Polythiol composition, polymerizable composition, resin, molded body, optical material, and lens
A polythiol composition with controlled peak areas in high-speed liquid chromatography is used to produce resins with reduced yellowness and devitrification, addressing the issue of increased yellowness in existing polymerizable compositions.
Patent Information
- Application Number
- KR1020267035185
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-14
- Filing Date
- 2023-09-05
- Publication Date
- 2026-11-09
AI Technical Summary
Existing polymerizable compositions containing polythiol compounds often result in resins with increased yellowness due to the presence of compounds other than polythiol compounds.
A polythiol composition comprising specific polythiol compounds and selected compounds, with controlled peak areas in high-speed liquid chromatography, is used to produce a resin with reduced yellowness and devitrification.
The solution effectively reduces yellowness and devitrification in the resulting resin, enhancing its optical properties.
Smart Images

Figure PAT00012_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a polythiol composition, a polymerizable composition, a resin, a molded article, an optical material, and a lens. Background Technology
[0002] Plastic lenses are lighter than inorganic lenses, less prone to cracking, and can be dyed, so in recent years they have been rapidly adopted in optical devices such as eyeglass lenses and camera lenses.
[0003] For plastic lens resins, there has been a demand for even higher performance, including high refractive index, high Abbe hydration, low specific gravity, and high heat resistance. Various lens resin materials have been developed and used to date.
[0004] For example, Patent Document 1 describes a mercapto compound represented by a specific structural formula.
[0005] For example, Patent Document 2 describes a method for producing a polythiol compound, comprising the steps of: reacting 2-mercaptoethanol with an epihalohydrin compound represented by a specific formula (1) at a temperature of 10 to 50°C to obtain a polyalcohol compound represented by a specific formula (2); reacting the obtained polyalcohol compound represented by the formula (2) with a thiourea in the presence of hydrogen chloride to obtain an isothiuronum salt; maintaining a reaction solution containing the obtained isothiuronum salt at a temperature of 15 to 60°C and adding ammonia water to the reaction solution within 80 minutes to hydrolyze the isothiuronum salt and obtain a polythiol compound represented by a specific formula (5); and adding hydrochloric acid at a concentration of 25 to 36% to a solution containing the obtained polythiol compound, washing at a temperature of 10 to 50°C, and purifying the polythiol compound. Prior art literature
[0006] Japanese Patent Publication No. Hei 2-270859, International Publication No. 2014-027427 The problem to be solved
[0007] For a resin obtained by curing a polymerizable composition containing a polythiol compound, it is sometimes required to reduce the yellowness.
[0008] In practice, polymerizable compositions containing polythiol compounds often contain compounds other than polythiol compounds.
[0009] The inventors have discovered that when a polymerizable composition includes a compound other than a polythiol compound, the yellowness of the resulting resin tends to increase.
[0010] As a result of conducting various reviews regarding the above trend, it was found that there are cases where it becomes difficult to obtain a resin with reduced yellowness.
[0011] The problem to be solved by one embodiment of the present disclosure is to provide a polythiol composition capable of producing a resin with reduced yellowness, a polymerizable composition comprising the polythiol composition, a resin, a molded article, an optical material, and a lens. means of solving the problem
[0012] The means for solving the above problem include the following embodiments.
[0013] <1> A polythiol composition comprising a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), wherein, in high-speed liquid chromatography measurement, the total peak area of the at least one compound selected from the group consisting of the compound represented by the formula (1) and the compound represented by the formula (2) is 1.00 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0014]
[0015] <2> The above polythiol compound (A) comprises a polythiol compound obtained from 2-mercaptoethanol and thiourea as raw materials, <1> Polythiol composition described in
[0016] <3> The above polythiol compound (A) comprises 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane, or comprises a mixture of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane. <1> or <2> Polythiol composition described in any one of the following.
[0017] <4> <1> inside <3> A polymerizable composition comprising a polythiol composition described in any one of the above and a polyiso(thio)cyanate compound.
[0018] <5> The above polyiso(thio)cyanate compound comprises at least one selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, bis(isocyanatocyclohexyl)methane, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and phenylene diisocyanate. <4> Polymerizable composition described in
[0019] <6> A polyiso(thio)cyanate composition comprising the above-mentioned polyiso(thio)cyanate compound, and
[0020] The above polyiso(thio)cyanate composition,
[0021] xylylene diisocyanate and,
[0022] At least one selected from the group consisting of the following compounds (N1), the following compounds (N2), and the following compounds (N3).
[0023] Includes,
[0024] When the above polyiso(thio)cyanate composition includes the compound (N1), the peak area of the compound (N1) in gas chromatography measurement is 0.20 ppm or more with respect to the peak area 1 of xylylene diisocyanate, and
[0025] When the above polyiso(thio)cyanate composition includes the compound (N2), the peak area of the compound (N2) in gas chromatography measurement is 0.05 ppm or more relative to the peak area 1 of xylylene diisocyanate, and
[0026] In the case where the above polyiso(thio)cyanate composition includes the compound (N3), the peak area of the compound (N3) in gas chromatography measurement is 0.10 ppm or more relative to the peak area 1 of xylylene diisocyanate,
[0027] <4> or <5> Polymerizable composition described in
[0028]
[0029] <7> <4> inside <6> A resin comprising a cured product of a polymerizable composition described in any one of the following.
[0030] <8> <7> A molded article comprising the resin described in
[0031] <9> <7> Optical material comprising the resin described in
[0032] <10> <7> A lens comprising the resin described in Effects of the invention
[0033] According to one embodiment of the present disclosure, a polythiol composition capable of producing a resin with reduced yellowness, a polymerizable composition comprising the polythiol composition, a resin, a molded article, an optical material, and a lens can be provided. Specific details for implementing the invention
[0034] In the present disclosure, a numerical range indicated by "to" represents a range that includes the values described before and after "to" as the minimum and maximum values, respectively.
[0035] In the numerical ranges described stepwise in the present disclosure, an upper or lower limit value described in any numerical range may be substituted with an upper or lower limit value of another numerical range described stepwise, or may be substituted with a value shown in the examples.
[0036] In the present disclosure, the amount of each component in the material refers to the total amount of the multiple substances present in the material, unless specifically determined, in cases where multiple substances corresponding to each component exist in the material.
