comprise step (c) indicates that step (c) may be added to the method in any order, and for example, the method may comprise steps (a), (b), and (c), steps (a), (c), and (b), or steps (c), (a), and (b), etc.
[0057] Unless otherwise specifically stated, terms such as “first,” “second,” etc. in this disclosure are used to distinguish different objects and are not used to describe a specific order or priority relationship.
[0058] In the present disclosure, the terms “plural” and “multiple types” mean two or more or two or more types.
[0059] In the description of the embodiments of the present disclosure, unless otherwise specifically stated, the first feature being "above" or "below" the second feature may mean that the first feature and the second feature are in direct contact, or that the first feature and the second feature are indirectly in contact through an intermediate medium. Additionally, the first feature being "above," "upper," and "upper surface" of the second feature may mean that the first feature is located directly above or obliquely above the second feature, or merely that the horizontal height of the first feature is higher than that of the second feature. The first feature being "below," "lower," and "lower surface" of the second feature may mean that the first feature is located directly below or obliquely below the second feature, or merely that the horizontal height of the first feature is lower than that of the second feature.
[0060] Unless otherwise specified, the test temperature of each parameter mentioned in this disclosure is 25°C.
[0061] The secondary battery cell mentioned in the embodiments of the present disclosure can independently implement charging and discharging functions and can be continuously used by activating the active material through a charging method after discharge. The secondary battery cell may be cylindrical, rectangular, or have other shapes, and the embodiments of the present disclosure are not limited thereto. FIG. 1 is a secondary battery cell (5) with a rectangular structure as one example.
[0062] The secondary battery cell provided in the embodiments of the present disclosure may include, but is not limited to, a lithium battery cell and a sodium battery cell, and may include, for example, a lithium-ion battery cell, a sodium-ion battery cell, a lithium-metal battery cell, a sodium-metal battery cell, etc.
[0063] The secondary battery cell provided in the embodiments of the present disclosure comprises an electrode assembly. The electrode assembly may have a wound structure or a laminated structure, and the embodiments of the present disclosure are not limited thereto. The secondary battery cell further comprises an outer casing, which may be used to seal the electrode assembly. The outer casing may be a hard case, for example, a rigid plastic case, an aluminum case, a steel case, etc. The outer packaging may be a flexible packaging, such as a pouch-type packaging. The material of the soft pack may be plastic, for example, one or more of aluminum plastic film, polypropylene, polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0064] The battery apparatus mentioned in the embodiments of the present disclosure may include one or more battery cell assemblies for providing voltage and capacity. The battery cell assembly may include a plurality of secondary battery cells, and the plurality of secondary battery cells are connected in series, parallel, or a mixed series-parallel manner through busbar members.
[0065] In some embodiments, the battery cell assembly is typically formed by arranging a plurality of secondary battery cells.
[0066] As an example, the battery cell assembly may be a battery module, and the battery module is formed as a single independent module by arranging and fixing multiple secondary battery cells. As an example, the battery module may be formed by binding multiple secondary battery cells together with a binding band.
[0067] In some embodiments, the battery device may be a battery pack, and the battery pack includes a case and one or more battery cell assemblies, and the battery cell assemblies are accommodated inside the case.
[0068] As an example, the battery cell assembly may be a battery module, and the battery cell assembly may be accommodated inside the case in a manner that secures the battery module to the case.
[0069] As an example, the battery cell assembly may be accommodated inside the case by directly fixing multiple secondary battery cells to the case.
[0070] As an example, the case may include a first case and a second case. By interlocking the first case and the second case, a closed space for accommodating a battery cell assembly may be formed inside the case. Here, “closed” means covering or closing, and may be sealed or not sealed. The first case may be an upper cover or a bottom plate.
[0071] As an example, the case may include an upper cover, a frame, and a bottom plate. The upper cover and the bottom plate may each be connected to the frame to form a closed space for accommodating a battery cell assembly inside the case.
[0072] In some embodiments, the box body may be part of the chassis structure of the vehicle. For example, a part of the box body may be at least part of the vehicle floor, or a part of the box body may be at least part of the vehicle's transverse and longitudinal beams.
[0073] All technical solutions described in the embodiments of the present disclosure may be applied to various power-using devices using secondary battery cells and battery devices, such as, for example, mobile devices (e.g., mobile phones, tablet computers, laptop computers, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Secondary battery cells and battery devices are used to store or supply electrical energy.
[0074] FIG. 2 is a schematic diagram of a power-using device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc.
[0075] In the context of the present disclosure, “organic particles” primarily serve to improve heat resistance in the coating layer of a separator and have little to no adhesive properties.
[0076] The separator is a critical component that supports the electrochemical charging and discharging reactions of secondary battery cells. While most commonly used separators are composed of polyolefin-based materials, these materials have relatively low glass transition temperatures, leading to severe thermal shrinkage upon heating. To improve the heat resistance of separators, boehmite or alumina are currently typically used as heat-resistant fillers and combined with a binder to form a coating layer. Since boehmite and alumina have high densities and therefore possess a greater mass than other materials within the same stacked volume, this affects the energy density of the secondary battery cell.
[0077] An embodiment of the present disclosure provides a separator, which enables a secondary battery cell using the same to have excellent capacity performance characteristics even under high voltage conditions.
[0078] The separator provided in the embodiment of the present disclosure comprises a porous substrate and a coating layer located on at least one side of the porous substrate, and the coating layer comprises organic particles and a binder. The first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V.
[0079] Both the porous substrate and the coating layer have a porous structure, thereby enabling the separation membrane to have relatively excellent air permeability, which facilitates the passage of ions. Organic particles in the coating layer are interconnected and fixed by a binder, and the gaps between the organic particles can form a porous structure.
[0080] Since the density of organic particles is low, secondary battery cells using them can have a higher mass energy density. Replacing boehmite and alumina with low-density organic particles can improve the energy density of secondary battery cells, but general organic particles generally have low electrochemical stability. The first cycle cyclic voltammetry curve of the organic particles of the separator of the present disclosure does not have an oxidation peak within the voltage range of 2.50 V to 4.40 V, which indicates that the organic particles are stable within the voltage range of 2.50 V to 4.40 V. Therefore, since the organic particles of the present disclosure have excellent electrochemical stability, they can be applied to high-voltage secondary battery cells, and the operating voltage and energy density of the secondary battery cells can be improved, and the secondary battery cells can also have excellent capacity performance characteristics even under high voltage conditions.
[0081] In some embodiments, the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.45 V.
[0082] In some embodiments, the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.50 V.
[0083] The oxidation peak potential of the cyclic voltammetry curve of organic particles can be tested by the following method: a slurry is prepared by dissolving organic particles, polyacrylate as a binder, and conductive carbon black as a conductive agent in water at a solid mass ratio of 64:7:29. A coin cell is assembled by applying the slurry to aluminum foil to use as the anode and using lithium foil as the cathode; a cyclic voltammetry (CV) test is performed on the coin cell. The scan rate is 0.10 mV / s, the voltage range is 2.50 V-5.00 V, and a total of 3 cycles are performed. The voltage corresponding to the peak onset point in the first cycle cyclic voltammetry curve is set as the oxidation peak potential. The electrolyte salt of the test electrolyte is LiPF6 with a concentration of 1 mol / L, and the solvent of the electrolyte is obtained by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7.
[0084] In some embodiments, the true density of the organic particles is 1.0 g / cm³ 3 -2.0g / cm 3 It may be. Optionally, the true density of the organic particles is 1.0 g / cm³. 3 -1.8g / cm 3 It could be.
[0085] Currently, the true density of inorganic particles such as boehmite and alumina is typically 2.5 g / cm³. 3 -3.5g / cm 3 The organic particles of the present disclosure have a low true density, so a secondary battery cell using the separator of the present disclosure can have a higher mass energy density.
[0086] In some embodiments, the volume distribution particle size Dv50 of the organic particles is less than 1 μm, and optionally may be 50 nm-840 nm, 88 nm-840 nm.
[0087] The organic particles of the present disclosure are not well soluble in water at 25°C, nor are they well soluble in organic solvents such as tetrahydrofuran (THF), dichloromethane (DCM), dimethylformamide (DMF), trichlorobenzene (TCB), and chloroform. That is, since they are not soluble in the mobile phase of a gel permeation chromatography test, the molecular weight of the organic particles cannot be measured through gel permeation chromatography.
[0088] The organic particles of the present disclosure are at least one of a thermosetting resin polymer or a crosslinked polymer.
[0089] Thermosetting resin polymers refer to polymer products that harden irreversibly upon curing, and once hardened, they do not soften or melt even if heated again.
[0090] A cross-linked polymer refers to a polymer product obtained by the formation of cross-links between monomer units.
[0091] The organic particles of the present disclosure are amorphous polymers.
[0092] In some embodiments, the organic particles do not have a melting point.
[0093] The fact that the organic particles of the present disclosure do not have a melting point indicates that the heat resistance and thermal stability of the organic particles are excellent, and thereby the thermal shrinkage of the porous substrate can be suppressed more effectively, thereby improving the heat resistance of the separator and improving the reliability of the secondary battery cell.
[0094] The melting point can be tested in the following manner: take an appropriate amount of sample (e.g., 5 mg–15 mg) and place it in the crucible of a differential scanning calorimeter (DSC), shake it to level it, and then close the crucible lid; set the measurement conditions to a nitrogen atmosphere, a purge gas flow rate of 60 mL / min, and a shield gas flow rate of 20 mL / min; set the measurement program to heat from 25°C to 200°C at a heating rate of 10°C / min, hold for 5 min to remove thermal history, then cool from 200°C to -40°C at a cooling rate of 10°C / min, and then heat again to 300°C at a heating rate of 10°C / min. Determine whether the organic particles have a melting point below 300°C through the DSC curve.
[0095] The fact that organic particles do not have a melting point means that there is no melting peak in the DSC curve of the organic particles.
[0096] In some embodiments, the organic particles may include one or more of phenol resin-based organic particles, polymer particles containing triazine ring structure units, cross-linked styrene-based organic particles, and silicon-containing organic resin particles.
[0097] [Phenol resin-based organic particles]
[0098] In some embodiments, the phenolic resin-based organic particles are thermosetting resin polymers.
[0099] In some embodiments, the phenolic resin-based organic particles are thermosetting resist resin polymers.
[0100] The raw materials for the phenol resin-based organic particles may include phenolic compounds and aldehyde compounds. In some embodiments, the phenolic compounds may include one or more of phenol, hydroquinone, resorcinol, catechol, cresol, and cardanol. In some embodiments, the aldehyde compounds may include one or more of formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, n-butylaldehyde, glyoxal, and furfural.
[0101] In some embodiments, the phenol resin-based organic particles do not have a glass transition temperature of 300°C or lower.
[0102] Phenolic resin-based organic particles do not have a glass transition temperature below 300°C, which indicates that the organic particles have excellent heat resistance and thermal stability. This allows for more effective suppression of thermal shrinkage of the porous substrate, thereby improving the heat resistance of the separator and improving the reliability of the secondary battery cell.
