Method for preparing super absorbent polymer particle
A two-step drying process using a hot air dryer and a heat conduction dryer addresses non-uniform drying in superabsorbent resin manufacturing, enhancing absorption performance and reducing fine powder content.
Patent Information
- Application Number
- KR1020220121702
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2042-09-26
AI Technical Summary
Existing methods for manufacturing superabsorbent resin particles face issues with non-uniform drying, leading to over-drying and increased fine powder generation, which deteriorates the physical properties of the final product.
A two-step drying process using a hot air dryer followed by a heat conduction dryer to maintain pore structure and improve drying uniformity, reducing fine powder content and enhancing the physical properties of the superabsorbent resin particles.
The method ensures high drying uniformity and reduces fine powder generation, thereby improving the absorption performance and physical properties of the superabsorbent resin particles.
Smart Images

Figure 112022101140094-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing superabsorbent resin particles, and more specifically, to a method for manufacturing superabsorbent resin particles with improved drying uniformity and physical properties through two types of dryers. Background Technology
[0002] Super Absorbent Polymer (SAP) is a synthetic polymer material capable of absorbing 500 to 1,000 times its own weight in moisture, and developers name it by different names such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). The above-mentioned super absorbent polymer began to be commercialized for sanitary devices and is currently widely used as a material for horticultural soil repair agents, waterproofing materials for civil engineering and construction, seedling sheets, freshness preservation agents in the food distribution sector, and compresses, and is mainly used in the hygiene product sector, such as diapers and sanitary pads.
[0003] Meanwhile, superabsorbent resin particles can generally be manufactured through polymerization, drying, grinding, and surface crosslinking steps. However, when the drying uniformity decreases during the drying step, over-drying is performed, which leads to a deterioration in physical properties and a large amount of fine powder is generated during the grinding step.
[0004] Therefore, there is a need for a drying method that can achieve high drying uniformity during the drying stage while improving the physical properties of the finally manufactured superabsorbent resin particles and reducing the fine powder content. Prior art literature
[0005] Republic of Korea Published Patent Application No. 10-2011-0136597 The problem to be solved
[0006] The problem to be solved by the present invention is to provide a method for manufacturing superabsorbent resin particles that can perform a drying step with high drying uniformity, reduce the amount of fine powder generated during the grinding step, and secure the physical properties of the final product, the superabsorbent resin particles, in order to solve the problem mentioned in the background technology of the invention. means of solving the problem
[0007] According to one embodiment of the present invention for solving the above problem, the present invention provides a method for manufacturing superabsorbent resin particles comprising the steps of: supplying a composition comprising a water-soluble ethylene-based unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor to polymerize and obtain a hydrogel polymer; drying the hydrogel polymer in a hot air dryer to obtain a primary dried body; drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and grinding the secondary dried body. Effects of the invention
[0008] According to the method for manufacturing superabsorbent resin particles of the present invention, the drying step can be carried out in a first drying step and a second drying step. By performing the first drying step in a hot air dryer, the pores of the dried body can be maintained, and by performing the second drying step in a heat conduction dryer, the uniformity of drying can be improved. Through this, the problem of an undried body being introduced into the subsequent grinding step can be resolved, and the amount of fine powder generated as grinding proceeds can be reduced. In addition, the physical properties of the final superabsorbent resin particles can be improved. Brief explanation of the drawing
[0009] FIG. 1 is a flowchart illustrating a method for manufacturing superabsorbent resin particles according to one embodiment of the present invention. Specific details for implementing the invention
[0010] Terms and words used in the description and claims of the present invention shall not be interpreted as being limited to their ordinary or dictionary meanings, but shall be interpreted in a meaning and concept consistent with the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.
[0011] Hereinafter, the present invention will be described in more detail with reference to FIG. 1 to facilitate understanding of the present invention.
[0012] A method for manufacturing superabsorbent resin particles according to one embodiment of the present invention may include the steps of: supplying a composition comprising a water-soluble ethylene-based unsaturated monomer having at least a portion of neutralized acidic groups, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor to polymerize and obtain a hydrogel polymer; drying the hydrogel polymer in a hot air dryer to obtain a primary dried body; drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and grinding the secondary dried body.
[0013] First, a method for manufacturing superabsorbent resin particles according to one embodiment of the present invention may perform the step of supplying a composition comprising a water-soluble ethylene-based unsaturated monomer having at least some neutralized acidic groups, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor to polymerize and obtain a hydrogel polymer. The composition may include the water-soluble ethylene-based unsaturated monomer, the internal crosslinking agent, and the polymerization initiator as described above, and may additionally include additives such as a thickener, a plasticizer, a preservative stabilizer, and an antioxidant as needed.