[0037] In the present disclosure, "iso(thio)cyanate" means isocyanate or isothiocyanate.
[0038] ≪Polythiol Composition≫
[0039] The present disclosure includes the following embodiments A and B.
[0040] That is, the concept of the polythiol composition of the present disclosure includes the polythiol composition of Embodiment A and the polythiol composition of Embodiment B.
[0041] Embodiments A and B may have overlapping parts.
[0042] For example, the polythiol composition of Embodiment A may have the characteristics of Embodiment B described below.
[0043] Here, the characteristic of embodiment B is that, although details will be described later, it comprises at least one compound selected from the group consisting of a polythiol compound (A), a compound represented by formula (3) described later, and a compound represented by formula (4) described later, and in high-speed liquid chromatography measurement, the total peak area of the at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) is 2.10 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0044] [Embodiment A]
[0045] The polythiol composition of embodiment A comprises a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), and in high-speed liquid chromatography measurement, the total peak area of at least one compound selected from the group consisting of a compound represented by the formula (1) and a compound represented by the formula (2) is 1.00 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0046]
[0047] The polythiol composition of Embodiment A can produce a resin with reduced yellowness by including the above composition.
[0048] In addition, the polythiol composition of Embodiment A may produce a resin with reduced devitrification.
[0049] <Polythiol Compound (A)>
[0050] The polythiol composition of embodiment A comprises a polythiol compound (A).
[0051] The polythiol compound (A) of embodiment A is not particularly limited.
[0052] The polythiol compound (A) preferably comprises a polythiol compound obtained from 2-mercaptoethanol and thiourea as raw materials.
[0053] As polythiol compounds obtained from 2-mercaptoethanol and thiourea as raw materials, for example;
[0054] At least one selected from the group consisting of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane;
[0055] 4-mercaptomethyl-1,8-dimercapto-3,6-dithioactane;
[0056] You can lift the back.
[0057] Polythiol compound (A) is,
[0058] It is preferable to include 4-mercaptomethyl-1,8-dimercapto-3,6-dithiauctane, or at least one selected from the group consisting of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaudecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaudecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaudecane.
[0059] It is more preferable to include 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane.
[0060] 4-mercaptomethyl-1,8-dimercapto-3,6-dithioactane is a compound represented by the following formula (a-1).
[0061]
[0062] The method of preparing the polythiol compound (A) is not particularly limited and can be prepared by known methods. For example, the polythiol compound (A) can be prepared by the method described in International Publication No. 2014 / 027427. In addition, the polythiol compound (A) is preferably a compound obtained by using a catalyst comprising at least one selected from the group consisting of metal hydroxides such as sodium hydroxide and potassium hydroxide and metal carbonates such as sodium carbonate and potassium carbonate when reacting, for example, 2-mercaptoethanol with an epihalohydrin compound.
[0063] The polythiol composition of embodiment A may include a polythiol compound (A) and a compound other than at least one compound selected from the group consisting of a compound represented by formula (1) and a compound represented by formula (2).
[0064] For example, it may include a polythiol compound (A), and a polythiol compound having a mercapto group other than at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2) (hereinafter also referred to as “other polythiol compounds”).
[0065] Other polythiol compounds include, for example, methanedithiol, 1,2-ethanedithiol, 1,2,3-propanetrithiol, pentaerythritoltetrakis(2-mercaptoacetate), pentaerythritoltetrakis(3-mercaptopropionate), tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, bis(2-mercaptoethyl)sulfide, bis(2,3-dimercaptopropyl)sulfide, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, Examples include 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithioundecane, 2,5-dimercaptomethyl-1,4-dithian, 2,5-dimercaptomethyl-2,5-dimethyl-1,4-dithian, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 4,6-bis(mercaptomethylthio)-1,3-dithian, etc.
[0066] <Compound represented by Formula (1), Compound represented by Formula (2)>
[0067] The polythiol composition of embodiment A comprises at least one compound selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2).
[0068]
[0069] The polythiol composition of embodiment A includes at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2), so that when a combination of the polythiol compound (A) and a specific sulfur compound is included in the polymerizable composition, the yellowness and devitrification of the resulting resin can be reduced.
[0070] In the polythiol composition of embodiment A, the total peak area of at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2) in high-speed liquid chromatography measurement is 1.00 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0071] The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) is 1.00 or less, thereby reducing the yellowness and de-transparency of the obtained resin.
[0072] In the same view above, it is preferable that the total peak area of at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2) is 0.90 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition, more preferable that it is 0.70 or less, even more preferable that it is 0.50 or less, and particularly preferable that it is 0.30 or less.
[0073] There is no particular limit to the lower limit of the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) for the total peak area of 100 of the compounds included in the polythiol composition, but the lower limit is, for example, 0.05, preferably 0.10.
[0074] "The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) relative to the total peak area of the compounds included in the polythiol composition, which is 100" means the relative value of the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) when the total peak area of the compounds included in the polythiol composition is 100.
[0075] In addition, the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) means, for example, the total peak area of the compound represented by Formula (1) and the compound represented by Formula (2) when the polythiol composition includes both the compound represented by Formula (1) and the compound represented by Formula (2), and the peak area of the compound represented by Formula (1) when the polythiol composition includes only one of the compound represented by Formula (1) and the compound represented by Formula (2).
[0076] In high-speed liquid chromatography measurements, the total peak area of at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2) is preferably greater than 0 with respect to the total peak area of 100 of the compounds included in the polythiol composition, more preferably greater than 0.02, even more preferably greater than 0.05, and particularly preferably greater than 0.1, in order to reduce the workload of purifying and removing at least one compound selected from the group consisting of the compound represented by formula (1) and the compound represented by formula (2) from the polythiol composition.
[0077] In addition, the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) satisfies the lower limit range, thereby increasing the thickening rate and thus promoting polymerization.
[0078] A method for adjusting the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) for a total peak area of 100 of compounds included in the polythiol composition is not particularly limited, but can be adjusted by operations such as column purification, washing, extraction, and purification, for example.
[0079] <Measurement of the peak area of the compound represented by Equation (1) and the compound represented by Equation (2)>
[0080] The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) for the total peak area of 100 of the compounds included in the polythiol composition is obtained by performing high-speed liquid chromatography (HPLC) measurements based on the following conditions.
