Absorbent composite containing embossed superabsorbent material

Micro-embossing SAM particles with controlled pressure increases surface area, addressing low absorption rates and leaks in absorbent products, resulting in faster fluid uptake and thinner, more flexible products.

KR103044501B1Active Publication Date: 2026-11-06KIMBERLY CLARK WORLDWIDE INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
KR1020227040783
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-30
Filing Date
2021-03-18
Publication Date
2026-11-06
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Conventional absorbent products containing superabsorbent materials (SAMs) suffer from low absorption rates and premature leaks due to the reduction in surface area and mechanical properties when compressed, leading to inefficient fluid absorption and increased leakage.

Method used

The surface area of SAM particles is increased through micro-embossing with an embossing roller at specific pressures, creating patterns ranging from 100 μm to 1000 μm, which enhances absorption capacity and flexibility.

Benefits of technology

The embossed SAM particles demonstrate significantly faster absorption rates and reduced product thickness, minimizing leaks and improving skin dryness in absorbent products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022124321618-PCT00002_ABST
    Figure 112022124321618-PCT00002_ABST
Patent Text Reader

Abstract

An absorbent composite containing an embossed superabsorbent material and a method for manufacturing the absorbent composite containing the embossed superabsorbent material are described herein. The absorbent composite has a significantly improved absorption rate. The composition and method described herein are useful in various absorbent products.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] Cross-reference regarding related applications

[0002] This application claims priority to U.S. provisional patent application No. 63 / 017,886 filed on April 30, 2020, the contents of which are incorporated herein by reference in their entirety.

[0003] Technology field

[0004] The present invention relates to an absorbent composite comprising an embossed superabsorbent material and a method for manufacturing an absorbent composite containing an embossed superabsorbent material. The absorbent composite has a significantly improved absorption rate compared to conventional absorbent composites. The composition and method according to the present invention are useful in various absorbent products. Background Technology

[0005] Superabsorbent materials (SAMs) are three-dimensional networks capable of absorbing and retaining physiological fluids, such as water (or other aqueous media) and urine and blood, at levels exceeding several hundred times their own dry weight, generally depending on the ion concentration of the aqueous solution. SAMs are applied in various fields, including medicine, personal hygiene products, biomaterials, biosorbents, and agriculture. SAMs were industrially developed in Japan and the United States for hygiene applications in the early 1980s. Due to their potential to replace lint, SAMs have been found to be a cost-effective alternative for use in hygiene products such as baby diapers and feminine hygiene products.

[0006] The benefits of using SAM to replace lint in absorbent products include higher absorption capacity and thinner, more flexible absorbent cores and products. One requirement for using SAM to replace lint in absorbent products is that the SAM must have a higher absorption rate to maximize the use of available capillary space and to compensate for the reduction of lint fibers, which are typically absorbed quickly. Accordingly, the object of the present invention is to provide a method for manufacturing a SAM sheet exhibiting an increased water absorption rate that enables thinner and more flexible absorbent products.

[0007] According to previous studies, absorbent products such as baby diapers and feminine hygiene products with a high SAM content (i.e., 70 wt%) leak prematurely as a result of a high amount of free fluid. Approximately 75% of leaks occur within 90 seconds of elimination. Additionally, 20 to 50% of leaks occur during the first elimination and under low loads. Therefore, there is a high need for SAMs that can rapidly absorb fluid and reduce the amount of free fluid during the use of absorbent products. This removal of excess free fluid from absorbent products can reduce leaks and improve skin dryness.

[0008] The suction velocity of SAM particles can be influenced by surface area and surface energy. A larger surface area results in a faster suction velocity. Furthermore, a faster suction velocity improves total fluid absorption by minimizing free fluid. Therefore, absorbent products with faster suction velocities absorb free fluid in a more efficient manner.

[0009] Embossing methods are known to increase the surface area of ​​conventional absorbent materials. However, compressing SAM particles can damage the particles and reduce their effectiveness. Specifically, the high pressure applied during the compression of SAM particles can impair their mechanical properties. Compressed SAM particles can reduce the pore volume, thereby reducing the absorption capacity.