[0014] At this time, the above-mentioned water-soluble ethylene-based unsaturated monomer may be (meth)acrylic acid or a salt thereof. For example, if an alkali metal salt is used which is an acrylic acid in which at least a portion of the acrylic acid has been neutralized and / or a sodium salt thereof, superabsorbent resin particles with improved absorbency can be obtained.
[0015] In addition, the above-mentioned water-soluble ethylene-based unsaturated monomers include anionic monomers of maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamide-2-methylpropanesulfonic acid and salts thereof; nonionic hydrophilic-containing monomers of (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and amino group-containing unsaturated monomers of (N,N)-dimethylaminoethyl (meth)acrylate and (N,N)-dimethylaminopropyl (meth)acrylamide and their quaternaries may be used, and the salt of the anionic monomer may be a metal salt, a divalent metal salt, an ammonium salt, or an organic amine salt.
[0016] The above-mentioned water-soluble ethylene-based unsaturated monomer may include at least a portion of neutralized acidic groups. The above-mentioned water-soluble ethylene-based unsaturated monomer including at least a portion of neutralized acidic groups may be prepared by neutralizing the acidic groups of the water-soluble ethylene-based unsaturated monomer using a neutralizing agent. In this case, basic substances such as sodium hydroxide (or caustic soda), potassium hydroxide, and ammonium hydroxide, which can neutralize acidic groups, may be used as the neutralizing agent.
[0017] Meanwhile, the above internal crosslinking agent can play a role in polymerizing by crosslinking the unsaturated bonds of the water-soluble ethylene-based unsaturated monomers described above.
[0018] The above internal crosslinking agent may be a (meth)acrylate-based compound in which the crosslinking reaction proceeds by a Free-Radical Polymerization (FRP) reaction. Specifically, the above internal crosslinking agent may be one or more compounds selected from the group consisting of ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. More specifically, among these, it may be polyethylene glycol di(meth)acrylate.
[0019] Meanwhile, in the above composition, a thermal polymerization initiator or a photopolymerization initiator based on UV irradiation may be used as the polymerization initiator depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by irradiation with ultraviolet rays, and since a certain amount of heat is also generated as the polymerization reaction, which is an exothermic reaction, proceeds, a thermal polymerization initiator may additionally be included.
[0020] The above photopolymerization initiator may be a compound capable of forming radicals by light such as ultraviolet light. The above photopolymerization initiator may be one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Meanwhile, specific examples of acyl phosphine may be diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphineate.
[0021] In addition, as the thermal polymerization initiator, one or more selected from the group of initiators consisting of persulfate-based initiators, azo-based initiators, hydrogen peroxide, and ascorbic acid may be used. Specifically, examples of persulfate-based initiators include sodium persulfate (Na2S2O8), potassium persulfate (k2S2O8), and ammonium persulfate ((NH4)2S2O8).
[0022] Specifically, polymerization methods are broadly classified into thermal polymerization and photopolymerization depending on the polymerization energy source; thermal polymerization can be carried out in a reactor equipped with a stirring shaft such as a kneader, and photopolymerization can be carried out in a reactor equipped with a movable conveyor belt.
[0023] The hydrogel polymer of the present invention can be prepared from a polymerization reaction carried out by supplying a composition comprising a water-soluble ethylene-based unsaturated monomer, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor, wherein the internal crosslinking agent in the composition may be 0.01 to 5 parts by weight per 100 parts by weight of the water-soluble ethylene-based unsaturated monomer. For example, the internal crosslinking agent may be 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.2 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less, relative to 100 parts by weight of the water-soluble ethylene-based unsaturated monomer. If the content of the internal crosslinking agent is excessively low, crosslinking may not occur sufficiently, making it difficult to achieve strength above an appropriate level, and if the content of the upper internal crosslinking agent is excessively high, the internal crosslinking density increases, making it difficult to achieve the desired water retention capacity.
[0024] The composition of the present invention may be prepared in the form of a solution dissolved in a solvent. In this case, a solvent capable of dissolving the aforementioned raw materials may be used. For example, the solvent may be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.
[0025] Next, a step of obtaining superabsorbent resin particles by drying and grinding the hydrogel polymer obtained through the above polymerization reaction may be performed. At this time, in order to increase efficiency when drying the hydrogel polymer, an additional step of chopping (coarse grinding) may be performed. The term 'chopping' may refer to coarse grinding the hydrogel polymer before the drying step, as it is distinguished from the grinding performed in the grinding step described later.
[0026] Specifically, any one selected from the group of grinding machines consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter can be used as the grinder used in the above chopping step.
[0027] Next, a drying step can be performed on the chopped hydrogel polymer as described above. The drying step may include first drying and second drying.