[0081] The peak area appearing at a retention time of 7.5 to 8.0 minutes is determined as the peak area of the compound represented by Equation (1) and the compound represented by Equation (2), and the ratio to the total peak area of the compounds included in the polythiol composition is calculated as 100.
[0082] (HPLC conditions)
[0083] Column: YMC-Pack ODS-A A-312(S5Φ6mm×150mm)
[0084] Mobile phase: Acetonitrile / 0.01 mol / L aqueous solution of potassium dihydrogen phosphate = 60 / 40 (vol / vol)
[0085] Column temperature: 40℃
[0086] Flow rate: 1.0 ml / min
[0087] Detector: UV detector, wavelength 230nm
[0088] Preparation of measurement solution: Dissolve and mix 160 mg of polythiol composition in 10 ml of acetonitrile.
[0089] Injection volume: 2μL
[0090] In the HPLC of the above conditions, the retention time of the compound represented by formula (1) and the retention time of the compound represented by formula (2) are both, for example, 6.0 minutes to 8.0 minutes.
[0091] The molecular weight of the compound represented by formula (1) and the molecular weight of the compound represented by formula (2) are both 166.
[0092] [Embodiment B]
[0093] The polythiol composition of embodiment B comprises a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by the following formula (3) and a compound represented by the following formula (4), and in high-speed liquid chromatography measurement, the total peak area of at least one compound selected from the group consisting of a compound represented by the formula (3) and a compound represented by the formula (4) is 2.10 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0094]
[0095] The polythiol composition of Embodiment B can be used to produce a resin with reduced yellowness by including the above composition.
[0096] In addition, the polythiol composition of Embodiment B may enable the production of a resin with reduced yellowness.
[0097] The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) for the total peak area of 100 of the compounds included in the polythiol composition (Embodiment B) is obtained by making it identical to the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) for the total peak area of 100 of the compounds included in the polythiol composition described above (i.e., by HPLC measurement under the same conditions).
[0098] There is no particular limit to the lower limit of the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) for the total peak area of 100 of the compounds included in the polythiol composition, but the lower limit is, for example, 0.10, preferably 0.20, more preferably 0.30.
[0099] In the HPLC of the above conditions, the retention time of the compound represented by formula (3) and the retention time of the compound represented by formula (4) are both, for example, 9.0 minutes to 11.0 minutes.
[0100] The molecular weight of the compound represented by formula (3) and the molecular weight of the compound represented by formula (4) are both 226.
[0101] <Polythiol Compound (A)>
[0102] The polythiol composition of embodiment B includes a polythiol compound (A).
[0103] With respect to the polythiol compound (A), the details of the specific example, preferred specific example, preferred embodiment, manufacturing method, etc. are the same as the details of the specific example, preferred specific example, preferred embodiment, manufacturing method, etc. of the polythiol compound (A) in Embodiment A.
[0104] The polythiol composition of embodiment B may include a polythiol compound (A) and a compound other than at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4).
[0105] For example, it may include a polythiol compound (A), and a polythiol compound having a mercapto group other than at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) (hereinafter also referred to as “other polythiol compounds”).
[0106] The details of specific examples of other polythiol compounds are the same as the details of specific examples of other polythiol compounds in Embodiment A.
[0107] In addition, other polythiol compounds may include at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2), which are characteristics of Embodiment A.
[0108] That is, the polythiol composition of Embodiment B may have the characteristics of the polythiol composition of Embodiment A described above.
[0109] <Compound represented by Formula (3), Compound represented by Formula (4)>
[0110] The polythiol composition of embodiment B comprises at least one compound selected from the group consisting of a compound represented by the following formula (3) and a compound represented by the following formula (4).
[0111]
[0112] The polythiol composition of embodiment B includes at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4), thereby reducing the yellowness and devitrification of the resin obtained when a combination of the polythiol compound (A) and a specific sulfur compound is included in the polymerizable composition.
[0113] In the polythiol composition of embodiment B, the total peak area of at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) in high-speed liquid chromatography measurement is 2.10 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.
[0114] The total peak area of at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) is 2.10 or less, thereby reducing the yellowness and de-transparency of the obtained resin.
[0115] In the same view above, it is preferable that the total peak area of at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) is 2.05 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition, more preferable that it is 1.90 or less, and even more preferable that it is 1.50 or less.
[0116] "The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) relative to the total peak area of the compounds included in the polythiol composition, which is 100" means the relative value of the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) when the total peak area of the compounds included in the polythiol composition is 100.
[0117] Additionally, the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) means, for example, the total peak area of the compound represented by Formula (3) and the compound represented by Formula (4) when the polythiol composition includes both the compound represented by Formula (3) and the compound represented by Formula (4), and the peak area of the compound represented by Formula (4) when the polythiol composition includes only one of the compound represented by Formula (3) and the compound represented by Formula (4).
[0118] In high-speed liquid chromatography measurements, the total peak area of at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) is preferably greater than 0, more preferably greater than 0.10, and even more preferably greater than 0.30, with respect to reducing the workload of purifying and removing at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) from the polythiol composition.
[0119] In addition, the total peak area of at least one compound selected from the group consisting of the compound represented by formula (3) and the compound represented by formula (4) satisfies the lower limit range, thereby increasing the thickening rate and thus promoting polymerization.
[0120] A method for adjusting the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) for a total peak area of 100 of compounds included in the polythiol composition is not particularly limited, but can be adjusted by operations such as column purification, washing, extraction, and purification, for example.
[0121] <Measurement of the peak area of the compound represented by Equation (3) and the compound represented by Equation (4)>
[0122] The total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) for the total peak area of 100 of the compounds included in the polythiol composition is obtained by performing high-speed liquid chromatography (HPLC) measurements based on the following conditions.
[0123] The peak area appearing at a retention time of 9.8 to 11.2 minutes is determined as the peak area of the compound represented by Equation (3) and the compound represented by Equation (4), and the ratio to the total peak area of the compounds included in the polythiol composition is calculated.
[0124] (HPLC conditions)
[0125] Column: YMC-Pack ODS-A A-312(S5Φ6mm×150mm)
[0126] Mobile phase: Acetonitrile / 0.01 mol / L aqueous solution of potassium dihydrogen phosphate = 60 / 40 (vol / vol)
[0127] Column temperature: 40℃
[0128] Flow rate: 1.0 ml / min
[0129] Detector: UV detector, wavelength 230nm
[0130] Preparation of measurement solution: Dissolve and mix 160 mg of polythiol composition in 10 ml of acetonitrile.
