Epoxide functionalization of a pentaethylenehexamine adsorbent supported on macroporous silica for post-combustion co2 capture

The use of macroporous silica-supported pentaethylenehexamine with propylene oxide functionalization addresses thermal stability and diffusion issues in CO2 adsorbents, enhancing CO2 capture efficiency and reducing regeneration heat.

KR103043959B1Active Publication Date: 2026-11-11KOREA INST OF ENERGY RES
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020230050036
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2026-11-11
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Existing CO2 adsorbents face issues such as poor thermal stability, high CO2 diffusion resistance, and amine evaporation losses, particularly under 100% CO2 regeneration conditions, leading to high regeneration thermal energy requirements and inefficient CO2 capture.

Method used

A dry carbon dioxide adsorbent using macroporous silica (MPS) as a support with pentaethylenehexamine (PEHA) as the active material, functionalized with propylene oxide (PO) to enhance stability and inhibit urea formation, combined with a wet impregnation method for manufacturing.

Benefits of technology

The adsorbent achieves high CO2 adsorption capacity and stability under 100% CO2 conditions, minimizing regeneration heat and maintaining dynamic adsorption capacity throughout multiple cycles, with reduced amine evaporation and improved thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023042951819-PAT00003_ABST
    Figure 112023042951819-PAT00003_ABST
Patent Text Reader

Abstract

The present invention relates to a dry carbon dioxide adsorbent comprising a silica support and an active material impregnated in the pores of the silica support, wherein the silica support is macroporous silica (MPS) and the active material contains a stabilizing material, a method for manufacturing the adsorbent, and a method for capturing the adsorbent. The dry carbon dioxide adsorbent of the present invention, in which PEHA amine is introduced into a macroporous silica support, has high adsorption capacity under adsorption conditions, and thus possesses high dynamic adsorption capacity and low regeneration thermal energy under 100% CO2 conditions, and the PEHA amine is regenerated without the formation of urea under regeneration conditions. Furthermore, when the adsorbent of the present invention is in operation, the dynamic adsorption capacity can be stably maintained during adsorption and desorption cycle experiments, so it can be widely used in CO2 capture and utilization (CCU) technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a dry carbon dioxide adsorbent and a method for manufacturing the same, which uses macroporous silica (MPS) combining a high surface area, large porosity, and large pore volume as a support for capturing CO2 after combustion, and introduces pentaethylenehexamine (PEHA), which has a high amine content, high adsorption capacity, high thermal stability, and low cost, as an active material. Background Technology

[0003] Carbon dioxide (CO2) gas is considered the most significant cause of climate change. Consequently, CO2 capture and sequestration (CCS) technology has been extensively developed over the past decade as the concentration of greenhouse gases contributing to global warming has increased. Among the various CO2 capture methods, post-combustion CO2 capture from large-scale emission sources is being widely researched as it can be easily applied through the retrofitting of existing power plants and industries.

[0004] Carbon dioxide capture technologies to minimize carbon dioxide generation include, for example, membrane separation, adsorption processes, chemical looping combustion, and chemical absorption. However, chemical absorption is the most advanced technology, and furthermore, it can be classified into three technologies: pre-combustion, oxygen fuel combustion, and post-combustion carbon dioxide capture.

[0005] The development of CO2 adsorbents for use in water-soluble amine solutions, such as monomethanolamine (MEA), is being widely studied. While these systems are effective, they have several drawbacks, such as amine volatilization loss, corrosion, heat loss due to water vaporization, and high regeneration heat capacity.

[0006] To overcome these drawbacks, many studies have been conducted on solid adsorbents that exhibit high CO2 dynamic adsorption capacity, high stability, and low regeneration thermal energy. According to conventional technology, amine-containing propylene oxide (PO)-modified polyethyleneimine (PEI) has been developed on porous polyethylene acrylate (PO-PEI@PMA) beads. Among these, adsorbents with an amine layer (PEI and PO-PEI) have higher stability due to the increased secondary amine content. In addition, magnetic induction swing adsorption processes using a combination of Mg-MOF-74 (metal-organic framework), magnetic nanoparticles (MgFe2O4), and porous hydrophobic polymers for CO2 capture, binary PEI-tetraethylenepentamine (TEPA) mixed adsorbents, PoBC-16 (porous organic polymer) with a rigid supramolecular structure efficient for CO2 capture due to its high specific surface area and large porosity, and adsorbents in which primary amines and push-pull azobenzene units are incorporated into mesoporous silica are being researched and developed.

[0007] However, in most prior literature, the dynamic CO2 adsorption capacity of adsorbents was measured under inert conditions such as N2 or He, rather than under the 100% CO2 regeneration conditions used in industrial applications. These regeneration conditions require additional costs for high-purity CO2 separation. Therefore, the development of adsorbents capable of regeneration under 100% CO2 conditions is important.

[0008] Among solid adsorbents, PEI and TEPA are widely used due to their high adsorption capacity and stability. TEPA-based adsorbents exhibit high adsorption capacity due to their low viscosity and the high mobility of low molecular weight compounds. However, they have poor thermal stability and may experience amine evaporation losses. On the other hand, while PEI-based adsorbents offer high thermal stability, their high viscosity results in high CO2 diffusion resistance, leading to a slower CO2 adsorption rate compared to TEPA-based adsorbents. To achieve high dynamic adsorption capacity and low regeneration thermal energy under 100% CO2 conditions, the adsorbent must possess high adsorption capacity under adsorption conditions, and the amine must be regenerated without urea formation under regeneration conditions. Furthermore, the dynamic adsorption capacity of the adsorbent must be maintained stably during adsorption and desorption cycle experiments.