[0028] According to one embodiment of the present invention, a primary dried body can be obtained by primary drying the above-mentioned hydrogel polymer in a hot air dryer. The hot air dryer may be a device that directly evaporates and discharges moisture by applying heat through high-temperature air (hot air) to the moisture of the object to be dried up to a target moisture content. In this specification, the hot air dryer may directly dry the object to be dried with hot air while stirring it by means of a rotating drum, etc. At this time, a kiln dryer, a tube bundle dryer, a rotary dryer, etc., may be used as the hot air dryer, and in the present invention, a rotary dryer may be used.
[0029] The rotary dryer described above may be configured to have a central tube within a rotating drum, and one or more hot air supply tubes attached to the central tube. The hydrogel polymer introduced into the rotary dryer is stirred by the rotation of the rotating drum and may be heated by hot air supplied from one or more hot air supply tubes. Since the hot air comes into direct contact with the hydrogel polymer introduced into the rotary dryer, drying can be performed efficiently and the drying time can be shortened.
[0030] At this time, the temperature of the hot air from the hot air supply pipe in the rotary dryer may be 100 ℃ or higher, 110 ℃ or higher, or 120 ℃ or higher, and 200 ℃ or lower, 190 ℃ or lower, or 180 ℃ or lower.
[0031] In addition, the wind speed of the hot air may be 20 m / s or more, 22 m / s or more, or 24 m / s or more, and 30 m / s or less, 29 m / s or less, or 27 m / s or less. By operating the temperature and wind speed of the hot air inside the rotary dryer within the above ranges to proceed with primary drying, the moisture content of the primary dried body desired in the present invention can be obtained.
[0032] According to one embodiment of the present invention, the moisture content of the primary dried body may be 20 wt% or more, 23 wt% or more, or 25 wt% or more, and 35 wt% or less, 32 wt% or less, or 30 wt% or less. By drying the moisture content of the primary dried body to within the above range, the primary dried body may be fed into the heat conduction type dryer described later without being excessively dried in the hot air type dryer and be dried a second time.
[0033] If the moisture content of the first dried body is less than 20 weight%, the fine powder content of the first dried body may increase excessively. If the moisture content of the first dried body exceeds 35 weight%, the adhesiveness of the first dried body may increase excessively, making it difficult to recover from a hot air dryer. In this case, the moisture content can be measured by a moisture meter (AND MX_50).
[0034] According to one embodiment of the present invention, the primary dried body can be secondarily dried in a heat conduction dryer to obtain a secondary dried body.
[0035] The above-described heat conduction dryer may be a dryer having a jacket structure in which a heat medium (heat medium oil or steam) flows inside, and in which the object to be dried is indirectly heated and dried by receiving thermal energy through conduction from the outside of the jacket. In this specification, the heat conduction dryer may perform indirect drying by stirring the object to be dried using a paddle or screw, etc., of the jacket structure. At this time, depending on the structure and type in which heat transfer occurs, the above-described heat conduction dryer may be a disc dryer, a screw dryer, a paddle dryer, a drum dryer, an agitated dryer, a thin film dryer, etc., and in the present invention, a paddle dryer may be used.
[0036] The paddle dryer described above is equipped with an agitator arranged in a horizontal direction, and the agitator may include one or more paddles. The agitator within the paddle dryer rotates, and a heat source, such as heat transfer fluid or steam, flows into the jacketed paddles, thereby indirectly drying the material to be dried through contact with the paddles and the inner wall surface. Accordingly, the thermal efficiency of the paddle dryer can be maximized through heat conduction by friction.
[0037] Meanwhile, the temperature of the heat medium (heat medium oil or steam) flowing inside the stirrer provided in the paddle dryer and the paddle attached to the stirrer may be 100°C or higher, 110°C or higher, 120°C or higher, or 130°C or higher, and 200°C or lower, 190°C or lower, 180°C or lower, or 170°C or lower. By raising the temperature of the heat medium to within the above range, the temperature of the secondary drying performed in the paddle dryer can be performed within the above range.
[0038] The agitator in the paddle dryer can rotate at 10 rpm or more, 15 rpm or more, 20 rpm or more, or 25 rpm or more, and 50 rpm or less, 45 rpm or less, 40 rpm or less, or 35 rpm or less. At this time, the rpm (rotations per minute) may represent the unit of the number of rotations per minute of the agitator. By rotating the agitator of the paddle dryer within the above range, secondary drying can be performed smoothly, thereby preventing the problem of undried material being introduced into the subsequent grinding step.
[0039] According to one embodiment of the present invention, the moisture content of the secondary dried body may be 8 wt% or more, 10 wt% or more, or 12 wt% or more, and 20 wt% or less, 18 wt% or less, or 16 wt% or less. When the moisture content of the secondary dried body is dried within the above range, it may be possible to achieve a desired level of absorption performance of the finally manufactured superabsorbent resin particles.
