Stone mastic asphalt concrete composition with excellent permeability and construction method using the same

The SMA concrete composition addresses drainage, noise, and durability issues in asphalt pavements by using a specific mix of aggregates and additives, ensuring rapid drainage, noise reduction, and enhanced strength, thus improving safety and reducing maintenance.

KR103044397B1Active Publication Date: 2026-11-10QUALITY SAFETY TECH RES INST
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020260072503
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-04-22
Publication Date
2026-11-10
Estimated Expiration
2046-04-22

AI Technical Summary

Technical Problem

Existing asphalt pavements face issues with drainage performance, noise generation, crack resistance, and durability under varying ambient temperatures, leading to safety hazards and maintenance challenges.

Method used

A crushed stone mastic asphalt (SMA) concrete composition comprising specific ratios of aggregate, filler, and asphalt binder, enhanced with additives like microcrystalline cellulose-aragonite composite particles and cyanoacrylate-based compounds, to improve drainage, reduce noise, and enhance strength and adhesion.

Benefits of technology

The SMA composition ensures rapid drainage, reduces noise, prevents cracking and peeling, and enhances durability, thereby reducing maintenance costs and improving safety and longevity of asphalt surfaces.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same. More specifically, the composition comprises 1) 75 to 90 weight% of aggregate mixed with coarse aggregate and fine aggregate in a weight ratio of 40 to 95: 5 to 60, 2) 0 to 5 weight% of filler, and 3) 5 to 20 weight% of asphalt binder, wherein the asphalt binder comprises 100 weight parts of asphalt; 0.01 to 5 weight parts of plasticizer; 0.1 to 10 weight parts of petroleum resin; 0.01 to 5 weight parts of process oil; 1 to 30 weight parts of styrene-butadiene-styrene (SBS); 0.1 to 10 weight parts of alkyd resin; and 0.1 to 5 weight parts of synthetic fluorophlogopite. Containing 0.1 to 5 parts by weight of aragonite; 0.01 to 2 parts by weight of a cyanoacrylate-based compound; and 0.1 to 5 parts by weight of a wax mixture comprising ethylene-bis-stearamide (EBS) wax and erucamide wax mixed in a weight ratio of 1:0.5 to 1, wherein the cyanoacrylate-based compound comprises one or more selected from the group consisting of 2-octyl cyanoacrylate, n-butyl cyanoacrylate, and mixtures thereof, The present invention relates to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same, which can ensure drainage by preventing pore clogging, ensure low noise by preventing the occurrence of popping and friction sounds on asphalt roads, prevent cracks, surface peeling, and detachment (potholes) by minimizing the impact of changes in ambient temperature, and significantly improve resistance to plastic deformation and low-temperature fatigue cracking through improved strength and adhesion, thereby preventing damage to the pavement surface and ensuring slip resistance to improve durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same, which can ensure drainage by preventing pore clogging, ensure low noise by preventing the occurrence of popping and friction sounds on asphalt roads, prevent the occurrence of cracks, surface peeling, and detachment (potholes) by minimizing the influence of changes in ambient temperature, and significantly improve resistance to plastic deformation and low-temperature fatigue cracking through improved strength and adhesion, thereby preventing damage to the pavement surface and ensuring slip resistance to improve durability. Background Technology

[0003] Water penetration in roads or bridges causes damage to the sublayer of the pavement and corrosion of the structure, thus requiring a waterproofing layer. Materials used for waterproofing layers are required to possess various performance characteristics in addition to simple waterproofing, such as resistance to stresses arising from vehicle loads and structural deformation, thermal stability against high temperatures during construction, adhesion to the structure, durability, and ease of work. However, there is a problem in that such waterproofing layers are expensive while lacking structural performance.

[0004] Accordingly, Stone Mastic Asphalt was developed by adding mastic (a mixture of fine aggregate, filler, and asphalt) to a matrix formed solely of coarse aggregate, resulting in superior resistance to plastic deformation and wear compared to ordinary asphalt mixtures, and resistance to fatigue cracking.

[0005] Meanwhile, as Korea's climate becomes subtropical, the number of rainy days is rapidly increasing. Consequently, water splashing occurs in potholes during rainy weather, and hydroplaning during driving leads to steering instability or increased braking distances, becoming a direct cause of traffic accidents. Furthermore, poor visibility during rainy nights, to the point where road surface glare or lane markings are invisible, is contributing to an increase in safety accidents.

[0006] Recently, taking these factors into account, development is focusing on improving the drainage of asphalt pavements to enhance driving safety during rainy conditions. Prior art literature

[0008] Republic of Korea Registered Patent No. 10-1838896 Republic of Korea Registered Patent No. 10-1793618 Republic of Korea Registered Patent No. 10-1955359 The problem to be solved

[0009] The present invention was devised to solve the aforementioned problems and aims to provide a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same, which can ensure drainage by preventing pore clogging and improve noise reduction effects by preventing the occurrence of popping and friction sounds in asphalt roads, while simultaneously ensuring durability such as plastic deformation, wear resistance, and crack resistance.

