Sulfide-based solid electrolyte used in lithium-ion secondary batteries, method of manufacturing the same, and lithium-ion secondary batteries
By integrating an oxide anion with a Q0 structure into the agirodite-type crystal, the stability of sulfide-based solid electrolytes is maintained during high-temperature treatment, improving lithium ion conductivity and reducing grain boundary resistance in lithium-ion secondary batteries.
Patent Information
- Application Number
- KR1020237000343
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-21
- Filing Date
- 2021-07-07
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2041-07-07
AI Technical Summary
Sulfide-based solid electrolytes decompose during high-temperature heat treatment, reducing lithium ion conductivity and limiting the effectiveness of grain boundary resistance reduction.
Incorporating an oxide anion with a Q0 structure into the agirodite-type crystal structure, specifically formed by an MO bond, to stabilize the crystal during high-temperature heat treatment, thereby maintaining lithium ion conductivity.
The stabilized agirodite-type crystal allows for effective reduction of grain boundary resistance and improved lithium ion conductivity, enhancing the performance of lithium-ion secondary batteries.
Smart Images

Figure 112023001159779-PCT00001 
Figure 112023001159779-PCT00002 
Figure 112023001159779-PCT00003
Abstract
Description
Technology Field
[0001] The present invention relates to a sulfide-based solid electrolyte used in a lithium-ion secondary battery, a method for manufacturing the same, and a lithium-ion secondary battery. Background Technology
[0002] Lithium-ion secondary batteries are widely used in portable electronic devices such as mobile phones and notebook personal computers.
[0003] Conventionally, liquid electrolytes have been used in lithium-ion secondary batteries, but there were concerns about leakage or ignition, so it was necessary to enlarge the case for safety design. In addition, improvements were desired regarding the short battery life and narrow operating temperature range.
[0004] In contrast, all-solid-state lithium-ion secondary batteries that use a solid electrolyte as the electrolyte are attracting attention due to the potential for improved safety, high-speed charging and discharging, and miniaturization of the case.
[0005] Solid electrolytes are broadly classified into sulfide-based and oxide-based solid electrolytes; however, sulfide ions exhibit a higher polarization rate and higher ionic conductivity compared to oxide ions. As a sulfide-based solid electrolyte, Li 10 GeP2S 12 LGPS-type crystals such as Li6PS5Cl, agirodite-type crystals such as Li7P3S 11 LPS crystallized glass, such as crystallized glass, is known.
[0006] Patent Document 1 can be cited as an example in which an agirodite-type sulfide-based solid electrolyte is disclosed. The sulfide-based solid electrolyte disclosed in Patent Document 1 has a cubic crystal structure belonging to the space group F-43m, and composition formula: Li 7-x PS 6-x Ha xIt contains a compound represented as (Ha is Cl or Br) (x=0.2 to 1.8), and also has a lightness L value of the L*a*b* color system of 60.0 or higher. This is intended to increase charge-discharge efficiency or cycle characteristics by increasing lithium ion conductivity and lowering electron conductivity. Prior art literature
[0007] International Publication No. 2015 / 012042 The problem to be solved
[0008] However, when attempting to sinter sulfide-based solid electrolytes using agarodite-type crystals by heat treatment at high temperatures to reduce inter-particle resistance known as grain boundary resistance, the lithium ion conductivity actually decreases due to thermal decomposition. Specifically, for example, in the case of Li6PS5Cl, it decomposes into Li3PS4+Li2S+LiCl. Therefore, there was a limit to heat treatment at high temperatures to reduce grain boundary resistance.
[0009] Therefore, the present invention aims to provide an agirodite-type sulfide-based solid electrolyte that can exist stably without decomposing even by heat treatment at high temperatures, and a method for manufacturing the same. means of solving the problem
[0010] The inventors, after repeated examinations, discovered that the above problem could be solved by having an oxide anion of a specific structure present in an agirodite-type crystal structure, and thus completed the present invention.
[0011] That is, the present invention relates to the following [1] to
[17] .
[0012] [1] As a sulfide-based solid electrolyte used in lithium-ion secondary batteries,
[0013] It comprises a crystalline phase and an anion existing in the crystal structure of the crystalline phase, and
[0014] The above crystal phase includes an agarhodite-type crystal containing Li, P, S and Ha, and
[0015] The above Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and
[0016] The above anion includes an oxide anion of a Q0 structure having an MO bond formed by the combination of M and O, and
[0017] The above M is a sulfide-based solid electrolyte, wherein M is at least one element selected from the group consisting of metallic elements and metalloid elements of groups 2 to 14 of the periodic table.
[0018] [2] A sulfide-based solid electrolyte described in [1] above, in which the content (at%) of each element satisfies the relationship {(M+O) / (Li+P+S+Ha+M+O)}≤0.2.
[0019] [3] The ratio of the content of elements (at%) included in the above agirodite-type crystals is Li a -PS b -Ha c When represented as, 5 <a<7, 4<b<6 또한 0<c<2의 관계를 만족시키는, 상기 [1] 또는 [2]에 기재된 황화물계 고체 전해질.
[0020] [4] A sulfide-based solid electrolyte described in any one of [1] to [3], wherein the total content of the elements Li, P, S, Ha, M and O is 90 mass% or more.
[0021] [5] A sulfide-based solid electrolyte described in any one of [1] to [4], wherein the M constituting the oxide anion comprises at least one element selected from the group consisting of Si, Al, Zr and B.
[0022] [6] A sulfide-based solid electrolyte described in any one of [1] to [5] above, satisfying the following relationship when using the content (at%) of each element as α=(Li+P+S+Ha), β=(Si+Al+Zr+B+O), and γ=(Ha / P).
[0023] 0<{β / (α+β)}<(D+0.1)
[0024] D=(0.1104×γ-0.1133)
[0025] [7] A sulfide-based solid electrolyte described in any one of [1] to [6], wherein the above Ha contains Cl and Br, and if the content of Cl in the above agirodite-type crystal is x (at%) and the content of Br is y (at%), then (x / y) is 0.1 or more and 10 or less.
[0026] [8] The above Ha contains Cl and Br, and the ratio of the content (at%) of the elements included in the above agirodite-type crystal is Li a -PS b -Cl c1 -Br c2 A sulfide-based solid electrolyte described in any one of [1] to [7], wherein c1 is 0.1 or more and c2 is 0.1 or more and 1.9 or less when expressed as such.
[0027] [9] The above agirodite-type crystal contains at least one element selected from the group consisting of Na, K, Mg and Ca represented by R, and the ratio of the content (at%) of the element included in the above agirodite-type crystal is Li a1 -R a2 -PS b -Ha c A sulfide-based solid electrolyte described in any one of [1] to [8], wherein a2 is 0.001 to 0.4 when expressed as such.
[0028]
[10] A sulfide-based solid electrolyte described in any one of [1] to [9], which has a capacity retention rate of 80% or more when a full-solid-state lithium-ion secondary battery is manufactured by the following method and a charge / discharge test is performed.
[0029] (method)
[0030] (Production of the positive pole composite material)
[0031] As a positive electrode active material, layered rock salt type LiCoO2 powder (volume average particle size: 10 μm) coated with LiNbO3 with a thickness of 7 nm is used to produce a positive electrode composite material by mixing 35 parts of the sulfide-based solid electrolyte, 60 parts of the positive electrode active material, and 5 parts of a conductivity aid (acetylene black, manufactured by Denka Co., Ltd., HS100). The thickness of the LiNbO3 coating is determined by transmission electron microscopy (TEM) observation.
[0032] (Fabrication of all-solid-state lithium-ion secondary batteries)
[0033] 80 mg of the above sulfide-based solid electrolyte is poured into a plastic cylinder with a diameter of 10 mm and pressure-molded to form a solid electrolyte layer. Subsequently, 10 mg of the above positive electrode composite is poured into the cylinder and pressure-molded again to form a positive electrode layer. In addition, indium foil and lithium foil are poured from the opposite side to the above positive electrode composite to form a negative electrode layer. In this way, an all-solid-state lithium-ion secondary battery is manufactured, and a charge-discharge test is performed at a confining pressure of 10 kN.
[0034] (Charge / Discharge Test)
[0035] Using the above-described all-solid-state lithium-ion secondary battery, a constant current charge-discharge test is performed for 100 cycles at 25°C with a charge-discharge current density of 0.1C and a charge-discharge potential range of 1.9-3.7V. From the results of the charge-discharge test, a capacity retention rate (%) expressed by the following formula is calculated.
[0036] Capacity retention rate (%) = (Discharge capacity at 100th cycle / Discharge capacity at 1st cycle) × 100
[0037]
[11] A sulfide-based solid electrolyte described in any one of [1] to
[10] , wherein when a lithium-ion secondary battery comprising a solid electrolyte layer containing the above sulfide-based solid electrolyte is charged and discharged, an oxide layer is formed at the interface between the solid electrolyte layer and the positive electrode layer.
[0038]
[12] A lithium-ion secondary battery comprising a sulfide-based solid electrolyte as described in any one of [1] to
[11] above.
[0039]
[13] A method for manufacturing a sulfide-based solid electrolyte used in lithium-ion secondary batteries,
[0040] Mixing raw materials containing Li, P, S and Ha and crystallizing by heating to obtain agirodite-type crystals,
[0041] Obtaining a mixture by mixing an oxide having an MO bond formed by the combination of M and O with the above agirodite-type crystal, and
[0042] The method comprises performing heat treatment of the above mixture to obtain an agirodite-type crystal in which an oxide anion of a Q0 structure having an MO bond exists within the crystal structure, and
[0043] The above Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and
[0044] The above M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table, and
[0045] A method for preparing a sulfide-based solid electrolyte comprising an agarodite-type crystal having an oxide anion of a Q0 structure with an MO bond in the crystal structure.
[0046]
[14] A method for manufacturing a sulfide-based solid electrolyte used in lithium-ion secondary batteries,
[0047] A raw material composition obtained by mixing raw materials including Li, P, S, and Ha with an oxide having an MO bond formed by the combination of M and O, and
[0048] The method comprises performing heat treatment on the above raw material composition to obtain an agirodite-type crystal in which an oxide anion of a Q0 structure having an MO bond exists within the crystal structure, and
[0049] The above Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and
[0050] The above M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table, and
[0051] A method for preparing a sulfide-based solid electrolyte comprising an agarodite-type crystal having an oxide anion of a Q0 structure with an MO bond in the crystal structure.