[0009] In the present invention, a macroporous silica (MPS) support having a high specific surface area, large porosity, and large pore volume was selected as the solid support, as this increases the adhesion of amine-based active sites, the loading amount of amine, and the dispersibility of amine. Pentaethylenehexamine (PEHA) is relatively inexpensive compared to PEI because it has a high amine content, high adsorption capacity, high thermal stability, and low cost. In addition, epoxide functionalization of PEHA was used to inhibit urea formation under regeneration conditions.

[0010] The dynamic adsorption capacity and cycle stability of the adsorbent were tested under 15% CO2 adsorption conditions and 100% CO2 desorption conditions, excluding oxidation stability tests. The morphology, surface area, pore volume, amine state distribution, and amine loading of the dry carbon dioxide adsorbent were determined using scanning electron microscopy (SEM), Brunauer-Emmett-Teller (BET), Hg porosity measurement, nuclear magnetic resonance spectroscopy (C-NMR), thermogravimetric analysis (TGA), and elemental analysis (EA). The dynamic CO2 adsorption capacity of the dry adsorbent was measured by TGA. The problem to be solved

[0012] The technical problem that the present invention aims to solve is to provide a dry carbon dioxide adsorbent in which PEHA amine is introduced into a macroporous silica support (MPS) manufactured to overcome the disadvantages of TEPA-based adsorbents, which have poor thermal stability and may experience amine evaporation loss, and PEI-based adsorbents, which have high thermal stability but high CO2 diffusion resistance due to high viscosity and slow CO2 adsorption rate, and a method for manufacturing the same.

[0013] In addition, we aim to provide a dry carbon dioxide adsorbent that uses less regeneration heat, can be used under adsorption and desorption conditions similar to actual process conditions, and minimizes sensible heat, reaction heat, and latent heat of vaporization, as well as a method for manufacturing the same.

[0015] However, the technical problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned technical problems will be clearly understood by those skilled in the art to which the present invention belongs from the description below. means of solving the problem

[0017] In order to achieve the above technical problem, one aspect of the present invention is,

[0018] A dry carbon dioxide adsorbent is provided, comprising: a silica support; and an active material impregnated in the pores of the silica support; wherein the silica support is macroporous silica (MPS) and the active material contains a stability material.

[0019] The BET surface area of ​​the above silica is 450 m² 2 / g to 500m 2 It may be characterized as being macroporous silica with a g / g content.

[0020] The pore volume of the above silica is 6.5 cm³ 3 / g to 7.5 cm 3It may be characterized as being a macroporous silica with a g / g content.

[0021] The above silica may be characterized as being macroporous silica with a pore size of 20 nm to 500 nm.

[0022] The above stability material may be characterized as being PO (propylene oxide).

[0023] The above active substance may be tetraethylenepentamine (TEP) or pentaethylenehexamine (PEHA), and may be characterized in that the amine group at the terminal end of the active substance reacts with the stability substance to form a secondary amine or a tertiary amine.

[0025] Another aspect of the present invention is,

[0026] A method for manufacturing a dry carbon dioxide adsorbent is provided, comprising the steps of: preparing a macroporous silica support (S100); preparing a mixture by adding a stability material to an active material (S200); and stirring the macroporous silica support and the mixture (S300), and characterized by using a wet impregnation method.

[0027] In the above S200 step, the stability material is PO (propylene oxide), the active material is tetraethylenepentamine (TEP) or pentaethylenehexamine (PEHA), and the stability material may be added after dissolving the active material in a solvent.

[0028] In the above S200 step, the mixture may be stirred at 20 to 30°C for 22 to 26 hours, and the stirred mixture may be dried under vacuum at 60 to 80°C for 46 to 50 hours.

[0029] In the above S300 step, the macroporous silica and the mixture may be introduced into a solvent and stirred, and the stirred mixture may be dried at 60 to 80°C for 22 to 26 hours.

[0031] Another aspect of the present invention is,

[0032] A method for adsorbing and desorbing a dry carbon dioxide adsorbent according to claim 1 is provided, characterized in that adsorption is performed under conditions of 10 to 15 vol% CO2 and desorption is performed under conditions of 100 vol% CO2 based on 100 vol% of the total gas introduced into the process.

[0033] The above adsorption and desorption may be characterized by being performed after pretreatment with nitrogen (N2) gas.

[0034] When H2O adsorption is minimized by the above adsorption time of 8 to 15 minutes, the regeneration heat of the adsorbent is 2.8 to 3.0 GJ tCO2 - 1 It may be characterized by being.

[0035] Even if the above adsorption and desorption experiments are repeated 20 or more times, the working capacity may be maintained at 90% or more compared to the initial cycle. Effects of the invention

[0037] According to one aspect of the present invention, macroporous silica (MPS) used as a support has a high specific surface area, large porosity and large pore volume, which increases the adhesion of amine-based active sites, the loading amount of amine, and the dispersibility of amine.

[0038] According to one aspect of the present invention, PEHA amine (Pentaethylene-hexaimne) has a high amine content, high adsorption capacity, high thermal stability, and low cost. In addition, epoxide functionalization of PEHA is used to inhibit urea formation under regeneration conditions.

[0039] According to one aspect of the present invention, a carbon dioxide adsorbent in which PEHA amine is introduced into a macroporous silica support has high adsorption capacity under adsorption conditions, and thus has high dynamic adsorption capacity and low regeneration heat under 100% CO2 conditions, and PEHA amine is regenerated without the formation of urea under regeneration conditions. In addition, the dynamic adsorption capacity of the adsorbent of the present invention is stably maintained during adsorption and desorption cycle experiments.

