High-durability polyurea composition having a dynamic hydrogen bond-based self-healing function and a polyurea resin film waterproofing material using the same, and a method for manufacturing the same

A self-healing polyurea composition with quadruple hydrogen bonding and hybrid nano-filler addresses the limitations of conventional polyurea by providing high strength, elongation, and ambient self-repair, enhancing structural durability and reducing maintenance.

KR103043903B1Active Publication Date: 2026-11-06KYUNGSHIN CONSTRUCTION LINE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020260132688
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-06
Estimated Expiration
2046-07-20

AI Technical Summary

Technical Problem

Conventional polyurea waterproofing materials suffer from irreversible covalent bonds that fracture under stress, leading to permanent damage, and lack the ability to self-heal under ambient conditions, while existing self-healing technologies compromise mechanical strength or adhesion.

Method used

A self-healing polyurea composition with quadruple hydrogen bonding units and hybrid nano-filler, allowing for reversible bonding and stress dispersion, applied via high-pressure mixing to form a dynamic network that self-repairs at room temperature.

Benefits of technology

The composition achieves high tensile strength, elongation, and self-healing capabilities, preventing crack propagation and maintaining structural integrity without artificial stimulation, reducing maintenance costs and extending the lifespan of civil engineering structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026087799664-PAT00001_ABST
    Figure 112026087799664-PAT00001_ABST
Patent Text Reader

Abstract

The present invention discloses a high-performance polyurea technology that forms a waterproof film with significantly improved mechanical properties and crack-following properties, while exhibiting permanent and reversible self-healing efficiency under ambient (RT) atmospheric conditions where external artificial stimuli are excluded. The self-healing polyurea composition according to the present invention comprises: a main component (100) comprising a reversible prepolymer (110) having a urea-dopyrimidinone (UPy)-based quadruple hydrogen bond head unit (112) attached to a terminal or side chain, and a hybrid nanofiller (120) in which an amino surface-modified silica nanoparticle (121) and a carbon-based reinforcing agent (122) are combined; and a curing agent component (200) comprising an aliphatic isocyanate trimer (210). The composition of the present invention is applied by high-speed spraying on the surface of a structural substrate (410) through a high-pressure spray mixing device (500) to form a coating film (300) based on a three-dimensional dynamic reversible network, and when a strong external force is applied, the quadruple hydrogen bond acts as a sacrificial bond to dissipate stress, and when damage to the coating film occurs, it restores more than 90% of its initial strength within 24 hours by simply leaving it at room temperature, thereby completely sealing and blocking dynamic behavior cracks in the lower part, ensuring long-term permanent waterproofing reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to high-performance coating material technology for waterproofing, corrosion protection, and crack control of civil engineering and building structures. More specifically, it relates to a self-healing polyurea composition, a main component intermediate composition, a coating structure formed therefrom, a method of construction therefrom, and a waterproofing system for concrete structures including the same, wherein the elongation at break and tensile strength caused by external movement are dramatically improved by providing a matrix in which a dynamic reversible quadruple hydrogen bond unit exhibiting permanent and repetitive room-temperature self-healing performance and an organic-inorganic hybrid nano-filler for stress dispersion are compositely cross-linked, thereby perfectly following micro-cracks in the underlying concrete structure and self-repairing in an ambient air environment without separate artificial stimulation when damage occurs.

[0002] The polyurea according to the present invention can be used in various ways, such as in concrete and steel structures, steel bridges, roofs, reservoirs, water purification plants, water treatment structures, roofs, parking lots, rooftops, and walls. Background Technology

[0003] In general, microcracks inevitably occur in concrete structures over time due to various environmental factors, such as external loads, ground settlement, thermal shrinkage and expansion caused by climate change, drying shrinkage, and carbonation caused by the infiltration of atmospheric carbon dioxide. Cracks in concrete structures not only cause a decrease in structural strength but also lead to exposure to rainwater, groundwater, and chloride ions (Cl - It provides a direct route for harmful factors such as ) to penetrate into the interior of the structure. The moisture and harmful factors that penetrate into the interior promote the corrosion of reinforcing steel and cause internal volume expansion, which further accelerates cracking in the concrete, ultimately causing serious problems that lead to the collapse or shortening of the lifespan of architectural and civil engineering structures.

[0004] To address these issues, various waterproofing and coating application methods have been applied to completely block moisture ingress into the surface of concrete structures. Existing waterproofing methods include sheet waterproofing, membrane waterproofing, and composite waterproofing. In particular, the polyurea membrane waterproofing method, which forms a film within seconds by spraying the main component and hardener component at ultra-high pressure using a spray gun on-site, is widely utilized. Conventional polyurea is based on strong urea covalent bonds formed by nucleophilic addition reactions between isocyanate and amine functional groups; therefore, it has the advantage of excellent tensile strength and a fast curing speed, allowing for the formation of a seamless continuous film even on vertical walls or structures with complex shapes.

[0005] However, these conventional general polyurea film waterproofing materials have the following fatal inherent limitations.

[0006] First, conventional polyureas form a three-dimensional cross-linked network structure composed solely of irreversible covalent bonds. Although a covalent matrix with a high cross-linking density may exhibit excellent initial mechanical strength, it undergoes a fracture phenomenon in which the molecular chains themselves are permanently destroyed if strong stress is applied locally or if the range of structural behavior exceeds the design threshold. Once the covalent main chain breaks and macroscopic cracks occur in the film, the structure cannot return to its original state on its own due to the irreversible nature of the polymer chains; consequently, microscopic damage rapidly propagates into large tears or interfacial delamination due to stress concentration.

[0007] Second, structural cracks in civil engineering and construction sites are not static but repeatedly exhibit 'dynamic movement,' constantly expanding and closing due to seasonal daily temperature fluctuations and vibrations caused by subway or vehicle traffic. Even if conventional polyureas possess a certain level of elongation properties, the accumulation of repetitive fatigue loads leads to the formation of micro-voids and cracks within the matrix, resulting in permanent deformation; furthermore, it is difficult to control so-called reflective cracking, where the coating ruptures along with the underlying concrete when it cracks.

[0008] Third, when damage or fracture occurs in the membrane waterproofing material, conventional maintenance methods have relied on an artificial repair process involving cutting the damaged area with a knife, grinding the surface, and reapplying the waterproofing material. However, access to underground structures, bridge decks, tunnel interiors, and the backs of structural walls is extremely limited, making it nearly impossible to detect damage visually at an early stage. By the time leakage becomes noticeable, internal rebar corrosion and concrete deterioration have already progressed severely, resulting in astronomical repair costs. Furthermore, a vicious cycle repeats as the adhesion between the reapplied waterproofing material and the existing material deteriorates, causing interfacial delamination to occur again.

[0009] To overcome this, research on self-healing polymers capable of self-healing damage has recently been actively conducted in academia and industry. Early self-healing technologies involved dispersing microcapsules containing healing substances within a matrix; however, this capsule method had a critical limitation: once a capsule was destroyed by external stimuli and the healing substance leaked out, repeated healing became impossible if damage occurred again in the same area.

[0010] As an alternative, a technique was proposed to introduce dynamic reversible bonds into the polymer chains themselves, allowing for reversible attachment and detachment at room temperature. However, this approach also came with limitations that made field application impossible in massive civil structures or climate-exposed environments, such as the fact that recovery only occurs upon applying heat (thermally reversible Diels-Alder reaction), irradiating with ultraviolet light, or introducing specific metal ions.

[0011] Furthermore, when simple double or triple hydrogen bonds that spontaneously detach and reattach at room temperature are introduced, while self-healing efficiency may be improved to some extent, the bond energy is too low, leading to a trade-off dilemma where mechanical properties such as tensile strength, adhesion strength, and elastic modulus—basic performance required for waterproofing materials—are significantly degraded compared to general-purpose products. Civil engineering waterproofing films must possess a strong tensile strength of at least 15 MPa and interfacial adhesion of several MPa or more, while also having an elongation of over 400%; however, it was technically impossible to simultaneously achieve these conflicting properties (high strength / high elongation / reversible self-healing at room temperature) using existing dynamic bonding technologies. Prior art literature

[0012] Korean Registered Patent KR 10-1451974 B1 Korean Registered Patent KR 10-2087093 B1 The problem to be solved

[0013] The present invention has been devised to overcome the various problems and technical limitations of the aforementioned prior art, and the main technical problem that the present invention aims to solve is as follows.

