Water-separable ink composition
The water-separable ink composition, using a styrene-maleic anhydride copolymer and other additives, addresses the issues of incomplete separation and curing in low-light UV environments, ensuring rapid alkaline removal and improved recycling efficiency.
Patent Information
- Application Number
- KR1020250168416
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-11-10
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-11-10
AI Technical Summary
Existing inks used in plastic packaging do not effectively separate in alkaline aqueous solutions during recycling, leading to residue and reduced recycling efficiency, and are not adequately cured in low-light UV environments, affecting print quality and durability.
A water-separable ink composition comprising a styrene-maleic anhydride copolymer resin binder, sodium polyacrylate and poly(maleic acid-acrylic acid) copolymer dispersants, humectants, surfactants, chelating agents, and neutralizing agents, which allows rapid curing in low-light UV environments and easy separation in alkaline solutions.
The ink composition ensures rapid curing and adhesion in low-light UV environments, maintains print quality, and facilitates easy removal in alkaline recycling processes, enhancing recycling efficiency and print stability.
Abstract
Description
Technology Field
[0001] The present invention relates to a water-separable ink composition, and more specifically, to a water-separable ink composition that can be rapidly cured even in a low-light UV environment and can be easily separated in an alkaline aqueous solution. Background Technology
[0002] With the recent tightening of environmental regulations on packaging materials such as plastic containers, labels, and films, there is a significantly increasing need for water-soluble alkali-soluble inks that can rapidly remove printed layers during the recycling process.
[0003] In particular, for transparent plastic substrates such as PET and PP, if the ink film printed on the surface is not completely removed during recycling, the optical transparency and the quality of the recycled resin deteriorate; therefore, an ink composition is required in which the printed film is easily separated by alkaline cleaning.
[0004] In addition, while a composition capable of complete separation within minutes in an alkaline aqueous solution is required to improve the efficiency of the recycling process, existing inks had limitations such as slow separation speeds or the presence of residue.
[0005] Meanwhile, in the field of printing inks for plastic packaging, UV-curable inks are widely used to reduce drying time after printing; however, because UV-curable inks primarily use insoluble acrylic monomers and radical-curing resins, they do not dissolve in alkaline aqueous solutions, leading to the problem of ink film residue remaining during the recycling process.
[0006] In addition, there was a limitation in that the photoinitiator reacted only at specific wavelengths (mainly 320–370 nm) during UV curing, so it was not sufficiently cured in low-light LED-UV equipment.
[0007] Therefore, there is a need to develop a water-separable ink composition that maintains sufficient water resistance and print quality under general printing conditions, can be rapidly separated by an aqueous NaOH solution during the recycling cleaning step, and can be fully cured even under low-light UV equipment. The problem to be solved
[0008] One objective of the present invention is to provide a water-removable ink composition that can be rapidly cured even in low-light UV environments, ensures detachability in recycling processes, and simultaneously ensures water resistance and print stability in general environments. means of solving the problem
[0009] The present invention provides a water-separating ink composition comprising: a resin binder composed of a styrene-maleic anhydride (SMA) copolymer having an acid value of 180 mgKOH / g to 300 mgKOH / g; a dispersant composed of sodium polyacrylate having a weight-average molecular weight of 3000 g / mol to 10000 g / mol and a sodium salt of a poly(maleic acid-acrylic acid) copolymer having a weight-average molecular weight of 8000 g / mol to 15000 g / mol; a humectant composed of propylene glycol and diethylene glycol; a surfactant composed of a polyether-modified polysiloxane; a chelating agent composed of disodium ethylenediaminetetraacetate (EDTA-2Na); and a neutralizing agent composed of monoethanolamine (MEA) and 2-amino-2-methyl-1-propanol.
[0010] In addition, the water-separable ink composition further comprises a pigment, and the pigment may be composed of at least one of quinacridone, carbon black, diarylamide, benzimidazolone, phthalocyanine, dioxazine, perylene, and indolinone.