[0052]
[15] A method for manufacturing a sulfide-based solid electrolyte used in lithium-ion secondary batteries,
[0053] Reacting raw materials containing Li, P, S and Ha to obtain an intermediate product,
[0054] Obtaining a mixture by mixing an oxide having an MO bond formed by the combination of M and O with the above intermediate product, and
[0055] The method comprises performing heat treatment of the above mixture to obtain an agirodite-type crystal in which an oxide anion of a Q0 structure having an MO bond exists within the crystal structure, and
[0056] The above Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and
[0057] The above M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table, and
[0058] A method for preparing a sulfide-based solid electrolyte comprising an agarodite-type crystal having an oxide anion of a Q0 structure with an MO bond in the crystal structure.
[0059]
[16] A method for manufacturing a sulfide-based solid electrolyte used in lithium-ion secondary batteries,
[0060] Mixing raw materials containing Li, P, S and Ha and crystallizing by heating to obtain agirodite-type crystals,
[0061] Obtaining a composition comprising an oxide anion of a Q0 structure having an MO bond formed by the combination of M and O,
[0062] Obtaining a mixture by mixing the above agirodite-type crystal and the above composition, and
[0063] The method comprises performing heat treatment of the above mixture to obtain an agirodite-type crystal in which an oxide anion of a Q0 structure having an MO bond exists within the crystal structure, and
[0064] The above Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and
[0065] The above M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table, and
[0066] A method for preparing a sulfide-based solid electrolyte comprising an agarodite-type crystal having an oxide anion of a Q0 structure with an MO bond in the crystal structure.
[0067]
[17] A method for manufacturing a sulfide-based solid electrolyte described in any one of
[13] to
[16] , wherein the above heat treatment is performed at a temperature of 500°C or higher. Effects of the invention
[0068] According to the sulfide-based solid electrolyte of the present invention, the grain boundary resistance can be reduced by sintering because it can exist stably without decomposing even by heat treatment at high temperatures. As a result, an improvement in lithium ion conductivity can be expected, making it very useful as a solid electrolyte for lithium-ion secondary batteries. Accordingly, the battery characteristics of lithium-ion secondary batteries are improved. Specific details for implementing the invention
[0069] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and may be implemented with arbitrary modifications within the scope that does not deviate from the gist of the present invention. Furthermore, the term "to" indicating a numerical range is used to mean including the values described before and after it as lower and upper limits.
[0070] Sulfide-based solid electrolytes
[0071] The sulfide-based solid electrolyte according to the present embodiment (hereinafter simply referred to as "solid electrolyte") is used in a lithium-ion secondary battery and comprises a crystalline phase and an anion present in the crystal structure of the crystalline phase.
[0072] The crystal phase comprises an agarodite-type crystal containing Li, P, S and Ha, and Ha is at least one element selected from the group consisting of F, Cl, Br and I.
[0073] The anion comprises an oxide anion having a Q0 structure having an MO bond formed by the combination of M and O (hereinafter simply referred to as "oxide anion" or "oxide anion having a Q0 structure"), wherein M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table.
[0074] (Oxide anion)
[0075] Since oxide anions with a Q0 structure exist in the crystal structure of the solid electrolyte, the heat resistance of the agarodite-type crystal is improved, allowing it to exist stably without decomposing even during heat treatment at high temperatures. Therefore, heat treatment that reduces grain boundary resistance can be performed while maintaining lithium ion conductivity as an electrolyte.
[0076] A Q0 structure is a structure in which all oxygen atoms bonded to the central cation M are non-bridged oxygen atoms. For example, when M is Si, the oxide that becomes SiO2 is a silicate ion, i.e., SiO4 4- It means existing as an oxide anion.
[0077] The existence of oxide anions with a Q0 structure within a crystal structure can be rephrased as being in a fixed state within the crystal structure. Specifically, this refers to cases where oxide anions with a Q0 structure become crystal nuclei to form an agirodite-type crystal phase, cases where oxide anions with a Q0 structure are introduced into an agirodite-type crystal structure, and both of these cases. This fixation of oxide anions with a Q0 structure is an inherent phenomenon observed in cases where the crystal is of the agirodite type containing at least three elements: Li, S, and Ha.
[0078] Meanwhile, a Li-P-S tricomponent crystal containing the three elements Li, P, and S and not containing Ha, e.g., Li7P3S 11 However, LGPS type determination, for example, Li 10 GeP2S 12 In cases like this, oxide anions of the Q0 structure are not well fixed within the crystal structure.
[0079] It is unclear why the presence of oxide anions with a Q0 structure allows agirodite-type crystals to exist stably without decomposing even at high temperatures. However, it is possible to consider the effect of crystallization stabilization as oxide anions with a Q0 structure act as crystal nuclei to form an agirodite-type crystal phase, or the effect of stabilization through the introduction of oxide anions with a Q0 structure into the agirodite-type crystal structure. Furthermore, it is speculated that when oxide anions with a Q0 structure acting as crystal nuclei and oxide anions with a Q0 structure introduced into the crystal structure exist together, the agirodite-type crystals can exist more stably due to the combined factors of the above effects.
[0080] For example, if the agirhodite-type crystal is Li6PS5Cl, the anion constituting Li6PS5Cl is PS4 3- It is. At this anion site, SiO4 4- It is thought that the inclusion of oxide anions with a Q0 structure, such as SiO4, strengthens electrostatic attraction and improves the heat resistance of the crystal. Additionally, lithium-ion conductive agirodite-type crystals are often high-temperature stable phases, and SiO4 4- It is speculated that a thermodynamic stabilization effect will be obtained by introducing oxide anions with a Q0 structure such as the above.
[0081] In addition, it is speculated that a small and dense crystallite may be formed by forming or reforming an agirodite-type crystal using an oxide anion of the Q0 structure as a crystal nucleus.
[0082] The elements constituting the oxide anion may include M and O, and M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table. In addition, the oxide anion may consist of only one type or may include multiple types.
[0083] Metallic elements of groups 2 to 14 are elements of groups 2 to 12 of the periodic table, elements of group 13 other than B, and elements of group 14 other than C, Si, and Ge.
[0084] The metalloid elements of groups 2 to 14 are B, Si, and Ge among the elements of groups 13 and 14 of the periodic table.
[0085] Even if an element M with a weak MO bonding strength is selected, the above effect as an oxide anion with a Q0 structure can be obtained, but there is a possibility of oxygen loss or volatilization during the heating process, or the introduction of oxygen atoms into unexpected anion sites in the crystal. Therefore, it is desirable to include an element M with an MO bonding strength of 400 kJ / mol or more, an element M with an MO bonding strength of 450 kJ / mol or more is more desirable, and an element M with an MO bonding strength of 500 kJ / mol or more is even more desirable.
[0086] In addition, regarding MO bonding strength, there is no specific upper limit, but it is generally 1000 kJ / mol or less.
[0087] For the above reasons, it is preferable that M includes at least one element selected from the group consisting of metallic elements and metalloid elements of groups 2 to 14 of the periodic table, and more preferable that it includes at least one element selected from the group consisting of Al, B, Ge, La, Ta, Nb, Ti, Si, Sn, V, Y, and Zr.
[0088] In addition, the MO bonding force in this specification refers to the bond dissociation energy, and the bond dissociation energy has a unique value for each bond. The calculation method is defined as the standard enthalpy change (ΔHf298) in the dissociation reaction MO→M+O, as ΔHf298=ΔHf298(M)+ΔHf298(O)-ΔHf298(MO).
[0089] In addition, it is desirable for oxide anions to have a wide potential window. This is because, considering their use in the solid electrolyte of lithium-ion secondary batteries, it is desirable for them to be difficult to be oxidized or reduced during the charging and discharging of lithium-ion secondary batteries.
[0090] For the reasons above, the reduction potential of M and M stably existing in M n+ Regarding ions, M n+ It is more preferable to include at least one element selected from the group of elements in which the reduction potential of / M is -0.5V (vs. SHE) or lower. In addition, from the perspective of the oxidation-reduction resistance of the oxide of M, it is even more preferable to include at least one element selected from the group consisting of Si, Al, Zr, and B.
[0091] The presence of MO bonds can be confirmed from Raman spectroscopy measurements or nuclear magnetic resonance (NMR) measurements.
[0092] In Raman spectroscopy measurements, the presence of MO coupling is 750 to 1500 cm⁻¹ -1 It is possible to confirm this as the Raman scattering spectrum. For example, Si-O bonds are at 800 to 1300 cm⁻¹. -1 , Al-O bonds are 775 to 1275 cm -1 , Zr-O bonds are 850 to 1350 cm -1 , BO bonds are 925 to 1425 cm -1 Each has a peak.
[0093] In NMR measurements, the nuclides are limited, but for example 29 In Si-NMR, the Si-O bond peak is visible in the range of -125 to -50 ppm (the reference material is tetramethylsilane). 27 In Al-NMR, the Al-O bond peak is visible in the range of 0 to 80 ppm (the reference material is aluminum chloride). 11In B-NMR, the BO bond peak is visible in the range of -10 to 20 ppm (the reference material is a boron trifluoride diethyl ether complex). Zr is 91 Although Zr-NMR exists as a radionuclide, it is not a very common analytical method at present.
[0094] The fact that the oxide anion has a Q0 structure can be confirmed by Raman spectroscopy or nuclear magnetic resonance (NMR) measurements.
[0095] In Raman spectroscopy measurements, for example, the Si-O bond of the Q0 structure is 800 to 900 cm⁻¹ -1 , Al-O bonds in the Q0 structure are 775 to 875 cm -1 , Zr-O bonds in the Q0 structure are 850 to 950 cm -1 , the BO bond of the Q0 structure is 925 to 1025 cm -1 Each has a peak.
[0096] In NMR measurements, for example 29 In Si-NMR, the peak of the Si-O bond of the Q0 structure is seen in the range of -70 to -60 ppm (the reference material is tetramethylsilane). 27 In Al-NMR, the peak of the Al-O bond with the Q0 structure is visible in the range of 50 to 80 ppm (the reference material is aluminum chloride). 11 In B-NMR, the peak of the BO bond of the Q0 structure is seen in the range of -5 to 15 ppm (the reference material is boron trifluoride diethyl ether complex).
