Method for manufacturing secondary battery

The method addresses resistance and rigidity issues in secondary batteries by using a separator with minimal binder and a gel polymer electrolyte, ensuring reduced resistance and improved mechanical durability through a curing process.

KR103045116B1Active Publication Date: 2026-11-06LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020220006031
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-14
Publication Date
2026-11-06
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Existing secondary batteries face issues with increased resistance due to excessive binder use in ceramic coating layers, leading to decreased energy density and cell rigidity, while liquid electrolytes pose leakage and safety concerns, and gel polymer electrolytes have high interfacial resistance and low ionic conductivity.

Method used

A method involving an electrode assembly with a separator having a ceramic coating layer containing 92% or more inorganic particles and minimal binder, bonded with a first oligomer compound, and impregnated with a gel polymer electrolyte composition comprising a lithium salt, organic solvent, and polymerization initiator, which cures to enhance adhesion and reduce resistance.

Benefits of technology

The method results in a secondary battery with reduced resistance, improved cell rigidity, and enhanced mechanical durability by minimizing binder content and utilizing the adhesive properties of the oligomer compound during curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022005297449-PAT00001_ABST
    Figure 112022005297449-PAT00001_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a secondary battery comprising: a step of manufacturing an electrode assembly in which an electrode and a separator are alternately stacked, and an adhesive is applied to at least one surface of the electrode and the separator so that the electrode and the separator are bonded to each other; a step of housing the electrode assembly in a battery case; a step of injecting a gel polymer electrolyte composition into the battery case to impregnate the electrode assembly; and a step of curing the gel polymer electrolyte composition; wherein the adhesive comprises a first oligomer compound, the separator comprises a porous substrate and a ceramic coating layer disposed on both sides of the porous substrate, the ceramic coating layer comprises 92% by weight or more and less than 100% by weight of inorganic particles and more than 0% by weight or less of a binder, and the gel polymer electrolyte composition comprises a lithium salt, an organic solvent, a polymerization initiator, and a second oligomer compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a secondary battery. Background Technology

[0002] With the increasing technological development and demand for electronic devices, the demand for secondary batteries as an energy source is rapidly rising, and among these secondary batteries, lithium secondary batteries, which possess high energy density and voltage, have been commercialized and are widely used.

[0003] The above secondary battery can be manufactured, for example, by housing an electrode assembly in which electrodes and separators are alternately stacked in a battery case, injecting an electrolyte into the battery case, and sealing it.

[0004] At this time, the separator is generally used in which a ceramic coating layer containing inorganic particles and a binder is formed on both sides of a porous substrate. At this time, the binder is generally included in large quantities to facilitate adhesion between the electrode and the separator, but in this case, there is a problem in that the resistance increases due to the excessive use of the binder and the energy density of the battery decreases as the thickness of the separator increases.

[0005] If the binder content in the ceramic coating layer included in the separator is lowered to prevent the aforementioned problem, there is a concern for quality degradation, such as reduced cell rigidity and misalignment of the electrodes, due to a decrease in adhesion between the electrode and the separator.

[0006] Meanwhile, liquid electrolytes, particularly ion-conducting organic liquid electrolytes in which salts are dissolved in non-aqueous organic solvents, have been primarily used as electrolytes for conventional secondary batteries. However, these liquid electrolytes present problems such as the possibility of leakage to the outside of the secondary battery, reduced safety, and decreased cell rigidity.

[0007] In this regard, research is emerging to commercialize polymer electrolytes, such as gel polymer electrolytes, instead of liquid electrolytes. The gel polymer electrolyte has advantages in that it can prevent leakage to the outside of the secondary battery and has excellent cell rigidity. However, gel polymer electrolytes have problems with high interfacial resistance and low ionic conductivity compared to liquid electrolytes.

[0008] In this regard, there is a need to develop secondary batteries that simultaneously improve resistance reduction and cell rigidity. The problem to be solved

[0009] One objective of the present invention is to solve the above-mentioned problems by providing a method for manufacturing a secondary battery capable of producing a secondary battery in which the resistance of the secondary battery is reduced while simultaneously improving cell rigidity and mechanical durability. means of solving the problem

[0010] The present invention provides a method for manufacturing a secondary battery comprising: a step of manufacturing an electrode assembly in which an electrode and a separator are alternately stacked, and an adhesive is applied to at least one surface of the electrode and the separator so that the electrode and the separator are bonded to each other; a step of housing the electrode assembly in a battery case; a step of injecting a gel polymer electrolyte composition into the battery case to impregnate the electrode assembly; and a step of curing the gel polymer electrolyte composition; wherein the adhesive comprises a first oligomer compound, the separator comprises a porous substrate and a ceramic coating layer disposed on both sides of the porous substrate, the ceramic coating layer comprises 92% by weight or more and less than 100% by weight of inorganic particles and more than 0% by weight or less of a binder, and the gel polymer electrolyte composition comprises a lithium salt, an organic solvent, a polymerization initiator, and a second oligomer compound. Effects of the invention

[0011] The method for manufacturing a secondary battery according to the present invention comprises an electrode assembly in which electrodes and separators are alternately stacked and a gel polymer electrolyte, and is characterized by manufacturing a secondary battery in which the separator contains inorganic particles and a binder in specific amounts. Since the ceramic coating layer included in the separator contains a small amount of binder, an increase in resistance due to an excess amount of binder can be prevented, and the gel polymer electrolyte can compensate for the decrease in cell rigidity of the secondary battery accompanying such resistance reduction. Accordingly, the secondary battery manufactured from the method for manufacturing a secondary battery according to the present invention can simultaneously improve resistance reduction, cell rigidity, and mechanical durability depending on the combination of the above components.

[0012] In addition, the method for manufacturing a secondary battery according to the present invention comprises an electrode assembly in which an electrode and a separator are alternately stacked and the electrode and separator are bonded by an adhesive, the assembly being manufactured by housing the electrode assembly in a battery case, injecting and curing a gel polymer electrolyte composition, wherein the adhesive comprises a first oligomer compound. Since the adhesive comprises a first oligomer compound, the first oligomer compound may also participate in the curing process when the gel polymer electrolyte composition is cured. Furthermore, the first oligomer compound can bond the electrode and the separator, thereby preventing the problem of misalignment of the electrode and separator positions during the manufacture of the electrode assembly, and can also improve cell rigidity by polymerizing through the final curing of the gel polymer electrolyte composition. Brief explanation of the drawing

[0013] FIG. 1 is a schematic side view of an exemplary electrode assembly to explain the manufacturing step of an electrode assembly in the method for manufacturing a secondary battery of the present invention. FIG. 2 is a schematic plan view of a separator or electrode, intended to explain the manufacturing step of an electrode assembly in the method for manufacturing a secondary battery of the present invention. FIG. 3 is a schematic side view of a separator, intended to explain the manufacturing step of an electrode assembly in the method for manufacturing a secondary battery of the present invention. FIG. 4 is a drawing for explaining the manufacturing method of a secondary battery of the present invention, and for explaining the manufacturing process of an electrode assembly. FIG. 5 is a drawing for explaining the manufacturing method of a secondary battery of the present invention, and for explaining the manufacturing process of an electrode assembly. FIG. 6 is a drawing for explaining the manufacturing method of a secondary battery of the present invention, and for explaining the manufacturing process of an electrode assembly. FIG. 7 is a drawing for explaining the manufacturing method of a secondary battery of the present invention, and for explaining the manufacturing process of an electrode assembly. FIG. 8 is a diagram illustrating the receiving step of an electrode assembly in the method for manufacturing a secondary battery of the present invention. FIG. 9 is a diagram illustrating the steps of injecting a gel polymer electrolyte composition and impregnating an electrode assembly in the method for manufacturing a secondary battery of the present invention. FIG. 10 is a diagram illustrating the curing step of a gel polymer electrolyte in the method for manufacturing a secondary battery of the present invention. Specific details for implementing the invention

[0014] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0015] In this specification, the average particle size (D 50 ) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. The above average particle size (D 50) can be measured, for example, using the laser diffraction method. The laser diffraction method generally enables the measurement of particle sizes ranging from the submicron range to several millimeters, and can obtain results with high reproducibility and high resolution.