[0010] A novel solution to the problem of low absorption rates in absorbent products containing SAM particles is described herein. The surface area of ​​the SAM particles is increased by embossing the particles into a micron-sized pattern. In this way, the surface area of ​​individual SAM particles can be increased. This embossing technique can be applied to any material containing SAM particles, such as a SAM sheet or a flexible absorbent binder (FAB) film.

[0011] The composition and method according to the present invention are useful for a variety of absorbent products, including but not limited to personal hygiene products, wet wipes, bibs, wound dressings, food packaging materials, baby and adult diaper products, feminine pads, arm bands, agricultural and pet products containing superabsorbent components, and superabsorbent composites having lint. The increased absorption rate can help reduce leakage of the product; and the embossing on the SAM particles can also help reduce the thickness of the product and increase its flexibility. Prior art literature

[65535] Patent Document 1: EP 1800638 A1 Patent Document 2: WO 2014 / 145312 A2 Patent Document 3: WO 2015 / 171972 A1 Patent Document 4: US 2018-0243139 A1 Patent Document 5: US 2009-0123707 A1 Patent Document 6: US 7833377 B2

[0012] In one embodiment of the present invention, an absorbent composite is provided herein. The absorbent composite comprises a plurality of superabsorbent particles micro-embossed with an average major dimension in the range of about 100 μm to about 1000 μm.

[0013] In another embodiment of the present invention, a method for manufacturing an absorbent composite is provided. The method comprises (i) contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins; and (ii) embossing the plurality of superabsorbent particles with the embossing roller at a pressure ranging from about 125 psi to about 1000 psi, wherein the plurality of superabsorbent particles are micro-embossed to an average major dimension ranging from about 100 μm to about 1000 μm.

[0014] In another embodiment of the present invention, a method for manufacturing an absorbent composite is provided. The method comprises: (i) contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins; and (ii) transferring the plurality of superabsorbent particles to the embossing roller to directly emboss the plurality of superabsorbent particles with the plurality of pins, wherein the plurality of superabsorbent particles are micro-embossed with an average major dimension in the range of about 100 μm to about 1000 μm. Brief explanation of the drawing

[0015] FIG. 1 is an exemplary embodiment illustrating a 1" x 1" metal pattern plate having protruding balls (spheres) with a diameter of 250 μm, used to produce embossed SAM and SAM-containing material according to the present invention, wherein the sides of the balls face downward toward the SAM sheet. FIG. 2 is an exemplary embodiment illustrating a SAM sheet having an embossing pattern on its surface according to the present invention. FIG. 3a shows a test beaker containing 30 mL of NaCl solution and a blue dye in an exemplary example illustrating a test process to compare the absorption characteristics of an unembossed SAM sheet sample and an embossed SAM sheet sample according to the present invention. FIG. 3b illustrates the time (0 min) when the test was started by adding the SAM sheet to each NaCl solution in an exemplary example showing a test process to compare the absorption capacity characteristics of an unembossed SAM sheet sample and an embossed SAM sheet sample according to the present invention. FIG. 3c illustrates the completion of liquid absorption for the embossed sample at 27 minutes in an exemplary embodiment showing a test process to compare the absorption characteristics of an unembossed SAM sheet sample and an embossed SAM sheet sample according to the present invention. FIG. 3d shows an exemplary embodiment illustrating a test process to compare the absorption capacity characteristics of an unembossed SAM sheet sample and an embossed SAM sheet sample according to the present invention, in which swollen embossed SAM particles are cast onto a blank sheet to confirm the complete absorption of fluid. FIG. 3e shows an exemplary embodiment illustrating a test process to compare the absorption capacity characteristics of an unembossed SAM sheet sample and an embossed SAM sheet sample according to the present invention, in which swollen unembossed SAM particles are cast onto a blank sheet to confirm complete absorption of fluid. FIG. 4a illustrates the start of the test (0 seconds) in an exemplary embodiment showing a test process for comparing the absorption characteristics of an unembossed FAB film sample and an embossed FAB film sample according to the present invention. FIG. 4b shows an exemplary embodiment illustrating a test process to compare the absorption characteristics of an unembossed FAB film sample and an embossed FAB film sample according to the present invention, in which once an NaCl solution is dropped onto each film sample, the embossed sample shows immediate absorption of the liquid and distributes it in all directions within the film. FIG. 4c shows an exemplary embodiment illustrating a test process for comparing the absorption characteristics of an unembossed FAB film sample and an embossed FAB film sample according to the present invention, starting at 12 seconds, the unembossed sample showed absorption behavior for the fluid and began distributing the liquid in all directions within the film. FIG. 4d is an exemplary embodiment showing a test process for comparing the absorption capacity characteristics of an unembossed FAB film sample and an embossed FAB film sample according to the present invention, and at 15 seconds, it can still be seen that for the unembossed sample, the central suction zone has a higher fluid volume compared to the surrounding zone. Specific details for implementing the invention