[0103] In some embodiments, the volume distribution particle size Dv50 of the phenol resin-based organic particles may be 200 nm to 840 nm.
[0104] If the volume distribution particle size Dv50 of the polymer particles of the phenol resin-based organic particles is within the above range, it is advantageous for the separation membrane to have excellent heat resistance and breathability.
[0105] Resol-type phenolic resin-based materials generally have relatively low electrochemical stability and cannot satisfy the electrochemical stability required for separators. Based on this, the present disclosure provides phenolic resin-based organic particles in which the first cycle cyclic voltammetry curve does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Embodiments of the present disclosure also provide a method for manufacturing said phenolic resin-based organic particles.
[0106] In some embodiments, a method for manufacturing phenol resin-based organic particles comprises the following steps: providing a resol-type phenol resin-based material; curing the resol-type phenol resin-based material in an oxygen-containing atmosphere at a first temperature for a first time, then curing it in an oxygen-containing atmosphere at a second temperature for a second time, and then crushing it again to obtain phenol resin-based organic particles. The first temperature is 100°C-170°C, and the second temperature is 220°C-290°C.
[0107] The embodiments of the present disclosure obtain phenolic resin-based organic particles with high electrochemical stability by curing a resol-type phenolic resin-based material in stages. First, the resol-type phenolic resin-based material is cured at 100°C to 170°C, and during this process, the resol-type phenolic resin-based material is gradually cured, and low molecular weight groups and easily oxidizable groups within the resol-type phenolic resin-based material begin to be removed; then, it is cured again at 220°C to 290°C, and during this process, the resol-type phenolic resin-based material continues the cross-linking curing reaction and is further sufficiently cured; additionally, the first stage curing and the second stage curing are selected to be performed in an oxygen-containing atmosphere, and curing in an oxygen-containing atmosphere allows the easily oxidizable groups of the resol-type phenolic resin-based material to be oxidized in advance. At this time, the phenolic structure is oxidized to a benzoquinone structure, and since the benzoquinone structure is not easily oxidized, thus, phenolic resin-based organic particles with high electrochemical stability can be obtained.
[0108] The phenolic resin-based organic particles produced in the present disclosure are thermosetting resist resin polymers.
[0109] In some embodiments, the oxygen-containing atmosphere may include oxygen and an inert gas, and the volume fraction of oxygen in the oxygen-containing atmosphere may be 5% to 50%. Optionally, the inert gas may include one or more of nitrogen, argon, and helium, but is not limited thereto.
[0110] Optionally, the volume fraction of oxygen in the oxygen-containing atmosphere can be 10%-30%.
[0111] More selectively, the oxygen-containing atmosphere can be an air atmosphere. This allows for further cost reduction.
[0112] The first temperature is 100℃-170℃, and may be a range consisting of, for example, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃, 140℃, 145℃, 150℃, 155℃, 160℃, 165℃, 170℃, or any of the above values.
[0113] Optionally, the first temperature may be 110℃-170℃, 110℃-160℃, 110℃-150℃, 120℃-170℃, 120℃-160℃, or 120℃-150℃.
[0114] If the first temperature is within the above range, the resol-type phenolic resin-based material can be cured more uniformly and sufficiently in the first step, so that phenolic resin-based organic particles with higher electrochemical stability can be obtained.
[0115] In some embodiments, the first time may be 2h-4h, and may be a range consisting of, for example, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h or any of the above values.
[0116] If the first time is within the above range, the resol-type phenolic resin-based material can be cured more uniformly and sufficiently in the first step, so that phenolic resin-based organic particles with higher electrochemical stability can be obtained.
[0117] The second temperature is 220℃-290℃, and may be a range consisting of, for example, 220℃, 225℃, 230℃, 235℃, 240℃, 245℃, 250℃, 255℃, 260℃, 265℃, 270℃, 275℃, 280℃, 285℃, 290℃, or any of the above values.
[0118] Optionally, the second temperature may be 220℃-280℃ or 220℃-270℃.
[0119] If the second temperature is within the above range, the deterioration (e.g., decomposition) of the phenol resin-based organic particles is prevented, and at the same time, the phenol resin-based organic particles can be further cured to further improve electrochemical stability.
[0120] In some embodiments, the second time may be 2h-6h, for example, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h, 6h, or a range consisting of any of the above values.
[0121] If the second time is within the above range, the phenol resin-based organic particles can be further cured sufficiently to further improve electrochemical stability.
[0122] In some embodiments, the method for manufacturing phenol resin-based organic particles further includes the step of performing sieving and magnetic foreign matter removal treatment after crushing treatment.
[0123] In some embodiments, the free phenol content of the resol-type phenolic resin-based material may be 5% or less, and optionally 4% or less, 3% or less, or 2% or less.
[0124] In some embodiments, the free aldehyde content of the resol-type phenolic resin-based material may be 5% or less, and optionally 4% or less, 3% or less, or 2% or less.
[0125] Low content of free phenol and free aldehyde is advantageous for obtaining phenol resin-based organic particles with higher electrochemical stability.
[0126] Resol-type phenolic resin-based materials may be commercially available products or synthesized according to methods known in the art. In some embodiments, a method for manufacturing a resol-type phenolic resin-based material includes the step of reacting a phenolic compound and an aldehyde compound under the catalyst of a basic substance to obtain a resol-type phenolic resin-based material.
[0127] Optionally, the molar ratio of the phenolic hydroxyl group of the phenolic compound to the aldehyde group of the aldehyde compound may be 1:1.1 to 1:1.5.
[0128] Optionally, the basic substance may include one or more of ammonia water, NaOH, and Na2CO3.
[0129] Optionally, the phenolic compound may include one or more of phenol, hydroquinone, resorcinol, catechol, cresol, and cardanol.
[0130] Optionally, the aldehyde compound may include one or more of formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, n-butylaldehyde, glyoxal, and furfural.
[0131] [Polymer particles containing triazine ring structural units]
[0132] The polymer particles containing triazine ring structure units of the present disclosure further include a cross-linking structure connecting the triazine ring structure units.
[0133] The molecular structure of the polymer particles containing triazine ring structure units contains multiple triazine ring structure units, and the cross-linking structure refers to a group connecting the triazine ring structure units, and each cross-linking structure is the same or different.
[0134] Optionally, the crosslinked structure may include one or more combinations of alkylene groups, alkylene ether groups, and alkylene amine groups.
[0135] In some embodiments, the triazine ring structure unit of the polymer particles containing the triazine ring structure unit may have additional substituents. The substituents may include a combination of one or more of alkyl groups, alkenyl groups, phenyl groups, cycloalkyl groups, amino groups, hydroxyl groups, and halogens.
[0136] In some embodiments, the polymer particles containing triazine ring structure units may include melamine aldehyde-based polymers and derivatives thereof.
[0137] In some embodiments, melamine aldehyde-based polymers and their derivatives may include melamine formaldehyde polymers and their derivatives.
[0138] Optionally, melamine aldehyde-based polymers and derivatives thereof may comprise one or more of melamine formaldehyde, benzoguanamine formaldehyde, melamine-benzoguanamine formaldehyde, melamine-(2,4-diamino-1,3,5-triazine) formaldehyde, melamine-(6-methyl-1,3,5-triazine-2,4-diamine) formaldehyde, melamine-(2,4,6-triethylamino-1,3,5-triazine) formaldehyde, trihydrazino-s-triazine formaldehyde, melamine-(2-amino-4-methylamino-1,3,5-triazine) formaldehyde, and melamine-(2,4-diamino-6-dimethylamino-1,3,5-triazine) formaldehyde.
[0139] In some embodiments, the polymer particles containing triazine ring structure units do not have a glass transition temperature of 300°C or lower.
[0140] The fact that polymer particles containing triazine ring structure units do not have a glass transition temperature at 300°C or lower indicates that the organic particles have excellent heat resistance and thermal stability, so the thermal shrinkage of the porous substrate can be more effectively suppressed to improve the heat resistance of the separator and improve the reliability of the secondary battery cell.
[0141] In some embodiments, the volume distribution particle size Dv50 of the polymer particles containing triazine ring structure units may be 200 nm to 840 nm.
[0142] If the volume distribution particle size Dv50 of the polymer particles containing triazine ring structure units is within the above range, it is advantageous for the separation membrane to have excellent heat resistance and breathability.
[0143] The present disclosure provides polymer particles containing triazine ring structure units, wherein the first cycle cyclic voltammetry curve does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Embodiments of the present disclosure also provide a method for manufacturing said polymer particles containing triazine ring structure units.
[0144] In some embodiments, a method for manufacturing polymer particles containing triazine ring structure units comprises the steps of: providing a triazine ring structure-containing precursor; and heat-curing the triazine ring structure-containing precursor in an oxygen-containing atmosphere and then crushing it again to obtain polymer particles containing triazine ring structure units, wherein the heat-curing temperature is 220°C to 290°C. When the triazine ring structure-containing precursor is heat-cured, a cross-linked structure is formed between the triazine ring structure units.
[0145] The heat curing temperature is 220℃-290℃, and may be a range consisting of, for example, 220℃, 225℃, 230℃, 235℃, 240℃, 245℃, 250℃, 255℃, 260℃, 265℃, 270℃, 275℃, 280℃, 290℃, or any of the above values.
[0146] By heat-curing a precursor containing a triazine ring structure at 220℃-290℃, polymer particles containing triazine ring structure units with high electrochemical stability can be obtained.
[0147] Optionally, the heat curing temperature may be 225℃-290℃, 230℃-290℃, 225℃-280℃, or 230℃-280℃.
[0148] In some embodiments, the heat curing time may be 3h to 6h, and may be a range consisting of, for example, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h, 6h or any of the above values.
[0149] If the heat curing time is within the above range, it is advantageous to form polymer particles containing triazine ring structure units with higher electrochemical stability from a precursor containing a triazine ring structure.
[0150] In some embodiments, the oxygen-containing atmosphere may include oxygen and an inert gas. Optionally, the inert gas may include one or more of nitrogen, argon, and helium, but is not limited thereto. In some embodiments, the volume fraction of oxygen in the oxygen-containing atmosphere may be 5% to 50%. Optionally, the volume fraction of oxygen in the oxygen-containing atmosphere may be 10% to 30%. More optionally, the oxygen-containing atmosphere may be an air atmosphere.
[0151] In some embodiments, the method for manufacturing polymer particles containing triazine ring structure units further includes the step of performing sieving and magnetic foreign matter removal treatment after crushing treatment.
[0152] In some embodiments, the triazine ring structure-containing precursor may comprise a melamine aldehyde-based resin. The melamine aldehyde-based resin may be obtained by reacting an aldehyde-based compound with an amine-substituted triazine compound, and the amine-substituted triazine compound may comprise melamine and / or melamine derivatives.
[0153] Optionally, the molar ratio of the aldehyde compound to the amine-substituted triazine compound may be 1.75:1 to 3:1, and may be, for example, a range consisting of 1.75:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3:1 or any of the above ratios.