[0016] The secondary battery of the present invention will be described in detail below with reference to the drawings. In assigning reference numerals to the components of each drawing, the same components may have the same reference numeral as much as possible, even if they are shown in different drawings. Furthermore, in describing the present invention, if it is determined that a detailed description of related known components or functions could obscure the essence of the present invention, such detailed description may be omitted.

[0018] Method for manufacturing a secondary battery

[0019] The present invention relates to a method for manufacturing a secondary battery, specifically a method for manufacturing a lithium secondary battery.

[0020] The present invention comprises the steps of: manufacturing an electrode assembly (100) in which electrodes (110, 120) and a separator (130) are alternately stacked, and an adhesive (140) is applied to at least one surface of the electrodes (110, 120) and the separator (130) so that the electrodes (110, 120) and the separator (130) are bonded to each other; housing the electrode assembly (100) in a battery case (300); and injecting a gel polymer electrolyte composition (200) into the battery case (300) to impregnate the electrode assembly (100). The present invention provides a method for manufacturing a secondary battery comprising the step of curing the gel polymer electrolyte composition (200); wherein the adhesive (140) comprises a first oligomer compound, the separator (130) comprises a porous substrate (131) and ceramic coating layers (132a, 132b) disposed on both sides of the porous substrate (131), the ceramic coating layers (132a, 132b) comprise 92% by weight or more and less than 100% by weight of inorganic particles and more than 0% by weight or less of a binder, and the gel polymer electrolyte composition (200) comprises a lithium salt, an organic solvent, a polymerization initiator, and a second oligomer compound.

[0022] (1) Manufacturing step of the electrode assembly

[0023] Referring to FIGS. 1 and 2, first, electrodes (110, 120) and separators (130) are alternately stacked, and an adhesive (140) is applied to at least one surface of the electrodes (110, 120) and the separator (130) so that the electrodes (110, 120) and the separator (130) are bonded to each other to manufacture an electrode assembly (100).

[0024] The electrode assembly (100) includes a plurality of electrodes (110, 120) stacked in a vertical direction (P). The electrodes (110, 120) may be two or more. In this specification, “vertical direction” may mean a vertical direction relative to the ground and is intended only to describe the stacking direction of the electrodes and is not intended to limit the angle of the stacking direction.

[0025] The electrodes (110, 120) may include a first electrode (110) and a second electrode (120). As shown in FIG. 3, the first electrode (110) and the second electrode (120) may be stacked alternately. The electrodes (110, 120) may be stacked alternately with a separator (130) in between. The first electrode (110) may be an anode and the second electrode (120) may be a cathode. Alternatively, the first electrode (110) may be a cathode and the second electrode (120) may be an anode. The first electrode and the second electrode may each be one or more, specifically two or more.

[0026] The first electrode (110) and the second electrode (120) may have a structure in which an active material slurry is coated on a current collector. The first electrode (110) and the second electrode (120) may have a structure in which the active material slurry is coated, dried, and rolled on both sides of a current collector. The active material slurry may be formed by stirring a state in which granular active material, conductive material, binder, etc. are added to a solvent. Active material, conductive material, binder, etc. used in a positive or negative electrode in the field may be used in the first electrode (110) and the second electrode (120) without limitation.

[0027] The above current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. Specifically, the above current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum-cadmium alloy. For example, when the electrode (110, 120) is a positive electrode, the current collector used for the electrode (110, 120) may include aluminum, and when the electrode (110, 120) is a negative electrode, the current collector used for the electrode (110, 120) may include copper.

[0028] The above current collector can be used in various forms such as films, sheets, foils, nets, meshes, porous bodies, foams, and nonwoven fabrics. Additionally, the above current collector may include a polymer layer and metal layers disposed on both sides of the polymer layer, and the metal layer may include at least one material selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum-cadmium alloy.

[0029] Specifically, when the electrode (110, 120) is a negative electrode, the negative electrode active material included therein may be, for example, a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of negative electrode active materials include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO βExamples include metal oxides capable of doping and dedoping lithium, such as (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, the carbon material may include low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0030] Additionally, specifically, when the electrode (110, 120) is a positive electrode, the positive electrode active material included therein is not particularly limited, and for example, the positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 Examples include lithium manganese composite oxides represented by O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); and LiMn2O4 in which a portion of the Li in the chemical formula is substituted with alkaline earth metal ions, but are not limited thereto. The anode may also be a Li-metal anode.

[0031] The binders included in the above electrode are polyvinylidene fluoride polymer, polyvinyl alcohol, styrene butadiene rubber, polyethylene oxide, carboxyl methyl cellulose, cellulose acetate, cellulose acetate butylate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, polymethyl methacrylate, polybutylacrylate, polyacrylonitrile, and polyvinylpyrrolidone. It may be any one binder polymer selected from the group consisting of polyvinylpyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate copolymer, polyarylate, and low molecular weight compounds with a molecular weight of 10,000 g / mol or less, or a mixture of two or more of these.

[0032] The conductive material included in the above electrode is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives may be used.

[0033] An example of a thickening agent included in the above electrode is carboxymethylcellulose (CMC).

[0035] As illustrated in FIGS. 1 and 2, the electrode assembly (100) includes a separator (130). The separator is alternately stacked with the electrode.

[0036] As illustrated in FIG. 1, the separator (130) may be folded or bent in a zigzag shape to wrap around one end of the electrodes (110, 120). For example, as illustrated in FIG. 1, when the first electrode (110) and the second electrode (120) are alternately stacked, the separator (130) may be folded to wrap around one end (110a) of the first electrode (110), and then folded again to wrap around one end of the second electrode (110) located opposite the one end (110a) of the first electrode (110). As this folding is repeated, the separator (130) may be folded or bent in a zigzag shape. The electrode assembly (100) may include one separator (130).

[0037] The electrode assembly (100) may be a zigzag stacked electrode assembly in which the separator (130) is folded or bent in a zigzag shape, and the first electrode (110), the separator (130), the second electrode (120), and the separator (130) are sequentially stacked in a basic unit, with one or more, specifically two or more, stacked.

[0038] As illustrated in FIG. 3, the separator (130) comprises a porous substrate (131) and ceramic coating layers (132a, 132b) disposed on both sides of the porous substrate.

[0039] The porous substrate (131) is not particularly limited as long as it is typically used as a separator for a secondary battery. Specifically, the porous substrate (131) is preferably low-resistance to the movement of electrolyte ions and has excellent electrolyte moisture retention capacity. More specifically, the porous substrate (131) may include at least one selected from the group consisting of polyolefin-based resins such as polyethylene, polypropylene, polybutylene, and polypentene; fluorine-based resins such as polyvinylidene fluoride and polytetrafluoroethylene; polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate; polyacrylonitrile resin; and cellulose-based resin, and may be a porous film or nonwoven fabric, or a laminated structure of two or more layers thereof, comprising one or more copolymers or mixtures of any one or more of these. The porous substrate (131) may be a porous film, nonwoven fabric, or a laminated structure of two or more layers thereof comprising the polyolefin-based resin.