[0016] Generally speaking, the present invention relates to a number of embodiments of a novel absorbent composite comprising a plurality of superabsorbent particles. In many embodiments, some or all of the superabsorbent particles are micro-embossed in a specific manner to increase the overall performance of the superabsorbent particles in a product, for example, such as an absorbent product. The superabsorbent particles present in the absorbent composite may be present in one or more different forms according to the present invention and may be micro-embossed in one or more preferred patterns.

[0017] In many embodiments, the absorbent composite according to the present invention comprises a plurality of superabsorbent particles micro-embossed with an average major dimension in the range of about 100 μm to about 1000 μm, but other average major dimensions may also be within the scope of the present invention. The entire superabsorbent particle or only a desired portion may be micro-embossed with a desired average major dimension depending on the intended use of the superabsorbent particle. In some embodiments, the plurality of superabsorbent particles may be in a form selected from the group consisting of glass particles, gels, fibers, beads, solids, pastes, SAM sheets, FAB films, and combinations thereof.

[0018] In some specific embodiments of the present invention, a plurality of superabsorbent particles are micro-embossed with an average major dimension ranging from about 100 μm to about 900 μm. In some specific embodiments of the present invention, a plurality of superabsorbent particles are micro-embossed with an average major dimension ranging from about 100 μm to about 300 μm.

[0019] A plurality of superabsorbent particles may have various sizes and size distributions. In some embodiments of the present invention, a plurality of superabsorbent particles are in a size range of about 300 to 600 μm. In some embodiments of the present invention, a plurality of superabsorbent particles are in a size range of about 90 to 300 μm. In some embodiments of the present invention, a plurality of superabsorbent particles are in a size range of less than about 90 μm. In some specific embodiments of the present invention, a plurality of superabsorbent particles are selected from the group consisting of a first plurality of superabsorbent particles in a size range of about 300 to 600 μm, a second plurality of superabsorbent particles in a size range of about 90 to 300 μm, a third plurality of superabsorbent particles in a size range of less than about 90 μm, and combinations thereof.

[0020] In some embodiments, a plurality of superabsorbent particles are micro-embossed with a pattern selected from the group consisting of homogeneous patterns and heterogeneous patterns. The pattern may include any geometric shape that increases the surface area of ​​the superabsorbent particles.

[0021] In some embodiments, a plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of geometric patterns, random patterns, symmetric patterns, asymmetric patterns, spheres, cubes, pyramids, and combinations thereof.

[0022] In some embodiments, a plurality of superabsorbent particles are micro-embossed with average major dimensions selected from diameter, major axis, length, width, and height.

