Semiconductor circuit manufacturing method

A single-step chemical mechanical polishing process using a viscoelastic polymer and colloidal silica slurry addresses the challenges of planarization in semiconductor circuits, simplifying the process and improving reliability and signal transmission while reducing environmental impact.

KR103043038B1Active Publication Date: 2026-11-06KOREA ADVANCED INST OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020230139596
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-18
Publication Date
2026-11-06
Estimated Expiration
2043-10-18

AI Technical Summary

Technical Problem

Conventional chemical mechanical polishing processes for semiconductor circuits face challenges in efficiently flattening fine patterns due to material differences, leading to complex processes, long times, environmental pollution, and reduced productivity.

Method used

A method involving a pattern forming step with a protruding polishing region, an insulating layer forming step with a microchannel, and a single-step chemical mechanical polishing process using a viscoelastic polymer and colloidal silica slurry, which self-regulates pressure and slurry flow to achieve planarization without toxic chemicals.

Benefits of technology

The method simplifies the process, achieves high planarization in a single step, reduces environmental impact, and enhances bonding reliability and signal transmission, while maintaining nanometer-level surface smoothness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023114338683-PAT00001_ABST
    Figure 112023114338683-PAT00001_ABST
Patent Text Reader

Abstract

A method for manufacturing a semiconductor circuit is disclosed. According to one aspect of the present invention, the method for manufacturing a semiconductor circuit comprises a pattern forming step of forming a conductive pattern protruding on a substrate, an insulating layer forming step of forming an insulating layer on a substrate, and a polishing step of polishing the pattern and the insulating layer to flatten them by a chemical mechanical polishing process. In the pattern forming step, the pattern is formed on a substrate and comprises a circuit area that becomes a semiconductor circuit and a polishing area formed on the circuit area and removed in the polishing step. The height of the polishing area may be set so as to protrude higher than the insulating layer after the insulating layer forming step.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a semiconductor circuit. More specifically, it relates to a method for manufacturing a semiconductor circuit using a chemical mechanical polishing process. Background Technology

[0003] For the miniaturization and 3D stacking of semiconductor transistors, it is important to ensure that there are no steps on the surface. If defects or differences in height within the area exist on the bonded surface, the circuits cannot be connected smoothly, which can consequently lead to a deterioration in bonding reliability.

[0004] In other words, the technology for smoothing the surface determines the structure and performance of semiconductors. Therefore, the Chemical Mechanical Polishing (CMP) process, which can reduce surface step height and mitigate surface roughness in semiconductor manufacturing, is becoming increasingly important and is steadily gaining weight in the overall device manufacturing process.

[0005] The chemical mechanical polishing process has difficulty flattening fine patterns due to the different mechanical properties of the circuit and the insulating layer.

[0006] In conventional chemical mechanical polishing processes, toxic chemical solutions were added to the polishing process or the process was performed in complex multiple stages to address the problem of selective polishing of two or more materials exposed on the surface. Consequently, the long process time resulted in reduced productivity and generated a large amount of wastewater, posing a significant problem of environmental pollution.

[0007] Therefore, a chemical mechanical polishing process is required to simplify complex processes and achieve planarization by controlling the material removal rate of areas that are difficult to polish. The problem to be solved

[0009] An embodiment of the present invention is intended to provide a method for manufacturing a semiconductor circuit using a chemical mechanical polishing process that simplifies the process and provides high planarization. means of solving the problem

[0011] According to one aspect of the present invention, a method for manufacturing a semiconductor circuit is provided, comprising a pattern forming step of forming a conductive pattern protruding from a substrate, an insulating layer forming step of forming an insulating layer on a substrate, and a polishing step of polishing the pattern and the insulating layer to flatten them by a chemical mechanical polishing process, wherein in the pattern forming step, the pattern is formed on the substrate and comprises a circuit region that becomes a semiconductor circuit and a polishing region formed on the circuit region and removed in the polishing step, and the height of the polishing region is set so as to protrude higher than the insulating layer after the insulating layer forming step.

[0012] At this time, in the polishing step, the chemical mechanical polishing process can be performed once.

[0013] At this time, in the polishing step, the pressure applied to the polishing area of ​​the pattern may decrease over time.

