Negative electrode active material, negative electrode comprising the same, and lithium secondary battery including the negative electrode

By controlling the particle size differences between natural and artificial graphite, and between artificial graphite and silicon-based active materials, the dispersibility and lifespan of lithium secondary battery electrodes are improved, addressing the issue of localized stress and degradation.

KR103042815B1Active Publication Date: 2026-11-06LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250070896
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-06-05
Filing Date
2025-05-30
Publication Date
2026-11-06
Estimated Expiration
2045-05-30

AI Technical Summary

Technical Problem

The dispersibility of silicon-based and graphite active materials in lithium secondary batteries is poor, leading to slurry clumping and reduced lifespan due to differences in particle sizes, causing localized volume expansion and stress concentration during charging and discharging.

Method used

Control the difference in average particle sizes (D50) between natural and artificial graphite to be within 10% or less, and between artificial graphite and the silicon-based active material to be within 40% or less, ensuring uniform dispersion and preventing localized stress and degradation.

Benefits of technology

Improves the dispersibility of the active materials, suppressing local volume expansion and stress concentration, thereby enhancing the lifespan characteristics of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025060899014-PAT00001_ABST
    Figure 112025060899014-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material, a negative electrode for a lithium secondary battery including the same, and a lithium secondary battery. The negative electrode active material comprises a silicon-based active material and graphite, wherein the graphite comprises natural graphite and artificial graphite, and the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite is 10% or less in absolute value, and the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material is 40% or less in absolute value.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2024-0073588 filed with the Korean Intellectual Property Office on June 5, 2024, the entire contents of which are incorporated herein.

[0002] The present application relates to a negative electrode active material, a negative electrode for a lithium secondary battery comprising the same, and a lithium secondary battery. Background Technology

[0003] Due to the rapid increase in the use of fossil fuels, there is a growing demand for alternative or clean energy. As part of this effort, the fields of power generation and energy storage utilizing electrochemical reactions are the most actively researched.

[0004] Currently, a representative example of an electrochemical device utilizing such electrochemical energy is the secondary battery, and its scope of application is steadily expanding.

[0005] Recently, accompanied by the rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, as well as power tools and vacuum cleaners, the demand for rechargeable batteries that are small and lightweight yet possess relatively high capacity and / or high output is rapidly increasing. In particular, lithium-ion batteries are gaining prominence as power sources for electronic devices due to their lightweight nature and high energy density. Accordingly, active research and development efforts are underway to improve the performance of lithium-ion batteries.

[0006] In a lithium secondary battery, electrical energy is produced by oxidation and reduction reactions when lithium ions are inserted into or removed from the anode and cathode while the anode and cathode are filled with an organic or polymer electrolyte between an anode and a cathode made of active materials capable of lithium ion intercalation and deintercalation.

[0007] Generally, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and extracts lithium ions from the positive electrode, and a material with a discharge capacity may be used as the negative electrode active material.

[0008] Metal oxides such as LiCoO2, LiMnO2, LiMn2O4, or LiNiO2 are used as the positive active material constituting the positive electrode of a lithium secondary battery, and carbon-based materials such as metal lithium, graphite, or activated carbon, or silicon oxide (SiO2) are used as the negative active material constituting the negative electrode. x Materials such as ) are being used. Among the above negative electrode active materials, metallic lithium was primarily used in the beginning, but as the charge and discharge cycles progressed, lithium atoms grew on the surface of the metallic lithium, damaging the separator and causing the battery to fail. Consequently, carbon-based materials are primarily being used recently.

[0009] Although graphite is mainly used as the negative electrode active material for lithium secondary batteries, it is difficult to increase the capacity of lithium secondary batteries because graphite has a low capacity per unit mass of 372 mAh / g. Accordingly, to increase the capacity of lithium secondary batteries, negative electrode materials such as silicon, tin, and their oxides are being developed as non-carbon negative electrode materials that have a higher energy density than graphite. However, in the case of these non-carbon negative electrode materials, although the capacity is high, there is a problem in that the initial efficiency is low, resulting in high lithium consumption during the initial charge and discharge cycles and large irreversible capacity loss.

[0010] Recently, due to the demand for high-density energy batteries, research is actively being conducted on methods to increase capacity by using silicon-based compounds such as Si / C or SiOx, which have a capacity more than 10 times greater than that of graphite-based materials, as negative electrode active materials. However, silicon-based compounds, which are high-capacity materials, have a problem in that, although they have a large capacity compared to graphite used conventionally, they rapidly expand in volume during the charging process, which disrupts the conductive path and degrades battery characteristics.

[0011] Accordingly, to ensure the appropriate capacity and stability of the cathode, a method of manufacturing the electrode is being attempted by using graphite and simultaneously mixing a silicon-based active material with a high specific capacity in an appropriate ratio.

[0012] However, even though a method is used in which a silicon-based active material and graphite are combined in the cathode, the dispersibility of each active material within the electrode is reduced due to the difference in particle sizes between the graphite material and the silicon-based active material, and consequently, slurry clumping occurs, which actually leads to a decrease in lifespan performance.

[0013] Therefore, even when silicon-based active materials are used as negative electrode active materials to improve capacity performance, research is required to improve the dispersibility of the aforementioned negative electrode active materials. Prior art literature

[0014] Japanese Published Patent Application No. 2009-080971 The problem to be solved

[0015] The inventors conducted research on improving dispersibility in the aforementioned mixed negative electrode active material of silicon-based active material and graphite. In particular, they discovered that when the average particle size (D50) of the graphite material and the silicon-based active material used as the negative electrode active material is controlled, the dispersibility of the active material within the electrode can be improved, and they found that clustering of the silicon-based active material can be prevented, thereby enabling optimal battery performance, which led to the present invention. means of solving the problem

[0016] One embodiment of the present invention provides a negative electrode active material, wherein the negative electrode active material comprises a silicon-based active material and graphite, wherein the graphite comprises natural graphite and artificial graphite, and the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite is 10% or less in absolute value, and the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material is 40% or less in absolute value.

[0017] Another embodiment of the present invention provides a negative electrode for a lithium secondary battery comprising: a negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, wherein the negative electrode active material layer comprises the aforementioned negative electrode active material.