[0131] Injection volume: 2μL
[0132] ≪Polymerizable Composition≫
[0133] The polymerizable composition of the present disclosure comprises the polythiol composition of the present disclosure and a polyiso(thio)cyanate compound.
[0134] (Polyiso(thio)cyanate compounds)
[0135] As for the polyiso(thio)cyanate compound, it is not particularly limited as long as it can exhibit the effects of the present disclosure, and conventionally known compounds may be used. It is not particularly limited as long as it is a compound having at least two iso(thio)cyanate groups in one molecule, and specifically, for example, aliphatic polyisocyanate compounds such as tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate, octamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate methyl ester, lysine triisocyanate, and xylylene diisocyanate; Alicyclic polyisocyanate compounds such as isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, bis(isocyanatocyclohexyl)methane, dicyclohexyl dimethylmethane diisocyanate, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 3,8-bis(isocyanatomethyl)tricyclodecane, 3,9-bis(isocyanatomethyl)tricyclodecane, 4,8-bis(isocyanatomethyl)tricyclodecane, 4,9-bis(isocyanatomethyl)tricyclodecane, etc.;
[0136] Aromatic polyisocyanate compounds such as tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, diphenylsulfide-4,4-diisocyanate, and phenylene diisocyanate;
[0137] Heterocyclic polyisocyanate compounds such as 2,5-diisocyanatothiophene, 2,5-bis(isocyanatomethyl)thiophene, 2,5-diisocyanatotetrahydrothiophene, 2,5-bis(isocyanatomethyl)tetrahydrothiophene, 3,4-bis(isocyanatomethyl)tetrahydrothiophene, 2,5-diisocyanato-1,4-dithiane, 2,5-bis(isocyanatomethyl)-1,4-dithiane, 4,5-diisocyanato-1,3-dithiolane, 4,5-bis(isocyanatomethyl)-1,3-dithiolane, etc.
[0138] Aliphatic polyisothiocyanate compounds such as hexamethylene diisothiocyanate, lysine diisothiocyanate methyl ester, lysine triisothiocyanate, and xylylene diisothiocyanate;
[0139] Alicyclic polyisothiocyanate compounds such as isophorone diisothiocyanate, bis(isothiocyanatomethyl)cyclohexane, bis(isothiocyanatocyclohexyl)methane, cyclohexane diisothiocyanate, methylcyclohexane diisothiocyanate, 2,5-bis(isothiocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isothiocyanatomethyl)bicyclo-[2.2.1]-heptane, 3,8-bis(isothiocyanatomethyl)tricyclodecane, 3,9-bis(isothiocyanatomethyl)tricyclodecane, 4,8-bis(isothiocyanatomethyl)tricyclodecane, 4,9-bis(isothiocyanatomethyl)tricyclodecane, etc.;
[0140] Aromatic polyisothiocyanate compounds such as tolylene diisothiocyanate, 4,4-diphenylmethane diisothiocyanate, and diphenyldisulfide-4,4-diisothiocyanate;
[0141] Examples include sulfur-containing heterocyclic polyisothiocyanate compounds such as 2,5-diisothiophene, 2,5-bis(isothiophenatomethyl)thiophene, 2,5-isothiophenatotetrahydrothiophene, 2,5-bis(isothiophenatomethyl)tetrahydrothiophene, 3,4-bis(isothiophenatomethyl)tetrahydrothiophene, 2,5-diisothiophenato-1,4-dithiane, 2,5-bis(isothiophenatomethyl)-1,4-dithiane, 4,5-diisothiophenato-1,3-dithiolan, and 4,5-bis(isothiophenatomethyl)-1,3-dithiolan. The polyiso(thio)cyanate compound may include at least one selected from these.
[0142] In addition, as polyiso(thio)cyanate compounds, halogen substituents such as chlorine substituents and bromine substituents, alkyl substituents, alkoxy substituents, nitro substituents, prepolymer-type modified compounds with polyhydric alcohols, carbodiimide modified compounds, urea modified compounds, biuret modified compounds, and products of dimerization or trimerization reactions can also be used.
[0143] As for the polyiso(thio)cyanate compound, a polyisocyanate compound is preferred, and it is preferable to include at least one selected from the group consisting of pentamethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, bis(isocyanatocyclohexyl)methane, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and phenylene diisocyanate.
[0144] The mixing ratio of the polythiol composition and the polyiso(thio)cyanate compound is not particularly limited, and for example, the molar ratio (mercapto group / iso(thio)cyanate group) of the mercapto group of the polythiol compound included in the polythiol composition and the iso(thio)cyanate group of the polyiso(thio)cyanate compound is preferably 0.5 to 3.0, more preferably 0.6 to 2.0, and even more preferably 0.8 to 1.3. If the mixing ratio is within the above range, it tends to be possible to satisfy various performance characteristics such as refractive index and heat resistance required for plastic lenses, etc., in a good balance.
[0145] The polymerizable composition of the present disclosure may include a polyiso(thio)cyanate composition comprising the polyiso(thio)cyanate compound.
[0146] Here, the term "polyisocyanate composition" means a composition containing at least one type of polyisocyanate compound.
[0147] The polyisocyanate composition may contain components other than polyisocyanate compounds as impurities.
[0148] It is preferable that the polyisocyanate composition includes at least one polyisocyanate compound as a main component.
[0149] The meaning of "included as a main component" is as previously explained.
[0150] The polyisocyanate composition preferably includes xylylene diisocyanate.
[0151] Hereinafter, a polyisocyanate composition containing xylylene diisocyanate is also referred to as an XDI composition.
[0152] It is preferable that the XDI composition includes xylylene diisocyanate as a main component.
[0153] The XDI composition preferably comprises at least one selected from the group consisting of the following compounds (N1), the following compounds (N2), and the following compounds (N3).
[0154]
[0155] The following describes a preferred form of the XDI composition in terms of the stability of the polyiso(thio)cyanate composition and the transparency of the resin formed using the polyiso(thio)cyanate composition.
[0156] When the XDI composition contains compound (N1), it is preferable that the peak area of compound (N1) in the gas chromatography measurement under the following GC condition 1 is 0.20 ppm or more relative to the peak area 1 of xylylene diisocyanate.
