Heat-resistant wrapper paper for aerosol-generating articles
A wrapper paper with high pulp fiber content and specific char-forming agents addresses heat resistance and flame retardancy issues, ensuring safe and biodegradable aerosol-generating articles.
Patent Information
- Application Number
- KR1020237002079
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-01
- Filing Date
- 2021-05-18
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2041-05-18
AI Technical Summary
Existing wrapper papers for aerosol-generating articles lack sufficient heat resistance, mechanical strength, and flame-retardant properties, leading to issues such as tearing during use, fire hazards, and unintentional combustion.
A wrapper paper composition comprising at least 70% pulp fibers and 5-20% char-forming agents, such as ammonium phosphate, with a tensile strength quotient of 0.20 to 0.90 after heat exposure, ensuring high tensile strength and flame retardancy.
The wrapper paper maintains strength and prevents combustion, allowing safe handling and use of aerosol-generating articles without material loss or fire hazards, while being biodegradable and processable.
Smart Images

Figure 112023006641028-PCT00001
Abstract
Description
Technology Field
[0001] The present invention relates to wrapper paper for aerosol-generating articles, which has relatively high heat resistance and sufficient mechanical strength to ensure trouble-free handling of the article even after use, and additionally possesses a flame-retardant effect that prevents the aerosol-generating article produced therefrom from being smoked like a smoking article. This is achieved by a high content of a specific char-forming agent in the wrapper paper. Background Technology
[0002] In the prior art, an aerosol-generating article is known that comprises not only an aerosol-generating material but also paper that wraps the aerosol-generating material and thereby typically forms a cylindrical rod. In this regard, the aerosol-generating material is a material that releases an aerosol upon heating, wherein the aerosol-generating material is heated but not combusted. In many cases, the aerosol-generating article also comprises a filter capable of filtering the components of the aerosol, which is wrapped not only by filter wrapper paper but also by additional wrapper paper connecting the filter and the wrapped rod of the aerosol-generating material.
[0003] During the intended use of an aerosol-generating article, the aerosol-generating material is typically heated but not combusted. This heating may be performed, for example, by an external device into which the aerosol-generating article is inserted, or by a heat source attached to one end of the aerosol-generating article that is activated by ignition for the use of the article. During the heating of the aerosol-generating material, the wrapper paper is also heated and thermally decomposed. As a result, the wrapper paper may lose enough strength to tear during the removal of the aerosol-generating article from the heating device. This requires the consumer to go through the trouble of cleaning, which is therefore undesirable. Additionally, even in the case of an aerosol-generating article with an integrated heat source, the wrapper paper may lose its strength during heating, causing the heat source to detach and creating a fire hazard.
[0004] Furthermore, it is desirable to prevent the aerosol-generating article from being unintentionally used by consumers in the same way as a cigarette and an attempt to ignite the end of the aerosol-generating article, thereby initiating the combustion or smoldering process of the aerosol-generating material. Therefore, the wrapper paper of the aerosol-generating article is required to have flame-retardant properties.
[0005] Research to make wrapper paper for these aerosol-generating articles heat-resistant or flame-retardant has been only partially successful.
[0006] WO 2015 / 082648 describes, for example, wrapper paper composed of relatively small pulp fibers and coated with a composition of calcium carbonate and a binder such that at least 50% of the wrapper paper consists of calcium carbonate. The disadvantages of such wrapper paper are that, due to the thick coating, it is relatively brittle and generates a large amount of dust during the manufacture of aerosol-generating articles from the wrapper paper. Furthermore, due to the low fiber content, the tensile strength is not particularly high.
[0007] WO 2011 / 117750 describes a wrapper paper made of a laminate of aluminum foil and paper. The aluminum foil faces the aerosol-generating material, which partially protects the paper from the effects of heat. The disadvantages of this wrapper paper are the complex manufacturing process and low biodegradability, as experience shows that after use, many aerosol-generating materials are discarded directly into the environment.
[0008] Therefore, there is interest in making available wrapper paper that retains sufficient tensile strength even after heating, possesses flame-retardant properties, and is nevertheless biodegradable. Furthermore, the design of wrapper paper for aerosol-generating articles must consider, in particular, legal regulations, toxicology, and the impact of the wrapper paper on the taste of the aerosol-generating articles.
[0009] The object of the present invention is to provide a wrapper paper for aerosol-generating articles that is essentially heat-resistant or flame-retardant and has advantageous properties with respect to strength, processability, biodegradability, and taste.
[0010] In relation to the present invention, the aerosol-generating article is a rod-shaped article comprising an aerosol-generating material and a wrapper paper wrapping the aerosol-generating material, wherein, during intended use, the aerosol-generating material is heated but not combusted. In the case of a typical aerosol-generating material, e.g., tobacco, in either case, heating without combustion will occur when the aerosol-generating material is heated to a temperature of up to 400°C.
[0011] The above objective is achieved by a wrapper paper for an aerosol-generating article according to claim 1, an aerosol-generating article comprising said wrapper paper according to claim 24, a use of said wrapper paper for an aerosol-generating article according to claim 26, and a method for manufacturing a wrapper paper according to the present invention according to claim 27. Further advantageous embodiments are provided in the dependent claims.