[0011] Additionally, the resin binder may be included in an amount of 40% to 55% by weight based on the total weight of the water-soluble ink composition, the dispersant may be included in an amount of 10% to 15% by weight based on the total weight of the water-soluble ink composition, the humectant may be included in an amount of 4% to 8% by weight based on the total weight of the water-soluble ink composition, the surfactant may be included in an amount of 0.5% to 5% by weight based on the total weight of the water-soluble ink composition, the chelating agent may be included in an amount of 0.1% to 5% by weight based on the total weight of the water-soluble ink composition, the neutralizing agent may be included in an amount of 0.1% to 5% by weight based on the total weight of the water-soluble ink composition, and the pigment may be included in an amount of 20% to 35% by weight based on the total weight of the water-soluble ink composition.
[0012] In addition, the water-separable ink composition further comprises a hydrolyzable plasticizer, wherein the hydrolyzable plasticizer is composed of glycerol triacetate, and the hydrolyzable plasticizer may be included in an amount of 0.5% to 2.0% by weight based on the total weight of the water-separable ink composition.
[0013] In addition, the above pigment has an average particle size (D 50 ) can be 80 nm to 200 nm.
[0014] In addition, the moisturizer may contain the propylene glycol and the diethylene glycol in a weight ratio of 1:1 to 1:1.5.
[0015] In addition, the above water-separable ink composition may have a surface tension of 28 mN / m to 32 mN / m and a viscosity of 30 mPa·s to 70 mPa·s.
[0016] In addition, the styrene-maleic anhydride (SMA) copolymer may contain styrene and maleic anhydride in a molar ratio of 1.5:1 to 3:1.
[0017] In addition, the neutralizing agent may contain the monoethanolamine (MEA) and the 2-amino-2-methyl-1-propanol in a weight ratio of 4:6 to 6:4.
[0018] In addition, the dispersant may include the sodium polyacrylate and the sodium poly(maleic-acrylic acid) copolymer salt in a weight ratio of 4:1 to 8:1. Effects of the invention
[0019] The water-separable ink composition according to the present invention comprises a resin binder composed of a styrene-maleic anhydride (SMA) copolymer having an acid value of 180 mgKOH / g to 300 mgKOH / g in an amount of 40% to 55% by weight based on the total weight of the water-separable ink composition, thereby enabling rapid curing even in low-light UV environments and maintaining stability in a general usage environment of pH 7 to 9, but rapidly hydrolyzing when exposed to an alkaline aqueous solution of pH 13 to 14 used in the recycling process, so that the printed film adhered to the container is rapidly removed during the washing process, making it easy to recycle the container.
[0020] In addition, the water-separable ink composition according to the present invention includes a dispersant composed of sodium polyacrylate having a weight-average molecular weight of 3,000 g / mol to 10,000 g / mol and a sodium salt of a poly(maleic acid-acrylic acid) copolymer having a weight-average molecular weight of 8,000 g / mol to 15,000 g / mol, thereby improving drying performance in a low-light UV environment and maintaining water resistance and viscosity stability of the printed film for a long period. Specific details for implementing the invention
[0021] The embodiments described in this specification are intended to clearly explain the concept of the invention to those skilled in the art to which the invention pertains, and therefore the invention is not limited to the embodiments described in this specification, and the scope of the invention should be interpreted to include modifications or variations that do not deviate from the concept of the invention.
[0022] The terms used in this specification have been selected to be as widely used as possible, taking into account their functions in the present invention; however, these terms may vary depending on the intent of those skilled in the art to which the present invention pertains, case law, or the emergence of new technologies. However, if a specific term is defined and used with an arbitrary meaning, the meaning of that term will be described separately. Accordingly, the terms used in this specification should be interpreted based on their actual meaning and the content throughout this specification, rather than merely their names.
[0023] In this specification, if it is determined that a specific description of known configurations or functions related to the present invention may obscure the essence of the present invention, such detailed description will be omitted as necessary.
[0024] In this specification, "D 50 "This refers to the particle size corresponding to 50% of the volume cumulative particle size distribution of the powder to be measured, and can be measured using the laser diffraction method. For example, pigment powder can be dispersed in a dispersion medium, then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S-3500), irradiated with ultrasound of approximately 28 kHz at an output of 60 W, and obtained a volume cumulative particle size distribution graph, and the particle size at the point where the volume cumulative amount is 50% can be measured from the obtained graph.
[0025] The present invention will be described in detail below.
[0027] The water-soluble ink composition according to the present invention comprises a resin binder, a dispersant, a humectant, a surfactant, a chelating agent, and a neutralizing agent, and may further comprise a pigment or a hydrolyzable plasticizer.