[0154] More optionally, the molar ratio of the aldehyde compound to the amine-substituted triazine compound can be 2:1-3:1, 2.1:1-3:1, 2.2:1-3:1, 2.3:1-3:1, or 2.4:1-3:1.
[0155] In some embodiments, the aldehyde compound may include one or more of formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, n-butylaldehyde, glyoxal, and furfural.
[0156] In some embodiments, the amine-substituted triazine compound may comprise one or more of the compounds represented by the following general formulas, R1 and R2 are each independently selected from any one of H, -NH2 and C1-C8 alkyl, R3 is selected from any one of H, -NH2, -NHR4, C1-C8 alkyl, C2-C8 alkenyl, phenyl, C7-C12 alkylphenyl, C7-C12 phenylalkyl and C5-C8 cycloalkyl, and R4 is selected from any one of -NH2 and C1-C8 alkyl. Optionally, R3 is selected from -NH2 or -NHR4.
[0157]
[0158] Optionally, amine-substituted triazine compounds include melamine, benzoguanamine, 2,4-diamino-1,3,5-triazine, 6-methyl-1,3,5-triazine-2,4-diamine, 2,4,6-triethylamino-1,3,5-triazine, trihydrazinotriazine, 2-amino-4-methylamino-1,3,5-triazine, 2,4-diamino-6-dimethylamino-1,3,5-triazine, 6-ethyl-1,3,5-triazine-2,4-diamine, 6-isopropyl-1,3,5-triazine-2,4-diamine, 6-pentyl-2,4-diamino-1,3,5-triazine, 6-heptyl-2,4-diamino-triazine, 2-vinyl-4,6-diamino-1,3,5-triazine, It may include one or more of 2,4-diamino-6-(4-methylphenyl)-1,3,5-triazine, 6-cyclohexyl-1,3,5-triazine-2,4-diamine, 6-(3-methylphenyl)-1,3,5-triazine-2,4-diamine, 6-o-tolyl-1,3,5-triazine-2,4-diamine, 6-(2,4-dimethylphenyl)-1,3,5-triazine-2,4-diamine, 6-phenylmethyl-1,3,5-triazine-2,4-diamine, (diamino-1,3,5-triazine-2-yl)methanol, and 2-chloro-4,6-diamino-1,3,5-triazine.
[0159] More optionally, the amine-substituted triazine compound may include one or more of melamine, benzoguanamine, 2,4-diamino-1,3,5-triazine, 6-methyl-1,3,5-triazine-2,4-diamine, 2,4,6-triethylamino-1,3,5-triazine, trihydrazinotriazine, 2-amino-4-methylamino-1,3,5-triazine, and 2,4-diamino-6-dimethylamino-1,3,5-triazine.
[0160] [Cross-linked styrene-based organic particles]
[0161] Cross-linked styrene-based organic particles comprise styrene or styrene derivative structural units and cross-linked structural units. The cross-linked structural units of cross-linked styrene-based organic particles refer to structural units used to link styrene or styrene derivative structural units.
[0162] In some embodiments, the styrene or styrene derivative structural unit may include one or more of a styrene structural unit, a 1-methyl-1-styrene structural unit, a 4-methylstyrene structural unit, a 2-methylstyrene structural unit, a 2,4-dimethylstyrene structural unit, and a 2,5-dimethylstyrene structural unit.
[0163] In some embodiments, the crosslinking structural unit may include one or more of a divinylbenzene structural unit, an ethylene glycol dimethacrylate structural unit, a pentaerythritol tetraacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, an N,N-methylenebisacrylamide structural unit, an N,N'-vinylbisacrylamide structural unit, a 1,3,5-triacryloylhexahydro-1,3,5-triazine structural unit, and a trialyl isocyanurate structural unit.
[0164] In some embodiments, the glass transition temperature of cross-linked styrene-based organic particles T g It can be 110℃ to 154℃.
[0165] Cross-linked styrene-based organic particles glass transition temperature T g The high value provides excellent heat resistance and thermal stability. This allows for more effective suppression of thermal shrinkage of the porous substrate, thereby improving the heat resistance of the separator and enhancing the reliability of the secondary battery cell.
[0166] In some embodiments, the volume distribution particle size Dv50 of the cross-linked styrene-based organic particles may be 88 nm to 295 nm.
[0167] If the volume distribution particle size Dv50 of the cross-linked styrene-based organic particles is within the above range, it is advantageous for the separation membrane to have excellent heat resistance and breathability.
[0168] The present disclosure provides cross-linked styrene-based organic particles in which the first cycle cyclic voltammetry curve does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Embodiments of the present disclosure also provide a method for manufacturing said cross-linked styrene-based organic particles.
[0169] In some embodiments, a method for preparing cross-linked styrene-based organic particles comprises the step of providing a pre-emulsion comprising a monomer, a crosslinking agent, an emulsifier, an initiator, and water, and performing an emulsion polymerization reaction under conditions of heating, inert gas protection, and stirring to obtain cross-linked styrene-based organic particles, wherein the monomer comprises one or more of styrene and its derivatives, the aging temperature of the emulsion polymerization reaction is 80°C-92°C, and the aging time of the emulsion polymerization reaction is 1h-4h.
[0170] The aging temperature of the emulsion polymerization reaction is 80°C to 92°C, and may be a range consisting of, for example, 80°C, 81°C, 82°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, or any of the above values.
[0171] The aging time of the emulsion polymerization reaction is 1h-4h, and may be a range consisting of, for example, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h or any of the above values.
[0172] If the aging temperature and aging time of the emulsion polymerization reaction are within the above range, cross-linked styrene-based organic particles with high electrochemical stability can be obtained.
[0173] In some embodiments, the emulsion polymerization reaction may include the step of obtaining cross-linked styrene-based organic particles by adding a pre-emulsion dropwise to a reactor containing water under conditions of a first heating temperature, inert gas protection, and stirring, reacting for a first time, and then raising the temperature to an aging temperature to perform an aging reaction.
[0174] Optionally, the first heating temperature may be 55℃-70℃.
[0175] Optionally, the first hour can be 3h-7h.
[0176] In some embodiments, when the total mass of the monomer and the crosslinking agent is 100%, the mass fraction of the crosslinking agent may be 4% to 28%, for example, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 22%, 24%, 26%, 28%, or any of the above figures.
[0177] If the mass fraction of the crosslinking agent is within the above range, the electrochemical stability and heat resistance of the crosslinked styrene-based organic particles can be improved.
[0178] Optionally, the mass fraction of the crosslinking agent may be 6%-28%, 8%-28%, 10%-28%, 4%-26%, 6%-26%, 8%-26%, and 10%-26%.
[0179] In some embodiments, the solid content of the emulsion polymerization reaction system may be 10% to 25%, and may be a range consisting of, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, or any of the above figures. The solid content of the emulsion polymerization reaction system refers to the mass fraction of monomer and crosslinking agent in the reaction system.
[0180] If the solid content of the emulsion polymerization reaction system is within the above range, the conversion rate of the monomer can be increased and the electrochemical stability of the cross-linked styrene-based organic particles can be improved.
[0181] Optionally, the solid content of the emulsion polymerization reaction system can be 12%-25%, 14%-25%, or 16%-25%.
[0182] In some embodiments, the monomer may include one or more of styrene, 1-methyl-1-styrene, 4-methylstyrene, 2-methylstyrene, 2,4-dimethylstyrene, and 2,5-dimethylstyrene.
[0183] After the crosslinking agent and the monomer are polymerized, crosslinking structural units of crosslinked styrene-based organic particles are formed. In some embodiments, the crosslinking agent may include one or more of divinylbenzene, ethylene glycol dimethacrylate, pentaerythritol tetraacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,8-octanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol trimethacrylate, tetraethylene glycol dimethacrylate, tripropylene glycol diacrylate, N,N-methylenebisacrylamide, N,N'-vinylbisacrylamide, 1,3,5-triacryloylhexahydro-1,3,5-triazine, and trialyl isocyanurate.
[0184] Optionally, the crosslinking agent may include one or more of divinylbenzene, N,N-methylenebisacrylamide, and N,N'-vinylbisacrylamide.
[0185] In some embodiments, the emulsifier may include one or more of sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, sorbitan fatty acid ester, polysorbate, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl alcohol, polyoxyethylene ether emulsifier, cellulose, and derivatives thereof, but is not limited thereto.
[0186] Optionally, the polyoxyethylene ether emulsifier may include OP-based emulsifiers, such as OP-4, OP-7, OP-10, OP-15, OP-20, etc.
[0187] In some embodiments, when the total mass of the monomer and crosslinking agent is 100%, the mass fraction of the emulsifier may be 0.1% to 3%.
[0188] In some embodiments, the initiator may include one or more of sodium persulfate, potassium persulfate, ammonium persulfate, sodium sulfite, sodium bisulfite, azobis-isobutyramidine hydrochloride, azobis-isobutylimidazoline hydrochloride, and azobis-isopropylimidazoline, but is not limited thereto.
[0189] In some embodiments, when the total mass of the monomer and crosslinking agent is 100%, the mass fraction of the initiator may be 0.16%-3%, and optionally 0.2%-2%, 0.25%-2%.
[0190] In some embodiments, the method for manufacturing cross-linked styrene-based organic particles further includes the step of performing a magnetic foreign matter removal treatment after the emulsion polymerization reaction is completed.
[0191] [Silicon-containing organic resin particles]
[0192] In some embodiments, the silicon-containing organic resin particles are silicon-containing organic cross-linked resin particles, and the silicon-containing organic resin particles contain carbon-carbon bonds and a siloxane structure.
[0193] Optionally, silicon-containing organic resin particles have a network structure formed with carbon-carbon bonds as the main chain, and the side chains contain a siloxane structure.
[0194] Optionally, silicon-containing organic resin particles have a network structure formed with carbon-carbon bonds as the main chain, and the side chains contain siloxane structures and benzene ring structures.
[0195] In some embodiments, silicon-containing organic crosslinked resin particles comprise crosslinked structural units. The crosslinked structural units of the silicon-containing organic crosslinked resin particles refer to silicon-non-containing structural units used to link silicon-containing structural units.
[0196] Optionally, the crosslinking structural unit is a divinylbenzene structural unit, a diethylene glycol divinyl ether structural unit, a triethylene glycol divinyl ether structural unit, a diallyl maleate structural unit, an ethylene glycol dimethacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, a 2,2,4-trimethyladipoylbis[2-ethylaziridine] structural unit, a 1,1-azellaoilbis[2-methylaziridine] structural unit, a 1,1-(1,3-phenylenedicarbonyl)bis[2-methylaziridine] structural unit, It may include one or more of the trimethylolpropane tri(2-methyl-1-aziridinylpropionate) structural unit, the trimethylolpropane-tri[3-(2-methylaziridinyl)propionate] structural unit, and the pentaerythritol tri(3-aziridinyl)propionate structural unit.