[0012] The inventors have provided a wrapper paper suitable for use in an aerosol-generating article comprising pulp fibers and a char-forming agent, wherein the pulp fibers constitute at least 70% and up to 95% of the mass of the wrapper paper, the char-forming agent is contained at a concentration of at least 5% and up to 20% of the mass of the wrapper paper, and the tensile strength R0 measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 and the tensile strength R measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 after the wrapper paper is exposed to a temperature of 230°C for 1 minute. T The quotient r=R T It was discovered that this can be achieved by a wrapper paper containing / R0 at a concentration of at least 0.20 and at most 0.90.
[0013] According to the findings of the inventors, a high pulp fiber content is required to obtain high initial strength in wrapper paper. It is known that many char-forming agents potentially used in paper damage the pulp fibers of the paper, causing a rapid and significant loss of strength upon heating. However, they also protect the pulp fibers additionally present within the paper structure from thermal decomposition. Since paper is generally easily combustible, it is a common belief that char-forming agents need to be used in paper at very high concentrations for an effective flame-retardant effect. However, according to the common belief and also the experiments of the inventors, at such concentrations, the pulp fibers are severely damaged and the strength is significantly reduced, so their use cannot be considered reasonable.
[0014] In contrast, the inventors have discovered that for some char-forming agents, excellent flame-retardant effects are exhibited and there actually exists a suitable narrow concentration range in which the reduction in paper strength is not too great.
[0015] Only a combination of high pulp fiber content and a suitably selected concentration of char-forming agent enables the production of wrapper paper having high tensile strength even after heating, such that, due to its high initial strength, the aerosol-generating article made from wrapper paper can be removed from the heating device without any problems despite the loss of strength caused by the char-forming agent, or there is no risk of the heat source integrated into the aerosol-generating article falling off. Furthermore, the flame-retardant effect is sufficient to prevent the aerosol-generating article from being smoked like a cigarette.
[0016] Additionally, the components of the wrapper paper enable excellent biodegradability and very good processability during the manufacture of aerosol-generating articles.
[0017] Wrapper paper requires pulp fibers for its strength, where the pulp fibers constitute at least 70% and up to 95% of the mass of the wrapper paper. To obtain a much more favorable ratio between the pulp fibers and the char-forming agent, the proportion of pulp fibers can be, respectively, at least 75% and up to 90% with respect to the mass of the wrapper paper, preferably at least 80% and up to 90%.
[0018] The pulp fibers are preferably obtained from one or more plants selected from the group consisting of conifers, deciduous trees, spruce, pine, fir, beech, birch, eucalyptus, flax, hemp, jute, ramie, abaca, sisal, hemp, and cotton. The pulp fibers may also consist wholly or partially of fibers derived from regenerated cellulose, such as Tencel™ fibers, Lyocell™ fibers, viscose fibers, or Modal™ fibers.
[0019] Preferably, the pulp fibers consist of softwood-derived pulp fibers in a ratio of at least 40% and up to 100% of the mass of the pulp fibers, because these pulp fibers provide high strength to the wrapper paper.
[0020] Wrapper paper contains a char-forming agent, wherein the char-forming agent constitutes at least 5% and up to 20% of the mass of the wrapper paper. According to the inventors' findings, while the char-forming agent protects the pulp fibers present within the paper structure from excessive oxidation, it also damages the pulp fibers themselves; therefore, the concentration of the char-forming agent must be within a narrow range and depends on the type of char-forming agent. As the concentration of the char-forming agent increases, the flame-retardant effect becomes stronger, but the strength of the wrapper paper after heating decreases due to increased damage to the pulp fibers. Accordingly, preferably, the proportion of the char-forming agent in the wrapper paper is at least 9% and up to 16% of the mass of the wrapper paper.
[0021] The char-forming agent is preferably ammonium phosphate, particularly preferably monoammonium phosphate, diammonium phosphate, triammonium phosphate, or ammonium polyphosphate or a mixture thereof. Less preferably, the char-forming agent is guanyle urea phosphate, guanidine phosphate, phosphoric acid, phosphonate, melamine phosphate, dicyandiamide, boric acid, or borax. These less preferred compounds are more difficult to process or are not entirely free of toxicological problems. Sodium polyphosphate is also a char-forming agent, but is not according to the present invention.
[0022] The selection of the concentration of the char-forming agent is not free within the provided range but depends on the type of char-forming agent, and must be selected so that the reduction in the strength of the wrapper paper after heating is not too significant.
[0023] For this purpose, the tensile strength in the machine direction of the wrapper paper is determined as a characteristic strength feature, first under the conditions of ISO 187:1990 and then after heating the wrapper paper. More precisely, the loss of strength can be determined according to the following method.
[0024] First, a paper sample of suitable geometry, typically a strip 15 mm wide, is conditioned according to ISO 187:1990 and tested in a tensile test according to ISO 1924-2:2008. Tensile strength depends on the direction in which the paper sample is taken. Here, it should always be understood that tensile strength is the tensile strength in the direction of travel of the wrapper paper during paper manufacturing, which is called the so-called machine direction.