[0014] First, by designing a unique prepolymer in which quadruple hydrogen bonding units based on urea-dopyrimidinone (UPy), which has very high bonding energy, are introduced in precise equivalents at the ends of the linear, flexible polyetheramine molecular main chain, we aim to provide a unique, infinitely repeatable self-healing polyurea composition that self-repairs broken interfaces and reforms reversible bonds even under ambient (RT) atmospheric conditions where external stimuli (heat, UV rays, chemicals, etc.) are entirely excluded.

[0015] Second, to solve the problem of 'low mechanical strength and stress reduction,' which is a chronic weakness of polymer matrices with dynamic reversibility, we intend to realize a high-strength / high-elongation organic-inorganic composite crosslinked network film that physically blocks the tip propagation of microcracks and dissipates stress when tensile stress is applied by mutually hybridizing spherical nano-silica particles with surfaces chemically modified with reactive amine groups and carbon-based plate-like reinforcing materials and embedding them in a matrix structure with ultra-high dispersion.

[0016] Third, we aim to provide an optimal mixing process and a composition of intermediate raw materials for the main component that can perfectly satisfy the process margins (ultra-high pressure collision mixing speed, prevention of nozzle clogging, etc.) of a high-pressure spray device used during on-site construction, and form a coating film of uniform thickness without dripping through an ultra-high-speed gelation reaction when sprayed on vertical walls or inclined surfaces.

[0017] Fourth, we aim to provide a high-performance composite waterproofing system for civil engineering and construction and a method for constructing the same, which forms a silane coupling cross-linking bond capable of completely preventing interfacial demolding and delamination with the concrete structure substrate, and is equipped with an infrastructure that prevents yellowing and deterioration of the polymer main chain due to UV exposure in an outdoor environment, thereby simultaneously securing crack bridging performance that stretches without fracture and long-term permanent waterproofing performance in response to large-scale behavior of the concrete substrate.

[0018] The polyurea according to the present invention can be used in various ways, such as in concrete and steel structures, steel bridges, roofs, reservoirs, water purification plants, water treatment structures, roofs, parking lots, rooftops, and walls. means of solving the problem

[0019] The first objective of the present invention can be achieved as a dynamic hydrogen bond-based self-healing polyurea composition comprising: a main component (100) comprising a reversible hydrogen-bonded polyetheramine prepolymer (110) having a ureidopyrimidinone (UPy) unit (112) bonded to a terminal or side chain and a hybrid functional nanofiller (120); and a curing agent component (200) comprising an aliphatic isocyanate trimer (210), wherein the main component (100) and the curing agent component (200) are mixed to exhibit room temperature self-healing properties.

[0020] The above-mentioned reversible hydrogen-bonded polyetheramine prepolymer (110) may be characterized by being synthesized by in-situ reaction in a ratio selected in the range of 1:0.05 to 1:0.25 for the reaction molar ratio of the amine group (-NH2) of the difunctional or trifunctional polyetheramine subcomponent (111) having a molecular weight of 2,000 to 4,000 g / mol to the isocyanate group (-NCO) of the UPy-NCO unit (112).

[0021] The above hybrid functional nanofiller (120) may be characterized by being composed of amino surface-modified silica nanoparticles (121) having an average particle size of 10 to 50 nm and having amine functional groups grafted on their surface; and graphene oxide or carbon-based reinforcing material (122) having a plate-like structure, mixed in a weight ratio of 1:0.1 to 1:0.5.

[0022] The above curing agent part (200) may be characterized by comprising 75 to 85 parts by weight of an aliphatic isocyanate trimer (210) which is a hexamethylene diisocyanate trimer (HDI trimer); and 15 to 25 parts by weight of a diisocyanate oligomer (220) for inducing reversible urea binding.

[0023] The above main component (100) may be characterized by including 1.0 to 10.0 parts by weight of the hybrid functional nano filler (120) relative to 100 parts by weight of the above prepolymer (110).

[0024] The above main component (100) may further comprise 0.5 to 3.0 parts by weight of an interfacial adhesion-promoting silane coupling agent (130) composed of epoxysilane or isocyanatesilane; and 0.1 to 1.0 parts by weight of a hindered amine light stabilizer (HALS) and a benzotriazole-based UV blocker (140).

[0025] The above main component (100) and hardener component (200) may be characterized by being colliding and mixed in a volume ratio of 1:1 by a high-pressure spray mixing device (500) during on-site construction.

[0026] The second objective of the present invention can be achieved as a self-healing polyurea waterproofing material intermediate composition comprising: a reversible hydrogen-bonded polyetheramine prepolymer (110) which is individually packaged or distributed as a raw material before reacting with a curing agent part (200), has a urea-dopyrimidinone (UPy) ring that induces quadruple hydrogen bonding at the end, and has a residual reactive amine group (-NH2) in the inner molecular main chain; and a hybrid functional nanofiller (120) comprising amino surface-modified silica nanoparticles (121) and carbon-based reinforcing material (122) ultrasonically dispersed in a liquid matrix of the prepolymer (110).

[0027] The residual reactive amine group (-NH2) in the above prepolymer (110) may be characterized by having a chemical equivalent that can cause a room temperature ultra-fast urea reaction when mixed in a volume ratio with the isocyanate group (-NCO) of the curing agent part (200).

[0028] The above-mentioned hybrid functional nano filler (120) may be included in a range of 1.0 to 10.0 parts by weight relative to 100 parts by weight of the above-mentioned prepolymer (110), and may be characterized by maintaining dispersion phase stability under high-speed shear force conditions by a homo mixer and an ultrasonic disperser.

[0029] The carbon-based reinforcing material (122) may be characterized by comprising at least one of a graphene oxide sheet and a single-walled or multi-walled carbon nanotube (CNT).

[0030] It can be characterized as a liquid form that is solvent-free through vacuum distillation and does not emit volatile organic compounds (VOCs).

[0031] It may be characterized by further including 0.5 to 3.0 parts by weight of epoxysilane or isocyanatesilane (131) to induce chemical covalent bonding with the substrate.

[0032] A third objective of the present invention can be achieved as a self-healing polyurea film structure that exhibits self-healing efficiency when left at room temperature after cutting damage by having a three-dimensional dynamic reversible network structure comprising: a hard segment crosslinking node comprising a hard molecular axis derived from an aliphatic isocyanate trimer (210) and a diisocyanate oligomer (220); a polyetheramine prepolymer (110) main chain connecting the crosslinking nodes by covalent bonds; a quadruple hydrogen bond axis (112) capable of reversibly detaching at room temperature between ureadopyrimidinone (UPy) units located at the ends or side chains of the main chain; and an amino surface modified silica nanoparticle (121) filled between the main chains and forming an interfacial bond with the polymer matrix through surface amine groups.

[0033] The above quadruple hydrogen bond axis (112) may be characterized by preferentially dissociating as a sacrificial bond prior to the breakdown of the covalent main chain when external tensile stress is applied, thereby relieving stress.

[0034] The above amino surface-modified silica nanoparticles (121) may be characterized by physically blocking and deflecting the leading edge propagation path of microcracks penetrating into the matrix.

[0035] The above quadruple hydrogen bond axis (112) may be characterized by having reversibility that spontaneously re-bonds under ambient temperature (25°C) atmosphere after undergoing a rearrangement step due to the molecular mobility of the polyetheramine main chain upon release of external stress.

[0036] It can be characterized by exhibiting high elongation characteristics in which the initial tensile strength in the final hardened state is 18.0 to 23.0 MPa and the initial elongation at break is maintained in the range of 400% to 500%.

[0037] The fourth objective of the present invention is a step (S100) of synthesizing an UPy-NCO unit (112) having an isocyanate group at the terminal end by reacting 6-methylisocytosine and an aliphatic diisocyanate compound under a nitrogen atmosphere; and a step (S200) of manufacturing a main component (100) by in situ synthesizing a reversible hydrogen-bonded polyetheramine prepolymer (110) by stirring the synthesized UPy-NCO unit (112) and a polyetheramine subcomponent (111) at 60°C, and adding a hybrid functional nanofiller (120) to the mixture and performing high-speed shear dispersion. A method for constructing a self-healing polyurea film can be achieved by comprising: a step (S300) of high-pressure impact mixing of the above-manufactured main component (100) and a curing agent component (200) including an aliphatic isocyanate trimer (210) in a volume ratio of 1:1 under a pressure of 2,000 to 3,500 psi and a temperature of 60 to 70°C using a high-pressure spray mixing device (500); and a step (S400) of forming a self-healing polyurea film (300) based on a three-dimensional dynamic reversible network by spraying and applying the impact-mixed composite liquid composition onto the surface of a concrete structure substrate (410) through ultra-high-speed curing at room temperature.

