Manufacturing method of positive electrode active material
The described method addresses the issue of residual lithium by-products and surface energy differences by using steam-introduced heat treatment to form a uniform coating on lithium composite transition metal oxides, improving the performance of high-nickel cathode active materials in lithium-ion batteries.
Patent Information
- Application Number
- KR1020240110193
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-08-17
- Filing Date
- 2024-08-19
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The manufacturing of high-nickel cathode active materials for lithium-ion batteries is hindered by residual lithium by-products on the surface, which react with electrolytes causing swelling and degrade capacity and rate characteristics, and the formation of a uniform coating layer is challenging due to surface energy differences.
A method involving calcination and heat treatment with a steam introduction step during the heating phase to form a coating layer on lithium composite transition metal oxides, eliminating the need for a washing step and ensuring a uniform coating without surface damage.
This method reduces surface by-products, enhances coating efficiency, and improves the capacity and rate characteristics of the cathode active material by forming a thin, uniform coating layer.
Smart Images

Figure 112024089555978-PAT00004_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing an anode active material. Background Technology
[0003] With the recent increase in technological development and demand for mobile devices and electric vehicles, the demand for secondary batteries as an energy source is rapidly rising. Among these secondary batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Lithium transition metal oxides, such as lithium cobalt oxide like LiCoO2, lithium nickel oxide like LiNiO2, lithium manganese oxide like LiMnO2 or LiMn2O4, and lithium iron phosphate compounds like LiFePO4, have been developed as cathode active materials for lithium secondary batteries, and recently, Li[Ni a Co b Mn c ]O2, Li[Ni a Co b Al c ]O2, Li[Ni a Co b Mn c Al d Lithium composite transition metal oxides containing two or more transition metals, such as O2, have been developed and are widely used.
[0005] In particular, with the recent technological advancements in electric vehicles and the like, the demand for high-capacity secondary batteries is increasing, and accordingly, research on cathodes using high-nickel (High-Ni) cathode active materials with excellent capacity characteristics is actively underway.
[0006] High-nickel cathode active materials are manufactured by mixing a precursor and a lithium raw material and then calcining the mixture. However, since calcination is performed at a relatively low temperature, the amount of residual lithium, which acts as a byproduct, on the surface of the cathode active material increases. This residual lithium, in the form of LiOH and / or Li2CO3, reacts with the electrolyte and other substances within the battery, generating gas and causing swelling.
[0007] When a washing process is introduced to remove these by-products, damage occurs to the surface of the cathode active material during washing, which degrades capacity and rate characteristics and complicates the process steps. In addition, due to the difference in surface energy between the surface of the cathode active material and the coating raw material after washing, it is difficult to form a uniform coating layer, and there is a problem of using an excessive amount of coating raw material.
[0008] Therefore, it is necessary to secure technology that reduces by-products on the surface of the aforementioned cathode active material and improves coating efficiency. Prior art literature
[0010] Korean Patent Publication No. 10-2020-0105474 The problem to be solved
[0011] To solve the above-mentioned problems, the technical objective of the present invention is to provide a method for manufacturing an anode active material capable of reducing by-products on the surface of a lithium composite transition metal oxide and improving coating efficiency. means of solving the problem
[0013] (1) The present invention provides a method for manufacturing a positive electrode active material comprising: (A) a step of mixing a positive electrode active material precursor and a lithium (Li)-containing raw material and then calcining to produce a lithium composite transition metal oxide; and (B) a step of mixing the lithium composite transition metal oxide and a coating raw material and then heat treating to form a coating layer on the lithium composite transition metal oxide; wherein the heat treatment includes a heating section for raising the temperature and a maintaining section for maintaining the temperature, and includes a section for introducing steam only in the heating section.
[0014] (2) The present invention provides a method for manufacturing a positive active material in which, in (1) above, the positive active material precursor has a composition represented by the following chemical formula 1.
[0015] [Chemical Formula 1]
[0016] Ni a Mn b Co c M 1 d (OH)2
[0017] In the above chemical formula 1,
[0018] M 1 is one or more selected from Al, Zr, W, Mg, Ti, Y, and B, and 0.5≤a<1, 0≤b<0.5, 0≤c<0.5, 0≤d≤0.1.
[0019] (3) The present invention provides a method for manufacturing an anode active material, wherein the calcination in (1) or (2) is performed at a temperature of 700°C to 1,000°C.
[0020] (4) The present invention provides a method for manufacturing an anode active material in any one of (1) to (3), wherein the lithium composite transition metal oxide has a composition represented by the following chemical formula 2.
[0021] [Chemical Formula 2]
[0022] Li 1+x1 Nia1 Mn b1 Co c1 M 2 d1 O2
[0023] In the above chemical formula 2, M 2 is one or more selected from Al, Zr, W, Mg, Ti, Y and B, and 0.0≤x1≤0.10, 0.5≤a1<1, 0≤b1<0.5, 0≤c1<0.5, 0≤d1≤0.1.
[0024] (5) The present invention provides a method for manufacturing a positive electrode active material in any one of (1) to (4), wherein the lithium composite transition metal oxide is in the form of a single particle.