[0025] According to the present invention, the initial tensile strength denoted by R0 is determined by conditioning a paper sample according to ISO 187:1990 without a preceding heat load and testing according to ISO 1924-2:2008. The tensile strength after a heat load, i.e., R Tis determined by exposing the sample to a temperature of 230°C in air for 1 minute, where air can reach virtually all sides of the paper sample and minimal airflow is present. Subsequently, the paper sample is conditioned according to ISO 187:1990, and the tensile strength is determined likewise according to ISO 1924-2:2008. Quotient r = R T / R0 describes the ratio of the tensile strength maintained after a thermal load of the wrapper paper, and thus characterizes the heat resistance of the wrapper paper. A larger value of the quotient r indicates high heat resistance. According to the present invention, the concentration of the char-forming agent in the wrapper paper [indicates] the tensile strength R after a thermal load (230°C for 1 minute). T and the quotient r of the initial tensile strength R0 should be selected to be at least 0.20 and at most 0.90, particularly preferably at least 0.25 and at most 0.80. This means that the tensile strength is not reduced by more than 80%.
[0026] The above quotient may be influenced by the amount of pulp fibers and the type and concentration of the char-forming agent, where a higher amount of pulp fibers results in a higher initial tensile strength R0, and generally, as the concentration of the char-forming agent increases, the tensile strength R after thermal loading T A decrease in tensile strength R is caused. T The negative effects of the char-forming agent on this should be offset by a superior flame-retardant effect at increasing concentrations depending on the type of application of the aerosol-generating article. It has been found that a very advantageous trade-off can be identified in the aerosol-generating article within the range and preferred range of the concentration of the char-forming agent according to the present invention.
[0027] Preferably, the tensile strength R after thermal loading is such that the aerosol-generating article can be handled without problems during and after use. TIt must not fall below a specific value. Preferably, the tensile strength R of the wrapper paper in the machine direction after heat loading. T It is at least 8 N / 15 mm and up to 50 N / 15 mm, particularly preferably at least 10 N / 15 mm and up to 40 N / 15 mm.
[0028] According to the inventors' findings, it is important to know how the char-forming agent is distributed across the thickness of the wrapper paper. Generally, excellent flame-retardant effects can actually be achieved when the char-forming agent is essentially homogeneously distributed in the wrapper paper. However, in a preferred embodiment, the wrapper paper is designed to contain a higher proportion of the char-forming agent on the side of the wrapper paper facing the aerosol-generating material than on the other side of the wrapper paper. The side facing the aerosol-generating material is typically exposed to a higher heat load. Therefore, the higher the content of the char-forming agent on this side of the wrapper paper, the more significantly it can contribute to the flame-retardant effect. In this way, the proportion of the char-forming agent in the wrapper paper can be reduced without loss of flame-retardant effect, and consequently, the proportion of pulp fibers in the wrapper paper can be increased at the same basis weight, resulting in an overall increase in the strength of the wrapper paper. Alternatively, with this desirable distribution of char-forming agents within the wrapper paper, the basis weight can also be reduced without loss associated with the flame-retardant effect, which reduces material requirements.
[0029] As described below, the distribution of the char-forming agent within the wrapper paper can be affected by the manufacturing process.
[0030] Preferably, the char-forming agent is essentially uniformly distributed over at least 70% of the surface area of the wrapper paper, particularly preferably over at least 95% of the surface area, wherein variations in the proportion of the char-forming agent within these surface areas are caused only by the manufacturing method and are not intended.
[0031] A disadvantage of the char-forming agent may be that it discolors the wrapper paper under a heat load, causing it to darken. This disadvantage can be overcome by combining the wrapper paper according to the present invention with an additional paper layer, for example by adhesion, such that the wrapper paper according to the present invention faces the aerosol-generating material and the additional paper layer is located on the opposite side of the aerosol-generating material. This additional paper layer covers the wrapper paper so that there is no external color change or only a slight color change under a heat load.
[0032] Accordingly, preferably, the wrapper paper is combined with a paper layer. Particularly preferably, this paper layer comprises pulp fibers and calcium carbonate particles, wherein the calcium carbonate particles constitute at least 15% and up to 40% of the mass of the paper layer. The calcium carbonate particles provide the paper layer with a white color and high opacity, so that discoloration of the wrapper paper according to the present invention located underneath is not visible or is only slightly visible. It should be noted that the wrapper paper having an additional paper layer may also be described as a “two-layer wrapper paper” as a whole, but this designation is avoided here. Instead, this two-layer structure is referred to as “wrapper paper having an additional paper layer” in the expression of this disclosure, because only a portion of the two-layer structure called “wrapper paper” needs to satisfy the above requirements regarding the pulp fibers, char-forming agent, and tensile strength.