[0023] In many embodiments, most of the multiple superabsorbent particles can be micro-embossed. In some embodiments, most of the plurality of superabsorbent particles are greater than about 50%, greater than about 51%, greater than about 52%, greater than about 53%, greater than about 54%, greater than about 55%, greater than about 56%, greater than about 57%, greater than about 58%, greater than about 59%, greater than about 60%, greater than about 61%, greater than about 62%, greater than about 63%, greater than about 64%, greater than about 65%, greater than about 66%, greater than about 67%, greater than about 68%, greater than about 69%, greater than about 70%, greater than about 71%, greater than about 72%, greater than about 73%, greater than about 74%, greater than about 75%, greater than about 76%, greater than about 77%, greater than about 78%, greater than about 79%, greater than about 80%, greater than about 81%, greater It means an amount greater than 82%, greater than approximately 83%, greater than approximately 84%, greater than approximately 85%, greater than approximately 86%, greater than approximately 87%, greater than approximately 88%, greater than approximately 89%, greater than approximately 90%, greater than approximately 91%, greater than approximately 92%, greater than approximately 93%, greater than approximately 94%, greater than approximately 95%, greater than approximately 96%, greater than approximately 97%, greater than approximately 98%, greater than approximately 99%, or 100%. In some specific embodiments, all of the plurality of superabsorbent particles are micro-embossed.

[0024] In some embodiments, the superabsorbent polymer does not contain a crosslinking agent. In some embodiments, the superabsorbent polymer contains one or more crosslinking agents. In some embodiments, the superabsorbent polymer contains two or more crosslinking agents. In some embodiments, the absorbent composite comprises a crosslinking agent selected from the group consisting of tetraallyloxyethane, N,N'-methylene bisacrylamide, N,N'-methylene bismethacrylamide, trialylamine, trimethylolpropane triacrylate, glycerol propoxytriacrylate, divinylbenzene, N-methylol acrylamide, N-methylol methacrylamide, glycidyl methacrylate, polyethylene polyamine, ethyl diamine, ethyl glycol, glycerin, tetraallyloxyethane and pentaerythritol, aluminate, silica, trialyl ether of alumosilicate, and combinations thereof.

[0025] The amount of the crosslinking agent may vary, but is typically present in an amount of about 0.005 to about 1.0 mol% based on the moles of the ethylenically unsaturated monomer compound(s). In some embodiments, the crosslinking agent is present in an amount ranging from about 0.005 mol% to about 1.0 mol%.

[0026] In some embodiments, the absorbent complex comprises 2-acrylamido-2-methylpropanesulfonic acid, a methacrylate monomer having a tethered sulfate group, a salt of a vinyl-linker-acid unit, a salt of a vinyl-linker-acid unit, a vinyl sulfate monomer, acrylic acid, vinyl sulfonic acid, vinyl phosphoric acid, partially hydrolyzed maleic anhydride, carboxymethylcellulose, sodium alginate, a chitosan salt, modified starch, modified soy protein, and combinations thereof.

[0027] In some embodiments, the absorbent composite is used in consumer products. In some embodiments, the consumer product includes the absorbent composite.

[0028] In some embodiments, a method of using an absorbent composite according to the present invention includes using the absorbent composite in a consumer product.

[0029] In some embodiments, consumer products are selected from the group consisting of cloth products, wet wipes, napkins, bibs, disposable bed liners, wound dressings, food packaging materials, baby and adult diaper products, feminine pads, arm bands, agricultural and pet products, and combinations thereof.

[0030] The absorbent composite according to the present invention may be processed and / or manufactured according to any suitable method. In one specific embodiment, the method may include the steps of contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins, and embossing the plurality of superabsorbent particles with the embossing roller at a pressure ranging from about 125 psi to about 1000 psi. In this method, the plurality of superabsorbent particles are micro-embossed with an average major dimension ranging from about 100 μm to about 1000 μm. The superabsorbent particles may also be combined with a composite material such as lint to form a superabsorbent composite.

[0031] An absorbent composite according to the present invention may be manufactured according to a method comprising the steps of: contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins; and transferring the plurality of superabsorbent particles to the embossing roller to directly emboss the plurality of superabsorbent particles with the plurality of pins. In this method, the plurality of superabsorbent particles are micro-embossed with an average major dimension in the range of about 100 μm to about 1000 μm. The superabsorbent particles may also be combined with a composite material such as lint to form a superabsorbent composite.