[0040] The pore size and porosity present in the porous substrate (131) are not particularly limited. Specifically, the porous substrate (131) may be a porous substrate containing pores with an average pore diameter of 0.01 μm to 1 μm, specifically 20 nm to 60 nm, with a porosity of 10 volume% to 90 volume%, specifically 30 volume% to 60 volume%. In this case, it is desirable in that it improves the mechanical strength of the porous substrate (131) and allows ionic materials to move more smoothly between the anode and the cathode. The average pore diameter and porosity may be measured by analysis using a focused ion beam (FIB), gas adsorption, or mercury intrusion.

[0041] The thickness of the porous substrate (131) is not particularly limited, but considering the appropriate mechanical strength as a separator and the ease of movement of ionic materials, it may be specifically 1 μm to 100 μm, specifically 2 μm to 15 μm.

[0042] The ceramic coating layers (132a, 132b) are disposed on both sides of the porous substrate (131).

[0043] The ceramic coating layer (132a, 132b) comprises inorganic particles and a binder. More specifically, the ceramic coating layer may consist only of the inorganic particles and the binder.

[0044] The above inorganic particles may be introduced to prevent thermal shrinkage of the porous substrate at high temperatures and the resulting short circuit between the anode and cathode, and the above inorganic particles may be provided as a type of spacer that maintains the physical shape of the porous substrate and minimizes thermal shrinkage.

[0045] The above-mentioned inorganic particles may be used without special restrictions as long as they are electrochemically stable within the operating voltage range of the battery (e.g., 0V to 5V based on Li / Li+) and do not cause oxidation and / or reduction reactions, i.e., electrochemical reactions. The above-mentioned inorganic particles are lithium phosphate (Li3PO4); lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3); 리튬알루미늄티타늄포스페이트(Li x Al y Ti z (PO4)3, 0 <x<2, 0<y<1, 0<z<3), 14Li2O-9Al2O3-38TiO2-39P2O5와 같은 (LiAlTiP) x O y Glass (0 <x<4, 0<y<13); 리튬란탄티타네이트(Li x La y TiO3, 0 <x<2, 0<y<3); Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 x Ge y P z S w , 0 <x<4, 0<y<1, 0<z<1, 0<w<5); Li3N 등과 같은 리튬나이트라이드(Li x N y , 0 <x<4, 0<y<2); Li3PO4-Li2S-SiS2 등과 같은 SiS2계 유리(Li x Si y S z , 0 <x<3, 0<y<2, 0<z<4); LiI-Li2S-P2S5 등과 같은 P2S5계 유리(Li x P y S z , 0 <x<3, 0<y<3, 0<z<7); Al2O3; AlOOH; BaTiO3; BaSO4; MgO; CaO; CeO2; NiO; SiO2; SnO2; SrTiO3; TiO2; Y2O3; ZnO; ZrO2; Pb(Zr,Ti)O3(PZT); Pb1-x La x Zr 1-y TiyO3(PLZT); PB(Mg3Nb 2 / 3 The inorganic particles may be Al2O3; AlOOH; BaTiO3; BaSO4; MgO; CaO; CeO2; NiO; SiO2; SnO2; SrTiO3; TiO2; Y2O3; ZnO; ZrO2; Pb(Zr,Ti)O3(PZT); Pb 1-x La x Zr 1-y TiyO3(PLZT); PB(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT); hafnia (HfO2); may be a mixture of two or more of these, and more specifically may include at least one selected from the group consisting of Al2O3; AlOOH; BaTiO3; BaSO4; and MgO.

[0046] Average particle size (D of the above inorganic particles) 50 ) can be 0.1㎛ to 1㎛, specifically 0.2㎛ to 0.7㎛.

[0047] The above inorganic particles are included in the ceramic coating layer (132a, 132b) in an amount of 92% by weight or more and less than 100% by weight. The content of the above inorganic particles should be considered in relation to the content of the binder described later, and can be controlled to prevent a decrease in thermal stability due to thermal shrinkage of the porous substrate while preventing an increase in resistance due to an excess amount of binder. Specifically, the above inorganic particles may be included in the ceramic coating layer in an amount of 93% to 98% by weight.

[0048] The above binder may be included in the ceramic coating layer (132a, 132b) for binding inorganic particles and binding the separator and the electrode.

[0049] At this time, the binder is included in the ceramic coating layer in an amount greater than 0% by weight and less than 8% by weight. If the binder is included in an amount greater than 8% by weight, the binder may be excessively included in the ceramic coating layer, which may lead to an increase in the resistance of the secondary battery. Meanwhile, although there is a concern that the cell rigidity of the secondary battery may decrease due to a decrease in the adhesion between the electrode and the separator when the binder is included in the above-described range, as described below, the present invention can simultaneously achieve an improvement in cell rigidity and mechanical durability along with an improvement in the resistance of the secondary battery by using a combination of a separator having the above-described characteristics and a gel polymer electrolyte.

[0050] Specifically, the binder may be included in the ceramic coating layer in an amount of 2% to 7% by weight, and when within this range, the binding force of the inorganic particles can be maximized while preventing an increase in the resistance of the secondary battery.

[0051] The above binder includes a fluorine group (-F), an acrylate group (CH2=CHCOO-), a methacrylate group (CH2=C(CH3)COO-), and a vinyl acetate group ( -It may be a hydrophobic binder containing one or more hydrophobic functional groups such as CH2=CHOCO-) or nitrile groups (-C≡N); or a hydrophilic binder containing one or more polar groups such as hydroxyl groups (-OH), carboxyl groups (-COOH), maleic anhydride groups (-COOOC-), sulfonic acid groups (-SO3H), or isocyanate groups (-NCO-), and any one or more of these may be used. More specifically, the hydrophobic binder may be polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylacetate, polyethylene-covinylacetate copolymer, polyimide, polyethylene oxide, etc. In addition, the hydrophilic binder may be cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, carboxyl methyl cellulose, polyvinylalcohol, polyacrylic acid, polymaleic anhydride, or polyvinylpyrrolidone, etc.

[0052] Specifically, the binder may be an acrylic binder. The acrylic binder enables good dispersion with the inorganic particles during the manufacture of the ceramic coating layer, thereby preventing the ceramic coating layer from separating into a binder layer on top and inorganic particles on the bottom. Since such separation of layers hinders ion movement at the cathode and anode and causes an increase in resistance, using an acrylic binder as the binder allows the resistance reduction effect intended by the present invention to be exhibited at a superior level.

[0053] The above acrylic binder may include at least one selected from the group consisting of a copolymer of ethylhexyl acrylate and methyl methacrylate; polymethylmethacrylate; polyethylhexyl acrylate; polybutyl acrylate; polyacrylonitrile; and a copolymer of butyl acrylate and methyl methacrylate.

[0054] The ceramic coating layer may contain inorganic particles and a binder in a weight ratio of 92:8 or more and less than 100:0, specifically 93:7 to 98:2.

[0055] The thickness of the ceramic coating layer (132a, 132b) may be 0.1㎛ to 10㎛, specifically 0.5㎛ to 5㎛, more specifically 1.0㎛ to 2.5㎛. Since the ceramic coating layer (132a, 132b) contains a binder in the aforementioned low amount, it is possible to implement a thin separator, thereby further improving the energy density of the secondary battery and achieving low resistance. The thickness of the ceramic coating layer may refer to the thickness of a single ceramic coating layer formed on one surface of the porous substrate.