[0097] The presence of oxide anions with a Q0 structure in the crystal structure, that is, in the anion sites of the crystal, can be confirmed by X-ray powder diffraction (XRD) measurements or neutron scattering measurements.
[0098] The oxide anions in the solid electrolyte do not all need to have a Q0 structure, nor do they all need to exist in an agirodite-type crystal structure. Even if the proportion of oxide anions with a Q0 structure relative to the total amount of oxide anions is small, the effect of the present invention is obtained.
[0099] (Agirodite crystals)
[0100] The agirodite-type crystal comprises Li, P, S, and Ha, wherein Ha is at least one halogen element selected from the group consisting of F, Cl, Br, and I. The agirodite-type crystal may consist of only one type with the same composition, or may include two or more types with different compositions.
[0101] The crystal structure can be determined from the X-ray powder diffraction (XRD) pattern. In the XRD pattern, the crystal can be described as agirodite type by having peaks at 2θ = 15.7±0.5° and 30.2±0.5°. In addition to the above, it is preferable for the XRD pattern to also have a peak at 2θ = 18.0±0.5°, and more preferable for it to also have a peak at 2θ = 25.7±0.5°.
[0102] The ratio of the content (at%) of elements constituting the agirhodite-type crystal (the ratio of the content (at%) of elements included in the agirhodite-type crystal) is Li a -PS b -Ha cWhen represented as, 5 <a<7, 4<b<6 또한 0<c<2의 관계를 만족시키는 것이, 결정이 아기로다이트형이 되기 쉽다는 점에서 바람직하다. 이러한 원소비는, 5.1<a<6.3, 4<b<5.3 또한 0.7<c<1.9의 관계를 만족시키는 것이 보다 바람직하고, 5.2<a<6.2, 4.1<b<5.2 또한 0.8<c<1.8의 관계를 만족시키는 것이 더욱 바람직하다. 즉, a에 대하여, 5<a<7이 바람직하고, 5.1<a<6.3이 보다 바람직하고, 5.2<a<6.2가 더욱 바람직하다. b에 대하여, 4<b<6이 바람직하고, 4<b<5.3이 보다 바람직하고, 4.1<b<5.2가 더욱 바람직하다. c에 대하여, 0<c<2가 바람직하고, 0.7<c<1.9가 바람직하고, 0.8<c<1.8이 더욱 바람직하다. 본 명세서에 있어서, 「원소비」는, 원소의 함유량(at%)의 비를 의미한다.
[0103] The preferred crystal structure is cubic (e.g., F-43m), but structures with poor symmetry such as hexagonal, tetragonal, orthogonal, monoclinic, etc., or structures with poor symmetry such as triclinic, may also exist.
[0104] The halogen element represented by Ha is at least one selected from the group consisting of F, Cl, Br, and I, but since the crystal is prone to becoming an agarodite type, it is preferable to include at least one of Cl and Br, more preferable to include Cl, and even more preferable to include Cl alone or a mixture of Cl and Br.
[0105] Here, when Ha contains Cl and Br, if x (at%) represents the Cl content in the agirodite-type crystal and y (at%) represents the Br content, (x / y) is preferably 0.1 or higher, more preferably 0.3 or higher, and even more preferably 0.5 or higher. Additionally, (x / y) is preferably 10 or lower, more preferably 3 or lower, and even more preferably 1.6 or lower. By satisfying the above range, the interaction between lithium ions and halide ions is weakened, making it easier for the lithium ion conductivity of the solid electrolyte after heat treatment to be improved. This is thought to be due to the influence of the mixed anion effect, which weakens the interaction between cations and anions by mixing bromide ions, which have a larger ionic radius than chloride ions. Furthermore, by satisfying the above range, the cycle characteristics of the lithium-ion secondary battery are more likely to be improved.
[0106] In addition, when Ha contains Cl and Br, the ratio of the content (at%) of the elements constituting the agirodite-type crystal is Li a -PS b -Cl c1 -Br c2When expressed as such, c1 is preferably 0.1 or higher, more preferably 0.3 or higher, and even more preferably 0.5 or higher. c1 is preferably 1.5 or lower, more preferably 1.4 or lower, and even more preferably 1.3 or lower. c2 is preferably 0.1 or higher, more preferably 0.3 or higher, and even more preferably 0.5 or higher. c2 is preferably 1.9 or lower, more preferably 1.6 or lower, and even more preferably 1.4 or lower. By satisfying the above ranges for c1 and c2, the ratio of halide ions present in the crystal is optimized, and a stable agirodite-type crystal is obtained while reducing the interaction between anions and lithium ions in the crystal. As a result, the lithium ion conductivity of the solid electrolyte after heat treatment tends to be improved. Furthermore, by satisfying the above ranges for c1 and c2, the cycle characteristics of the lithium-ion secondary battery tend to be improved.
[0107] Here, it is desirable that a, b, and (c1+c2) satisfy the same relationship as a, b, and c described above.
[0108] The crystallite size of the agirodite-type crystal is preferably small from the perspective of obtaining good lithium-ion conductivity when the solid electrolyte is finely ground and converted into a battery. Specifically, the crystallite size is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 250 nm or less. The lower limit of the crystallite size is not particularly limited, but is typically 5 nm or more.
[0109] The crystallite size can be calculated by using the peak full width of the XRD pattern and Scherrer's formula.
[0110] The raw materials for agirodite-type crystals will be explained in detail later, but a mixture containing lithium sulfide (Li2S) is suitably used as such raw materials. Here, it is widely known that lithium sulfide is produced from lithium hydroxide (LiOH), but lithium hydroxide may contain at least one element selected from the group consisting of Na, K, Mg, and Ca as an impurity (hereinafter also referred to as "R"). When agirodite-type crystals are manufactured using raw materials containing R, R may also be present in the agirodite-type crystals. Here, in order to reduce the content of R in the agirodite-type crystals, it is necessary to use high-purity raw materials, which may lead to an increase in manufacturing costs.
[0111] The inventors examined the effect on the physical properties of a solid electrolyte when an agirodite-type crystal contains R, and found that if the content ratio of R is within a predetermined range, there is no effect on the lithium ion conductivity or heat resistance of the solid electrolyte.
[0112] That is, the agirodite-type crystal may contain at least one element selected from the group consisting of Na, K, Mg, and Ca, represented by R. In addition, the ratio of the content (at%) of the element constituting the agirodite-type crystal when R is included is Li a1 -R a2 -PS b -Ha c When expressed as such, a2 is preferably 0.001 or higher, more preferably 0.01 or higher, and even more preferably 0.02 or higher from the perspective of suppressing manufacturing costs. Additionally, a2 is preferably 0.4 or lower, more preferably 0.3 or lower, and even more preferably 0.2 or lower from the perspective of suppressing the decrease in lithium ion conductivity. The agirodite-type crystal does not need to contain R.
[0113] Here, it is desirable that a1, b, and c each satisfy the same relationship as a, b, and c described above. However, the value of a1 may be smaller than the desired numerical range of a described above depending on the value of a2. In that case, it is desirable that the value of (a1+a2) satisfies 5 < (a1+a2) < 7.
[0114] In addition, among Na, K, Mg, and Ca, Mg and Ca may also be included in the solid electrolyte as M constituting the oxide anions described above. If the solid electrolyte contains at least one of the elements Mg and Ca, whether these elements are included as M or as R can be determined by analyzing the crystal structure through Rietveld analysis of the XRD pattern. If the above elements are included as R, Mg and Ca are present in the crystal structure, and O is also present nearby. 2- This results in a case where does not exist. Here, in the vicinity O 2- The fact that it does not exist means that O within the second nearest elements of Mg and Ca 2- It means that it does not exist.
[0115] (Solid electrolyte)
[0116] With respect to the total components constituting the solid electrolyte, the sum of the content of the elements constituting the oxide anion and the crystal phase including agirodite-type crystals is preferably 90 mass% or more, more preferably 92 mass% or more, and even more preferably 94 mass% or more from the perspective of realizing high ionic conductivity. In addition, the upper limit of the sum of the contents is not particularly limited and may be 100 mass%. In addition to agirodite-type crystals, amorphous crystals may also be included in the crystal phase. Furthermore, the agirodite-type crystal composed of at least one of Li, P, S, and Ha may include other crystal phases.
[0117] The sum of the above contents is, for example, the sum of the contents of the elements Li, P, S, Ha, M, and O, and if the agirodite-type crystal contains R, the sum also includes the content of R. In addition, in this specification, the content of Ha is the sum of the contents of F, Cl, Br, and I.
[0118] The content of each element or their total is determined by compositional analysis using ICP emission analysis, atomic absorption spectroscopy, ion chromatography, etc.
[0119] In the solid electrolyte, the proportion of agirodite-type crystals is preferably 50 mass% or more, more preferably 65 mass% or more, and more preferably 80 mass% or more from the perspective of realizing high lithium-ion conductivity. In addition, the upper limit is not particularly limited and may be 100 mass%, but generally it is 99 mass% or less. The proportion of agirodite-type crystals can be calculated by including an internal standard material, measuring by XRD or neutron scattering, and comparing the peak intensity with that of the internal standard material.
[0120] Examples of solid electrolytes that may be included in addition to crystalline phases and oxide anions containing agirodite-type crystals include Li3PS4, Li4P2S6, Li2S, LiHa (where Ha is at least one halogen element selected from F, Cl, Br, and I).
[0121] The ratio of the total elements constituting the oxide anion (at%) to the total elements constituting the agirodite-type crystal and oxide anion (at%), i.e., the element ratio, can be expressed, for example, as {(M+O) / (Li+P+S+Ha+M+O)}.
[0122] The ratio expressed as {(M+O) / (Li+P+S+Ha+M+O)} is preferably 0.2 or less, more preferably 0.18 or less, and even more preferably 0.15 or less, from the perspective that including a large amount of oxide anions lowers ionic conductivity and makes the electrolyte more susceptible to oxidation during fabrication. Additionally, although a stabilizing effect on heat treatment at high temperatures by oxide anions can be observed even in small amounts, the above ratio is preferably 0.0005 or more from the perspective of suitably obtaining this effect. Furthermore, from the perspective of obtaining higher conductivity, the above ratio is more preferably 0.05 or more, and even more preferably 0.01 or more.