[0014] Meanwhile, in the pattern forming step, a plurality of patterns are formed on the substrate, and in the insulating layer forming step, the insulating layer is formed concavely so that a microchannel is formed between the plurality of patterns, and in the polishing step, a slurry can flow into the microchannel.

[0015] At this time, in the pattern formation step, the pattern can be formed by laminating a metal material onto the substrate.

[0016] Meanwhile, in the above step of forming the insulating layer, the insulating layer may include a viscoelastic polymer.

[0017] At this time, in the step of forming the insulating layer, the insulating layer can be formed by spin-coating the viscoelastic polymer.

[0018] In addition, in the step of forming the insulating layer, the thickness of the insulating layer formed on the substrate can be controlled by adjusting at least one of the solvent concentration and the spin rotation speed of the viscoelastic polymer in the spin coating.

[0019] In the above polishing step, a slurry containing distilled water and colloidal silica may be used. Effects of the invention

[0021] According to an embodiment of the present invention, since the pressure applied to the pattern and the flow of the slurry flowing into the microchannel decrease as the process progresses, the pressure and the flow of the slurry are self-regulated rather than being artificially changed, so that the chemical mechanical polishing process can be performed in one step.

[0022] In addition, sufficient effectiveness can be achieved in the chemical mechanical polishing process without using toxic chemicals in the slurry. Brief explanation of the drawing

[0024] FIG. 1 is a flowchart of a semiconductor circuit manufacturing method according to one embodiment of the present invention. FIGS. 2 to 6 are drawings illustrating a method for manufacturing a semiconductor circuit according to an embodiment of the present invention. FIG. 7 is a drawing illustrating the shape of an insulating layer in a semiconductor circuit manufacturing method according to one embodiment of the present invention. FIGS. 8 and 9 are drawings illustrating the control of the thickness of an insulating layer formed by spin coating in a semiconductor circuit manufacturing method according to an embodiment of the present invention. FIG. 10 is a diagram illustrating the removal rate in a chemical mechanical polishing process in a semiconductor circuit manufacturing method according to one embodiment of the present invention. FIGS. 11 to 13 are drawings showing pressure changes in the chemical mechanical polishing process of a semiconductor circuit manufacturing method according to one embodiment of the present invention. FIG. 14 is a diagram illustrating a change in the depth of a microchannel in a chemical mechanical polishing process in a semiconductor circuit manufacturing method according to one embodiment of the present invention. Specific details for implementing the invention

[0025] The terms used in this application are used merely to describe specific embodiments and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.

[0026] In this application, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. Furthermore, throughout the specification, "on" means located above or below the subject part, and does not necessarily mean located on the upper side with respect to the direction of gravity.

[0027] In addition, regarding the contact relationship between each component, the term "combination" is used not only to mean cases where each component is in direct physical contact with each other, but also to encompass cases where another component is interposed between each component and each component is in contact with that other component.

[0028] Additionally, terms such as "first," "second," etc., may be used to describe various components, but said components should not be limited by said terms. These terms are used solely for the purpose of distinguishing one component from another.

[0029] The size and thickness of each component shown in the drawings are depicted arbitrarily for convenience of explanation, and therefore the present invention is not necessarily limited to what is illustrated.

[0030] Hereinafter, embodiments of the semiconductor circuit manufacturing method according to the present invention will be described in detail with reference to the accompanying drawings. In describing with reference to the accompanying drawings, identical or corresponding components are given the same reference numerals, and redundant descriptions thereof will be omitted.

[0031] FIG. 1 is a flowchart of a semiconductor circuit manufacturing method according to one embodiment of the present invention, and FIGS. 2 to 6 are drawings showing a semiconductor circuit manufacturing method according to one embodiment of the present invention.

[0032] Referring to FIGS. 1 to 6, a semiconductor circuit manufacturing method according to one embodiment of the present invention includes a pattern forming step (S110), an insulating layer forming step (S120), and a polishing step (S130).

[0033] In the pattern formation step (S110), a conductive pattern (120) protruding from the substrate (110) is formed.

[0034] Referring to FIG. 2, in the pattern formation step (S110) of the present embodiment, a silicon wafer is used as a substrate (110), and a conductive pattern (120) can be formed on the silicon wafer using various pattern (120) formation methods. For example, a metal material such as copper can be laminated on the substrate (110) to form a pattern (120) with a structure protruding from the substrate (110).