[0040] Meanwhile, for example, if the above primary drying or secondary drying is performed in a band-type dryer, the drying uniformity of the object to be dried may be reduced. The band-type dryer may be, for example, a conveyor belt, and such a dryer can dry the object to be dried by loading it onto a conveyor (wire mesh, perforated plate, etc.) and moving it while blowing hot air over it. However, since the object to be dried is not agitated and is dried in the form (such as a block) loaded on the conveyor, a part of the object to be dried (the inside of the block) may remain undried, which may result in over-drying. However, over-drying may reduce the absorption rate (vortex) and absorption performance of the superabsorbent resin particles, and excessive fine powder may be generated during the grinding stage. Therefore, to improve this, a hot-air dryer and a heat conduction dryer that agitate the object to be dried while drying may be used according to one embodiment of the present invention.
[0041] The above-mentioned hot air dryer facilitates the improvement of the absorption rate of the object to be dried by maintaining the pores of the object to be dried through rotation by a rotating drum, etc., but the drying capacity relative to the equipment size is low because the filling level of the object to be dried in the rotating drum of the hot air dryer must be within 15% of the total capacity. In addition, the drying uniformity of the object to be dried by the above-mentioned hot air dryer may be relatively low.
[0042] On the other hand, while the above-mentioned thermal conduction dryer has a high drying capacity and can dry the material to be dried with high drying uniformity, the high shear applied to the material can reduce its porosity. Consequently, the absorption rate (vortex) of the material to be dried may decrease.
[0043] In order to compensate for the disadvantages of the aforementioned hot air dryer and the heat conduction dryer, the hot air dryer and the heat conduction dryer may be connected in series in the present invention. As previously described, by performing primary drying through the hot air dryer, the pores of the hydrogel polymer are maintained, and by performing secondary drying through the heat conduction dryer, the drying uniformity of the secondary dried body can be further improved. By connecting the hot air dryer and the heat conduction dryer in series to perform primary and secondary drying in this manner, it is possible to prevent un-dried material from entering the subsequent grinding stage, and ultimately, it is easier to secure the physical properties of the completed superabsorbent resin particles. At this time, the physical properties of the superabsorbent resin particles may refer to the absorption properties intended for the superabsorbent resin particles, and specifically, may be properties related to absorption such as absorption performance and absorption rate.
[0044] Next, a step of grinding the secondary dried body obtained through the drying steps of the primary and secondary drying as described above may be performed. The grinding step may be performed once, but, for example, may be performed in one or more cycles. According to the present invention, a classification step may be further performed after the grinding step. Furthermore, the classification may be performed after each cycle of grinding.
[0045] For example, a primary grinding process may be carried out to grind the above secondary dried body. Specifically, the grinder used at this time may be a ball mill, pin mill, hammer mill, screw mill, roll mill, disc mill, or jog mill.
[0046] Next, the primary ground material, after the primary grinding is completed, can be classified based on a specific particle size using a standard sieve of ASTM specifications. At this time, the specific particle size may be the reference particle size of the particles classified to perform the secondary grinding described later. Through such classification, the material can be classified into particles smaller than the specific particle size and particles larger than the specific particle size. For example, the primary ground material can be fed into a mesh set and classified based on a #40 mesh into particles corresponding to #40 upper (425 μm or more) and particles corresponding to #40 lower (less than 425 μm).
[0047] Next, secondary grinding can be performed to obtain secondary ground material by separately grinding particles of a specific particle size or larger classified by the primary classification above. At this time, the secondary grinding can be carried out using the same grinder used in the primary grinding.
[0048] After such secondary grinding, secondary classification may be performed to manage the physical properties of the superabsorbent resin particles that are finalized into a product. The secondary classification may utilize the ASTM standard mesh used in the primary classification, and may involve finally classifying a mixture of particles classified below a specific particle size in the primary classification and the secondary ground material from the secondary grinding according to an appropriate particle size. In this case, the appropriate particle size (D50) may be between 150 μm and 850 μm, and particles having such a particle size may be classified as normal particles. Conversely, particles having a particle size of less than 150 μm may be classified as fine particles. These particle sizes may be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 220.3 method.
[0049] Through such a series of grinding steps, normal particles, namely superabsorbent resin particles, can be manufactured.
[0050] Subsequently, if necessary, the method may further include the step of surface-crosslinking the manufactured superabsorbent resin particles in the presence of a surface crosslinking agent to produce superabsorbent resin particles having a surface crosslinking layer formed on at least a portion thereof. At this time, the surface crosslinking layer may be generated from a surface crosslinking agent, wherein the surface crosslinking agent comprises a polyvalent epoxy compound, and the polyvalent epoxy compound may be a glycidyl ether compound of a polyvalent alcohol.
[0051] Specifically, the surface crosslinking agent is ethyleneglycol diglycidyl ether, diethyleneglycol diglycidyl ether, or triethyleneglycol diglycidyl ether.
