Curable carbon nanotube ink and transparent conductive film produced using the ink

The curable CNT ink with a resin binder and diluent addresses adhesion and resistance issues in TCFs, enhancing electrical and optical properties by forming a multilayer structure with metal nanowires or meshes, surpassing non-curable CNT inks in performance.

KR103044463B1Active Publication Date: 2026-11-06CHASM ADVANCED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020237016355
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-13
Filing Date
2021-10-13
Publication Date
2026-11-06
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Existing transparent conductive films (TCFs) using non-curable carbon nanotube (CNT) inks suffer from poor adhesion, wear resistance, and chemical resistance, while maintaining electrical conductivity and transparency, necessitating surfactant removal and additional processing steps.

Method used

A curable CNT ink comprising a radiation-curable or thermosetting resin binder, a viscous diluent, and catalyst, which eliminates the need for surfactants, ensuring adhesion and resistance without additional processing, and a multilayer structure with a metal nanowire or mesh layer for enhanced properties.

Benefits of technology

The curable CNT ink provides improved adhesion, wear resistance, and chemical resistance while maintaining excellent electrical conductivity and transparency, outperforming non-curable CNT inks in TCFs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023053417256-PCT00006_ABST
    Figure 112023053417256-PCT00006_ABST
Patent Text Reader

Abstract

Curable carbon nanotube ink and transparent conductive film manufactured using the ink. The ink comprises a curable resin binder, a catalyst configured to be activated and to cure the resin binder, a viscous-evaporative diluent, and carbon nanotubes (CNT). The concentration of CNT in the ink ranges from about 0.001 wt% to about 0.2 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

Background Technology

[0001] Cross-reference regarding related applications

[0002] This application claims priority to Provisional Application 63 / 090,956 filed on October 13, 2020, the entire contents of which are incorporated herein by reference for all purposes.

[0003] background

[0004] The present disclosure relates to a curable conductive coating.

[0005] Carbon nanotube ink (i.e., conductive coating) can be used as part of a transparent conductive film (TCF).

[0006] summation

[0007] The present invention comprises a curable carbon nanotube (CNT) ink (i.e., a printable conductive coating) and a transparent conductive film (TCF) produced using the ink (e.g., printed). The ink contributes to both the conductivity of the film and its ability to withstand environmental conditions. The ink also serves as an etching mask. The ink contains one or both of a radiation-curable and a thermosetting resin that acts as a binder for the CNTs when the resin is cured, and also promotes good adhesion, abrasion resistance, and chemical resistance. A catalyst facilitates the curing of the resin. The ink also contains a viscous diluent that evaporates completely during the ink drying / curing process. The diluent helps achieve the desired viscosity of the ink so that it can be coated onto an underlying substrate, for example, by screen printing. In some examples, the viscosity of the ink ranges from about 1,000 cP to about 50,000 cP. In some examples, the curable carbon nanotube ink consists of a single-walled carbon nanotube component and a UV and / or thermosetting polymer binder component. CNT ink is a screen-printable ink that does not contain surfactants. Generally, CNTs require surfactants to remain as a dispersion; otherwise, they may aggregate. When a coating containing surfactants is printed or dried, the surfactants must be washed away. If the surfactants are not washed away, the electronic properties of the CNT layer are significantly poor. In this case, the V2V diluent is highly viscous (rheological) to prevent aggregation by ensuring that the particles do not find or come into contact with each other. The diluent is then completely dried, resulting in a conductive coating from the ink without the need to wash away the surfactants.

[0008] The present ink can be used to create TCFs. The TCF comprises a substrate, a metal nanowire coating or a metal mesh (MM) layer on the substrate surface, and an ink on the nanowire or MM layer. After the ink is cured, the resulting multilayer structure exhibits excellent electrical conductivity, high visible light transmittance, and excellent adhesion of the metal nanowire (or metal mesh) / CNT composite structure to the substrate. In some examples, the TCF also comprises a substrate (polymer film, glass panel, etc.) without a metal nanowire or metal mesh coating and with printed CNT ink.

[0009] The present invention gives rise to the production of novel curable carbon nanotube inks and printed films that exhibit the advantages of better adhesion to metal nanowire coatings or metal mesh layers, improved wear resistance, and better solvent resistance and chemical resistance during the etching process compared to TCFs prepared using non-curable CNT inks, while maintaining excellent electrical conductivity, high visible light transmittance, and low blur.