[0040] According to one aspect of the present invention, silica, which is a support for the dry carbon dioxide adsorbent of the present invention, can be impregnated with an active material content of up to 70%, and by combining PO (propylene oxide) therewith, stability can be improved.

[0042] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the composition of the invention described in the description or claims of the present invention. Brief explanation of the drawing

[0044] Figure 1 shows scanning electron microscope (SEM) data of the polystyrene precursor (Figs. 1a, 1b) and macroporous silica (Figs. 1c, 1d) of macroporous silica (MPS) in Example 1. Figure 2 shows data regarding the cumulative pore analysis (Fig. 2a) and pore volume distribution (Fig. 2b) of the macroporous silica (MPS) support. Figure 3 shows data representing the nuclear magnetic resonance spectroscopy (NMR) spectra of PEHA amine (Fig. 3a) and 2.0 PO-PEHA (Fig. 3b) in Example 2. Figure 4 shows the EDS-SEM mapping image and corresponding elemental mapping image of PO-PEHA. Figure 5 shows the thermogravimetric analysis (TGA) curve data of the PO-PEHA / MPS adsorbent in Example 3. Figure 6 shows data representing the adsorption isotherms of the MPS support and the PO-PEHA / MPS adsorbent. Figure 7 shows the PO-PEHA / MPS adsorbent This is data regarding the isobaric CO2 adsorption amount according to temperature. Fig. 7a is under conditions of 15% CO2 and balanced N2, and Fig. 7b is under conditions of 100% CO2. Fig. 8 is data regarding the temperature swing adsorption (TSA) of the PO-PEHA / MPS adsorbent according to temperature. Fig. 9 is data regarding the CO2 adsorption and desorption stability test of the PO-PEHA / MPS adsorbent. The adsorption conditions are 15% CO2 and 85% N2 for 30 minutes at 50°C, and the desorption conditions are 100% CO2 for 10 minutes at 120°C. Fig. 9a is the CO2 adsorption and desorption curve, and Fig. 9b concerns the dynamic adsorption capacity of the material during the adsorption and desorption cycle. Fig. 10 is data regarding the CO2 dynamic adsorption capacity of the PO-PEHA / MPS adsorbent. The dry feed conditions are 15% CO2 and 85% N2 at 50°C for 30 minutes under adsorption conditions, and 100% CO2 at 120°C for 10 minutes under desorption conditions. The wet feed conditions are 15% CO2, 3% H2O, and 72% N2 at 50°C for 30 minutes under adsorption conditions, and 100% CO2 at 120°C for 10 minutes under desorption conditions.Figure 11 shows (a) the adsorption-desorption graph of a second-cycle PO-PEHA / MPS adsorbent under wet, dry, and H2O conditions, and (b) comparative data on regeneration heat according to adsorption time. Figure 12 shows comparative data on the regeneration heat of the PO-PEHA / MPS adsorbent according to adsorption time. Specific details for implementing the invention

[0045] The present invention will be described in more detail below with reference to the attached drawings. However, the present invention may be implemented in various different forms and is therefore not limited to the embodiments described herein. Furthermore, in order to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification have been given similar reference numerals.

[0046] Throughout the specification, when it is stated that a part is "connected (connected, in contact, combined)" with another part, this includes not only cases where they are "directly connected," but also cases where they are "indirectly connected" with other members interposed between them. Furthermore, when it is stated that a part "includes" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.

[0047] The terms used herein are merely for describing specific embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “comprising” or “having” are intended to indicate the presence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0048] In describing the present invention, if it is determined that a detailed description of related known configurations or functions could obscure the essence of the invention, such detailed description may be omitted.

[0050] The first aspect of the present invention is,

[0051] A dry carbon dioxide adsorbent is provided, comprising: a silica support; and an active material impregnated in the pores of the silica support; wherein the silica support is macroporous silica (MPS) and the active material contains a stability material.

[0053] Hereinafter, a dry carbon dioxide adsorbent according to the first aspect of the present invention is described.

[0055] In one embodiment of the present invention, as shown in FIG. 1, the MPS structure (Fig. 1c, d) was prepared using a polystyrene sphere of about 1 μm (Fig. 1a, b) as a template for the macropores. As shown in the cross-sectional SEM images of FIG. 1c and d, the MPS structure is monodisperse, with spherical macropores of about 600 nm separated by walls. The windows of the silica walls formed a hierarchical structure between the macropores, and this hierarchical structure of the solid adsorbent can improve CO2 capture performance.

[0056] In one embodiment of the present invention, since nitrogen (N2) adsorption cannot measure pore sizes much larger than 20 nm, Hg porosimetry was performed to measure the macropores of the silica support. Figure 2 shows the measurement of Hg penetration and pore size distribution of MPS.

[0057] In one embodiment of the present invention, the BET surface area of ​​the silica is 400 m² 2 / g or more, 420m 2 / g or more, 450m 2 / g or more, 470m 2 It may be / g or more, and 550m 2 / g or less, 530m 2 / g or less, 500m 2 / g or less, 480m 2 It may be / g or less, most preferably 470m 2 / g to 480m 2 It may be macroporous silica with a pore size of 1 / g. If the pore size is below the range described above, the attachment of amine-based active sites, loading of amines, and dispersion of amines may not be properly performed, and CO2 capture may not be carried out smoothly. If the pore size exceeds the range described above, an unnecessarily large silica support is required, so the size of the carbon dioxide adsorbent may become larger than necessary.