[0010] The various problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem

[0012] One embodiment of the present invention comprises 1) 75 to 90 weight% of aggregate mixed with coarse aggregate and fine aggregate in a weight ratio of 40 to 95:5 to 60, 2) 0 to 5 weight% of filler, and 3) 5 to 20 weight% of asphalt binder, and

[0013] The above asphalt binder comprises 100 parts by weight of asphalt; 0.01 to 5 parts by weight of a plasticizer; 0.1 to 10 parts by weight of a petroleum resin; 0.01 to 5 parts by weight of a process oil; 1 to 30 parts by weight of styrene-butadiene-styrene (SBS); 0.1 to 10 parts by weight of an alkyd resin; 0.1 to 5 parts by weight of synthetic fluorophlogopite; 0.1 to 5 parts by weight of aragonite; 0.01 to 2 parts by weight of a cyanoacrylate-based compound; and 0.1 to 5 parts by weight of a wax mixture comprising ethylene-bis-stearamide (EBS) wax and erucamide wax mixed in a weight ratio of 1:0.5 to 1,

[0014] The present invention provides a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance, wherein the above cyanoacrylate-based compound is one or more selected from the group consisting of 2-octyl cyanoacrylate, n-butyl cyanoacrylate, and mixtures thereof.

[0015] The above aragonite is

[0016] It is a microcrystalline cellulose-aragonite composite particle;

[0017] The above-mentioned microcrystalline cellulose-aragonite composite particles are manufactured by a method comprising the steps of: preparing a mixed solution in which 100 parts by weight of a glucoside surfactant, 10 to 50 parts by weight of microcrystalline cellulose, and 0.1 to 3 parts by weight of trans-stilbene [Cas No. 103-30-0] are mixed; and preparing microcrystalline cellulose-aragonite composite particles by spray-drying a dispersion in which 50 to 100 parts by weight of aragonite are dispersed in 100 parts by weight of the mixed solution;

[0018] The above glucoside surfactant may be a mixture of lauryl glucoside and decyl glucoside mixed in a weight ratio of 1:0.1 to 0.5.

[0019] The above aragonite is

[0020] It is surface-treated aragonite, and

[0021] The surface-treated aragonite may be prepared by ball-milling 100 parts by weight of acetone, 10 to 50 parts by weight of aragonite, 1 to 20 parts by weight of xyloglucan, and 1 to 10 parts by weight of hexa(methoxymethyl)melamine for 3 to 5 hours, and then drying.

[0022] The above asphalt binder is

[0023] 100 parts by weight of asphalt further containing 0.01 to 5 parts by weight of a sulfoxymin compound, and

[0024] The above sulfoxymine compound may be one or more selected from the group consisting of butionine sulfoxymine, methionine sulfoxymine, 2-ethylmethionine sulfoxymine, and mixtures thereof.

[0025] In addition, another embodiment of the present invention provides a construction method using a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance, comprising the steps of: washing and pre-treating a target surface to be constructed; mixing and dispersing the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance; pouring the mixed and dispersed crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance onto the target surface to be constructed after the washing and pre-treatment are completed; compacting the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance after the pouring step is completed to form a pavement layer having a void ratio of 1.5 to 25%; and curing after the compaction step is completed. Effects of the invention

[0027] According to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same according to one embodiment of the present invention, it is possible to ensure drainage by preventing pore clogging. In particular, rapid drainage during rain prevents the occurrence of a water film, thereby reducing traffic accidents. Furthermore, it is possible to ensure noise reduction for moving vehicles by preventing the occurrence of popping and friction sounds on asphalt roads. Additionally, it is possible to prevent the occurrence of cracks, surface peeling, and detachment (potholes) by minimizing the impact of changes in ambient temperature. Moreover, through the improvement of strength and adhesion, resistance to plastic deformation and low-temperature fatigue cracking are significantly improved, thereby preventing damage to the pavement surface and ensuring slip resistance, which improves durability. Consequently, it is possible to reduce maintenance costs and human and material losses caused by congestion and delays during road maintenance.