[0010] All examples and features mentioned below can be combined in any technically possible way.

[0011] In one embodiment, the curable carbon nanotube ink comprises a curable resin binder, a catalyst configured to be activated and to cure the resin binder, a viscous-evaporative diluent, and carbon nanotubes (CNT). The concentration of CNT in the ink ranges from about 0.001 wt% to about 0.2 wt%.

[0012] Some examples include one of the above and / or below features, or any combination thereof. In one example, the concentration range of the resin binder in the ink is about 0.1 wt% to about 5 wt%. In one example, the concentration range of the catalyst in the ink is about 0.001 wt% to about 1.0 wt%. In one example, the concentration range of the diluent in the ink is about 90 wt% to about 99 wt%. In one example, the curable carbon nanotube ink further comprises a filler resin having a concentration range in the ink of about 0.1 wt% to about 5 wt%. In one example, the resin binder comprises a mixture of a UV-curable resin and a thermosetting resin. In one example, the curable carbon nanotube ink has a viscosity of about 1,000 cP to about 50,000 cP. In one example, the CNT comprises single-walled CNTs.

[0013] Some examples include one of the above and / or below features, or any combination thereof. In one example, the resin binder is radiation-curable. In one example, the resin binder comprises one or more of a UV-curable polyfunctional acrylic copolymer, a UV-curable urethane polymer, or a UV-curable polyester. In one example, the curable carbon nanotube ink further comprises one or more of a non-UV-curable resin, a polyfunctional oligopolymer, or a monomer. In one example, the catalyst comprises a type I or type II free radical photoinitiator. In one example, the resin binder is thermosetting. In one example, the resin binder comprises one or more of an acrylic copolymer, a urethane polymer, or a polyester having an acidic functional group. In one example, the catalyst comprises at least one of a polyaziridine crosslinker, a polycarbodiimide crosslinker, or a peroxide-type catalyst.

[0014] In another embodiment, a transparent conductive film (TCF) comprises a polymer film substrate, a metal nanowire layer or a metal mesh layer on the surface of the film, and a cured carbon nanotube (CNT) ink covering at least a portion of the metal nanowire layer or the metal mesh layer. The CNT ink comprises a curable resin binder, a catalyst configured to be activated and curing the resin binder, a viscous-evaporative diluent, and CNTs. The concentration of CNTs in the ink ranges from about 0.001 wt% to about 0.2 wt%.

[0015] Some examples include one of the above and / or below features, or any combination thereof. In one example, the TCF exhibits excellent electrical conductivity, high visible light transmittance, and excellent adhesion to a substrate of a metal nanowire layer or metal mesh layer and a cured CNT ink. In one example, the TCF exhibits better adhesion to a metal nanowire layer or metal mesh layer, improved wear resistance, and better solvent resistance and chemical resistance during the etching process compared to a TCF prepared using a non-cured CNT ink. In one example, the TCF maintains excellent electrical conductivity, high visible light transmittance, and low opacity. Brief explanation of the drawing

[0016] Various embodiments of at least one example are discussed below with reference to the attached drawings, which are not intended to be drawn in proportion. The drawings are included to provide further understanding of the examples and various embodiments and examples, and while they constitute part of the specification, they are not intended to define the limitations of the invention. In the drawings, identical or nearly identical components shown in various drawings may be indicated by similar reference letters or numbers. For clarity, not all components are shown in all drawings. In the drawings: Figure 1 is a schematic side view of the TCF. Figures 2A-2D illustrate a method for generating TCF. Figure 3 illustrates the steps of the process for generating TCF. Figure 4 is a graph showing the ink viscosity for different levels of CNT. Specific details for implementing the invention

[0017] Examples of systems, methods, and apparatus discussed herein are not limited to the details of the configuration and arrangement of components presented in the following description or illustrated in the attached drawings. Systems, methods, and apparatus may be implemented in other examples and may be executed or performed in various ways. Examples of specific implementations are provided herein for illustrative purposes only and are not intended to be limiting. In particular, functions, components, elements, and features discussed in connection with one or more examples are not intended to be excluded from similar roles in other examples.

