Binder comprising copolymer, anode for secondary battery comprising the same, secondary battery comprising the anode, and method for polymerizing the copolymer

A water-soluble copolymer with covalent and non-covalent bonds addresses the volume expansion issues in high-silicon anodes, improving adhesion and stability, thereby enhancing the performance and capacity retention of lithium-ion batteries.

KR103045560B1Active Publication Date: 2026-11-10HANSOL CHEM
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
KR1020250160767
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-10-30
Publication Date
2026-11-10
Estimated Expiration
2045-10-30

AI Technical Summary

Technical Problem

Existing binders for high-silicon anodes in lithium-ion batteries fail to adequately address the volume expansion and contraction issues caused by lithium insertion and extraction, leading to reduced conductivity, adhesion, and stability problems, which affect the cycle characteristics and safety of the battery.

Method used

A water-soluble copolymer with a combination of covalent and non-covalent bonds, comprising acrylic acid, acrylonitrile, and acrylamide-based monomer units, is used to form a complex network that enhances adhesion and stability, mitigating volume changes in high-silicon anodes.

Benefits of technology

The copolymer significantly improves the performance and stability of high-silicon anodes by controlling volume expansion and contraction, increasing bonding strength with the current collector, and enhancing capacity retention rates per cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure R1020250160767_ABST
    Figure R1020250160767_ABST
Patent Text Reader

Abstract

The invention relates to a negative electrode slurry, a negative electrode, and a secondary battery comprising an acrylic acid-based monomer unit, an acrylonitrile-based monomer unit, and an acrylamide-based monomer unit, wherein the acrylamide-based monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, and at least one acrylic acid-based monomer unit is ionically bonded with an alkali metal ion, an ammonium ion, or a combination thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a copolymer that can be used as a binder, a slurry containing the same, an electrode, and a secondary battery. Background Technology

[0002] Due to their high energy density, lithium-ion batteries are widely used in the electrical, electronic, telecommunications, and computer industries. Following small lithium-ion batteries for portable electronic devices, their applications are expanding to include high-capacity batteries for hybrid vehicles, electric vehicles (EVs), and energy storage systems (ESS).

[0003] With the expansion of application fields, high energy density, fast charging, and high safety are required for lithium secondary batteries. To meet these requirements, an active material containing a high content of silicon atoms is used as the negative electrode.

[0004] When applying an active material containing silicon atoms that has a higher amount of lithium insertion / extraction compared to conventional carbon-based active materials, an improvement in battery capacity can be expected. Furthermore, when a high-silicon content anode is applied, a larger electrode capacity and improved fast charging characteristics can be expected compared to existing graphite anodes, making it advantageous for EV applications requiring longer driving range and shorter charging times. However, since silicon-containing active materials undergo significant volume changes associated with lithium insertion / extraction, the anode active material layer expands and contracts significantly during charging and discharging.

[0005] As a result, there was a decrease in conductivity between negative electrode active materials or a blockage of the conductive path between the negative electrode active material and the current collector, leading to problems of deterioration in the cycle characteristics and reduced safety of the secondary battery.

[0006] However, various binders developed in the past (PAA, PAA / CMC, Na-PAA, crosslinked PAA, Alginate, PVA, etc.) lack adhesion or have electrodes that are too brittle, resulting in poor durability, and it is difficult to expect a solution to the volume expansion problem mentioned above. In particular, water-soluble binders such as PAA series show a certain level of effectiveness in low-silicon anodes, but in high-silicon anodes, they fail to sufficiently suppress the collapse of the microstructure due to expansion and contraction, so the effect of improving performance and stability is limited.

[0007] Therefore, a new binder is required to solve these problems and simultaneously secure the structural stability and electrochemical performance of high-content silicon anodes. Prior art literature

[0008] Republic of Korea Published Patent Application No. 10-2016-0024921 The problem to be solved

[0009] Accordingly, the present invention aims to control and mitigate the volume expansion and contraction of the anode caused by the deinsertion and insertion of lithium ions in a high-content silicon anode by using a water-soluble copolymer having a combination of covalent and non-covalent bonds, and thereby significantly improve the performance and stability of the battery. Through this, the overall performance of a secondary battery using a high-content silicon anode is to be excellent.

[0010] In addition, the present invention aims to ensure manufacturing process safety by securing dispersion stability and coating uniformity in water-soluble processes through a water-soluble copolymer that forms a complex network in which covalent and non-covalent bonds (ionic bonds, hydrogen bonds, etc.) coexist.