[0035] At this time, the pattern (120) formed on the substrate (110) may have a circuit area (122) that becomes a semiconductor circuit and a polishing area (124) that is removed in the polishing step (S130). The circuit area (122) is formed on the substrate (110), and the polishing area (124) may be formed integrally with the circuit area (122) on the circuit area (122). Accordingly, when the polishing area (124) is removed in the polishing step (S130) to be described later, the circuit area (122) remains on the substrate (110) and can become a semiconductor circuit.

[0036] Additionally, a plurality of patterns (120) may be formed on the substrate (110). The plurality of patterns (120) may have circuit areas (122) of the same height, and polishing areas (124) may be formed on each circuit area (122).

[0038] In the insulating layer formation step (S120), an insulating layer (120) is formed on the substrate (110).

[0039] In the insulating layer formation step (S120) of the present embodiment, the insulating layer (120) may include a viscoelastic polymer. In conventional semiconductor devices, silica (SiO2) was mainly used as the insulating layer (120), but silica exhibits low bonding strength and is susceptible to contamination or defects, making the process difficult, and the high diffusion rate of copper causes reliability problems.

[0040] In the insulating layer formation step (S120) of this embodiment, a viscoelastic polymer is utilized to enhance bonding reliability and prevent copper diffusion, and also offers advantages for high-speed signal transmission due to its low dielectric constant (Low-K) characteristics. Furthermore, since the properties of the polymer are easy to control, it can provide mechanical properties and bonding characteristics suitable for bonding conditions.

[0041] Referring to FIG. 3, after the insulating layer formation step (S120), the polishing area (124) of the pattern (120) may protrude higher than the insulating layer (120). To this end, in the pattern formation step (S110), the height of the polishing area (124) may be set so as to protrude higher than the insulating layer (120), taking into account the thickness of the insulating layer (120) to be formed later.

[0042] Meanwhile, in the insulating layer formation step (S120), the thickness of the insulating layer (120) is adjusted so that the polished area (124) of the pattern (120) can protrude higher than the insulating layer (120).

[0043] Additionally, in the insulating layer formation step (S120), the insulating layer (120) may be formed concavely so that a microchannel (132) is formed between a plurality of patterns (120). When the insulating layer (120) is formed with a uniform thickness on the substrate (110), a microchannel (132) may be formed in a concave structure between the protruding plurality of patterns (120).

[0044] At this time, the starting point (lowest) height of the polishing area (124) can be formed lower than the bottom of the micro channel (132). Accordingly, when the polishing of the polishing area (124) is almost complete in the polishing step (S130) to be described later, and the micro channel (132) is also almost eliminated, the bottom of the polishing area (124) and the micro channel (132) can be polished together.

[0045] FIG. 7 is a drawing illustrating the shape of an insulating layer (120) in a semiconductor circuit manufacturing method according to one embodiment of the present invention.

[0046] Referring to FIG. 7, the depth and shape of the microchannel (132) can be controlled by adjusting the formation conditions of the insulating layer (120).

[0047] For example, the insulating layer (120) of the present embodiment can be formed by spin-coating a viscoelastic polymer onto a silicon wafer, which is the substrate (110). At this time, in the spin coating, the thickness of the insulating layer (120) formed on the substrate (110) can be controlled by adjusting at least one of the solvent concentration of the viscoelastic polymer and the spin rotation speed of the substrate (110). The depth or shape of the microchannel (132) can be controlled according to the thickness of the insulating layer (120) formed on the substrate (110).

[0048] FIGS. 8 and 9 are drawings illustrating the control of the thickness of an insulating layer (120) formed by spin coating in a semiconductor circuit manufacturing method according to one embodiment of the present invention. FIG. 8 shows the result of performing spin coating by using mesitylene as a solvent and mixing it with a polymer, BCB (Benzocyclobutene) (the mixing ratio is indicated as the BCB:mesitylene ratio).