[0018] Examples disclosed herein may be combined with other examples in any manner consistent with at least one of the principles disclosed herein, and references to “examples,” “some examples,” “alternative examples,” “various examples,” “one example,” etc. are not necessarily mutually exclusive and are intended to indicate that the specific features, structures, or characteristics described may be included in at least one example. The appearance of these terms herein does not necessarily refer to the same example.

[0019] Furthermore, the grammar and terminology used herein are for illustrative purposes only and should not be construed as restrictive. Any reference to an example, component, element, action, or function of a computer program product, system, or method mentioned herein in the singular may include a specific example including the plural, and any reference to any example, component, element, action, or function including the plural may include an example including only the singular. Accordingly, references in the singular or plural form are not intended to limit the currently disclosed system or method, its component, action, or element. The use of "including," "comprising," "having," "containing," "involving," and variations thereof in this document means including additional items as well as the items and equivalents listed later. References to "or" may be interpreted as inclusive, so that any term described using "or" may represent a single, two or more, or all of the described terms.

[0020] CNT ink can be printed on flexible and rigid substrates. The substrate may be inorganic and / or organic, including but not limited to glass, silicon wafers, and plastic films of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), thermoplastic polyurethane (TPU), cyclic olefin polymer (COP), silicon or polyimide (CPI). The plastic substrate may have a primer layer or surface treatment to improve surface tension (e.g., corona treatment, flame treatment, other plasma, etc.), and in some examples, the film thickness is in the range of 12.5 microns to 300 microns.

[0021] The substrate of the TCF, the nanowire layer (e.g., silver nanowire (AgNW) or metal mesh (MM) layer) and the method of fabrication according to the present disclosure may be of the type disclosed in International Patent Application Publication No. WO 2016 / 172315 and / or International Patent Application Publication No. WO 2020 / 102392, the entire disclosures thereof are incorporated herein by reference for all purposes.

[0022] In some examples, TCF is produced according to the following procedure.

[0023] Preparation of coating solution:

[0024] Curable CNT Ink:

[0025] UV-curable CNT ink:

[0026] UV CNT ink formulations consist of a viscous-to-vapor ("V2V") diluent that evaporates completely during the ink drying / curing process, a dispersion of CNTs in alcohols and amines, a radiation-curable resin binder, a photoinitiator, and optionally a non-UV-curable resin added to the UV resin mixture. In some examples, the CNT concentration ranges from 0.01 to 2.0 g / L (i.e., about 0.001 wt% to about 0.2 wt% in the ink). In some examples, the concentration ratio of CNT to UV resin or resin mixture binder (CNT / binder) ranges from about 1:1 to about 1:1200.

[0027] V2V diluents help achieve the desired viscosity of an ink so that it can be coated onto a substrate underneath, for example, by screen printing. In some examples, V2V diluents are of the type disclosed in U.S. Patents 9,777,167 and 9,777,168, the full disclosures of which are incorporated herein by reference for all purposes.

[0028] In some examples, UV resin binders include, but are not limited to:

[0029] 1. Multifunctional UV-curable oligomers and monomers, e.g., Allnex’s Ebecryl 4859, Ebecryl 4858, Ebecryl 8701, Ebecryl 8605, Ebecryl 225, Ebecryl 4740, Ebecryl 4859, Ebecryl 8405, Ebecryl 1290, Ebecryl 4738, Ebecryl 4513, Ebecryl 284; Sartomer’s SR 399, SR 368, CN 9210, CN 9276, CN 9196, CN 9209, CN 2306; MIWON’s Miramer M140, Miramer M1 50, Miramer M1 182, Miramer M200, Miramer M262, Miramer M 300, Miramer M 3130, Miramer M 420, Miramer PU 610, Miramer PU6510, Miramer PU5000, Miramer PU640, Miramer Sc2100, Miramer SC2152, Miramer MU 9500.

[0030] 2. Multifunctional UV-curable acrylic copolymers, DSM’s NeoRad-A 20, Allnex’s Ebecryl 4654, Enstron’s Lumicryl U-72 IS, Lumicryl02, Lumicryl2882 and Lumicryl 245.