[0018] Finally, the present invention provides a lithium secondary battery comprising: a positive electrode; a negative electrode for the aforementioned lithium secondary battery; a separator provided between the positive electrode and the negative electrode; and an electrolyte. Effects of the invention

[0019] According to one embodiment of the present invention, the ratio of the difference in average particle size (D50) between natural graphite and artificial graphite is controlled to an absolute value of 10% or less, and the ratio of the difference in average particle size (D50) between artificial graphite and silicon-based active material is controlled to an absolute value of 40% or less. By controlling the average particle size (D50) of the negative electrode active material contained in the negative electrode in this manner, the dispersibility of the negative electrode active material in the negative electrode slurry can be improved. Accordingly, the negative electrode manufactured has improved dispersibility of two or more active materials within the electrode, thereby suppressing local volume expansion and stress concentration phenomena, and thus has the characteristic of improving the lifespan characteristics of the electrode.

[0020] Specifically, by limiting the average particle size of the silicon-based active material and artificial graphite as described above, the silicon-based active material has a smaller particle size than the graphite-based active material. When a negative electrode slurry is mixed and the electrode is coated in a state where there is a difference in particle size, a phenomenon occurs in which the silicon-based active material, which has a smaller particle size compared to the graphite-based active material, forms local clusters. Since the clusters of silicon-based active material undergo a significant volume change during the charge / discharge process compared to the surrounding graphite-based active material, acting as a factor that accelerates electrode degradation, it is necessary to control the difference in average particle size between the silicon-based active material and artificial graphite as described above.

[0021] Similarly, in the case of natural graphite and artificial graphite within the graphite-based active material, the average particle size is controlled as in the present application. Through such control, the active material within the electrode is evenly dispersed, thereby preventing the occurrence of localized stress, accelerated reactions, and degradation during the operation of the battery, and enabling the manufacture of a uniformly dispersed electrode.

[0022] In other words, the aforementioned problem can be solved by controlling the difference in average particle sizes between the silicon-based active material and the artificial graphite, and between the artificial graphite and the natural graphite contained within the graphite, rather than simply controlling the average particle size of the silicon-based active material and the graphite, or controlling the average particle size of the artificial graphite and the natural graphite within the graphite alone. Brief explanation of the drawing

[0023] FIG. 1 is a diagram showing a stacked structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application. FIG. 2 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application. Specific details for implementing the invention

[0024] Hereinafter, the present invention will be described in more detail to aid in understanding the invention.

[0025] Terms and words used in this specification and claims shall not be interpreted as being limited to their ordinary or dictionary meanings, but shall be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0026] The terms used in this specification are used merely to describe exemplary embodiments and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.

[0027] In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0028] Furthermore, when it is said that a part, such as a layer, is "above" or "on" another part, this includes not only the case where it is "directly above" the other part, but also the case where there is another part in between. Conversely, when it is said that a part is "directly above" another part, it means that there is no other part in between. Also, saying that a part is "above" or "on" a reference part means that it is located above or below the reference part, and it does not necessarily mean that it is located "above" or "on" facing the opposite direction of gravity.

[0029] In this specification, "specific surface area" refers to a measurement by the BET method. Specifically, it can be measured by using a BET measuring instrument (BEL-SORP-mini, Nippon Bell) on the subject to measurement, degassing at 130°C for 2 hours, and performing N2 absorption / desorption at 77K. That is, in this specification, the BET specific surface area may refer to the specific surface area of ​​the particle itself measured by the above measurement method.

[0030] In this specification, the average length or diameter of the conductive material can be measured using SEM or TEM.

[0031] In this specification, "Dn" refers to the particle size distribution and represents the particle size at the n% point of the cumulative distribution of the number of particles according to particle size. That is, D50 is the particle size (average particle size) at the 50% point of the cumulative distribution of the number of particles according to particle size, D90 is the particle size at the 90% point of the cumulative distribution of the number of particles according to particle size, and D10 is the particle size at the 10% point of the cumulative distribution of the number of particles according to particle size. Meanwhile, the average particle size can be measured using the laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction patterns according to particle size is measured as the particles pass through the laser beam to calculate the particle size distribution.

[0032] In the present application, the measurement of “Dn” of the active material in the cathode can be performed by confirming the size of the active material contained in the cathode after the final charge and discharge following the manufacture of the cathode. Specifically, the average particle size (D50) can be measured at the electrode cross-section when the cross-section of the cathode active material layer is continuously cut after the manufacture of the cathode and the final charge and discharge. At this time, a three-dimensional imaging technique can be utilized. Specifically, a three-dimensional image can be obtained by stacking images of the cross-sections obtained continuously, and through this, it is possible to compare the average particle size between active materials within the battery after charge and discharge.

[0033] In one embodiment of the present application, particle size or particle diameter may refer to the average diameter or representative diameter of each individual grain constituting the metal powder.

[0034] In this specification, the meaning that a polymer contains a monomer in monomer units means that the monomer participates in a polymerization reaction and is included as a repeating unit within the polymer. In this specification, when it is stated that a polymer contains a monomer, this is interpreted as the same as the polymer containing the monomer in monomer units.

[0035] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers unless specified as "homopolymer."

[0036] In this specification, the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) are polystyrene equivalent molecular weights measured by gel permeation chromatography (GPC), using commercially available monodisperse polystyrene polymers of various degrees of polymerization (standard samples) for molecular weight measurement as standard materials. In this specification, the term "molecular weight" means weight-average molecular weight unless otherwise specified.

[0037] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in various different forms and is not limited to the description below.

[0038] One embodiment of the present invention provides a negative electrode active material, wherein the negative electrode active material comprises a silicon-based active material and graphite, wherein the graphite comprises natural graphite and artificial graphite, and the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite is 10% or less in absolute value, and the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material is 40% or less in absolute value.

[0039] The cathode according to the present application comprises natural graphite, artificial graphite, and a silicon-based active material. Artificial graphite has a relatively slow rate limit but high structural stability, while natural graphite has a relatively larger volume change compared to artificial graphite but a high rate limit, so the two graphites differ in their properties. By utilizing these properties, the two graphites are blended to compensate for the differences in properties when configuring a graphite electrode. In particular, the present application uses a silicon-based active material together with the graphite to compensate for the relatively low specific capacity of the graphite.

[0040] While using a single type of active material does not pose a significant problem, using multiple types simultaneously leads to differences in particle size. Smaller particles form clusters within the electrode, causing localized non-uniformity. In this scenario, the volume change of the clustered Si-based active material is accompanied by significant volume expansion compared to the surrounding graphite-based active material. Consequently, localized stress, structural changes, and loss of conductivity occur within the electrode, resulting in increased internal resistance and reduced lifespan.