[0028] When using the water-separable ink composition according to the present invention, it is possible to rapidly cure the surface of plastic containers such as PET and PP even in a low-light UV environment, thereby forming a printed film with excellent water resistance, and subsequently, the carboxyl group is rapidly ionized in a 2 wt% sodium hydroxide (NaOH) solution environment so that the printed film is easily separated, so the efficiency of the recycling process can be greatly improved.
[0029] The resin binder can impart adhesion to the printing film even in low-light UV environments and facilitate easy separation of the film in a subsequent sodium hydroxide (NaOH) solution environment; the dispersant can prevent the aggregation of pigment particles and maintain a stable dispersion state; the humectant can control the ink evaporation rate and mitigate viscosity changes; the surfactant can reduce the surface tension of the ink to help it wet the substrate uniformly; the chelating agent captures metal ions present in the water-based ink to prevent pigment aggregation and discoloration; and the neutralizing agent neutralizes maleic anhydride residues (-COOH) within the resin binder to convert them into an alkali-soluble state and stabilize the pH of the composition. Additionally, the pigment can perform the coloring function of the ink, and the hydrolyzable plasticizer can improve the flexibility of the printing film and accelerate the breakdown of the printing film upon exposure to alkali.
[0031] The resin binder consists of a styrene-maleic anhydride (SMA) copolymer with an acid value of 180 mgKOH / g to 300 mgKOH / g.
[0032] Styrene-maleic anhydride (SMA) copolymer is a copolymer in which the non-polar structure of styrene and the polar carboxyl group structure of maleic anhydride are alternately bonded. During the drying process after printing, resin molecules can cross-link or bond with each other to form a dense film structure. It exhibits excellent adhesion even in low-light UV environments through van der Waals bonding with the surface of plastic containers such as PET and PP, thereby maintaining a stable printed film with excellent water resistance and abrasion resistance under general usage conditions.
[0033] In addition, the maleic anhydride units in the styrene-maleic anhydride (SMA) copolymer are rapidly hydrolyzed in an alkaline aqueous solution and converted into carboxylates (-COONa), which destroys the hydrogen bonds and non-polar interactions between resin chains in the printed film, allowing the printed film to be rapidly separated from the surface of plastic containers such as PET and PP.
[0034] The styrene-maleic anhydride (SMA) copolymer may have an acid value of 180 mgKOH / g to 300 mgKOH / g, specifically 200 mgKOH / g to 250 mgKOH / g. The acid value of the styrene-maleic anhydride (SMA) copolymer represents the amount of carboxyl groups per unit mass, and when the above range is satisfied, the printed film can be easily separated in a sodium hydroxide (NaOH) solution environment while maintaining water resistance under normal conditions.
[0035] The resin binder may be included in an amount of 40% to 55% by weight, specifically 49% to 51% by weight, based on the total weight of the water-separable ink composition. When the above range is satisfied, the balance between the mechanical strength, adhesion, water resistance, and alkali separation properties of the printed film in a low-light UV environment can be optimized.
[0036] The styrene-maleic anhydride (SMA) copolymer may contain styrene and maleic anhydride in a molar ratio of 1.5:1 to 3:1, specifically 2.2:1 to 2.3:1. As the styrene content increases, non-polarity increases, which strengthens water resistance, but there is a problem of slow separation speed; and as the maleic anhydride content increases, solubility increases, but there is a problem of reduced film strength. When the above range is satisfied, the styrene region can improve the mechanical strength and adhesion of the coating film during printing, and when exposed to a sodium hydroxide (NaOH) solution environment, the maleic anhydride region becomes a reaction point for ionization and hydration, thereby ensuring separation.
[0038] The dispersant consists of sodium polyacrylate having a weight-average molecular weight of 3,000 g / mol to 10,000 g / mol and sodium poly(maleic acid-acrylic acid) copolymer having a weight-average molecular weight of 8,000 g / mol to 15,000 g / mol.
[0039] Sodium polyacrylate is a linear anionic polymer, comprising a number of carboxylates (-COO₀). - Since it has a ) group, it can electrostatically combine with the positive charge on the surface of the pigment to suppress the aggregation of the pigment, and because it exists in a stable anionic state even under alkaline conditions, it can stably disperse pigment particles and prevent precipitation even when the coating film collapses during cleaning in a sodium hydroxide (NaOH) solution.