[0031] In some examples, UV photoinitiators include, but are not limited to, BASF’s Irgacure 651, Irgacure 369, Irgacure 901, Irgacure 84, Irgacure 2959, Irgacure TPO, Irgacure 819 and Darocur 1173, IGM’s Omnirad 500, Esacure kip 160, Esacure kip 100F, Esacure kip 150, Esacure TZT, Esacure 3644, Esacure 1001M, Omnirad 4-PBZ, and Omnirad BP.

[0032] In some examples, non-UV cured (i.e., non-curable) resin binders, when used, are DSM's Neocryl 819, Neocryl 817, Neocryl 890, and Neocryl 813; Includes, but is not limited to, BASF’s Joncryl 857, Joncryl 586, Joncryl 611, Joncryl 678, Joncryl 680, Joncryl 682, Joncryl 683, Joncryl 693, JoncrylECO 675, Joncryl ECO684, Joncryl 817, Joncryl 819, Joncryl 820, Joncryl 821, Joncryl 901, Joncryl 903, Joncryl 843, Joncryl 848, Joncryl 67, Joncryl 690, Joncryl HPD 671 and Joncryl HPD 696.

[0033] Thermosetting CNT ink:

[0034] The thermosetting CNT ink formulation consists of a V2V diluent, carbon nanotubes, a thermosetting resin binder, and a crosslinking agent or crosslinking agent.

[0035] In some examples, the CNT concentration and CNT / binder ratio are as described above.

[0036] In some examples, crosslinkable resin binders include, but are not limited to:

[0037] 1. An acrylic copolymer having a carboxyl functional group, including but not limited to Neocryl 818, Neocryl 819, Neocryl 890 of DSM, and Joncryl 817, Joncryl 819, Joncryl 820, Joncryl 821, Joncryl 901, Joncryl 903, Joncryl 857, Joncryl 586, Joncryl 611, Joncryl 678, Joncryl 680, Joncryl 682, Joncryl 683, Joncryl 693, Joncryl ECO 675, Joncryl ECO684, Joncryl 843, Joncryl 848, Joncryl 67, Joncryl 690, Joncryl HPD 671, and Joncryl HPD 696 of BASF.

[0038] 2. Crosslinkers include the following: (A) DSM’s Crosslinker CX-300 and Crosslinker XL-1; polycarbodiimide crosslinkers including, but not limited to, STAHL’s Picassian® XL-702, XL-712, XL-752, XL-762 and ANGUS’s ZOLDINE® XL-29SE; (B) polyaziridine crosslinkers including, but not limited to, DSM’s Crosslinker CX-100 and NeoAdd™ PAX-521, STAHL’s Picassian® XL-048 and Picassian® XL-706, and Poly Aziridine LLC’s PZ-28 and PZ-33.

[0039] 3. The curing process is dependent on temperature and time.

[0040] UV and Thermal (Double Curing) CNT Ink:

[0041] UV and thermal dual-curing CNT ink formulations consist of a "V2V" diluent, a CNT dispersion in alcohol and / or amine, a binder resin mixture of a radiation-curable acrylic copolymer and an acrylic copolymer having carboxylic acid functional groups, a photoinitiator, and a crosslinking agent. The UV-curable acrylic copolymer, the thermosetting acrylic copolymer having carboxylic acid functional groups, the photoinitiator, and the thermal crosslinking agent are defined above. The CNT concentration and the CNT / binder ratio are as described above.

[0042] Printing process:

[0043] CNT Ink Printing Process:

[0044] Set the 355 polyester mesh screen to a 3 mm snap-off distance.

[0045] Attach an AgNW-coated PET or polycarbonate substrate to a smooth surface with tape.

[0046] Apply ~5 ml of curable CNT ink onto the pattern.

[0047] Fill the screen with CNT ink by drawing fluid over the pattern using a squeegee.

[0048] Ink is sheared onto the substrate through the screen using a ~75-degree squeegee angle, even (uniform) pressure, and speed.

[0049] The coated sample was dried with an airflow for 10 minutes in a convection oven set to 105℃.