[0032] The above-described method for preparing an absorbent composite of the present invention may include the use of one or more heating cycles during an embossing step. In some embodiments, the above-described method according to the present invention includes an embossing step in which no heat is applied substantially or completely. In other embodiments, heat may be applied in some embossing steps but not in others.

[0033] yes

[0034] It is assumed that those skilled in the art can make the most of the present invention using the preceding description without further detailed explanation. Accordingly, the following embodiments are to be interpreted merely as illustrative and do not limit the invention in any way.

[0035] Prepare SAM sheets.

[0036] Due to the stiffness of individual SAM particles, it is very difficult to reshape SAM particles through surface cross-linking. Therefore, plasticization and softening of these SAM particles are required. In this case, water (H2O) is applied to the SAM particles as a plasticizer. Other plasticizers, namely glycerol or other polymers with small molecular weights, may also be used to soften the SAM particles.

[0037] The SAM used in the SAM sheet of the embodiment of the present invention is SG200. SG200 is a white, odorless, free-flowing powder capable of absorbing solution. It is a cross-linked and partially neutralized sodium acrylate polymer that is classified to reduce dust and chemically treated to prevent caking. 9% of the particles are larger than 600 μm, 70% of the particles are within a size range of about 300–600 μm, 20.5% of the particles are within a size range of about 90–300 μm, and 0.5% of the particles are smaller than 90 μm. The apparent density of SG200 is 0.61 g / cc. It has a residual monomer amount of about 60 ppm.

[0038] Ten grams of superabsorbent particles (SG200) were spread onto bell glass and placed in a humidity chamber at 80% relative humidity (RH) for 12 hours. After humidity treatment, the SAM particles became soft and sponge-like. Two grams of plasticized SAM were weighed and carefully spread between two flat metal sheets to ensure no gaps existed between the particles. A Carver automatic hydraulic compressor (CE, Model 4350) compressed the SAM particles into a thin SAM sheet by applying an 18,000 lb load for 5 minutes. The resulting SAM sheet was opaque in color and highly elastic. Two SAM sheets were prepared for contrast and compression embossing, respectively.

[0039] Comparative Example 1. SAM sheet without embossing.

[0040] A 1g compressed SAM sheet was formed without embossing. To ensure that Comparative Example 1 had the same density as Example 1—that is, to ensure that both samples experienced the same compression pressure—the SAM sheets were each placed between two flat metal plates and compressed twice for 10 minutes at a load of 1000 lb using a Carver hydraulic compressor (CE, Model 4350). In this way, the void volume between the SAM particles and the void volume within the SAM particles were very similar for Comparative Example 1 and Example 1, even if not identical. The samples were tested after being dried in a convection oven at 80°C for 12 hours.

[0041] Example 1. Embossed SAM sheet.

[0042] A 1g compressed SAM sheet was formed without embossing. The prepared SAM sheet was placed on a flat metal plate and covered with a 1" x 1" metal pattern plate having protruding balls with a diameter of 250μm, with the sides of the balls facing downward toward the SAM sheet (Fig. 1). A Carver hydraulic compressor (CE, Model 4350) was used to create an embossing pattern by applying a 1000 lb load to the plasticized SAM sheet for 5 minutes. Subsequently, the SAM sheet was flipped over under the same pressure and residence time and compressed once more with the metal balls. The resulting SAM sheet has a distinct pattern on its surface (Fig. 2). The scale bar indicates a dent diameter of 243μm. The size of the dents corresponds to the size of the metal balls on the embossing plate.

[0043] The final 1g compressed SAM sheet had double-sided embossing. The sample was tested after drying in a convection oven at 80°C for 12 hours.

[0044] The protrusion of the present embodiment is ball-shaped, but the protrusion of the pin may be of any shape. A shape without sharp edges, such as a sphere, may cause less damage to the SAM particles. The depth of the indentation from that shape may be in the range of about 10 μm to 200 μm.

[0045] Absorption capacity evaluation.