[0040] Sodium polyacrylate may have a weight-average molecular weight of 3,000 g / mol to 10,000 g / mol, specifically 4,000 g / mol to 6,000 g / mol. When the above range is satisfied, the short chains can minimize the increase in viscosity of the ink while rapidly adsorbing to the pigment surface, thereby increasing the dispersion speed and fluidity.
[0041] Poly(maleic acid-acrylic acid) copolymer sodium salt contains adjacent diionic carboxyl groups (-COOH-COONa) of maleic acid units and acrylic acid units simultaneously, so it can form multi-point anchoring with the pigment surface, thereby stabilizing the interface between the pigment and the resin binder and suppressing precipitation during long-term storage.
[0042] The poly(maleic acid-acrylic acid) copolymer sodium salt may have a weight-average molecular weight of 8,000 g / mol to 15,000 g / mol, specifically 9,000 g / mol to 11,000 g / mol. When the above range is satisfied, a network can be formed within the printed film to ensure stability during printing, and when exposed to a sodium hydroxide (NaOH) solution, the carboxyl groups are completely ionized and water-soluble, so that it can be dissolved cleanly without any residual polymer residue.
[0043] The dispersant may be included in an amount of 10% to 15% by weight, specifically 11% to 13% by weight, based on the total weight of the water-separated ink composition. When the above range is satisfied, the entire surface of the pigment particles is completely coated (steric stabilization) by sodium polyacrylate and sodium poly(maleic acid-acrylate) salt, and sufficient electrical repulsion is formed between the particles to suppress aggregation. In addition, since the dispersant is uniformly distributed over the entire area of the printed film, the sodium hydroxide (NaOH) solution diffuses evenly, allowing for uniform dissolution and separation, which enables the printed film to be separated quickly.
[0044] The dispersant may include the sodium polyacrylate and the sodium poly(maleic-acrylic acid) copolymer salt in a weight ratio of 4:1 to 8:1, specifically 5:1 to 7:1. When the above range is satisfied, the surface of the pigment particles is uniformly coated, thereby improving long-term storage stability and color uniformity, stabilizing the viscosity and printability of the ink, and optimizing the ionization balance in the alkaline aqueous solution so that the printed film can be uniformly and quickly separated from the sodium hydroxide (NaOH) solution.
[0046] The humectant consists of propylene glycol and diethylene glycol. Propylene glycol has high water retention capacity, which suppresses ink evaporation, mitigates viscosity changes, and can improve jetting stability during printing, while diethylene glycol controls drying speed and increases film flexibility to form a uniform printing film and prevent cracking of the printing film after printing.
[0047] The humectant may be included in an amount of 4% to 8% by weight, specifically 5% to 7% by weight, based on the total weight of the water-soluble ink composition. When the above range is satisfied, viscosity stability, applicability, and drying uniformity of the water-soluble ink can be secured simultaneously.
[0048] The humectant may contain the propylene glycol and the diethylene glycol in a weight ratio of 1:1 to 1:1.5, specifically 1:1.1 to 1:1.3. When the above range is satisfied, the evaporation rate and drying rate of the ink are balanced, so viscosity stability and coating uniformity can be improved, cracking and smudging of the printed film after printing are prevented, and printing quality and water resistance can be simultaneously ensured.
[0050] The surfactant is composed of a polyether-modified polysiloxane. The polyether-modified polysiloxane may include a hydrophobic portion having a siloxane backbone and a polyether hydrophilic chain composed of at least one of ethylene oxide and propylene oxide. Accordingly, the hydrophilic-hydrophobic dual structure rapidly aligns at the interface between the ink and the substrate to suppress the formation and retention of bubbles, and can improve leveling properties by allowing the coating film to be naturally smoothed during the printing film formation process.
[0051] The surfactant may be included in an amount of 0.5% to 5% by weight, specifically 0.5% to 1.5% by weight, based on the total weight of the water-separable ink composition. When the above range is satisfied, printing stability can be secured through bubble suppression, and the printability of the ink and the quality of the final film can be improved.
[0053] The chelating agent consists of disodium ethylenediaminetetraacetate (EDTA-2Na). Disodium ethylenediaminetetraacetate (EDTA-2Na) can selectively capture metal ions that may be present in the water-separable ink composition, thereby improving the color stability, viscosity stability, and long-term storage stability of the ink.