[0025] (6) The present invention provides a method for manufacturing an anode active material that does not include a washing step in any one of (1) to (5).
[0026] (7) The present invention provides a method for manufacturing an anode active material in any one of (1) to (6), wherein the coating raw material is a hydroxide comprising one or more selected from Co, Al and Nb.
[0027] (8) The present invention provides a method for manufacturing an anode active material in any one of (1) to (7), wherein the coating raw material is cobalt hydroxide.
[0028] (9) The present invention provides a method for manufacturing an anode active material in any one of (1) to (8), wherein the coating raw material is mixed in an amount of 0.5 to 5 parts by weight per 100 parts by weight of the lithium composite transition metal oxide.
[0029] (10) The present invention provides a method for manufacturing an anode active material, wherein in any one of (1) to (9), the heating section includes a section for introducing steam at a temperature of 600°C or lower.
[0030] (11) The present invention provides a method for manufacturing a positive electrode active material in any one of (1) to (10), wherein the heating section has a heating rate of 1℃ / min to 10℃ / min.
[0031] (12) The present invention provides a method for manufacturing an anode active material in any one of (1) to (11), wherein the water vapor is introduced in an amount such that the moisture content (χ) according to Formula 1 below is 1% to 10%.
[0032] [Equation 1]
[0033]
[0034] In the above Equation 1,
[0035] The above α is the mass (g) of the lithium composite transition metal oxide and coating raw material immediately after passing through the section where steam is introduced, and the above β is the mass (g) of the lithium composite transition metal oxide and coating raw material after being completely dried immediately after passing through the section where steam is introduced.
[0036] (13) The present invention provides a method for manufacturing an anode active material in any one of (1) to (12), wherein the section for introducing water vapor is performed under an oxidizing atmosphere.
[0037] (14) The present invention provides a method for manufacturing an anode active material, wherein in any one of (1) to (13), the maintenance section maintains the temperature at 500°C to 900°C and performs heat treatment.
[0038] (15) The present invention provides a method for manufacturing a positive electrode active material, wherein in any one of (1) to (14), the maintenance period is performed for 1 hour to 12 hours.
[0039] (16) The present invention provides a method for manufacturing an anode active material in any one of (1) to (15), wherein the maintenance section does not include a section for introducing steam. Effects of the invention
[0041] The manufacturing method of the present invention includes a section for introducing steam during the heating section when heat treatment for forming a coating layer, which can reduce by-products on the surface of the anode active material and form a thin and uniform coating layer, as well as improve coating efficiency. Brief explanation of the drawing
[0043] Figure 1 is an EPMA (ELECTRON PROBE MICROANALYSIS) mapping image of the cathode active material prepared in Example 1. Figure 2 is an EPMA mapping image of the positive electrode active material prepared in Example 2. Figure 3 is an EPMA mapping image of the positive electrode active material prepared in Example 3. Figure 4 is an EPMA mapping image of the cathode active material prepared in Comparative Example 1. Specific details for implementing the invention
[0044] Hereinafter, the present invention will be described in more detail to aid in understanding the invention.
[0045] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.
[0046] In this specification, terms such as 'comprising,' 'having,' or 'having' are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0047] In this specification, the term "on" means not only cases where one configuration is formed on the surface immediately above another configuration, but also cases where a third configuration is interposed between these configurations.
[0048] In this specification, the single particle form refers to a cathode active material and / or a lithium composite transition metal oxide having a non-spherical particle form formed by the aggregation of primary particles with a size of 0.5 μm or more, as opposed to a spherical secondary particle form formed by the aggregation of primary particles having a size of several nm to less than 0.5 μm manufactured by conventional methods.
[0049] For example, in the present invention, the anode active material in the form of a single particle may be a single particle consisting of one primary particle of 0.5 μm or larger, or it may be in the form of several primary particles of 0.5 μm or larger aggregated. Meanwhile, 'primary particle' refers to the smallest unit of a particle recognized when the anode active material is observed through a scanning electron microscope.
[0050] In this specification, 'moisture content' may be measured using a heating type moisture meter (e.g., AND Corporation's MX-50). Specifically, about 5g of the sample is placed in a sample dish within the device, and then the lid of the device is closed to set the temperature of the sample dish to 100°C to 150°C, thereby evaporating the moisture contained in the powder sample and measuring the degree of mass reduction. At this time, the point at which the mass no longer decreases is referred to as the completely dried state. The moisture content may be expressed as a percentage (%) of the difference between the mass (g) of the sample before and after complete drying and the mass (g) of the sample before complete drying.
[0052] Method for manufacturing positive electrode active material
[0053] Hereinafter, a method for manufacturing a positive electrode active material according to the present invention will be described.
[0055] A method for manufacturing a positive electrode active material according to the present invention comprises: (A) a step of mixing a positive electrode active material precursor and a lithium (Li)-containing raw material and then calcining to produce a lithium composite transition metal oxide; and (B) a step of mixing the lithium composite transition metal oxide and a coating raw material and then heat treating to form a coating layer on the lithium composite transition metal oxide; wherein the heat treatment includes a heating section for raising the temperature and a maintaining section for maintaining the temperature, and includes a section for introducing steam only in the heating section.