[0028] As a result, it can be very usefully applied to paving roads such as roadways and sidewalks, bridges, and aircraft landing strips. Specific details for implementing the invention

[0030] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0031] One embodiment of the present invention comprises 1) 75 to 90 weight% of aggregate mixed with coarse aggregate and fine aggregate in a weight ratio of 40 to 95:5 to 60, 2) 0 to 5 weight% of filler, and 3) 5 to 20 weight% of asphalt binder, and

[0032] The above asphalt binder comprises 100 parts by weight of asphalt; 0.01 to 5 parts by weight of a plasticizer; 0.1 to 10 parts by weight of a petroleum resin; 0.01 to 5 parts by weight of a process oil; 1 to 30 parts by weight of styrene-butadiene-styrene (SBS); 0.1 to 10 parts by weight of an alkyd resin; 0.1 to 5 parts by weight of synthetic fluorophlogopite; 0.1 to 5 parts by weight of aragonite; 0.01 to 2 parts by weight of a cyanoacrylate-based compound; and 0.1 to 5 parts by weight of a wax mixture comprising ethylene-bis-stearamide (EBS) wax and erucamide wax mixed in a weight ratio of 1:0.5 to 1,

[0033] The present invention relates to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance, wherein the above-mentioned cyanoacrylate-based compound is one or more selected from the group consisting of 2-octyl cyanoacrylate, n-butyl cyanoacrylate, and mixtures thereof.

[0034] According to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same according to one embodiment of the present invention, it is possible to ensure drainage by preventing pore clogging. In particular, rapid drainage during rain prevents the occurrence of a water film, thereby reducing traffic accidents. Furthermore, it is possible to ensure noise reduction for moving vehicles by preventing the occurrence of popping and friction sounds on asphalt roads. Additionally, it is possible to prevent the occurrence of cracks, surface peeling, and detachment (potholes) by minimizing the impact of changes in ambient temperature. Moreover, through the improvement of strength and adhesion, resistance to plastic deformation and low-temperature fatigue cracking are significantly improved, thereby preventing damage to the pavement surface and ensuring slip resistance, which improves durability. Consequently, it is possible to reduce maintenance costs and minimize human and material losses caused by congestion and delays during road maintenance. Thus, it is highly useful for paving roads such as lanes and sidewalks, bridges, and aircraft landing pads.

[0035] Hereinafter, a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance according to one embodiment of the present invention will be described in more detail as follows.

[0036] A crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance according to one embodiment of the present invention comprises 1) 75 to 90 weight% of aggregate mixed with coarse aggregate and fine aggregate in a weight ratio of 40 to 95:5 to 60, 2) 0 to 5 weight% of filler, and 3) 5 to 20 weight% of asphalt binder.

[0037] 1) According to one embodiment of the present invention, the aggregate is a mineral material for construction that can be clumped together with other components of a crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance to form a single mass, and is chemically stable. Depending on the size, the aggregate is referred to as fine aggregate if it is 0.074 mm or larger and less than 4.76 mm, and as coarse aggregate if it is 4.76 mm or larger.

[0038] To ensure drainage by preventing pore clogging, it is preferable to use aggregate in which coarse aggregate and fine aggregate are mixed in a weight ratio of 40 to 95:5 to 60. Such aggregate is generally used in the field and is not specifically limited in type; for example, sand, gravel, basalt, black stone, basalt, etc. may be used.

[0039] It is preferable that such aggregates be mixed in an amount of 75 to 90 weight percent with respect to the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance according to the present invention. In addition, the size of the aggregates is not limited as it is determined according to the type and void ratio of the pavement to be constructed, the ground conditions of the road surface to be constructed, weather conditions, traffic volume, and the number of lanes.

[0040] 2) A filler according to one embodiment of the present invention fills the voids between the aggregates, thereby maximizing water tightness, waterproofing performance, water permeability, strength, and abrasion resistance.

[0041] The particle size of the above-mentioned filler may preferably conform to the standard of KS F 3501. In addition, the above-mentioned filler is generally used in the field and is not specifically limited in type, but for example, limestone powder, Portland cement, fly ash, recovered dust, electric furnace steelmaking dust, foundry dust, various types of incineration ash, blast furnace slag powder, cellulose fiber, carbon black, clay powder, light carbon powder, etc. may be used.

[0042] Considering the improvement effect described above, it is preferable that the above-mentioned filler be contained in a range of 0 to 5 weight percent with respect to the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance of the present invention.

[0043] 3) An asphalt binder according to one embodiment of the present invention minimizes friction noise and tearing noise of tires on the asphalt road surface to provide low noise, and attaches and bonds aggregate and filler materials to achieve excellent adhesive strength, tensile strength, watertightness, waterproofing performance, water permeability, abrasion resistance, and salt damage resistance, and improves elongation, elasticity, and flexibility so that external impacts or pressures can be absorbed or mitigated within the asphalt. In addition, it minimizes the effects of changes in ambient temperature and effectively prevents phase separation.

[0044] Considering the improvement effect described above, it is preferable that the above-mentioned asphalt binder be contained in a range of 5 to 20 weight percent with respect to the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance of the present invention.