[0056] The ceramic coating layer (132a, 132b) can be manufactured by applying a composition for forming a ceramic coating layer, in which inorganic particles and a binder are dispersed in a solvent, to the porous substrate and drying it. The method of applying the composition for forming a ceramic coating layer is not particularly limited and may use dip coating, die coating, roll coating, comma coating, gravure coating, etc., and specifically, gravure coating may be used. After applying the composition for forming a ceramic coating layer, the drying method may include natural drying, reversible drying, or hot air drying.

[0057] The thickness of the separator (130) may be 1 μm to 20 μm, specifically 5 μm to 14 μm. According to the present invention, a thin separator can be implemented by reducing the binder content in the ceramic coating layer, thereby further improving the energy density of the secondary battery and achieving low resistance.

[0059] The electrode assembly (100) has an adhesive (140) applied to at least one surface of the electrode (110, 120) and the separator (130), so that the electrode (110, 120) and the separator (130) are bonded to each other.

[0060] The adhesive (140) may be introduced for bonding the electrodes (110, 120) and the separator (130). Specifically, the adhesive (140) may be introduced to fix the alignment position of the electrodes and the separator during the process of stacking, assembling, and stacking the electrodes and the separator during the manufacturing process of the secondary battery. As described above, the separator (130) according to the present invention has a reduced binder content, so the bonding strength between the electrodes and the separator may not be sufficient during the manufacturing of the secondary battery. Therefore, the adhesive (140) can compensate for this problem to easily bond the electrodes and the separator, and prevent the separator from shifting during the manufacturing process of the electrode assembly, thereby enabling the improvement of process efficiency and quality.

[0061] The above adhesive includes a first oligomer compound.

[0062] In this specification, "oligomer compound" may mean a compound in which monomers are polymerized into about 10 or fewer, and "oligomer compound" may include crosslinking groups.

[0063] The first oligomer compound is included in the adhesive as an adhesive component for bonding the electrode and the separator. After being used as an adhesive component for the electrode and the separator, the first oligomer compound can be dissolved and polymerized by the injection of the gel polymer electrolyte composition to become a component of the gel polymer electrolyte.

[0064] The first oligomer compound may include one or more selected from the group consisting of polyether-based oligomers, polycarbonate-based oligomers, acrylate-based oligomers, polysiloxane-based oligomers, phosphazene-based oligomers, polyethylene-based oligomers, urethane-based oligomers, epoxy-based oligomers, fluorine-based oligomers, polyethylene oxide, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride, specifically at least one selected from fluorine-based oligomers, polycarbonate-based oligomers, and polysiloxane-based oligomers.

[0065] For example, the above-mentioned fluorine-based oligomer may specifically include units derived from fluorine-based monomers. The above-mentioned fluorine-based oligomer has the advantage of further improving battery stability by suppressing the generation of oxygen radicals caused by the decomposition of the cathode active material through the fluorine-based functional groups included therein, and also has excellent flame retardancy. More specifically, the above-mentioned fluorine-based oligomer may include at least one selected from tetrafluoroethylene (TFE)-vinyl acetate copolymer, (allyl 1,1,2,2-tetrafluoroethyl ether)-(2,2,2-trifluoroethyl acrylate) copolymer, tetrafluoroethylene-(2-vinyl-1,3-dioxolane) copolymer, and tetrafluoroethylene-vinyl methacrylate copolymer.

[0066] In addition, the polycarbonate-based oligomer has the advantages of being affinity for the anode, having a structure similar to an organic electrolyte, and having excellent ionic conductivity or ionic dissociation. The polycarbonate-based oligomer may be a polycarbonate having a weight-average molecular weight of 1,000 g / mol to 50,000 g / mol, specifically 4,500 g / mol to 30,000 g / mol, and more specifically 10,000 g / mol to 25,000 g / mol.

[0067] In addition, the above polysiloxane-based oligomer can function as a scavenger for gases (such as HF) generated by side reactions in the electrolyte, and accordingly, can have the effect of improving high-temperature storage characteristics.

[0068] The weight-average molecular weight of the first oligomer compound may be 1,000 g / mol to 50,000 g / mol, specifically 4,500 g / mol to 30,000 g / mol.

[0069] The adhesive (140) is used to manufacture an electrode assembly (100) by bonding the electrodes (110, 120) and the separator (130), and after the electrode assembly (100) is housed in a battery case (300) and the gel polymer electrolyte composition (200) is injected into the battery case (300), the adhesive (140) can be dissolved in the organic solvent contained in the gel polymer electrolyte composition (200). Since the adhesive (140) according to the present invention dissolves after being used to manufacture the electrode assembly (100), the electrodes (110, 120) and the separator (130) can be easily bonded without increasing the amount of binder in the separator (130), and the energy density of the secondary battery can be further improved by preventing an increase in the thickness of the separator due to an increase in the amount of binder.

[0070] As illustrated in FIG. 3, the adhesive (140) may be applied in the form of a plurality of spaced-apart patterns. Specifically, the adhesive (140) may be applied to at least one surface of the electrode and the separator in the form of a plurality of spaced-apart patterns. Specifically, the adhesive may be applied to at least one surface of the electrode and the separator in the form of a plurality of spaced-apart dots.

[0071] The application area of ​​the adhesive may be greater than 0% and less than or equal to 1% with respect to the surface area where the separator and the electrode come into contact, specifically 0.0001% to 0.05%. According to the above range, the electrode and the separator can be bonded with sufficient adhesive strength, and at the same time, it is desirable to prevent the problem of the adhesive being excessively applied and remaining undissolved in the solvent, thereby causing an increase in resistance.

[0073] Hereinafter, an exemplary method of manufacturing the electrode assembly is described with reference to FIGS. 4 to 7.

[0074] Specifically, referring to FIGS. 4 to 7, the electrode (110, 120) includes a first electrode (110) and a second electrode (120), and the electrode assembly (100) can be manufactured by a method including the following steps (a) to (d).

[0075] (a) a step of applying the adhesive (140) to at least a portion of the separator (130) and the first electrode (110);

[0076] (b) a step of bonding the separator (130) and the first electrode (110) through the applied adhesive (140);

[0077] (c) A step of folding one side of the separator (130) to cover the first electrode (110);

[0078] (d) a step of applying the adhesive (140) to at least a portion of the separator (130) and the second electrode (120).

[0079] (e) a step of bonding the separator (130) and the second electrode (120) through the applied adhesive (140); and

[0080] (d) A step of folding the other side of the separator (130) to cover the second electrode (120).

[0082] Referring to FIG. 4, the adhesive (140) is applied to at least a portion of the separator (130) and the first electrode (110). The application of the adhesive (140) may be achieved by applying the adhesive (140) to at least a portion of the separator (130) and the first electrode (110) using a first nozzle (1110). FIG. 4 is illustrated with the adhesive (140) applied to the separator (130), but is not limited thereto, and the adhesive (140) may be applied to at least a portion of the separator (130); the first electrode (110); or both the separator (130) and the first electrode (110).

[0083] As illustrated in FIG. 4, specifically, the separator (130) may be unwound from the separator reel (630) and placed on the upper surface of the table (700).

[0084] Referring to FIG. 5, the separator (130) and the first electrode (110) are bonded together through the applied adhesive (140).