[0054] The chelating agent may be included in an amount of 0.1% to 5% by weight, specifically 0.2% to 0.4% by weight, based on the total weight of the water-separating ink composition. When the above range is satisfied, metal ions in the water-separating ink composition can be stably captured to prevent pigment aggregation and color change, and long-term storage stability can be improved by suppressing viscosity increase and precipitation.
[0056] The neutralizing agent consists of monoethanolamine (MEA) and 2-amino-2-methyl-1-propanol.
[0057] Monoethanolamine (MEA) can rapidly neutralize the styrene-maleic anhydride (SMA) copolymer to promote initial dissolution and solubilization, and 2-amino-2-methyl-1-propanol has low volatility and remains in a certain amount even after printing, maintaining long-term pH stability and viscosity.
[0058] The neutralizing agent may be included in an amount of 0.1% to 5% by weight, specifically 1.1% to 1.3% by weight, based on the total weight of the water-separating ink composition. When the above range is satisfied, the carboxyl groups of the styrene-maleic anhydride (SMA) copolymer are appropriately neutralized, thereby ensuring stable alkali solubility and viscosity balance.
[0059] The neutralizing agent may contain the monoethanolamine (MEA) and the 2-amino-2-methyl-1-propanol in a weight ratio of 4:6 to 6:4. When the above range is satisfied, the viscosity and pH of the ink can be maintained for a long period, and the quality of the printed film can be maintained uniformly during printing and after cleaning.
[0061] The water-soluble ink composition may further include a pigment, and the pigment may consist of at least one of quinacridone, carbon black, diarylamide, benzimidazolone, phthalocyanine, dioxazine, perylene, and indolinone. The pigment plays a role in reproducing the color of the ink and can improve the saturation and heat resistance stability of the printed film. Specifically, quinacridone is stable even in an alkaline environment, so no discoloration or residual color occurs when cleaning in a sodium hydroxide solution, and thus the transparency of the substrate surface and printing quality can be maintained even after the recycling process.
[0062] The pigment may be included in an amount of 20% to 35% by weight, specifically 27% to 30% by weight, based on the total weight of the water-soluble ink composition. When the above range is satisfied, the color of the ink can be reproduced, and the transparency of the substrate surface and printing quality after the recycling process can be maintained.
[0063] Pigments have an average particle size (D 50 The particle size may be 80 nm to 200 nm, specifically 110 nm to 130 nm. When the above range is satisfied, particles that are too small or too large can be suppressed to ensure jetting stability and smoothness of the printed film during printing, and the sodium hydroxide solution can penetrate uniformly to ensure rapid separation of the printed film.
[0065] The water-separable ink composition may further include a hydrolyzable plasticizer, and the hydrolyzable plasticizer may consist of glycerol triacetate. Glycerol triacetate can improve film stability during printing by imparting flexibility and crack resistance to the printed film, and when washed in a sodium hydroxide solution, the ester bonds are hydrolyzed, which can promote the breakdown and separation reaction of the printed film.
[0066] The hydrolyzable plasticizer may be included in an amount of 0.5% to 2.0% by weight, specifically 1.4% to 1.6% by weight, based on the total weight of the water-separable ink composition. When the above range is satisfied, it is possible to maintain a rigid printed film while allowing it to be quickly detached during the recycling process.
[0068] The water-soluble ink composition may have a surface tension of 28 mN / m to 32 mN / m and a viscosity of 30 mPa·s to 70 mPa·s. When the surface tension satisfies the above range, the water-soluble ink can be uniformly wetted on the substrate surface to suppress coating defects and bubble formation, and when the viscosity satisfies the above range, clear print quality and dispersibility can be secured without smudging during printing.
[0070] The present invention will be explained in more detail below through specific embodiments.
[0071] Embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more fully explain the present invention to those with average knowledge in the art.
[0073] Example 1
[0074] A dispersant containing distilled water, sodium polyacrylate (weight-average molecular weight: 5000 g / mol), and poly(maleic-acrylic acid) copolymer sodium salt (weight-average molecular weight 10000 g / mol) in a weight ratio of 6:1 was added to a stirring tank and stirred at a speed of 800 rpm for 25 minutes at a temperature of 25℃ to completely dissolve the mixture, thereby obtaining a preliminary solution of the dispersant.