[0197] The raw material for silicon-containing organic resin particles may include a monomer and a crosslinking agent, and the monomer may include a silane coupling agent containing an alkenyl group and / or an acryloyloxy group. After the crosslinking agent and the monomer are polymerized, crosslinked structural units of the silicon-containing organic crosslinked resin particles are formed. In some embodiments, the crosslinking agent may be a polyfunctional crosslinking agent. Optionally, the crosslinking agent is divinylbenzene, diethylene glycol divinyl ether, triethylene glycol divinyl ether, diallyl maleate, ethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,8-octanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol trimethacrylate, tetraethylene glycol dimethacrylate, tripropylene glycol diacrylate, 2,2,4-trimethyladipoylbis[2-ethylaziridine], 1,1-azellaoilbis[2-methylaziridine], 1,1-(1,3-phenylenedicarbonyl)bis[2-methylaziridine], trimethylolpropane tri(2-methyl-1-aziridinylpropionate), It may include one or more of trimethylolpropane-tri[3-(2-methylaziridinyl)propionate] and pentaerythritol tri(3-aziridinyl)propionate.
[0198] In some embodiments, silicon-containing organic resin particles do not have a glass transition temperature of 300°C or lower.
[0199] The fact that silicon-containing organic resin particles do not have a glass transition temperature at 300°C or lower indicates that the silicon-containing organic particles have excellent heat resistance and thermal stability, which allows for more effective suppression of thermal shrinkage of the porous substrate, improved heat resistance of the separator, and improved reliability of the secondary battery cell.
[0200] In some embodiments, the volume distribution particle size Dv50 of the silicon-containing organic resin particles may be 88 nm to 295 nm.
[0201] If the volume distribution particle size Dv50 of the silicon-containing organic resin particles is within the above range, it is advantageous for the separation membrane to have excellent heat resistance and breathability.
[0202] The present disclosure provides silicon-containing organic resin particles in which the first cycle cyclic voltammetry curve does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Embodiments of the present disclosure also provide a method for manufacturing said silicon-containing organic resin particles.
[0203] In some embodiments, a method for preparing silicon-containing organic resin particles comprises the step of providing a pre-emulsion comprising a monomer, a crosslinking agent, an emulsifier, an initiator, and water, and performing an emulsion polymerization reaction under conditions of heating, inert gas protection, and stirring to obtain silicon-containing organic resin particles. The monomer comprises a silane coupling agent containing alkenyl groups and / or acryloyloxy groups. When the total mass of the monomer and the crosslinking agent is 100%, the mass fraction of the crosslinking agent is 3% to 15%.
[0204] Since the monomer contains a silane coupling agent containing alkenyl groups and / or acryloyloxy groups, free radicals are generated between the monomers to cause a crosslinking reaction, and a crosslinking reaction also occurs between the monomer and the crosslinking agent. Therefore, when the monomer and crosslinking agent of the present disclosure are used as raw materials, silicon-containing organic resin particles with a three-dimensional network structure can be formed, which do not easily soften or deform at high temperatures and possess relatively high heat resistance and electrochemical stability.
[0205] When the total mass of the monomer and the crosslinking agent is 100%, the mass fraction of the crosslinking agent is 3%-15%, and may be, for example, a range consisting of 3%, 4%, 5%, 6%, 7%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15% or any of the above values.
[0206] If the mass fraction of the crosslinking agent is within the above range, silicon-containing organic resin particles with high electrochemical stability and excellent heat resistance can be obtained.
[0207] Optionally, the mass fraction of the crosslinking agent may be 8%-14%, 8%-13%, 8%-12%, 9%-14%, 9%-13%, or 9%-12%.
[0208] After the crosslinking agent and monomer are polymerized, crosslinking structural units of silicon-containing organic crosslinked resin particles are formed.
[0209] In some embodiments, the crosslinking agent may be a polyfunctional crosslinking agent.
[0210] Optionally, the crosslinking agent is divinylbenzene, diethylene glycol divinyl ether, triethylene glycol divinyl ether, diallyl maleate, ethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,8-octanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol trimethacrylate, tetraethylene glycol dimethacrylate, tripropylene glycol diacrylate, 2,2,4-trimethyladipoylbis[2-ethylaziridine], 1,1-azellaoilbis[2-methylaziridine], 1,1-(1,3-phenylenedicarbonyl)bis[2-methylaziridine], trimethylolpropane tri(2-methyl-1-aziridinylpropionate), It may include one or more of trimethylolpropane-tri[3-(2-methylaziridinyl)propionate] and pentaerythritol tri(3-aziridinyl)propionate.
[0211] In some embodiments, the monomer may include a vinylsilane coupling agent and / or an acryloyloxysilane coupling agent.
[0212] Optionally, the monomer is γ-methacryloyloxypropyltris(trimethylsiloxy)silane, (3-acryloyloxypropyl)tris(trimethylsiloxy)silane, 3-methacryloyloxypropyltrimethoxysilane, acryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, acryloyloxypropyltriethoxysilane, γ-methacryloyloxypropyltriisopropoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-methacryloyloxypropyltris(methoxyethoxy)silane, vinyltrimethoxysilane, 7-octenyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, tri-tert-butoxyvinylsilane, vinyltris(β-methoxyethoxy)silane, It may include one or more of ethylenetris[(1-methylvinyl)oxy]silane, vinyltri-tert-butylperoxysilane, 3-methacryloyloxypropylmethyldimethoxysilane, 3-acryloyloxypropylmethyldimethoxysilane, methacryloyloxypropyldimethylmethoxysilane, (3-acryloyloxy)dimethylmethoxysilane, 3-methacryloyloxypropyldimethylethoxysilane, diethylmethylvinylsilane, vinyldimethylethoxysilane, methylvinyldiethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, methylvinyldimethoxysilane, and 3-(methacryloyloxy)propylmethyldiethoxysilane.
[0213] In some embodiments, the monomer may include a first monomer and a second monomer.
[0214] The first monomer is γ-methacryloyloxypropyltris(trimethylsiloxy)silane, (3-acryloyloxypropyl)tris(trimethylsiloxy)silane, 3-methacryloyloxypropyltrimethoxysilane, acryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, acryloyloxypropyltriethoxysilane, γ-methacryloyloxypropyltriisopropoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, 3-methacryloyloxypropyltris(methoxyethoxy)silane, vinyltrimethoxysilane, 7-octenyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, tri-tert-butoxyvinylsilane, vinyltris(β-methoxyethoxy)silane, It may include one or more of ethylenetris[(1-methylvinyl)oxy]silane and vinyltri-tert-butylperoxysilane.
[0215] The second monomer may include one or more of 3-methacryloyloxypropylmethyldimethoxysilane, 3-acryloyloxypropylmethyldimethoxysilane, methacryloyloxypropyldimethylmethoxysilane, (3-acryloyloxy)dimethylmethoxysilane, 3-methacryloyloxypropyldimethylethoxysilane, diethylmethylvinylsilane, vinyldimethylethoxysilane, methylvinyldiethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, methylvinyldimethoxysilane, and 3-(methacryloyloxy)propylmethyldiethoxysilane.
[0216] Since the first monomer and the second monomer have different activities, silicon-containing organic resin particles with a narrow particle size distribution can be obtained by combining them and reacting them with a crosslinking agent.
[0217] In some embodiments, the emulsifier may comprise, but is not limited to, one or more of alkyl sulfates, alkyl sulfonates, Tween-based emulsifiers, aliphatic alcohol polyoxyethylene ethers, aliphatic alcohol polyoxypropylene ethers, ceteareth, and oleth. Optionally, the emulsifier comprises one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, Tween 20, Tween 40, laureth-7, laureth-9, laureth-10, and oleth-10.
[0218] In some embodiments, the initiator may include one or more of sodium persulfate, potassium persulfate, ammonium persulfate, sodium sulfite, sodium bisulfite, azobis-isobutyronitrile, azobis-isobutyramidine hydrochloride, azobis-isobutylimidazoline hydrochloride, and azobis-isopropylimidazoline, but is not limited thereto.
[0219] In some embodiments, the heating temperature of the emulsion polymerization reaction aging step may be 75°C-85°C, and may be a range consisting of, for example, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C or any of the above values.
[0220] In some embodiments, the heating time of the emulsion polymerization reaction aging step may be 1h to 4h, and may be a range consisting of, for example, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h or any of the above values.
[0221] In some embodiments, the emulsion polymerization reaction may include the step of obtaining silicon-containing organic resin particles by adding a pre-emulsion dropwise to a reactor containing water under conditions of a second heating temperature, inert gas protection, and stirring, reacting for a second time, and then raising the temperature to the heating temperature of the aging step to perform an aging reaction.
[0222] Optionally, the second heating temperature may be 55℃-70℃.
[0223] Optionally, the second time can be 3h-8h.
[0224] In some embodiments, the pre-emulsion may further comprise a pH adjuster. Optionally, the pH adjuster may comprise one or more of sodium bicarbonate, sodium hydroxide, and ammonia water, but is not limited thereto.
[0225] In some embodiments, the method for manufacturing silicon-containing organic resin particles may further include a step of performing a magnetic foreign matter removal treatment after the emulsion polymerization reaction is completed.
[0226] In some embodiments, based on the total mass of the coating layer, the mass content of organic particles in the coating layer may be 50% to 99%.
[0227] Optionally, the mass content of organic particles in the coating layer may be 60%-99%, 70%-99%, 80%-99%, 85%-99%, 88%-99%, 80%-97%, 85%-97%, 88%-97%, 80%-95%, 85%-95%, 88%-95%.
[0228] In some embodiments, the binder in the coating layer may include one or more of a polyacrylate-based binder, a nitrile rubber-based binder, polyacrylic acid, polymethacrylic acid, sodium polyacrylate, polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS), but is not limited thereto.
[0229] In some embodiments, the coating layer may further comprise a dispersant, for example, a polyacrylic acid-based dispersant or a carboxymethylcellulose-based dispersant, but is not limited thereto. As an example, the dispersant may comprise one or more of sodium carboxymethylcellulose, sodium polyacrylate, and ammonium polyacrylate, but is not limited thereto.
[0230] In some embodiments, the separator may further include polymer binder particles. The “polymer binder particles” serve to improve adhesion between the separator and the electrode plate in the separator and basically do not possess high temperature resistance.
[0231] In some embodiments, polymer binder particles may be embedded between organic particles and form protrusions on the surface of the coating layer.
[0232] In some other embodiments, the coating layer of the separator comprises a heat-resistant layer and an adhesive layer, the heat-resistant layer is disposed on a porous substrate, the adhesive layer is disposed on at least a portion of the surface of the heat-resistant layer on the side far from the porous substrate, organic particles are disposed on the heat-resistant layer, and polymer binder particles are disposed on the adhesive layer.
[0233] In another embodiment, the coating layer of the separator comprises a heat-resistant layer and an adhesive layer, the heat-resistant layer is disposed on one side of the porous substrate, the adhesive layer is disposed on at least a portion of the other side surface of the porous substrate, organic particles are disposed on the heat-resistant layer, and polymer binder particles are disposed on the adhesive layer.