[0038] The step (S100) of synthesizing the above UPy-NCO unit (112) may be characterized as a process of heating and stirring for 4 to 6 hours under constant temperature conditions of 70°C to 90°C.

[0039] The step (S200) of manufacturing the above main component (100) may be characterized by including a process of shear dispersion at a rotational speed of 3,000 rpm or more by simultaneously operating a homo mixer and an ultrasonic disperser to prevent aggregation of silica nanoparticles (121) and carbon-based reinforcing material (122) within a polymer matrix.

[0040] The collision mixing of the above S300 step may be characterized by being performed instantaneously within a mixing chamber inside a dedicated spray gun.

[0041] The composite liquid composition sprayed in the above spray application step (S400) may be characterized by undergoing a gelation step in which it loses fluidity within 5 to 15 seconds after settling on the concrete structure substrate (410), thereby controlling sagging during vertical wall construction.

[0042] After the above spraying application step (S400), the method may further include a step of additionally curing for 24 hours at room temperature (25℃) to fully stabilize the trimer crosslinked framework and the UPy tetrahydrogen bonded dimer stationary phase.

[0043] In the step (S200) of manufacturing the above main part (100), an epoxy or isocyanate silane (131) may be mixed to provide chemical adhesion that suppresses interfacial peeling with the surface of the concrete structure substrate (410) when the final coating is formed.

[0044] The fifth objective of the present invention can be achieved as a concrete structure waterproofing system comprising: a concrete structure substrate (410) forming a crack control target surface due to behavior and environmental stress; a self-healing polyurea film (300) that is closely laminated to the upper surface of the concrete structure substrate (410) and is formed by high-pressure impact mixing spraying, having an aliphatic trimer covalent crosslinked framework, reversible UPy quadrivalent hydrogen bonds, and amino-modified silica filler mutually infiltrated inside; and an interface adhesion-promoting silane coupling agent (130) bonding layer existing between the adhesive interface of the concrete structure substrate (410) and the self-healing polyurea film (300), which chemically fixes both interfaces through a reactor of epoxy or isocyanate silane (131); wherein the film (300) exhibits crack bridging characteristics in which it is stretched without fracture in response to the width deformation of microcracks occurring in the concrete structure substrate (410).

[0045] The above self-healing polyurea coating (300) may be characterized by relieving and dissipating stress without permanent destruction for micro-crack behavior of 2.0 mm or less occurring in the above concrete structure substrate (410).

[0046] The self-healing polyurea film (300) may be characterized by containing a complex of hindered amine light stabilizer and UV blocker (140) to prevent reversible hydrogen bonding degradation in an environment where it is constantly exposed to the outside.

[0047] The self-healing polyurea film (300) may be characterized by having a top-coat protective layer additionally laminated with a thickness thereon to provide wear resistance and prevent external contamination.

[0048] After foreign substances and laitance present on the surface of the above concrete structure substrate (410) are removed, the self-healing polyurea coating film (300) is uniformly applied by a high-pressure spray mixing device (500) in a thickness range of 2.0 to 3.0 mm to form an upper surface waterproof barrier layer. Effects of the invention

[0049] The dynamic hydrogen bond-based self-healing polyurea composition according to the present invention, the coating structure formed therefrom, and the waterproofing system exhibit the following remarkable and unique effects compared to conventional general waterproofing materials.

[0050] First, it offers room-temperature self-healing capabilities without artificial stimulation and a significant reduction in maintenance costs. Due to the room-temperature dynamic reversibility between UPy units forming quadruple hydrogen bonds, the present invention allows the coating film to perfectly restore more than 90% (up to 96.2%) of its initial mechanical properties within 24 hours simply by being left at room temperature, without any artificial measures such as heat treatment, light irradiation, or catalyst injection, even if micro-cracks or cut damage occur. Accordingly, when applied to underground structures or tunnels where visual inspection or access is impossible, it maintains a permanent waterproof barrier, thereby fundamentally reducing post-maintenance costs to zero.

[0051] Second, the trade-off limit between mechanical strength and self-healing performance was completely overcome. By introducing functional nanofillers hybridized with amino surface-modified silica nanoparticles and graphene oxide / CNT reinforcement, the strength of the flexible dynamically reversible polymer matrix was dramatically reinforced, exhibiting ultra-high tensile strength of 18.0 to 23.0 MPa while simultaneously maximizing the elongation at break to the 400% to 500% range. When external force is applied, quadruple hydrogen bonds act as sacrificial bonds to absorb and disperse energy first, thereby dramatically improving the structural lifespan of the coating film.

[0052] Third, it achieves a reflective crack prevention effect through excellent crack bridging performance. Even if the underlying concrete structure substrate separates due to dynamic load or shrinkage and cracks up to 2.5 mm wide occur, the coating structure of the present invention flexibly stretches without interfacial delamination or accompanying tearing to tightly seal the upper part of the crack. Subsequently, when the structural stress is released and the crack closes again, the coating also elastically restores and perfectly bonds the internal micro-pores at room temperature, thereby protecting the long-term durability of the structure.

[0053] Fourth, it provides on-site construction stability and environmental friendliness. The main component intermediate and the entire composition of the present invention are designed as a solvent-free type, so they are environmentally friendly as they do not emit harmful volatile organic compounds (VOCs) during construction. Furthermore, they are uniformly collided and mixed inside a high-pressure spray gun under a pressure of 2,000 to 3,500 psi, and ultra-high-speed gelation is completed within 5 to 15 seconds after spraying, which is highly advantageous for shortening on-site construction time and forming a high-quality coating film.

[0054] Meanwhile, the effects obtainable from the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by those skilled in the art to which the present invention belongs from the description below. Brief explanation of the drawing

[0055] The following drawings attached to this specification illustrate preferred embodiments of the present invention and serve to further enhance understanding of the technical concept of the present invention together with the detailed description of the invention; therefore, the present invention should not be interpreted as being limited only to the matters described in such drawings. Fig. 1 This is a process flowchart illustrating a method for manufacturing and constructing a dynamic hydrogen bond-based self-healing polyurea composition according to one embodiment of the present invention. Fig. 2This is a system structure block diagram showing the main upper and lower components of a self-healing polyurea film waterproofing system according to one embodiment of the present invention. Fig. 3 This is a composite structural diagram visualizing a composite cross-linked network structure inside a coating film formed by ultra-high pressure collision mixing of an aliphatic isocyanate trimer (curing agent part), a hydrogen-bonded prepolymer, and a functional nano filler (main part) by a high-pressure spray device according to one embodiment of the present invention. Fig. 4 This is a schematic diagram of a dynamic self-healing mechanism in which quadruple hydrogen bonds between UPy units in a polyurea film according to one embodiment of the present invention dissociate into sacrificial bonds under conditions of external stress application, and then spontaneously re-bond at room temperature upon stress release. Fig. 5 This is a chemical reaction scheme representing the process of pre-preparing a reversible hydrogen-bonded prepolymer by the nucleophilic addition reaction of a UPy-NCO unit and a polyetheramine subcomponent used in one embodiment of the present invention. Fig. 6 This is a graph of the results of a physical property evaluation showing the recovery tendency of the stress-strain curve after artificial cutting damage of a self-healing polyurea film according to one embodiment of the present invention and after the passage of time at room temperature. Fig. 7 This is a schematic diagram of a macroscopic construction cross-section showing, over time, the crack-following phenomenon in which a self-healing polyurea film according to one embodiment of the present invention stretches without fracture and the room temperature self-healing stage as cracks occur and close in the substrate of the lower concrete structure. Specific details for implementing the invention

[0056] The above objects, other objects, features, and advantages of the present invention will be easily understood through the following preferred embodiments associated with the accompanying drawings. However, the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosed content is thorough and complete and to ensure that the spirit of the invention is sufficiently conveyed to a person skilled in the art.

[0057] In this specification, when a component is described as being on another component, it means that it may be formed directly on the other component or that a third component may be interposed between them. Also, in the drawings, the thicknesses of the components are exaggerated for the effective description of the technical content.