[0011] The present invention aims to provide a slurry composition with excellent binding strength using the copolymer.

[0012] In addition, the present invention aims to provide an electrode (particularly a negative electrode) with excellent performance to which the above-mentioned slurry composition is applied, and a secondary battery having excellent capacity retention rate per cycle including the same.

[0013] However, the problems that this invention seeks to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem

[0014] One aspect of the present invention comprises an acrylic acid-based monomer unit, an acrylonitrile-based monomer unit, and an acrylamide-based monomer unit, and

[0015] The above-mentioned acrylamide-based monomer unit is formed by polymerizing nonionic acrylamide, acrylamide containing a hydroxyl group, acrylamide containing a sulfonic acid group, or a combination thereof, and

[0016] At least one of the above-mentioned acrylic acid series monomer units is ionically bonded with an alkali metal ion, an ammonium ion, or a combination thereof,

[0017] Provides a copolymer.

[0018] Another aspect of the present invention is the copolymer; and

[0019] A cathode active material; comprising

[0020] Provides a cathode slurry.

[0021] Another aspect of this institution is,

[0022] The whole house; and

[0023] A negative electrode active material layer comprising the copolymer formed on the above current collector; comprising

[0024] Provides a negative electrode.

[0025] Another aspect of this institution is,

[0026] including the above cathode,

[0027] Provides a secondary battery. Effects of the invention

[0028] By applying the water-soluble copolymer having the combined effect of covalent and non-covalent bonds of the present invention, volume expansion and contraction in the high-content silicon anode can be controlled and mitigated, thereby significantly improving the performance and stability of the battery.

[0029] It can increase the bonding strength with the negative electrode current collector and improve the capacity retention rate per cycle of a secondary battery using a high silicon content negative electrode. Brief explanation of the drawing

[0030] Figure 1 is a graph showing the capacity retention rate of batteries of Manufacturing Examples 1 to 6 measured by Evaluation Example 3 of the present invention. Figure 2 is a graph showing a comparison of the capacity retention rates of the batteries of Manufacturing Example 1 and Comparative Manufacturing Examples 1 and 2, measured by Evaluation Example 3 of the present invention. Specific details for implementing the invention

[0031] The operation and effects of the invention will be described in more detail below through specific embodiments. However, these embodiments are merely examples of the invention and do not define the scope of the invention.

[0032] Prior to this, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0033] Therefore, it should be understood that the configuration of the embodiments described in this specification is merely one of the most preferred embodiments of the present invention and does not represent all of the technical ideas of the present invention, and that various equivalents and modifications that can replace them may exist at the time of filing this application.

[0034] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0035] In the present specification, "a to b" and "a~b" indicating numerical ranges are defined as ≥ a and ≤ b.

[0037] A copolymer according to one aspect of the present invention comprises an acrylic acid-based monomer unit, an acrylonitrile-based monomer unit, and an acrylamide-based monomer unit, wherein the acrylamide-based monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, and at least one acrylic acid-based monomer unit may ionicly bond with an alkali metal ion, an ammonium ion, or a combination thereof.

[0038] For example, the above acrylamide series monomer unit may be formed by polymerizing acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, hydroxyethyl acrylamide, or a combination thereof.

[0039] In one embodiment, the copolymer is polymerized using a degrading initiator or a water-soluble azo initiator, wherein the degrading initiator is potassium persulfate (K₂S₂O₅), ammonium persulfate ((NH₄)₂S₂O₅), sodium persulfate (Na₂S₂O₅), or a combination thereof, and the water-soluble azo initiator is 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (VA-057), 2,2′-azobis(2-methylpropionamidine) dihydrochloride (V-50). It may be 4,4′-Azobis(4-cyanovaleric acid), ACVA / ACPA, 2,2′-Azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, VA-044, 2,2′-Azobis[2-methyl-N-(2-hydroxyethyl)propionamide], VA-086, or a combination thereof.

[0040] For example, the above-mentioned decomposition initiator may be ammonium persulfate, and the above-mentioned water-soluble azo initiator may be 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (2,2′-Azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, VA-057).

[0041] In one embodiment, the copolymer may comprise 30 to 60 weight% of the acrylic acid-based monomer unit, 30 to 60 weight% of the acrylonitrile-based monomer unit, and 10 to 40 weight% of the acrylamide-based monomer unit, based on 100 weight% of the total copolymer.