[0057] Hereinafter, a method for manufacturing a positive electrode active material according to the present invention will be described in more detail.
[0059] (A) Step
[0060] The method includes the step of preparing a lithium composite transition metal oxide by mixing a positive electrode active material precursor and a lithium (Li)-containing raw material, and then calcining the mixture.
[0062] According to one embodiment of the present invention, the positive active material precursor may have a composition represented by the following chemical formula 1.
[0063] [Chemical Formula 1]
[0064] Ni a Mn b Co c M 1 d (OH)2
[0065] In the above chemical formula 1,
[0066] M 1 It is one or more selected from Al, Zr, W, Mg, Ti, Y, and B, and
[0067] 0.5≤a<1, 0≤b<0.5, 0≤c<0.5, 0≤d≤0.1.
[0068] The above M 1 is a doping element, specifically the above M 1 It may be at least one selected from Al, Zr, W, Mg, Ti, Y, and B.
[0069] The above a is the molar ratio of nickel (Ni) among the total metals in the cathode active material precursor, and may be 0.5 or more, 0.7 or more, 0.8 or more, 0.85 or more, or 0.88 or more, and may be 0.9 or less, 0.95 or less, 0.98 or less, or less than 1. When a satisfies the above range, high energy density is exhibited, and high capacity characteristics can be realized.
[0070] The above b is the molar ratio of manganese (Mn) among the total metals in the positive active material precursor, which may be 0 or more, 0.03 or more, 0.05 or more, or 0.07 or more, and may be 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, or less than 0.5.
[0071] The above c is the molar ratio of cobalt (Co) among the total metals in the positive active material precursor, and may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.05 or less, 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, or less than 0.5.
[0072] The above d is M among the total metals in the positive electrode active material precursor. 1 The molar ratio may be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, or 0.04 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, or 0.1 or less.
[0073] When the above a, b, c, and d satisfy the above ranges, a positive electrode active material with excellent energy density and high capacity characteristics can be realized.
[0074] The transition metal hydroxide having the composition represented by the above chemical formula 1 may be a commercially available product or may be manufactured according to a method for manufacturing transition metal hydroxides well known in the art, such as a coprecipitation method.
[0076] The above lithium (Li)-containing raw material may be a lithium-containing sulfate, nitrate, carbonate, or hydroxide, etc. Specifically, the above lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiBr, LiI, Li2O, Li2SO4, etc.
[0078] The above-mentioned positive electrode active material precursor and lithium (Li)-containing raw material may be mixed such that the molar ratio (M:Li) of the transition metal (M) contained in the positive electrode active material precursor and the lithium (Li) contained in the lithium (Li)-containing raw material is 1:1.00 to 1.10. In this case, not only can an excess amount of lithium be prevented from entering the structure of the positive electrode active material, but the content of unreacted residual lithium may also be low.
[0080] The above mixing can be performed by dry mixing or wet mixing. When mixing each component through dry mixing, the calcination process can be performed without a separate drying process. When mixing each component through wet mixing, the components may be prepared by adding them to a solvent, specifically water, or a mixture of water and an organic solvent that is uniformly miscible with water (specifically alcohol, etc.), or a solution containing each raw material, specifically an aqueous solution, is prepared and mixed, and then the mixed components are spray-dried before proceeding with the calcination process.
[0081] Each raw material and cathode active material precursor can be used in appropriate amounts considering the content of each metal element in the final lithium composite metal oxide.
[0083] According to one embodiment of the present invention, the calcination may be performed at a temperature of 700°C or higher, 750°C or higher, 800°C or higher, 850°C or lower, 900°C or lower, 950°C or lower, or 1,000°C or lower. Furthermore, the calcination may be performed for 10 hours or more, 15 hours or more, or 20 hours or more, or for 25 hours or less, 30 hours or less, or 40 hours or less, and the calcination may be performed under an oxygen atmosphere. When performed under the above temperature range, time range, and atmosphere, the lithium (Li)-containing raw material is efficiently melted, and the reaction between the cathode active material precursor and the lithium (Li)-containing raw material is promoted, thereby enabling the efficient growth of lithium composite transition metal oxide particles.
[0085] According to one embodiment of the present invention, the lithium composite transition metal oxide may have a composition represented by the following chemical formula 2.
[0086] [Chemical Formula 2]
[0087] Li 1+x1 Ni a1 Mn b1 Co c1M 2 d1 O2
[0088] In the above chemical formula 2,
[0089] M 2 is one or more selected from Al, Zr, W, Mg, Ti, Y, and B, and
[0090] 0.0≤x1≤0.10, 0.5≤a1<1, 0≤b1<0.5, 0≤c1<0.5, 0.0≤d1≤0.1.
[0091] The above M 2 is a doping element, specifically the above M 2 may be at least one selected from Al, Zr, W, Mg, Ti, Y, and B. The above M 2 Although it is not necessarily included, if included in an appropriate amount, the particle shape of the positive active material can be improved and the stability of the crystal structure can be enhanced.