[0123] In addition, for example, if an agirodite-type crystal contains R, this elemental ratio is expressed as {(M+O) / (Li+P+S+Ha+R+M+O)}.
[0124] In addition, the ratio of the total elements constituting the oxide anion (at%) to the total elements constituting the agirodite-type crystal and oxide anion (at%) depends on the composition, particularly the content of Ha.
[0125] The ratio of the elemental content (at%) of agirhodite-type crystals Li 7-γ PS 6-γ Ha γ When expressed as such, the ratio of Ha to P is γ = Ha / P. If the value of γ is small, there are many sulfur atoms with weak bonding forces among the isolated anion sites in the agirodite-type crystal structure. As a result, it becomes difficult to incorporate a large amount of oxide anions because it is prone to oxidative decomposition. On the other hand, if the value of γ is large, it becomes easy for lithium halide crystals, such as LiCl, to precipitate. Therefore, it is desirable to incorporate more oxide anions to achieve stabilization.
[0126] When manufacturing a sulfide-based solid electrolyte, the form of the oxide added to become an oxide anion may be a nano-sized fine powder, a micro-sized powder, or a coarse granule. In addition, it may be intentionally incorporated from the container used during manufacturing. Furthermore, the oxide does not need to have a Q0 structure at the time of addition when manufacturing the sulfide-based solid electrolyte.
[0127] As an indicator representing the above relationship, when using the content (at%) of each element, α=(Li+P+S+Ha), β=(Si+Al+Zr+B+O), and γ=(Ha / P), it is desirable to satisfy the following relationship. In addition, if the agirodite-type crystal contains R, α=(Li+P+S+Ha+R).
[0128] 0<{β / (α+β)}<(D+0.1)
[0129] D=(0.1104×γ-0.1133)
[0130] The value expressed as {β / (α+β)} is the same as the ratio expressed as {(M+O) / (Li+P+S+Ha+M+O)}, but the above relationship implies that if the amount of Ha included in the solid electrolyte is large, the effect of the present invention is further obtained, and thus the amount of the optimal oxide anion also increases. The function representing D represents the optimal value of {β / (α+β)} for each elemental ratio of Ha to P, and is a function derived from the results of the examples and comparative examples described below.
[0131] It is more desirable for the value expressed as {β / (α+β)} to satisfy the following relationship.
[0132] 0<{β / (α+β)} <E
[0133] E=(0.2018×γ-0.1608)
[0134] As an indicator of heat resistance, the heat decomposition test temperature of the solid electrolyte is preferably 500°C or higher, more preferably 600°C or higher, and even more preferably 650°C or higher. In addition, the upper limit is not particularly limited, but is typically 900°C or lower.
[0135] The heat resistance of a solid electrolyte can be evaluated by placing the solid electrolyte in a container that does not react with the solid electrolyte, performing heat treatment at a predetermined temperature for 10 to 60 minutes, and investigating the change in ionic conductivity before and after the heat treatment. It is desirable that the ionic conductivity does not change before and after the heat treatment, and if it becomes less than half of what it was before the heat treatment after the heat treatment, it can be said that the heat resistance, that is, the heat resistance, is low.
[0136] As an indicator of the above heat resistance, the lithium ion conductivity when heat treatment is performed at a high temperature will be explained in detail below.
[0137] For example, let σ1 be the lithium ion conductivity of an agirodite-type crystal of a specific composition. If the lithium ion conductivity σ2 after heat treatment at a specific temperature is lower than σ1 (σ1 > σ2), it means that at least a portion of the crystal has undergone thermal decomposition. Conversely, if the lithium ion conductivity σ3 after heat treatment under the same conditions for a solid electrolyte according to the present embodiment containing an agirodite-type crystal of the same composition is higher than σ2 (σ3 > σ2), it can be determined that the thermal decomposition has been suppressed and that the heat resistance is excellent. Furthermore, if σ3 is higher than σ1 (σ3 > σ1), it can be determined that the agirodite-type crystal has been reconstituted with a higher lithium ion conductivity through heat treatment. Additionally, if an agirodite-type crystal of such composition is used, it can be assumed that both effects of improving the bulk lithium ion conductivity and reducing grain boundary resistance are obtained during the sintering process.
[0138] In addition, in this specification, lithium ion conductivity refers to the lithium ion conductivity at 25°C and is obtained from a Nyquist plot obtained by measuring AC impedance.
[0139] The solid electrolyte according to the present embodiment satisfies the relationship σ3 > σ2. It is preferable that the solid electrolyte according to the present embodiment satisfies the relationship σ3 ≥ 1.5 × σ2, more preferable that it satisfies the relationship σ3 ≥ 3 × σ2, and it is preferable that σ3 be as high as possible.
[0140] In addition, it is also desirable that the solid electrolyte according to the present embodiment satisfies the relationship σ3 > σ1.
[0141] Although the solid electrolyte according to the present embodiment exhibits high heat resistance, it is desirable to control the cooling rate after heat treatment. From the perspective of making the crystallite size smaller, it is desirable to cool at a cooling rate of 1°C / second or higher. In addition, from the perspective of inducing crystal growth during cooling, it is desirable to cool at a cooling rate of 1°C / second or lower. Thus, it is desirable to change the cooling rate according to the desired physical properties.
[0142] When used in a lithium-ion secondary battery, the solid electrolyte forms a solid electrolyte layer together with other components, such as a binder, as needed. The binder or other components are conventionally known.
[0143] With respect to the entire solid electrolyte layer, the content of the solid electrolyte is preferably 80 mass% or more, and more preferably 90 mass% or more.
[0144] A conventionally known method is also used for forming a solid electrolyte layer. For example, a solid electrolyte layer can be formed by dispersing or dissolving a component constituting the solid electrolyte layer in a solvent to form a slurry, coating it in a layered (sheet-like) form, drying it, and pressing it as desired. If necessary, a debinding treatment may be performed by applying heat. The thickness of the solid electrolyte layer can be easily adjusted by adjusting the coating amount of the slurry.
[0145] In addition, instead of wet molding, a solid electrolyte layer may be formed by dry press molding of solid electrolyte powder, etc., on the surface of a positive electrode or a negative electrode. Alternatively, a solid electrolyte layer may be formed on another substrate and transferred onto the surface of a positive electrode or a negative electrode.
[0146] The solid electrolyte may be mixed with a positive electrode active material or a negative electrode active material and used as a positive electrode layer or a negative electrode layer. The positive electrode active material or negative electrode active material, current collector, binder, conductivity aid, etc. used in the positive electrode layer or negative electrode layer may be conventionally known.
[0147] A lithium-ion secondary battery using a solid electrolyte comprises the solid electrolyte layer, a positive electrode layer, and a negative electrode layer.
[0148] The material of the casing of the lithium-ion secondary battery may also be conventionally known. The shape of the lithium-ion secondary battery may also be conventionally known, but examples include coin type, sheet type (film type), foldable type, cylindrical type with a wound bottom, button type, etc., and can be appropriately selected according to the application.
[0149] A lithium-ion secondary battery comprising a sulfide-based solid electrolyte according to the present embodiment has excellent cycle characteristics. For example, when an all-solid-state lithium-ion secondary battery is manufactured by the following method and a charge-discharge test is performed, the capacity retention rate expressed by the following formula is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. A higher capacity retention rate is preferable, and it may be 100%.
[0150] (method)
[0151] (Production of the positive pole composite material)
[0152] As a positive electrode active material, layered rock salt type LiCoO2 powder (volume average particle size: 10 μm) coated with LiNbO3 with a thickness of 7 nm is used, and a positive electrode composite is prepared by mixing 35 parts of the sulfide-based solid electrolyte according to the present embodiment, 60 parts of the positive electrode active material, and 5 parts of a conductivity aid (acetylene black, manufactured by Denka Co., Ltd., HS100). The thickness of the LiNbO3 coating is determined by transmission electron microscopy (TEM) observation.
[0153] (Fabrication of all-solid-state lithium-ion secondary batteries)
[0154] 80 mg of the sulfide-based solid electrolyte according to the present embodiment is poured into a plastic cylinder with a diameter of 10 mm and pressure-molded to form a solid electrolyte layer. Subsequently, 10 mg of the positive electrode composite material prepared above is poured into the same cylinder and pressure-molded again to form a positive electrode layer. In addition, indium foil and lithium foil are poured from the opposite side to the positive electrode composite material to form a negative electrode layer. In this way, an all-solid-state lithium-ion secondary battery is manufactured, and a charge-discharge test is performed at a confining pressure of 10 kN.
[0155] In addition, for the sulfide-based solid electrolyte used in the positive electrode composite material and solid electrolyte layer, it is preferable that it be in powder form by grinding or the like.
[0156] (Charge / Discharge Test)
[0157] Using the fabricated all-solid-state lithium-ion secondary battery, a constant current charge-discharge test is performed for 100 cycles at 25°C with a charge-discharge current density of 0.1C and a charge-discharge potential range of 1.9-3.7V. From the results of the charge-discharge test, the capacity retention rate (%) expressed by the following formula is calculated.
[0158] Capacity retention rate (%) = (Discharge capacity at 100th cycle / Discharge capacity at 1st cycle) × 100
[0159] The higher the capacity retention rate, the more the degradation of battery characteristics is suppressed when charging and discharging is repeated, and thus the cycle characteristics can be judged to be excellent. The reason why the lithium-ion secondary battery containing the sulfide-based solid electrolyte according to the present embodiment exhibits excellent cycle characteristics is believed to be, for example, that during the charge-discharge test under the above conditions, a thin oxide layer derived from oxygen in the solid electrolyte is formed at the interface between the solid electrolyte layer and the positive electrode layer. As a result, it is believed that the cycle characteristics are improved because the sulfide ions in the solid electrolyte become difficult to decompose. Furthermore, even when the sulfide-based solid electrolyte according to the present embodiment is used in the solid electrolyte layer of a lithium-ion secondary battery with a different composition from the all-solid-state lithium-ion secondary battery in the above charge-discharge test, a similar oxide layer may be formed by the charging and discharging of such a battery.