[0033] In addition to pulp fibers and char-forming agents, the wrapper paper according to the present invention may contain additional components. These include, for example, filler materials, sizing agents, wet strength enhancers, additives, processing aids, humectants, and flavoring agents. A person skilled in the art can select these components based on experience. In particular, since the aerosol formed during the use of the aerosol-generating article has a high moisture content, it may be useful to apply a wet strength enhancer to the aerosol-generating article. Wrapper paper can absorb water from the aerosol, and as a result, its strength is reduced. This can be prevented by the use of a wet strength enhancer.
[0034] In wrapper paper, filler material can contribute to reduced discoloration of the wrapper paper. However, since filler material also reduces the tensile strength of the wrapper paper, its proportion should not be too high. Therefore, preferably, the proportion of filler material in the wrapper paper is at least 0% and at most 20%, particularly preferably at least 0% and at most 10%, with respect to the mass of the wrapper paper, and particularly at least 0% and at most 5%.
[0035] The filler material is selected from the group consisting of calcium carbonate, magnesium carbonate, titanium dioxide, magnesium oxide, magnesium hydroxide, aluminum hydroxide, kaolin, talc, and mixtures thereof. Less preferably, the filler material is a carbonate.
[0036] In a preferred embodiment, the wrapper paper additionally contains starch or a starch derivative, or is coated with starch or a starch derivative. In this preferred embodiment, the proportion of starch or a starch derivative is at least 2% and up to 10% of the mass of the wrapper paper. This preferred embodiment provides resistance to oil penetration as an additional advantage. The aerosol-generating material may contain oil, for example, a flavoring agent, which penetrates the wrapper paper during storage or use of the aerosol-generating article and causes staining. Resistance to oil penetration can be determined according to TAPPI T559 cm-12 and is given as a KIT level. In this preferred embodiment, the KIT level is at least 4 and up to 8.
[0037] The basis weight of wrapper paper can vary, where a larger basis weight generally implies higher tensile strength. However, wrapper paper with a larger basis weight has greater stiffness, becomes more difficult to process, and requires more material. Therefore, preferably, the basis weight of the wrapper paper according to the present invention is at least 15 g / m² 2 and up to 80 g / m² 2 , particularly preferably at least 20 g / m² 2 and up to 60 g / m² 2 The basis weight of the wrapper paper can be determined according to ISO 536:2019.
[0038] The thickness of the wrapper paper primarily affects bending stiffness and heat transfer within the wrapper paper. High bending stiffness is advantageous because it causes the aerosol-generating article manufactured from the wrapper paper to deform less; however, on the other hand, high bending stiffness can cause problems due to resilience when attempting to wrap the aerosol-generating material with the wrapper paper. Large thickness delays heat transfer through the wrapper paper, which is also advantageous for this reason. Preferably, the thickness of the wrapper paper according to the present invention is at least 25 μm and up to 100 μm, particularly preferably at least 40 μm and up to 80 μm. The thickness can be determined according to ISO 534:2011 for a single layer.
[0039] The initial tensile strength R0 of the wrapper paper, measured in the machine direction, is preferably at least 10 N / 15 mm and up to 100 N / 15 mm, particularly preferably at least 20 N / 15 mm and up to 80 N / 15 mm. High tensile strength can be achieved by a high proportion of pulp fibers. However, since this also implies higher material requirements, it is not reasonable to desire particularly high tensile strength for this reason. The preferred range enables a particularly favorable combination of problem-free processability and material requirements. Tensile strength can be determined according to ISO 1924-2:2008.
[0040] Since aerosol-generating materials often contain desiccant, the aerosol generated during heating has a relatively high moisture content. Since this moisture can reduce the strength of the wrapper paper, it is advantageous for the wrapper paper to also have a suitable wetting strength for this reason. Accordingly, the wetting strength in the machine direction is preferably at least 1 N / 15 mm and up to 10 N / 15 mm, particularly preferably at least 2 N / 15 mm and up to 8 N / 15 mm. The wetting strength can be determined according to ISO 12625-5:2016.
[0041] The air permeability of wrapper paper can be low. Low air permeability can often be achieved by more intensively refining the pulp fibers. Since this also contributes to an increase in strength, preferably, the air permeability is at least 0 cm⁻¹. 3 / (cm 2 ·min·kPa) and up to 50 cm 3 / (cm 2 ·min·kPa), particularly preferably at least 0 cm 3 / (cm 2 ·min·kPa) and up to 20 cm 3 / (cm 2 It is ·min·kPa). Air permeability can be measured according to ISO 2965:2019.
[0042] If the wrapper paper according to the present invention is visible from the outside of an aerosol-generating article, optical properties may be important. Generally, high opacity and high brightness are desirable. Both of these properties may be substantially influenced by the type and amount of filler material within the wrapper paper. Preferably, the opacity is at least 40% and up to 90%, particularly preferably at least 45% and up to 80%. Preferably, the brightness is at least 80% and up to 95%, particularly preferably at least 83% and up to 90%.
[0043] An aerosol-generating article can be manufactured from the wrapper paper according to the present invention in accordance with a method known in the prior art. Accordingly, the aerosol-generating article according to the present invention comprises an aerosol-generating material and a wrapper paper according to any one of the embodiments mentioned above, wherein the wrapper paper encloses the aerosol-generating material.