[0234] In some embodiments, the average particle size of the polymer binder particles may be 6 μm to 18 μm.
[0235] The average particle size of the particles to be measured can be tested according to the following method: An SEM image of the membrane is obtained using a scanning electron microscope with reference to JY / T 010-1996. One test sample with dimensions of 50 mm × 100 mm (length × width) is randomly selected from the membrane, and multiple test regions (e.g., 5) are randomly selected from the test sample. The particle size of the particles to be measured in each test region is read at a constant magnification (e.g., 500x or more); the number of particles to be measured and their particle size values present in each test region are aggregated, and the arithmetic mean of the particle sizes of all particles to be measured present in each test region is taken as the average particle size of the particles to be measured. To ensure the accuracy of the test results, multiple test samples (e.g., 10) may be taken to perform the above test, and the average value of each test sample may be used as the final test result. The test instrument may be a ZEISS Sigma 300. If the particles to be measured have an irregular shape, the distance between the two farthest points on the particles to be measured is taken as the particle size of the particles to be measured.
[0236] In some embodiments, the polymer binder particles may include vinylidene fluoride-based polymer particles, for example, polyvinylidene fluoride (PVDF) particles and / or copolymer particles of vinylidene fluoride monomer and comonomer.
[0237] The comonomer may include at least one of an olefin monomer, a fluorine-containing olefin monomer, a chlorine-containing olefin monomer, an acrylate-based monomer, an acrylic acid-based monomer, and a fluoroether-based monomer.
[0238] Optionally, the comonomer may comprise at least one of trifluoroethylene, chlorotrifluoroethylene, 1,2-difluoroethylene, tetrafluoroethylene, hexafluoropropylene, perfluoro(alkyl vinyl) ether (e.g., perfluoro(methyl vinyl) ether, perfluoro(ethyl vinyl) ether, perfluoro(propyl vinyl) ether), perfluoro(1,3-dioxol), and perfluoro(2,2-dimethyl-1,3-dioxol).
[0239] In some embodiments, the thickness of the coating layer may be 0.5 μm to 5 μm. The thickness of the coating layer refers to the thickness of the coating layer located on one side of the porous substrate. Optionally, the thickness of the coating layer may be 0.5 μm to 4 μm, 0.5 μm to 3 μm, 0.5 μm to 2 μm, 0.6 μm to 4 μm, 0.6 μm to 3 μm, 0.6 μm to 2 μm, 0.8 μm to 4 μm, 0.8 μm to 3 μm, or 0.8 μm to 2 μm.
[0240] In some embodiments, the areal density of the coating layer is 0.45 g / m² 2 -5g / m 2 It could be.
[0241] In some embodiments, the porous substrate may comprise a film or nonwoven web composed of any one or at least two of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cycloolefin copolymer, polyphenylene sulfide, and polyethylene naphthalate.
[0242] The porous substrate may be a single-layer film or a multilayer composite film. In the case where the porous substrate is a multilayer composite film, the material of each layer may be the same or different.
[0243] In some embodiments, the thickness of the porous substrate may be 4 μm to 12 μm, and optionally 4 μm to 9 μm.
[0244] In some embodiments, the porosity of the porous substrate may be 25%-60%, and optionally 28%-50%.
[0245] In some embodiments, the ratio of the volume distribution particle size Dv50 of the organic particles to the average pore diameter of the porous substrate may be 1.2 or higher.
[0246] The volume distribution particle size Dv50 of organic particles and the average pore diameter of the porous substrate use the same unit, for example, nm.
[0247] This can reduce pore clogging problems and improve the breathability and ion conductivity characteristics of the separation membrane.
[0248] In some embodiments, the average pore diameter of the porous substrate may be 25 nm to 82 nm.
[0249] The average pore diameter of a porous substrate can be tested using a capillary porosity tester (bubble point method). An exemplary test method is as follows: Take a circular sample with a diameter of 25 mm and place 3 to 5 drops of wetting liquid on it. After the sample is fully wetted, place it in a mold, and then use an inert gas (e.g., nitrogen) to push the wetting liquid out of the pores of the sample under measurement. The pressurized pressure and flow rate are inversely proportional to the pore diameter, and the average pore diameter of the sample under measurement is obtained through sampling via software and pressure-pore diameter conversion analysis. The test instrument may be a PMI CFP 1500 type pore diameter analyzer, and the test pressure may be between 100 psi and 350 psi.
[0250] In some embodiments, the thickness of the separator may be 5μm-14μm, and optionally 5μm-12μm or 6μm-12μm. This is advantageous for improving the energy density of the secondary battery cell.
[0251] glass transition temperature T g It can be tested according to the following method: Take an appropriate amount of sample (e.g., 5 mg–15 mg) and place it in the crucible of a Differential Scanning Calorimeter (DSC), shake to level it, and then close the crucible lid; set the measurement conditions to a nitrogen atmosphere, a purge gas flow rate of 60 mL / min, and a shielding gas flow rate of 20 mL / min; set the measurement program to heat from 25°C to 200°C at a heating rate of 10°C / min, hold for 5 min to remove thermal history, then cool from 200°C to -40°C at a cooling rate of 10°C / min, and then heat again to 300°C at a heating rate of 10°C / min. The glass transition temperature of the organic particles is determined through the DSC curve. T g to obtain or organic particles glass transition temperature T g Determines whether it has.
[0252] glass transition temperatureT g represents the transition temperature from the glassy state to the hyperelastic state, which indicates a step-like change in the DSC curve.
[0253] Glass transition temperature of organic particles at 300°C or below T g Not having means that the DSC curve of the organic particles does not show a step-like change within the range of 300°C or lower.
[0254] Dv50 represents the particle size corresponding when the cumulative volume distribution percentage of the material reaches 50%, and can be tested using a laser particle size analyzer in reference to GB / T 19077-2016. For the test, 1 g of the sample to be measured is placed in a clean small beaker, 20 ml of deionized water is added, and the sample is completely dispersed by ultrasonic treatment at 53 kHz / 120 W for 5 min; the laser particle size analyzer is operated, the optical system is cleaned, and the background is automatically measured; the ultrasonically treated solution to be measured is stirred to disperse it uniformly, placed in a sample cell according to the requirements, and the particle size measurement is started. The test instrument may be a MasterSizer 3000 laser particle size analyzer.
[0255] It must be explained that the parameters regarding the coating layer of the above-mentioned separation membrane are all parameters of the coating layer located on one side of the porous substrate. If the coating layer is disposed on both sides of the porous substrate, and the parameters of the coating layer on either side satisfy the present disclosure, it is deemed to be included within the scope of protection of the present disclosure.
[0256] The separator can be manufactured according to methods known in the art.
[0257] In some embodiments, a slurry containing organic particles and a binder is applied to at least one side of a porous substrate, and after drying, a separation membrane can be obtained.
[0258] In some embodiments, the slurry may further include polymer binder particles. After the slurry is dried, the polymer binder particles are embedded between the organic particles and form protrusions on the surface of the coating layer.
[0259] In some embodiments, a method for manufacturing a separator may include the steps of: applying a heat-resistant layer slurry containing organic particles and a binder to at least one side of a porous substrate and forming a heat-resistant layer after drying; and applying an adhesive layer slurry containing polymer binder particles and a binder to at least a portion of the surface of the heat-resistant layer and obtaining a separator after drying.
[0260] In some embodiments, a method for manufacturing a separation membrane may include the step of applying a heat-resistant slurry containing organic particles and a binder to one side of a porous substrate, applying an adhesive layer slurry containing polymer binder particles and a binder to at least a portion of the other side surface of the porous substrate, and obtaining a separation membrane after drying.
[0261] In some embodiments, the solvent of the slurry may be water, for example, deionized water.
[0262] In some embodiments, the slurry may further include other components, such as a dispersant and / or a wetting agent.
[0263] Embodiments of the present disclosure also provide a secondary battery cell. The secondary battery cell includes a separator provided in the embodiments of the present disclosure.
[0264] The secondary battery cell further comprises a positive plate, a negative plate, and an electrolyte, and a separator is disposed between the positive plate and the negative plate. The positive plate, separator, and negative plate can form an electrode assembly through a winding process and / or a lamination process.
[0265] The secondary battery cells provided in the present disclosure may include, but are not limited to, lithium battery cells, sodium battery cells, etc. Depending on the type of secondary battery cell, the composition of the positive plate, negative plate, and electrolyte may vary.
[0266] [Polar Plate]
[0267] In some embodiments, the positive plate may include a positive current collector and a positive film layer disposed on at least one surface of the positive current collector and comprising a positive active material. For example, the positive current collector has two surfaces facing each other in its thickness direction, and the positive film layer is disposed on either or both of the two surfaces facing each other of the positive current collector.
[0268] Taking a lithium battery cell as an example, the cathode active material may include, but is not limited to, one or more of lithium transition metal oxides, lithium-containing phosphates, and modified compounds thereof. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and modified compounds thereof. Examples of lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, composite materials of lithium iron phosphate and carbon, lithium manganese phosphate, composite materials of lithium manganese phosphate and carbon, lithium iron manganese phosphate, composite materials of lithium iron manganese phosphate and carbon, and modified compounds thereof. In some embodiments, to further improve the energy density of the secondary battery cell, the cathode active material is of the general formula Li a Ni b Co c M d O e A fIt may include one or more of the lithium transition metal oxides represented by and their modified compounds. Here, 0.8≤a≤1.2, 0.5≤b<1, 0 <c<1, 0<d<1, 1≤e≤2, 0≤f≤1이고, M은 Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti 및 B 중 하나 이상을 포함할 수 있으나 이에 한정되지 않으며, A는 N, F, S 및 Cl 중 하나 이상을 포함할 수 있으나 이에 한정되지 않는다.
[0269] As an example, the cathode active material is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.1 Al 0.05 It may include one or more of O2, LiFePO4, and LiMnPO4, but is not limited thereto.
[0270] Secondary battery cells involve the deinsertion and consumption of Li during the charging and discharging process, and the molar content of Li changes as the secondary battery cell is discharged to different states. Among the cathode active materials listed in this disclosure, the molar content of Li is based on the initial state of the material, that is, the state before the input of raw materials. When the cathode active material is applied to a secondary battery cell and undergoes charge-discharge cycles, the molar content of Li changes. Among the cathode active materials listed in this disclosure, the molar content of O is merely a theoretical state value, and the molar content of O may change due to the release of lattice oxygen, and fluctuations may also appear in the actual molar content of O.
[0271] Taking a sodium battery cell as an example, the positive electrode active material may include, but is not limited to, one or more of sodium-containing transition metal oxides, polyanionic materials (e.g., phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials. As an example, the positive electrode active material may be NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, or NaNi 1 / 2 Ti 1 / 2 O2, NaNi 1 / 2 Mn 1 / 2 O2, Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2, NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials and general formula X p M' q (PO4) r O x Y 3-x It may include one or more of the materials indicated by, but is not limited to. General formula X p M' q (PO4) r O x Y 3-x In, 0 <p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2이고, X는 H + , Li + , Na + , K + and NH4 + It includes, but is not limited to, one or more of the following, M' is a transition metal cation and optionally includes, but is not limited to, one or more of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion and optionally may be one or more of F, Cl and Br.