[0160] In particular, if Ha in an agirodite-type crystal contains Cl and Br, and their elemental ratios are within the aforementioned preferred range, it is easier and more desirable to improve the cycle characteristics.
[0161] Method for manufacturing sulfide-based solid electrolytes
[0162] The method for manufacturing a sulfide-based solid electrolyte used in a lithium-ion secondary battery according to the present embodiment is not particularly limited if an agirodite-type crystal is obtained that includes Li, P, S, and Ha, in which an oxide anion of a Q0 structure having an MO bond formed by combining M and O is present in the crystal structure.
[0163] Specifically, for example, by performing heat treatment on a mixture of at least one of a plurality of compounds that serve as materials for an agirodite-type crystal and an agirodite-type crystal, and at least one of a composition comprising an oxide having an MO bond and an oxide anion having a Q0 structure having an MO bond, an agirodite-type crystal is obtained in which an oxide anion having a Q0 structure having an MO bond exists in the crystal structure.
[0164] In that the timing of the above heat treatment is not particularly limited, for example, any of the following manufacturing methods (i) to (iv) is used to obtain the sulfide-based solid electrolyte according to the present embodiment.
[0165] (Manufacturing method (i))
[0166] (Process i-1) A process of mixing raw materials containing Li, P, S and Ha and crystallizing by heating to obtain agirodite-type crystals,
[0167] (Process i-2) A process for obtaining a mixture by mixing an oxide having an MO bond formed by the M and O bonding with the obtained agarodite-type crystal, and
[0168] (Process i-3) The process includes heat treatment of the obtained mixture to obtain an agarodite-type crystal in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure.
[0169] Ha is at least one element selected from the group consisting of F, Cl, Br, and I. M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table.
[0170] (Manufacturing method (ii))
[0171] (Process ii-1) A process for obtaining a raw material composition by mixing raw materials including Li, P, S and Ha with an oxide having an MO bond formed by the combination of M and O, and
[0172] (Process ii-2) A process of heat-treating the obtained raw material composition to obtain an agirodite-type crystal in which an oxide anion of a Q0 structure having an MO bond exists in the crystal structure.
[0173] Ha is at least one element selected from the group consisting of F, Cl, Br, and I. M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table.
[0174] (Manufacturing method (iii))
[0175] (Process iii-1) A process for obtaining an intermediate product by reacting raw materials containing Li, P, S and Ha,
[0176] (Process iii-2) A process for obtaining a mixture by mixing an oxide having an MO bond formed by the combination of M and O with the obtained intermediate product, and
[0177] (Process iii-3) The process includes heat treatment of the obtained mixture to obtain an agarodite-type crystal in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure.
[0178] Ha is at least one element selected from the group consisting of F, Cl, Br, and I. M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table.
[0179] (Manufacturing method (iv))
[0180] (Process iv-1) A process of mixing raw materials containing Li, P, S and Ha and crystallizing them by heating to obtain agirodite-type crystals,
[0181] (Process iv-2) A process for obtaining a composition comprising an oxide anion of a Q0 structure having an MO bond formed by the combination of M and O,
[0182] (Process iv-3) A process for obtaining a mixture of the obtained agirodite-type crystals and the obtained composition, and
[0183] (Process iv-4) The process includes heat treatment of the obtained mixture to obtain an agarodite-type crystal in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure.
[0184] (Process iv-1) and (Process iv-2) may be performed either first or simultaneously.
[0185] Ha is at least one element selected from the group consisting of F, Cl, Br, and I. M is at least one element selected from the group consisting of metallic and metalloid elements of groups 2 to 14 of the periodic table.
[0186] As the raw material containing Li, P, S, and Ha in (process i-1) of the above manufacturing method (i), a material conventionally known as a material for obtaining agirodite-type crystals containing Li, P, S, and Ha may be used.
[0187] For example, a mixture of a compound containing Li (lithium), a compound containing P (phosphorus), a compound containing S (sulfur), and a compound containing Ha (halogen) can be cited.
[0188] Examples of compounds containing Li include lithium compounds such as lithium sulfide (Li2S), lithium oxide (Li2O), lithium carbonate (Li2CO3), lithium hydroxide (LiOH), and lithium sulfate (Li2SO4), as well as lithium metal elements.
[0189] Examples of compounds containing P include phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5), phosphorus compounds such as lithium phosphate (LiPO3, Li4P2O7, Li3PO4) and sodium phosphate (NaPO3, Na4P2O7, Na3PO4), and phosphorus elements.
[0190] Examples of compounds containing S include the above lithium sulfide (Li2S), the above phosphorus sulfide (P2S3, P2S5), or hydrogen sulfide (H2S), and sulfur compounds can also be used.
[0191] Among compounds containing Ha, compounds containing Cl (chlorine) include, for example, lithium chloride (LiCl), phosphorus trichloride (PCI3), phosphorus chloride (PCI5), phosphorus tetrachloride (P2Cl4), phosphoryl chloride (POCl3), sulfur dichloride (SCl2), sulfur dichloride (S2Cl2), sodium chloride (NaCl), boron trichloride (BCl3), etc.
[0192] Among compounds containing Ha, compounds containing Br (bromine) include, for example, lithium bromide (LiBr), phosphorus tribromide (PBr3), phosphoryl bromide (POBr3), disulfide disulfide (S2Br2), sodium bromide (NaBr), boron tribromide (BBr3), etc.
[0193] Among these, a combination with at least one of lithium sulfide, phosphorus sulfide, lithium chloride, and lithium bromide is preferred.
[0194] These raw materials are highly unstable in the atmosphere and decompose upon reaction with water, raising concerns about the generation of hydrogen sulfide gas or oxidation. Therefore, it is desirable to mix them in an inert atmosphere.
[0195] Mixing of raw materials can be carried out using media such as a planetary ball mill, or media-free mixing such as a fin mill, powder stirrer, or airflow mixing. The raw materials may be amorphized by mixing prior to heating.
[0196] Agirodite-type crystals are obtained by crystallizing raw materials containing Li, P, S, and Ha, or amorphous sulfide solid electrolyte materials, by heating. Furthermore, as described above, as long as they are within a range that does not affect the lithium ion conductivity or heat resistance of the solid electrolyte, the agirodite-type crystals may contain impurities such as R originating from the raw materials, etc.
[0197] It is preferable to perform heating under, for example, an inert gas atmosphere, a hydrogen sulfide gas atmosphere, a sulfur gas atmosphere, or a vacuum seal.
[0198] From the perspective of promoting solid-state reactions, i.e., crystallization, the heating temperature is preferably 400°C or higher, more preferably 450°C or higher, and even more preferably 500°C or higher. In addition, from the perspective of suppressing thermal decomposition, it is preferably less than 600°C, and more preferably 575°C or lower.
[0199] In the same regard, a heating time of 1 hour or more is preferable, 2 hours or more is more preferable, and 4 hours or more is even more preferable. Additionally, a heating time of 100 hours or less is preferable, 50 hours or less is more preferable, and 24 hours or less is even more preferable.
[0200] In (Process i-2), a mixture is obtained by mixing an oxide having an MO bond in which M and O are bonded with the agirodite-type crystal obtained in (Process i-1). The oxide having the MO bond may be manufactured or a commercially available one may be used as is.
[0201] The mixing method is not particularly limited, but grinding and mixing may be performed using, for example, a ball mill, bead mill, homogenizer, pin mill, powder stirrer, airflow mixer, etc.
[0202] In (Process i-3), heat treatment is performed on the mixture obtained in (Process i-2). By doing so, crystals of agirodite are obtained in which oxide anions of the Q0 structure having MO bonds exist within the crystal structure.
[0203] Although the mechanism is unclear, the inventors believe that through heat treatment, the oxide becomes an oxide anion with a Q0 structure, and this oxide anion with a Q0 structure acts as a crystal nucleus, thereby reconstructing an agirodite-type crystal, or that the oxide anion with a Q0 structure enters the sites of the agirodite-type crystal structure. By doing so, high heat resistance can be achieved.
[0204] Although the conditions for heat treatment vary depending on the composition, from the perspective of forming oxide anions with a Q0 structure well, the heat treatment temperature is preferably 500°C or higher, more preferably 600°C or higher, even more preferably 650°C or higher, and particularly preferably 700°C or higher. In addition, from the perspective of reducing grain boundary resistance, the heat treatment temperature is preferably 500°C or higher, and more preferably 600°C or higher. Meanwhile, from the perspective of preventing thermal decomposition caused by unnecessary high temperatures, the heat treatment temperature is preferably 900°C or lower, and more preferably 800°C or lower. The atmosphere under which the heat treatment is performed is preferably, for example, an inert gas atmosphere, a hydrogen sulfide gas atmosphere, a sulfur gas atmosphere, or under a vacuum seal.
[0205] For the same reason, the heat treatment time is preferably 0.1 hours or more, more preferably 0.25 hours or more, and even more preferably 0.5 hours or more. In addition, the heat treatment time is preferably 4 hours or less, more preferably 2 hours or less, and even more preferably 1 hour or less.
[0206] The raw material containing Li, P, S and Ha in (Process ii-1) of manufacturing method (ii) and the oxide having an MO bond formed by combining M and O are, respectively, the raw material in (Process i-1) and (Process i-2) of manufacturing method (i) and the oxide having an MO bond formed by combining M and O.
[0207] (Process ii-1) differs from manufacturing method (i) in that, before performing the agirodite-type crystal precipitation of raw materials containing Li, P, S and Ha, a raw material composition is obtained by mixing with an oxide having MO bonds.
[0208] Mixing of raw materials and oxides having MO bonds is carried out, for example, in an inert atmosphere by a ball mill, bead mill, homogenizer, fin mill, powder stirrer, air stream mixing, etc.
[0209] In (Process ii-2), by performing heat treatment on the raw material composition obtained in (Process ii-1), an agirodite-type crystal is obtained in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure. The heat treatment in (Process ii-2) is the same as the heat treatment in (Process i-3) of manufacturing method (i).