[0092] The above x1 may be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, or 0.04 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, or 0.1 or less.
[0093] The above a1 is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium composite transition metal oxide, and may be 0.5 or more, 0.7 or more, 0.8 or more, 0.85 or more, or 0.88 or more, and may be 0.9 or less, 0.95 or less, 0.98 or less, or less than 1. When a1 satisfies the above range, high energy density is exhibited, and high capacity characteristics can be realized.
[0094] The above b1 is the molar ratio of manganese (Mn) among all metals excluding lithium in the lithium composite transition metal oxide, and may be 0 or more, 0.03 or more, 0.05 or more, or 0.07 or more, and may be 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, or less than 0.5.
[0095] The above c1 is the molar ratio of cobalt (Co) among all metals excluding lithium in the lithium composite transition metal oxide, and may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.05 or less, 0.1 or less, 0.2 or less, 0.3 or less, 0.4 or less, or less than 0.5.
[0096] The above d1 is M among the total metals excluding lithium in the lithium complex transition metal oxide. 2 The molar ratio may be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, or 0.04 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, or 0.1 or less. When d1 satisfies the above range, the stability of the crystal structure of the positive active material may be improved, and the output characteristics, capacity characteristics, and lifespan characteristics may be improved.
[0097] When the above x1, a1, b1, c1, and d1 satisfy the above range, a positive electrode active material with excellent energy density and high capacity characteristics can be obtained.
[0099] According to one embodiment of the present invention, the lithium composite transition metal oxide may be in the form of a single particle. When the lithium composite transition metal oxide is in the form of a single particle, the structural stability of the cathode active material containing the lithium composite transition metal oxide can be enhanced. In this regard, when rolling for electrode manufacturing or operating the cell, micro / macro cracks caused by grain boundaries can be suppressed, the grain boundary area in contact with the electrolyte is reduced, and gas generation due to side reactions with the electrolyte is reduced, thereby improving the lifespan characteristics of the secondary battery.
[0101] (B) Step
[0102] The method includes the step of forming a coating layer on the lithium composite transition metal oxide by mixing the lithium composite transition metal oxide and the coating raw material and then heat treating; wherein the heat treatment includes a heating section for raising the temperature and a maintaining section for maintaining the temperature, and includes a section for introducing steam only in the heating section.
[0104] Conventionally, when forming a coating layer on a lithium composite transition metal oxide, an excessive amount of coating raw material was used or a washing treatment was performed to reduce by-products on the surface of the lithium composite transition metal oxide. However, when an excessive amount of coating raw material is used, by-products still remain and efficiency is reduced, and when a washing treatment is performed, the surface of the cathode active material is damaged, the process steps become complicated, and it is not economical.
[0105] The inventors have discovered that when forming a coating layer on a lithium composite transition metal oxide, by mixing the lithium composite transition metal oxide and the coating raw material and then introducing steam during a specific section of the heating section during heat treatment, bypasses on the surface of the lithium composite transition metal oxide can be reduced, the coating layer can be formed thinly and uniformly, and the coating efficiency can be improved, and thus the present invention has been completed.
[0106] Meanwhile, when steam is introduced during the temperature maintenance section of the heat treatment, the steam promotes the reduction reaction between Li2O and H2O, which leads to an increase in residual lithium, a byproduct on the surface of the lithium complex transition metal oxide, and a decrease in coating efficiency.
[0108] According to one embodiment of the present invention, the coating layer may be in a discontinuous form or a continuous form.
[0110] According to one embodiment of the present invention, a washing step may not be included. As a result, damage to the surface of the positive electrode active material is prevented, the process is simplified, and there is an economic effect.
[0112] According to one embodiment of the present invention, the coating raw material may be a hydroxide comprising one or more selected from Co, Al, and Nb. In particular, in the case of cobalt hydroxide, the resistance characteristics of the lithium transition metal oxide can be improved, thereby improving output characteristics and capacity characteristics.
[0114] According to one embodiment of the present invention, the coating raw material may be 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more, based on 100 parts by weight of the lithium composite transition metal oxide, or may be mixed in an amount of 3 parts by weight or less, 4 parts by weight or less, or 5 parts by weight or less. When the amount of the coating raw material mixed is within the above range, the coating layer is thin and uniform, the coating efficiency is improved, and there is an economic effect.
[0116] Meanwhile, the above heat treatment includes a heating section for raising the temperature and a holding section for maintaining the temperature, and includes a section for introducing steam only in the heating section. That is, the section for introducing steam exists only in the heating section, and other sections excluding the heating section do not include a section for introducing steam. Specifically, the holding section may not include a section for introducing steam. If a section for introducing steam is included in the heating section, the steam promotes the reaction between the coating raw material and residual lithium, and an additional washing process to remove surface byproducts may not be performed, thereby reducing byproducts on the surface of the lithium composite transition metal oxide compared to conventional methods and simplifying the process steps. On the other hand, if a section for introducing steam is included in other sections excluding the heating section, specifically the holding section, the steam promotes the reduction reaction between Li2O and H2O, which leads to an increase in residual lithium, a byproduct on the surface of the lithium composite transition metal oxide, and a decrease in coating efficiency.