[0052] It may include one or more polyvalent epoxy compounds selected from the group consisting of triethyleneglycol diglycidyl ether, tetraethyleneglycol diglycidyl ether, glycerin polyglycidyl ether, and sorbitol polyglycidyl ether.
[0053] The surface crosslinking agent may be mixed into the superabsorbent resin particles in a solution state, specifically in the form of a surface crosslinking solution dissolved in a solvent. In addition to the surface crosslinking agent, the surface crosslinking solution may contain water and methanol. Generally, the surface crosslinking solution is applied to the surface of the superabsorbent resin particles. Thus, the surface crosslinking reaction occurs on the surface of the superabsorbent resin particles, which improves the crosslinking ability on the surface of the particles without substantially affecting the interior of the particles. Therefore, surface-crosslinked superabsorbent resin particles have a higher degree of crosslinking near the surface than in the interior. By heating the polymer to which the surface crosslinking agent has been added, the surface crosslinking reaction and drying can occur simultaneously.
[0055] The present invention will be described in more detail below through examples. However, the following examples are intended to illustrate the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the present invention, and the scope of the present invention is not limited only to these examples.
[0057] Examples
[0058] Example 1
[0059] (1) Preparation of a hydrogel polymer
[0060] A composition was prepared by mixing 1000 g of acrylic acid, 1.6 g of polyethylene glycol diacrylate (PEGDA) as an internal crosslinking agent, 0.08 g of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide as a photopolymerization initiator, 1.2 g of sodium persulfate as a thermal polymerization initiator, and 1235 g of caustic soda (NaOH) solution as a neutralizing agent in a 3L glass container equipped with a stirrer and a thermometer, at room temperature so that the solid content was 45.0 wt%.
[0061] Subsequently, the above composition was supplied at a speed of 500 to 2000 mL / min onto a conveyor belt with a width of 10 cm and a length of 2 m, moving at a speed of 10 cm / min. At this time, 10 mW / cm² was supplied simultaneously with the supply of the monomer composition. 2 A polymerization reaction was carried out for 60 seconds by irradiating with ultraviolet light having an intensity of , and after the polymerization reaction was completed, the polymer was crushed with a chopper to obtain a hydrogel polymer with a water content of 65 wt%.
[0063] (2) Manufacture of superabsorbent resin particles
[0064] Next, 1 kg of the above-mentioned hydrogel polymer was supplied to a rotary dryer, and primary drying was carried out until the moisture content of the primary dried body reached 24.9 wt%. At this time, the hydrogel polymer was dried using hot air supplied from the hot air supply pipe of the rotary dryer at a temperature of 100 ℃ and a wind speed of 26 m / s to obtain the primary dried body. At this time, the moisture content was measured by a moisture meter (AND MX_50; heating temperature: 180 ℃, heating time: 40 min).
[0065] Next, the first dried body was introduced into a paddle dryer, and a second drying process was carried out until the moisture content of the second dried body reached 12.0 wt%. At this time, the second drying temperature was also maintained at 105°C through a heat medium of 105°C flowing through an agitator provided in the paddle dryer and the inside of the paddle attached to the agitator, and the agitator in the paddle dryer was rotated at 10 rpm.
[0066] Next, the above secondary dried body was first crushed using a roll mill to obtain a primary crushed material. The primary crushed material was fed into a mesh set (a set composed of meshes #6, #10, #20, #25, #30, #40, #50, #70, and #100), and a primary classification was performed to classify the particles into #40 or larger (425 μm or larger) and particles smaller than #40 (less than 425 μm). The particles larger than #40 (425 μm or larger) classified in the primary classification were secondarily crushed using the same roll mill as in the primary crushing to obtain a secondary crushed material. Finally, the mixture of the particles smaller than #40 (less than 425 μm) classified in the primary classification and the secondary crushed material was secondarily classified to obtain superabsorbent resin particles having a particle size of 150 μm to 850 μm. At this time, the second classification was carried out using the same mesh set as the first classification.
[0068] Example 2
[0069] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 25.5 wt%, and the moisture content of the second dried body was dried until it reached 12.9 wt% (stirrer speed: 30 rpm).
[0071] Example 3
[0072] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 21.9 wt%, and the moisture content of the second dried body was dried until it reached 10.8 wt% (stirrer speed: 50 rpm).
[0074] Example 4
[0075] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 33.6 wt%, and the moisture content of the second dried body was dried until it reached 11.4 wt%.
[0077] Example 5
[0078] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 29.1 wt%, and the moisture content of the second dried body was dried until it reached 11.8 wt% (temperature: 200 ℃).
[0080] Example 6
[0081] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 29.3 wt%, and the moisture content of the second dried body was dried until it reached 7.5 wt% (temperature: 200 ℃, stirrer speed: 50 rpm).