[0085] The first electrode (110) may be formed by cutting a first electrode sheet (1101), which is unwound by a first electrode reel (610) as shown in FIG. 5, with a first cutter (810). At this time, when the first transfer device (910) transfers the first electrode (110), the first header (1010) can adsorb the first electrode. Subsequently, the first electrode (110) may be seated or placed on the separator (130) depending on the movement of the first header (1010) and / or the table (700).

[0086] Referring to FIG. 6, one side of the separator (130) is folded to cover the first electrode (110); and the adhesive (140) can be applied to at least a portion of the separator (130) and the second electrode (120).

[0087] After the first electrode (110) is attached to the separator (130), one side of the separator (130) is folded to cover the first electrode (110). For example, the folding of the separator (130) can be achieved by moving the side of the table (700).

[0088] Meanwhile, the adhesive (140) is applied to at least a portion of the separator (130) and the second electrode (120). The application of the adhesive (140) may be achieved by applying the adhesive (140) to at least a portion of the separator (130) and the second electrode (120) using a second nozzle (1120). FIG. 6 is illustrated with the adhesive (140) applied to the separator (130), but is not limited thereto, and the adhesive (140) may be applied to at least a portion of the separator (130); the second electrode (120); or both the separator (130) and the second electrode (120).

[0089] Referring to FIG. 7, the separator (130) and the second electrode (120) are bonded together using the applied adhesive (140); and the other side of the separator (130) is folded to cover the second electrode (120).

[0090] A second electrode (120) is attached to the opposite side of the separator (130) and the first electrode (110) that are in contact with each other.

[0091] The second electrode (120) may be formed by cutting a first electrode sheet (1201), which is unwound by a second electrode reel (620) as shown in FIG. 7, with a second cutter (820). At this time, when the second transfer device (920) transfers the second electrode (120), the second header (1020) can adsorb the second electrode. Subsequently, the second electrode may be seated or adhered to the separator as the second header (1020) and / or table (700) move.

[0092] Referring to FIG. 7, after the second electrode (120) is bonded, the other side of the separator (130) is folded to cover the second electrode (120). Accordingly, it is possible to manufacture an electrode assembly in which the first electrode and the second electrode are alternately stacked, a separator is interposed between the first electrode and the second electrode, and the separator is folded in a zigzag shape. Subsequently, by repeating the process described above, it is possible to realize an electrode assembly in which a plurality of first electrodes and second electrodes are alternately stacked.

[0093] At this time, in the case of an electrode assembly including a separator folded in a zigzag shape as described above, a slipping phenomenon of the separator and / or electrode occurs due to the folding or bending of the separator during the manufacturing process, which leads to problems such as quality defects and reduced process efficiency. However, according to the present invention, since an adhesive is applied to bond the electrode and the separator, the aforementioned slipping phenomenon of the electrode and / or separator can be prevented to a significant degree, and it is possible to manufacture a secondary battery with improved quality. Such application of the adhesive is particularly desirable in terms of supplementing the adhesive strength of the separator of the present invention, which contains a low amount of binder.

[0095] (2) Receiving step of the electrode assembly

[0096] Referring to FIG. 8, the electrode assembly (100) is housed in a battery case (300).

[0097] For convenience of explanation, the electrode assembly is briefly shown in FIG. 8.

[0098] The above battery case (300) may be provided for the purpose of accommodating an electrode assembly (100) and a gel polymer electrolyte (200).

[0099] The battery case (300) may be a pouch-shaped case made of a flexible material, for example, an aluminum pouch battery case.

[0100] If the battery case (300) is an aluminum pouch battery case, the battery case (300) may be formed from a pouch film laminated in the order of a polypropylene layer (PP layer), an aluminum layer, and a polyethylene terephthalate layer (PET layer) from the inside out.

[0101] The battery case (300) may include a cup portion which is a receiving space for housing an electrode assembly.

[0102] The battery case (300) may include a cover (310), and after housing the electrode assembly and curing and gelling of the gel polymer electrolyte composition, the battery case (300) may be sealed with the cover to manufacture a sealed secondary battery.

[0104] As illustrated in FIG. 8, a plurality of electrode tabs (400, 500) may be connected to the electrode assembly. Specifically, the plurality of electrode tabs (400, 500) are connected to the electrodes (110, 120) of the electrode assembly (100), more specifically, they are connected to the first electrode (110) and the second electrode (120), respectively, and may protrude outside the battery case (300) to form a path through which electrons can move. Additionally, FIG. 8 shows two electrode tabs (400, 500) arranged in different directions relative to the electrode assembly (100), but is not limited thereto and may protrude side by side in the same direction from one side of the electrode assembly (100). The plurality of electrode tabs (400, 500) may be positive electrode tabs and negative electrode tabs, and may be connected to the positive and negative electrodes, respectively.

[0106] (3) Injection of gel polymer electrolyte composition and impregnation step of electrode assembly

[0107] Referring to FIG. 9, the gel polymer electrolyte composition (200) is injected into the battery case (300) to impregnate the electrode assembly (100). The gel polymer electrolyte composition (200) may be impregnated and cured in the electrode assembly (100) and placed inside and outside the electrode assembly.

[0108] The gel polymer electrolyte (200a) cured with the above gel polymer electrolyte composition (200) has no flowability, and since a gelled electrolyte is used, the cell rigidity of the secondary battery can be improved. In particular, the present invention enables the realization of a secondary battery with reduced resistance and improved cell rigidity by using the above gel polymer electrolyte together with the aforementioned separator. On the other hand, if the above separator and liquid electrolyte are used, the cell rigidity is excessively reduced, so there is a concern about reduced processability and product defects due to cell sagging, separator slippage, etc., and safety is reduced, leading to the possibility of explosion of the secondary battery.

[0109] The gel polymer electrolyte composition (200) comprises a lithium salt, an organic solvent, a polymerization initiator, and a second oligomer compound.

[0110] The above lithium salt can be used for the purpose of providing lithium ions to a secondary battery.

[0111] The above lithium salt can be used without special limitations as long as it is a compound capable of providing lithium ions used in secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1M to 5.0M, more preferably 0.1M to 3.0M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0112] The above polymerization initiator can be used for the purpose of polymerizing oligomer compounds included in the gel polymer electrolyte composition to form a polymer network bonded in a three-dimensional structure.

[0113] The polymerization initiator can proceed with the polymerization of an oligomer compound by decomposing in the presence of heat or light to form radicals. Specifically, the polymerization initiator can proceed with the polymerization of a first oligomer compound dissolved by the gel polymer electrolyte composition after being used to assemble the second oligomer compound included in the gel polymer electrolyte composition and the electrode assembly.

[0114] The above polymerization initiator may be a photopolymerization initiator or a thermal polymerization initiator depending on the polymerization method.

[0115] Specifically, representative examples of the above photopolymerization initiators include 2-hydroxy-2-methylpropiophenone (HMPP), 1-hydroxy-cyclohexylphenyl-ketone, benzophenone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, oxy-phenylacetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester, oxy-phenyl-acetic 2-[2-hydroxyethoxy]-ethyl ester, alpha-dimethoxy-alpha-phenylacetophenone, 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, and diphenyl It may include at least one compound selected from the group consisting of (2,4,6-trimethylbenzoyl)-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(etha 5-2,4-cyclopentadiene-1-yl), bis[2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl]titanium, 4-isobutylphenyl-4'-methylphenyliodonium, hexafluorophosphate, and methyl benzoyl formate.