[0118] According to one embodiment of the present invention, the heating section may include a section for introducing steam at a temperature of 600°C or lower. Specifically, it may include a section for introducing steam at a temperature of 0°C to 250°C, a section for introducing steam at a temperature of 250°C to 500°C, or a section for introducing steam at a temperature of 0°C to 500°C. When the section for introducing steam is within the above temperature range, the reaction between the coating raw material and residual lithium can be efficiently controlled, and sufficient heat required for the reaction can be supplied.
[0120] According to one embodiment of the present invention, the heating rate of the heating section may be 1°C / min or more, 2°C / min or more, 3°C / min or more, or 4°C / min or more, and 6°C / min or less, 7°C / min or less, 8°C / min or less, 9°C / min or less, or 10°C / min or less. When the heating rate in the heating section is within the above range, the production yield is excellent, and since the temperatures of the reactor, the lithium composite transition metal oxide, and the coating raw material are similar, the entire amount of heat required for the set maintenance temperature can be received. In particular, when the heating rate is 5°C / min, the amount of heat required for the reaction can be supplied efficiently.
[0122] According to one embodiment of the present invention, the water vapor may be introduced in an amount such that the moisture content (χ) according to Formula 1 below is 1% or more, 2% or more, 3% or more, 4% or more, or 5% or more, and 6% or less, 7% or less, 8% or less, 9% or less, or 10% or less.
[0123] [Equation 1]
[0124]
[0125] In the above Equation 1,
[0126] The above α is the mass (g) of the lithium composite transition metal oxide and coating raw material immediately after passing through the section where steam is introduced, and the above β is the mass (g) of the lithium composite transition metal oxide and coating raw material after being completely dried immediately after passing through the section where steam is introduced.
[0128] According to one embodiment of the present invention, the section for introducing water vapor may be performed under an oxidizing atmosphere. In this case, by providing an atmosphere necessary for the reaction, the reaction between the coating raw material and residual lithium can be efficiently controlled.
[0130] According to one embodiment of the present invention, the holding section may be 500°C or higher, 600°C or higher, or 700°C or higher, and may perform heat treatment while maintaining the temperature at 800°C or lower, 850°C or lower, or 900°C or lower. When the temperature of the holding section is within the above range, the coating raw material melts, and there is a surface stabilization effect of the cathode active material through recrystallization of the surface of the lithium composite transition metal oxide.
[0132] According to the present invention, the maintenance period may be 1 hour or more, or 2 hours or more, or may be performed for 3 hours or less, 5 hours or less, or 12 hours or less. When the duration of the maintenance period is within the above range, sufficient thermal energy is supplied to the lithium composite transition metal oxide and the coating raw material, and the coating becomes uniform overall.
[0134] positive electrode active material
[0135] In addition, the present invention provides a positive electrode active material manufactured by the manufacturing method described above.
[0136] The positive electrode active material according to the present invention is a positive electrode active material manufactured by the manufacturing method described above, wherein a uniform coating layer exists on a lithium composite transition metal oxide. The coating layer may have a small variation in the concentration of the coating element.
[0138] anode
[0139] In addition, the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.
[0140] Specifically, the anode comprises an anode current collector and an anode active material layer located on at least one surface of the anode current collector and comprising the anode active material described above.
[0141] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0143] The above positive active material layer may include a conductive material and a binder together with the positive active material.
[0144] At this time, the positive active material may be included in an amount of 80 to 99 weight%, more specifically 85 to 98 weight%, based on the total weight of the positive active material layer. Excellent capacity characteristics can be exhibited when included within the above-mentioned content range.
[0145] At this time, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powder or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The conductive material may be included in an amount of 1 to 30 weight% based on the total weight of the positive electrode active material layer.
[0147] The above binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The above binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.
[0149] The above-described anode may be manufactured according to a conventional anode manufacturing method, except for using the above-described anode active material. Specifically, it may be manufactured by applying an anode composite material, prepared by dissolving or dispersing the above-described anode active material and, optionally, a binder and a conductive material in a solvent, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the above-described anode active material, binder, and conductive material are as previously described.
[0151] The above solvent may be a solvent commonly used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that dissolves or disperses the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.
[0153] In addition, the anode may also be manufactured by casting the anode composite material onto a separate support and then laminating the film obtained by peeling from the support onto an anode current collector.
[0155] lithium secondary battery
[0156] In addition, the present invention can manufacture an electrochemical device including the anode. Specifically, the electrochemical device may be a battery, a capacitor, etc., and more specifically, a lithium secondary battery.
[0157] Specifically, the above lithium secondary battery comprises a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is identical to the one described above, a detailed description is omitted, and only the remaining components are described in detail below.
[0158] In addition, the lithium secondary battery may optionally further include a battery container that accommodates the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member that seals the battery container.
[0160] In the above lithium secondary battery, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0161] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 μm to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0163] The above-mentioned cathode active material layer optionally includes a binder and a conductive material together with the cathode active material.