[0272] The modified compound of the positive electrode active material of each of the above lithium battery cells and sodium battery cells may be one in which doping modification and / or surface coating modification has been performed on the positive electrode active material.
[0273] In some embodiments, the anode film layer may further include an anode conductive agent. As an example, the anode conductive agent may include, but is not limited to, one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0274] In some embodiments, the anode film layer may further include an anode binder. As an example, the anode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate-based resin, but is not limited thereto.
[0275] In some embodiments, the positive current collector may use a metal foil or a composite current collector. An example of a metal foil may be aluminum foil. The composite current collector may include a polymer material substrate layer and a metal material layer formed on at least one surface of the polymer material substrate layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, but is not limited thereto. As an example, the polymer material substrate layer may include one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene, and polyethylene, but is not limited thereto.
[0276] The anode film layer is typically formed by applying an anode slurry onto an anode current collector, drying, and cold rolling. The anode slurry is typically formed by dispersing an anode active material, an anode conductive agent, an anode binder, and any other components in a solvent and stirring uniformly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto.
[0277] [Cathode]
[0278] In some embodiments, the cathode plate may include a cathode current collector and a cathode film layer disposed on at least one surface of the cathode current collector and comprising a cathode active material. For example, the cathode current collector has two surfaces facing each other in its thickness direction, and the cathode film layer is disposed on either or both of the two surfaces facing each other of the cathode current collector.
[0279] The negative electrode active material may be a material for a secondary battery cell known in the art. As an example, the negative electrode active material may include one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, but is not limited thereto. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloy materials, but are not limited thereto. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials, but are not limited thereto.
[0280] In some embodiments, the cathode film layer may further comprise a cathode conductive agent. As an example, the cathode conductive agent may comprise one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, but is not limited thereto.
[0281] In some embodiments, the cathode film layer may further include a cathode binder. As an example, the cathode binder may include, but is not limited to, one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0282] In some embodiments, the cathode film layer may further include other auxiliary agents. As an example, other auxiliary agents may include thickeners, such as sodium carboxymethylcellulose (CMC), PTC thermistor materials, etc.
[0283] In some embodiments, the negative current collector may use a metal foil or a composite current collector. Copper foil may be used as an example of a metal foil. The composite current collector may include a polymer material substrate layer and a metal material layer formed on at least one surface of the polymer material substrate layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, but is not limited thereto. As an example, the polymer material substrate layer may include one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene, and polyethylene, but is not limited thereto.
[0284] The cathode film layer is typically formed by applying a cathode slurry onto a cathode current collector, drying, and cold rolling. The cathode slurry is typically formed by dispersing a cathode active material, a cathode conductive agent, a cathode binder, and other optional auxiliary agents in a solvent and stirring uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.
[0285] The cathode plate does not exclude additional functional layers other than the cathode film layer. For example, in some embodiments, the cathode plate further comprises a conductive underlayer (e.g., composed of a conductive agent and a binder) interposed between the cathode current collector and the cathode film layer and disposed on the surface of the cathode current collector.
[0286] In some embodiments, the cathode plate may use a foamed metal. The foamed metal may be foamed nickel, foamed copper, foamed aluminum, foamed alloy, foamed carbon, etc. When a foamed metal is used as the cathode plate, the cathode active material may not be disposed on the surface of the foamed metal, or the cathode active material may be disposed on the surface of the foamed metal.
[0287] [Electrolyte]
[0288] The electrolyte acts as an ion conductor between the positive and negative plates.
[0289] In some embodiments, an electrolyte is used as the electrolyte, and the electrolyte comprises an electrolyte salt and an organic solvent.
[0290] For example, in a lithium battery cell, the electrolyte salt may include, but is not limited to, one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonylimide (LiFSI), lithium bistrifluoromethanesulfonylimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP), and lithium tetrafluorooxalatophosphate (LiTFOP).
[0291] For example, in a sodium battery cell, the electrolyte salt may include, but is not limited to, one or more of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bisfluorosulfonylimide (NaFSI), sodium bistrifluoromethanesulfonylimide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium bisoxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobisoxalatophosphate (NaDFOP), and sodium tetrafluorooxalatophosphate (NaTFOP).
[0292] In some embodiments, the organic solvent is ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulforain (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), diethyl sulfone (ESE), ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol It may include one or more of dimethyl ether, 1,3-dioxolane, tetrahydrofuran, methyltetrahydrofuran, diphenyl ether, and crown ether, but is not limited thereto.
[0293] In some embodiments, the electrolyte may further include additives. For example, the additives may include a cathode film-forming additive and an anode film-forming additive, and may also include additives that can improve some performance of the secondary battery cell, such as an additive that improves overcharge performance, an additive that improves high temperature performance, an additive that improves low temperature performance, etc.
[0294] Optionally, the additive may include one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC), 1,3-propane sulfone (PS), and ethylene sulfate (DTD).
[0295] A method for manufacturing a secondary battery cell is known. In some embodiments, a secondary battery cell can be formed by assembling a positive plate, a separator, a negative plate, and an electrolyte. As an example, a positive plate, a separator, and a negative plate can be formed into an electrode assembly through a winding process and / or a lamination process, the electrode assembly can be placed in an outer casing and dried, the electrolyte can be injected, and a secondary battery cell can be obtained through processes such as vacuum sealing, settling, and formation.
[0296] Examples
[0297] The following examples further elaborate upon the contents disclosed herein. These examples are for illustrative purposes only, and it will be apparent to those skilled in the art that various modifications and changes are possible within the scope of the contents disclosed herein. Unless otherwise specified, all parts, percentages, and ratios described in the following examples are based on mass. Furthermore, all reagents used in the examples may be commercially available or obtained by synthesis according to conventional methods and may be used directly without further processing, and all equipment used in the examples may also be commercially available.
[0298] A commercially available resol-type phenolic resin material made from phenol and formaldehyde was used, with a free phenol content of 4% and a free aldehyde content of 2%. The resol-type phenolic resin material was placed in a curing furnace, the atmosphere was set to an air atmosphere, and the temperature was set to 140°C. The material was then cured for 3 hours while maintaining the above temperature; after completion, the temperature of the curing furnace was raised to 275°C and cured for 4 hours while maintaining the above temperature. After the second curing cycle was completed, the cured phenolic resin material was removed and left to cool naturally in the air. Subsequently, it underwent crushing, sand milling, sieving, and magnetic foreign matter removal treatments to obtain phenolic resin-based organic particles 1-1#.
[0299] A commercially available resol-type phenolic resin material made from phenol and formaldehyde was used, with a free phenol content of 4% and a free aldehyde content of 2%. The resol-type phenolic resin material was placed in a curing furnace, the atmosphere was set to an air atmosphere, and the temperature was set to 140°C. The material was then cured for 3 hours while maintaining the above temperature; after completion, the temperature of the curing furnace was raised to 290°C and cured for 4 hours while maintaining the above temperature. After the second curing cycle was completed, the cured phenolic resin material was removed and left to cool naturally in the air. Subsequently, it underwent crushing, sand milling, sieving, and magnetic foreign matter removal treatments to obtain phenolic resin-based organic particles 1-2#.
[0300] A commercially available resol-type phenolic resin material made from phenol and formaldehyde was used, with a free phenol content of 4% and a free aldehyde content of 2%. The resol-type phenolic resin material was placed in a curing furnace, the atmosphere was set to an air atmosphere, and the temperature was set to 140°C. The material was then cured for 3 hours while maintaining the above temperature; after completion, the temperature of the curing furnace was raised to 260°C and cured for 4 hours while maintaining the above temperature. After the second curing cycle was completed, the cured phenolic resin material was removed and left to cool naturally in the air. Subsequently, it underwent crushing, sand milling, sieving, and magnetic removal to obtain phenolic resin-based organic particles 1-3#.
[0301] A commercially available resol-type phenolic resin material made from phenol and formaldehyde was used, with a free phenol content of 10% and a free aldehyde content of 10%. The resol-type phenolic resin material was placed in a curing furnace, the atmosphere was set to an air atmosphere, and the temperature was set to 140°C. The material was then cured for 3 hours while maintaining the above temperature. After the curing was completed, the cured phenolic resin material was removed and left to cool naturally in the air. Subsequently, the material underwent crushing, sand milling, sieving, and magnetic removal to obtain phenolic resin-based organic particles D1-1#.
[0302] Organic particle performance test
[0303] Glass transition temperature of organic particles T g test
[0304] An appropriate amount of sample (e.g., 5 mg–15 mg) was taken and placed into the crucible of a Differential Scanning Calorimeter (DSC), shaken to level it, and then the crucible lid was closed; the measurement conditions were set to a nitrogen atmosphere, a purge gas flow rate of 60 mL / min, and a shielding gas flow rate of 20 mL / min; the measurement program was set to heat from 25°C to 200°C at a heating rate of 10°C / min, hold for 5 min to remove thermal history, cool from 200°C to -40°C at a cooling rate of 10°C / min, and then heat again to 300°C at a heating rate of 10°C / min. The glass transition temperature of the organic particles was determined through the DSC curve. T g Calculate or the glass transition temperature of organic particles T g It was determined whether it has.
[0305] (2) Melting point test of organic particles
[0306] An appropriate amount of sample (e.g., 5 mg–15 mg) was taken and placed into the crucible of a differential scanning calorimeter (DSC), shaken to level it, and then the crucible lid was closed; the measurement conditions were set to a nitrogen atmosphere, a purge gas flow rate of 60 mL / min, and a shielding gas flow rate of 20 mL / min; the measurement program was set to heat from 25°C to 200°C at a heating rate of 10°C / min, hold for 5 min to remove thermal history, then cool from 200°C to -40°C at a cooling rate of 10°C / min, and then heat again to 300°C at a heating rate of 10°C / min. Whether the organic particles had a melting point was determined through the DSC curve.
[0307] (3) Cyclic voltage and current test
[0308] A slurry was prepared by dissolving organic particles, a binder (polyacrylate), and a conductive agent (conductive carbon black) in water at a solid mass ratio of 64:7:29. A coin cell was assembled by applying the slurry to aluminum foil to use as the anode and using lithium foil as the cathode; Cyclic Voltammetry (CV) tests were performed on the coin cell at a scan rate of 0.10 mV / s and a voltage range of 2.50 V–5.00 V, with a total of three cycles performed. The voltage corresponding to the peak onset point of the first cycle cyclic voltammetry curve was set as the oxidation peak potential. The electrolyte salt of the test electrolyte was LiPF6, and the concentration was 1 mol / L. The solvent for the electrolyte was prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7.