[0041] Recognizing the above-mentioned problem, the present application is characterized by controlling the particle size relationship between natural graphite and silicon-based active material, respectively, based on artificial graphite, in a cathode that simultaneously applies artificial graphite, natural graphite, and silicon-based active material. That is, it has the characteristic of being able to control the occurrence of local non-uniformity according to the interrelationship of the particle sizes of each active material.

[0042] In the present application, the negative electrode active material comprises a silicon-based active material and graphite.

[0043] In the present application, the silicon-based active material is Si, SiOx (0 <x<2), Si / C, 및 Si 합금으로 이루어진 군에서 선택되는 1 이상을 포함할 수 있다.

[0044] In the present application, when the silicon-based active material is Si, the content of Si in the silicon-based active material may be 98% or more, 99% or more, specifically 100%.

[0045] In the present application, when the silicon-based active material is the remainder excluding Si, the content of Si based on 100 parts by weight of the silicon-based active material may be 40 parts by weight or more and 80 parts by weight or less. That is, the content of the Si element itself within the silicon-based active material may satisfy the above range.

[0046] In the present application, the Si / C can be expressed as a silicon carbon composite.

[0047] In this specification, the silicon carbon composite is a composite of Si and C and is distinguished from silicon carbide denoted as SiC. Since the silicon carbide does not electrochemically react with lithium, all performance characteristics, such as lifespan, can be measured as zero.

[0048] The above silicon carbon composite may be a composite of silicon and graphite, etc., and may form a structure in which graphene or amorphous carbon, etc. surrounds a core composed of silicon and graphite, etc. In the above silicon carbon composite, the silicon may be nano silicon. For example, the nano silicon may be silicon in the range of 1 nm to 999 nm.

[0049] In the present application, the graphite includes natural graphite and artificial graphite.

[0050] In the present application, the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite may be 10% or less in absolute value.

[0051] In another embodiment, the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite may be 10% or less in absolute value, preferably 9% or less, more preferably 8.5% or less, and may be 1% or more, or 3% or more.

[0052] In the present application, the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material may be 40% or less in absolute value.

[0053] In another embodiment, the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material may be 40% or less in absolute value, preferably 38% or less, more preferably 35% or less, and may be 1% or more, 5% or more, 10% or more, or 20% or more.

[0054] The present application is characterized by controlling the average particle size of the silicon-based active material, artificial graphite, and the artificial graphite and natural graphite contained within the graphite as described above. By satisfying the above range, the three types of active materials contained within the cathode slurry can exhibit uniform dispersion without forming separate clusters. Accordingly, localized reaction promotion, stress concentration, and electrode degradation caused by differing reactivity with lithium ions can be improved, and the effect of improving the lifespan of the manufactured cathode can be manifested.

[0055] Specifically, the reason for limiting the difference in particle size between the silicon-based active material and artificial graphite as described above is that the silicon-based active material has a smaller particle size than the graphite material. When a slurry is mixed and an electrode is coated under conditions where there is a difference in particle size, the silicon-based active material with the smaller particle size forms local clusters. Since these clusters of silicon-based active material undergo a larger volume change during the charge / discharge process compared to the surrounding graphite material, they act as a factor that accelerates the degradation of the electrode; therefore, this is intended to prevent such a phenomenon. At this time, the particle size of the silicon-based active material was not compared with the total particle size of the graphite, but rather with the particle size of the artificial graphite within the graphite, which has a similar meaning to comparing it with the total particle size of the graphite.

[0056] In the present application, the ratio of the absolute value of the difference in average particle size (D50) between the artificial graphite and the natural graphite can be calculated as |{(AB) / A}| x 100% when the average particle size of the artificial graphite is defined as A and the average particle size of the natural graphite is defined as B.

[0057] In the present application, the ratio of the absolute value of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material can be calculated as |{(AC) / A}| x 100% when the average particle size of the artificial graphite is defined as A and the average particle size of the silicon-based active material is defined as C.

[0058] That is, the aforementioned effect can be achieved when the average particle size of the silicon-based active material or natural graphite is larger or smaller than a specific range based on artificial graphite, and is included within a certain proportion.

[0059] In the present application, the average particle size (D50) of the silicon-based active material may be 1 μm or more and 10 μm or less.

[0060] In another embodiment, the average particle size (D50) of the silicon-based active material may satisfy the range of 1 μm or more and 10 μm or less, 2 μm or more and 10 μm or less, and 4 μm or more and 10 μm or less.

[0061] In the present application, the average particle size (D50) of the graphite may be 5㎛ or more and 20㎛ or less.

[0062] In another embodiment, the average particle size (D50) of the graphite may be 5㎛ or more and 20㎛ or less, preferably 6㎛ or more and 18㎛ or less, and more preferably 7㎛ or more and 17㎛ or less.

[0063] In the present application, the average particle size (D50) of the natural graphite is 5㎛ or more and 20㎛ or less, and the average particle size (D50) of the artificial graphite may be 5㎛ or more and 20㎛ or less.

[0064] In another embodiment, the average particle size (D50) of the natural graphite may be 5㎛ or more and 20㎛ or less, preferably 7㎛ or more and 17㎛ or less, and more preferably 9㎛ or more and 15㎛ or less.

[0065] In another embodiment, the average particle size (D50) of the artificial graphite may be 5㎛ or more and 20㎛ or less, preferably 8㎛ or more and 18㎛ or less, and more preferably 10㎛ or more and 16㎛ or less.

[0066] In the present application, the average particle size of the graphite may refer to the average particle size (D50) relative to the overall average of the artificial graphite and natural graphite contained within the graphite. In this case, the present application did not compare the particle size of the silicon-based active material with that of the graphite as a whole, but rather compared it with the particle size of the artificial graphite within the graphite; however, this has a meaning similar to comparing it with the particle size of the graphite as a whole.

[0067] In the present application, the average particle size of the silicon-based active material and the graphite may be used without limitation as long as they satisfy the aforementioned difference in average particle size. In particular, when using a silicon-based active material and graphite having an average particle size within the above range, it is possible to prevent the silicon-based active material from forming local clusters within the electrode. Consequently, negative reactions such as local stress generation, accelerated reaction with lithium ions, and rapid degradation of the active material can be suppressed due to the silicon-based active material, which undergoes a large volume change during the charging / discharging process compared to surrounding graphite materials.