[0116] In addition, the above thermal polymerization initiator is, as a representative example, benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, t-butyl peroxy-2-ethyl-hexanoate, cumyl hydroperoxide and hydrogen peroxide, 2,2'-azobis(2-cyanobutane), 2,2'-azobis(methylbutyronitrile), 2,2'-azobis(isobutyronitrile) (AIBN; 2,2'-Azobis(iso-butyronitrile)), and 2,2'-azobisdimethyl-valeronitrile (AMVN; It may include at least one compound selected from the group consisting of 2,2'-Azobisdimethyl-Valeronitrile).

[0117] The above polymerization initiator can decompose by heat of 30°C to 100°C in a secondary battery or by light such as UV at room temperature (5°C to 30°C) to form radicals, and can form cross-links through free radical polymerization to enable the polymerization of oligomers.

[0118] The second oligomer compound may be of the same type as the first oligomer compound described above. The first oligomer compound and the second oligomer compound may be the same or different.

[0119] Specifically, the second oligomer compound may include one or more selected from the group consisting of polyether-based oligomers, polycarbonate-based oligomers, acrylate-based oligomers, polysiloxane-based oligomers, phosphazene-based oligomers, polyethylene-based oligomers, urethane-based oligomers, epoxy-based oligomers, fluorine-based oligomers, polyethylene oxide, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride, specifically at least one selected from fluorine-based oligomers, polycarbonate-based oligomers, and polysiloxane-based oligomers.

[0120] For example, the above-mentioned fluorine-based oligomer may specifically include units derived from fluorine-based monomers. The above-mentioned fluorine-based oligomer has the advantage of further improving battery stability by suppressing the generation of oxygen radicals caused by the decomposition of the cathode active material through the fluorine-based functional groups included therein, and also has excellent flame retardancy. More specifically, the above-mentioned fluorine-based oligomer may include at least one selected from tetrafluoroethylene (TFE)-vinyl acetate copolymer, (allyl 1,1,2,2-tetrafluoroethyl ether)-(2,2,2-trifluoroethyl acrylate) copolymer, tetrafluoroethylene-(2-vinyl-1,3-dioxolane) copolymer, and tetrafluoroethylene-vinyl methacrylate copolymer.

[0121] In addition, the above-mentioned polycarbonate-based oligomer has the advantages of being affinity for the anode, having a structure similar to an organic electrolyte, and having excellent ionic conductivity or ionic dissociation.

[0122] In addition, the above polysiloxane-based oligomer can function as a scavenger for gases (such as HF) generated by side reactions in the electrolyte, and accordingly, can have the effect of improving high-temperature storage characteristics.

[0123] The weight-average molecular weight of the second oligomer compound may be 1,000 g / mol to 50,000 g / mol, specifically 4,500 g / mol to 30,000 g / mol.

[0124] The second oligomer compound may be included in the gel polymer electrolyte composition in an amount of 1% to 20% by weight, specifically 3% to 10% by weight, and when within this range, the effect of improving the cell rigidity of the secondary battery is excellently exhibited, and the ion conductivity of the gel polymer electrolyte and the mobility of lithium ions can be exhibited at an excellent level. The organic solvent may be used for the purpose of dissolving or dispersing the lithium salt and the second oligomer compound.

[0125] The above organic solvent is one commonly used in secondary batteries, and for example, ethers, esters (acetates, propionates), amides, linear carbonates or cyclic carbonates, nitriles (acetonitrile, SN, etc.), etc., can be used individually or in a mixture of two or more types.

[0126] Among these, carbonate-based solvents containing carbonate compounds that are cyclic carbonates, linear carbonates, or mixtures thereof can be used as a representative example.

[0127] Specific examples of the above-mentioned cyclic carbonate compounds include a single compound selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, and their halides, or a mixture of at least two of these. Additionally, specific examples of the above-mentioned linear carbonate compounds may include, but are not limited to, compounds selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethylmethyl carbonate (EMC), methylpropyl carbonate (MPC), and ethylpropyl carbonate (EPC), or a mixture of at least two of these.

[0128] In particular, among the carbonate-based solvents mentioned above, propylene carbonate and ethylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts in the electrolyte, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as ethylmethyl carbonate, diethyl carbonate, or dimethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.

[0129] In addition, among the organic solvents, a single compound selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, α-valerolactone, and ε-caprolactone, or a mixture of at least two or more, may be used as the ester, but is not limited thereto.

[0131] Depending on the injection of the gel polymer electrolyte composition, the first oligomer compound may be dissolved in the gel polymer electrolyte composition. Specifically, depending on the injection of the gel polymer electrolyte composition, the first oligomer compound used in the assembly of the electrode assembly may be dissolved in the gel polymer electrolyte composition. As described below, the first oligomer compound is polymerized upon curing of the gel polymer electrolyte composition.

[0132] The dissolution of the first oligomer compound may be more smoothly achieved during the pressurization in the activation and degassing processes generally involved in the secondary battery manufacturing process. The activation is a process of forming a Surface Electrolyte Interface (SEI) layer on the surface of the electrode plate of an electrode assembly through a charging process in an initial secondary battery and making it chargeable, thereby enabling the secondary battery to supply power; it may be performed, for example, at 45°C or higher, specifically between 50°C and 70°C. The degassing process is a process of discharging gas generated during the activation process, etc., to the outside, and may involve a process of pressurizing the secondary battery using a jig, etc. The first oligomer compound may be more smoothly dissolved or removed by such temperature increase, pressurization, etc.

[0133] The gel polymer electrolyte composition (200) is poured into a battery case (300), and the electrode assembly (100) is impregnated with the gel polymer electrolyte composition (200). The impregnation can be performed at a temperature of 10°C to 30°C for 0.5 hours to 72 hours, and preferably at a temperature of 15°C to 30°C for 40 hours to 60 hours.

[0135] (4) Curing step of the gel polymer electrolyte composition

[0136] Subsequently, as illustrated in FIG. 10, the gel polymer electrolyte composition (200) is cured. Specifically, the gel polymer electrolyte composition (200) is cured to form a gel polymer electrolyte (200a).

[0137] When the gel polymer electrolyte composition is cured, the oligomer compounds can be crosslinked and cured to form an electrolyte (gel polymer electrolyte) that has solidified into a gel form. Specifically, the second oligomer compound included in the gel polymer electrolyte composition and the first oligomer compound dissolved by the gel polymer electrolyte composition are crosslinked or polymerized together by the curing process to form a gelled electrolyte.

[0138] The gel polymer electrolyte formed by curing the above gel polymer electrolyte composition can contribute to improving the cell rigidity of a secondary battery. As described above, the separator according to the present invention can contribute to resistance reduction by including a ceramic coating layer using a low content of binder. Accordingly, a secondary battery combining the separator and the gel polymer electrolyte can simultaneously improve resistance reduction and cell rigidity.

[0139] At this time, the curing of the gel polymer electrolyte composition can be performed at a temperature of 50°C to 100°C for 0.5 hours to 48 hours, and preferably at a temperature of 60°C to 80°C for 0.5 hours to 24 hours.

[0140] Meanwhile, the curing can be performed while the battery case (300) is sealed. For example, the gel polymer electrolyte composition can be heat-cured by heat treatment after sealing the battery case (300) containing the electrode assembly (100) and the gel polymer electrolyte composition (200) with a cover or the like.

[0141] After the above curing or sealing and curing, further processes such as activation, degassing, and resealing known in the art may be performed.

[0143] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0145] Examples and Comparative Examples

[0146] Example 1

[0147] 1. Manufacture of separator membranes

[0148] Al2O3 as inorganic particles (average particle size (D 50 A composition for forming a ceramic coating layer was prepared by adding an acrylic binder and a 0.5㎛ (0.5㎛) and an acrylic binder to water, which is the solvent, in a weight ratio of 96:4. As the acrylic binder, a mixture of JSR’s product name TRD 202A and APEC’s product name AP-0821 was used.