[0058] In one embodiment of the present invention, the pore volume of the silica is 3.0 cm³ 3 / g or more, 4.0 cm 3 / g or more, 5.0 cm 3 / g or more, 6.0 cm 3 / g or more, 6.5 cm 3 It may be / g or more, and 9.0 cm 3 / g or less, 8.0 cm 3 / g or less, 7.5 cm 3 / g or less, 7.0 cm 3 It may be / g or less, most preferably 6.5 cm 3 / g to 7.0 cm 3 It may be macroporous silica with a pore size of / g. If it is below the above-mentioned range, it may be difficult to load a large amount of amine, which is an active material for CO2 adsorption, and if it exceeds the above-mentioned range, there is a risk that the pore volume of the silica will become too large and lose its function as a support.

[0059] In one embodiment of the present invention, the pore size of the silica may be 50 nm or more, 70 nm or more, 100 nm or more, 130 nm or more, 150 nm or more, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, and most preferably macroporous silica of 150 nm to 200 nm. If the size is less than the above-described range, it may be difficult to load a large amount of amine, which is an active material for CO2 adsorption, and if the size exceeds the above-described range, there is a risk that the pore volume of the silica will become too large and lose its function as a support.

[0060] In one embodiment of the present invention, this hierarchical pore size distribution combining the high surface area of ​​micropores and mesopores with the accessible diffusion pathway of macropores can be advantageous for high CO2 capture performance.

[0061] In one embodiment of the present invention, the pore size of the silica was measured by Hg porosimetry. The pore size distribution through N2 adsorption can only be measured when the silica support has pores in the range of 20 nm or less. Therefore, since pore sizes much larger than 20 nm cannot be measured, Hg porosimetry was performed to measure the macropores of the silica support.

[0062] In one embodiment of the present invention, the mercury porosimetry method (Hg porosimetry) described above is described in detail. When mercury comes into contact with other substances, the cohesive force that causes mercury to clump together is much stronger than the adhesive force that acts with other substances. This property of mercury is called non-wetting. By utilizing this non-wetting property of mercury, external pressure is applied to forcibly inject mercury into the pores of a porous sample. Based on the amount of mercury injected according to the pressure, the diameter and volume of the pores can be measured, and the density and porosity of the pores can also be measured.

[0063] In one embodiment of the present invention, the stability material may be characterized as being PO (propylene oxide). PO has the molecular formula C3H6O, is a colorless liquid, and in the present invention, it was used for the functionalization of PEHA to inhibit urea formation during carbon dioxide adsorption.

[0064] In one embodiment of the present invention, the active substance may be an amine compound, such as tetraethylenepentamine (TEP) or pentaethylenehexamine (PEHA), and may be characterized in that the amine group at the terminal end of the active substance reacts with the stability substance to form a secondary amine or a tertiary amine.

[0065] In one embodiment of the present invention, the ratio of primary, secondary, and tertiary amines is related to the CO2 adsorption capacity and stability of the solid adsorbent, and C-NMR was performed to quantify the amine state distribution of PEHA and 2.0PO-PEHA. The amine state distribution was determined using the following chemical formula.

[0066]

[0068] In one embodiment of the present invention, the amine state distribution of PEHA and the functionalization of PEHA (2.0 PO-PEHA) are shown in FIG. 3. As shown in FIG. 3a, pristine PEHA was represented with a primary (1°) / secondary (2°) / tertiary (3°) amine ratio of 46:54:0. After PO functionalization, the amine state distribution changed to a primary (1°) / secondary (2°) / tertiary (3°) amine ratio of 14:78:8 ( FIG. 3b).

[0069] In one embodiment of the present invention, many primary amines were converted to secondary amines, and some secondary amines were converted to tertiary amines. While a decrease in the primary amine content may reduce the CO2 adsorption capacity, an increase in the secondary and tertiary amine content may improve the oxidation stability of the solid adsorbent.

[0070] In one embodiment of the present invention, the EDS-SEM mapping image shown in FIG. 4 illustrates the distribution of various elements in the 2.0-PO-PEHA / MPS adsorbent. Each element is uniformly dispersed within the porous support, and the N element of the 2.0-PO-PEHA / MPS is uniformly distributed, indicating that a large amount of PO-PEHA has been introduced into the MPS support.

[0071] In one embodiment of the present invention, the amine loading was estimated from the total organic loading weight loss at 100 to 500°C based on TGA curves. Weight loss of MPS occurred almost in the temperature range, and consequently, the thermal stability of 2.0-PO-PEHA / MPS was affected by the amine. The amine loading of the 2.0-PO-PEHA / MPS adsorbent was 70 wt%, as expected from the prepared amount (Fig. 5). The adsorbent exhibited high thermal stability with respect to the decomposition temperature, and this result occurred because the weight did not change even at temperatures exceeding the desorption temperature of 120°C. The amine loading of the adsorbent was 10.2 mmol Ng through elemental analysis. -1 It was measured as.

[0072] In one embodiment of the present invention, the micropores and mesopores of the MPS support before and after 2.0 PO-PEHA loading were analyzed using N2 adsorption-desorption measurements. A loss of surface area indicates high amine introduction into the support.

[0073] In one embodiment of the present invention, as shown in Table 1 below, it can be seen that the MPS support has large porosity and pore volume. After loading 2.0PO-PEHA, porosity and pore volume decreased by 23.3% and 82.6%, respectively. This result shows that the large internal pores of the MPS support provide sufficient space for high amine loading. High amine loading of the 2.0PO-PEHA / MPS adsorbent is expected to increase CO2 adsorption capacity.