[0044] In a preferred embodiment of the aerosol-generating article, the proportion of the char-forming agent is higher on one side of the wrapper paper than on the other, and the side having the higher proportion of the char-forming agent faces the aerosol-generating material.
[0045] Since the wrapper paper according to the present invention can be advantageously used in aerosol-generating articles, for this reason, the use of the wrapper paper according to the present invention in aerosol-generating articles is also an object of the present invention.
[0046] The wrapper paper according to the present invention comprises steps A to G:
[0047] A - Step of suspending pulp fibers in an aqueous suspension,
[0048] B - Step of refining suspended pulp fibers in a refining unit,
[0049] C - Step of applying the suspension to the running wire,
[0050] D - Step of forming a fiber web by dehydrating the suspension,
[0051] E - Step of pressing the fiber web,
[0052] F - Step of drying the fiber web,
[0053] G - The step of winding the wrapper paper, here
[0054] Between steps F and G, at least one composition containing a char-forming agent is applied to a fiber web, and the fiber web is dried to form a wrapper paper, wherein the wrapper paper from step G comprises pulp fibers and a char-forming agent, the pulp fibers constitute at least 70% and up to 95% of the mass of the wrapper paper, and the char-forming agent constitutes at least 5% and up to 20% of the mass of the wrapper paper, wherein the char-forming agent has a tensile strength R0 measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 and a tensile strength R measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 after the wrapper paper is exposed to a temperature of 230°C for 1 minute. T The quotient r = R TIt is contained in wrapper paper at a concentration where / R0 is at least 0.20 and at most 0.90.
[0055] Preferably, the step of applying a composition containing a char-forming agent to a fiber web is performed by one of the following steps or a combination of two or more of them:
[0056] F.1 Step of applying a composition containing a char-forming agent to a fiber web in a size press of a paper machine,
[0057] F.2 A step of applying a composition containing a char-forming agent to a fiber web in a film press or coating unit of a paper machine, and
[0058] F.3 Step of applying a composition containing a char-forming agent to a fiber web by printing, particularly roto-gravure printing, or spraying.
[0059] In this regard, step F.1 is performed in a size press, thereby impregnating the fiber web with a composition containing a char-forming agent. This modification offers the advantage that it can be easily performed. Since this generally ensures that the char-forming agent is distributed substantially homogeneously over the thickness of the wrapper paper, a relatively larger amount of char-forming agent is required to achieve the desired effect. However, in practice, it is also possible to adjust the settings of the size press so that the char-forming agent is distributed non-uniformly over the fiber web and, ultimately, the thickness of the wrapper paper at this stage.
[0060] According to step F.2, a composition containing a char-forming agent is applied to one side of a fiber web in a film press or a coating unit. This results in an uneven distribution of the char-forming agent across the thickness of the wrapper paper, and a high flame retardant effect can be obtained with a smaller proportion of the char-forming agent in the wrapper paper.
[0061] According to step F.3, a composition containing a char-forming agent is applied to one side of a fiber web by printing or spraying, wherein, in a particularly preferred embodiment, the composition is printed on one side of the fiber web by a roto-gravure printing unit. In this regard, the fiber web is preferably dried, wound, and unwound before step F.3. The fiber web in the wound state can then be transferred to an additional device where the application of the composition can be performed by printing or spraying. While steps F.1 and F.2 can generally be performed on the same paper machine where the wrapper paper is manufactured, the application according to step F.3 is typically performed in a separate device.
[0062] In a very particularly preferred embodiment, steps F.1 and F.3 are combined such that, first in step F.1, a fiber web is impregnated with a composition containing a char-forming agent in a size press, and in step F.3, an additional composition containing a char-forming agent is printed on one side of the fiber web in a roto-gravure printing unit. In this very particularly preferred embodiment, both char-forming agents are distributed in the wrapper paper and are present at a higher concentration on one side of the wrapper paper, so that the flame-retardant effect can be further significantly increased.
[0063] In an additional very particularly preferred embodiment, steps F.1 and F.2 are combined, wherein step F.1 is performed in a size press and step F.2 is performed in a coating unit. In this very particularly preferred embodiment, wrapper paper can be manufactured particularly efficiently, for example, because all application devices can be integrated into a single paper machine.
[0064] Regardless of which step F.1, F.2, or F.3 is used, the composition containing the char-forming agent is preferably applied to at least 70% of the surface area of the wrapper paper, and particularly preferably to at least 95% of the surface area of the wrapper paper.
[0065] The composition used in step F.1, F.2, or F.3 contains a char-forming agent and a solvent, wherein the solvent is preferably water. The amount of the char-forming agent in the composition may vary and depends on the type of application process, the amount applied, and the desired amount of the char-forming agent in the wrapper paper. A person skilled in the art would be able to determine a suitable composition and design the application process accordingly by taking these factors into account.
[0066] In a very particularly preferred embodiment, one of steps F.1 and F.2 is performed, and then the fiber web is dried, wound, and unwound again, and then step F.3 is performed, wherein the fiber web in the dried and wound state prior to step F.3 preferably contains a char-forming agent in an amount of at least 5% and up to 10% of the mass of the fiber web in the dried and wound state.