[0149] A separator (thickness: 12㎛ = 1.5㎛ + 9㎛ + 1.5㎛) was prepared by applying the composition for forming the ceramic coating layer to both sides of a polyethylene porous substrate (thickness: 9㎛, average pore diameter: 0.05㎛, porosity: 45% by gravure coating) and drying it to form a ceramic coating layer (thickness of one layer: 1.5㎛).

[0151] 2. Manufacture of electrode assembly

[0152] The separator reel on which the separator was wound was unwound, and the separator was placed on the table. An adhesive was applied to the separator using a first nozzle in a pattern of multiple spaced-apart dots. Polycarbonate (weight-average molecular weight Mw: 20,000) was used as the first oligomer compound for the adhesive. Subsequently, the anode sheet was unwound from the first electrode reel on which it was wound, and then cut with a first cutter to manufacture the anode. The anode was then transferred to a first transfer device and adsorbed onto a first header. The first header was moved toward the table to attach the anode to the separator.

[0153] Afterwards, the table was moved to the side, and the separator was folded to one side to cover the anode.

[0154] Subsequently, the same adhesive used above was applied to the surface of the separator (the side opposite to the surface where the separator contacts the anode) using a second nozzle in a pattern of multiple spaced-apart dots.

[0155] Afterward, the cathode sheet was unwound from the second electrode reel and cut with a second cutter to manufacture the cathode, and the cathode was transferred to a second transfer device and adsorbed onto a second header. The second header was moved toward the table side to attach the cathode to the surface of the separator (the side opposite to the surface where the separator and the anode come into contact).

[0156] Afterwards, the table was moved to the side again to fold the separator to the other side and cover the cathode.

[0157] By repeating the above process several times, an electrode assembly was manufactured in which 18 basic units, each having a separator / anode / separator / cathode sequentially stacked, were stacked. At this time, the separator was folded in a zigzag shape.

[0158] In this case, for the anode, Li[Ni 0.8 Co 0.1 Mn 0.1An anode slurry was prepared by adding O2, PVdF as a binder, and carbon black as a conductive material to N-methylpyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1.5:1.0, and the anode slurry was applied to both sides of an aluminum current collector as an anode current collector, and then dried and rolled to form an anode active material layer, which was used.

[0159] In addition, for the cathode, a cathode slurry was prepared by adding graphite as a cathode active material, styrene-butadiene rubber as a binder, carbon black as a conductive material, and carboxymethylcellulose (CMC) as a thickener to water as a solvent in a weight ratio of 95.5:2.5:1.0:1.0, and the cathode slurry was applied to both sides of a copper current collector as a cathode current collector, and a cathode active material layer was formed by drying and rolling.

[0161] 3. Preparation of gel polymer electrolyte composition

[0162] The gel polymer electrolyte composition was prepared by mixing a polycarbonate-based oligomer (weight average molecular weight Mw: 20,000) as an oligomer, LiPF6 as a lithium salt, and AIBN (Azobisisobutyronitrile) as a polymerization initiator in a solvent.

[0163] The solvent is a mixture of ethyl carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, the lithium salt is included in the gel polymer electrolyte composition at a concentration of 1.0 M, the oligomer is included in the gel polymer electrolyte composition at 5% by weight, and the polymerization initiator is included in the gel polymer electrolyte composition at 0.6 parts by weight per 100 parts by weight of the oligomer.

[0165] 4. Manufacturing of secondary batteries

[0166] A pouch-type battery case made of aluminum was prepared as the battery case, and an electrode assembly was housed in the receiving space of the battery case.

[0167] Subsequently, the gel polymer electrolyte composition was injected into the battery case housing the electrode assembly. After injecting the gel polymer electrolyte composition, vacuum sealing was performed.

[0168] Upon injection of the gel polymer electrolyte composition, the adhesive present in the electrode assembly was dissolved by the solvent of the gel polymer electrolyte composition.

[0169] Subsequently, the gel polymer electrolyte composition injected into the battery case was cured. The curing was performed by heat treatment at a temperature of 60°C for 5 hours.

[0170] Subsequently, a secondary battery was manufactured by cooling, sealing, and degassing the battery case. The thickness of the secondary battery was 0.8 cm.

[0172] Comparative Example 1

[0173] 1. Manufacture of separator membranes

[0174] The same separator as prepared in Example 1 was used.

[0176] 2. Manufacture of electrode assembly

[0177] An electrode assembly was prepared in the same manner as in Example 1, except that polyvinylidene fluoride (PVdF) was used as the adhesive.

[0179] 3. Preparation of gel polymer electrolyte composition

[0180] A gel polymer electrolyte composition identical to that of Example 1 was prepared.

[0182] 4. Manufacturing of secondary batteries

[0183] A secondary battery was manufactured in the same manner as in Example 1, except that the electrode assembly manufactured above was used. The thickness of the secondary battery was 0.8 cm.

[0185] Comparative Example 2

[0186] 1. Manufacture of separator membranes

[0187] Al2O3 as inorganic particles (average particle size (D 50 A composition for forming a ceramic coating layer was prepared by adding PVdF as a binder and acetone, a solvent, in a weight ratio of 70:30.

[0188] A separator (thickness: 15㎛ = 3㎛+9㎛+3㎛) was prepared by applying the composition for forming the ceramic coating layer to both sides of a polyethylene porous substrate (thickness: 9㎛, average pore diameter: 0.05㎛, porosity: volume%) by gravure coating and drying to form a ceramic coating layer (thickness of one layer: 3㎛).

[0190] 2. Manufacture of electrode assembly

[0191] A plurality of the separators manufactured above were prepared. In addition, a plurality of the same as the anode and cathode manufactured in Example 1 were prepared.

[0192] The first oligomer compound used in Example 1 was applied as an adhesive onto one separator in a pattern of multiple spaced-apart dots. An anode was adhered to the separator. The first oligomer compound was applied onto the anode in a pattern of multiple spaced-apart dots, and another separator was adhered to the anode. Subsequently, the first oligomer compound was applied onto the separator in a pattern of multiple spaced-apart dots, and a cathode was adhered to the separator.

[0193] By repeating the above process, an electrode assembly was manufactured in which 18 basic units, each having a separator / anode / separator / cathode sequentially stacked, were stacked. At this time, the two separators in the basic units are separate separators and are not folded in a zigzag shape as in Example 1.

[0195] 3. Preparation of gel polymer electrolyte composition

[0196] A gel polymer electrolyte composition identical to that of Example 1 was prepared.

[0198] 4. Manufacturing of secondary batteries

[0199] A secondary battery was manufactured in the same manner as in Example 1, except that the electrode assembly manufactured above was used. The thickness of the secondary battery was 0.8 cm.

[0201] Experimental Example

[0202] 1. Resistance Evaluation

[0203] (1) Initial resistance measurement

[0204] In the secondary batteries of Example 1, Comparative Example 1, and Comparative Example 2, the initial resistance value calculated using the voltage change amount (ΔV) measured when discharged for 30 seconds at a rate of 0.33C at 100% SOC is shown in Table 1 below.

[0206] (2) Resistance measurement after 100 charge-discharge cycles

[0207] In the secondary batteries of Example 1, Comparative Example 1, and Comparative Example 2, 100 cycles of charge and discharge were performed under the following charge and discharge conditions. Subsequently, the 100 cycle resistance values ​​calculated using the voltage change amount (ΔV) measured when discharged for 30 seconds at a rate of 0.33C from 100% SOC are shown in Table 1.