[0058] The embodiments described herein will be explained with reference to cross-sectional and / or plan views, which are exemplary illustrations of the invention. In the drawings, the thicknesses of films and regions are exaggerated for effective explanation of the technical content. Accordingly, the shapes of the exemplary drawings may be modified by manufacturing techniques and / or tolerances, etc. Accordingly, the embodiments of the invention are not limited to the specific shapes depicted but include variations in shape produced according to the manufacturing process. For example, a region depicted as a right angle may be rounded or have a certain curvature. Accordingly, the regions illustrated in the drawings have properties, and the shapes of the regions illustrated in the drawings are intended to illustrate specific shapes of the regions of the device and are not intended to limit the scope of the invention. Although terms such as first, second, etc., have been used to describe various components in the various embodiments of this specification, these components should not be limited by such terms. These terms are used merely to distinguish one component from another. The embodiments described and illustrated herein also include their complementary embodiments.

[0059] The terms used herein are for describing the embodiments and are not intended to limit the invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used herein, 'comprises' and / or 'comprising' do not exclude the presence or addition of one or more other components to the mentioned components.

[0060] In describing the specific embodiments below, various specific details have been included to explain the invention more specifically and to aid understanding. However, a reader with sufficient knowledge in the art to understand the invention will recognize that it can be used without these various specific details. In some cases, it is noted in advance that commonly known aspects that are not significantly related to the invention have been omitted to prevent unnecessary confusion in describing the invention.

[0062] Fig. 1 This is a process flowchart that systematically shows the overall manufacturing process and construction steps of a dynamic hydrogen bond-based self-healing polyurea composition according to one embodiment of the present invention.

[0063] Fig. 2 This is a composite structure drawing of a raw material supply section, a mixing and application section, and a final internal network, showing the entire process in which a main component (100) and a curing agent section (200) are collided and mixed through a high-pressure spray mixing device (500) according to one embodiment of the present invention, and then sprayed onto the surface of a concrete structure substrate (410) to finally form a self-healing polyurea film (300) having a reversible dynamic network structure inside.

[0065] The self-healing polyurea composition according to the present invention is largely composed of a main component (100, liquid A) and a curing agent component (200, liquid B), and is characterized by the fact that these are collide-mixed through a high-pressure spray mixing device (500) to form a self-healing polyurea film (300).

[0066] Hereinafter, all components for implementing the present invention are subdivided into sub-concepts and described in detail.

[0067] The main component (100) is a mixture of liquid components that impart flexibility, high elongation characteristics, and dynamic self-healing performance to the final coating.

[0068] Reversible hydrogen-bonded polyetheramine prepolymer (110) As a core component of the present invention, it is a reversible dynamic bonding structure in which a soft segment of the polyetheramine series having an amino group at the end and a ureadopyrimidinone isocyanate (UPy-NCO) unit having a quadruple hydrogen bonding functional group are chemically pre-bonded.

[0069] Polyetheramine subcomposition (111) One or more selected from the group consisting of polypropylene glycol diamine (e.g., Jeffamine D-2000, D-4000) having a molecular weight in the range of 2,000 to 4,000 g / mol or trifunctional amine-terminated oligomer (PTMEG-based amine-terminated oligomer, e.g., Jeffamine T-3000) having a molecular weight in the range of 3,000 to 5,000 g / mol are used. If the molecular weight is less than 2,000, the flexibility and elongation of the coating film decrease, and if it exceeds 4,000, the viscosity increases excessively, resulting in reduced sprayability.

[0070] UPy-NCO unit subconfiguration (112) It is a mono-isocyanate functionalized 2-ureado-4[1H]-pyrimidinone structure synthesized by reacting 6-methylisocytosine and a diisocyanate (e.g., hexamethylene diisocyanate, HDI) in a molar ratio of 1:1 to 1:1.2.

[0071] Equivalent ratio and bonding structure The reaction molar ratio of the amine group (-NH2) of the polyetheramine subcomponent (111) to the isocyanate group (-NCO) of the UPy-NCO unit (112) is limited to a range of 1:0.05 to 1:0.25. Only when synthesized within this range can mechanical properties and self-healing power be simultaneously satisfied by introducing an optimal quadruple hydrogen bond network throughout the film while sufficiently maintaining the remaining amine group for film formation.

[0072] Hybrid functional nano filler (120) It is an organically modified nanoparticle designed to disperse external stress within a polyurea matrix and to absorb and block propagation energy at the crack tip.

[0073] Amino surface-modified silica nanoparticles (121) This involves reacting an aminosilane (e.g., APTES, 3-Aminopropyltriethoxysilane) with the surface of colloidal silica having an average particle size of 10 to 50 nm to introduce reactive amine groups to the surface. By forming covalent bonds with the isocyanate of the curing agent part (200), the filler is uniformly dispersed in nano-sized units within the matrix without aggregation.

[0074] Graphene oxide or carbon nanotube reinforcement (122) To further maximize shear stress and barrier properties, it may additionally include layered functionalized graphene oxide mixed with the silica nanoparticles (121) in a weight ratio of 1:0.1 to 1:0.5. This physically blocks moisture penetration pathways, thereby extending waterproof performance by more than twofold.

[0075] Interfacial adhesion-promoting silane coupling agent (130) It is a component that prevents interfacial peeling of the coating film by forming a chemical bond with hydroxyl groups (-OH) present on the surface of a concrete structure (410) or a metal substrate.

[0076] Epoxy or isocyanate silane (131) One or more selected from the group consisting of GPTMS (3-Glycidoxypropyltrimethoxysilane), amino silane, epoxy silane, and isocyanate silane are used, and are included in an amount of 0.5 to 3.0 parts by weight relative to 100 parts by weight of the total main component (100). If less than 0.5 parts by weight, the effect of improving adhesion is negligible, and if more than 3.0 parts by weight, the strength of the coating film may be reduced due to residual silane.

[0077] The light stabilizer and UV blocker (140) It includes HALS (Hindered Amine Light Stabilizer) and a benzotriazole-based ultraviolet absorber. Since the dynamic hydrogen bonding of the present invention can be affected by heat and light, it helps to maintain long-term self-healing persistence by suppressing the yellowing or decomposition of the hydrogen bonding unit (112) by ultraviolet light in an external exposure environment.

[0078] The polyurea according to the present invention can be used in various ways, such as in concrete and steel structures, steel bridges, roofs, reservoirs, water purification plants, water treatment structures, roofs, parking lots, rooftops, and walls.

[0080] The curing agent part (200) according to the present invention is a component that is mixed with the main part (100) to form a high-speed curing urea bond within a few seconds.

[0081] The aliphatic isocyanate trimer (210) is To ensure excellent weather resistance and prevent yellowing, a hexamethylene diisocyanate trimer (HDI trimer, isocyanurate type structure) is used as the base. It is preferable that the NCO content be in the range of 20 to 25%.

[0082] The reversible urea binding-inducing diisocyanate oligomer (220) is In addition to UPy quadruple hydrogen bonds within the matrix, it may include an isocyanate-modified oligomer capable of forming a hindered urea bond to form an additional self-healing axis.

[0084] S100 Step: Self-healing unit (UPy-NCO) pre-synthesis step

[0085] This step is a process of precisely synthesizing a ureidopyrimidinone-isocyanate (UPy-NCO) unit (112) having an isocyanate functional group at the end in the form of a solid or intermediate in advance, in order to permanently and stably introduce the reversible quadruple hydrogen bonding, which is the core identity of the present invention, into the coating film.

[0086] Specifically, a solid powder raw material of 6-methylisocytosine, which is a chemical self-healing active group, is introduced into a reactor, and then a corresponding diisocyanate compound is introduced in a measured amount such that their molar ratio is in the range of 1:1 to 1:1.2. At this time, the diisocyanate compound used is preferably selected from the group of aliphatic diisocyanates consisting of hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), or a mixture thereof, in order to ensure weather resistance of the final coating film and prevent yellowing.

[0087] This synthesis reaction is carried out inside a closed reactor in which an inert atmosphere is formed by nitrogen (N2) gas to thoroughly block external moisture ingress and side reactions of the isocyanate group. The reaction temperature is maintained within a constant range of 70°C to 90°C, and a continuous stirring reaction is carried out for 4 to 6 hours using an oil bath or jacket heating method. If the temperature is below 70°C, a large amount of unreacted raw material remains, causing the synthesis yield to drop sharply, and if it exceeds 90°C, thermal polymerization or gelation side reactions of the diisocyanate itself may occur.

[0088] When the reaction is complete, the reaction is confirmed by analyzing the free isocyanate (Free NCO) content, and then the residual solvent is removed by vacuum distillation, thereby obtaining an intermediate powder or high-concentration liquid of high-density quadruple hydrogen-bonded UPy-NCO units (112) that are white to pale yellow at room temperature.