[0067] If steps F.1, F.2 and / or F.3 are combined in any form, the composition containing the char-forming agent applied in steps F.1, F.2 and / or F.3 may differ.
[0068] In the wrapper paper after step G, the pulp fibers constitute at least 70% and up to 95% of the mass of the wrapper paper. To obtain a much more favorable ratio between the pulp fibers and the char-forming agent, the proportion of the pulp fibers can be, with respect to the mass of the wrapper paper after step G, preferably at least 75% and up to 90%, particularly preferably at least 80% and up to 90%.
[0069] The pulp fibers in step A are preferably obtained from one or more plants selected from the group consisting of conifers, deciduous trees, spruce, pine, fir, beech, birch, eucalyptus, flax, hemp, jute, ramie, abaca, sisal, hemp, and cotton. The pulp fibers may also consist of fibers produced wholly or partially from regenerated cellulose, such as Tencel™ fibers, Lyocell™ fibers, viscose fibers, or Modal™ fibers.
[0070] Preferably, the pulp fibers in step A consist of pulp fibers derived from conifers in a ratio of at least 40% and up to 100% of the mass of the pulp fibers, because these pulp fibers provide high initial strength to the wrapper paper in step G.
[0071] The wrapper paper after step G contains a char-forming agent, wherein the char-forming agent constitutes at least 5% and up to 20% of the mass of the wrapper paper. Preferably, the proportion of the char-forming agent in the wrapper paper after step G is at least 9% and up to 16% of the mass of the wrapper paper.
[0072] The char-forming agent is preferably ammonium phosphate, particularly preferably monoammonium phosphate, diammonium phosphate, triammonium phosphate, or ammonium polyphosphate or a mixture thereof. Less preferably, the char-forming agent is guanyle urea phosphate, guanidine phosphate, phosphoric acid, phosphonate, melamine phosphate, dicyandiamide, boric acid, or borax. These less preferred compounds are more difficult to process or are not entirely free of toxicological problems. Sodium polyphosphate is also a char-forming agent, but is not according to the present invention.
[0073] In a preferred embodiment, the wrapper paper after step G is a wrapper paper according to any one of the embodiments mentioned above. Specific details for implementing the invention
[0074] Some preferred embodiments of the wrapper paper according to the present invention will now be described.
[0075] Wrapper paper P1 according to the present invention was manufactured on a long-mesh paper machine. To this end, pulp fibers were suspended in water (Step A) and refined in a refining unit (Step B). Subsequently, the suspension was applied to a running wire (Step C) and dehydrated thereon to form a fiber web (Step D). The fiber web was pressed (Step E) to further dehydrate it and dried by contact with a heated drying cylinder (Step F). In the size press of the paper machine, the fiber web was impregnated with a composition containing water and monoammonium phosphate over the entire surface of both sides (Step F.1), and the fiber web was subsequently dried by contact with a heated drying cylinder. Finally, the fiber web was wound (Step G) to obtain wrapper paper P1 according to the present invention.
[0076] The amount of pulp fiber was selected such that approximately 87% of the mass contained in wrapper paper P1 is pulp fiber. The composition in step F.1 included water and monoammonium phosphate, and with the setting of the size press, the amount of monoammonium phosphate in the wrapper paper after step G was selected such that it is approximately 7%. The distribution of monoammonium phosphate in wrapper paper P1 can be assumed to be essentially homogeneous over the thickness.
[0077] Wrapper paper P2 according to the present invention was prepared from wrapper paper P1 according to the present invention by unwinding the reel of wrapper paper P1 and printing over the entire surface of one side of the wrapper paper in a roto-gravure printing unit with a composition comprising water and monoammonium phosphate (step F.3). Subsequently, the wrapper paper was dried by hot air drying and re-rolled (step G). The composition in step F.3 was selected, along with the settings of the roto-gravure printing unit and, in particular, the geometry of the printing cylinder, such that the total mass of the wrapper paper in the final wrapper paper P2 consists of monoammonium phosphate. In this way, a heterogeneous distribution of monoammonium phosphate was obtained in the wrapper paper such that the content of monoammonium phosphate on the printed side is higher than on the other side.
[0078] In wrapper paper P2, 82% of the mass consists of pulp fibers.
[0079] Wrapper paper Z1, which does not conform to the present invention and contains 70% pulp fibers and 29% precipitated calcium carbonate but does not contain a char-forming agent, was used as a comparative example.
[0080] Additionally, 90% pulp fibers and 10% sodium polyphosphate (NaPO3) as a char-forming agent n Wrapper paper Z2, which does not follow the present invention and includes [the following], was used as a comparative example.
[0081] To obtain additional wrapper paper P3, a wrapper paper Z1 not according to the present invention was bonded to a wrapper paper P2 according to the present invention in such a way that the side of the wrapper paper P2 having a higher content of monoammonium phosphate faced opposite to the wrapper paper Z1, thereby forming a two-layer structure.
[0082] Data for wrapper papers P1 and P2, a two-layer structure P3 according to the present invention, and comparative examples Z1 and Z2 not according to the present invention were determined according to conventional standard methods.