[0046] Equal masses of embossed SAM sheet samples and unembossed SAM sheet samples were each individually dropped into a 100 mL beaker containing 30 mL of NaCl solution, which contained a blue dye to improve visualization during the test. The time and process of the SAM sheets completely absorbing the salt solution were monitored and compared.

[0047] The test process for two samples to compare the absorption characteristics of the two samples is illustrated in Figures 3a to 3e. Figure 3a shows a test beaker containing 30 mL of NaCl solution and blue dye. Figure 3b shows the start of the test (0 min) by adding SAM sheets to each NaCl solution. Figure 3c shows the completion of liquid absorption for Example 1 at 27 min. After completion, the swollen SAM particles were cast onto a white sheet of paper to confirm the complete absorption of the fluid (Figure 3d). At 40 min, Comparative Example 1 completed absorbing all the fluid and was cast onto a white sheet of paper to confirm completion (Figure 3e). When Comparative Example 1 was cast onto the white sheet of paper, Example 1 had completed the absorption process 13 minutes earlier and had already turned white because the absorbed fluid had already diffused to the center of each SAM particle. The absorption times are summarized in Table 1.

[0048] Absorption time for SAM sheets. Sample Inhalation time (minutes) Comparative Example 1 40 Example 1 27

[0049] Compressing SAM particles into sheets generally results in lower inhalation rates and longer inhalation times compared to SAM particles that are not compressed into sheets, due to the loss of free volume within the SAM molecular structure and surface area. However, the results presented herein demonstrate that SAM with surface embossing can lead to an increase in surface area, and consequently, increase the absorption inhalation rate compared to SAM compressed without embossing.

[0050] Flexible absorbent binder film.

[0051] FAB is a patented cross-linked acrylic acid copolymer that develops absorbent properties after being applied to a substrate and dried. While FAB itself can also be cast into a film and dried, the resulting 100% FAB film is significantly rigid and stiff. The chemical properties of FAB are similar to standard SAP, except that the latent cross-linking component can be applied as an aqueous solution onto a selected substrate and then converted into a superabsorbent coating upon drying. When water is removed, cross-linking agent molecules within the polymer chains come into contact with each other and form covalent bonds, creating a cross-linked absorbent.

[0052] In an embodiment of the present invention, a FAB was coated onto a nonwoven substrate to provide a single layer having both suction and retention functions as well as flexibility. A FAB solution having a solid content of 32% (wt / wt) was coated onto a nonwoven substrate through a slot die with two rolls. After coating, the coated film was dried in a convection oven at 55°C for 20-30 minutes, or cured until the film was dried to remove water.

[0053] Compression embossing was applied to the FAB film. Double-sided embossing was applied to the FAB film. Absorption characteristics were characterized and compared through a saline absorption test. The FAB film with the embossed pattern exhibited a 91.67% faster absorption rate compared to the FAB film without the embossed pattern.

[0054] Comparative Example 2. FAB film without embossing.

[0055] A FAB film was formed without embossing. The sample was dried in a convection oven at 80°C for 4 hours and then tested.

[0056] Example 2. FAB film having embossing.

[0057] A FAB film was formed without embossing. The film was placed on a flat metal plate and then covered with a 12" x 12" metal pattern plate having protruding 1 mm x 1 mm square pins (each having a height of 0.5 mm), with the sides of the pins facing downward toward the FAB film. The plates and the FAB film between them were placed between the plates of a Carver automatic hydraulic compressor. The FAB film was embossed by applying a load of 18,000 lb for 1.5 minutes. Afterward, the FAB film was flipped over and compressed once more with the metal pins under the same pressure and residence time.

[0058] The average main dimension of the pins was in the range of about 100 μm to about 1000 μm. The indentation from each pin was in the range of about 10 μm to about 200 μm.

[0059] The final FAB film had double-sided embossing. The sample was tested after drying it in a convection oven at 80°C for 4 hours.

[0060] Absorption capacity evaluation.