[0049] Referring to FIG. 8, when spin-coating a viscoelastic polymer onto a wafer, the thickness of the insulating layer (120) formed on the substrate (110) can be controlled by adjusting the solvent concentration of the viscoelastic polymer. It can be seen that the higher the ratio of the solvent, the thinner the thickness of the insulating layer (120) is formed.

[0050] Additionally, referring to FIG. 9, when spin-coating a viscoelastic polymer, the thickness of the insulating layer (120) formed on the substrate (110) can be controlled by adjusting the rotational speed of the rotating substrate (110). It can be confirmed that as the rotational speed increases in spin-coating, the thickness of the insulating layer (120) is formed thinner.

[0052] In the polishing step (S130), the pattern (120) and the insulating layer (120) can be polished and flattened using a chemical mechanical polishing process.

[0053] The chemical mechanical polishing process is a process that performs planarization by simultaneously utilizing chemical reactions and mechanical forces. In the chemical mechanical polishing process, in addition to mechanical elements such as the rotational speed of the polishing pad (200) and the wafer (substrate (110)), the applied pressure, and the orientation of the pattern (120), chemical elements such as the interaction between the slurry (300) and the wafer surface and the role of additives also act as polishing variables.

[0054] In particular, in the polishing step (S130) of the present embodiment, the chemical mechanical polishing process can be performed once due to the structure of the unique pattern (120) and the insulating layer (120) formed in the pattern forming step (S110) and the insulating layer forming step (S120) described above.

[0055] Generally, in chemical mechanical polishing processes, the circuit and insulating layer on the surface are composed of different materials, so the process is performed in a complex manner with multiple stages to improve the problem of selective polishing. In particular, when a polymer is used as the insulating layer (120) as in this embodiment, more polishing is performed because the polymer is a softer material than the circuit. Consequently, step differences or large grooves may occur between the circuits, which can lead to dishing and erosion problems.

[0056] In the polishing step (S130) of the present embodiment, the polishing area (124) of the pattern (120) protrudes higher than the insulating layer (120), so that the pressure applied to the polishing area (124) of the pattern (120) is initially applied strongly but decreases over time.

[0057] FIG. 10 is a diagram illustrating the removal rate in a chemical mechanical polishing process in a semiconductor circuit manufacturing method according to one embodiment of the present invention, and FIGS. 11 to 13 are diagrams conceptually illustrating pressure changes in a chemical mechanical polishing process in a semiconductor circuit manufacturing method according to one embodiment of the present invention. In FIGS. 11 to 13, the size of the arrow indicates the magnitude of the pressure.

[0058] Referring to FIGS. 10 and FIGS. 11, in the chemical mechanical polishing process of the present embodiment, it can be seen that the polishing of the pattern (120) proceeds intensively by applying strong pressure to the pattern (120) while the pattern (120) protrudes above the insulating layer (120).

[0059] Referring to FIGS. 10 and FIGS. 12, it can be seen that as the protrusion of the pattern (120) decreases as the chemical mechanical polishing process proceeds, the pressure applied to the pattern (120) decreases, and thus the polishing of the pattern (120) decreases.

[0060] Additionally, referring to FIG. 13, when the chemical mechanical polishing process is carried out and the height of the pattern (120) and the insulating layer (120) become similar in the latter part of the process, the effect of the pattern (120) and the insulating layer (120) being polished evenly together can be confirmed.

[0062] Meanwhile, in the polishing step (S130) of the present embodiment, the slurry (300) used in the chemical mechanical polishing process can flow into the microchannel (132). In the present embodiment, since the microchannel (132) is formed with a concave structure between a plurality of protruding patterns (120), the slurry (300) used in the chemical mechanical polishing process can be moved through the microchannel (132).

[0063] Referring to FIGS. 4 to 6, in the chemical mechanical polishing process of the present embodiment, the microchannels (132) between the patterns (120) allow the slurry (300) to spread evenly over the wafer (substrate, 110), thereby inducing uniform polishing of the patterns (120). As polishing proceeds, the depth of the microchannels (132) naturally decreases, so the amount of slurry (300) flowing in can also be reduced.

[0064] FIG. 14 is a diagram illustrating a change in the depth of a microchannel in a chemical mechanical polishing process in a semiconductor circuit manufacturing method according to one embodiment of the present invention.