[0042] For example, the content of the above acrylic acid-based monomer unit may be 30 to 50 weight%, 40 to 50 weight%, 35 to 45 weight%, or 30 to 45 weight%.

[0043] In addition, for example, the content of the acrylonitrile-based monomer unit may be 30 to 50 weight%, 40 to 50 weight%, 35 to 45 weight%, or 30 to 45 weight%.

[0044] For example, the content of the acrylamide-based monomer unit may be 10 to 30 weight%, 10 to 20 weight%, 20 to 40 weight%, 20 to 30 weight%, or 15 to 25 weight%.

[0045] In addition, when the above-mentioned acrylamide series monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, the content of the nonionic acrylamide may be 0 to 30 weight%, 0 to 25 weight%, 0 to 20 weight%, 0 to 15 weight%, 0 to 10 weight%, or 5 to 15 weight%.

[0046] When the above-mentioned acrylamide series monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, the content of the acrylamide containing a hydroxyl group may be 0 to 30 weight%, 0 to 25 weight%, 0 to 20 weight%, 0 to 15 weight%, 0 to 10 weight%, or 5 to 15 weight%.

[0047] When the above-mentioned acrylamide series monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, the content of the acrylamide containing a sulfonic acid group may be 0 to 30 weight%, 0 to 25 weight%, 0 to 20 weight%, 0 to 15 weight%, 0 to 10 weight%, or 5 to 15 weight%.

[0048] If the content of the above acrylic acid-based monomer unit exceeds the range of the present invention, the hydrophilicity is high, the viscosity of the solution and slurry increases, and processability and dispersibility are significantly reduced, and problems such as reduced cycle life may occur due to reduced electrode coating properties. If it falls below the range of the present invention, the number of ionic or hydrogen bonding sites is reduced, weakening the bonding force with the current collector and active material, which may result in reduced electrode adhesion and problems such as reduced cycle life.

[0049] If the content of the acrylonitrile-based monomer unit exceeds the range of the present invention, polymerization stability is significantly reduced, hydrophilicity is lowered, and adhesion may be reduced due to a decrease in molecular weight; if it falls below the range of the present invention, usability with the negative electrode active material and ion conductivity decrease, which may lead to problems such as reduced cycle life.

[0050] If the content of the above-mentioned acrylamide-based monomer unit exceeds the range of the present invention, the processability of the slurry may be reduced due to excessive polarity and increased viscosity and reduced dispersibility, and if it falls below the range of the present invention, the ionic conductivity and hydrogen bonding may decrease, leading to increased cracking and peeling of the electrode due to reduced adhesion, and problems such as reduced cycle life due to low ionic conductivity may occur.

[0051] In one embodiment, the decomposition-type initiator or water-soluble azo initiator may be used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the total monomer (solid content) during copolymer polymerization.

[0052] For example, the content of a degrading initiator or a water-soluble azo initiator may be 0.01 to 3, 0.01 to 1, 0.1 to 3, 0.1 to 1, 0.1 to 0.5, or 0.1 to 0.3 parts by weight based on 100 parts by weight of the total monomer (solid content).

[0053] If the content of a degradable initiator or a water-soluble azo initiator exceeds the range of the present invention, it may not grow to a sufficient molecular weight to mitigate adhesion and volume expansion, and if it falls below the range of the present invention, the conversion rate may be significantly reduced or the molecular weight may be too large, which may significantly impair workability and processability.

[0054] In one embodiment, the acrylic acid-based monomer unit is formed by polymerizing acrylic acid and (methacrylic) acid, or a combination thereof, and

[0055] The above acrylonitrile-based monomer unit is formed by polymerizing acrylonitrile, methacrylonitrile, or a combination thereof, and

[0056] (i) the nonionic acrylamide of the above acrylamide series monomer unit is formed by polymerizing acrylamide, methacrylamide, N-isopropylacrylamide, N-tert-butylacrylamide, N-dodecylacrylamide, or a combination thereof, and

[0057] (ii) The acrylamide containing the hydroxyl group is formed by polymerizing N-(hydroxymethyl)acrylamide, N-(hydroxyethyl)acrylamide, N-(2-hydroxypropyl)acrylamide, 2-hydroxyethyl methacrylamide, or a combination thereof, and

[0058] (iii) The acrylamide containing the sulfonic acid group may be formed by polymerizing 2-acrylamido-2-methylpropane sulfonic acid (AMPS).