[0068] In this application, limiting the difference in particle size between natural and artificial graphite to a level below a certain threshold is for the same reasons as described above. Since a difference in particle size prevents the active material from being evenly dispersed within the electrode, it can lead to localized stress, accelerated reactions, and degradation during the operation of the battery. Accordingly, in order to produce a uniform electrode, all active materials must have a difference in particle size within the scope of this application.

[0069] In one embodiment of the present application, the weight ratio of the silicon-based active material to graphite based on 100 parts by weight of the negative electrode active material may be 5:95 to 40:60.

[0070] In another embodiment, the weight ratio of the silicon-based active material to graphite based on 100 parts by weight of the cathode active material may satisfy 5:95 to 40:60, preferably 7:93 to 35:75, and more preferably 10:90 to 30:70.

[0071] In the present application, the ratio of silicon-based active material and graphite within the negative electrode active material satisfies the above range. Although silicon-based active material is known to have excellent capacity characteristics, if applied in a high content, lifespan performance may be degraded due to volume expansion during charging and discharging, and if included in a low content, it may be difficult to improve capacity characteristics. Therefore, by having the above-mentioned content, it is characterized by improving both capacity and lifespan characteristics.

[0072] In the present application, the weight ratio of artificial graphite to natural graphite based on 100 parts by weight of the graphite may be 60:40 to 80:20.

[0073] In another embodiment, the weight ratio of artificial graphite to natural graphite based on 100 parts by weight of the graphite may satisfy 60:40 to 80:20, preferably 65:35 to 78:22, and more preferably 70:30 to 75:25.

[0074] Graphite may include both synthetic and natural graphite; as it has been confirmed that synthetic graphite exhibits superior cell characteristics compared to natural graphite, the use of natural graphite is being reduced while the amount of synthetic graphite is being increased. However, from a cost perspective, synthetic graphite poses a problem due to high processing costs resulting from the calcination and graphitization of coke. Consequently, satisfying the aforementioned range provides the characteristic of improving cell characteristics while addressing cost issues.

[0075] In the present application, the negative electrode active material may be included in small weight proportions in the order of artificial graphite, natural graphite, and silicon-based active material.

[0076] In the present application, the average particle size (D50) of the artificial graphite is larger than the average particle size (D50) of the natural graphite, and the average particle size (D50) of the natural graphite may be larger than the average particle size (D50) of the silicon-based active material.

[0077] In the present application, based on the average particle size (D50) of the artificial graphite with the highest weight ratio in the negative electrode active material, the relationship of artificial graphite > natural graphite > average particle size (D50) of the silicon-based active material can be satisfied.

[0078] In the present application, based on the average particle size (D50) of the artificial graphite with the highest weight ratio in the negative electrode active material, the relationship of natural graphite > artificial graphite > average particle size (D50) of the silicon-based active material can be satisfied.

[0079] In the present application, the relationship between artificial graphite > natural graphite > silicon-based active material average particle size (D50) is satisfied based on the average particle size (D50) of artificial graphite, which has the highest weight ratio in the negative electrode active material, and the average particle size of the natural graphite based on the average particle size of the artificial graphite is in a range having a difference of 10% or less, and the average particle size of the silicon-based active material based on the average particle size of the artificial graphite may be in a range of 20% or more and 40% or less.

[0080] In the present application, the relationship between natural graphite > artificial graphite > silicon-based active material average particle size (D50) is satisfied based on the average particle size (D50) of artificial graphite with the highest weight ratio in the negative electrode active material, and the average particle size of the artificial graphite based on the average particle size of the natural graphite is in a range having a difference of 10% or less, and the average particle size of the silicon-based active material based on the average particle size of the artificial graphite may be smaller in the range of 20% or more and 40% or less.

[0081] In other words, if the average particle size values ​​of artificial graphite and natural graphite satisfy the aforementioned difference value, the average particle size of artificial graphite may be larger or smaller than that of natural graphite.

[0082] In the present application, a cathode composition comprising the above-mentioned cathode active material is provided.

[0083] In the present application, the cathode composition may further include, in addition to the silicon-based active material, a cathode conductive material; and a cathode binder.

[0084] That is, in the present application, as a cathode composition comprising the above-mentioned cathode active material, the cathode composition may further comprise a cathode conductive material; and a cathode binder.

[0085] At this time, the cathode composition and the cathode slurry are different from each other, and if the cathode composition includes a slurry solvent, it can be expressed as a cathode slurry.

[0086] In the present application, the negative electrode active material may comprise 90 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0087] In another embodiment, the cathode active material may be 90 parts by weight or more, 91 parts by weight or more, 92 parts by weight or more, and 95 parts by weight or less, based on 100 parts by weight of the cathode composition.

[0088] By including a cathode active material within the range described above, the cathode has the characteristic of being able to secure capacity characteristics and energy density.

[0089] Conventionally, it was common practice to use only graphite-based compounds as negative electrode active materials. However, with the recent increase in demand for high-capacity batteries, there have been increasing attempts to mix and use silicon-based active materials to increase capacity. However, in the case of silicon-based active materials, even if the characteristics of the silicon-based active material itself are controlled as described above, the volume expands rapidly during the charging and discharging process, which can cause some problems that damage the conductive paths formed within the negative electrode active material layer.

[0090] Accordingly, in one embodiment of the present application, the cathode conductive material may include one or more selected from the group consisting of point conductive materials, planar conductive materials, and linear conductive materials.

[0091] In one embodiment of the present application, the point-shaped conductive material can be used to improve conductivity of the cathode and refers to a point-shaped or spherical conductive material having conductivity without causing chemical changes. Specifically, the point-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably may include carbon black in terms of achieving high conductivity and excellent dispersibility.

[0092] In one embodiment of the present application, the point-shaped conductive material has a BET specific surface area of ​​40 m² 2 / g or more 70m 2 It may be less than / g, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 It may be less than / g.

[0093] In one embodiment of the present application, the point-shaped conductive material may satisfy a volatile matter content of 0.01% or more and 1% or less, preferably 0.01% or more and 0.3% or less, and more preferably 0.01% or more and 0.1% or less.

[0094] In particular, when the functional group content of the point-shaped conductive material satisfies the above range, the functional groups present on the surface of the point-shaped conductive material allow the point-shaped conductive material to be smoothly dispersed within the solvent when water is used as the solvent. In particular, in the present invention, the functional group content of the point-shaped conductive material can be lowered by using a specific silicon-based active material, thereby providing an excellent effect in improving dispersibility.