[0061] Equal masses of embossed FAB film samples and unembossed FAB film samples were placed individually in bell glasses. 1 mL of NaCl solution was placed on top of each sample using a pipette. The solution also contained a blue dye to improve visualization during the test. After dropping 1 mL of NaCl solution onto each sample, time was started. The time taken for the samples to absorb the salt solution was monitored, and the absorption behavior was observed. Differences in absorption capacity were qualitatively characterized.

[0062] Figures 4a through 4d illustrate the test process of the two samples to compare their absorption characteristics. Figure 4a shows the start of the test (0 seconds). Once the NaCl solution was dropped onto each film sample, Example 2 showed immediate absorption of the liquid and distributed it in all directions within the film (Figure 4b). This observation indicates a potentially more hydrophilic surface with a lower contact angle compared to Comparative Example 2. This rapid absorption is beneficial for fluid absorption. Starting at 12 seconds, Comparative Example 2 exhibited absorption behavior for the fluid and began distributing the liquid in all directions within the film (Figure 4c). In Figure 4d, at 15 seconds, it can still be seen that in the case of Comparative Example 2, the central absorption zone has a higher fluid volume compared to the surrounding zones. This observation indicates that the fluid distribution in the unembossed FAB film is not as uniform as that in the embossed FAB film. The absorption times are summarized in Table 2.

[0063] Absorption time for FAB film. Sample Inhalation time (seconds) Comparative Example 2 12 Example 2 1

[0064] One possible reason for the improved distribution and relatively high absorption characteristics of Example 2 may be the reduction in surface tension affected by the embossing treatment, which also increases osmotic pressure to improve the absorption behavior of SAM by causing a reduction in the contact angle.

[0065] The described description uses embodiments comprising the best mode to illustrate the invention and enables any person skilled in the art to practice the invention, including manufacturing and using any composition or system and performing any included method. The patentable scope of the invention is defined by the claims and may include other embodiments that occur to those skilled in the art. Such other embodiments are intended to be within the scope of the claims if they have elements that are not different from the literal language of the claims or include structural elements equivalent to those that are not substantially different from the literal language of the claims.

[0066] As used herein, the terms “include,” “include,” “have,” “have,” “contain,” “contain,” “characteristic,” or any other variation thereof are intended to be included non-exclusively, subject to any expressly indicated limitations. For example, a composition, mixture, process, or method comprising a list of elements is not necessarily limited to these elements alone and may include other elements not explicitly listed or not unique to such composition, mixture, process, or method.

[0067] The transition phrase "constituting" excludes any unspecified elements, steps, or components. In a claim, this will generally close the claim to include materials other than those cited, excluding associated impurities. When the phrase "constituting" appears in a provision of the claim body rather than immediately following the preamble, it limits only the elements specified in that provision and does not exclude other elements from the entire claim.

[0068] The transition phrase “essentially constituting” is used to define a composition or method comprising a material, step, feature, component, or element in addition to those literally disclosed, provided that such additional material, step, feature, component, or element does not substantially affect the basic and novel feature(s) of the claimed invention. The term “essentially constituting” occupies an intermediate area between “comprising” and “constituting.”

[0069] Where the present invention or part thereof is defined by open terms such as “comprising,” it should be readily understood that the description should also be interpreted as describing such invention using the terms “essentially comprising” or “constituting” (unless otherwise noted).

[0070] Furthermore, conversely, unless explicitly stated otherwise, "or" refers to inclusive or / and non-exclusive. For example, condition A or B is satisfied by either of the following: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0071] Furthermore, the indefinite article preceding an element or component of the present invention is intended to be non-limiting with respect to the number of instances (i.e., occurrences) of the element or component. Accordingly, the indefinite article should be read to include one or at least one, and the singular word of the element or component also includes the plural form, except where the number is clearly singular.

[0072] As used herein, the term "approximately" means ±10% of the value.