[0065] Referring to FIG. 14, as the chemical mechanical polishing process proceeds, the pattern (120) is polished more intensively than the insulating layer (120), so the polishing of the pattern (120) proceeds rapidly, and as a result, the depth of the microchannel (132) is reduced. When the depth of the microchannel (132) is reduced, the flow of the slurry (300) through the microchannel (132) is reduced, and thus the polishing of the pattern (120) can be reduced. Accordingly, when the chemical mechanical polishing process reaches the later stages, the step difference between the pattern (120) and the insulating layer (120) becomes at a nanometer level similar to the surface roughness, and the effect of evenly polishing the pattern (120) and the insulating layer (120) can be confirmed.

[0066] Accordingly, in the chemical mechanical polishing process of the present embodiment, since the pressure applied to the pattern (120) and the flow of the slurry (300) flowing into the microchannel (132) decrease as the process progresses, the pressure and the flow of the slurry (300) are not artificially changed, but rather the pressure and the flow of the slurry (300) can be self-regulated. Accordingly, the chemical mechanical polishing process can be performed in a single step.

[0067] In addition, even if toxic chemicals are not used in the slurry (300) and the slurry (300) contains distilled water and colloidal silica, the chemical mechanical polishing process of this embodiment can have a sufficient polishing effect.

[0069] Although preferred embodiments of the present invention have been described above, those skilled in the art may modify and change the present invention in various ways by adding, changing, deleting, or adding components without departing from the spirit of the invention as described in the claims, and such modifications and changes are also to be included within the scope of the rights of the present invention. Explanation of the symbols

[0071] 110: Substrate 120: Pattern 122: Circuit area 124: Grinding area 120: Insulating layer 200: Grinding pad 300: Slurry

Claims

Claim 1 A method for manufacturing a semiconductor circuit comprising: a pattern forming step for forming a conductive pattern protruding on a substrate; an insulating layer forming step for forming an insulating layer on the substrate; and a polishing step for polishing the pattern and the insulating layer to flatten them using a chemical mechanical polishing process, wherein in the pattern forming step, the pattern comprises a circuit area formed on the substrate and becoming a semiconductor circuit, and a polishing area formed on the circuit area and removed in the polishing step, wherein the height of the polishing area is set so as to protrude higher than the insulating layer after the insulating layer forming step, wherein in the pattern forming step, a plurality of patterns are formed on the substrate, and in the insulating layer forming step, the insulating layer is formed concavely so as to form a microchannel between the plurality of patterns, and in the polishing step, a slurry flows into the microchannel, and as the polishing process proceeds, the amount of slurry flowing into the microchannel is reduced, thereby enabling self-regulation of flow in which the flow of slurry in the microchannel decreases as the polishing process progresses. Claim 2 A semiconductor circuit manufacturing method according to claim 1, characterized in that, in the polishing step, the chemical mechanical polishing process is performed once. Claim 3 A semiconductor circuit manufacturing method according to paragraph 2, wherein in the polishing step, the pressure applied to the polishing area of ​​the pattern decreases over time. Claim 4 delete Claim 5 A semiconductor circuit manufacturing method according to claim 1, wherein in the pattern forming step, a metal material is laminated onto the substrate to form the pattern. Claim 6 A semiconductor circuit manufacturing method according to claim 1, wherein in the step of forming the insulating layer, the insulating layer comprises a viscoelastic polymer. Claim 7 A semiconductor circuit manufacturing method according to claim 6, wherein in the step of forming the insulating layer, the insulating layer is formed by spin-coating the viscoelastic polymer. Claim 8 A semiconductor circuit manufacturing method according to claim 7, wherein in the insulating layer forming step, at least one of the solvent concentration and spin rotation speed of the viscoelastic polymer in the spin coating is controlled to control the thickness of the insulating layer formed on the substrate. Claim 9 A method for manufacturing a semiconductor circuit according to claim 1, wherein in the polishing step, a slurry comprising distilled water and colloidal silica is used.

Citation Information

Patent Citations

  • A method of manufacturing semiconductor apparatus and a mehtod of flattening

    KR100153787B1

  • Semiconductor device manufacturing method

    KR100484607B1

  • Reactive aqueous metal oxide sols as polishingslurries for low dielectric constant materials

    US20030005647A1