[0050] Curing process:

[0051] In the case of a radiation curing system, a coated sample (coating facing the radiation source) is placed under a radiation source, such as a UV lamp, for a specific period to achieve the required radiation dose. The radiation curing setup can be static or a conveyor system. For example, a conveyor UV system is equipped with a mercury, LED, or xenon lamp and the conveyor belt speed is set to achieve a UV curing dose of 1400 mJ / cm², and a UV CNT-coated film is placed at the feed end of the UV conveyor system; the UV curing process is completed after the coated film passes through the UV radiation zone and exits the conveyor system. The UV curing process can also be performed without a conveyor system as long as the dose is in the range of about 400 to about 1800 mJ / cm².

[0052] In the case of the heat curing process, in some examples, the sample is cured at 110°C for 60 seconds (60–600 seconds is a preferred range).

[0053] In the case of a combined UV curing and heat curing process after initial sample drying during the printing process, curing can be performed by primary UV curing / secondary heat curing or primary heat curing / secondary UV curing.

[0054] Pattern Etching Process:

[0055] Subsequently, the radiation-cured sample was sprayed with 1-20% iron nitrate (Fe(NO3)3) in an aqueous solution for 5-200 seconds. Using a separate wash bottle, the sample was then sprayed with deionized water on both sides of the film for 30 seconds. The film was then dried by beating it with a lint-free cloth to remove large water droplets, and then baked in a convection oven at 105°C for 1 minute. Etching may also be performed through an automated system consisting of etching, washing, and drying, which has a motorized film transfer section.

[0056] measurement:

[0057] The electrical characteristics of the sheet resistance of the CNT ink printed film are measured using an R-Check 4-point sheet resistance meter (EDTM product).

[0058] The optical characteristics of total transmittance and transmittance blur are measured with BYK Haze-Guard.

[0059] The ASTM D3359 tape adhesion test is used to measure ink adhesion to a plastic film substrate; any peeling of the printed ink (less than 5B as defined in ASTM D3359) is considered a failure.

[0060] The abrasion test is performed by rubbing the printed ink surface with a cloth, and any removal of the printed ink is considered a failure.

[0061] The ethanol resistance rub test is performed by wiping the surface of the printing ink with a cloth soaked in ethanol, and then the sheet resistance is measured after a drying time of 30 seconds at ambient temperature. After passing 5 repeated wiping tests, if the change in sheet resistance is less than 10% of the original value, the sample is considered to have passed the test.

[0062] The CNT-based hybrid TCF (10) of FIG. 1 comprises an MM layer (13) containing metal traces (14-16) and a CNT ink layer (18) on top that is adhered to the upper surface of a substrate (12) and encapsulates the MM layer (13) with a conductive medium. A circuit pattern is created after any exposed MM (i.e., areas where the CNT ink is not printed) is removed via chemical etching. Note that the circuit pattern may be created alternatively or additionally from a metal nanowire layer rather than a metal mesh layer.

[0063] FIGS. 2A-2D illustrates the results of a process for generating the TCF of the present disclosure. Note that the dimensions and other aspects of FIGS. 2A-2D are for illustrative purposes only and may be out of scale and exaggerated. An actual example is presented below. The assembly (20) of FIG. 2A comprises a substrate (22) having an MM that includes traces (24-27). The MM may be created on the substrate by various means as described herein. Additionally, the MM may include various conductive materials (e.g., metals) as further described. The MM comprises a series of electrically connected thin traces (lines). The traces are typically arranged in a regular pattern, but are not necessarily required to be so.

[0064] FIG. 2B illustrates an additional assembly (30) in which the MM is over-plated with a second metal (in this non-limiting example, the second metal is copper). Thus, traces (24-27) are covered with a generally thicker layer of the second metal containing portions (34-37), creating thicker and less porous MM traces (40-43), respectively.

[0065] FIG. 2C illustrates an additional assembly (50) in which CNT ink (48) is printed or otherwise placed over part or all of the MM layer shown in FIG. 2B. In this illustration, the ink (48) is printed over traces (41 and 42) but not over traces (40 and 43). Thus, traces (40 and 43) are exposed, while traces (41 and 42) are covered by a conductive medium that creates a conductive line or conductive area (49).

[0066] FIG. 2D illustrates the final TCF (60) in which the exposed traces (40 and 43) are removed by etching, as described in more detail elsewhere in the present invention. This leaves a conductor (49) on the substrate (22).