[0164] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ βExamples include metal oxides capable of doping and dedoping lithium, such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, the carbon material may include low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0165] The above-mentioned negative electrode active material may be included in an amount of 80% to 99% by weight relative to the total weight of the negative electrode active material layer.
[0167] The above binder is a component that assists in the bonding between the conductive material, the active material, and the current collector, and can typically be added in an amount of 0.1% to 10% by weight relative to the total weight of the negative active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0168] The above conductive material is a component for further improving the conductivity of the negative electrode active material and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such conductive material is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; fluorinated carbon; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives may be used.
[0170] The above-mentioned cathode active material layer may be manufactured by applying a cathode composite material, prepared by dissolving or dispersing a cathode active material and optionally a binder and a conductive material in a solvent, onto a cathode current collector and drying it, or by casting the cathode composite material onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.
[0172] Meanwhile, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator typically used in lithium secondary batteries may be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.
[0174] In addition, the electrolytes used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing lithium secondary batteries, but are not limited to these.
[0175] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0176] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.
[0177] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the above lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2, etc., may be used. It is preferable to use the lithium salt in a concentration range of 0.1 to 4.0 M, preferably 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0179] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the above additive may be included in an amount of 0.1 to 5 parts by weight per 100 parts by weight of the total weight of the electrolyte.
[0181] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention exhibits excellent lifespan characteristics, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0182] Accordingly, according to another embodiment of the present invention, a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same are provided.
[0183] The above battery module or battery pack can be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0184] The external shape of the lithium secondary battery of the present invention is not particularly limited, but can be a cylindrical shape using a can, a prismatic shape, a pouch shape, or a coin shape.
[0185] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also preferably be used as a unit cell in a medium-to-large battery module comprising a plurality of battery cells.
[0187] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more completely explain the invention to those with average knowledge in the art.
[0189] Examples and Comparative Examples
[0190] Example 1
[0191] Ni 0.885 Co 0.035 Mn 0.08(OH)2 and LiOH were mixed such that the molar ratio of (Ni+Co+Mn):Li was 1:1.03, and then calcined at 800°C for 22 hours under an oxidizing atmosphere to produce LiNi 0.885 Co 0.035 Mn 0.08 A lithium complex transition metal oxide in the form of a single particle having a composition represented by O2 was prepared.
[0192] After mixing 2.5 parts by weight of Co(OH)2 with 100 parts by weight of the above lithium composite transition metal oxide, steam was introduced into a kiln at a rate of 2.0 kg / hour and the temperature was raised from 0°C to 500°C at a rate of 5°C / minute under an oxidizing atmosphere, then the introduction of steam was stopped and the temperature was raised from 500°C to 700°C at a rate of 5°C / minute under an oxidizing atmosphere. Then, a positive electrode active material was prepared by heat treatment while maintaining the temperature at 700°C for 2 hours under an oxidizing atmosphere to form a coating layer containing Co on the lithium composite transition metal oxide.
[0194] Example 2
[0195] Co(OH)2 was mixed with 100 parts by weight of the lithium composite transition metal oxide prepared in Example 1 at a content of 2.5 parts by weight, and steam was introduced into a kiln at a rate of 2.0 kg / hour and the temperature was raised from 0°C to 250°C at a rate of 5°C / minute under an oxidizing atmosphere, then the introduction of steam was stopped and the temperature was raised from 250°C to 700°C at a rate of 5°C / minute under an oxidizing atmosphere. Then, a positive electrode active material was prepared by heat treatment while maintaining the temperature at 700°C under an oxidizing atmosphere for 2 hours to form a coating layer containing Co on the lithium composite transition metal oxide.
[0197] Example 3
[0198] Co(OH)2 was mixed with 100 parts by weight of the lithium composite transition metal oxide prepared in Example 1 at a content of 2.5 parts by weight, and then the temperature was increased from 0°C to 250°C at a rate of 5°C / min. Then, steam was introduced into the kiln at a rate of 2.0 kg / hour, and the temperature was increased from 250°C to 500°C at a rate of 5°C / min under an oxidizing atmosphere. After that, the introduction of steam was stopped, and the temperature was increased from 250°C to 700°C at a rate of 5°C / min under an oxidizing atmosphere. Then, the temperature was maintained at 700°C under an oxidizing atmosphere for 2 hours and heat-treated to produce an anode active material having a coating layer containing Co formed on the lithium composite transition metal oxide.
[0200] Comparative Example 1
[0201] A positive electrode active material was prepared by mixing 2.5 parts by weight of Co(OH)2 with 100 parts by weight of the lithium composite transition metal oxide prepared in Example 1, increasing the temperature from 0°C to 700°C at a rate of 5°C / min under an oxidizing atmosphere, and then heat treating by maintaining the temperature at 700°C under an oxidizing atmosphere for 2 hours to form a coating layer containing Co on the lithium composite transition metal oxide.