[0074] Sample Porosity (%) Pore ​​surface area (m²) 2 / g) Pore ​​volume (cm²) 3 / g) MPS 87.59 168 6.84 2.0PO-PEHA / MPS 67.17 5.63 1.19

[0075] In one embodiment of the present invention, isothermal CO2 adsorption at 50°C at a CO2 partial pressure for the 2.0 PO-PEHA / MPS adsorbent is shown in FIG. 6. It can be seen that the adsorption capacities of 2.0 PO-PEHA / MPS at CO2 partial pressures of 0.15 bar and 1.0 bar are 2.5 mmol g-1 and 3.1 mmol g-1, respectively.

[0077] The present invention provides a method for manufacturing a dry carbon dioxide adsorbent, comprising the steps of: preparing a macroporous silica support (S100); preparing a mixture by adding a stabilizing material to an active material (S200); and stirring the macroporous silica support and the mixture (S300), and characterized by using a wet impregnation method.

[0079] Detailed explanations have been omitted for parts that overlap with the first aspect of the present invention; however, the content described in the first aspect of the present invention may be applied equally even if such explanations are omitted in the second aspect.

[0081] Hereinafter, a method for manufacturing a dry carbon dioxide adsorbent according to the second aspect of the present invention will be described in detail.

[0083] First, in one embodiment of the present invention, in step S200, the stability material is PO (propylene oxide) and the active material is tetraethylenepentamine (TEPA) or pentaethylenehexamine (PEHA), and the stability material may be added after dissolving the active material in a solvent.

[0084] In one embodiment of the present invention, in step S200, the mixture may be stirred at 20 to 30°C for 22 to 26 hours, and the stirred mixture may be dried under vacuum at 60 to 80°C for 46 to 50 hours. If stirring and drying are performed below the range described above, sufficient stirring and drying may not occur, which may result in problems with the effectiveness of the dry carbon dioxide adsorbent.

[0085] In one embodiment of the present invention, in step S300, the macroporous silica and the mixture are introduced into a solvent and stirred, and the stirred mixture is dried at 60 to 80°C for 22 to 26 hours. If drying is performed for less than the range described above, sufficient drying is not achieved, which may result in problems with the effectiveness of the dry carbon dioxide adsorbent.

[0087] The third aspect of the present invention provides a method for adsorbing and desorbing a dry carbon dioxide adsorbent according to claim 1, characterized in that adsorption is performed under conditions of 10 to 15 vol% CO2 and desorption is performed under conditions of 100 vol% CO2 based on 100 vol% of the total gas introduced into the process.

[0089] Detailed explanations have been omitted for parts that overlap with the first aspect of the present invention; however, the content explained in the first aspect of the present invention may be applied in the same way even if such explanation is omitted in the third aspect.

[0091] Hereinafter, a method for capturing a dry carbon dioxide adsorbent according to the third aspect of the present invention will be described in detail.

[0093] In one embodiment of the present invention, the process may be characterized by being performed after pretreatment with nitrogen (N2) gas before the adsorption and desorption.

[0094] In one embodiment of the present invention, when H2O adsorption is minimized by the adsorption time being 8 to 15 minutes, the regeneration heat of the adsorbent is 2.8 to 3.0 GJ tCO2 - 1 It may be characterized by being.

[0095] In one embodiment of the present invention, as shown in FIG. 11b, when the adsorption time is 42 minutes, the heat of regeneration is 4.10 GJ tCO2 -1 ...and when the adsorption time was reduced to 9 minutes, the regeneration heat was 2.86 GJ tCO2 -1 Considering CO2 dynamic adsorption capacity and H2O adsorption, since a large amount of latent heat was required for H2O desorption, reducing H2O adsorption is important to minimize regeneration heat even if CO2 dynamic adsorption capacity is slightly reduced.

[0096] In one embodiment of the present invention, the regeneration heat of 2.0 PO-PEHA / MPS (2.86 GJ tCO2 -1 ) is an MEA process that generally assumes 90% sensible heat recovery (2.7-3.3 GJ tCO2 1 It was similar to ). This value was obtained under 100% CO2 conditions for high-purity CO2 separation, not under inert conditions such as N2 or He.

[0097] In one embodiment of the present invention, even if the adsorption and desorption are repeated 20 or more times, the dynamic adsorption capacity may be maintained at 90% or more compared to the initial cycle.

[0098] In one embodiment of the present invention, the repeated experiment was subsequently conducted through 20 consecutive TSA cycles to investigate the long-term stability of the adsorbent. Adsorption conditions were performed at 50°C under 15% CO2 and 85% N2, and desorption conditions were performed at 120°C under 100% CO2. As shown in Fig. 9, the dynamic adsorption capacity of 2.0 PO-PEHA / MPS was 1.8 mmol / g, and the working capacity remained constant without decreasing during 20 cycles.

[0099] In one embodiment of the present invention, since the first cycle was adsorbed after N2 pretreatment rather than under 100% CO2 regeneration conditions, the dynamic adsorption capacity from the 2nd to the 21st adsorption cycles was compared. Functionalization of PHEA using PO inhibited urea formation by reducing the amine content and increasing steric hindrance. As a result, 2.0PO-PEHA / MPS maintained stability during 20 consecutive TSA cycles.

[0100] In one embodiment of the present invention, 20 consecutive TSA cycles were performed on the adsorbent to investigate CO2 adsorption in the presence of water vapor. CO2 and H2O adsorption were recorded as 15% CO2, 3% H2O, and 72% N2 under wet conditions at 50°C. As shown in Fig. 10, the dynamic adsorption capacity was 7.9 wt% under dry conditions and 14.0 wt% under wet conditions.

[0101] In one embodiment of the present invention, the dynamic adsorption capacity was found to be higher under wet conditions than under dry conditions due to H2O adsorption. The weight measured under wet conditions (CO2 15%, H2O 3%, 72% N2) was considered as the amount of CO2 and H2O adsorbed (14.0 wt%).