[0067] An exemplary method (70) for generating a TCF is illustrated in FIG. 3. In step (72), a suitable substrate is provided. In step (74), a metal mesh is printed on the surface of the substrate. In step (76), a second metal (e.g., copper) is plated onto the metal mesh. Step (76) is optional, and there may not be a need to increase the thickness (i.e., height) of the MM line, such as when the MM itself has an acceptable Rs. The added plated metal increases the volume of the MM trace, thereby reducing resistance. Additionally, this can help make the thin MM more rigid and allow it to bond better with the conductive ink. In step (78), a curable conductive medium (referred to as "ink") is printed onto selected areas of the MM to form part of the circuit. In one example, the curable ink contains carbon nanotubes as the conductive medium and also contains a binder and other components as described herein. CNT ink is further described elsewhere in this invention. In step (80), the ink is cured in a manner suitable for the specific ink and as further described elsewhere in this invention. The final step (82) involves etching the exposed MM / copper to leave only the circuit on the substrate.

[0068] Figure 4 is a graph illustrating ink viscosity for different levels of CNT. As evidenced by the curve in Figure 4, the CNT concentration has a direct effect on the viscosity of the ink. Generally, the ink of the present invention is screen printed using conventional printing techniques and must have a viscosity in the range of about 1,000 cp to about 50,000 cp to be useful without the need for surfactants as discussed above. In the ink, 1 gram / liter of CNT is equivalent to about 0.1%, which is equivalent to a viscosity of about 50,000 cp. From the viscosity graph in Figure 4, it is evident that including 3 grams / liter of CNT could push the ink to millions of cp, a region unusable for printing. Even 0.2% CNT would be estimated to be about 700,000 cp.

[0069] Desirable specific example result:

[0070] Performance:

[0071] UV and / or thermosetting CNT inks offer the advantages of excellent adhesion to substrates with a layer of metal nanowire coating or a metal mesh layer, excellent wear resistance during the etching process, and chemical resistance, while maintaining equivalent electrical and optical properties and blur number of VLT compared to TCF designs using the same but non-curing resin binder.

[0072] Example 1:

[0073] UV-curable CNT ink with a CNT concentration of 0.1 g / l and a CNT / binder ratio of 1:120. The binder resin consists of Enstron’s UV-curable polymer Lumicryl 245 60% wt and DSM’s non-UV-curable polymer Neocryl B-890 40% wt. The photoinitiator Esacure KIP 100F is used with a photoinitiator-to-binder ratio of 1:50. A non-UV-curable CNT ink (identified as VC200) was tested for comparison (as a control baseline). VC200 has the same CNT, polymer binder, and diluent concentrations as the UV CNT ink, but the resin binder is a non-curable thermoplastic polymer, e.g., 100% NeoCryl® B-890.

[0074] UV CNT ink and VC200 were screen printed onto a C3 Nano AgNW-coated PET film (125 μm thickness) with a sheet resistance of 30 + / - 2 Ω / □. The screen mesh size was 305, and the drying conditions were described above. Subsequently, the UV CNT ink printed samples were UV cured with a UV irradiation dose of 1400 mJ / cm². The UV-cured samples and the coated VC200 samples were subsequently etched with 10% iron nitrate (Fe(NO3)3) in an aqueous solution for 12 seconds, then washed with deionized water and oven-dried as described above. Performance tests were performed on the dry-etched samples, and the test results are listed in Table 1. The tests were repeated for C3 Nano AgNW PET films with sheet resistances of 10 Ω / □ and 75 Ω / □.

[0075] The test data listed in Tables 1A, 1B, and 1C clearly demonstrate that UV-cured CNT ink exhibits superior adhesion performance to AgNW film substrates and excellent wear resistance and solvent resistance compared to the VC200 control group using non-cured CNT ink.

[0076] Table 1A, VC200 and UV CNT inks printed on C3 Nano 30 Ω / □ PET film

[0077]

[0078] Table 1B, VC200 and UV CNT inks printed on C3 Nano 10 Ω / □ PC film

[0079]

[0080] Table 1C, C3 VC200 and UV CNT inks printed on Nano 75 Ω / □ PET film

[0081]

[0082] Example 2:

[0083] A thermosetting CNT ink with a CNT concentration of 0.1 g / l and a CNT / binder ratio of 1:120. The binder resin consists of BASF's carboxylic acid functional acrylic resin Joncryl HPD 671 and DSM's curing agent CX-100, with a crosslinker-to-polymer ratio of 1:12. A non-curing CNT ink, VC200, was tested for comparison. VC200 has the same CNT concentration of 0.1 g / l and a CNT / polymer binder ratio of 1:120 as the thermosetting CNT ink.