[0090] S200 Step: Main component (100, Liquid A) mixing composition step

[0091] This step is a highly dispersed formulation process in which the UPy-NCO unit (112) obtained in the above S100 step is combined with a soft segment to form a reversible hydrogen-bonded polyetheramine prepolymer (110), and various nano fillers and additives are combined therewith to maximize mechanical properties and barrier performance to produce a liquid main component (100, liquid A) having a uniform phase.

[0092] First, a polyetheramine subcomponent (111) (e.g., a Jeffamine-based solvent-free liquid amine) comprising a difunctional polypropylene glycol diamine having a molecular weight of 2,000 to 4,000 g / mol or a trifunctional amine terminal oligomer having a molecular weight of 3,000 to 5,000 g / mol is introduced into a mixing tank as a base material to exhibit high molecular mobility (chain mobility) and high elongation characteristics. Subsequently, the UPy-NCO unit (112) synthesized in step S100 is introduced by precise control so that the reaction molar ratio of the terminal amine group (NH2) of the polyetheramine subcomponent (111) to the isocyanate group (NCO) of the UPy-NCO unit (112) is in the range of 1:0.05 to 1:0.25. Synthesis must be performed within this range to ensure sufficient residual amine groups to bond with the isocyanate curing agent when forming the final film, while also providing optimal reversible crosslinking points throughout the film. The mixture is subjected to a gentle stirring reaction for 2 hours at a temperature of about 60°C, during which reversible hydrogen-bonded polyetheramine prepolymer (110) chains are synthesized in-situ by the urea reaction between the amine groups and the isocyanate groups.

[0093] After that, a hybrid functional nanofiller (120) is introduced to structurally reinforce the matrix and block microcrack propagation. The nanofiller (120) is mainly composed of amino surface modified silica nanoparticles (121) having an average particle size of 10 to 50 nm and having reactive amine strands formed by chemically grafting aminosilane (APTES, etc.) onto the surface, and a plate-shaped graphene oxide or carbon-based reinforcing material (122) is mixed and introduced in a weight ratio of 1:0.1 to 1:0.5 to double the long-term moisture barrier properties and tensile strength.

[0094] In order to prevent the aggregation of nanoparticles at the source and achieve a complete nano-dispersion state, a homo-mixer and an ultrasonic dissipator are operated simultaneously in a mixing tank to apply a high-speed shear force of 3,000 rpm or more. At the same time, an interfacial adhesion-promoting silane coupling agent (130) [e.g., epoxy or isocyanate silane (131) such as GPTMS] is added in an amount of 0.5 to 3.0 parts by weight relative to 100 parts by weight of the total main component to dramatically improve adhesion with the concrete interface, and a light stabilizer and UV blocker (140) (HALS and benzotriazole-based composite) is added in a small amount to prevent hydrogen bond decomposition and yellowing caused by ultraviolet rays in an outdoor exposure environment and to provide long-term self-healing sustainability, thereby completing the dispersion mixing to complete the final stabilized main component (100, liquid A) liquid composition.

[0096] S300 Step: On-site application of membrane waterproofing material (spray application) Step

[0097] This step is an actual field construction process in which the liquid main component (100) manufactured through the above S200 step and the separately prepared isocyanate-based curing agent component (200, liquid B) are mixed at high speed using special construction equipment at the site, and at the same time applied to the surface of the concrete substrate with a uniform thickness.

[0098] The curing agent part (200, B liquid) supplied for construction contains an aliphatic isocyanate trimer (210) (HDI trimer, isocyanurate type) as the main component, which has low viscosity, excellent structural weather resistance, and can prevent yellowing, and is a composition in which a diisocyanate oligomer (220) for inducing reversible urea bonds that forms hindered urea bonds to introduce additional recovery axes is partially hybridized.

[0099] When constructing on-site, the main component (100) and the hardener component (200) are stored and transported through completely independent storage tanks and transport lines, respectively. Since general stirring mixing is impossible due to the unique ultra-high-speed curing characteristics of polyurea (gelation within seconds), a dedicated high-pressure spray mixing device (500) is essential in the present invention.

[0100] The main component (100) and the curing agent (200) transported through each line come into high-pressure contact with each other in a volume ratio of exactly 1:1 in the mixing chamber inside the spray gun of the high-pressure spray mixing device (500). At this time, the applied process pressure is in the ultra-high pressure range of 2,000 to 3,500 psi, and the temperature inside the device and the transport hose is maintained at a high temperature of 60°C to 70°C (Primary heating) to prevent viscosity increase in winter and to maintain a uniform spray atomization state.

[0101] The liquid mixture, which is impinged and mixed at ultra-high pressure inside the chamber, is sprayed through the nozzle tip in the form of a high-speed radial stream and is uniformly and densely applied to the surface of the concrete structure substrate (410) at the bottom, which is the target for crack control, with a target thickness (e.g., 2.0 to 3.0 mm).

[0103] S400 Step: Dynamic Reversible Network and Film Formation Step

[0104] This step is a final curing mechanism step in which a composite mixed liquid applied by high-pressure spraying onto a concrete structure substrate (410) completes an ultra-fast chemical crosslinking reaction at room temperature to complete a final permanent self-healing polyurea film (300) in which a rigid framework and a reversible composite self-healing network structure are simultaneously interpenetrated.

[0105] The mixed composition, having left the spray nozzle and settled on the concrete structure substrate (410), enters a gelation stage where it loses fluidity within 5 to 15 seconds after spraying due to the extremely high reactivity between the residual amine groups of the prepolymer and the isocyanate groups of the curing agent, without the need for a separate catalyst or heat treatment, and reaches a tack-free state where a person can walk within 1 minute. Due to these ultra-high-speed curing characteristics, a uniform film thickness can be secured without sagging even when applied to vertical walls or ceiling surfaces.

[0106] After construction, the final chemical curing and physical arrangement are completely finished after 24 hours at room temperature (RT). At this curing completion stage, a rigid cross-linked matrix framework is formed inside the film, in which polyetheramine prepolymer chains (110) are connected by strong covalent bonds around three-dimensional nodes of aliphatic isocyanate trimers (210).

[0107] At the same time, the UPy units (112) present at the chain ends and side chains face each other through spatial rearrangement to form a total of four dense quadruple hydrogen bonding units per molecule, thereby forming a stable reversible dimer stationary phase. Additionally, the surface-modified silica nanoparticles (121) penetrate uniformly between the polymer network structures and bond through amino groups via covalent bonding or interfacial hydrogen bonding, thereby becoming capable of absorbing mechanical shear stress.

[0108] As a result, even if a microcrack is induced in the building due to external stress or tensile behavior, the quadruple hydrogen bonds between the UPy units (112) are temporarily separated instead of the polymer main chains, absorbing the shock, and when the stress is released, the soft segments perform spontaneous self-reconnection at room temperature by their mobility, thereby finally completing the formation of a long-lasting, self-healing polyurea film (300) that can permanently and infinitely heal micro-damage.

[0110] Fig. 3 This is a composite structural diagram showing a composite cross-linked network structure formed by collision mixing of an aliphatic isocyanate trimer (liquid A), a hydrogen-bonded prepolymer, and nano silica (liquid B) by a high-pressure spray device according to one embodiment of the present invention.

[0111] Fig. 4 This is a schematic diagram of a dynamic self-healing mechanism in which quadruple hydrogen bonds between UPy units in a polyurea film according to one embodiment of the present invention dissociate and recombine depending on the conditions of external stress application and release.

[0112] Fig. 5 is a chemical reaction scheme representing the reversible prepolymer synthesis step of UPy-NCO unit and polyetheramine used in one embodiment of the present invention.

[0114] Fig. 3 According to one embodiment of the present invention, the curing agent part (A liquid, 200) and the main part (B liquid, 100), which are separately separated and transported, pass through the internal manifold and mixing chamber of a high-pressure spray mixing device (500) and are collide and mixed, and thereby finally settle on the surface of a concrete structure substrate (410) to form a molecular-level structure of a fine cross-linked network within the coating film.

[0115] Referring to Fig. 3, the top left box (A)The curing agent portion (200) shown in the area contains an aliphatic isocyanate trimer (HDI trimer, isocyanurate type) (210) as a main component that has excellent structural weather resistance and induces ultra-high-speed curing at room temperature, and is supplied in a quantitatively measured form in which a diisocyanate oligomer (220) for inducing reversible urea bonding is mixed in a certain equivalent amount to combine reversible deformation flexibility between molecular chains.