[0309] The organic particles 1-1# to 1-3# prepared above satisfied the following characteristics: the phenolic resin-based organic particles are thermosetting resist resin polymers, have no melting point, and have a glass transition temperature of 300°C or lower. T g did not have.
[0310] Next, the organic particles prepared above were applied to a separator, and the effect on the performance of the separator and the secondary battery cell was verified.
[0311] The membrane manufacturing process is as follows.
[0312] A commercially available polyethylene microporous film with a thickness of 7 μm was used as a porous substrate; the organic particles prepared above, sodium carboxymethylcellulose as a dispersant, and polyacrylate as a binder were added to deionized water such that the solid mass ratio of the organic particles, dispersant, and binder was 90:2:8, and the mixture was uniformly stirred and mixed to obtain a coating layer slurry; the coating layer slurry was uniformly applied to both surfaces of the porous substrate and dried to remove the solvent, after which a separation membrane was obtained. The thickness of the coating layer was 1.5 μm, and the thickness of the separation membrane was 10 μm.
[0313] The manufacturing process of a secondary battery cell is as follows.
[0314] Cathode active material LiNi 0.6 Co 0.2 Mn 0.2 An anode slurry was prepared by adding O2, polyvinylidene fluoride (PVDF) as an anode binder, and carbon black as an anode conductive agent to N-methylpyrrolidone (NMP) in a mass ratio of 97:2:1 and mixing them uniformly by stirring sufficiently; the anode slurry was uniformly coated onto an aluminum foil serving as an anode current collector, and then subjected to drying, cold rolling, and slitting to obtain an anode plate.
[0315] A cathode slurry was prepared by adding artificial graphite as a cathode active material, acetylene black as a cathode conductive agent, styrene-butadiene rubber (SBR) as a cathode binder, and sodium carboxymethylcellulose as a thickener to deionized water in a mass ratio of 96.0:1.5:1.5:1 and mixing them uniformly by stirring sufficiently; the cathode slurry was uniformly coated onto a copper foil as a cathode current collector, and then subjected to drying, cold rolling, and slitting to obtain a cathode plate.
[0316] At 25°C, a mixed solvent was prepared by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then LiPF6 and fluoroethylene carbonate (FEC) were dissolved in the mixed solvent to obtain an electrolyte. The concentration of LiPF6 was 1 mol / L. The mass fraction of FEC was 3% based on the mass of the electrolyte.
[0317] An electrode assembly was obtained by stacking a positive plate, a separator, and a negative plate in sequence, winding them, and then hot-press molding. Subsequently, the electrode assembly was placed in an aluminum plastic film and sealed on the top and sides. Then, a pouch-type secondary battery cell was obtained by undergoing processes such as electrolyte injection, settling, formation, aging, gas ejection, and secondary sealing.
[0318] Performance test
[0319] Thermal shrinkage rate test of separator membrane
[0320] For the thermal shrinkage rate test of the separator, refer to GB / T 36363-2018.
[0321] The separator was punched out into a sample with a width of 50 mm and a length of 100 mm using a press. After placing five parallel samples on an A4 sheet of paper, the A4 sheet with the samples on it was placed on a corrugated cardboard with a thickness of 1 mm to 5 mm.
[0322] The temperature of the hot air circulation oven was set to 130°C, and the temperature was stabilized for 60 minutes after reaching the set temperature. Then, an A4 sheet of paper placed on a corrugated cardboard was placed in the hot air circulation oven, and time measurement was started. After reaching the set time (1h in this disclosure), the length and width of the separator were measured, and the values were indicated as a and b, respectively.
[0323] The thermal shrinkage rate was calculated as follows: longitudinal (MD) thermal shrinkage rate = [(100-a) / 100]×100%, transverse (TD) thermal shrinkage rate = [(50-b) / 50]×100%, and the average value of three parallel samples was taken as the test result.
[0324] (2) Initial Coulomb efficiency test of a secondary battery cell
[0325] At 25℃, the secondary battery cell was charged to 4.5V with a constant current of 1 / 3C, and then charged again at a constant voltage of 4.5V until the current reached 0.05C. After leaving it for 5 minutes, it was discharged again to 2.8V with a constant current of 1 / 3C to obtain the initial charge capacity and initial discharge capacity. Initial Coulomb efficiency of the secondary battery cell = Initial discharge capacity / Initial charge capacity × 100%.
[0326] [Table 1]
[0327]
[0328] As can be seen from the above test results, the phenol resin-based organic particles prepared in the embodiments of the present disclosure have relatively high electrochemical stability and can improve the heat resistance of the separator and the initial Coulomb efficiency of the high-voltage secondary battery cell.
[0329] Next, the phenol resin-based organic particles were replaced with polymer particles containing triazine ring structure units.
[0330] Commercial resol-type melamine formaldehyde resin particles were cured at 285°C for 5 hours in an air atmosphere, followed by crushing, sand milling, sieving, and magnetic foreign matter removal treatment to obtain polymer particles 2-1# containing triazine ring structure units. The molar ratio of formaldehyde and melamine, which are raw materials in the resol-type melamine formaldehyde resin, was 2.8:1.
[0331] Commercial resol-type melamine formaldehyde resin particles were cured at 265°C for 5 hours in an air atmosphere, followed by crushing, sand milling, sieving, and magnetic foreign matter removal treatment to obtain polymer particles 2-2# containing triazine ring structure units. The molar ratio of formaldehyde and melamine, which are raw materials in the resol-type melamine formaldehyde resin, was 2.8:1.
[0332] Commercial resol-type melamine formaldehyde resin particles were cured at 245°C for 6 hours in an air atmosphere, followed by crushing, sand milling, sieving, and magnetic foreign matter removal treatment to obtain polymer particles 2-3# containing triazine ring structure units. The molar ratio of formaldehyde and melamine, which are raw materials in the resol-type melamine formaldehyde resin, was 2.8:1.
[0333] Commercial resol-type melamine formaldehyde resin particles were cured at 285°C for 5 hours in an air atmosphere, followed by crushing, sand milling, sieving, and magnetic foreign matter removal treatment to obtain polymer particles 2-4# containing triazine ring structure units. The molar ratio of formaldehyde and melamine, which are raw materials in the resol-type melamine formaldehyde resin, was 3.0:1.
[0334] Commercial resol-type melamine formaldehyde resin particles were cured at 150°C for 5 hours in an air atmosphere, followed by crushing, sand milling, sieving, and magnetic foreign matter removal treatment to obtain polymer particles D2-1# containing triazine ring structure units. The molar ratio of formaldehyde and melamine, which are raw materials in the resol-type melamine formaldehyde resin, was 2.8:1.
[0335] The organic particles 2-1# to 2-4# prepared above do not have a melting point and have a glass transition temperature of 300℃ or lower. T g It satisfied the characteristic of not having.
[0336] [Table 2]
[0337]
[0338] As can be seen from the above test results, the polymer particles containing triazine ring structure units prepared in the embodiments of the present disclosure have relatively high electrochemical stability and can improve the heat resistance of the separator and the initial Coulomb efficiency of the high-voltage secondary battery cell.
[0339] Next, the phenol resin-based organic particles were replaced with cross-linked styrene-based organic particles.
[0340] A preliminary emulsion was prepared by emulsifying 0.8 g of sodium dodecyl sulfate, 64 mg of sodium persulfate, 20 ml of deionized water, 35 g of styrene, and 5 g of divinylbenzene. 140 g of deionized water was added to a reactor, and after raising the temperature to 68°C, the preliminary emulsion prepared above was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle 3-1# emulsion. The solid content of the reaction system was 20%.
[0341] A preliminary emulsion was prepared by emulsifying 0.8 g of sodium dodecyl sulfate, 100 mg of sodium persulfate, 20 ml of deionized water, 35 g of styrene, and 5 g of divinylbenzene. 140 g of deionized water was added to a reactor, and after raising the temperature to 68°C, the preliminary emulsion prepared above was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle 3-2# emulsion. The solid content of the reaction system was 20%.
[0342] A preliminary emulsion was prepared by emulsifying 0.8 g of sodium dodecyl sulfate, 100 mg of sodium persulfate, 20 ml of deionized water, 35 g of styrene, and 5 g of divinylbenzene. 190 g of deionized water was added to a reactor, and after raising the temperature to 68°C, the prepared preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle 3-3# emulsion. The solid content of the reaction system was 16%.
[0343] A preliminary emulsion was prepared by emulsifying 0.8g of sodium dodecyl sulfate, 100mg of sodium persulfate, 20ml of deionized water, 35g of styrene, and 5g of divinylbenzene. 100g of deionized water was added to a reactor, and after raising the temperature to 68°C, the preliminary emulsion prepared above was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle 3-4# emulsion. The solid content of the reaction system was 25%.
[0344] A preliminary emulsion was prepared by emulsifying 0.8g of sodium dodecyl sulfate, 100mg of sodium persulfate, 20ml of deionized water, 30g of styrene, and 10g of divinylbenzene. 140g of deionized water was added to a reactor, and after raising the temperature to 68°C, the preliminary emulsion prepared above was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle 3-5# emulsion. The solid content of the reaction system was 20%.
[0345] A preliminary emulsion was prepared by emulsifying 0.8 g of sodium dodecyl sulfate, 100 mg of sodium persulfate, 20 ml of deionized water, 39.5 g of styrene, and 0.5 g of divinylbenzene. 440 g of deionized water was added to a reactor, and after raising the temperature to 68°C, the prepared preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 6 hours, the temperature was raised to 86°C and an aging reaction was performed for 2 hours to obtain a cross-linked styrene-based organic particle D3-1# emulsion. The solid content of the reaction system was 8%.
[0346] The organic particles 3-1# to 3-5# manufactured above do not have a melting point, and the glass transition temperature T g It satisfied the characteristic of being in the range of 110℃ to 154℃.
[0347] [Table 3]
[0348]
[0349] As can be seen from the above test results, the cross-linked styrene-based organic particles prepared in the embodiments of the present disclosure have relatively high electrochemical stability and can improve the heat resistance of the separator and the initial Coulomb efficiency of the high-voltage secondary battery cell.
[0350] Next, the phenol resin-based organic particles were replaced with silicon-containing organic resin particles.
[0351] A preliminary emulsion was prepared by emulsifying 0.3g sodium persulfate, 0.3g sodium bicarbonate, 1.5g sodium dodecyl sulfate, 30g deionized water, 52.2g γ-methacryloyloxypropyltriisopropoxysilane, 3g 3-methacryloyloxypropyltriethoxysilane, and 4.8g divinylbenzene. 210g of deionized water was added to a reactor, and after raising the temperature to 70°C, the preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 4 hours, the temperature was raised to 80°C and an aging reaction was performed for 1 hour to obtain a silicon-containing organic resin particle 4-1# emulsion.