[0045] More specifically, the asphalt binder may preferably be used to contain 100 parts by weight of asphalt; 0.01 to 5 parts by weight of a plasticizer; 0.1 to 10 parts by weight of a petroleum resin; 0.01 to 5 parts by weight of a process oil; 1 to 30 parts by weight of styrene-butadiene-styrene (SBS); 0.1 to 10 parts by weight of an alkyd resin; 0.1 to 5 parts by weight of synthetic fluorophlogopite; 0.1 to 5 parts by weight of aragonite; 0.01 to 2 parts by weight of a cyanoacrylate-based compound; and 0.1 to 5 parts by weight of a wax mixture in which ethylene-bis-stearamide (EBS) wax and erucamide wax are mixed in a weight ratio of 1:0.5 to 1.

[0046] The above asphalt is generally used in the field and is not specifically limited in type, but for example, petroleum-based asphalt, natural asphalt, or a mixture thereof may be used. In this case, the above petroleum-based asphalt may be straight asphalt, cutback asphalt, blown asphalt, etc., and the above petroleum-based asphalt may preferably be used with a penetration of 20 to 100. In addition, the above natural asphalt may be Trinidad Lake asphalt, Trinidad Epure asphalt, etc. More preferably, straight asphalt with a penetration of 20 to 100 may be used.

[0047] Hereinafter, the content of other components constituting the asphalt binder is based on 100 parts by weight of the asphalt.

[0048] The above-mentioned plasticizer plays a role in controlling viscosity, improving adhesion, enhancing compatibility between components, and improving workability and processability, thereby enabling uniform mixing and ensuring quality. Additionally, it provides excellent cold resistance, enabling improved crack resistance at low temperatures.

[0049] The above plasticizers are dibutyl phthalate (DBP), diethyl phthalate (DEP), dimethyl phthalate (DMP), dioctyl phthalate (DOP), dioctyl adipate (DOA), dioctyl sebacate (DOS), dioctyl phthalate (DOP), isodecylpelargonate (IDP), triphenyl phosphate (TPP), tricresyl phosphate (TCP), resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), and One or more selected from the group consisting of mixtures of these may be used.

[0050] It is preferable that such a plasticizer be contained in a range of 0.01 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the plasticizer is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the plasticizer is too high, there is a problem that the heat resistance may be reduced.

[0051] The above petroleum resin significantly improves tackiness and adhesion, enhances compatibility between components, and improves workability and processability, thereby enabling uniform mixing and ensuring quality. Furthermore, it plays a role in increasing heat resistance to prevent sagging, and improving weather resistance, such as preventing cracking, particularly at low temperatures.

[0052] The above petroleum resin may be one or more selected from the group consisting of C5-based petroleum resin, C9-based petroleum resin, maleated petroleum resin, esterified petroleum resin, and mixed petroleum resins thereof. More preferably, a mixture of C5-based petroleum resin and C9-based petroleum resin in a weight ratio of 1:1 to 2 may be used to further improve the above-mentioned effect.

[0053] It is preferable that such petroleum resin be contained in a range of 0.1 to 10 parts by weight per 100 parts by weight of the asphalt. If the content of the petroleum resin is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the petroleum resin is too high, there is a problem that the resistance to plastic deformation and adhesion may be reduced.

[0054] The above process oil enhances the dispersibility and compatibility among components, improves workability and processability, and lowers the temperature required for construction, thereby enabling uniform melting, mixing, and quality assurance. Furthermore, by improving elongation, elasticity, and flexibility, it absorbs or mitigates external shocks or pressures, thus serving to prevent fatigue cracks and damage caused by traffic loads.

[0055] The above process oil may preferably be one or more selected from the group consisting of paraffin oil, naphthenic oil, aromatic oil, natural oil, mineral oil, and mixtures thereof.

[0056] It is preferable that such process oil be contained in a range of 0.01 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the process oil is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the process oil is too high, there is a problem that the resistance to plastic deformation may be reduced.

[0057] The above styrene-butadiene-styrene (SBS) block copolymer provides excellent adhesive performance, elasticity, and elongation, and compensates for deformation to prevent fatigue cracks, low-temperature cracks, aggregate detachment, surface peeling, and detachment (potholes).

[0058] Such styrene-butadiene-styrene (SBS) block copolymer may be contained in a range of 1 to 20 parts by weight per 100 parts by weight of the asphalt. If the content of the styrene-butadiene-styrene (SBS) block copolymer is too low, there is a problem that the above-mentioned improvement effect may be insufficient, and if the content of the styrene-butadiene-styrene (SBS) block copolymer is too high, there is a problem that workability may be reduced or price competitiveness may be reduced.

[0059] The above alkyd resin enhances resistance to plastic deformation by increasing viscosity and high-temperature stiffness, and improves adhesion to the asphalt binder by strengthening adsorption and bonding at the interface of the aggregate.