[0116] At the same time, the bottom left box (B) The main component (100) illustrated in the area is a composition that serves as the basis for the flexibility and self-healing performance of the present invention, and includes a reversible hydrogen-bonded polyetheramine prepolymer (110) synthesized by chemically and precisely bonding a quadruple hydrogen-bonding functional group, UPy-NCO unit (112), to at least one of the two ends or side chains of the polyetheramine sub-component (Soft segment) (111) as a base frame.

[0117] Furthermore, within the matrix of the main component (100), a hybrid functional nanofiller (120) is uniformly dispersed in the liquid phase without phase separation to enhance mechanical shear strength and suppress microcrack propagation. The nanofiller (120) has a core component of amino surface-modified silica nanoparticles (121) having a plurality of amine strands chemically grafted onto a spherical surface, and a graphene oxide or carbon-based reinforcing agent (122) having a sheet structure is hybridized and combined with the silica nanoparticles in a mutually complementary ratio to improve the resistance to tensile stress in the plane direction of the matrix. In addition, to prevent demolding and interfacial delamination with the concrete surface, an interfacial adhesion-promoting silane coupling agent (130) of the epoxy or isocyanate silane (131) series, a light stabilizer and a UV blocker (140) that prevent polymer main chain decomposition in an ultraviolet exposure environment are maintained in a state of complete interpenetration dispersion (IPN) within the liquid matrix of the main component (100).

[0118] When the main component (100) and the curing agent component (200) prepared in this manner are collided at the construction site through a high-pressure spray mixing device (500) under ultra-high pressure conditions of 2,000 to 3,500 psi, ultra-high-speed urea crosslinking curing is initiated by a spontaneous nucleophilic addition reaction between the residual amine groups of the prepolymer and the isocyanate groups of the curing agent component, even in the absence of a chemical catalyst.

[0119] As shown in the enlarged structural diagram on the right side of FIG. 3, when the three-dimensional network of the final cured self-healing polyurea film (300) is analyzed at the molecular scale, chains of polyetheramine prepolymer (110), which are flexible and have excellent elastic deformation ability, form a strong covalent framework centered around the hard segment cross-linking nodes of the aliphatic isocyanate trimer (210).

[0120] The UPy units (112) located between these covalent frameworks align to form a mutually symmetric structure through spatial behavior, thereby forming a stable quadruple hydrogen bonding assembly. At the same time, the amino surface-modified silica nanoparticles (121) spheres form organic organic-inorganic hybrid interfacial hydrogen bonding with the surrounding polymer matrix main chains via reactive amine surface strands, thereby completing a dense cross-linked network structure that uniformly relieves and dissipates local stress concentrations applied within the matrix throughout the entire film structure.

[0122] Fig. 4This is a schematic diagram of a dynamic self-healing mechanism in macroscopic and microscopic stepwise stages in which a dynamic hydrogen bond network built inside a self-healing polyurea film (300) according to one embodiment of the present invention spontaneously repairs damage during a series of processes in which physical tensile behavior, thermal shock, or shear stress is applied and then released from the outside.

[0123] Referring to FIG. 4, the self-healing mechanism of the present invention is performed continuously and reversibly over time through a total of three different molecular and interfacial state structures.

[0124] initial stable state

[0125] In a normal coating environment where no external stress is applied, the interior of the self-healing polyurea coating (300) consists of polyetheramine subcomponents (111), which are high-elongation main chains with excellent flexibility, arranged in parallel or randomly, and the UPy hydrogen bond units (112) bonded to the side chains and ends of the chains face each other to form a perfect dimer (quadruple H-bond) stationary phase. In this state, the coating maintains excellent initial tensile strength and elastic modulus and acts as a high-performance waterproof layer that blocks the upper surface of the lower concrete structure substrate (410) from external moisture and harmful ions.

[0128] Under stress and crack occurrence

[0129] When strong tensile stress exceeding the design threshold is partially applied to the self-healing polyurea film (300) due to the movement of the building, earthquake, external load, or drying shrinkage, the matrix undergoes deformation. At this time, before atomic destruction of the covalent main chains that causes permanent deformation occurs, a phenomenon is first induced in which dynamic quadruple hydrogen bond axes between UPy units (112) with relatively low bond energy are temporarily and sacrificially separated (dissociated).

[0130] External forces are primarily absorbed and dissipated at the molecular level through the reversible dissociation of hydrogen bonds, and if stress persists, micro-cracks and micro-voids occur inside the film. At this stage, the stress concentrated at the crack tip is physically blocked and bypassed (crack deflection) by the surrounding highly dispersed amino surface-modified silica nanoparticles (121) and graphene oxide / CNT reinforcement (122), thereby strongly suppressing the phenomenon of micro-cracks progressing into large propagating cracks.

[0132] Stress release and room temperature self-healing state (After stress release / self-healing)

[0133] When the external behavioral stress applied to the film is removed or relieved (Time / RT condition), the polymer chains that were dissociated by the inherent high molecular chain mobility of the polyetheramine subcomponent (111) begin to rearrange themselves toward the center of the crack.

[0134] In this process, the UPy units (112) that are spatially re-arranged adjacently re-bond a total of four dynamic hydrogen bond axes (H·O, H·N) at ultra-high speed, as shown in the chemical structure formula of the pop-up box on the right side of the drawing, by spontaneous intermolecular forces under ambient temperature (RT) atmospheric conditions, without any artificial stimulation such as the injection of separate external heat energy, UV irradiation, or catalyst injection.

[0135] As a result, partial crack closure occurs in which the separated crack interfaces are tightly closed at the molecular scale, and the damaged mechanical properties and waterproofing performance are completely restored to levels prior to the crack formation. This dynamic hydrogen bond dissociation and recombination mechanism exhibits unrivaled long-term durability that operates permanently and infinitely repeatedly against micro-damage occurring in the same area, provided there is no chemical degradation of the matrix.

[0137] Fig. 5 This is a chemical reaction equation that clearly shows the pre-synthesis mechanism of a reversible hydrogen-bonded polyetheramine prepolymer (110), which is a key intermediate performed to equip the entire matrix with reversible quadruple hydrogen bonding performance during the manufacturing process (step S200) of the main part (100) of the present invention, as a chemical structural equation.

[0138] Referring to FIG. 5, the synthesis equation visualizes the process of inducing the modified prepolymer product on the right through the quantitative reaction between the two reactants on the left, the UPy-NCO unit (112) and the polyetheramine subcomponent (PEA, Jeffamine D-2000) (111), using flow arrows.

[0139] The first reactant, the UPy-NCO unit (112), is an asymmetric organic functional group compound having a ureaidopyrimidinone ring structure capable of forming quadruple hydrogen bonds at the left end and a highly reactive isocyanate group (-NCO) capable of chemical chain extension and attachment reactions at the right end.

[0140] The second reactant, the polyetheramine subcomposition (111), has a molecular weight of about 2,000 g / mol and is a linear soft segment oligomer raw material having a repeating unit (n) of a flexible polypropylene glycol (PPG) chain structure in the center in the form of an ether bond and primary amine groups (-NH2) with excellent nucleophilic reactivity at both ends.

[0141] During the synthesis process, the molar ratio of the terminal amine group concentration of the polyetheramine subcomponent (111) to the isocyanate functional group of the UPy-NCO unit (112) is precisely limited to an asymmetric microequivalent range of 1:0.05 to 1:0.25, and then a reaction temperature environment of 60°C is provided. Under these conditions, the terminal -NCO functional group of the UPy-NCO undergoes a highly selective urea bonding reaction with the -NH2 functional group of the polyetheramine terminal without a catalyst.

[0142] As a result, a reversible hydrogen-bonded polyetheramine prepolymer (110) is synthesized in high yield, in which the flexible, high-elongation soft main chain skeleton shape of the polyetheramine subcomponent (111) is perfectly preserved and maintained, while a portion of the molecular chain ends are capped and modified into UPy heads that possess quadruple hydrogen bonding capabilities.

[0143] The prepolymer (110) synthesized in-situ through this process still retains a large amount of reactive residual amine groups (-NH2) within the molecule, so it can perfectly perform an immediate secondary cross-linking reaction with the aliphatic isocyanate trimer (210) of the curing agent (200) introduced during the subsequent on-site spray application stage (S300), and serves as the legal and technical key basis for establishing a permanent self-healing infrastructure (dynamic network) inside the final coating.