[0095] In one embodiment of the present application, the invention is characterized by including a point-shaped conductive material having a functional group content within the above range together with a silicon-based active material, wherein the control of the functional group content can be controlled according to the degree of heat treatment of the point-shaped conductive material.

[0096] In one embodiment of the present application, the particle size of the dot-shaped conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.

[0097] In one embodiment of the present application, the conductive material may include a planar conductive material.

[0098] The above-described planar conductive material can improve conductivity by increasing surface contact between silicon particles within the cathode, while simultaneously suppressing the disruption of conductive pathways due to volume expansion. The above-described planar conductive material may be described as a plate-shaped conductive material or a bulk-shaped conductive material.

[0099] In one embodiment of the present application, the planar conductive material may comprise at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and preferably may be plate-shaped graphite.

[0100] In one embodiment of the present application, the average particle size (D50) of the planar conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 3.5 μm to 5 μm. When the above range is satisfied, dispersion is easy without causing an excessive increase in the viscosity of the cathode slurry due to the sufficient particle size. Therefore, when dispersion is performed using the same equipment and time, the dispersion effect is excellent.

[0101] In one embodiment of the present application, the planar conductive material provides a cathode composition in which D10 is 0.5 μm or more and 2.0 μm or less, D50 is 2.5 μm or more and 3.5 μm or less, and D90 is 6.5 μm or more and 15.0 μm or less.

[0102] In one embodiment of the present application, the planar conductive material may be a high specific surface area planar conductive material having a high BET specific surface area; or a low specific surface area planar conductive material.

[0103] In one embodiment of the present application, a planar conductive material with a high specific surface area or a planar conductive material with a low specific surface area may be used without limitation as the planar conductive material; however, since the planar conductive material according to the present application may be affected to some extent by dispersion in electrode performance, it may be particularly preferable to use a planar conductive material with a low specific surface area that does not cause problems with dispersion.

[0104] In one embodiment of the present application, the planar conductive material has a BET specific surface area of ​​0.25 m² 2 It can be more than / g.

[0105] In another embodiment, the planar conductive material has a BET specific surface area of ​​1 m²2 / g or more than 500m 2 It may be less than / g, preferably 5m 2 / g or more than 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 It may be less than / g.

[0106] The planar conductive material according to the present application may use a planar conductive material with a high specific surface area; or a planar conductive material with a low specific surface area.

[0107] In another embodiment, the planar conductive material is a high specific surface area planar conductive material, and has a BET specific surface area of ​​50 m² 2 / g or more than 500m 2 / g or less, preferably 80m 2 / g or more than 300m 2 / g or less, more preferably 100m 2 / g or more than 300m 2 It can satisfy a range of / g or less.

[0108] In another embodiment, the planar conductive material is a low specific surface area planar conductive material, and has a BET specific surface area of ​​1 m² 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 It can satisfy a range of / g or less.

[0109] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may comprise a plurality of carbon nanotube units. Specifically, "bundle type" here refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged in parallel or intertwined with the axes along the length direction of the carbon nanotube units in substantially the same orientation, unless otherwise noted. The carbon nanotube units have a graphite sheet having a cylindrical shape with a nano-sized diameter and an sp2 bonding structure. Depending on the angle and structure in which the graphite sheet is rolled, it may exhibit conductive or semiconductor properties. Compared to entangled type carbon nanotubes, the bundled carbon nanotubes described above can be uniformly dispersed during cathode manufacturing and smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.

[0110] In one embodiment of the present application, the cathode conductive material provides a cathode composition in which the cathode composition is 0.1 parts by weight or more and 5 parts by weight or less based on 100 parts by weight of the cathode composition.

[0111] In another embodiment, the cathode conductive material may comprise 0.1 parts by weight or more and 5 parts by weight or less, preferably 0.2 parts by weight or more and 3 parts by weight or less, more preferably 0.2 parts by weight or more and 2 parts by weight or less, and most preferably 0.2 parts by weight or more and 1 part by weight or less, based on 100 parts by weight of the cathode composition.

[0112] In particular, in one embodiment of the present application, the negative electrode conductive material includes a linear conductive material and satisfies the composition and ratio respectively, so that the lifespan characteristics of the existing lithium secondary battery are not significantly affected, and the number of points capable of charging and discharging increases, resulting in excellent output characteristics at a high C-rate.

[0113] The cathode conductive material according to the present application has a completely separate composition from the anode conductive material applied to the anode. That is, the cathode conductive material according to the present application serves to hold the contact points between silicon-based active materials, which undergo significant volume expansion of the electrodes due to charging and discharging, whereas the anode conductive material serves as a buffer during rolling and provides partial conductivity; thus, their composition and roles are completely different from those of the cathode conductive material of the present invention.

[0114] Furthermore, the cathode conductive material according to the present application is applied to silicon-based active materials and has a completely different composition from that of a conductive material applied to graphite-based active materials. That is, a conductive material used in an electrode having a graphite-based active material simply has particles smaller than the active material, thereby providing improved output characteristics and some conductivity; thus, its composition and role are completely different from that of a cathode conductive material applied together with a silicon-based active material as in the present invention.

[0115] In one embodiment of the present application, the planar conductive material used as the aforementioned negative electrode conductive material has a structure and role different from that of a carbon-based active material generally used as a negative electrode active material. Specifically, the carbon-based active material used as a negative electrode active material may be artificial graphite or natural graphite, and refers to a material processed into a spherical or dot shape to facilitate the storage and release of lithium ions.

[0116] On the other hand, planar conductive materials used as cathode conductive materials are substances having a planar or plate-like form, which can be described as plate-like graphite. In other words, they refer to materials included to maintain conductive pathways within the cathode active material layer; they do not serve the role of lithium storage or release, but rather are materials intended to secure conductive pathways in a planar form within the cathode active material layer.

[0117] In other words, in the present application, the fact that plate-shaped graphite is used as a conductive material means that it is processed into a planar or plate-shaped form and used as a material that secures a conductive pathway rather than serving the role of storing or releasing lithium. At this time, the negative electrode active material included together has high capacity characteristics for lithium storage and release and plays a role in storing and releasing all lithium ions delivered from the positive electrode.

[0118] On the other hand, in the present application, the fact that graphite is used as an active material means that it is processed into a point or spherical shape and used as a material that serves the role of storing or releasing lithium.

[0119] That is, in one embodiment of the present application, the graphite, whether artificial graphite or natural graphite, is in a point-like form and has a BET specific surface area of ​​0.1 m² 2 / g or more than 4.5 m 2 It can satisfy a range of / g or less. In addition, plate-shaped graphite, a planar conductive material, has a planar form with a BET specific surface area of ​​5m² 2 It can be more than / g.