[0210] The method of producing the intermediate product from the raw material containing Li, P, S and Ha in (Process iii-1) of manufacturing method (iii) is not specifically defined. It may be reacted mechanically and chemically using a mixer, or sulfide crystals may be produced by heat treatment, or both.
[0211] In (Process iii-1), raw materials are reacted to obtain an intermediate product.
[0212] The intermediate product may be an amorphous sulfide solid electrolyte material or a crystalline sulfide solid electrolyte material. Compared to the raw material, which has poor atmospheric stability and poor handling properties, the intermediate product has improved atmospheric stability.
[0213] For intermediate products and raw materials, the manufacturing conditions can be appropriately modified depending on the target solid electrolyte.
[0214] In (Process iii-2), a mixture is obtained by mixing the intermediate product obtained in (Process iii-1) with an oxide having an MO bond formed by combining M and O. The oxide having an MO bond formed by combining M and O here is the same as the oxide having an MO bond formed by combining M and O in (Process i-2) of manufacturing method (i).
[0215] Mixing of the intermediate product and the oxide having MO bonds can be done in a dry inert atmosphere, but for the sake of reducing manufacturing costs, it may also be done in a dry air atmosphere, for example, by a ball mill, bead mill, homogenizer, fin mill, powder stirrer, airflow mixing, etc.
[0216] In (Process iii-3), by performing heat treatment on the mixture obtained in (Process iii-2), an agarodite-type crystal is obtained in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure. The heat treatment in (Process iii-3) is the same as the heat treatment in (Process i-3) of manufacturing method (i).
[0217] The (process iv-1) of manufacturing method (iv) is the same as the (process i-1) of manufacturing method (i).
[0218] In (Process iv-2), a composition is obtained that includes an oxide anion of a Q0 structure having an MO bond formed by combining M and O. Specifically, an oxide is used that is similar to the oxide having an MO bond formed by combining M and O in (Process i-2) of manufacturing method (i) to obtain a composition that exists as an oxide anion of a Q0 structure.
[0219] For example, an agirodite-type crystal having an oxide anion of a Q0 structure having an MO bond in the crystal structure obtained by manufacturing method (i) to manufacturing method (iii), etc., may be used as the composition. In addition, the composition is not limited to an agirodite-type crystal, and may have a crystal having a different crystal structure as long as the oxide exists as an oxide anion of a Q0 structure. In addition, it is not limited to a crystal and may be amorphous.
[0220] In (Process iv-3), a mixture is obtained by mixing the agirodite-type crystal obtained in (Process iv-1) and the composition obtained in (Process iv-2).
[0221] Mixing of the agirodite-type crystals and the composition is carried out, for example, in a dry inert atmosphere using a ball mill, bead mill, homogenizer, pin mill, powder stirrer, airflow mixing, etc.
[0222] In (Process iv-4), by performing heat treatment on the mixture obtained in (Process iv-3), an agirodite-type crystal is obtained in which an oxide anion of a Q0 structure having an MO bond is present in the crystal structure. The heat treatment in (Process iv-4) is the same as the heat treatment in (Process i-3) of manufacturing method (i).
[0223] It is presumed that by performing the heat treatment of (Process iv-4), the oxide anions of the Q0 structure in the composition obtained in (Process iv-2) will enter into the agirodite-type crystal structure obtained in (Process iv-1) and be reconfigured.
[0224] Examples
[0225] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.
[0226] Examples 2 to 5, Examples 7 to 9, Examples 11 to 16, Examples 18 to 28, Examples 30 to 34, Examples 36, 38, 39, Examples 41, 42, 44, 46, 48, 50, 52 to 54, Examples 1-1 to 1-3, Examples 2-1 to 2-3, and Examples 3-1 to 3-10 are examples. Additionally, Examples 1, 6, 10, 17, 29, 35, 37, 40, 43, 45, 47, 49, and 51 are comparative examples.
[0227] [evaluation]
[0228] The lithium ion conductivity was measured using an AC impedance measuring device (Potentistat / Galvanostat VSP manufactured by Bio-Logic Sciences Instruments) with the obtained powder as a measurement sample at a pressure of 380 kN.
[0229] The measurement conditions were set as follows: measurement frequency: 100 Hz to 1 MHz, measurement voltage: 100 mV, measurement temperature: 25 ℃.
[0230] [Example 1]
[0231] Under a dry nitrogen atmosphere, lithium sulfide powder (Sigma, purity 99.98%), phosphorus pentasulfide powder (Sigma, purity 99%), and lithium chloride powder (Sigma, purity 99.99%) were weighed to the elemental ratios listed in Table 1, and mixed at 400 rpm for 4 hours using a planetary ball mill in the same atmosphere. Subsequently, the mixture was vacuum-sealed in a carbon-coated quartz tube and heated at 550°C for 5 hours to obtain agirodite-type crystals of Li6PS5Cl.
[0232] A sulfide-based solid electrolyte was obtained by pelletizing the obtained crystals, vacuum sealing them again in a carbon-coated quartz tube, and performing heat treatment at 650°C for 30 minutes.
[0233] The lithium ion conductivity of the agirodite-type crystal of Li6PS5Cl before heat treatment was 2.7 mS / cm, and the lithium ion conductivity of the obtained sulfide-based solid electrolyte was 1.1 mS / cm.
[0234] In addition, the table also shows the values of {(M+O) / (Li+P+S+Ha+M+O)}, {β / (α+β)}, and (D+0.1) using the elemental ratios of the elements constituting the crystal and the elements constituting the oxide anion. Furthermore, in the table, if the elemental ratio is blank, it means that these elements are not contained and is equivalent to "0.000".
[0235] [Example 2]
[0236] SiO2 powder (made by grinding As One Co., Ltd.'s SJT series quartz test tubes) was added to the agirodite-type crystal of Li6PS5Cl obtained in the same manner as in Example 1, and the mixture was mixed in a mortar and pestle to obtain a mixture. The amount of SiO2 powder added was adjusted so that the elemental ratios of Si and O were each the amounts listed in Table 1.
[0237] The obtained mixture was pelletized in the same manner as in Example 1, vacuum-sealed again in a carbon-coated quartz tube, and heat-treated at 650°C for 30 minutes to obtain a sulfide-based solid electrolyte containing an agarodite-type crystal having an oxide anion with a Q0 structure having Si-O bonds.
[0238] The lithium ion conductivity of the obtained sulfide-based solid electrolyte is shown in Table 1.
[0239] Furthermore, the composition of the agirodite-type crystal Li6PS5Cl and the oxide composition SiO2 differ strictly from the actual compositions in that they are both input compositions used as raw materials. However, based on the results of ICP emission spectroscopic analysis of elements P and S, atomic absorption analysis of element Li, and ion chromatography analysis of element Cl, this difference is within a range of at most ±10% and does not affect the results or discussion. The same applies to other examples.
[0240] [Examples 3 to 5]
[0241] A sulfide-based solid electrolyte containing an agarodite-type crystal having an oxide anion with a Q0 structure having Si-O bonds was obtained in the same manner as in Example 2, except that the amount of SiO2 powder, which is an oxide, was changed to the amount listed in Table 1. The lithium ion conductivity of the obtained sulfide-based solid electrolyte is shown in Table 1.
[0242] [Examples 6 to 34]
[0243] A sulfide-based solid electrolyte containing an oxide anion having a Q0 structure with MO bonds was obtained by performing heat treatment without including oxides, in the same manner as in Example 2, except that the elemental ratio of the agirodite-type crystal and the type or amount of oxide added were changed to those listed in Table 1 or Table 2. Additionally, in Examples 6, 10, 17, and 29, a sulfide-based solid electrolyte was obtained by performing heat treatment without including oxides, in the same manner as in Example 1.
[0244] The agirodite-type crystals before heat treatment and the lithium ion conductivity of the obtained sulfide-based solid electrolyte are shown in Table 1 or Table 2.
[0245] In addition, when Br was included in the crystal, lithium bromide powder (Sigma, purity 99.995%) was used as the Br source. In addition, when Al was included as the oxide anion, Al2O3 powder (Sigma Type CG-20) was used, and when Zr was included, ZrO2 powder (Sigma, purity 99%) was used.
[0246]
[0247]
[0248] [Examples 35 to 44]
[0249] Under a dry nitrogen atmosphere, lithium sulfide powder (Sigma, purity 99.98%), phosphorus pentasulfide powder (Sigma, purity 99%), lithium chloride powder (Sigma, purity 99.99%), lithium bromide powder (Sigma, purity 99.995%), and SiO2 powder (As One, ground using a quartz test tube SJT series) were weighed to the elemental ratios shown in Table 3, and mixed using a mortar and pestle to obtain a raw material composition.
[0250] By vacuum sealing the obtained raw material composition in a carbon-coated quartz tube and heat-treating it at 750°C for 1 hour, a sulfide-based solid electrolyte, or a sulfide-based solid electrolyte containing an agarodite-type crystal having an oxide anion with a Q0 structure having an MO bond, was obtained.
[0251] The lithium ion conductivity of sulfide-based solid electrolytes is shown in Table 3.
[0252]
[0253] [Examples 45 to 52]
[0254] For each of the sulfide-based solid electrolytes obtained in Example 1, Example 4, Example 17, Example 26, Example 35, Example 36, Example 40, and Example 41, heat treatment is performed again at 650°C for 30 minutes. The change in lithium ion conductivity before and after re-heat treatment of the sulfide-based solid electrolytes is shown in Table 4.
[0255] In addition, the lithium ion conductivity after re-heat treatment is a value predicted from the fact that in Examples 1 and 17, the conductivity was reduced to less than half after heat treatment at 650°C for 30 minutes, and in Examples 4 and 27, the decrease in conductivity was small or the conductivity improved. Also, in Examples 49 to 52, crystals were not formed before mixing with oxide due to the manufacturing method. Therefore, the lithium ion conductivity in "Crystals" of Table 4 is left blank to indicate that there is no
[0256]
[0257] [Example 53]
[0258] A mixture is obtained by mixing equimolar amounts of the sulfide-based solid electrolyte of Example 35 and the sulfide-based solid electrolyte containing oxide anions of a Q0 structure having MO bonds of Example 36. The mixture is heat-treated at 650°C for 30 minutes to obtain a sulfide-based solid electrolyte containing agirodite-type crystals containing oxide anions of a Q0 structure having MO bonds.