[0059] In one embodiment, the copolymer may include repeating units represented by the following chemical formula 1.

[0060] [Chemical Formula 1]

[0061]

[0062] In the above chemical formula 1,

[0063] R1 is each independently hydrogen, a linear or branched hydrocarbon having 1 to 10 carbon atoms, or a combination thereof, and

[0064] R2 is hydrogen, alkali metal ions, ammonium ions, or a combination thereof, and

[0065] R3 is each independently hydrogen, a saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms, a saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms substituted with a hydroxyl group (-OH), a sulfonic acid group (-SO₃H), or an acyl group (-CO-R4), or a combination thereof.

[0066] The R4 of the above acyl group (-CO-R4) is a linear or branched hydrocarbon group having 1 to 8 carbon atoms, and

[0067] a+b+c=1.

[0068] The hydrocarbon group of the above R3 may be a linear or branched hydrocarbon, and may be a saturated or unsaturated hydrocarbon.

[0069] For example, the above R3 is -CH3, -CH2OH, -CH2CH3, -CH2CH2OH, -CH2CH2CH2CH3, -C(C H3)2-(CH3)2CCH2SO3H, -C6H5, -C6H 11 It may be -CH2CHCH3OH, -C(CH3)2-(CH3)2CCH2COCH3 or a combination thereof.

[0070] For example, 0.3 ≤ a ≤ 0.6, 0.1 ≤ b ≤ 0.4, and 0.3 ≤ c ≤ 0.6.

[0071] The above hydrocarbon group includes a linear, branched, or cyclic structure, and the cyclic structure encompasses both alicyclic and aromatic groups and may be saturated or unsaturated.

[0072] In one embodiment, R1 of Formula 1 is each independently selected from the group consisting of hydrogen, methyl, ethyl, n-propyl, and iso-propyl, and

[0073] R2 of Chemical Formula 1 above is independently hydrogen, lithium ion (Li + ), sodium ions (Na + ), potassium ions (K + ) or ammonium ions (NH4 + It is any one selected from the group consisting of ),

[0074] R3 of the above chemical formula 1 is each independently hydrogen, methyl, ethyl, n-propyl, iso-propyl, n-butyl, iso-butyl, sec-butyl, tert-butyl, n-pentyl, allyl, phenyl, cyclohexyl, hydroxymethyl, 2-hydroxyethyl, 1-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, 4-hydroxybutyl, methylsulfonic group, ethylsulfonic group, propylsulfonic group, butylsulfonic group, Isopropylmethylsulfonic group, isobutylmethylsulfonic group, sec-butylmethylsulfonic group, tert-butylmethylsulfonic group, tert-butylethylsulfonic group, (2,2,3,3-tetramethylpropyl)methylsulfonic group, methyl acetyl group, ethyl acetyl group, propyl acetyl group, butyl acetyl group, isopropylmethyl acetyl group,It is any one selected from the group consisting of isobutylmethylacetyl group, sec-butylmethylacetyl group, tert-butylmethylacetyl group, and (2,2,3,3-tetramethylpropyl)methylacetyl group, and

[0075] R4 of the above chemical formula 1 is each independently from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl (2-methylpropyl), tert-butyl (1,1-dimethylethyl), n-pentyl, isopentyl (3-methylbutyl), neopentyl (2,2-dimethylpropyl), n-hexyl, 2-methylpentyl, 3-methylpentyl, n-heptyl, 2-methylhexyl, 3-methylhexyl, n-octyl, and 2-ethylhexyl It can be any one of the selected ones.

[0076] For example, R4 of the above chemical formula 1 may each be independently selected from the group consisting of methyl, ethyl, n-propyl, and iso-propyl.

[0077] In addition, for example, R2 of the above chemical formula 1 may each be independently selected from the group consisting of hydrogen, lithium ions (Li), sodium ions (Na), and potassium ions (K).

[0078] For example, R3 of the above chemical formula 1 is each independently hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, allyl, phenyl, cyclohexyl, hydroxymethyl, 2-hydroxyethyl, 1-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, (2,2,3,3-tetramethylpropyl)methylsulfonic group, It may be any one selected from the group consisting of (2,2,3,3-tetramethylpropyl)methylacetyl groups.

[0079] In addition, for example, R4 of the above chemical formula 1 may be 2,2,3,3-tetramethylpropyl.