[0157] -GC Condition 1-
[0158] Filler; DB-1 (film thickness) 1.5㎛
[0159] Column; inner diameter 0.53mm × length 60m (Agilent)
[0160] Oven temperature; increase from 130℃ to 220℃ at 3℃ / min, and after reaching 220℃, increase to 300℃ at 10℃ / min.
[0161] Split-ratio; Pulsed splitless method
[0162] Inlet temperature; 280℃
[0163] Detector temperature; 300℃
[0164] Carrier gas; N 2158kPa, H 255kPa, Air 45kPa
[0165] (Static pressure control)
[0166] Solvent; chloroform
[0167] Sample concentration: 2.0 mass% chloroform solution
[0168] Injection volume: 2μL
[0169] Detection method; FID
[0170] The peak area of the above compound (N1) is, with respect to the peak area 1 of xylylene diisocyanate, more preferably 5.0 ppm or more, even more preferably 50 ppm or more, and even more preferably 100 ppm or more.
[0171] The peak area of the above compound (N1) is preferably 4000 ppm or less, more preferably 3000 ppm or less, even more preferably 2000 ppm or less, even more preferably 1500 ppm or less, and even more preferably 1000 ppm or less, with respect to the peak area 1 of xylylene diisocyanate.
[0172] The peak area of the above compound (N1) can be measured in accordance with the method described in paragraph 0377 of Japanese Patent Publication No. 6373536.
[0173] When the XDI composition contains compound (N2), it is preferable that the peak area of compound (N2) in the gas chromatography measurement under the following GC conditions 2 is 0.05 ppm or more relative to the peak area 1 of xylylene diisocyanate.
[0174] -GC Condition 2-
[0175] Column; HP-50+, inner diameter 0.25mm × length 30m × film thickness 0.25㎛ (Made by Hewlett-Packard)
[0176] Oven temperature; increase from 50℃ to 280℃ at 10℃ / min, hold for 6 min after reaching 280℃.
[0177] Split-ratio; Pulsed splitless method
[0178] Inlet temperature; 200℃
[0179] Detector temperature; 280℃
[0180] Carrier gas; He
[0181] Carrier gas flow rate; 1.0 ml / min (constant flow rate control)
[0182] Sample concentration: 1.0 mass% dichloromethane solution
[0183] Injection volume: 1.0μL
[0184] Detection method; SIM (monitoring ion: m / z 180, 215) (content ratio of xylylene diisocyanate (XDI))
[0185] The peak area of the above compound (N2) is, with respect to the peak area 1 of xylylene diisocyanate, more preferably 0.1 ppm or more, even more preferably 0.3 ppm or more, and even more preferably 0.6 ppm or more.
[0186] The peak area of the above compound (N2) is preferably 200 ppm or less, more preferably 150 ppm or less, even more preferably 100 ppm or less, even more preferably 80 ppm or less, even more preferably 70 ppm or less, and even more preferably 60 ppm or less, with respect to the peak area 1 of xylylene diisocyanate.
[0187] The peak area of the above compound (N2) can be measured in accordance with the method described in paragraphs 0375 and 0376 of Japanese Patent Publication No. 6373536.
[0188] When the XDI composition includes compound (N3), it is preferable that the peak area of compound (N3) in the gas chromatography measurement under the aforementioned GC condition 1 is 0.10 ppm or more with respect to the peak area 1 of xylylene diisocyanate.
[0189] The peak area of the above compound (N3) is, more preferably 0.1 ppm or more, even more preferably 3.0 ppm or more, and even more preferably 5.0 ppm or more, with respect to the peak area 1 of xylylene diisocyanate.
[0190] The peak area of the above compound (N3) is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 300 ppm or less, even more preferably 100 ppm or less, and even more preferably 75 ppm or less, with respect to the peak area 1 of xylylene diisocyanate.
[0191] The peak area of the above compound (N3) can be measured in accordance with the method described in paragraph 0377 of Japanese Patent Publication No. 6373536.
[0192] The acid content of the XDI composition is preferably 3000 ppm or less, more preferably 2000 ppm or less, even more preferably 1000 ppm or less, even more preferably 100 ppm or less, even more preferably 50 ppm or less, even more preferably 30 ppm or less, and even more preferably less than 15 ppm.
[0193] The lower limit of the acid content of the XDI composition is not specifically limited, but the lower limit is, for example, 1 ppm.
[0194] The acid content of the XDI composition can be measured in accordance with the method described in paragraph 0091 of International Publication No. 2021 / 256417.
[0195] In addition, the XDI composition may include a stabilizer.
[0196] The polymerizable composition of the present disclosure may include other components other than polythiol compounds and polyiso(thio)cyanate compounds for the purpose of improving various physical properties of the resin, workability, and polymerization reactivity of the polymerizable composition.
[0197] Other components include polymerization catalysts, internal release agents, resin modifiers, chain extenders, crosslinking agents, radical scavengers, light stabilizers, ultraviolet absorbers, antioxidants, useful dyes, fillers, adhesion enhancers, antibacterial agents, antistatic agents, dyes, fluorescent whitening agents, fluorescent pigments, inorganic pigments, etc.
[0198] Examples of polymerization catalysts include tertiary amine compounds, their inorganic or organic salts, metal compounds, quaternary ammonium salts, organic sulfonic acids, etc.
[0199] Acidic phosphate esters may be used as internal release agents. Examples of acidic phosphate esters include phosphate monoesters and phosphate diesters, and each may be used individually or in a mixture of two or more types.
[0200] Examples of resin modifiers include episulfide compounds, alcohol compounds, amine compounds, epoxy compounds, organic acids and their anhydrides, and olefin compounds including (meth)acrylate compounds.
[0201] The polymerizable composition of the present disclosure can be obtained by mixing the above components.
[0202] ≪Plastic Body≫
[0203] The molded article of the present disclosure comprises the resin of the present disclosure.
[0204] The resin of the present disclosure comprises a cured product of the polymerizable composition of the present disclosure.
[0205] The method for manufacturing the molded article of the present disclosure is not particularly limited, and mold polymerization may be cited as a preferred manufacturing method. First, a polymerizable composition is injected between molding molds that are held and supported by a gasket or tape, etc. At this time, depending on the physical properties required for the resulting plastic lens, it is often desirable to perform degassing treatment under reduced pressure, filtration treatment such as pressurization and reduced pressure, etc., as necessary.