[0075] Next, as a pigment in the above-mentioned dispersant pre-solution, the average particle size (D 50 Quinacridone with a wavelength of 120 nm was added, and the mixture was stirred at a speed of 1000 rpm for 30 minutes at a temperature of 30°C. Afterwards, high-shear dispersion was performed for 60 minutes using a high-shear disperser at a tip speed of 13 m / s.
[0076] Next, styrene-maleic anhydride (SMA) (acid value: 220 mgKOH / g, styrene:maleic anhydride molar ratio = 2.2:1) was added as a resin binder and stirred at a speed of 500 rpm for 15 minutes at a temperature of 40°C.
[0077] Next, a neutralizing agent mixed with monoethanolamine (MEA) and 2-amino-2-methyl-1-propanol (AMP-95) in a weight ratio of 5:5 was injected by drip infusion to adjust the pH to 9.0, and the mixture was stirred at a speed of 600 rpm for 15 minutes at a temperature of 50°C.
[0078] Next, propylene glycol and diethylene glycol (weight ratio = 1:1.2) were added as humectants, polyether-modified polysiloxane as a surfactant, disodium ethylenediaminetetraacetate (EDTA-2Na) as a chelating agent, and glycerol triacetate as a plasticizer, and the mixture was stirred at a speed of 600 rpm for 30 minutes at a temperature of 25°C to prepare a water-separating ink.
[0079] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0081] Example 2
[0082] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 200 mgKOH / g was used.
[0083] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0085] Example 3
[0086] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 250 mgKOH / g was used.
[0087] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0089] Example 4
[0090] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 180 mgKOH / g was used.
[0091] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0093] Example 5
[0094] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 300 mgKOH / g was used.
[0095] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0097] Example 6
[0098] A water-separating ink was prepared in the same manner as in Example 1, except that sodium polyacrylate with a weight-average molecular weight of 3000 g / mol was used.
[0099] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0101] Example 7
[0102] A water-separating ink was prepared in the same manner as in Example 1, except that sodium polyacrylate with a weight-average molecular weight of 10,000 g / mol was used.
[0103] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0105] Example 8
[0106] A water-separating ink was prepared in the same manner as in Example 1, except that a sodium salt of a poly(maleic acid-acrylic acid) copolymer with a weight-average molecular weight of 8000 g / mol was used.
[0107] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0109] Example 9
[0110] A water-separating ink was prepared in the same manner as in Example 1, except that a sodium salt of a poly(maleic acid-acrylic acid) copolymer with a weight-average molecular weight of 15,000 g / mol was used.
[0111] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0113] Example 10
[0114] Average particle size (D 50 A water-removing ink was prepared in the same manner as in Example 1, except that quinacridone with a wavelength of 80 nm was used.
[0115] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0117] Example 11
[0118] Average particle size (D 50 A water-removing ink was prepared in the same manner as in Example 1, except that quinacridone with a diameter of 200 nm was used.
[0119] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0121] Example 12
[0122] A water-separating ink was prepared in the same manner as in Example 1, except that it was mixed in the weight ratios shown in Table 1 below.
[0123] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0125] Example 13
[0126] A water-separating ink was prepared in the same manner as in Example 1, except that it was mixed in the weight ratios shown in Table 1 below.
[0127] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0129] Example 14
[0130] A water-separating ink was prepared in the same manner as in Example 1, except that it was mixed in the weight ratios shown in Table 1 below.
[0131] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0133] Example 15
[0134] A water-separating ink was prepared in the same manner as in Example 1, except that it was mixed in the weight ratios shown in Table 1 below.
[0135] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0137] Comparative Example 1
[0138] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 150 mgKOH / g was used.
[0139] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0141] Comparative Example 2
[0142] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer with an acid value of 320 mgKOH / g was used.
[0143] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0145] Comparative Example 3
[0146] A water-separating ink was prepared in the same manner as in Example 1, except that sodium polyacrylate with a weight-average molecular weight of 2000 g / mol was used.
[0147] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0149] Comparative Example 4
[0150] A water-separating ink was prepared in the same manner as in Example 1, except that sodium polyacrylate with a weight-average molecular weight of 12,000 g / mol was used.