[0080] The repeating units represented by the above chemical formula 1 can be cross-linked with each other.

[0081] For example, the repeating unit represented by the above chemical formula 1 can be cross-linked to each other by covalent bonds with adjacent chains.

[0082] For example, monomers that can be crosslinked to each other by covalent bonds with adjacent chains may include N,N′-methylenebisacrylamide, polyethylene glycol diacrylate, or a combination thereof.

[0083] In one embodiment, when the copolymer comprises 30 to 60 weight% of acrylic acid (AA) and 30 to 60 weight% of acrylonitrile (AN), based on 100 weight% of the total copolymer, and comprises 10 to 40 weight% of acrylamide (MAM) as a functional monomer, the counter ion is K + or Na + It could be.

[0084] In one embodiment, when the copolymer comprises 30 to 60 weight% of acrylic acid (AA) and 30 to 60 weight% of acrylonitrile (AN) based on 100 weight% of the total copolymer, and comprises 10 to 40 weight% of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) as a functional monomer, the counter ion is K + It could be.

[0085] In one embodiment, when the copolymer comprises 30 to 60 weight% of acrylic acid (AA) and 30 to 60 weight% of acrylonitrile (AN) based on 100 weight% of the total copolymer, and comprises 10 to 40 weight% of hydroxyethyl acrylamide (N-(hydroxyethyl)acrylamide; 2-hydroxyethyl acrylamide, HEMAM) as a functional monomer, the counter ion is K + It could be.

[0086] In one embodiment, based on 100% by weight of the total copolymer, the copolymer comprises 30 to 60% by weight of acrylic acid (AA) and 30 to 60% by weight of acrylonitrile (AN), and as functional monomers, comprises 0 to 30% by weight of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 0 to 30% by weight of hydroxyethyl acrylamide (N-(hydroxyethyl)acrylamide; 2-hydroxyethyl acrylamide, HEMAM), wherein the counter ion is Li + or K + It could be.

[0087] In one embodiment, the copolymer may have a viscosity of 3,000 to 11,000 cps at 25°C.

[0088] For example, the viscosity may be 3,500 to 11,000 cps, 3,500 to 10,000 cps, 4,000 to 11,000 cps, 4,000 to 10,000 cps, or 4,000 to 8,000 cps.

[0089] If the above viscosity exceeds the range of the present invention, the viscosity of the slurry increases, which may significantly degrade battery performance due to reduced coating properties and non-uniformity of the electrode surface, and if it falls below, it may significantly degrade battery performance because it fails to mitigate the adhesion and volume expansion of the negative electrode active material caused by the low molecular weight.

[0090] In one embodiment, the copolymer may have a conversion rate of 70 to 90%. For example, the conversion rate may be 75 to 90%, or 80 to 90%.

[0091] If the above conversion rate falls below the range of the present invention, battery performance may be significantly degraded due to side reactions within the battery caused by residual substances.

[0092] In one embodiment, the copolymer may have a pH of 6 to 8. For example, the pH may be 6.5 to 7.5, 6.5 to 7, 7 to 7.5, or 7.

[0093] In one embodiment, the copolymer may have a solid content of 5 to 10% based on the total monomer. For example, the solid content may be 5 to 8%, 6 to 9%, 6 to 8%, or 6 to 7%.

[0094] If the solid content of the above copolymer exceeds the range of the present invention, processability may be significantly reduced, and if it falls below, non-uniform coating may occur due to low viscosity during slurry preparation.

[0095] In one embodiment, the copolymer may be a random or block copolymer.

[0096] In addition, the number average molecular weight of the copolymer may be 10,000 g / mol or more and 2,000,000 g / mol or less.

[0097] The number average molecular weight was measured by Gel filtration chromatography (GFC) using water and a mixed solution of 0.2 M NaNO₃ and 0.01 M NaH₂PO₄ as solvents.

[0098] A cathode slurry according to another aspect of the present invention may include the copolymer and the cathode active material.

[0099] That is, the above copolymer can be used as a binder for the cathode.

[0100] The peel strength between the cathode active material layer formed using the above cathode slurry and the copper current collector may be 9 gf / cm or more, and preferably 9.5 g / cm or more.

[0101] The above-mentioned cathode active material may be a compound comprising one or more selected from the group consisting of carbon-based materials, silicon, alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, and rare earth elements, and preferably may be silicon or a compound containing silicon.