[0206] Regarding polymerization conditions, they are not limited as they vary significantly depending on the composition of the polymerizable composition, the type and amount of catalyst, the shape of the mold, etc., and are, for example, carried out over 1 hour to 50 hours at a temperature of -50°C to 150°C. In some cases, it is preferable to maintain the temperature in the range of 10°C to 150°C or gradually increase the temperature and cure for 1 hour to 48 hours.
[0207] If necessary, annealing or similar treatments may be performed on the molded body. The annealing or similar treatments are typically performed between 50°C and 150°C, preferably between 90°C and 140°C, and more preferably between 100°C and 130°C.
[0208] [use]
[0209] The resin obtained from the polymerizable composition of the present disclosure can be used as a material for manufacturing molded articles of various shapes by changing the type of mold during mold polymerization.
[0210] Optical Materials
[0211] The optical material of the present disclosure comprises the resin of the present disclosure.
[0212] A molded article obtained from the polymerizable composition of the present disclosure can obtain a material with reduced yellowness without impairing transparency. In addition, a molded article obtained from a polymerizable composition comprising a polythiol composition of the first embodiment can obtain a material having excellent devitrification.
[0213] For this reason, it is possible to use it in various optical materials, such as plastic lenses.
[0214] ≪Lens≫
[0215] The lens of the present disclosure comprises the resin of the present disclosure.
[0216] Lenses are particularly suitable as optical materials.
[0217] Examples of lenses include plastic eyeglass lenses and plastic polarized lenses.
[0218] [Plastic eyeglass lenses]
[0219] A plastic spectacle lens using a lens substrate formed from the molded body of the present disclosure may, if necessary, have a coating layer applied to one side or both sides.
[0220] The plastic spectacle lens of the present disclosure comprises a lens substrate comprising a cured product of the polymerizable composition described above, and a coating layer.
[0221] Specifically, the coating layer may include a primer layer, a hard coat layer, an anti-reflective layer, an anti-fog coating layer, an anti-contamination layer, a water-repellent layer, etc. Each of these coating layers may be used individually, or multiple coating layers may be used in a multilayered manner. When coating layers are applied to both sides, the same coating layer may be applied to each side, or different coating layers may be applied.
[0222] Each of these coating layers may contain an infrared absorber for the purpose of protecting the eyes from infrared rays, a light stabilizer, an antioxidant, etc. for the purpose of improving the weather resistance of the lens, a photochromic compound, a dye, a pigment, etc. for the purpose of enhancing the fashionability of the lens, and other known additives such as an antistatic agent for the purpose of enhancing the performance of the lens.
[0223] For the layer coated by application, various leveling agents intended to improve applicability may be used.
[0224] In addition, an anti-fog layer, an anti-contamination layer, and a water-repellent layer may be formed on the anti-reflective layer as needed.
[0225] Although embodiments of the present disclosure have been described above, these are examples of the present disclosure, and various configurations other than those described above may be adopted to the extent that they do not impair the effects of the present disclosure.
[0226] Examples
[0227] The present disclosure will be described in detail below with reference to examples. Furthermore, the present disclosure is not limited in any way to the descriptions in these examples. Also, unless otherwise specified, "part" is based on mass.
[0228] Evaluation Method
[0229] In this embodiment, the method for evaluating each physical property of the plastic lens is as follows.
[0230] · Yellow Index (also known as YI)
[0231] The resin was prepared as a circular plastic plate with a thickness of 9 mm and a diameter of 75 mm, and the YI value was calculated using a Konica Minolta Corporation spectrophotometer CM-5.
[0232] In addition, there is a correlation where the smaller the YI value, the lower the yellowness of the plastic plate, and the larger the YI value, the higher the yellowness.
[0233] ·Actual projection
[0234] A resin was fabricated into a circular plastic plate with a thickness of 9 mm and a diameter of 75 mm, and light from a light source (Luminar Ace LA-150A manufactured by Hayashi Refic) was transmitted through the side of the plate. An image of the light from the front of the plate was introduced into an image processing device (manufactured by Ube Information Systems), and shading processing was performed on the introduced image. The degree of shading of the processed image was quantified for each pixel, the average value of the shading degree values for each pixel was obtained, and the actual transparency of the plate was calculated.
[0235] The lower the devitrivity, the less the transparency of the resin (in this case, a flat plate) is compromised (i.e., the transparency of the resin is excellent).
[0236] <Preparation of Polythiol Composition (A)>
[0237] 124.6 parts by mass of 2-mercaptoethanol and 18.3 parts by mass of degassed water were charged into a reactor. 101.5 parts by mass of a 32 mass% aqueous sodium hydroxide solution was added dropwise over 40 minutes at 12°C to 35°C, followed by the addition of 73.6 parts by mass of epichlorohydrin over 4.5 hours at 29°C to 36°C, followed by stirring for 40 minutes. The formation of 1,3-bis(2-hydroxyethylthio)-2-propanol was confirmed from NMR data.
[0238] 331.5 parts by mass of 35.5% hydrochloric acid were added, followed by 183.8 parts by mass of thiourea with a purity of 99.90%, and a thiuronium chloride reaction was carried out by stirring for 3 hours under reflux at 110°C. After cooling to 45°C, 320.5 parts by mass of toluene were added and cooled to 31°C, 243.1 parts by mass of a 25% aqueous ammonia solution were added over 44 minutes at 31°C to 41°C, and a hydrolysis reaction was carried out by stirring for 3 hours at 54°C to 62°C to obtain a toluene solution of a polythiol with 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane as the main component. 162.8 parts by mass of 35.5% hydrochloric acid was added to this toluene solution, and acid washing was performed at 35°C to 43°C for 1 hour. 174.1 parts by mass of degassed water was added, and washing was performed twice at 35°C to 45°C for 30 minutes. 162.1 parts by mass of 0.1% ammonia water was added, and washing was performed for 30 minutes. 174.2 parts by mass of degassed water was added, and washing was performed twice at 35°C to 45°C for 30 minutes. After removing toluene and trace amounts of moisture under reduced pressure, the mixture was vacuum filtered using a 1.2 μm PTFE type membrane filter to obtain 205.0 parts by mass of a polythiol composition (A) having 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane, which is a polythiol compound (A), as the main component.