[0084] Thermosetting CNT ink and VC200 were screen printed onto a C3 Nano AgNW-coated PET film (125 μm thickness) with a sheet resistance of 75 + / - 2 Ω / □ (screen size 305). The printed film samples were dried in a conveyor belt oven set to 110°C for a drying time of 180 seconds. The thermosetting samples could be cured at ambient temperature for 120 hours or accelerated cured at 110°C for 600 seconds. The VC200 printed and thermosetting samples were subsequently etched with 10% iron nitrate (Fe(NO3)3) in an aqueous solution for 12 seconds, then washed with deionized water and dried in an oven at 110°C for 60 seconds. Performance tests followed, and the results are listed in Table 2. The curable ink exhibits excellent performance in resistance to abrasion, solvent wiping, and etching.

[0085] Table 2, VC200 and UV CNT inks printed on C3 Nano 75 Ω / □ PET film

[0086]

[0087] Example 3:

[0088] A dual-curing CNT ink with a CNT concentration of 0.1 g / l and a CNT / binder ratio of 1:120. The binder resin consists of Enstron's UV-curable polymer Lumicryl 245 30% wt, BASF's carboxylic acid functional resin Joncryl HPD 671 70 wt%, IGM's type II photoinitiator Omnirad 4PBZ and release agent Esacure A198, and DSM's thermosetting agent CX-100. A non-curing CNT ink, VC200, was tested for comparison. VC200 has the same CNT concentration of 0.1 g / l and a CNT / polymer binder ratio of 1:120 as the dual-curing CNT ink.

[0089] Dual-curable CNT ink and VC200 were screen-printed onto a C3 Nano AgNW-coated PET film (125 μm thickness) with a sheet resistance of 75 + / - 2 Ω / □ (screen size 305). The printed film samples were dried in a conveyor belt oven set to 110°C for a drying time of 180 seconds. The samples were subsequently UV-cured with a UV irradiation dose of 1400 mJ / cm², followed by thermal curing at 110°C for 600 seconds. The cured samples were then etched with 10% iron nitrate (Fe(NO3)3) in an aqueous solution for 12 seconds. Performance tests followed, and the results are listed in Table 3. The dual-curable ink exhibits superior performance in etching resistance compared to UV-curable alone and thermal-curable alone CNT inks.

[0090] Table 3, VC200, UV / thermal dual-curing, UV-curing, and thermal-curing CNT inks printed on C3 Nano 75 Ω / □ PET film

[0091]

[0092] Although various embodiments of at least one example have been described above, it should be understood by those skilled in the art that various changes, modifications, and improvements will readily occur. Such changes, modifications, and improvements are intended to be part of the present disclosure and within the scope of the invention. Accordingly, the foregoing description and drawings are merely examples, and the scope of the invention should be determined from the appropriate configuration of the appended claims and their equivalents.