[0120] In one embodiment of the present application, the cathode binder may comprise at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and materials in which hydrogens thereof are substituted with Li, Na, or Ca, etc., and may also comprise various copolymers thereof.

[0121] The cathode binder according to one embodiment of the present application serves to hold the active material and the conductive material to prevent distortion and structural deformation of the cathode structure during volume expansion and relaxation of the silicon-based active material. Any general binder that satisfies the above role can be applied, specifically a water-based binder can be used, and more specifically, a PAM-based binder can be used.

[0122] In one embodiment of the present application, the cathode binder may be 1 part by weight or more and 10 parts by weight or less, preferably 2 parts by weight or more and 9 parts by weight or less, based on 100 parts by weight of the cathode composition, more preferably 2 parts by weight or more and 8 parts by weight or less.

[0123] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, comprising: a negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, wherein the negative electrode active material layer comprises a negative electrode active material according to the present application.

[0124] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, comprising: a negative electrode current collector layer; and a negative electrode active material layer formed on one or both sides of the negative electrode current collector layer, the negative electrode composition according to the present application, a cured product thereof, or a dried product thereof.

[0125] FIG. 1 is a diagram showing a stacked structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and FIG. 1 shows that the negative active material layer is formed on one surface, but it can be included on both surfaces of the negative current collector layer.

[0126] In one embodiment of the present application, the negative electrode for the lithium secondary battery may be formed by applying and drying a negative electrode slurry containing the negative electrode composition on one or both sides of a negative electrode current collector layer.

[0127] At this time, the cathode slurry may include the aforementioned cathode composition; and a slurry solvent.

[0128] In one embodiment of the present application, the solid content of the cathode slurry may satisfy 5% or more and 40% or less.

[0129] In another embodiment, the solid content of the cathode slurry may satisfy a range of 5% or more and 40% or less, preferably 7% or more and 35% or less, and more preferably 10% or more and 30% or less.

[0130] The solid content of the above cathode slurry may refer to the content of the cathode composition included in the above cathode slurry, and may refer to the content of the cathode composition based on 100 parts by weight of the cathode slurry.

[0131] When the solid content of the above cathode slurry satisfies the above range, the viscosity is suitable when forming the cathode active material layer, thereby minimizing particle aggregation of the cathode composition and enabling the cathode active material layer to be formed efficiently.

[0132] In one embodiment of the present application, the slurry solvent may be used without limitation as long as it can dissolve the cathode composition, and specifically, water or NMP may be used.

[0133] In one embodiment of the present application, the negative current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative current collector layer is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy may be used. In addition, fine irregularities may be formed on the surface to strengthen the bonding strength of the negative active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven body, etc.

[0134] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, wherein the thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, and the thickness of the negative electrode active material layer is 5 μm or more and 500 μm or less.

[0135] However, the thickness may vary depending on the type and application of the cathode used, and is not limited thereto.

[0136] In one embodiment of the present application, the porosity of the negative electrode active material layer may satisfy a range of 10% or more and 60% or less.

[0137] In another embodiment, the porosity of the negative electrode active material layer may satisfy a range of 10% or more and 60% or less, preferably 20% or more and 50% or less, and more preferably 30% or more and 45% or less.

[0138] The above porosity varies depending on the composition and content of the silicon-based active material, conductive material, and binder included in the cathode active material layer, and in particular, satisfies the above range by including the silicon-based active material and conductive material according to the present application in a specific composition and content portion, thereby characterized in that the electrical conductivity and resistance of the electrode have an appropriate range.

[0139] In one embodiment of the present application, a lithium secondary battery is provided, comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.

[0140] In the present application, the cathode active material layer may further include a cathode conductive material; and a cathode binder.

[0141] In the present application, the negative electrode active material may comprise at least 90 parts by weight based on 100 parts by weight of the composition included in the negative electrode active material layer.

[0142] In the present application, the cathode conductive material is 0.1 parts by weight or more and 5 parts by weight or less based on 100 parts by weight of the composition included in the cathode active material layer, and the cathode binder is 1 part by weight or more and 10 parts by weight or less based on 100 parts by weight of the composition included in the cathode active material layer.

[0143] At this time, the composition included in the cathode active material layer may be the aforementioned cathode composition.

[0144] FIG. 2 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and a positive electrode (200) for a lithium secondary battery including a positive active material layer (40) on one surface of a positive current collector layer (50) can be seen, and the structure is formed such that the negative electrode (100) for a lithium secondary battery and the positive electrode (200) for a lithium secondary battery are stacked with a separator (30) in between.

[0145] A secondary battery according to one embodiment of the present specification may particularly include a negative electrode for a lithium secondary battery as described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the negative electrode is identical to the negative electrode described above. Since the negative electrode has been described above, a detailed description thereof is omitted.

[0146] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and comprising the positive electrode active material.

[0147] In the above-mentioned positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above-mentioned positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0148] The above-mentioned positive electrode active material may be a commonly used positive electrode active material. Specifically, the above-mentioned positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 Examples include lithium manganese composite oxides represented by O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); and LiMn2O4 in which a portion of the Li in the chemical formula is substituted with alkaline earth metal ions, but are not limited thereto. The anode may also be Li-metal.

[0149] The above-described positive active material layer may include a positive conductive material and a positive binder together with the positive active material described above.

[0150] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that has electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powder or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.

[0151] In addition, the anode binder serves to improve adhesion between anode active material particles and adhesion between the anode active material and the anode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.

[0152] The above separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator typically used as a separator in a secondary battery can be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0153] Examples of the above electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., but are not limited to these.

[0154] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0155] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolone, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolone derivative, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivative, tetrahydrofuran derivative, ether, methyl propionate, ethyl propionate, etc. may be used.

[0156] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.

[0157] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.

[0158] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.

[0159] One embodiment of the present invention provides a battery module including the secondary battery as a unit cell and a battery pack including the same. Since the battery module and the battery pack include the secondary battery having high capacity, high rate capability and cycle capability, they can be used as a power source for medium-to-large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.

[0160] In one embodiment of the present application, the lithium secondary battery is a cylindrical battery.

[0161] According to one example, the cylindrical battery may mean that the shape of the battery itself is cylindrical, comprising an assembly including a positive electrode, a negative electrode, a separator, and an electrolyte, and specifically may consist of a cylindrical can, a battery assembly provided inside the cylindrical can, and a top cap.