[0083] Example 7
[0084] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 31.4 wt%, and the moisture content of the second dried body was dried until it reached 21.3 wt%.
[0086] Example 8
[0087] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 16.5 wt%, and the moisture content of the second dried body was dried until it reached 10.3 wt%.
[0089] Example 9
[0090] Superabsorbent resin particles were prepared using the same method as in Example 1, except that in Example 1, the moisture content of the first dried body was dried until it reached 37.5 wt%, and the moisture content of the second dried body was dried until it reached 12.9 wt%.
[0092] Comparative Example 1
[0093] Superabsorbent resin particles were prepared using the same method as in Example 1, except that the first drying was performed in a rotary dryer (hot air temperature: 100 ℃, wind speed: 26 m / s) until the moisture content of the first dried body reached 10.2 wt%, and the second drying was not performed.
[0095] Comparative Example 2
[0096] Superabsorbent resin particles were prepared using the same method as in Example 1, except that the first drying was performed in a rotary dryer (hot air temperature: 250 ℃, wind speed: 8 m / s) until the moisture content of the first dried body reached 11.0 wt%, and the second drying was not performed.
[0098] Comparative Example 3
[0099] Superabsorbent resin particles were prepared using the same method as in Example 1, except that the first drying was performed in a paddle dryer (temperature: 105 ℃, stirrer rotation speed: 10 rpm) until the moisture content of the first dried body reached 12.6 wt%, and the second drying was not performed.
[0101] Comparative Example 4
[0102] Superabsorbent resin particles were prepared using the same method as in Example 1, except that the first drying was performed in a paddle dryer (temperature: 200 ℃, stirrer rotation speed: 50 rpm) until the moisture content of the first dried body reached 11.0 wt%, and the second drying was not performed.
[0104] Comparative Example 5
[0105] Superabsorbent resin particles were prepared using the same method as in Example 1, except that the first dried body was dried in a paddle dryer (temperature: 105 ℃, stirrer speed: 10 rpm) until the moisture content of the first dried body was 31.1 wt%, and the second dried body was dried in a rotary dryer (temperature: 100 ℃, wind speed: 26 m / s) until the moisture content of the second dried body was 12.6 wt%.
[0107] Experimental Example
[0108] The results of measuring the superabsorbent resin particles prepared in the above examples to comparative examples using the following method are shown in Tables 1 and 2 below.
[0110] 1) Moisture content
[0111] The moisture content was measured through the weight change resulting from evaporating moisture by heating the primary dried body and the secondary dried body, which were dried first during the manufacturing process of the superabsorbent resin particles of the Examples and Comparative Examples, with a halogen lamp (400 W) inside a moisture meter (AND MX_50). Specifically, the moisture content was measured in the following order.
[0112] ① Set the measurement conditions of the moisture meter (heating temperature: 180 ℃, heating time: 40 min).
[0113] ② Stabilize the weight to zero (0) when there is no sample on the sample pan.
[0114] ③ 5 g (error: 0.02%) of the primary or secondary dry body to be measured is sampled and evenly loaded onto the sample pan.
[0115] ④ Check the moisture content after the measurement is finished.
[0117] 2) Drying uniformity
[0118] Drying uniformity can refer to the uniformity of the moisture content of superabsorbent resin particles according to particle size. Specifically, the drying uniformity of the superabsorbent resin particles prepared by the examples and comparative examples was measured according to Equation 1.
[0119] [Mathematical Formula 1]
[0120]
[0121] At this time, the drying uniformity was measured by sampling 200 g of the final manufactured superabsorbent resin particles. The 200 g of the secondary dried body was placed into a mesh set composed of meshes #6, #10, #20, #25, #30, #40, #50, #70, and #100, and mounted on a sieve shaker. The superabsorbent resin particles were classified by operating the sieve shaker at an amplitude of 1.5 for 10 minutes.
[0122] After separating particles according to the particle size of each mesh, the moisture content of the particles separated as described above was measured using a moisture meter (AND MX_50; heating temperature: 180 ℃, heating time: 40 min). The standard deviation of the moisture content of particles for each particle size is represented as 'Std' in Equation 1.
[0124] 3) Average particle size after drying and average particle size after grinding
[0125] The method for measuring the average particle size after drying was carried out as follows.
[0126] First, the secondary dried body was classified using the same method as the previously described method for measuring 'drying uniformity'. Specifically, the secondary dried body (200 g) in which the secondary drying was completed in the examples and comparative examples was placed into a mesh set composed of meshes #6, #10, #20, #25, #30, #40, #50, #70, and #100, and then classified by mounting it on a sieve vibrator (time: 10 min, amplitude: 1.5). The fraction of the secondary dried body classified by mesh (6, #10, #20, #25, #30, #40, #50, #70, and #100) was analyzed, and the result calculated by arithmetic mean based on the weight fraction for each mesh is the 'average particle size after drying' in Tables 1 and 2.