[0060] Such alkyd resin may be contained in a range of 0.1 to 10 parts by weight per 100 parts by weight of the asphalt. If the content of the alkyd resin is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the alkyd resin is too high, there is a problem that the low-temperature crack resistance may be reduced.

[0061] The above-mentioned synthetic fluorophlogopite enhances deformation resistance at high temperatures, preventing rutting and suppressing binder leakage to strengthen the skeletal structure of mastic, while also maintaining excellent drainage properties over the long term and reducing noise.

[0062] Such synthetic fluorophlogopite may be contained in a range of 0.1 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the synthetic fluorophlogopite is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the synthetic fluorophlogopite is too high, there is a problem that workability may be reduced.

[0063] The above aragonite not only improves mastic strength and moisture resistance but also improves high-temperature deformation resistance and reduces rutting and fatigue cracking.

[0064] In addition, to ensure long-term noise reduction by forming surface micropores and absorbing and scattering tire-road noise, in addition to the aforementioned roles, it is desirable to use microcrystalline cellulose-aragonite composite particles.

[0065] Specifically, the microcrystalline cellulose-aragonite composite particles can be manufactured by a method comprising the steps of: preparing a mixed solution in which 100 parts by weight of a glucoside surfactant, 10 to 50 parts by weight of microcrystalline cellulose, and 0.1 to 3 parts by weight of trans-stilbene [Cas No. 103-30-0] are mixed; and spray-drying a dispersion in which 50 to 100 parts by weight of aragonite are dispersed in 100 parts by weight of the mixed solution to produce microcrystalline cellulose-aragonite composite particles.

[0066] The above-mentioned glucoside surfactant is used to improve the miscibility and dispersibility of microcrystalline cellulose and aragonite to form composite particles of uniform size, and it is preferably a mixture of lauryl glucoside and decyl glucoside mixed in a weight ratio of 1:0.1 to 0.5. The above-mentioned trans-stilbene serves to improve resistance to high-temperature deformation by imparting low penetration and a high softening point.

[0067] In addition, the aragonite may be surface-treated with xyloglucan and hexa(methoxymethyl)melamine. Specifically, the surface-treated aragonite may be prepared by ball-milling 100 parts by weight of acetone, 10 to 50 parts by weight of aragonite, 1 to 20 parts by weight of xyloglucan, and 1 to 10 parts by weight of hexa(methoxymethyl)melamine for 3 to 5 hours, and then drying.

[0068] At this time, the xyloglucan and hexa(methoxymethyl)melamine improve the adhesion between microcrystalline cellulose and aragonite, block moisture penetration, and reduce stripping and fatigue cracking, thereby preventing pore clogging over the long term and ensuring the sustainability of low-noise performance.

[0069] Such aragonite may be contained in a range of 0.1 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the aragonite is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the aragonite is too high, there is a problem that the viscosity increases excessively, which may reduce workability or reduce price competitiveness.

[0070] The above cyanoacrylate-based compound plays a role in extending low-noise performance by rapidly filling microcracks and maintaining the pore structure, as well as improving adhesion.

[0071] One or more selected from the group consisting of the above-mentioned 2-octyl cyanoacrylate, n-butyl cyanoacrylate, and mixtures thereof may be used.

[0072] These cyanoacrylate compounds may be contained in a range of 0.1 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the cyanoacrylate compounds is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the cyanoacrylate compounds is too high, there is a problem that crack resistance may be reduced.

[0073] It controls the viscosity and workability of the aforementioned wax mixture and forms a waterproof coating layer on the asphalt surface to prevent moisture penetration and freeze-thaw cycles. Furthermore, it prevents high-temperature softening and delays thermal oxidation, thereby ensuring long-term storage stability. Additionally, it enhances the compatibility between components, improves workability and processability, and lowers the temperature required for application, enabling uniform melting, mixing, and quality assurance.

[0074] The above wax mixture is preferably a mixture of ethylene-bis-stearamide (EBS) wax and erucamide wax in a weight ratio of 1:0.5 to 1.

[0075] This wax mixture may be contained in a range of 0.1 to 5 parts by weight per 100 parts by weight of the asphalt. If the content of the wax mixture is too low, there is a problem that the improvement effect described above may be insufficient, and if the content of the wax mixture is too high, there is a problem that workability may be reduced or strength performance may be reduced.

[0076] In addition, the asphalt binder according to the present invention may further contain 0.01 to 5 parts by weight of a sulfoxymin compound in 100 parts by weight of asphalt.

[0077] The above sulfoxymine compound may be one or more selected from the group consisting of butionine sulfoxymine, methionine sulfoxymine, 2-ethylmethionine sulfoxymine, and mixtures thereof.