[0259] The change in lithium ion conductivity before and after heat treatment is shown in Table 5. In addition, the elemental ratio of crystals and oxide anions of the mixture is the average of the elemental ratios of Examples 35 and 36. Furthermore, the lithium ion conductivity before heat treatment is a value within the range achievable by referring to Examples 1 to 5 in Table 1. The lithium ion conductivity after heat treatment is a value expected in the same way as in Examples 45 to 52.
[0260] [Example 54]
[0261] Except for using the sulfide-based solid electrolyte of Example 40 instead of Example 35, and the sulfide-based solid electrolyte of Example 41 containing an oxide anion of a Q0 structure having an MO bond instead of Example 36, a sulfide-based solid electrolyte containing an oxide anion of a Q0 structure having an MO bond is obtained in the same manner as in Example 53.
[0262] The change in lithium ion conductivity before and after heat treatment is calculated in the same manner as in Example 53. The results are shown in Table 5.
[0263]
[0264] From the results in Tables 1 and 2, it was found that for sulfide-based solid electrolytes that do not contain Q0-structured oxide anions in their crystal structure, the lithium ion conductivity decreased to less than half, and in some cases, to less than 20%, upon heat treatment at 650°C for 30 minutes. This implies that the crystals underwent thermal decomposition due to this heat treatment. On the other hand, it was confirmed that for sulfide-based solid electrolytes containing Q0-structured oxide anions in their crystal structure, the rate of decrease in lithium ion conductivity was reduced and stability at high temperatures was improved. Furthermore, depending on the crystal structure and the type and amount of oxide anions, higher lithium ion conductivity was exhibited than before heat treatment. This suggests that the crystals exhibit excellent stability at high temperatures and were reconfigured into agirodite-type crystals with higher lithium ion conductivity through heat treatment. Additionally, it is believed that using agirodite-type crystals with this composition allows for the attainment of both improved bulk ion conductivity and reduced grain boundary resistance during the sintering process. The inventors believe that the results predicted in Table 4 are valid from this stability at high temperatures.
[0265] From the results in Table 3, the above effect was confirmed even when the heat treatment temperature was increased to a higher temperature of 750°C, and very high thermal stability was exhibited. In addition, a sulfide-based solid electrolyte containing oxide anions with a Q0 structure was obtained even when a raw material composition mixed with oxides of Li, P, S, and Ha was heat-treated without going through an agirodite-type crystal. That is, it was confirmed that a sulfide-based solid electrolyte with a desired structure can be obtained whether heat treatment is performed after obtaining an agirodite-type crystal beforehand or heat treatment is performed in conjunction with crystallization.
[0266] In addition, from the results of Table 5, it is presumed that when a composition containing oxide anions of the Q0 structure is mixed with an agirodite-type crystal that does not contain oxide and heat-treated, the oxide anions of the Q0 structure in the composition enter the agirodite-type crystal structure and are reconfigured, thereby obtaining a sulfide-based solid electrolyte that is stable at high temperatures.
[0267] For the sulfide-based solid electrolyte of Example 4, to which SiO2 powder, an oxide, was added, X-ray diffraction measurements were performed, and a structural refinement analysis was performed using the Rietveld method. Then, three types of ion distances that can be considered as the movement paths of lithium ions in the agarodite crystal structure were calculated: (1) the distance between lithium sites 48h-24g-48h (doublelet jump distance), (2) the distance within the cage (intra-cage jump distance), and (3) the distance between cages (inter-cage jump distance) (J. Am. Chem. Soc. 2017, 139, 10909-10918 Figure 1). As a result, the distance of (1) in Example 4 was 2.26396 Å, the distance of (2) was 2.28013 Å, and the distance of (3) was 2.42153 Å. In addition, the lattice constant was calculated. The lattice constant of Example 4 was 9.85087 Å. Also, in the agirodite-type crystal (Li6PS5Cl) of the basic structure shown in Figure 1 of J. Am. Chem. Soc. 2017, 139, 10909-10918, the distance of (1) is 1.95772 Å, the distance of (2) is 2.25333 Å, and the distance of (3) is 2.76089 Å. Also, according to the same literature, the lattice constant of the agirodite-type crystal of the basic structure is 9.85980 Å.
[0268] [Examples 1-1 to 1-3]
[0269] Under a dry nitrogen atmosphere, lithium sulfide powder (Sigma, purity 99.98%), phosphorus pentasulfide powder (Sigma, purity 99%), and lithium chloride powder (Sigma, purity 99.99%) were weighed to have the elemental ratios listed in Table 6, and mixed at 400 rpm for 4 hours using a planetary ball mill in the same atmosphere. Subsequently, the mixture was vacuum-sealed in a carbon-coated quartz tube and heated at 450°C for 5 hours to obtain agarodite-type crystals. In addition, when the crystals contained Br, lithium bromide powder (Sigma, purity 99.995%) was used as the Br source.
[0270] SiO2 powder (made by grinding As One Co., Ltd.'s SJT series quartz test tube) was added to the obtained agirodite-type crystal and mixed in a mortar and pestle to obtain a mixture. The amount of SiO2 powder added was adjusted so that the elemental ratios of Si and O were each the amounts listed in Table 6.
[0271] The obtained mixture was pelletized, vacuum-sealed in a quartz tube, and heat-treated at 750°C for 30 minutes to obtain a sulfide-based solid electrolyte containing an agirodite-type crystal having an oxide anion with a Q0 structure having Si-O bonds. Here, the agirodite-type crystals in Examples 1-2 and 1-3 both contain Cl and Br as Ha. If the content of Cl in the agirodite-type crystal is x (at%) and the content of Br is y (at%), then in Example 1-2, (x / y) = 7, and in Example 1-3, (x / y) = 1.
[0272] Table 6 shows the agirodite-type crystals before heat treatment and the lithium ion conductivity of the obtained sulfide-based solid electrolyte.
[0273]
[0274] [Examples 2-1 to 2-3]
[0275] The cycle characteristics of all-solid-state lithium-ion secondary batteries using each of the sulfide-based solid electrolytes of Examples 1-1 to 1-3 were evaluated.
[0276] (Production of solid electrolyte powder)
[0277] First, the sulfide-based solid electrolytes of Example 1-1, Example 1-2, and Example 1-3 were each placed in a carbon container and heat-treated by heating at 450°C for 60 minutes in an N2 atmosphere with a dew point of -60°C or lower to obtain the sulfide-based solid electrolytes of Example 2-1, Example 2-2, and Example 2-3, respectively.
[0278] The compositional formulas and lithium ion conductivity of the sulfide-based solid electrolytes of Examples 2-1, 2-2, and 2-3 are shown in Table 7. The compositional formulas here are values obtained by compositional analysis using the following method. Note that O was set to twice the value of Si.
[0279] (Composition analysis method)
[0280] The solid electrolyte powder weighed inside the glove box was dissolved in an alkaline aqueous solution, and composition analysis was performed by ICP emission spectroscopy for P, S, and Si (device: Hitachi High-Tech Science, model number PS3520UVDDII), analysis by atomic absorption for Li (device: Hitachi High-Tech, model number ZA3300; CsCl was added to the solution concentration to 0.1% when measuring Li), and analysis by ion chromatography for elements Cl and Br (device: Thermo Fisher Scientific, model number ICS-2100 (column: AS11HC); a small amount of H2O2 was added and the solution was diluted with ultrapure water).
[0281] Each of the obtained sulfide-based solid electrolytes of Examples 2-1 to 2-3 was dry-ground using alumina balls with a particle size of 2 mm in a planetary ball mill (manufactured by Ito Seisakusho Co., Ltd., model number LP-4) and passed through a sieve with a mesh size of 43 μm to obtain sulfide-based solid electrolyte powder with a particle size distribution of D50 of 3 μm. In addition, the lithium ion conductivity in Table 7 is the measured value before the grinding was performed. All operations were carried out under a dry nitrogen atmosphere. The particle size distribution was measured using a Microtrac laser diffraction particle size distribution meter MT3300EXII, and the average particle size (D50) was measured from the obtained volume-based particle size distribution chart.
[0282] (Production of the positive pole composite material)
[0283] As a positive electrode active material, layered rock salt type LiCoO2 powder coated with LiNbO3 (volume average particle size: 10 μm) was used to prepare a positive electrode composite by mixing 35 parts of the sulfide-based solid electrolyte powder prepared above, 60 parts of the positive electrode active material, and 5 parts of a conductivity aid (acetylene black, manufactured by Denka Co., Ltd., HS100). The thickness of the LiNbO3 coating was 7 nm from TEM observation.
[0284] (Fabrication of all-solid-state lithium-ion secondary batteries)
[0285] 80 mg of the sulfide-based solid electrolyte powder prepared above was placed into a plastic cylinder with a diameter of 10 mm and pressure-molded to form a solid electrolyte layer. Subsequently, 10 mg of the positive electrode composite material prepared above was placed into the same cylinder and pressure-molded again to form a positive electrode layer. In addition, indium foil and lithium foil were placed from the opposite side of the positive electrode composite material to form a negative electrode layer. In this way, an all-solid-state lithium-ion secondary battery was fabricated, and a charge-discharge test was performed at a confining pressure of 10 kN.
[0286] (Charge / Discharge Test)
[0287] Using the fabricated all-solid-state lithium-ion secondary batteries, 100 cycles of constant current charge-discharge tests were performed at 25°C with a charge-discharge current density of 0.1C and a charge-discharge potential range of 1.9-3.7V. From the results of the charge-discharge tests, the capacity retention rate (%) expressed by the following formula was calculated to evaluate the cycle characteristics of the all-solid-state lithium-ion secondary batteries. The capacity retention rates (%) for each example are shown in Table 7.