[0127] Meanwhile, the above 'average particle size after grinding' was measured using the same method as the aforementioned 'average particle size after drying'. However, unlike the 'average particle size after drying' which was measured on a secondary dried body, the 'average particle size after grinding' was measured by classifying a mixture that underwent an additional grinding step (particles smaller than #40 classified in the first classification and secondary ground material from the second grinding).
[0129] 4) Fine content
[0130] In the method for manufacturing superabsorbent resin particles of the above examples and comparative examples, the weight of the mixture (particles of size #40 or smaller classified in the first classification and the second-ground material obtained from the second grinding) was measured before the second classification. Subsequently, after proceeding with the second classification, the weight of fine particles having a particle size of 150 μm or less was measured. The percentage of the weight of the fine particles relative to the weight of the mixture was expressed as the 'fine content'. That is, the fine content may refer to the amount of fine particles contained in the mixture.
[0132] 5) Absorption rate (Vortex)
[0133] The absorption rate of the superabsorbent resin particles of the above examples and comparative examples was measured in the following manner.
[0134] 50 ml of 0.9% brine, maintained at a temperature of 24°C using a graduated cylinder, was added to a 100 ml beaker on a magnetic stirrer. During stirring, the magnetic stirrer was operated at a speed such that the lowest surface (center space) of the vortex generated in the 100 ml beaker touched the magnetic bar. Superabsorbent resin particles (1.99 g to 2.01 g) corresponding to particle sizes #40 to #50 (300 μm to 425 μm) of the superabsorbent resin particles of the above examples and comparative examples were added to the vortex while the time was measured simultaneously. Since viscosity is created by adding the superabsorbent resin particles to the brine as described above, the time measured in seconds until the vortex disappears and the liquid surface becomes horizontal was defined as the 'absorption rate' of the present invention.
[0136] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Drying conditions 1st dryer (drying conditions 1) ) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Rotary (100℃ 26m / s) Primary dry moisture content (wt%) 24.9 25.5 21.9 33.6 29.1 29.3 31.4 16.5 37.5 Secondary dryer (drying conditions 1) ) Paddle (105℃ 10rpm) Paddle (105℃ 30rpm) Paddle (105℃ 50rpm) Paddle (105℃ 10rpm) Paddle (200℃ 10rpm) Paddle (200℃ 50rpm) Paddle (105℃ 10rpm) Paddle (105℃ 10rpm) Paddle (105℃ 10rpm) Secondary drying moisture content (wt%) 12.0 12.9 10.8 11.4 11.8 7.5 21.3 10.3 12.9 Measurement results Drying uniformity (%) 98.3 98.4 98.4 98.5 98.3 98.0 98.3 96.7 98.5 Average particle size after drying 3,472 3,495 3,489 3,497 3,533 3,434 3,671 2,249 3,466 Average particle size after grinding 354 359 354 353 362 346 Unground 345 351 Fine powder content (%) 8.8 9.3 8.9 9.6 8.9 11.3 - 2) 11.8 7.5 Absorption rate (seconds) 21 21 22 21 21 23 - 2) 23 26 1) The drying conditions performed within the dryer are indicated as the temperature and wind speed of the hot air from the hot air supply pipe in the case of a rotary dryer, and the temperature of the heat medium and the rotation speed of the stirrer in the case of a paddle dryer. 2) Since the secondary dried body of Example 7 is in a state where grinding is impossible, the fine powder content and absorption rate could not be measured because the grinding step could not be performed.
[0137] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Drying conditions 1st dryer (drying conditions 1) ) Rotary (100℃, 26m / s) Rotary (250℃, 8m / s) Paddle (105℃, 10rpm) Paddle (200℃, 50rpm) Paddle (105℃, 10rpm) Primary dry moisture content (wt%) 10.2 11.0 12.6 11.0 31.1 Secondary dryer (drying conditions 1) ) - - - - Rotary (100℃, 26m / s) Secondary drying moisture content (wt%) - - - - 12.6 Measurement results Drying uniformity (%) 96.1 95.7 98.6 98.6 98.0 Average particle size after drying 2,176 3,076 2,523 2,568 2,528 Average particle size after grinding 340 389 371 439 373 Fine powder content (%) 12.4 12.5 7.8 6.9 7.9 Absorption rate (seconds) 22 23 26 28 27 1) The drying conditions performed within the dryer are indicated as the temperature and wind speed of the hot air from the hot air supply pipe in the case of a rotary dryer, and the temperature of the heat medium and the rotation speed of the stirrer in the case of a paddle dryer.