[0102] The above carbon-based material may include, for example, artificial graphite, natural graphite, hard carbon, soft carbon, etc., but is not limited thereto. The above silicon-containing cathode active material is not particularly limited in type as long as it is silicon or a silicon-containing compound, but preferably Si, SiO x (0 <x<2), Si-Y 합금(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 또는 이들의 조합이며, Si은 아님.) 및 Si-C 복합체로 이루어진 군으로부터 선택되는 1종 이상일 수 있다.

[0103] The above-mentioned negative electrode active material may be included in an amount of 50 to 90 weight%, preferably 60 to 80 weight%, based on the total weight of the negative electrode active material layer.

[0104] If the above negative electrode active material is included in an amount of less than 50 weight%, the energy density decreases, making it impossible to manufacture a high-energy-density battery, and if it exceeds 90 weight%, the content of the conductive material and binder decreases, resulting in reduced electrical conductivity and reduced adhesion between the electrode active material layer and the current collector.

[0105] Meanwhile, the copolymer may be included in an amount of 5 to 20 weight%, preferably 5 to 15 weight%, based on the total weight of the negative electrode active material layer. If the copolymer is less than 5 weight%, the physical properties of the negative electrode may deteriorate, causing the negative electrode active material and conductive material to detach, and if it exceeds 20 weight%, the ratio of the negative electrode active material and conductive material may decrease relatively, which may reduce the battery capacity and lower the electrical conductivity of the negative electrode.

[0106] In addition, the cathode slurry may further include a polymer in addition to the copolymer of the present invention. Specifically, the polymer may include, but is not limited to, polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polyacrylic acid (PAA), metal polyacrylate salt (Metal-PAA), polymethacrylic acid (PMA), polymethyl methacrylate (PMMA), polyacrylamide (PAM), polymethacrylamide, polyacrylonitrile (PAN), polymethacrylonitrile, polyimide (PI), chitosan, starch, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, hydroxypropylcellulose, regenerated cellulose, and various copolymers thereof.

[0108] A cathode according to another aspect of the present invention may include a current collector and a cathode active material layer comprising a copolymer of the present invention formed on the current collector.

[0109] The above-mentioned negative electrode active material layer may additionally include a conductive material. The conductive material is used to further enhance the conductivity of the negative electrode active material. Such conductive material is not particularly limited as long as it possesses conductivity without causing chemical changes in the battery, and examples may include graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as carbon fluoride, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; polyphenylene derivatives, etc.

[0110] The conductive material may be included in an amount of 5 to 30 weight%, preferably 15 to 25 weight%, based on the total weight of the negative electrode active material layer. If the conductive material is included in an amount of less than 5 weight%, the electrical conductivity of the negative electrode is reduced. If it exceeds 30 weight%, the ratio of silicon-based negative electrode active material to binder decreases relatively, resulting in a decrease in battery capacity. Furthermore, since the content of the binder must be increased to maintain the negative electrode active material layer, the content of the negative electrode active material decreases, making it impossible to manufacture a high-energy-density battery.

[0111] The cathode of the present invention has a cathode active material layer that includes the copolymer of the present invention, which can suppress the volume expansion of the cathode active material that occurs during charging and discharging of a secondary battery and can improve the capacity retention rate per cycle.

[0112] The above cathode can be manufactured through the steps of (a) preparing a composition for forming a cathode active material layer comprising a cathode active material and a copolymer of the present invention, and (b) applying the composition for forming a cathode active material layer onto a cathode current collector and then drying.

[0113] The above composition for forming a negative electrode active material layer is prepared in the form of a negative electrode slurry, and the solvent for preparing the slurry state should be easy to dry and should be able to dissolve the copolymer binder of the present invention well, while keeping the negative electrode active material in a dispersed state without dissolving it.

[0114] The solvent according to the present invention may be water or an organic solvent, and the organic solvent may be one or more organic solvents selected from the group consisting of methylpyrrolidone, dimethylformamide, isopropyl alcohol, acetonitrile, methanol, ethanol, and tetrahydrofuran.

[0115] The above composition for forming the cathode active material layer can be mixed by stirring in a conventional manner using a conventional mixer, such as a rate mixer, a high-speed shear mixer, a homo mixer, etc.

[0116] The above step (b) is a step of manufacturing a negative electrode for a lithium secondary battery by applying the composition for forming a negative electrode active material layer prepared in step (a) onto a negative electrode current collector and drying it.