Claims

Claim 1 An absorbent composite comprising a plurality of superabsorbent particles; wherein the plurality of superabsorbent particles are micro-embossed with an average major dimension in the range of 100 μm to 300 μm. Claim 2 In claim 1, the plurality of superabsorbent particles are an absorbent composite in a form selected from the group consisting of glass particles, gel, fiber, bead, solid, paste, SAM sheet, FAB film, and combinations thereof. Claim 3 delete Claim 4 An absorbent composite according to claim 1, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of homogeneous patterns and heterogeneous patterns. Claim 5 An absorbent composite according to claim 1, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of geometric patterns, random patterns, symmetric patterns, asymmetric patterns, spheres, cubes, pyramids, and combinations thereof. Claim 6 A consumer product comprising the absorbent composite of claim 1, wherein the consumer product is selected from the group consisting of personal hygiene products, wet wipes, bibs, wound dressings, napkins, disposable bed liners, food packaging materials, infant and adult diaper products, feminine pads, arm bands, agricultural and pet products containing superabsorbent components, superabsorbent composites including lint, and combinations thereof. Claim 7 A method for manufacturing an absorbent composite, the method comprises: contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins; and embossing the plurality of superabsorbent particles with the embossing roller at a pressure ranging from 125 psi to 1000 psi; wherein the plurality of superabsorbent particles are micro-embossed with an average major dimension ranging from 100 μm to 300 μm. Claim 8 A method according to claim 7, wherein the plurality of superabsorbent particles are in a form selected from the group consisting of glass particles, gels, fibers, beads, solids, pastes, SAM sheets, FAB films, and combinations thereof. Claim 9 delete Claim 10 A method according to claim 7, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of homogeneous patterns and heterogeneous patterns. Claim 11 A method according to claim 7, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of geometric patterns, random patterns, symmetric patterns, asymmetric patterns, spheres, cubes, pyramids, and combinations thereof. Claim 12 In claim 7, a method in which no heat is applied to the embossing step. Claim 13 A consumer product comprising an absorbent composite manufactured according to claim 7, wherein the consumer product is selected from the group consisting of personal hygiene products, wet wipes, bibs, wound dressings, napkins, disposable bed liners, food packaging materials, infant and adult diaper products, female pads, arm bands, agricultural and pet products containing superabsorbent components, superabsorbent composites containing lint, and combinations thereof. Claim 14 A method for manufacturing an absorbent composite, the method comprising: a step of contacting a plurality of superabsorbent particles with an embossing roller comprising a plurality of pins; and a step of transferring the plurality of superabsorbent particles to the embossing roller to directly emboss the plurality of superabsorbent particles with the plurality of pins; wherein the plurality of superabsorbent particles are micro-embossed with an average major dimension in the range of 100 μm to 300 μm. Claim 15 A method according to claim 14, wherein the plurality of superabsorbent particles are in a form selected from the group consisting of glass particles, gels, fibers, beads, solids, pastes, SAM sheets, FAB films, and combinations thereof. Claim 16 delete Claim 17 A method according to claim 14, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of homogeneous patterns and heterogeneous patterns. Claim 18 A method according to claim 14, wherein the plurality of superabsorbent particles are micro-embossed in a pattern selected from the group consisting of geometric patterns, random patterns, symmetric patterns, asymmetric patterns, spheres, cubes, pyramids, and combinations thereof. Claim 19 In claim 14, a method in which no heat is applied to the embossing step. Claim 20 A consumer product comprising an absorbent composite manufactured in accordance with paragraph 14, said consumer product selected from the group consisting of personal hygiene products, wet wipes, bibs, wound dressings, napkins, disposable bed liners, food packaging materials, infant and adult diaper products, female pads, arm bands, agricultural and pet products containing superabsorbent components, superabsorbent composites containing lint, and combinations thereof.

Citation Information

Patent Citations

  • Absorbent sheet and absorbent article using the same

    EP1800638A1

  • Absorbent composite

    US20180243139A1

  • Plasticized superabsorbent polymer sheets and use thereof in hygienic articles

    US7662460B2

  • Method of making an absorbent composite and absorbent articles employing the same

    WO2014145312A2

  • Plasticized superabsorbent polymer sheets and use thereof in hygienic articles

    US20050153123A1