[0102] In one embodiment of the present invention, cycle tests were performed under wet, dry, and H2O conditions to reduce H2O adsorption. The dry condition consisted of adsorption of 15% CO2 and 75% N2 at 50°C and regeneration under 100% CO2 conditions at 120°C. The wet condition consisted of adsorption of 15% CO2, 3% H2O, and 72% N2 at 50°C and regeneration under 100% CO2 conditions at 120°C. The H2O condition consisted of adsorption of 3% H2O and 97% N2 at 50°C and regeneration under 100% N2 conditions at 120°C.

[0103] In one embodiment of the present invention, as shown in FIG. 11a, CO2 adsorption in the dry state was almost completed in 14 minutes, and H2O adsorption in the H2O state continued even after 14 minutes. The increase in the amount of adsorption after 14 minutes under wet conditions can be interpreted as indicating that H2O adsorption continues due to the pores remaining after CO2 adsorption is completed. When the adsorption time of the adsorbent exceeds 14 minutes, CO2 adsorption remains constant while only H2O adsorption increases. H2O adsorption can be minimized by controlling the adsorption time of the adsorbent.

[0105] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0107] Example 1 : Preparation of macroporous silica (MPS)

[0108] First, 0.2 g of PVP was dissolved in ethanol (500 ml). Styrene monomer (44 ml) was added to the solution and stirred at room temperature for 10 minutes. The mixture was stirred at 70°C for 30 minutes. Finally, an aqueous solution of APS (0.652 g in 60 ml of distilled water) was added to the mixture. The mixture was stirred at 70°C for 24 hours, and after the reaction was complete, the reactor was quenched in an ice bath. Subsequently, the solid was separated by centrifugation and washed with ethanol. The solid was dried under vacuum at 70°C for 12 hours.

[0109] A solution was prepared by dissolving 10 g of P123, 9 g of distilled water, and 0.6 g of 2M HCl in 77 ml of ethanol. After completely dissolving the P123, 20.8 g of TEOS was added to the solution and stirred for 10 minutes. Subsequently, a polystyrene suspension (8 g in 100 ml of ethanol) was added to the solution and stirred overnight. The mixture was separated by centrifugation and washed with ethanol. The precipitate was dried under vacuum at 60°C for 48 hours. The obtained solid was calcined in air at 550°C for 12 hours.

[0111] Example 2 : PEHA of amine (Pentaethylene-hexaimne) manufacturing

[0112] To inhibit urea formation during CO2 adsorption, PEHA was functionalized using PO. 8.6 mmol PEA was dissolved in methanol (3 ml), and 17.2 mmol PO was added dropwise to the mixture. The mixture was stirred at ambient temperature for 24 hours. The resulting solid was vacuum dried at 70°C for 48 hours. The functionalized PEHA is denoted as xPO-PEPA, where x represents the molar ratio of PO to PEHA.

[0114] Example 3 : PO- PEHA Manufacture of / MPS adsorbent

[0115] MPS-supported amine adsorbents (PO-PEHA / MPS) are prepared using a wet impregnation method. A mixture of 2.0% PO-PEHA (70 wt%) and MPS support (30 wt%) was stirred in a methanol solution. After stirring overnight, the mixture was dried in an oven at 70°C for 24 hours.

[0117] Experimental Example 1 : PO- PEHA / MPS Adsorbent Characterization

[0118] 1. Scanning electron microscope ( SEM ) analyze

[0119] Field emission scanning electron microscope (FE-SEM) images were analyzed using a Hitachi S-4800 instrument operating at 15 kV. The corresponding results are shown in Figure 1.

[0121] 2. BET surface area

[0122] The BET method was used to determine a specific surface area.

[0124] 3. Mercury porosity measurement (Hg porosimetry ) by Measurement of pore volume and pore size

[0125] Mercury intrusion porosimetry was used to analyze the surface area and pore volume of macropores (AutoPore V9600, Micromeritics, USA).

[0127] 4. amine Distribution characterization, amine Loading and elemental content analysis

[0128] C-NMR (600 MHz Avance III, Bruker, USA) was used to quantitatively analyze the ratios of primary, secondary, and tertiary amines.

[0129] Amine loading was measured by TGA (SDT Q600, TA Instruments, USA) at a heating rate of 10°C / min in an N2 atmosphere from 25°C to 500°C. The nitrogen element content of the adsorbent was analyzed using an elemental analyzer (EA, CHN628C, LECO Corporation, USA).

[0131] Experimental Example 2: PO - PEHA / MPS Adsorbent Isostatic Test

[0132] TGA experiments were performed under isobaric conditions to determine the effect of CO2 adsorption on the adsorption temperature and desorption temperature for a given CO2 partial pressure. These experiments were conducted from room temperature up to 150°C. 15% CO2 and 75% N2 gas were used to determine the adsorption temperature, and 100% CO2 gas was used to determine the desorption temperature.

[0134] Experimental Example 3 : PO- PEHA / MPS Adsorbent CO2 and H2O Adsorption-Desorption Experiment

[0135] CO2 adsorption-desorption experiments were performed using a thermogravimetric analyzer (TGA 8000, Perkin Elmer, USA). Prior to measurement, the adsorbent underwent a pretreatment process at 110°C for 30 minutes under an N2 flow rate (40 cm³ min⁻¹). Adsorption experiments were conducted at 50°C using a simulated gas containing 15% CO2, 3% H2O, and 72% N2. H2O vapor was generated using a moisture saturator. After 30 minutes of adsorption, the gas was subjected to a 100% CO2 flow rate (40 cm³ min⁻¹). 3 min -1 Switch to ), and 5℃ min -1 It was gradually heated to 120°C at a rate. The temperature was maintained for 10 minutes to regenerate the adsorbent. The dynamic adsorption capacity of CO2 and H2O was measured based on the weight change of TGA.