[0078] The above-mentioned sulfoxymine compound has excellent resistance to heat and light, maintaining long-term durability of drainage and low noise while simultaneously improving water resistance and controlling high-temperature stiffness and low-temperature brittleness, thereby playing a role in improving high-temperature deformation resistance, low-temperature crack resistance, plastic deformation resistance, and viscoelasticity.

[0079] In addition, another embodiment of the present invention is a construction method using the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance, comprising the steps of: washing and pre-treating a target surface to be constructed; mixing and dispersing the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance; pouring the mixed and dispersed crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance onto the target surface to be constructed after the washing and pre-treatment are completed; compacting the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance after the pouring step is completed to form a pavement layer having a void ratio of 1.5 to 25%; and curing after the compaction step is completed.

[0080] The present invention controls the content of aggregate and filler contained in the crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance, thereby easily realizing the effects of drainage and noise reduction performance of the constructed pavement.

[0081] According to a crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a construction method using the same according to one embodiment of the present invention, it is possible to ensure drainage by preventing pore clogging. In particular, rapid drainage during rain prevents the occurrence of a water film, thereby reducing traffic accidents. Furthermore, it is possible to ensure noise reduction for moving vehicles by preventing the occurrence of popping and friction sounds on asphalt roads. Additionally, it is possible to prevent the occurrence of cracks, surface peeling, and detachment (potholes) by minimizing the impact of changes in ambient temperature. Moreover, through the improvement of strength and adhesion, resistance to plastic deformation and low-temperature fatigue cracking are significantly improved, thereby preventing damage to the pavement surface and ensuring slip resistance, which improves durability. Consequently, it is possible to reduce maintenance costs and minimize human and material losses caused by congestion and delays during road maintenance. Thus, it is highly useful for paving roads such as lanes and sidewalks, bridges, and aircraft landing pads.

[0082] Although preferred embodiments of the present invention have been described in detail above, the present invention is not limited to the above embodiments, and various modifications are possible by those skilled in the art within the scope of the technical concept of the present invention.

[0084] <Preparation Example 1> Microcrystalline cellulose-aragonite composite particles

[0085] A mixed solution was prepared by adding 30 parts by weight of lauryl glucoside, 10 parts by weight of decyl glucoside, 30 parts by weight of microcrystalline cellulose, and 0.15 parts by weight of trans-stilbene [Cas No. 103-30-0] to 250 parts by weight of distilled water. Subsequently, 70 parts by weight of aragonite were added to the mixed solution, dispersed at room temperature using a homogenizer, and spray-dried to produce microcrystalline cellulose-aragonite composite particles. During the spray drying, the inlet temperature of the spray dryer was maintained at 140 ℃, and the air flow rate was supplied at 400 L / h.

[0087] <Preparation Example 2>

[0088] Microcrystalline cellulose-aragonite composite particles were prepared in the same manner as in Preparation Example 1 above, but using surface-treated aragonite instead of aragonite. The surface-treated aragonite was prepared by ball-milling 100 parts by weight of acetone, 25 parts by weight of aragonite, 12 parts by weight of xyloglucan, and 5 parts by weight of hexa(methoxymethyl)melamine for 4 hours, followed by drying at a temperature of 60°C.

[0090] <Examples 1 to 3 and Comparative Examples 1 to 2>

[0091] A crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance and a comparative composition were prepared by mixing with the components and content as shown in Table 1 below.

[0092] Classification (Weight%) Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 aggregate 86 86 86 86 86 weight ratio Coarse aggregate 75 75 75 75 75 fine aggregate 25 25 25 25 25 Filler 1 1 1 1 1 weight ratio Blast furnace slag powder 1 1 1 1 1 calcium carbonate 0.5 0.5 0.5 0.5 0.5 Asphalt binder 13 13 13 13 13 weight part asphalt 100 100 100 100 100 Plasticizer (Resorcinol bis(diphenylphosphate)) 2 2 2 2 2 Petroleum resin (C5 petroleum resin) 5 5 5 5 5 Process oil (paraffin oil) 3 3 3 3 3 Styrene-butadiene-styrene (SBS) 15 15 15 15 15 Alkyd Resin [Cas No. 63148-69-6] 5 5 5 - - Synthetic Fluorphlogopite 3 3 3 - - silicone resin - - - - 5 Aragonite 3 3 [Manufacturing Example 1] 3 [Manufacturing Example 2] - - 2-Octyl Cyanoacrylate 1 0.7 0.5 - - n-butyl cyanoacrylate - 0.3 0.5 - - wax mixture 2 2 2 - - polyethylene wax - - - - 2 Butionine Sulfoxin - 1 1 - - Asphalt: Straight asphalt wax mixture with a penetration of 20 to 40 Mixture: A mixture of ethylene-bis-stearamide (EBS) wax and erucamide wax in a weight ratio of 1:0.6

[0094] The following test examples represent experimental results comparing the characteristics of the embodiments according to the present invention with those of Comparative Examples 1 and 2, so that the characteristics of Examples 1 to 3 according to the present invention disclosed above can be more easily identified.