[0151] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0153] Comparative Example 5
[0154] A water-separating ink was prepared in the same manner as in Example 1, except that a sodium salt of a poly(maleic acid-acrylic acid) copolymer with a weight-average molecular weight of 7000 g / mol was used.
[0155] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0157] Comparative Example 6
[0158] A water-separating ink was prepared in the same manner as in Example 1, except that a sodium salt of a poly(maleic acid-acrylic acid) copolymer with a weight-average molecular weight of 17,000 g / mol was used.
[0159] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0161] Comparative Example 7
[0162] A water-separating ink was prepared in the same manner as in Example 1, except that a styrene-maleic anhydride (SMA) copolymer was not mixed as a resin binder.
[0163] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0165] Comparative Example 8
[0166] A water-separating ink was prepared in the same manner as in Example 1, except that sodium polyacrylate and poly(maleic acid-acrylic acid) copolymer sodium salt were not mixed as dispersants.
[0167] The weight ratio of the water-separated ink composition excluding distilled water is shown in Table 1 below.
[0169] Examples 1–11 and Comparative Examples 1–6 Example 12 Example 13 Example 14 Example 15 Comparative Example 7 Comparative Example 8 Suzy Binder 50 wt% 40 wt% 55 wt% 35 wt% 60 wt% - 62 wt% Dispersant 12 wt% 22 wt% 7 wt% 27 wt% 2 wt% 62 wt% - moisturizer 6 wt% 6 wt% 6 wt% 6 wt% 6 wt% 6 wt% 6 wt% surfactants 1 wt% 1 wt% 1 wt% 1 wt% 1 wt% 1 wt% 1 wt% Chelating agent 0.3 wt% 0.3 wt% 0.3 wt% 0.3 wt% 0.3 wt% 0.3 wt% 0.3 wt% corrector 1.2 wt% 1.2 wt% 1.2 wt% 1.2 wt% 1.2 wt% 1.2 wt% 1.2 wt% pigment 28 wt% 28 wt% 28 wt% 28 wt% 28 wt% 28 wt% 28 wt% hydrolyzable plasticizer 1.5 wt% 1.5 wt% 1.5 wt% 1.5 wt% 1.5 wt% 1.5 wt% 1.5 wt%
[0170] Experimental Example 1 : Separation speed evaluation
[0171] Water-removable inks prepared according to Examples 1 to 15 and Comparative Examples 1 to 8 were each applied to a PET film (thickness: 100 μm) to a thickness of 3 μm by gravure coating, and dried at 80°C for 2 minutes to prepare test specimens.
[0172] Afterwards, the test specimen was immersed in a 2 wt% NaOH aqueous solution (40℃, 200 mL) and stirred at 200 rpm, and the degree of separation of the printed film over time was observed.
[0173] The results of the observations are shown in Table 2 below.
[0175] Separation start time (minutes) Complete separation time (minutes) Example 1 1.2 3.2 Example 2 1.3 3.3 Example 3 1.3 3.2 Example 4 1.8 4.2 Example 5 1.5 3.9 Example 6 1.6 4.1 Example 7 1.8 4.5 Example 8 1.5 4.2 Example 9 1.6 4.1 Example 10 1.5 3.5 Example 11 1.4 3.5 Example 12 2.1 5.1 Example 13 1.7 4.1 Example 14 2.0 4.9 Example 15 1.6 3.5 Comparative Example 1 2.8 6.5 Comparative Example 2 2.3 5.8 Comparative Example 3 2.2 5.4 Comparative Example 4 2.3 5.6 Comparative Example 5 2.4 5.4 Comparative Example 6 2.7 6.1 Comparative Example 7 6.4 11.2 Comparative Example 8 5.4 8.2
[0176] Referring to Table 2 above, it can be seen that the water separation ink prepared according to Examples 1 to 15 has a faster separation time compared to the water separation ink prepared according to Comparative Examples 1 to 8.
[0178] Experimental Example 2 : Print smoothness evaluation
[0179] Water-removable inks prepared according to Examples 1 to 15 and Comparative Examples 1 to 8 were each applied to a PET film (thickness: 100 μm) to a thickness of 3 μm by gravure coating, and a UV-LED (395 nm) device was used to apply 200 mJ / cm² 2 It was dried by irradiating with a irradiation dose. Afterwards, the volume of the generated bubbles and the smoothness of the printed film were measured.