[0083] Tensile strength R after heat load T To determine the results, wrapper papers P1, P2, P3 and Z1, Z2 were placed in a drying oven heated to 230°C for 1 minute. Subsequently, they were conditioned according to ISO 187:1990 and their tensile strength was measured according to ISO 1924-2:2008.
[0084] Initial tensile strength R0 and tensile strength R after thermal loading T From, quotient r = R T Heat resistance was characterized by determining / R0.
[0085] All data for wrapper papers P1, P2, P3 and Z1, Z2 can be found in Table 1.
[0086] Table 1
[0087]
[0088] Table 1 shows that in the case of wrapper papers P1 and P2 according to the present invention, as well as a two-layer structure P3 containing wrapper paper P2 according to the present invention, a heat load reduces the tensile strength by 34% to 55%. In the case of Comparative Example Z1 not according to the present invention, which does not contain a char-forming agent, the tensile strength is hardly reduced by the heat load and remains about 94% of the initial tensile strength. In the case of Comparative Example Z2 not according to the present invention, which contains sodium polyphosphate as a char-forming agent, the tensile strength after the heat load is only about 19% of the initial tensile strength, and the absolute value of 6.3 N / 15 mm is too low to remove the aerosol-generating article produced therefrom from the heating device without issue after use.
[0089] Wrapper papers P1 and P2 and the two-layer structure P3 according to the present invention all exhibit an acceptable reduction in tensile strength. However, in a comparison of wrapper papers P1 and P2 according to the present invention, it can be seen that the higher content of monoammonium phosphate in wrapper paper P2 damages the fibers more and causes a more severe reduction in tensile strength after heat loading.
[0090] In addition to not reducing tensile strength too significantly, flame-retardant properties are also important. To test flame-retardant properties, aerosol-generating articles intended for use in a heating device were prepared from wrapper papers P1 / P2 according to the present invention, a two-layer structure P3, and comparative examples Z1 and Z2 not according to the present invention. For all wrapper papers, there were no problems with the preparation of the aerosol-generating articles. When an attempt was made to ignite an aerosol-generating article, such as a cigarette, with a lighter, it was immediately apparent that comparative example Z1 not according to the present invention did not have flame-retardant properties. The aerosol-generating article prepared therefrom could be ignited without problems. Even when the lighter flame acted for a longer period, the aerosol-generating articles having wrapper papers P1 / P2 according to the present invention, a two-layer structure P3, and comparative example Z2 not according to the present invention could not be ignited in a manner that would initiate combustion or a stable smoldering process. Furthermore, these aerosol-generating articles could not be smoked according to a standardized process. Regarding the flame retardant effect, wrapper paper P2 according to the present invention was proven to be slightly superior to P1, which indicates that the non-uniform distribution of the char-forming agent across the thickness of the wrapper paper can contribute to an increase in the flame retardant effect.
[0091] The two-layer structure P3 is a laminate of wrapper paper P2 according to the present invention and comparative example Z1 not according to the present invention, and after use of an aerosol-generating article made therefrom, it exhibited significantly weaker discoloration than an aerosol-generating article having P1 and P2. Thus, wrapper paper Z1 performed its function of masking the discoloration of wrapper paper P2.
[0092] The effect of aerosol-generating products on taste could not be confirmed.
[0093] Accordingly, the wrapper paper according to the present invention is highly suitable for use in aerosol-generating articles and, along with excellent biological degradability, has strength and flame retardant effects after heating in a combination superior to comparable wrapper papers of the prior art.
Claims
Claim 1 An aerosol-generating article comprising wrapper paper and an aerosol-generating material, wherein the aerosol-generating article is heated but not combusted upon its intended use, wherein the wrapper paper wraps the aerosol-generating material and comprises pulp fibers and a char-forming agent, wherein the pulp fibers constitute at least 70% and up to 95% of the mass of the wrapper paper, and the char-forming agent is contained at a concentration of at least 5% and up to 20% of the mass of the wrapper paper, and a tensile strength R0 measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 and a tensile strength R measured according to ISO 1924-2:2008 under the conditions of ISO 187:1990 after the wrapper paper is exposed to a temperature of 230°C for 1 minute T The quotient r = R T Aerosol-generating article that is present in wrapper paper at a concentration where / R0 is at least 0.20 and at most 0.