[0239] <Preparation of a polythiol composition (A1) comprising a compound represented by formula (1) and a compound represented by formula (2)>
[0240] 200.0 parts by mass of a polythiol composition having 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane as the main component, 4.0 parts by mass of diethylenetriamine, 400 ml of toluene, and 100 ml of water were added to a reactor and heated and stirred at 80 to 85°C for 5 hours. After settling and separation, the lower water layer was discharged, and 200 parts by mass of 35% hydrochloric acid were added to the upper layer (toluene layer) remaining in the reactor, and acid washing was performed twice at 35 to 40°C for 1 hour. After settling and separation, the lower water layer was discharged, and 200.0 parts by mass of degassed water was added to the toluene layer and washed at 35 to 45°C for 30 minutes. After settling and separating, the aqueous layer was discharged, and 200.0 parts by mass of 0.1% ammonia water was added to the toluene layer and washed for 30 minutes. After settling and separating, the lower aqueous layer was discharged, and 200.0 parts by mass of degassed water was added to the toluene layer and washed for 30 minutes twice. After removing toluene and trace amounts of moisture under reduced pressure, the mixture was filtered under reduced pressure using a 1.2 μm PTFE type membrane filter to obtain 188.7 parts by mass of a polythiol composition (A1) having 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane, a polythiol compound, as the main component.
[0241] For a total peak area of 100 of the compounds included in the obtained polythiol composition (A1), the compound represented by formula (1) and the compound represented by formula (2) were included in total of 1.50.
[0242] <Preparation of a polythiol composition (A2) comprising a compound represented by formula (3) and a compound represented by formula (4)>
[0243] 152.19 parts by mass of 2-mercaptoethanol and 23.1 parts by mass of degassed water were charged into a reactor. At 15 to 30°C, 128.32 parts by mass of a 30.3% by mass aqueous sodium hydroxide solution were added dropwise over 30 minutes, followed by the addition of 89.99 parts by mass of epichlorohydrin over 3 hours at 27 to 30°C, followed by stirring for 1 hour.
[0244] 405.1 parts by mass of 35% hydrochloric acid were added, followed by 224.3 parts by mass of thiourea with a purity of 99.4%, and a thiuronium chloride reaction was carried out by stirring for 3 hours under reflux at 110°C. After cooling to 40°C, 395.0 parts by mass of toluene were added and cooled to 34°C, and 293.3 parts by mass of a 25.4% by mass aqueous ammonia solution were added over 25 minutes at 34 to 40°C, and a hydrolysis reaction was carried out by stirring at 60°C to 62°C for 3 hours to obtain a toluene solution of a polythiol composition having 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane as the main component. To this toluene solution, 180.0 parts by mass of 35% hydrochloric acid was added, and acid washing was performed twice at 75 to 80°C for 3 hours. 200.0 parts by mass of degassed water was added, and washing was performed at 35 to 45°C for 30 minutes. 200.0 parts by mass of 0.1% ammonia water was added, and washing was performed for 30 minutes. 200.0 parts by mass of degassed water was added, and washing for 30 minutes was performed twice. After removing toluene and trace amounts of moisture under reduced pressure, the mixture was filtered under reduced pressure using a 1.2 μm PTFE type membrane filter to obtain 247.1 parts by mass of a polythiol composition (A2) having 4-mercaptomethyl-1,8-dimercapto-3,6-dithioctane, which is a polythiol compound (A), as the main component.
[0245] For the total peak area of 100 of the compounds included in the obtained polythiol composition (A2), the compound represented by formula (3) was included in an amount of 1.31 and the compound represented by formula (4) was included in an amount of 1.50.
[0246] [Examples 1 to 3]
[0247] A polythiol composition was obtained by mixing the polythiol composition (A) and the polythiol composition (A1) obtained as described above.
[0248] At that time, the mixing ratio was changed so that the total peak area of the compound represented by Formula (1) and the compound represented by Formula (2) for the total peak area of the compounds included in the polythiol composition 100 was the value listed in Table 1.
[0249] [Comparative Example 1]
[0250] Polythiol composition (A1) was used as the polythiol composition.
[0251] <Measurement of the ratio (area%) of the compound represented by Formula (1) and the compound represented by Formula (2)>
[0252] The ratio (area%) of the compound represented by Formula (1) and the compound represented by Formula (2) by HPLC was measured by the method described in the above-mentioned <Measurement of the peak area of the compound represented by Formula (1) and the compound represented by Formula (2)>.
[0253] The results are shown in Table 1.
[0254] Manufacture of plastic lenses
[0255] [Preparation Example 1]
[0256] 52 parts by mass of m-xylylene diisocyanate, 0.01 parts by mass of dibutyltin dichloride as a curing catalyst, 0.10 parts by mass of Zellec UN (product of Stepan Corporation; acidic phosphate ester), and 1.5 parts by mass of Biosorb 583 (manufactured by Kyodo Yakuhin Co.; UV absorber) were mixed and dissolved at 20°C. 48 parts by mass of the polythiol composition of Example 1 were charged and mixed to form a homogeneous mixture. This homogeneous mixture was degassed at 600 Pa for 1 hour, filtered through a 1 μm Teflon (registered trademark) filter, and then poured into a mold made of a glass mold and tape. This mold was placed in an oven, the temperature was gradually increased from 10°C to 120°C, and polymerization was carried out for 38 hours. After the polymerization was completed, the mold was removed from the oven and released to obtain a resin. The obtained resin was also annealed at 120°C for 1 hour to manufacture a plastic lens. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0257] [Preparation Example 2]
[0258] In Preparation Example 1, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Example 1 was changed to 48 parts by mass of the polythiol composition of Example 2. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0259] [Preparation Example 3]
[0260] In Preparation Example 1, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Example 1 was changed to 48 parts by mass of the polythiol composition of Example 3. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0261] [Preparation Example 4]
[0262] In Preparation Example 1, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Example 1 was changed to 48 parts by mass of the polythiol composition of Comparative Example 1. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0263] The physical properties of each plastic lens of Preparation Examples 1 to 4 (i.e., Examples 1 to 3, Comparative Example 1) are shown in Table 1.
[0264]
[0265] As shown in Table 1, Examples 1 to 3, which include a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by Formula (1) and a compound represented by Formula (2), and in high-speed liquid chromatography measurement, the total peak area of at least one compound selected from the group consisting of a compound represented by Formula (1) and a compound represented by Formula (2) is 1.00 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition, had superior YI and devitrility.