[0203] Comparative Example 2
[0204] A positive electrode active material was prepared by mixing 2.5 parts by weight of Co(OH)2 with 100 parts by weight of the lithium composite transition metal oxide prepared in Example 1, then increasing the temperature from 0°C to 700°C at a rate of 5°C / min under an oxidizing atmosphere, and then heat treating the mixture by introducing steam into a kiln at a rate of 2.0 kg / hour and maintaining the temperature at 700°C under an oxidizing atmosphere for 2 hours to form a coating layer containing Co on the lithium composite transition metal oxide.
[0206] Comparative Example 3
[0207] 2.5 parts by weight of Co(OH)2 was mixed with 100 parts by weight of the lithium composite transition metal oxide prepared in Example 1, and steam was introduced into a calcination furnace at a rate of 2.0 kg / hour while increasing the temperature from 0°C to 500°C at a rate of 5°C / minute under an oxidizing atmosphere, then the introduction of steam was stopped and the temperature was increased from 500°C to 700°C at a rate of 5°C / minute under an oxidizing atmosphere. Then, steam was introduced into the calcination furnace at a rate of 2.0 kg / hour and heat treatment was performed while maintaining the temperature at 700°C for 2 hours under an oxidizing atmosphere to produce an anode active material having a coating layer containing Co formed on the lithium composite transition metal oxide.
[0209] Experimental Example
[0210] Experimental Example 1: Evaluation of Residual Lithium
[0211] To confirm the quality of the positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 above, the content of residual lithium present on the surface of the positive electrode active materials was measured.
[0212] Specifically, pH titration was performed to measure the content of residual lithium present on the surface of the cathode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3. A Metrohm pH meter was used, and the pH was recorded by titrating 1 mL at a time. Specifically, 5 g of the cathode active material powder prepared in Examples 1 to 3 and Comparative Examples 1 to 3 and 100 mL of distilled water were stirred. While adding a 1N HCl solution to the solution, the pH was titrated, and the content of Li2CO3 and LiOH was determined. The results are shown in Table 1 below.
[0213] Li2CO3(wt%) LiOH (wt%) Total residual lithium (Li2CO3+LiOH) (wt%) Example 1 0.13 0.08 0.21 Example 2 0.13 0.1 0.24 Example 3 0.13 0.07 0.19 Comparative Example 1 0.25 0.14 0.39 Comparative Example 2 0.29 0.26 0.55 Comparative Example 3 0.34 0.25 0.59
[0214] Through Table 1, it can be confirmed that the amount of byproducts existing in the form of Li2CO3 and LiOH on the surface of the cathode active materials prepared in Examples 1 to 3, which include a section where steam is introduced only during the heating section, is lower than the amount of byproducts (total sum of residual lithium) existing on the surface of the cathode active material prepared in Comparative Example 1, which does not include a section where steam is introduced during the heating and holding sections; the cathode active material prepared in Comparative Example 2, which includes a section where steam is introduced during the holding section; and Comparative Example 3, which includes a section where steam is introduced during the heating and holding sections.
[0216] Experimental Example 2: Evaluation of Coating Efficiency
[0217] EPMA mapping images of each of the cathode active materials prepared in Examples 1 to 3 and Comparative Example 1 are shown sequentially in Figures 1 to 4 below.
[0218] Specifically, EPMA is a technique for determining the concentration and distribution of elements within solid samples through the analysis of emitted X-rays by EDS after bombarding sample particles with an electron beam. The distribution of Co within the positive electrode active material was shown using EPMA (JXA-8350F, -15kV, 20nA stage mapping conditions) of the positive electrode active material prepared in Examples 1 to 3 and Comparative Example 1. Fig. 1 is an EPMA (ELECTRON PROBE MICROANALYSIS) mapping image of the positive electrode active material prepared in Example 1, Fig. 2 is an EPMA mapping image of the positive electrode active material prepared in Example 2, Fig. 3 is an EPMA mapping image of the positive electrode active material prepared in Example 3, and Fig. 4 is an EPMA mapping image of the positive electrode active material prepared in Comparative Example 1.
[0219] The red (dark shaded) portions in Figures 1 to 4 below represent areas where the coating layer containing Co exists in a clustered form. In the case of Comparative Example 1, which does not include a section for introducing steam during the heating section, it can be seen that the coating layer containing Co is clustered in multiple places compared to Examples 1 to 3.
[0220] In conclusion, when a section in which steam is introduced only during the heating section is included, it can be confirmed that the coating layer is formed thinly and uniformly, the concentration variation of the coating element on the positive active material is reduced, and the coating efficiency is improved.
[0222] Experimental Example 3: Evaluation of Moisture Content
[0223] To measure the moisture content present in the powders prepared in Examples 1 to 3 and Comparative Examples 1 to 3, the moisture content of each powder prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was measured using a heating moisture meter (MX-50, AND Co.), and the results are shown in Table 2 below.
[0224] Specifically, in Examples 1 to 3 and Comparative Examples 1 to 3 above, the lithium composite transition metal oxide and coating raw material were obtained immediately after passing through the section where steam was introduced, and about 5 g was placed in a sample dish inside the device. Then, the lid of the device was closed and the temperature of the sample dish was set to 130°C to evaporate the moisture contained in the lithium composite transition metal oxide and coating raw material, and the degree of mass reduction was measured. At this time, the point at which the mass no longer decreases is referred to as the completely dried state.