[0352] A preliminary emulsion was prepared by emulsifying 0.3g sodium persulfate, 0.3g sodium bicarbonate, 1.5g sodium dodecyl sulfate, 30g deionized water, 49.8g γ-methacryloyloxypropyltriisopropoxysilane, 3g 3-methacryloyloxypropyltriethoxysilane, and 7.2g divinylbenzene. 210g of deionized water was added to a reactor, and after raising the temperature to 70°C, the preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 4 hours, the temperature was raised to 80°C and an aging reaction was performed for 1 hour to obtain a silicon-containing organic resin particle 4-2# emulsion.
[0353] A preliminary emulsion was prepared by emulsifying 0.3g sodium persulfate, 0.3g sodium bicarbonate, 1.5g sodium dodecyl sulfate, 30g deionized water, 48.5g γ-methacryloyloxypropyltriisopropoxysilane, 3g 3-methacryloyloxypropyltriethoxysilane, and 8.5g divinylbenzene. 210g of deionized water was added to a reactor, and after raising the temperature to 70°C, the preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 4 hours, the temperature was raised to 80°C and an aging reaction was performed for 1 hour to obtain a silicon-containing organic resin particle 4-3# emulsion.
[0354] A preliminary emulsion was prepared by emulsifying 0.3g sodium persulfate, 0.3g sodium bicarbonate, 1.5g sodium dodecyl sulfate, 30g deionized water, 57g γ-methacryloyloxypropyltriisopropoxysilane, and 3g 3-methacryloyloxypropyltriethoxysilane. 210g of deionized water was added to a reactor, and after raising the temperature to 65°C, the preliminary emulsion was added dropwise under nitrogen protection and stirring conditions. After reacting for 4 hours, the temperature was raised to 70°C and an aging reaction was performed for 1 hour to obtain a silicon-containing organic resin particle D4-1# emulsion.
[0355] The organic particles 4-1# to 4-3# prepared above satisfy the following characteristics: the silicon-containing organic resin particles have a network structure formed with carbon-carbon bonds as the main chain, the side chains contain a siloxane structure, have no melting point, and the glass transition temperature is 300°C or lower. T g It does not have.
[0356] [Table 4]
[0357]
[0358] As can be seen from the above test results, the silicon-containing organic resin particles prepared in the embodiments of the present disclosure have relatively high electrochemical stability and can improve the heat resistance of the separator and the initial Coulomb efficiency of the high-voltage secondary battery cell.
[0359] It should be noted that the present disclosure is not limited to the embodiments mentioned above. The above embodiments are merely examples, and all embodiments having substantially the same configuration as the technical concept of the technical solution of the present disclosure and producing the same effect are included within the technical scope of the present disclosure. Furthermore, within the scope of the present disclosure, various modifications conceived by a person skilled in the art, or the configuration of other forms by combining some components of the embodiments, are also included within the scope of the present disclosure without departing from the gist of the present disclosure.
Claims
Claim 1 A secondary battery cell comprising a positive plate, a negative plate, and a separator, wherein the separator is disposed between the positive plate and the negative plate, and the separator comprises a porous substrate and a coating layer located on at least one side of the porous substrate, wherein the coating layer comprises organic particles, and the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Claim 2 A secondary battery cell according to claim 1, wherein the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50V to 4.50V. Claim 3 A secondary battery cell according to claim 1 or 2, wherein the organic particles are at least one of a thermosetting resin polymer or a crosslinked polymer; and / or the organic particles are an amorphous polymer. Claim 4 In any one of claims 1 to 3, the true density of the organic particles is 1.0 g / cm³ 3 -2.0g / cm 3 and; optionally 1.0 g / cm² 3 -1.8g / cm 3 A secondary battery cell in which the volume distribution particle size Dv50 of the organic particles is less than 1 μm and optionally 50 nm to 840 nm. Claim 5 A secondary battery cell according to any one of claims 1 to 4, wherein the organic particles do not have a melting point. Claim 6 A secondary battery cell according to any one of claims 1 to 5, wherein the organic particles comprise one or more of phenol resin-based organic particles, polymer particles containing triazine ring structure units, cross-linked styrene-based organic particles, and silicon-containing organic resin particles. Claim 7 A secondary battery cell according to claim 6, wherein the phenol resin-based organic particles are a thermosetting resist resin polymer; and / or the phenol resin-based organic particles do not have a glass transition temperature of 300°C or lower; and / or the volume distribution particle size Dv50 of the phenol resin-based organic particles is 200 nm to 840 nm. Claim 8 A secondary battery cell according to claim 6 or 7, wherein the polymer particles containing triazine ring structure units comprise a cross-linking structure connecting the triazine ring structure units; and / or the polymer particles containing triazine ring structure units do not have a glass transition temperature of 300°C or lower; and / or the volume distribution particle size Dv50 of the polymer particles containing triazine ring structure units is 200 nm to 840 nm. Claim 9 A secondary battery cell according to claim 8, wherein the cross-linking structure comprises one or a combination of two or more of an alkylene group, an alkylene ether group, an alkylene amine group, an ester group, and an amide group. Claim 10 A secondary battery cell according to any one of claims 6 to 9, wherein the triazine ring structure unit of the polymer particle containing the triazine ring structure unit further has a substituent, said substituent comprises a combination of one or more of an alkyl group, an alkenyl group, a phenyl group, a cycloalkyl group, an amino group, a hydroxyl group, and a halogen. Claim 11 A secondary battery cell according to any one of claims 6 to 10, wherein the polymer particles containing triazine ring structure units comprise a melamine aldehyde-based polymer and a derivative thereof. Claim 12 In claim 11, the melamine aldehyde-based polymer and its derivative comprises one or more of melamine formaldehyde, benzoguanamine formaldehyde, melamine-benzoguanamine formaldehyde, melamine-(2,4-diamino-1,3,5-triazine) formaldehyde, melamine-(6-methyl-1,3,5-triazine-2,4-diamine) formaldehyde, melamine-(2,4,6-triethylamino-1,3,5-triazine) formaldehyde, trihydrazino-s-triazine formaldehyde, melamine-(2-amino-4-methylamino-1,3,5-triazine) formaldehyde, and melamine-(2,4-diamino-6-dimethylamino-1,3,5-triazine) formaldehyde, in a secondary battery Cell. Claim 13 In any one of claims 6 to 12, the cross-linked styrene-based organic particles comprise a styrene or styrene derivative structural unit and a cross-linked structural unit; and / or the glass transition temperature of the cross-linked styrene-based organic particles T g A secondary battery cell in which the temperature is 110°C to 154°C; and / or the volume distribution particle size Dv50 of the cross-linked styrene-based organic particles is 88 nm to 295 nm. Claim 14 In paragraph 13, the styrene or styrene derivative structural unit comprises one or more of a styrene structural unit, a 1-methyl-1-styrene structural unit, a 4-methylstyrene structural unit, a 2-methylstyrene structural unit, a 2,4-dimethylstyrene structural unit, and a 2,5-dimethylstyrene structural unit; and / or a secondary battery cell wherein the crosslinking structural unit comprises one or more of a divinylbenzene structural unit, an ethylene glycol dimethacrylate structural unit, a pentaerythritol tetraacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, an N,N-methylenebisacrylamide structural unit, an N,N'-vinylbisacrylamide structural unit, a 1,3,5-triacryloylhexahydro-1,3,5-triazine structural unit and a trialyl isocyanurate structural unit. Claim 15 A secondary battery cell according to any one of claims 6 to 14, wherein the silicon-containing organic resin particles are silicon-containing organic crosslinked resin particles, and the silicon-containing organic resin particles contain carbon-carbon bonds and a siloxane structure; and / or the silicon-containing organic resin particles do not have a glass transition temperature of 300°C or lower; and / or the volume distribution particle size Dv50 of the silicon-containing organic resin particles is 88 nm to 295 nm. Claim 16 A secondary battery cell according to any one of claims 6 to 15, wherein the silicon-containing organic resin particles are silicon-containing organic crosslinked resin particles, the silicon-containing organic resin particles have a network structure formed with carbon-carbon bonds as the main chain, and the side chains contain a siloxane structure. Claim 17 In claim 15 or 16, the silicon-containing organic crosslinked resin particles comprise a crosslinked structural unit; optionally, the crosslinked structural unit comprises a divinylbenzene structural unit, a diethylene glycol divinyl ether structural unit, a triethylene glycol divinyl ether structural unit, a diallyl maleate structural unit, an ethylene glycol dimethacrylate structural unit, a 1,4-butanediol diacrylate structural unit, a 1,6-hexanediol diacrylate structural unit, a 1,8-octanediol diacrylate structural unit, a trimethylolpropane triacrylate structural unit, a pentaerythritol trimethacrylate structural unit, a tetraethylene glycol dimethacrylate structural unit, a tripropylene glycol diacrylate structural unit, a 2,2,4-trimethyladipoylbis[2-ethylaziridine] structural unit, a 1,1-azellaoilbis[2-methylaziridine] structural unit, A secondary battery cell comprising one or more of the following: a 1,1-(1,3-phenylenedicarbonyl)bis[2-methylaziridine] structural unit, a trimethylolpropane tri(2-methyl-1-aziridinylpropionate) structural unit, a trimethylolpropane-tri[3-(2-methylaziridinyl)propionate] structural unit, and a pentaerythritol tri(3-aziridinyl)propionate structural unit. Claim 18 A secondary battery cell according to any one of claims 1 to 17, wherein the ratio of the volume distribution particle size Dv50 of the organic particles to the average pore diameter of the porous substrate is 1.2 or more. Claim 19 In any one of claims 1 to 18, the coating layer further comprises a binder; and / or, based on the total mass of the coating layer, the mass content of organic particles in the coating layer is 50%-99%; and / or the thickness of the coating layer is 0.5μm-5μm; and / or the areal density of the coating layer is 0.45g / m² 2 -5g / m 2 Phosphorus, secondary battery cell. Claim 20 A battery device comprising a plurality of secondary battery cells according to any one of claims 1 to 19. Claim 21 A power-using device comprising a secondary battery cell according to any one of claims 1 to 19 or a battery device according to claim 20. Claim 22 A separator comprising a porous substrate and a coating layer located on at least one side of the porous substrate, wherein the coating layer comprises organic particles, and the first cycle cyclic voltammetry curve of the organic particles does not have an oxidation peak within a voltage range of 2.50 V to 4.40 V. Claim 23 In paragraph 22, the organic particles are at least one of a thermosetting resin polymer or a crosslinked polymer; and / or the organic particles are an amorphous polymer, a separator. Claim 24 In paragraph 22 or 23, the true density of the organic particles is 1.0 g / cm³ 3 -2.0g / cm 3 and; optionally 1.0 g / cm² 3 -1.8g / cm 3 A separation membrane in which the volume distribution particle size Dv50 of the organic particles is less than 1 μm and optionally 50 nm to 840 nm. Claim 25 A separation membrane according to any one of paragraphs 22 to 24, wherein the organic particles do not have a melting point. Claim 26 A separation membrane according to any one of claims 22 to 25, wherein the organic particles comprise one or more of phenol resin-based organic particles, polymer particles containing triazine ring structure units, cross-linked styrene-based organic particles, and silicon-containing organic resin particles.