[0138] Referring to Tables 1 and 2 above, in the case of an example in which superabsorbent resin particles were prepared by performing primary drying using a rotary dryer and secondary drying using a paddle dryer during the drying step, it was confirmed that the absorption rate was improved by maintaining the pores with the rotary dryer and the drying uniformity was improved with the paddle dryer, thereby reducing the fine content of the superabsorbent resin particles.
[0139] On the other hand, Comparative Example 1 is a superabsorbent resin particle dried using only a rotary dryer until the moisture content of the primary dried body, i.e., the final moisture content, reached 10.2 wt%, and not only was secondary drying not performed, but the drying step was also performed using only one type of dryer. Although Comparative Example 1 performed primary drying to a level similar to the moisture content of the secondary dried body of the Example, it was confirmed that the drying uniformity decreased and the fine powder content increased due to the rotary dryer. Comparative Example 2 performed the drying step using only a rotary dryer as in Comparative Example 1, but the drying was performed with the operating conditions of the rotary dryer changed. By using only a rotary dryer in Comparative Example 2 as well, results similar to Comparative Example 1 were confirmed.
[0140] Meanwhile, Comparative Example 3 consisted of superabsorbent resin particles dried using only a paddle dryer until the moisture content of the primary dried body reached 12.6 wt%. Not only was secondary drying not performed, but the drying step was carried out using only one type of dryer. It was confirmed that the absorption rate was reduced compared to the example where secondary drying was performed using two types of dryers. In other words, it was confirmed that the absorption rate was reduced because stress was generated in the body to be dried due to the high force (shear) applied by the paddles of the paddle dryer, and the pores were reduced due to said stress. Comparative Example 4 carried out the drying step using only a paddle dryer as in Comparative Example 3, but the operating conditions of the paddle dryer were changed. Again, by using only a paddle dryer, results similar to Comparative Example 3 were confirmed.
[0141] Meanwhile, Comparative Example 5 is a superabsorbent resin particle prepared by proceeding the drying step with primary drying using a paddle dryer and secondary drying using a rotary dryer, and the types of primary and secondary dryers were changed compared to the example. As mentioned above, when using a paddle dryer, the pores of the dried body may decrease, which can lower the absorption rate. In Comparative Example 5, by using the paddle dryer first as the primary dryer, the primary dried body with reduced pores could be fed into the rotary dryer, which is the secondary dryer. However, it was confirmed through the reduced absorption rate that the pores of the primary dried body, which had already been reduced in the paddle dryer, were maintained by the rotating drum of the rotary dryer.
Claims
Claim 1 A method for manufacturing superabsorbent resin particles, comprising the steps of: supplying a composition comprising a water-soluble ethylene-based unsaturated monomer having at least some neutralized acidic groups, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor to polymerize and obtain a hydrogel polymer; drying the hydrogel polymer in a hot air dryer to obtain a primary dried body; drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and grinding the secondary dried body, wherein the hot air dryer and the heat conduction dryer are connected in series, and grinding of the primary dried body is not performed before the secondary drying of the primary dried body obtained by the primary drying, and the moisture content of the primary dried body is 21.9 wt% to 29.1 wt%, the hot air dryer is a rotary dryer, and the heat conduction dryer is a paddle dryer. Claim 2 A method for manufacturing superabsorbent resin particles according to claim 1, further comprising the step of chopping the hydrogel polymer before first drying the hydrogel polymer. Claim 3 A method for manufacturing superabsorbent resin particles according to claim 1, further comprising the step of surface crosslinking in the presence of a surface crosslinking agent after the grinding step to form a surface crosslinking layer on at least a portion of the surface. Claim 4 delete Claim 5 delete Claim 6 A method for manufacturing superabsorbent resin particles according to claim 1, wherein the moisture content of the secondary dried body is 8% to 20% by weight. Claim 7 delete Claim 8 A method for manufacturing superabsorbent resin particles according to claim 1, wherein the rotary dryer comprises a central tube and one or more hot air supply tubes attached to the central tube, the temperature of the hot air supplied from the one or more hot air supply tubes is 100 ℃ to 200 ℃, and the wind speed of the hot air is 20 m / s to 30 m / s. Claim 9 A method for manufacturing superabsorbent resin particles according to claim 1, wherein the paddle dryer is equipped with a stirrer, and the stirrer rotates at 10 rpm to 50 rpm. Claim 10 A method for manufacturing superabsorbent resin particles according to claim 1, wherein the water-soluble ethylene-based unsaturated monomer is (meth)acrylic acid or a salt thereof.
Citation Information
Patent Citations
Production of hydrophilic crosslinked polymer
JP1999240914A
Method for manufacturing water-absorbent resins
JP5405304B2
Method for manufacturing absorbent
KR1020190031483A
Method for producing absorbent resin powder and apparatus for producing the same
KR1020190077541A