[0137] The CO2 adsorption and desorption cycle experiments of the adsorbent were investigated in a temperature-dependent adsorption and desorption (TSA) cycle using TGA. First, as shown in Figure 7, experiments were conducted to determine the adsorption and desorption temperatures of the adsorbent. Figure 7a shows the isobaric CO2 adsorption of the 2.0 PO-PEHA / MPS adsorbent under conditions of 15% CO2 and 75% N2. CO2 adsorption reaches a maximum value at approximately 40–50°C and drops to a minimum value at approximately 110°C. Although the highest CO2 adsorption amount was observed at 40°C, there was no significant difference compared to the CO2 adsorption amount at 50°C; thus, sensible heat could be reduced by selecting 50°C as the adsorption temperature, which is close to 60°C, the exhaust gas temperature for CO2 capture after combustion.

[0138] Figure 7b shows the isobaric CO2 adsorption of the 2.0 PO-PEHA / MPS adsorbent under 100% CO2 conditions. Desorption under 100% CO2 conditions is required for high-purity CO2 separation. Good desorption performance was observed, with the CO2 adsorption amount being closest to zero at 130°C. However, since the CO2 adsorption amount was negative at 130°C and there were concerns regarding stability during continuous cycle experiments, 120°C was selected as the desorption temperature.

[0139] Next, cycle experiments were performed based on selected adsorption and desorption temperatures. For the adsorption conditions, a simulated gas containing 15% CO2 and 75% N2 at 50°C was used, and for the adsorbent regeneration conditions, 100% CO2 gas at 120°C was used to simulate experimental conditions similar to actual industrial conditions for post-combustion CO2 capture.

[0140] As shown in Fig. 8, the initial adsorption amount was 2.2 mmol / g (Fig. 8a) because adsorption proceeded after N2 pretreatment. The adsorption amount in the second cycle was 1.8 mmol / g (Fig. 8c), which was lower than that of the first cycle because the process was performed after regeneration under 100% CO2 conditions (Fig. 8b) rather than 100% N2 conditions. The CO2 adsorption amount (Fig. 8c) and CO2 regeneration amount (Fig. 8d) in the second cycle were also found to be 1.8 mmol / g. These results confirmed that the adsorbent stably maintains dynamic adsorption capacity under 100% CO2 regeneration conditions.

[0142] Subsequently, the long-term stability of the adsorbent was investigated over 20 consecutive TSA cycles (adsorption at 50°C: 15% CO2, 75% N2; desorption at 120°C: 100% CO2). As shown in Figure 9, the working capacity of 2.0 PO-PEHA / MPS was 1.8 mmol / g, and the working capacity remained constant without decreasing during the 20 cycles.

[0143] Since the first cycle was adsorbed after N2 pretreatment rather than under 100% CO2 regeneration conditions, the working capacity from the 2nd to the 21st adsorption cycles was compared. Functionalization of PHEA using PO inhibited urea formation by reducing the 1° amine content and increasing steric hindrance. Consequently, 2.0PO-PEHA / MPS maintained stability during 20 consecutive TSA cycles.

[0144] In addition, to investigate CO2 adsorption in the presence of moisture, the adsorbent was subjected to 20 consecutive TSA cycles. CO2 and H2O adsorption were recorded as 15% CO2, 3% H2O, and 72% N2 under wet conditions at 50°C. As shown in Figure 10, the dynamic adsorption capacity was 7.9 wt% under dry conditions and 14.0 wt% under wet conditions. The dynamic adsorption capacity was higher under wet conditions than under dry conditions due to H2O adsorption. The weight measured under wet conditions (15% CO2, 3% H2O, 72% N2) was considered as the CO2 and H2O adsorption amount (14.0 wt%).

[0145] Next, the weight measured under dry conditions (15% CO2, 75% N2) was considered as the CO2 adsorption amount (7.9 wt%). Finally, neglecting the effect of H2O co-adsorption on CO2 adsorption, the difference between the weight under wet conditions and the weight under dry conditions was considered as the H2O adsorption amount (6.1 wt%). The negligible effect of H2O co-adsorption on CO2 adsorption has also been confirmed in conventional technology, which may imply that there is little competition for adsorption sites between CO2 and H2O. Although H2O adsorption was somewhat high, the adsorbent maintained stability during 20 consecutive TSA cycles.

[0146] To reduce H2O adsorption, cycle tests were performed under wet, dry, and H2O conditions. The dry condition consisted of 15% CO2 and 75% N2 adsorption at 50°C, and 100% CO2 regeneration at 120°C. The wet condition consisted of 15% CO2, 3% H2O, and 72% N2 adsorption at 50°C, and 100% CO2 regeneration at 120°C. The H2O condition consisted of 3% H2O and 97% N2 adsorption at 50°C, and 100% N2 regeneration at 120°C.

[0147] As shown in Fig. 11a, CO2 adsorption in the dry state was almost completed in 14 minutes, and H2O adsorption in the H2O state continued even after 14 minutes. The increase in adsorption amount after 14 minutes under wet conditions can be interpreted as H2O adsorption continuing due to the pores remaining after CO2 adsorption is completed. When the adsorption time of the adsorbent exceeded 14 minutes, CO2 adsorption remained constant while only H2O adsorption increased. H2O adsorption can be minimized by adjusting the adsorption time of the above adsorbent. When the adsorption time was 42 minutes, the CO2 working capacity was 7.7 wt% (1.8 mmol / g) and H2O adsorption was 6.4 wt% (3.6 mmol / g). However, when the adsorption time was reduced to 9 minutes, the CO2 working capacity and H2O adsorption changed to 5.0 wt% (1.2 mmol / g) and 1.0 wt% (0.6 mmol / g), respectively.