[0117] The above-mentioned cathode current collector may specifically be selected from the group consisting of copper, stainless steel, titanium, silver, palladium, nickel, alloys thereof, and combinations thereof. The stainless steel may be surface-treated with carbon, nickel, titanium, or silver, and an aluminum-cadmium alloy may be used as the alloy. In addition, calcined carbon, a non-conductive polymer surface-treated with a conductive material, or a conductive polymer may be used.

[0118] The composition for forming a negative electrode active material layer prepared in step (a) above is applied onto a negative electrode current collector, and the current collector can be coated with an appropriate thickness according to the thickness to be formed, preferably within the range of 10 to 300 μm.

[0119] At this time, there are no limitations on the method of applying the above-mentioned slurry-type composition for forming a negative electrode active material layer, and it can be manufactured by performing, for example, doctor blade coating, dip coating, gravure coating, slit die coating, spin coating, comma coating, bar coating, reverse roll coating, screen coating, cap coating, etc.

[0120] A negative electrode for a secondary battery (especially a lithium secondary battery) can be manufactured by drying after coating to finally form a negative electrode active material layer.

[0121] In one embodiment, the peel strength (adhesion strength) of the cathode may be 13 gf / cm or more.

[0122] For example, it may be 13 gf / cm to 30 gf / cm, 13 gf / cm to 25 gf / cm, 13 gf / cm to 20 gf / cm, or 13 gf / cm to 15 gf / cm.

[0123] A battery according to another aspect of the present invention may include a negative electrode comprising a current collector and a negative active material layer comprising a copolymer of the present invention formed on the current collector.

[0124] The above battery may be a secondary battery (in particular, a lithium secondary battery) comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0125] The composition of the positive electrode, separator, and electrolyte of the above-mentioned lithium secondary battery is not specifically limited in the present invention and follows what is known in the art.

[0126] The positive electrode includes a positive active material formed on the positive electrode current collector.

[0127] The positive current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In this case, the positive current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric having fine irregularities formed on its surface to increase adhesion with the positive active material.

[0128] Any cathode active material available in the relevant technical field may be used as the cathode active material constituting the cathode active material layer. Specific examples of such cathode active materials include lithium metal; lithium cobalt-based oxides such as LiCoO2; Li 1+x Mn 2-xLithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxides such as Li2CuO2; vanadium oxides such as LiV3O8, LiFe3O4, V2O5, Cu2V2O7, etc.; LiNi 1-x M x Lithium nickel-based oxide represented by O2 (where M=Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x=0.01 to 0.3); LiMn 2-x M x Lithium manganese composite oxide represented by O2 (where M=Co, Ni, Fe, Cr, Zn, or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (where M=Fe, Co, Ni, Cu, or Zn); Li(Ni a Co b Mn c Examples include lithium-nickel-manganese-cobalt oxides represented by )O2 (where 0<a<1, 0<b<1, 0<c<1, a+b+c=1); sulfur or disulfide compounds; phosphates such as LiFePO4, LiMnPO4, LiCoPO4, LiNiPO4; Fe2(MoO4)3, but are not limited to these.

[0129] At this time, the positive active material layer may additionally include a binder, a conductive material, a filler, and other additives in addition to the positive active material, and the conductive material is the same as that described above for the negative electrode of the lithium secondary battery.

[0130] In addition, the binder may include, but is not limited to, polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polyacrylic acid (PAA), polymethacrylic acid (PMA), polymethyl methacrylate (PMMA), polyacrylamide (PAM), polymethacrylamide, polyacrylonitrile (PAN), polymethacrylonitrile, polyimide (PI), chitosan, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof.

[0131] The above-mentioned separator may be made of a porous substrate, and any porous substrate typically used in electrochemical devices may be used; for example, a polyolefin-based porous membrane or a nonwoven fabric may be used, but is not specifically limited thereto.

[0132] The above separator may be a porous substrate composed of any one selected from the group consisting of polyethylene, polypropylene, polybutylene, polypentene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate, or a mixture of two or more of these.

[0133] The electrolyte of the above-mentioned lithium secondary battery is a non-aqueous electrolyte containing a lithium salt, composed of a lithium salt and a solvent, and the solvent used is a non-aqueous organic solvent, an organic solid electrolyte, and an inorganic solid electrolyte.

[0134] The above lithium salt is a substance that dissolves well in the above-mentioned non-aqueous electrolyte, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl10 LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiC4BO8, LiCF3CO2, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiN(SO2F)2, LiN(SO2C2F5)2, LiC4F9SO3, LiC(CF3SO2)3, (CF3SO2)·2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate imide, etc. may be used.