[0145] Fig. 6 This is a self-healing efficiency evaluation graph showing the change in the stress-strain curve according to the time of leaving at room temperature (RT) after artificial cutting damage of a self-healing polyurea film (300) according to one embodiment of the present invention. Fig. 7This is a schematic diagram of a step-by-step construction cross-section showing a crack bridging phenomenon in which a self-healing polyurea coating (300) according to one embodiment of the present invention stretches without fracture in response to a crack that occurred in a lower concrete structure substrate (410), and a macroscopic mechanism in which micro-damage caused by this is healed at room temperature over time.

[0146] Fig. 6 This is a stress-strain curve graph showing the recovery behavior of mechanical properties over time at room temperature (RT, 25℃) after artificial mechanical cut damage is applied to a self-healing polyurea film (300) that has been finally cured according to one embodiment of the present invention.

[0147] Referring to Fig. 6, the Y-axis represents the tensile stress (MPa) that the coating specimen withstands, and the X-axis represents the strain (%), which is the degree of elongation of the specimen. Inside the graph, based on the initial state curve (Intact State) without damage, the changes in tensile properties immediately after cutting (As-cut), after 2 hours at room temperature (2 h), after 6 hours at room temperature (6 h), and after 24 hours at room temperature (24 h) are plotted in a time series.

[0148] The initial (Intact) film simultaneously exhibits high initial tensile strength and excellent elongation at break of more than 400% through a composite network between the hard segment cross-linked structure of the aliphatic isocyanate trimer (210), the soft segment main chain of the reversible hydrogen-bonded polyetheramine prepolymer (110), and the amino surface-modified silica nanoparticles (121).

[0149] On the other hand, immediately after the specimen is completely cut (as-cut), the molecular cross-linking structure between the fracture surfaces is severed, so it cannot withstand tensile stress and exhibits fracture behavior at an early strain level. However, if left at room temperature (RT) without separate heat treatment, UV irradiation, or the addition of adhesive, self-healing behavior is observed in which the material properties recover dramatically.

[0150] As the storage time progresses to 2 hours (2 h) and 6 hours (6 h), the molecular main chains interdiffuse due to the high chain mobility of the polyetheramine subcomponent (111) located at the cut interface, and as a result, the adjacent UPy units (112) begin to reform reversible quadruple hydrogen bonds. Accordingly, it can be observed that the slope (modulus) of the stress-strain curve and the maximum tensile strength value gradually increase.

[0151] Finally, when examining the curve after 24 hours (24 h) of storage at room temperature, the elongation characteristics not only fully recover to the initial state (Intact) level (100% restoration), but the maximum tensile strength also achieves a high self-healing efficiency of over 90% compared to the initial strength. This is a variable that quantitatively proves that the damaged interface within the coating film has been perfectly re-bonded through reversible dynamic hydrogen bonding at the molecular level.

[0153] Fig. 7 This is a step-by-step macroscopic schematic diagram showing the actual mechanism of suppressing cracks caused by the behavior of the underlying ground or external impact and maintaining waterproofing performance when a self-healing polyurea coating (300) according to one embodiment of the present invention is applied at an actual civil engineering and construction site.

[0154] Referring to FIG. 7, the system construction structure of the present invention is macroscopically composed of a lower concrete structure substrate (410) and a self-healing polyurea coating film (300) that is continuously and precisely applied to a certain thickness on the upper surface of the substrate (410) through a high-pressure spray mixing device (500).

[0156] Stage 1: Structural Behavior and Crack Initiation Stage (Crack Initiation)

[0157] Due to environmental changes, loads, vibrations, etc., localized micro-cracks (e.g., 0.5 mm or less) occur inside the lower concrete structure substrate (410), causing behavior that spreads to both sides. At this time, in the case of a general organic coating agent or a modified urethane film, it cannot withstand the stress concentrated at the crack tip, and a phenomenon of reflective cracking occurs in which the film tears together in the vertically upward direction of the concrete crack.

[0158] On the other hand, the coating film (300) of the present invention, due to the high elongation characteristics and stress relief effect of the polyetheramine subcomponent (111) contained therein, does not break or delaminate at the interface even if the lower substrate is opened, but flexibly extends in the upper region of the crack and firmly seals the crack from the top. Crack bridging Exhibits performance.

[0160] Step 2: Micro-void Formulation Stage

[0161] When the tensile behavior of the lower substrate (410) continues and the coating film (300) stretches beyond a limit point, microscopic micro-voids and micro-cracks are primarily formed inside the polymer matrix inside the coating film instead of macroscopic fractures.

[0162] At this time, as described above in FIG. 4, the quadruple hydrogen bond between the UPy units (112) is preferentially destroyed (dissociated) as a sacrificial bond, dissipating energy and preventing the destruction of the main chain covalent bond. At the same time, the amino surface-modified silica nanoparticles (121) and the graphene oxide / CNT reinforcement (122) physically deflect and block the crack propagation path within the matrix, thereby fundamentally preventing micro-damage from growing into a large leakage crack that penetrates the entire film.

[0164] Step 3: Structural Stress Release and Coating Self-Healing Phase (Self-healing & Closure)

[0165] Afterward, when the movement pressure of the concrete structure substrate (410) is released or relieved due to a decrease in temperature or a change in load, the stretched coating (300) shrinks back to its original shape due to rubber elasticity (Elastic recovery), and the internal micro-void interfaces are physically strongly bonded to each other.

[0166] At the close interface, spontaneous room temperature (RT) quadruple hydrogen bond rearrangement between the UPy units (112) occurs within hours, causing the molecular chains to reversibly re-crosslink. As a result, internal micro-damage is completely closed and restored to a flawless continuous film identical to the initial state, thereby completely blocking the path for external moisture or chloride ions to enter the concrete cracks and permanently maintaining the long-term waterproofing performance and durability of the structure. Explanation of the symbols

[0167] 1 00: Main component (A liquid ingredient mixture) 110: Reversible hydrogen-bonded polyetheramine prepolymer 111: Polyetheramine substructure (Soft segment main chain oligomer) 112:UPy-NCO unit (ureaidopyrimidinone-based quadruple hydrogen bond head) 120: Hybrid functional nano filler (composite reinforcement) 121: Amino surface-modified silica nanoparticles 122: Graphene oxide or carbon nanotube reinforcement 130: Interfacial adhesion-promoting silane coupling agent 131: Epoxy or isocyanate silane 140: Photostabilizer and UV blocker (HALS complex) 200: Curing agent part (Liquid B raw material mixture) 210: Aliphatic isocyanate trimer (HDI trimer) 220: Diisocyanate oligomer for inducing reversible urea binding 300: Self-healing polyurea film (final cross-linked structure) 410: Concrete structure substrate (construction and protection target) 500: High-pressure spray mixing device (mixing nozzle and gun mechanism)

Claims

Claim 1 A dynamic hydrogen bond-based self-healing polyurea composition comprising: a main component (100) comprising a reversible hydrogen-bonded polyetheramine prepolymer (110) having a ureidopyrimidinone (UPy) unit (112) bonded to a terminal or side chain and a hybrid functional nanofiller (120); and a curing agent component (200) comprising an aliphatic isocyanate trimer (210), wherein the main component (100) and the curing agent component (200) are mixed to exhibit room temperature self-healing properties. Claim 2 A self-healing polyurea composition according to claim 1, wherein the reversible hydrogen-bonded polyetheramine prepolymer (110) is synthesized by in-situ reaction in a ratio selected in the range of 1:0.05 to 1:0.25 for the reaction molar ratio of the amine group (-NH2) of the difunctional or trifunctional polyetheramine subcomponent (111) having a molecular weight of 2,000 to 4,000 g / mol to the isocyanate group (-NCO) of the UPy-NCO unit (112). Claim 3 A self-healing polyurea composition according to claim 1, wherein the hybrid functional nanofiller (120) comprises: amino surface modified silica nanoparticles (121) having an average particle size of 10 to 50 nm and having amine functional groups grafted on their surface; and a carbon-based reinforcing material (122) comprising at least one of graphene oxide and carbon nanotubes having a plate-like structure, mixed in a weight ratio of 1:0.1 to 1:0.