[0095] <Test Example 1>

[0096] After preparing an asphalt concrete layer with a thickness of about 50 mm using the compositions prepared in Examples 1 to 3 and Comparative Examples 1 to 2 above, water resistance, low-temperature (at -10℃) gelation (confirmation of low-temperature curing ability), porosity, deformation strength, dynamic stability (confirmation of resistance to plastic deformation), hardness, elongation, tensile adhesive strength, and chloride ion penetration were measured and are shown in Table 2 below.

[0097] The above tensile adhesive strength was measured using an asphalt tensile adhesive strength tester, and dynamic stability was measured using a wheel tracking tester.

[0098] division Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Water resistance (%) 94 96 97 78 86 Gelation / 1hr (at -10℃) 63 65 66 42 53 porosity 2.1 2.2 2.4 1.2 1.6 Deformation strength (MPa) 6.76 6.82 6.97 5.10 5.65 Dynamic stability (cycles / mm) 6672 6669 6874 2724 4079 Hardness (Shore A) 81 83 85 63 68 Growth rate (%) 180 190 195 70 110 Tensile adhesive strength (MPa) 1.66 1.73 1.79 0.88 1.12 Chloride ion penetration resistance (coulombs) 53 49 47 187 146

[0099] As can be seen in Table 2 above, the crushed stone mastic asphalt (SMA) concrete compositions with excellent drainage performance according to Examples 1 to 3 were found to have a high porosity compared to the comparative compositions according to Comparative Examples 1 and 2, thereby improving drainage performance, and exhibiting excellent water resistance, deformation strength, dynamic stability, hardness, elongation, tensile adhesive strength, and chloride ion penetration resistance. In addition, it was confirmed that gelation proceeds at low temperatures, allowing for rapid hardening.

[0101] <Test Example 2>

[0102] Dynamic shear test (to verify resistance to plastic deformation), deflection test (to verify resistance to low-temperature cracking), elongation test (to verify resistance to room-temperature cracking), and accelerated weathering were measured and are shown in Table 3 below.

[0103] The above Dynamic Shear Rheometer (DSR) measured the temperature when the G* / sinδ value before aging was 1 kPa and the G* / sinδ value after aging was 2.2 kPa, and the above Bending Beam Rheometer (BBR) measured the temperature when the creep stiffness (S) value derived from the BBR test was 0.3 or higher. In addition, the above accelerated weathering (Xenon, 300hr) was performed according to the ASTM C 793 method, under the conditions of black panel temperature: 633 ℃, relative humidity: 505%, spray cycle: 120 minutes of irradiation followed by 18 minutes of irradiation and water spraying, and radiant intensity: 0.51 W / (340 nm).

[0104] division Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Dynamic shear test (plastic deformation resistance) Before aging (°C) 126 129 133 89 95 After aging (°C) 115 120 128 83 92 Deflection test (°C (low-temperature cracking resistance) -18 -17 -20 -11 -13 Strength test (cm) (crack resistance) 10℃ 41 44 45 21 28 25℃ 55 57 59 34 40 Accelerated weathering strain No issues No issues No issues generation generation peeling No issues No issues No issues generation generation Low-temperature adhesive No issues No issues No issues Cracks and peeling occur cracks

[0105] As can be seen in Table 3 above, the crushed stone mastic asphalt (SMA) concrete compositions with excellent drainage performance according to Examples 1 to 3 showed significantly improved resistance to plastic deformation at high temperatures, resistance to cracking at low temperatures, resistance to cracking at 10°C and 25°C, and accelerated weathering resistance compared to the comparative compositions according to Comparative Examples 1 and 2.

[0107] <Test Example 3>

[0108] Asphalt concrete was constructed by pouring the compositions prepared in Examples 1 to 3 and Comparative Examples 1 to 2 onto a concrete road surface in accordance with the asphalt concrete pavement construction guidelines (Ministry of Land, Infrastructure and Transport), and after applying deterioration conditions (a pressurized-non-pressurized cycle of 10 ton weight continuously at 50°C for 7 days) to the construction surface, CPX (near-field noise) was measured according to the ISO Standard 11819-2.

[0109] In the above CPX (near-field noise) measurement method, mechanical noise such as that from the engine accounts for a large proportion of the total noise generated by the moving vehicle at low speeds, and as the driving speed increases, the proportion of noise generated from tires / pavement increases; therefore, measurements are taken at high speeds when evaluating the degree of noise generation according to the construction surface. As a measurement method, microphones were installed at the front and rear at a distance of 20 cm from the center of the vehicle tire, with a height of 10 cm from the ground, and measurements were taken when the vehicle was traveling at a speed of 90 km / h at an ambient temperature of 20℃.