[0162] In one embodiment of the present application, a battery module including the lithium secondary battery is provided.

[0163] In one embodiment of the present application, a battery pack comprising a battery module according to the above embodiment is provided.

[0164] Further embodiments of the present invention provide a battery module comprising the aforementioned cylindrical battery as a unit cell and a battery pack comprising the same. Since the battery module and the battery pack include the secondary battery having high capacity, high rate capability and cycle capability, they can be used as a power source for medium-to-large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.

[0165] Since the lithium secondary battery according to the embodiments of the present invention stably exhibits excellent discharge capacity, output characteristics, and cycle performance, it can be used as a power source for portable devices such as mobile phones, laptop computers, and digital cameras, as well as for medium-to-large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems. For example, the battery module or battery pack can be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0166] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the above embodiments are merely illustrative of the description, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the description, and that such variations and modifications fall within the scope of the appended claims.

[0167] <Preparation Example>

[0168] <Example 1>

[0169] Manufacturing of the cathode

[0170] A cathode composition was prepared based on 100 parts by weight of the total content of the cathode active material in the cathode composition, comprising 15 parts by weight of Si / C, 85 parts by weight of graphite (synthetic graphite: natural graphite = 80:20 weight ratio), and 0.001 parts by weight of single-walled carbon nanotubes, and based on 100 parts by weight of the cathode composition, comprising 2.5 parts by weight of SBR (styrenebutadiene rubber) and 1.1 parts by weight of CMC (carboxymethyl cellulose) as binders, and additionally comprising 0.06 parts by weight of a dispersant and 0.04 parts by weight of single-walled CNTs, comprising 0.108 parts by weight of a CNT pre-dispersion liquid. At this time, the average particle size (D50) of the synthetic graphite, natural graphite, and silicon carbon composite in the composition was prepared to be 12.4 μm, 11.4 μm, and 9.39 μm, respectively.

[0171] A cathode composition was prepared by adding the silicon carbon composite, graphite, binder carboxymethylcellulose (CMC), and styrene butadiene rubber (SBR) to a single-walled carbon nanotube dispersion using distilled water as a dispersion medium and CMC (carboxymethyl cellulose) as a dispersant, stirring the mixture, and then adding distilled water (solid content = 50 parts by weight).

[0172] The above cathode composition was applied to a copper (Cu) metal thin film, which is a cathode current collector with a thickness of 15 μm, and dried. At this time, the temperature of the circulating air was 60 ℃. Subsequently, a cathode was prepared by rolling and drying in a vacuum oven at 130 ℃ for 12 hours, in which a cathode active material layer was disposed on the cathode current collector.

[0173] At this time, the weight of the CMC added as a binder among the above CMC: the weight of the CMC added as a dispersant is 1.14:0.06. In the above cathode active material layer, the average length of the single-walled carbon nanotube unit was 10 μm, and the average diameter was 2 nm.

[0174] The above cathode was manufactured in the same manner as Example 1, except that the average particle size was controlled as shown in Table 1 below.

[0175] Silicon-based active material (㎛) Artificial graphite (㎛) Natural graphite (㎛) Difference in absolute average particle size between silicon-based active material and artificial graphite (%) (based on artificial graphite) Difference in absolute average particle size between artificial graphite and natural graphite (%) (based on artificial graphite) Example 1 9.39 12.4 11.4 24.27% 8.06% Example 2 9.39 12.4 12.0 24.27% 3.22% Example 3 9.86 12.4 11.4 20.48% 8.06% Example 4 9.86 12.4 12.0 20.48% 3.22% Example 5 9.15 10.8 10.1 15.28% 6.48% Example 6 10.0 13.0 12.4 23.08% 4.62% Comparative Example 1 9.39 16.8 17 44.11% 1.19% Comparative Example 2 9.39 16.8 11.4 44.11% 32.14% Comparative Example 3 9.39 12.4 17 24.27% 37.10% Comparative Example 4 6.53 12.4 11.4 47.34% 8.06%

[0176] (2) Manufacturing of the anode

[0177] A positive electrode slurry was prepared by adding a positive electrode active material (Li(NiaCobMnc)O2, where the NCM excluding lithium (Li) and oxygen (O2) has a ratio of Ni:Co:Mn=60 / 10 / 30, satisfying the ratio (a:b:c=0.60:0.10:0.30), a positive electrode conductive material (LB.CNT), and a binder (PVdF) in a weight ratio of 97.0:1.56:1.44 to a solvent (N-methylpyrrolidone, NMP). The positive electrode slurry was coated onto an aluminum (Al) thin film, which serves as a positive electrode current collector, with a thickness of 12 μm, dried, and then rolled using a roll press to produce a positive electrode.

[0178] (3) Manufacturing of secondary batteries

[0179] An electrode assembly was manufactured by interposing a compression-resistant thin film separator (PE 9um) ceramic coating 3um / 3um between the anode and the cathode. After placing the electrode assembly inside a case, an electrolyte was injected into the case to manufacture a lithium secondary battery.

[0180] <Experimental Example>

[0181] Cell resistance evaluation and lifespan evaluation

[0182] The internal resistance of the manufactured batteries was evaluated and is listed in Table 2 below. The 1st and 2nd cycles were charged and discharged at 0.1C, and the 3rd and 4th cycles were charged and discharged at 0.33C. Subsequently, based on the discharge capacity of the 4th cycle, the batteries were partially charged to SOC 50%, and then a discharge current of 2.5C was applied. The internal resistance of the batteries was calculated through the voltage change (HPPC test).

[0183] In addition, the battery life performance of the manufactured batteries was evaluated and is listed in Table 2 below. Each battery is 45 o Charge and discharge were performed at a charging rate of 3.0C and a discharge rate of 0.5C.

[0184] Table 2 below describes a comparison of the internal resistances of the batteries in Examples 1 to 6 and Comparative Examples 1 to 4. This describes the internal resistances of the batteries in Comparative Examples 1 to 4 relatively when the internal resistance of the battery in Example 1 is set to 1.0.