[0209] (3) Calculation of resistance growth rate

[0210] The resistance increase rate after 100 charge-discharge cycles was evaluated using the following formula and is shown in Table 1 below.

[0212] Resistance Increase Rate (%) = (100 Cycle Resistance - Initial Resistance) / Initial Resistance × 100

[0214] 2. Life Performance Evaluation

[0215] The secondary batteries of Example 1, Comparative Example 1, and Comparative Example 2 prepared above were charged and discharged for 100 cycles at 45°C under the following conditions, and the capacity retention rate at 100 cycles was evaluated.

[0217] ※ Charging and Discharging Conditions

[0218] Charging: CC / CV mode; 0.33C; 4.2V, 1 / 20C cut-off

[0219] Discharge: CC mode; 0.33C; 2.5V cut-off

[0221] Under the above experimental conditions, the capacity retention rate was defined as the value obtained by dividing the discharge capacity for the 100th cycle by the discharge capacity for the first cycle. The results are shown in Table 1 below.

[0223] 3. Cell stiffness measurement

[0224] Stress values ​​were measured when a downward force of 10 mm / min was applied to the center of each secondary battery using the 3-point bending method to induce a displacement of 2 mm. At this time, a pre-load of 30 gf was applied, the experiment was performed at room temperature, and stress values ​​were measured using a universal testing machine (UTM). The results are shown in Table 1 below.

[0226] 4. Ignition temperature measurement test

[0227] After fully charging the secondary batteries of Example 1, Comparative Example 1, and Comparative Example 2 to 100% SOC, they were placed in a hot box and heated at a rate of 0.5°C / minute to measure the temperature at which ignition began, and this is shown in Table 1.

[0229] Experimental Example 1 Experimental Example 2 Experimental Example 3 Experimental Example 4 Initial resistance (mΩ) 100-cycle resistance (mΩ) Resistance increase rate (%) 100-Cycle Capacity Retention Rate (%) Cell rigidity Ignition temperature (°C) Example 1 2.99 3.15 5.3 98.9 4.46 177 Comparative Example 1 3.05 4.13 35.4 98.9 4.39 178 Comparative Example 2 3.19 3.31 3.8 95.8 6.81 168

[0231] Referring to Table 1, it can be seen that the secondary battery manufactured from Example 1 has low resistance and resistance growth rate, high lifespan characteristics, and excellent thermal stability.

[0232] Meanwhile, the secondary battery of Comparative Example 1 shows a higher resistance and resistance increase rate compared to Example 1. This is thought to be due to the fact that an oligomer compound was not used as the adhesive used in the manufacture of the electrode assembly.

[0233] In addition, the secondary battery of Comparative Example 2 uses a separator containing a large amount of binder and a gel polymer electrolyte together. Accordingly, the secondary battery manufactured in Comparative Example 2 has a much higher resistance and significantly degraded lifespan characteristics compared to the case of Example 1. Meanwhile, in the case of Comparative Example 2, thermal stability is significantly reduced, which appears to be due to the relatively low content of inorganic particles in the separator, which does not sufficiently prevent thermal shrinkage and short circuits of the separator. Explanation of the symbols

[0235] 10: Secondary battery 100: Electrode assembly U: Basic unit 110: First electrode 110a: One end of the first electrode 120: Second electrode 120a: One end of the second electrode 130: Separator 131: Porous substrate 132a, 132b: Ceramic coating layer 140: Applied adhesive 200: Gel polymer electrolyte 300: Battery case 310: Cover 400, 500: Electrode tabs 610: First electrode reel 620: Second electrode reel 630: Separator Reel 700: Table 810: 1st Cutter 820: 2nd Cutter 910: First transfer device 920: Second transfer device 1010: 1st header 1020: 2nd header 1101: First electrode sheet 1201: Second electrode sheet 1110: 1st nozzle 1120: 2nd nozzle

Claims

Claim 1 A step of manufacturing an electrode assembly in which an electrode and a separator are alternately stacked, and an adhesive is applied to the surface of at least one of the electrode and the separator so that the electrode and the separator are bonded to each other; a step of housing the electrode assembly in a battery case; and a step of injecting a gel polymer electrolyte composition into the battery case to impregnate the electrode assembly. A method for manufacturing a secondary battery comprising the step of curing the gel polymer electrolyte composition; wherein the adhesive comprises a first oligomer compound, the separator comprises a porous substrate and a ceramic coating layer disposed on both sides of the porous substrate, the ceramic coating layer comprises 92% by weight or more and less than 100% by weight of inorganic particles and more than 0% by weight or less of a binder, the gel polymer electrolyte composition comprises a lithium salt, an organic solvent, a polymerization initiator, and a second oligomer compound, wherein the first oligomer compound is dissolved in the gel polymer electrolyte composition according to the injection of the gel polymer electrolyte composition, and the first oligomer compound is cured together with the gel polymer electrolyte composition when the gel polymer electrolyte composition is cured. Claim 2 delete Claim 3 A method for manufacturing a secondary battery according to claim 1, wherein the adhesive is applied in the form of a plurality of spaced-apart patterns. Claim 4 A method for manufacturing a secondary battery according to claim 1, wherein the coating area of ​​the adhesive is greater than 0% and less than or equal to 1% with respect to the surface area where the separator and the electrode come into contact. Claim 5 A method for manufacturing a secondary battery according to claim 1, wherein the ceramic coating layer comprises 93% to 98% by weight of inorganic particles and 2% to 7% by weight of a binder. Claim 6 A method for manufacturing a secondary battery according to claim 1, wherein the binder comprises an acrylic binder. Claim 7 A method for manufacturing a secondary battery according to claim 6, wherein the acrylic binder comprises at least one selected from the group consisting of a copolymer of ethylhexyl acrylate and methyl methacrylate; polymethyl methacrylate; polyethylhexyl acrylate; polybutyl acrylate; polyacrylonitrile; and a copolymer of butyl acrylate and methyl methacrylate. Claim 8 A method for manufacturing a secondary battery according to claim 1, wherein the thickness of the ceramic coating layer is 0.1 μm to 10 μm. Claim 9 A method for manufacturing a secondary battery according to claim 1, wherein the thickness of the separator is 1 μm to 20 μm. Claim 10 A method for manufacturing a secondary battery according to claim 1, wherein the first oligomer compound and the second oligomer composition independently comprise at least one selected from the group consisting of fluorine-based oligomers, polycarbonate-based oligomers, and polysiloxane-based oligomers. Claim 11 A method for manufacturing a secondary battery according to claim 1, wherein the electrode comprises a first electrode and a second electrode, and the electrode assembly is manufactured by a method comprising the following steps (a) to (d): (a) applying the adhesive to at least a portion of the separator and the first electrode; (b) bonding the separator and the first electrode through the applied adhesive; (c) folding one side of the separator to cover the first electrode; (d) applying the adhesive to at least a portion of the separator and the second electrode; (e) bonding the separator and the second electrode through the applied adhesive; and (d) folding the other side of the separator to cover the second electrode.

Citation Information

Patent Citations

  • Polymer electrolyte, lithium secondary battery using same, and method for manufacturing lithium secondary battery

    US10135092B2

  • UV or EB cured polymer-bonded ceramic particle lithium secondary battery separators, method for the production thereof

    US20170170441A1

  • Lithium secondary battery and manufacturing method thereof

    US20210043934A1