[0180] The measurement results are shown in Table 3 below.
[0182] Foam volume (mL) Smoothness (Ra, μm) Example 1 5 0.25 Example 2 5 0.25 Example 3 5 0.25 Example 4 6 0.27 Example 5 6 0.27 Example 6 5 0.26 Example 7 5 0.29 Example 8 6 0.26 Example 9 5 0.25 Example 10 6 0.24 Example 11 12 0.38 Example 12 8 0.28 Example 13 17 0.32 Example 14 7 0.27 Example 15 16 0.35 Comparative Example 1 18 0.45 Comparative Example 2 18 0.31 Comparative Example 3 17 0.38 Comparative Example 4 19 0.41 Comparative Example 5 18 0.29 Comparative Example 6 18 0.37 Comparative Example 7 29 0.29 Comparative Example 8 28 0.32
[0183] Referring to Table 3 above, it can be seen that the water-separating inks prepared according to Examples 1 to 15 suppress bubble generation and have excellent leveling properties compared to the water-separating inks prepared according to Comparative Examples 1 to 8.
Claims
Claim 1 A resin binder composed of a styrene-maleic anhydride (SMA) copolymer having an acid value of 200 mgKOH / g to 250 mgKOH / g; a dispersant composed of sodium polyacrylate having a weight-average molecular weight of 4,000 to 6,000 and a sodium salt of a poly(maleic acid-acrylic acid) copolymer having a weight-average molecular weight of 9,000 to 11,000; a humectant composed of propylene glycol and diethylene glycol; a surfactant composed of a polyether-modified polysiloxane; a chelating agent composed of disodium ethylenediaminetetraacetate (EDTA-2Na); a neutralizing agent composed of monoethanolamine (MEA) and 2-amino-2-methyl-1-propanol; a pigment; A water-dissolving ink composition comprising a pigment and a hydrolyzable plasticizer, wherein the pigment is composed of at least one of quinacridone, carbon black, diarylamide, benzimidazolone, phthalocyanine, dioxazine, perylene, and indolinone; the hydrolyzable plasticizer is composed of glycerol triacetate; the hydrolyzable plasticizer is included in an amount of 0.5% to 2.0% by weight based on the total weight of the water-dissolving ink composition; the resin binder is included in an amount of 40% to 55% by weight based on the total weight of the water-dissolving ink composition; the dispersant is included in an amount of 10% to 15% by weight based on the total weight of the water-dissolving ink composition; the humectant is included in an amount of 4% to 8% by weight based on the total weight of the water-dissolving ink composition; the surfactant is included in an amount of 0.5% to 5% by weight based on the total weight of the water-dissolving ink composition; and the chelating agent is included based on the total weight of the water-dissolving ink composition Included in an amount of 0.1% to 5% by weight, the neutralizing agent is included in an amount of 0.1% to 5% by weight based on the total weight of the water-separating ink composition, the pigment is included in an amount of 20% to 35% by weight based on the total weight of the water-separating ink composition, the humectant includes the propylene glycol and the diethylene glycol in a weight ratio of 1:1 to 1:1.5, and the styrene-maleic anhydride (SMA) copolymer comprises styrene and maleic anhydride 1.A water-separating ink composition comprising, in a molar ratio of 5:1 to 3:1, the neutralizing agent comprising the monoethanolamine (MEA) and the 2-amino-2-methyl-1-propanol in a weight ratio of 4:6 to 6:4, and the dispersing agent comprising the sodium polyacrylate and the poly(maleic-acrylic acid) copolymer sodium salt in a weight ratio of 5:1 to 7:1, having a surface tension of 28 mN / m to 32 mN / m and a viscosity of 30 mPa·s to 70 mPa·s. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 In paragraph 1, the pigment has an average particle size (D 50 A water-removing ink composition having a thickness of 80 nm to 200 nm. Claim 6 delete Claim 7 delete Claim 8 delete Claim 9 delete Claim 10 delete
Citation Information
Patent Citations
The composition of the pigmented ink
KR1020000055023A
Pigment dispersion, recording ink, ink cartridge, ink-jet recording method and ink-jet recording apparatus
KR1020080080403A
Water-based pigment ink
KR1020230029984A