[0149] Experimental Example 4 : Regeneration heat

[0150] The regeneration heat was calculated based on the results obtained in Experimental Example 3 above. The regeneration heat for adsorbent regeneration can be calculated using the following chemical formula 2.

[0151]

[0153] Q r (GJ tCO2 -1 ) is the regenerative heat requirement, q w (mmol g -1 ) is the CO2 dynamic adsorption capacity, and α, β, and γ are the ratios of heat recovered from sensible heat, adsorption heat, and latent heat of vaporization, respectively. C p,s (kJ kg -1 °C -1 ) is the specific heat capacity of the adsorbent, T ad (°C is the adsorption temperature, T de (°C is the desorption temperature, △H a (kJ mol -1 ) is the heat of adsorption, Q v (kJ kg -1 ) is the heat of vaporization of water, f H2O(mmol g -1 ) represents the amount of moisture adsorbed.

[0154] As shown in Fig. 11b, when the adsorption time is 42 minutes, the heat of regeneration is 4.10 GJ tCO2 -1 ...and when the adsorption time was reduced to 9 minutes, the regeneration heat was 2.86 GJ tCO2 -1 Considering CO2 dynamic adsorption capacity and H2O adsorption, it can be seen that reducing H2O adsorption is important to minimize regeneration heat, even if CO2 dynamic adsorption capacity decreases slightly. This result occurred because a large amount of latent heat is required for H2O desorption (Table 2 and Figure 12).

[0155] parameters Adsorption: 42 minutes Attachment / Removal: 9 minutes α 0.75* 0.75* β 0 0 γ 0 0 q w (mmol g -1 ) 1.74 1.15 C p,s (kJ kg -1 °C -1 ) 1.54 1.54 T ad (℃) 50 50 T de (℃) 120 120 △H (kJ mol) -1 ) 82 82 Q v (kJ kg -1 ) 2257.6 2257.6 f H2O (mmol g -1 ) 3.56 0.58

[0156] * It was assumed that a 75% sensible heat recovery rate could be achieved through process optimization.

[0158] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical spirit or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.

[0159] The scope of the present invention is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention.

Claims

Claim 1 It comprises a silica support; and an active material impregnated in the pores of the silica support; wherein the silica support is macroporous silica (MPS), the active material is pentaethylenehexamine (PEHA), the active material contains a stabilizing material, the stabilizing material is propylene oxide (PO), the amine groups at the terminals of the PEHA react with the PO to form a secondary or tertiary amine, and the ratio of the primary amine / secondary amine / tertiary amine of the PEHA after reaction with the PO is 14:78:8 based on C-NMR quantitative analysis, the active material is uniformly dispersed within the pores of the silica support, and the BET surface area of ​​the silica is 5.63 m² 2 / g, and the pore volume of the silica before loading the active substance is 6.5 cm³ 3 / g to 7.5 cm 3 A dry carbon dioxide adsorbent characterized by having a weight of / g. Claim 2 delete Claim 3 delete Claim 4 A dry carbon dioxide adsorbent according to claim 1, characterized in that the silica is macroporous silica with a pore size of 20 nm to 500 nm. Claim 5 delete Claim 6 delete Claim 7 A method for manufacturing a dry carbon dioxide adsorbent according to claim 1, comprising the steps of: preparing a macroporous silica support (S100); preparing a mixture by adding a stability material to an active material (S200); and stirring the macroporous silica support and the mixture (S300); using a wet impregnation method, wherein in step S200, the stability material is PO (propylene oxide) and the active material is pentaethylenehexamine (PEHA), and the stability material is added after dissolving the active material in a solvent. Claim 8 delete Claim 9 A method for manufacturing a dry carbon dioxide adsorbent according to claim 7, characterized in that, in step S200, the mixture is stirred at 20 to 30°C for 22 to 26 hours, and the stirred mixture is dried under vacuum at 60 to 80°C for 46 to 50 hours. Claim 10 A method for manufacturing a dry carbon dioxide adsorbent according to claim 7, characterized in that, in step S300, the macroporous silica and the mixture are introduced into a solvent and stirred, and the stirred mixture is dried at 60 to 80°C for 22 to 26 hours. Claim 11 A method for adsorption and desorption of a dry carbon dioxide adsorbent according to claim 1, characterized in that adsorption is performed under conditions of 10 to 15 vol% CO2 and desorption is performed under conditions of 100 vol% CO2 based on 100 vol% of the total gas introduced into the process. Claim 12 A method for capturing a dry carbon dioxide adsorbent, characterized in that, in claim 11, the adsorption and desorption are performed after pretreatment with nitrogen (N2) gas. Claim 13 In claim 11, when H2O adsorption is minimized by the adsorption time being 8 to 15 minutes, the regeneration heat of the adsorbent is 2.8 to 3.0 GJ tCO2 -1 A method for capturing a dry carbon dioxide adsorbent characterized by the following: Claim 14 A method for capturing a dry carbon dioxide adsorbent according to claim 11, wherein the dynamic adsorption capacity is maintained at 90% or more compared to the initial cycle even when the above-mentioned adsorption and desorption experiments are repeated 20 or more times.

Citation Information

Patent Citations

  • Regenerative adsorbents of modified amines on solid supports

    KR1020170127416A