5. Claim 4 A self-healing polyurea composition according to claim 1, wherein the curing agent part (200) comprises 75 to 85 parts by weight of an aliphatic isocyanate trimer (210) which is a hexamethylene diisocyanate trimer (HDI trimer); and 15 to 25 parts by weight of a diisocyanate oligomer (220) for inducing reversible urea binding. Claim 5 A self-healing polyurea composition according to claim 1, characterized in that the main component (100) comprises 1.0 to 10.0 parts by weight of the hybrid functional nano filler (120) relative to 100 parts by weight of the prepolymer (110). Claim 6 A self-healing polyurea composition according to claim 1, further comprising 0.5 to 3.0 parts by weight of an interfacial adhesion-promoting silane coupling agent (130) composed of epoxysilane or isocyanatesilane within the main component (100); and 0.1 to 1.0 parts by weight of a hindered amine light stabilizer (HALS) and a benzotriazole-based UV blocker (140). Claim 7 A self-healing polyurea composition according to claim 1, characterized in that the main component (100) and the curing agent component (200) are collide-mixed and sprayed at a volume ratio of 1:1 by a high-pressure spray mixing device (500) during on-site construction. Claim 8 A self-healing polyurea waterproofing material intermediate composition comprising: a reversible hydrogen-bonded polyetheramine prepolymer (110) which is individually packaged or distributed as a raw material before reacting with a curing agent part (200), has a urea-dopyrimidinone (UPy) ring that induces quadruple hydrogen bonding at the end, and has residual reactive amine groups (-NH2) in the inner molecular main chain; and a hybrid functional nanofiller (120) comprising amino surface-modified silica nanoparticles (121) and carbon-based reinforcing material (122) ultrasonically dispersed in a liquid matrix of the prepolymer (110). Claim 9 A main component intermediate composition according to claim 8, characterized in that the residual reactive amine group (-NH2) in the prepolymer (110) possesses a chemical equivalent capable of causing a room temperature ultrafast urea reaction when mixed in volume ratio with the isocyanate group (-NCO) of the curing agent part (200). Claim 10 A main component intermediate composition according to claim 8, wherein the hybrid functional nano filler (120) is included in a range of 1.0 to 10.0 parts by weight relative to 100 parts by weight of the prepolymer (110), and is characterized by maintaining dispersion phase stability under high-speed shear force conditions using a homo mixer and an ultrasonic disperser. Claim 11 A main component intermediate composition according to claim 8, wherein the carbon-based reinforcing material (122) comprises at least one of a graphene oxide sheet and a single-walled or multi-walled carbon nanotube (CNT). Claim 12 A main component intermediate composition characterized in that, in claim 8, it is in a liquid form that is solvent-free by vacuum distillation and does not emit volatile organic compounds (VOCs). Claim 13 A main component intermediate composition characterized by further comprising 0.5 to 3.0 parts by weight of epoxysilane or isocyanatesilane (131) for inducing a chemical covalent bond with the substrate in claim 8. Claim 14 A self-healing polyurea film structure having a three-dimensional dynamic reversible network structure comprising: a hard segment crosslinking node comprising a hard molecular axis derived from an aliphatic isocyanate trimer (210) and a diisocyanate oligomer (220); a polyetheramine prepolymer (110) main chain connecting the crosslinking nodes by covalent bonds; a quadruple hydrogen bond axis (112) capable of reversible detachment at room temperature between ureadopyrimidinone (UPy) units located at the end or side chain of the main chain; and an amino surface modified silica nanoparticle (121) filled between the main chains and forming an interfacial bond with the polymer matrix through surface amine groups; thereby exhibiting self-healing efficiency when left at room temperature after cutting damage. Claim 15 A coating structure characterized in that, in claim 14, the above quadruple hydrogen bond axis (112) preferentially dissociates as a sacrificial bond prior to the destruction of the covalent main chain when external tensile stress is applied, thereby relieving stress. Claim 16 In claim 14, the above amino surface-modified silica nanoparticles (121) are characterized by physically blocking and deflecting the leading edge propagation path of microcracks penetrating into the matrix, forming a film structure. Claim 17 A coating structure according to claim 14, characterized in that the quadruple hydrogen bond axis (112) has reversibility to spontaneously re-bond under ambient temperature (25°C) atmosphere by undergoing a rearrangement step due to the molecular mobility of the polyetheramine main chain upon release of external stress. Claim 18 A coating structure according to claim 14, characterized by exhibiting high elongation characteristics in which the initial tensile strength in the final hardened state is 18.0 to 23.0 MPa and the initial elongation at break is maintained in the range of 400% to 500%. Claim 19 A step (S100) of synthesizing an UPy-NCO unit (112) having an isocyanate group at the terminal end by reacting 6-methylisocytosine and an aliphatic diisocyanate compound under a nitrogen atmosphere; a step (S200) of manufacturing a main component (100) by in-situ synthesizing a reversible hydrogen-bonded polyetheramine prepolymer (110) by stirring the synthesized UPy-NCO unit (112) and a polyetheramine subcomponent (111) at 60°C, and adding a hybrid functional nanofiller (120) to the mixture and performing high-speed shear dispersion; and a step (S200) of the manufactured main component (100) and a curing agent component (200) including an aliphatic isocyanate trimer (210) through a high-pressure spray mixing device (500) under conditions of a pressure of 2,000 to 3,500 psi and a temperature of 60°C to 70°C A method for constructing a self-healing polyurea film, comprising: a step of high-pressure collision mixing in a volume ratio of 1:1 (S300); and a step of spraying the collision-mixed composite liquid composition onto the surface of a structural substrate (410) to form a self-healing polyurea film (300) based on a three-dimensional dynamic reversible network through ultra-high-speed curing at room temperature (S400). Claim 20 A construction method according to claim 19, wherein the step (S100) of synthesizing the UPy-NCO unit (112) is a process of heating and stirring for 4 to 6 hours under constant temperature conditions of 70°C to 90°C. Claim 21 A construction method according to claim 19, wherein the step (S200) of manufacturing the above-mentioned main part (100) includes a process of shear dispersion at a rotational speed of 3,000 rpm or more by simultaneously operating a homo mixer and an ultrasonic disperser to prevent aggregation of silica nanoparticles (121) and carbon-based reinforcing material (122) within a polymer matrix. Claim 22 A construction method according to claim 19, characterized in that the collision mixing of the above S300 step is performed instantaneously within a mixing chamber inside a dedicated spray gun. Claim 23 A construction method according to claim 19, characterized in that the composite liquid composition sprayed in the spray application step (S400) undergoes a gelation step in which it loses fluidity within 5 to 15 seconds after settling on the structural substrate (410), thereby controlling sagging during vertical wall construction. Claim 24 A construction method according to claim 19, further comprising, after the spraying application step (S400), a step of additionally curing for 24 hours at room temperature (25℃) to fully stabilize the trimer crosslinked framework and the UPy tetrahydrogen bonded dimer stationary phase. Claim 25 A construction method characterized by, in claim 19, incorporating an epoxy or isocyanate silane (131) during the step (S200) of manufacturing the main part (100) to provide chemical adhesion that suppresses interfacial peeling with the surface of the structural substrate (410) when forming the final coating film. Claim 26 A structural waterproofing system comprising: a structural substrate (410) forming a target surface for crack control due to behavior and environmental stress; a self-healing polyurea coating (300) that is closely laminated to the upper surface of the structural substrate (410) and is formed by high-pressure impact mixing spraying, wherein an aliphatic trimer covalent crosslinking framework, reversible UPy quadrivalent hydrogen bonds, and amino-modified silica fillers are mutually infiltrated inside; and an interface adhesion-promoting silane coupling agent (130) bonding layer existing between the adhesive interface of the structural substrate (410) and the self-healing polyurea coating (300), which chemically fixes both interfaces through a reactor of epoxy or isocyanate silane (131); wherein the coating (300) exhibits crack-following characteristics in which it is stretched without fracture in response to width deformation of microcracks occurring in the structural substrate (410). Claim 27 A waterproofing system according to claim 26, wherein the self-healing polyurea coating (300) relieves and dissipates stress without permanent destruction for micro-crack behavior of 2.0 mm or less occurring in the structure substrate (410). Claim 28 A waterproof system according to claim 26, wherein the self-healing polyurea film (300) contains a composite of hindered amine light stabilizer and UV blocker (140) to prevent reversible hydrogen bonding degradation in an environment constantly exposed to the outside. Claim 29 A waterproof system according to claim 26, characterized in that a top-coat protective layer for wear resistance and prevention of external contamination is additionally laminated on top of the self-healing polyurea film (300) with a set thickness. Claim 30 A waterproofing system according to claim 26, characterized in that after foreign substances and laitance present on the surface of the above-mentioned structural substrate (410) are removed, the self-healing polyurea coating film (300) is uniformly applied by a high-pressure spray mixing device (500) in a thickness range of 2.0 to 3.0 mm to form an upper surface waterproof barrier layer.

Citation Information

Patent Citations

  • Coating

    EP3601785A1

  • Methods of preparing and using polyurea elastomers

    US20070066786A1