[0110] division Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 CPX(near-field noise, dB) 83.7 80.4 78. 98.1 93.5

[0111] As can be seen in Table 4 above, it was confirmed that the crushed stone mastic asphalt (SMA) concrete compositions with excellent drainage performance according to Examples 1 to 3 showed a significantly improved near-field noise reduction effect compared to the comparative compositions according to Comparative Examples 1 and 2.

[0113] As explained above, those skilled in the art to which the present invention pertains will understand that the present invention may be implemented in other specific forms without altering its technical concept or essential features. Therefore, all embodiments described above should be understood as illustrative and not restrictive. The scope of the present invention should be interpreted as including all modified or altered forms derived from the meaning and scope of the claims set forth below and their equivalents, rather than from the detailed description above.

Claims

Claim 1 1) 75 to 90 weight% of aggregate mixed with coarse aggregate and fine aggregate in a weight ratio of 40 to 95 : 5 to 60, 2) 0 to 5 weight% of filler, and 3) 5 to 20 weight% of asphalt binder, wherein the asphalt binder comprises 100 weight parts of asphalt; 0.01 to 5 weight parts of plasticizer; 0.1 to 10 weight parts of petroleum resin; 0.01 to 5 weight parts of process oil; 1 to 30 weight parts of styrene-butadiene-styrene (SBS); 0.1 to 10 weight parts of alkyd resin; 0.1 to 5 weight parts of synthetic fluorophlogopite; 0.1 to 5 weight parts of aragonite; and 0.01 to 2 weight parts of a cyanoacrylate-based compound. and contains 0.1 to 5 parts by weight of a wax mixture in which ethylene-bis-stearamide (EBS) wax and erucamide wax are mixed in a weight ratio of 1:0.5 to 1, wherein the aragonite is a microcrystalline cellulose-aragonite composite particle; and the microcrystalline cellulose-aragonite composite particle comprises 100 parts by weight of a glucoside surfactant, 10 to 50 parts by weight of microcrystalline cellulose and trans-stilbene [Cas No. A crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance, characterized by being prepared by a method comprising the steps of: preparing a mixed solution in which 0.1 to 3 parts by weight are mixed; and preparing microcrystalline cellulose-aragonite composite particles by spray-drying a dispersion in which 50 to 100 parts by weight of aragonite are dispersed in 100 parts by weight of the mixed solution; wherein the glucoside surfactant is a mixture in which lauryl glucoside and decyl glucoside are mixed in a weight ratio of 1:0.1 to 0.5; and wherein the cyanoacrylate-based compound is one or more selected from the group consisting of 2-octyl cyanoacrylate, n-butyl cyanoacrylate, and mixtures thereof. Claim 2 delete Claim 3 The crushed stone mastic asphalt (SMA) concrete composition with excellent drainage performance according to claim 1, wherein the aragonite used in the manufacture of the microcrystalline cellulose-aragonite composite particles is surface-treated aragonite, and the surface-treated aragonite is prepared by ball-milling 100 parts by weight of acetone, 10 to 50 parts by weight of aragonite, 1 to 20 parts by weight of xyloglucan, and 1 to 10 parts by weight of hexa(methoxymethyl)melamine for 3 to 5 hours, and then drying. . Claim 4 A crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance according to claim 1, wherein the asphalt binder further contains 0.01 to 5 parts by weight of a sulfoxymin compound per 100 parts by weight of asphalt, and the sulfoxymin compound is one or more selected from the group consisting of butionine sulfoxymin, methionine sulfoxymin, 2-ethylmethionine sulfoxymin, and mixtures thereof. Claim 5 A construction method using a crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance according to any one of claims 1, 3, and 4, comprising: a step of washing and pre-treating a target surface to be constructed; a step of mixing and dispersing a crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance; a pouring step of pouring the mixed and dispersed crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance onto the target surface to be constructed after the washing and pre-treatment are completed; a step of compacting the crushed stone mastic asphalt (SMA) concrete composition having excellent drainage performance after the pouring step is completed to form a pavement layer having a void ratio of 1.5 to 25%; and a curing step of curing after the compaction step is completed.

Citation Information

Patent Citations

  • Sand mastic asphalt concrete composition for thin overlay coating comprising high grade asphalt binder, and constructing method of thin overlay water-inpermeable pavement using the same

    KR102478619B1

  • Sand Mastic Asphalt Concrete Composition with Improved Crack Resistance in Low Temperature and Constructing Methods Using Thereof

    KR102641799B1

  • Mastic Asphalt Concrete Composition and Constructing Methods Using Thereof

    KR102641800B1

  • Crack-Reducing Sand Mastic Asphalt Concrete Composition with Improved Low Temperature Performance of Asphalt Binder and Constructing Methods Using Thereof

    KR102951076B1