[0225] The moisture content (χ), that is, the percentage difference (moisture content (%)) between the mass (g) of the lithium composite transition metal oxide and coating raw material immediately after passing through the steam introduction section and the mass (g) of the lithium composite transition metal oxide and coating raw material after completely drying immediately after passing through the steam introduction section, is shown in Table 2 below.
[0226] Meanwhile, in the case of Comparative Example 1, which does not include a section for introducing steam, the percentage difference (moisture content (%)) between the mass (g) of the lithium composite transition metal oxide and the coating raw material and the mass (g) of the lithium composite transition metal oxide and the coating raw material after completely drying is shown in Table 2 below.
[0227] division Moisture content (%) Example 1 5.2 Example 2 1.7 Example 3 3.5 Comparative Example 1 0.3 Comparative Example 2 10.3 Comparative Example 3 11.7
[0228] Through Table 2, it was confirmed that in the case of Examples 1 to 3, which include a section where steam is introduced only during the heating section, the moisture content is 1.7% to 5.2%.
[0229] In conclusion, by introducing water vapor to satisfy the above moisture content, it can be seen that the by-products present on the surface of the positive electrode active material and the coating raw material reacted appropriately, and the coating became uniform overall.
Claims
Claim 1 (A) a step of preparing a lithium composite transition metal oxide by mixing a positive electrode active material precursor and a lithium (Li)-containing raw material and then calcining; and (B) a step of preparing a lithium composite transition metal oxide by mixing the lithium composite transition metal oxide and a coating raw material and then heat treating to form a coating layer on the lithium composite transition metal oxide; wherein the heat treatment includes a heating section for raising the temperature and a maintaining section for maintaining the temperature, and includes a section for introducing steam only in the heating section. Claim 2 A method for manufacturing a positive electrode active material according to claim 1, wherein the positive electrode active material precursor has a composition represented by the following chemical formula 1: [Chemical Formula 1]Ni a Mn b Co c M 1 d (OH)2 In the above chemical formula 1, M 1 is one or more selected from Al, Zr, W, Mg, Ti, Y, and B, and 0.5≤a<1, 0≤b<0.5, 0≤c<0.5, 0≤d≤0.
1. Claim 3 A method for manufacturing an anode active material according to claim 1, wherein the calcination is performed at a temperature of 700°C to 1,000°C. Claim 4 A method for manufacturing an anode active material according to claim 1, wherein the lithium composite transition metal oxide has a composition represented by the following chemical formula 2: [Chemical Formula 2]Li 1+x1 Ni a1 Mn b1 Co c1 M 2 d1 In the above chemical formula 2, O2, M 2 is one or more selected from Al, Zr, W, Mg, Ti, Y and B, and 0.0≤x1≤0.10, 0.5≤a1<1, 0≤b1<0.5, 0≤c1<0.5, 0≤d1≤0.
1. Claim 5 A method for manufacturing an anode active material according to claim 1, wherein the lithium composite transition metal oxide is in the form of a single particle. Claim 6 A method for manufacturing an anode active material according to claim 1, wherein the method does not include a washing step. Claim 7 A method for manufacturing an anode active material according to claim 1, wherein the coating raw material is a hydroxide comprising one or more selected from Co, Al, and Nb. Claim 8 A method for manufacturing an anode active material according to claim 1, wherein the coating raw material is cobalt hydroxide. Claim 9 A method for manufacturing an anode active material according to claim 1, wherein the coating raw material is mixed in an amount of 0.5 to 5 parts by weight per 100 parts by weight of the lithium composite transition metal oxide. Claim 10 A method for manufacturing an anode active material according to claim 1, wherein the heating section includes a section for introducing steam at a temperature of 600°C or lower. Claim 11 A method for manufacturing an anode active material according to claim 1, wherein the heating section has a heating rate of 1℃ / min to 10℃ / min. Claim 12 A method for manufacturing an anode active material according to claim 1, wherein the water vapor is introduced in an amount such that the moisture content (χ) according to the following Formula 1 is 1% to 10%: [Formula 1] In the above Equation 1, α is the mass (g) of the lithium composite transition metal oxide and coating raw material immediately after passing through the section where steam is introduced, and β is the mass (g) of the lithium composite transition metal oxide and coating raw material after being completely dried immediately after passing through the section where steam is introduced. Claim 13 A method for manufacturing an anode active material according to claim 1, wherein the section for introducing water vapor is performed under an oxidizing atmosphere. Claim 14 A method for manufacturing an anode active material according to claim 1, wherein the maintaining section performs heat treatment while maintaining the temperature at 500°C to 900°C. Claim 15 A method for manufacturing a positive electrode active material according to claim 1, wherein the maintenance period is performed for 1 to 12 hours. Claim 16 A method for manufacturing an anode active material according to claim 1, wherein the maintenance section does not include a section for introducing steam.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous secondary battery, manufacture thereof and nonaqueous secondary battery
JP2001052684A
Positive electrode active material for lithium secondary battery, preparing method of the same
KR1020230054296A