[0266] Meanwhile, Comparative Example 1, in which the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (1) and the compound represented by Formula (2) is not 1.00 or less, has lowered YI and devitrility.
[0267] [Reference Examples 1 to 3]
[0268] A polythiol composition was obtained by mixing the polythiol composition (A) and the polythiol composition (A2) obtained as described above.
[0269] At that time, the mixing ratio was changed so that the total peak area of the compound represented by Formula (3) and the compound represented by Formula (4) for the total peak area of the compound included in the polythiol composition 100 was the value listed in Table 2.
[0270] [Comparative Example 2]
[0271] Polythiol composition (A2) was used as the polythiol composition.
[0272] <Measurement of the ratio (area%) of the compound represented by Equation (3) and the compound represented by Equation (4)>
[0273] The ratio (area%) of the compound represented by Equation (3) and the compound represented by Equation (4) by HPLC is the above-described <measurement of the peak area of the compound represented by Equation (3) and the compound represented by Equation (4)>
[0274] It was measured by the method described in the paragraph.
[0275] The results are shown in Table 2.
[0276] Manufacture of plastic lenses
[0277] [Preparation Example 5]
[0278] 52 parts by mass of m-xylylene diisocyanate, 0.01 parts by mass of dibutyltin dichloride as a curing catalyst, 0.10 parts by mass of Zellec UN (product of Stepan Corporation; acidic phosphate ester), and 1.5 parts by mass of Biosorb 583 (manufactured by Kyodo Yakuhin Co.; UV absorber) were mixed and dissolved at 20°C. 48 parts by mass of the polythiol composition of Reference Example 1 were added and mixed to form a homogeneous mixture. This homogeneous mixture was degassed at 600 Pa for 1 hour, filtered through a 1 μm Teflon (registered trademark) filter, and then poured into a mold made of a glass mold and tape. This mold was placed in an oven, and the temperature was gradually increased from 10°C to 120°C to polymerize for 38 hours. After the polymerization was completed, the mold was removed from the oven and released to obtain a resin. The obtained resin was also annealed at 120°C for 1 hour to manufacture a plastic lens. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0279] [Preparation Example 6]
[0280] In Preparation Example 5, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Reference Example 1 was changed to 48 parts by mass of the polythiol composition of Reference Example 2. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0281] [Preparation Example 7]
[0282] In Preparation Example 5, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Reference Example 1 was changed to 48 parts by mass of the polythiol composition of Reference Example 3. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0283] [Preparation Example 8]
[0284] In Preparation Example 5, a plastic lens was prepared using the same method as described in Preparation Example 1, except that 48 parts by mass of the polythiol composition of Reference Example 1 was changed to 48 parts by mass of the polythiol composition of Comparative Example 2. Each physical property was determined based on the evaluation method for each physical property of the plastic lens described above.
[0285] The physical properties of each plastic lens of Preparation Examples 5 to 8 (i.e., Reference Examples 1 to 3, Comparative Example 2) are shown in Table 2.
[0286]
[0287] As shown in Table 2, Reference Examples 1 to 3, which include a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by the following formula (3) and a compound represented by the following formula (4), and in high-speed liquid chromatography measurement, the total peak area of the at least one compound selected from the group consisting of the compound represented by the formula (3) and the compound represented by the formula (4) is 2.10 or less with respect to the total peak area of the compounds included in the polythiol composition 100, had excellent YI.
[0288] Meanwhile, Comparative Example 2, in which the total peak area of at least one compound selected from the group consisting of the compound represented by Formula (3) and the compound represented by Formula (4) is not 2.10 or less, YI decreased.
[0289] [Example 1X, Example 2X, Example 3X, Reference Example 1X, Reference Example 2X and Reference Example 3X]
[0290] Except for changing the manufacturing of the molded body as follows for each of Example 1X, Example 2X, Example 3X, Reference Example 1X, Reference Example 2X, and Reference Example 3X, the same operation as Example 1, Example 2, Example 3, Reference Example 1, Reference Example 2, and Reference Example 3 was performed, and the same results as the results of Example 1, Example 2, Example 3, Reference Example 1, Reference Example 2, and Reference Example 3 (Tables 1 and 2) were obtained.
[0291] -Changes in each of Example 1, Example 2, Example 3, Reference Example 1, Reference Example 2, and Reference Example 3-
[0292] In each of Examples 1, 2, 3, Reference Example 1, Reference Example 2, and Reference Example 3, m-xylylene diisocyanate (52 parts by mass) was used in the manufacture of the molded body, but in Examples 1X, 2X, 3X, Reference Example 1X, Reference Example 2X, and Reference Example 3X, XDI (52 parts by mass) was changed to XDI composition X1 (an amount in which the amount of m-xylylene diisocyanate contained is 52 parts by mass) as the aforementioned XDI composition.
[0293] XDI composition X1 was prepared by adding trace amounts of compound (N1), compound (N2), and compound (N3) to the main component XDI and mixing them.
[0294] In XDI composition X1, as a result of performing gas chromatography measurements under each of the aforementioned GC condition 1 and GC condition 2,
[0295] The peak area of compound (N1) is 0.20 ppm or more (specifically 600 ppm) relative to the peak area 1 of xylylene diisocyanate, and
[0296] The peak area of compound (N2) is 0.05 ppm or more (specifically 18 ppm) relative to the peak area 1 of xylylene diisocyanate, and
[0297] The peak area of compound (N3) was 0.10 ppm or more (specifically 100 ppm) compared to the peak area 1 of xylylene diisocyanate.
[0298] The disclosure of Japanese patent application 2022-146425 filed on September 14, 2022, is incorporated herein by reference in its entirety.
[0299] All documents, patent applications, and technical specifications described in this specification are incorporated by reference in this specification to the same extent that individual documents, patent applications, and technical specifications are incorporated by reference as they are specifically and individually described.
Claims
Claim 1 Use of a polythiol composition comprising a polythiol compound (A) and at least one compound selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), wherein, in high-speed liquid chromatography measurement, the total peak area of the at least one compound selected from the group consisting of the compound represented by the formula (1) and the compound represented by the formula (2) is 1.00 or less with respect to the total peak area of 100 of the compounds included in the polythiol composition.