[0288] Capacity retention rate (%) = (Discharge capacity at 100th cycle / Discharge capacity at 1st cycle) × 100
[0289]
[0290] [Examples 3-1 to 3-10]
[0291] Assuming that the raw material for the agirodite-type crystal contains impurities, a sulfide-based solid electrolyte was prepared under conditions identical to those of Example 26, except that a portion of the lithium sulfide was substituted with Na2S, K2S, MgS, or CaS. Specifically, the sulfide-based solid electrolytes of Examples 3-1 to 3-10 were obtained by adjusting the mixing ratio of the raw materials, etc., in the same manner as in Example 26, except that the agirodite-type crystal had the composition ratio shown in Table 8. Here, Na2S powder (Kojunto Kagaku Genkyuzo, 2N) was used when the agirodite-type crystal contains Na, K2S powder (Kojunto Kagaku Genkyuzo, 2Nup) was used when it contains K, MgS powder (Kojunto Kagaku Genkyuzo, 3N) was used when it contains Mg, and CaS powder (Kojunto Kagaku Genkyuzo, 2Nup) was used when it contains Ca.
[0292] In addition, in Table 8, R represents at least one element selected from the group consisting of Na, K, Mg and Ca.
[0293]
[0294] From the results of Table 6, the sulfide-based solid electrolytes of Examples 1-1 to 1-3 all contained oxide anions with a Q0 structure in their crystal structure, resulting in a lithium ion conductivity that was higher after heat treatment than before heat treatment at 750°C for 30 minutes. Among them, in Examples 1-2 and 1-3, in which the agirodite-type crystal contained Cl and Br as Ha and the ratio was adjusted to a desirable range, the lithium ion conductivity after heat treatment was particularly high.
[0295] In addition, from the results of Table 7, the lithium ion conductivity was further improved in the sulfide-based solid electrolytes of Examples 2-1, 2-2, and 2-3, which were subjected to heat treatment at 450°C for 60 minutes on the sulfide-based solid electrolytes of Examples 1-1, 1-2, and 1-3. That is, it is presumed that the heat treatment yields both effects of improving bulk ion conductivity and reducing grain boundary resistance. Furthermore, from the results of charge-discharge tests using all-solid-state lithium-ion secondary batteries containing the sulfide-based solid electrolytes of Examples 2-1, 2-2, and 2-3, it was confirmed that Examples 2-1, 2-2, and 2-3 all had high capacity retention values and excellent cycle characteristics. Among them, in the sulfide-based solid electrolytes of Examples 2-2 and 2-3, in which the agirodite-type crystal contains Cl and Br as Ha and the ratio is adjusted to a desirable range, the cycle characteristics were particularly excellent.
[0296] In addition, from the results of Table 8, it was confirmed that even when the sulfide-based solid electrolyte contains R, the lithium ion conductivity after heat treatment at 650°C for 30 minutes is greater than before, and stability at high temperatures is improved, just as in the case where R is not included.
[0297] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese patent application filed on July 7, 2020 (Japanese Patent Application No. 2020-117194), Japanese patent application filed on October 13, 2020 (Japanese Patent Application No. 2020-172693), and Japanese patent application filed on May 21, 2021 (Japanese Patent Application No. 2021-086406), the contents of which are incorporated herein by reference.
Claims
Claim 1 A sulfide-based solid electrolyte used in a lithium-ion secondary battery comprises a crystalline phase and an anion present in the crystal structure of the crystalline phase, wherein the crystalline phase comprises an agirodite-type crystal comprising Li, P, S, and Ha, wherein Ha is at least one element selected from the group consisting of F, Cl, Br, and I, wherein the anion comprises an oxide anion having a Q0 structure having an MO bond formed by the combination of M and O, wherein M is at least one element selected from the group consisting of metallic elements and metalloid elements of groups 2 to 14 of the periodic table, and the ratio of the content (at%) of the element included in the agirodite-type crystal is Li a -PS b -Ha c When represented as, 5 <a≤6, 4<b<6 또한 1≤c<2의 관계를 만족시키는, 황화물계 고체 전해질. Claim 2 A sulfide-based solid electrolyte according to claim 1, wherein the content (at%) of each element satisfies the relationship {(M+O) / (Li+P+S+Ha+M+O)}≤0.
2. Claim 3 delete Claim 4 A sulfide-based solid electrolyte according to claim 1 or 2, wherein the sum of the content of the elements Li, P, S, Ha, M and O is 90 mass% or more. Claim 5 A sulfide-based solid electrolyte according to claim 1 or 2, wherein M constituting the oxide anion comprises at least one element selected from the group consisting of Si, Al, Zr, and B. Claim 6 A sulfide-based solid electrolyte according to claim 1 or 2, satisfying the following relationship when using the content (at%) of each element, α=(Li+P+S+Ha), β=(Si+Al+Zr+B+O), and γ=(Ha / P): 0<{β / (α+β)}<(D+0.1)D=(0.1104×γ -0.1133) Claim 7 A sulfide-based solid electrolyte according to claim 1 or 2, wherein the Ha comprises Cl and Br, and if the content of Cl in the agirodite-type crystal is x (at%) and the content of Br is y (at%), then (x / y) is 0.1 or more and 10 or less. Claim 8 In claim 1 or 2, the Ha comprises Cl and Br, and the ratio of the content (at%) of the elements included in the agirodite-type crystal is Li a -PS b -Cl c1 -Br c2 A sulfide-based solid electrolyte in which, when expressed as such, c1 is 0.1 or more and 1.5 or less, and c2 is 0.1 or more and 1.9 or less. Claim 9 In claim 1 or 2, the agirodite-type crystal comprises at least one element selected from the group consisting of Na, K, Mg, and Ca represented by R, and the ratio of the content (at%) of the element included in the agirodite-type crystal is Li a1 -R a2 -PS b -Ha c A sulfide-based solid electrolyte in which a2 is 0.001 to 0.4 when expressed as . Claim 10 A sulfide-based solid electrolyte having a capacity retention rate of 80% or more, expressed by the following formula, when a full-solid-state lithium-ion secondary battery is manufactured by the method described below and a charge-discharge test is performed in accordance with claim 1 or 2. (Method) (Manufacturing of positive electrode composite) As a positive electrode active material, layered rock salt type LiCoO2 powder (volume average particle size: 10㎛) coated with LiNbO3 with a thickness of 7 nm is used, and a positive electrode composite is manufactured by mixing 35 parts of the sulfide-based solid electrolyte, 60 parts of the positive electrode active material, and 5 parts of a conductivity aid (acetylene black, manufactured by Denka Co., Ltd., HS100). The thickness of the above LiNbO3 coating is determined by transmission electron microscopy (TEM) observation. (Fabrication of an all-solid-state lithium-ion secondary battery) 80 mg of the above sulfide-based solid electrolyte is poured into a plastic cylinder with a diameter of 10 mm and pressure-molded to form a solid electrolyte layer. Subsequently, 10 mg of the above positive electrode composite is poured into the cylinder and pressure-molded again to form a positive electrode layer. In addition, indium foil and lithium foil are poured from the opposite side of the above positive electrode composite to form a negative electrode layer. In this way, an all-solid-state lithium-ion secondary battery is fabricated, and a charge-discharge test is performed at a confining pressure of 10 kN. (Charge-discharge test) Using the above all-solid-state lithium-ion secondary battery, a constant current charge-discharge test is performed for 100 cycles at 25°C with a charge-discharge current density of 0.1 C and a charge-discharge potential range of 1.9-3.7 V. From the results of the charge / discharge test, the capacity retention rate (%) is calculated using the following formula. Capacity retention rate (%) = (Discharge capacity at the 100th cycle / Discharge capacity at the 1st cycle) × 100 Claim 11 A sulfide-based solid electrolyte according to claim 1 or 2, wherein when a lithium-ion secondary battery comprising a solid electrolyte layer including the sulfide-based solid electrolyte is charged or discharged, an oxide layer is formed at the interface between the solid electrolyte layer and the positive electrode layer. Claim 12 A lithium-ion secondary battery comprising a sulfide-based solid electrolyte as described in claim 1 or 2. Claim 13 A method for manufacturing a sulfide-based solid electrolyte used in a lithium-ion secondary battery as described in claim 1, comprising mixing raw materials including Li, P, S, and Ha and crystallizing by heating to obtain an agrodite-type crystal; obtaining a mixture by mixing an oxide having an MO bond formed by combining M and O with the agrodite-type crystal; and performing heat treatment of the mixture to obtain an agrodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure, wherein Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table, and comprising an agrodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure. Claim 14 A method for manufacturing a sulfide-based solid electrolyte used in a lithium-ion secondary battery as described in claim 1, comprising: mixing raw materials including Li, P, S, and Ha with an oxide having an MO bond formed by the combination of M and O to obtain a raw material composition; and performing heat treatment on the raw material composition to obtain an agirodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure, wherein Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table, and comprising an agirodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure. Claim 15 A method for manufacturing a sulfide-based solid electrolyte used in a lithium-ion secondary battery as described in claim 1, comprising: reacting raw materials including Li, P, S, and Ha to obtain an intermediate product; mixing the intermediate product with an oxide having an MO bond formed by the combination of M and O to obtain a mixture; and performing heat treatment on the mixture to obtain an agirodite-type crystal having an oxide anion having a Q0 structure with an MO bond in the crystal structure, wherein Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table, and comprising an agirodite-type crystal having an oxide anion having a Q0 structure with an MO bond in the crystal structure. Claim 16 A method for manufacturing a sulfide-based solid electrolyte used in a lithium-ion secondary battery as described in claim 1, comprising mixing raw materials including Li, P, S, and Ha and crystallizing by heating to obtain an agirodite-type crystal; obtaining a composition including an oxide anion having a Q0 structure having an MO bond formed by combining M and O; obtaining a mixture by mixing the agirodite-type crystal and the composition; and performing heat treatment of the mixture to obtain an agirodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure, wherein Ha is at least one element selected from the group consisting of F, Cl, Br, and I, and M is at least one element selected from the group consisting of metal elements and metalloid elements of groups 2 to 14 of the periodic table, and comprising an agirodite-type crystal having an oxide anion having a Q0 structure having an MO bond in the crystal structure. Claim 17 A method for manufacturing a sulfide-based solid electrolyte, wherein, in any one of claims 13 to 16, the heat treatment is performed at a temperature of 500°C or higher.
Citation Information
Patent Citations
Solid Electrolyte, Method for Preparing the Same and All Solid Battery Compring the Same
KR101952196B1
Ion-conducting compounds and related uses
KR1020200000849A