[0185] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Battery internal resistance 1.00 0.99 0.98 0.98 0.96 0.99 1.07 1.03 1.17 1.01 Lifespan (300 cycles @ 45℃, %) 96.1 96.2 96.1 96.3 96.5 96.0 94.6 94.8 93.9 95.5

[0186] In the case of Examples 1 to 6 according to the present application, the average particle size of the silicon-based active material and the graphite-based active material (artificial graphite) is limited to the range of the present application. In the case of the silicon-based active material, the particle size is smaller than that of the graphite-based active material. It can be seen that when a negative electrode slurry is mixed and an electrode is coated in a state where there is a difference in particle size, the phenomenon in which the silicon-based active material, which has a smaller particle size compared to the graphite-based active material, forms local clusters is controlled. Furthermore, in the case of natural graphite and artificial graphite within the graphite-based active material, the average particle size is controlled as in Examples 1 to 6. Through such control, the active material within the electrode is evenly dispersed, thereby preventing local stress generation, reaction acceleration, and degradation during the operation of the battery, and it was found that a uniformly dispersed electrode can be manufactured.

[0187] Specifically, in the case of Example 2, the absolute difference (%) in the average particle size between artificial graphite and natural graphite was reduced compared to Example 1, and in the case of Example 3, the absolute difference (%) in the average particle size between silicon-based active material and artificial graphite was reduced compared to Example 1, and in the case of Example 4, both cases were reduced compared to Example 1. In such cases, when comparing the examples, the smaller the difference in absolute value, the less the increase in internal resistance and the more the lifespan tends to increase.

[0188] Likewise, Examples 5 and 6 partially modified the average particle size of the silicon-based active material and graphite (synthetic graphite, natural graphite), and it can be confirmed that the effect is superior compared to the comparative example when the absolute value of the difference in average particle size of the present invention is satisfied.

[0189] Comparative Examples 1 and 4 correspond to cases where the difference in the average particle size (D50) between the silicon-based active material and the graphite (artificial graphite) is 40% or more, and Comparative Examples 2 and 3 correspond to cases where the difference in the average particle size (D50) between natural graphite and artificial graphite is 10% or more in absolute value.

[0190] Specifically, Comparative Examples 1 and 4 are cases where the difference in average particle size between silicon and graphite exceeds the scope of the present application. In this case, silicon-based active materials with relatively small particle sizes form clusters within the graphite, and local non-uniformity occurs. Subsequently, when charging and discharging are repeated, a significant change in the volume of the clustered silicon-based active materials occurs, leading to an increase in internal resistance and a decrease in lifespan.

[0191] In the case of Comparative Examples 2 and 3, not only is the difference in average particle size between the silicon-based active material and artificial graphite large, but the difference in average particle size (D50) between natural graphite and artificial graphite is also more than 10%, which is a case where the difference in particle size of each active material is larger compared to Comparative Examples 1 and 4. This is a case where non-uniform dispersion occurs between natural graphite and artificial graphite in addition to the non-uniformity of the silicon-based active material that occurred in Comparative Examples 1 and 4, and it was confirmed that each active material forms a cluster, resulting in relatively high internal battery resistance and degraded lifespan.

[0192] Ultimately, it was confirmed that the active material within the electrode was not evenly dispersed, and consequently, the resistance inside the battery increased. This was confirmed again in a high-speed charging cycle performed at 45°C, and it was confirmed that the example meeting the above conditions exhibited superior lifespan performance compared to Comparative Examples 1 to 4. Explanation of the symbols

[0193] 10: Cathode current collector layer 20: Cathode active material layer 30: Separator 40: Positive active material layer 50: Positive current collector layer 100: Negative electrode for lithium secondary battery 200: Cathode for lithium secondary batteries

Claims

Claim 1 A negative electrode active material comprising a silicon-based active material; and graphite, wherein the graphite comprises natural graphite and artificial graphite, wherein the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite is an absolute value of 10% or less, and the ratio of the difference in average particle size (D50) between the artificial graphite and the silicon-based active material is an absolute value of 40% or less, wherein the average particle size (D50) of the artificial graphite is larger than the average particle size (D50) of the natural graphite, and the average particle size (D50) of the natural graphite is larger than the average particle size (D50) of the silicon-based active material. Claim 2 delete Claim 3 delete Claim 4 A negative electrode active material according to claim 1, wherein the weight ratio of the silicon-based active material to graphite is 5:95 to 40:60 based on 100 parts by weight of the negative electrode active material. Claim 5 A negative electrode active material according to claim 1, wherein the weight ratio of the artificial graphite to the natural graphite is 60:40 to 80:20 based on 100 parts by weight of the graphite. Claim 6 In claim 1, the silicon-based active material is Si, SiOx (0 <x<2), Si / C, 및 Si 합금으로 이루어진 군에서 선택되는 1 이상을 포함하는 것인 음극 활물질. Claim 7 A negative electrode active material according to claim 1, wherein the ratio of the difference in average particle size (D50) between the artificial graphite and the natural graphite is an absolute value of 1% or more and 10% or less. Claim 8 A negative electrode active material according to claim 1, wherein the ratio of the difference in average particle size (D50) with respect to the artificial graphite and the silicon-based active material is an absolute value of 20% or more and 40% or less. Claim 9 delete Claim 10 A negative electrode for a lithium secondary battery comprising: a negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, wherein the negative electrode active material layer comprises a negative electrode active material according to any one of claims 1 and 4 to 8. Claim 11 A negative electrode for a lithium secondary battery according to claim 10, wherein the thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, and the thickness of the negative electrode active material layer is 5 μm or more and 500 μm or less. Claim 12 A negative electrode for a lithium secondary battery according to claim 10, wherein the negative electrode active material layer further comprises a negative electrode conductive material; and a negative electrode binder. Claim 13 A negative electrode for a lithium secondary battery according to claim 10, wherein the negative electrode active material comprises 90 parts by weight or more based on 100 parts by weight of the composition included in the negative electrode active material layer. Claim 14 A negative electrode for a lithium secondary battery according to claim 12, wherein the negative electrode conductive material is 0.1 parts by weight or more and 5 parts by weight or less based on 100 parts by weight of the composition included in the negative electrode active material layer, and the negative electrode binder is 1 part by weight or more and 10 parts by weight or less based on 100 parts by weight of the composition included in the negative electrode active material layer. Claim 15 A lithium secondary battery comprising: a positive electrode; a negative electrode for a lithium secondary battery according to claim 10; a separator provided between the positive electrode and the negative electrode; and an electrolyte.

Citation Information

Patent Citations

  • Composite graphite material and preparation method thereof and lithium-ion battery comprising composite graphite material

    CN106654235A

  • Porous silicon based anode active material and lithium secondary battery comprising the same

    KR1020150032015A