Claims

Claim 1 A curable, electrically conductive, screen-printable carbon nanotube ink configured to be screen-printed onto a substrate and then cured to be coated onto the substrate, comprising: a curable resin binder; a catalyst configured to be activated to cure the resin binder; and an evaporable viscous-evaporative diluent configured to completely evaporate during the curing of the curable carbon nanotube ink occurring after the ink is applied to the substrate. A curable, electrically conductive, screen-printable carbon nanotube ink comprising carbon nanotubes (CNT); wherein the concentration range of CNTs in the curable carbon nanotube ink is 0.001 wt% to 0.1 wt%, the concentration range of an evaporative viscous-evaporative diluent in the curable carbon nanotube ink is 90 wt% to 99 wt%, and the weight ratio of curable carbon nanotubes to curable resin binders in the curable carbon nanotube ink is 1:120 to 1:1,200, and wherein the curable carbon nanotube ink has a viscosity of 1,000 cP to 50,000 cP sufficient to allow the ink to be screen-printed on a substrate. Claim 2 A curable, electrically conductive, screen-printable carbon nanotube ink according to claim 1, wherein the concentration range of the curable resin binder in the ink is 0.1% to 5% by weight. Claim 3 A curable, electrically conductive, screen-printable carbon nanotube ink according to claim 1, wherein the catalyst concentration range in the ink is 0.001% to 1.0% by weight. Claim 4 delete Claim 5 A curable, electrically conductive, screen-printable carbon nanotube ink according to claim 1, further comprising a filler resin having a concentration range in the ink of 0.1% to 5% by weight. Claim 6 In claim 1, the resin binder is a radiation-curable, curable, electrically conductive, screen-printable carbon nanotube ink. Claim 7 In paragraph 6, the resin binder is a curable, electrically conductive, screen-printable carbon nanotube ink comprising one or more of a UV-curable polyfunctional acrylic copolymer, a UV-curable urethane polymer, or a UV-curable polyester. Claim 8 In claim 7, a curable, electrically conductive, screen-printable carbon nanotube ink further comprising one or more of a non-UV curable resin, a polyfunctional oligopolymer, or a monomer. Claim 9 In claim 6, the catalyst is a curable, electrically conductive, screen-printable carbon nanotube ink comprising a type I or type II free radical photoinitiator. Claim 10 In claim 1, the resin binder is a thermosetting, curable, electrically conductive, screen-printable carbon nanotube ink. Claim 11 In paragraph 10, the resin binder comprises one or more of an acrylic copolymer, a urethane polymer, or a polyester having an acidic functional group, a curable, electrically conductive, screen-printable carbon nanotube ink. Claim 12 In claim 10, the catalyst comprises at least one of a polyaziridine crosslinking agent, a polycarbodiimide crosslinking agent, or a peroxide-type catalyst, a curable, electrically conductive, screen-printable carbon nanotube ink. Claim 13 In claim 1, the resin binder comprises a mixture of a UV-curable resin and a thermosetting resin, a curable, electrically conductive, screen-printable carbon nanotube ink. Claim 14 delete Claim 15 In claim 1, the CNT is a curable, electrically conductive, screen-printable carbon nanotube ink comprising single-walled CNTs. Claim 16 A transparent conductive film (TCF) comprising: a polymer film substrate; a metal nanowire layer or a metal mesh layer on the surface of the film; and a cured electrically conductive, screen-printable carbon nanotube (CNT) ink covering at least a portion of the metal nanowire layer or the metal mesh layer, wherein the cured CNT ink comprises a curable resin binder and an evaporable viscous-evaporative diluent configured to completely evaporate during the curing of the curable carbon nanotube ink occurring after the ink is applied to the substrate; A transparent conductive film (TCF) comprising carbon nanotubes (CNT); wherein the concentration range of CNTs in the curable carbon nanotube ink is 0.001% to 0.1% by weight, the concentration range of an evaporative viscous-evaporative diluent in the curable carbon nanotube ink is 90% by weight to 99% by weight, and the weight ratio of curable carbon nanotubes to curable resin binders in the curable carbon nanotube ink is 1:120 to 1:1,200, and wherein the curable carbon nanotube ink has a viscosity of 1,000 cP to 50,000 cP sufficient for the ink to be screen printed on a substrate. Claim 17 In claim 16, a TCF showing electrical conductivity, visible light transmittance, and adhesion of a metal nanowire layer or metal mesh layer and a cured CNT ink to a substrate. Claim 18 In claim 16, a TCF showing adhesion to a metal nanowire layer or a metal mesh layer, improved wear resistance, and solvent resistance and chemical resistance during the etching process compared to a TCF prepared using a non-curing CNT ink. Claim 19 delete Claim 20 In paragraph 16, a TCF further comprising a metal plated on a metal mesh layer to increase the volume of the metal mesh and reduce resistance.

Citation Information

Patent Citations

  • Metal nanowire inks for the formation of transparent conductive films with fused networks

    KR1020170039253A

  • Liquid formulations for coating and printing substrates

    JP2008500448A

  • carbon nanotube dispersion

    JP2012502144A

  • Transparent conductive laminate and method for producing transparent conductive laminate

    JP2020024916A

  • Coating composition for transparent electrode and transparent conductive film including the same

    KR1020150097875A