90. Claim 2 An aerosol-generating article according to claim 1, wherein the proportion of pulp fibers in the wrapper paper is, respectively, at least 75% and up to 90% or at least 80% and up to 90% with respect to the mass of the wrapper paper. Claim 3 An aerosol-generating article according to claim 1 or 2, wherein the pulp fiber is obtained wholly or partially from one or more plants selected from the group consisting of conifers, deciduous trees, spruce, pine, fir, beech, birch, eucalyptus, flax, hemp, jute, ramie, abaca, sisal, hemp, and cotton. Claim 4 An aerosol-generating article according to claim 1 or 2, wherein the pulp fibers consist wholly or partially of fibers derived from regenerated cellulose. Claim 5 An aerosol-generating article according to claim 1 or 2, wherein the pulp fibers are obtained from coniferous trees in a ratio of at least 40% and up to 100% of the mass of the pulp fibers. Claim 6 An aerosol-generating article according to claim 1 or 2, wherein the proportion of the char-forming agent in the wrapper paper constitutes at least 9% and at most 16% of the mass of the wrapper paper. Claim 7 An aerosol-generating article according to claim 1 or 2, wherein the char-forming agent is monoammonium phosphate, diammonium phosphate, triammonium phosphate, ammonium polyphosphate or a mixture thereof, or wherein the char-forming agent is composed at least partially of guanyle urea phosphate, guanidine phosphate, phosphoric acid, phosphonate, melamine phosphate, dicyandiamide, boric acid, or borax. Claim 8 In claim 1 or 2, the tensile strength R of the wrapper paper after the wrapper paper is exposed to a temperature of 230°C for 1 minute. T Aerosol-generating article having at least 8 N / 15 mm and up to 50 N / 15 mm or at least 10 N / 15 mm and up to 40 N / 15 mm. Claim 9 An aerosol-generating article according to claim 1 or 2, wherein the side of the wrapper paper facing the aerosol-generating material during intended use contains a higher proportion of a char-forming agent than the other side of the wrapper paper. Claim 10 An aerosol-generating article according to claim 1 or 2, wherein the char-forming agent is distributed at least substantially uniformly over at least 70% or at least 90% of the surface area of the wrapper paper. Claim 11 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper is combined with an additional paper layer such that, during intended use, the wrapper paper according to the invention faces the aerosol-generating material and the additional paper layer is located on the opposite side of the aerosol-generating material. Claim 12 An aerosol-generating article according to paragraph 11, wherein an additional paper layer comprises pulp fibers and calcium carbonate particles, wherein the calcium carbonate particles constitute at least 15% and up to 40% of the mass of the additional paper layer. Claim 13 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper further comprises at least one additional component selected from the group consisting of filler material, sizing agent, wet strength enhancer, additive, processing aid, humectant and flavoring agent. Claim 14 An aerosol-generating article according to paragraph 13, wherein the proportion of the filler material is, respectively, at least 0% and up to 20%, at least 0% and up to 10%, or at least 0% and up to 5% with respect to the mass of the wrapper paper. Claim 15 An aerosol-generating article in paragraph 13, wherein the filler material is selected from the group consisting of calcium carbonate, magnesium carbonate, titanium dioxide, magnesium oxide, magnesium hydroxide, aluminum hydroxide, kaolin, talc, and mixtures thereof. Claim 16 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper contains starch or a starch derivative or is coated with starch or a starch derivative, wherein the proportion of starch or a starch derivative is at least 2% and at most 10% of the mass of the wrapper paper. Claim 17 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper has a KIT level of at least 4 and at most 8 as determined according to TAPPI T559 cm-12. Claim 18 In claim 1 or 2, the wrapper paper is at least 15 g / m² 2 and up to 80 g / m² 2 or at least 20 g / m² 2 and up to 60 g / m² 2 Aerosol-generating article having a basis weight of Claim 19 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper has a thickness of at least 25 μm and up to 100 μm or at least 40 μm and up to 80 μm. Claim 20 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper has a tensile strength R0 before heat loading, measured in the machine direction, of at least 10 N / 15 mm and up to 100 N / 15 mm or at least 20 N / 15 mm and up to 80 N / 15 mm. Claim 21 An aerosol-generating article according to claim 1 or 2, wherein the wetting strength in the machine direction according to ISO 12625-5:2016 is at least 1 N / 15 mm and at most 10 N / 15 mm or at least 2 N / 15 mm and at most 8 N / 15 mm. Claim 22 In claim 1 or 2, the wrapper paper is at least 0 cm 3 / (cm 2 ·min·kPa) and up to 50 cm 3 / (cm 2 ·min·kPa) or at least 0 cm 3 / (cm 2 ·min·kPa) and up to 20 cm 3 / (cm 2 Aerosol-generating article having an air permeability of ·min·kPa). Claim 23 An aerosol-generating article according to claim 1 or 2, wherein the wrapper paper has an opacity of at least 40% and up to 80% or at least 45% and up to 80%, or a lightness of at least 80% and up to 95% or at least 83% and up to 90%. Claim 24 An aerosol-generating article according to claim 1 or 2, wherein the ratio of the char-forming agent is higher on one side of the wrapper paper than on the other side, and the side having the higher ratio of the char-forming agent faces the aerosol-generating material. Claim 25 delete Claim 26 delete Claim 27 delete Claim 28 delete Claim 29 delete Claim 30 delete Claim 31 delete Claim 32 delete Claim 33 delete Claim 34 delete Claim 35 delete Claim 36 delete Claim 37 delete Claim 38 delete Claim 39 delete
Citation Information
Patent Citations
Cigarette paper containing carbon fibers for improved ash charactaristics
EP1084629A1
Smoking article exhibiting reduced sidestream smoke, and wrapper paper therefor
US4998543A
Low-ignition-tendency cigarette paper
CN108589420A