[0135] Non-aqueous organic solvents are, for example, N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydroxyfranc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, Aprotic organic solvents such as tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate may be used.

[0136] The above organic solid electrolyte may be, for example, a polyethylene derivative, a polyethylene oxide derivative, a polypropylene oxide derivative, a phosphate ester polymer, agitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, a polymer containing a secondary dissociating group, etc.

[0137] As the above-mentioned inorganic solid electrolyte, for example, nitrides, halides, sulfates of Li such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, Li3PO4-Li2S-SiS2, etc., may be used.

[0138] In addition, non-aqueous electrolytes may further include other additives for the purpose of improving charge / discharge characteristics, flame retardancy, etc. Examples of the above additives include pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphate trialamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propene sulfone (PRS), vinylene carbonate (VC), etc.

[0139] The lithium secondary battery according to the present invention enables lamination, stacking, and folding processes of the separator and electrode in addition to the general winding process. Furthermore, the battery case may be cylindrical, prismatic, pouch-type, or coin-type.

[0140] In one embodiment, the capacity retention rate of the secondary battery may be 81.8% or higher when charging and discharging is repeated 300 cycles.

[0141] For example, the above capacity retention rate may be 81.8 to 99%, 81.8 to 95%, or 81.8 to 90%.

[0142] In one embodiment, even after repeating the charge and discharge cycles 300 times, the cathode surface may not show any delamination.

[0144] The present invention will be explained in more detail below using examples, but the present invention is not limited thereto.

[0146] Preparation Example 1. Preparation of a polymer for a binder

[0147] 1,000 to 1,300 parts by weight of distilled water were added to a reaction vessel, and the temperature was raised to 65°C while injecting high-purity nitrogen gas to generate internal bubbles.

[0148] 100 parts by weight of a monomer mixture aqueous solution (solid content 15-30%) were added to a reaction vessel. A decomposition initiator (ammonium persulfate) or a water-soluble azo initiator 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (VA-057) was added at a concentration of 0.1-0.3 parts by weight based on 100 parts by weight of the monomer (solid content). Additionally, a crosslinking monomer was added at a concentration of 0.1-1 part by weight based on 100 parts by weight of the monomer (solid content), and continuous solution polymerization was carried out for at least 10 hours. After polymerization, residual monomers were removed by vacuum purification to produce a copolymer.

[0149] The carboxylic acid group was ionized by adding an aqueous solution of an alkali metal hydroxide (NaOH, LiOH, KOH, etc.) or an aqueous solution of ammonia / amine (primary, secondary, tertiary) to adjust the pH to 7.

[0150] The composition of the above monomer was set by appropriately adjusting the content of (meth)acrylic acid (M)AA, (meth)acrylonitrile (M)AN, acrylamide (MAM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS), and hydroxyethyl acrylamide (HEMAM).

[0152] [Example 1]

[0153] A copolymer was prepared by reacting 40 parts by weight of acrylic acid, 40 parts by weight of acrylonitrile, and 20 parts by weight of acrylamide based on 100 parts by weight of monomer (solid content), and using potassium hydroxide as an alkali metal hydroxide.

[0155] [Example 2]

[0156] A copolymer was prepared in the same manner as in Example 1, except that the above alkali metal hydroxide was changed to sodium hydroxide.

[0158] [Example 3]

[0159] A copolymer was prepared in the same manner as in Example 1, except that the acrylamide (MAM) was changed to 2-acrylamido-2-methylpropanesulfonic acid (AMPS).

[0161] [Example 4]

[0162] A copolymer was prepared in the same manner as in Example 1, except that the acrylamide (MAM) was changed to hydroxyethyl acrylamide (HEMAM).

[0164] [Example 5]

[0165] A copolymer was prepared in the same manner as in Example 1, except that 20 parts by weight of the acrylamide (MAM) were replaced with 10 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 10 parts by weight of hydroxyethyl acrylamide (HEMAM), and the alkali metal hydroxide was replaced with lithium hydroxide.

[0167] [Example 6]

[0168] A copolymer was prepared in the same manner as in Example 1, except that 20 parts by weight of the acrylamide (MAM) were replaced with 10 parts by weight of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and 10 parts by weight of hydroxyethyl acrylamide (HEMAM).

[0170] [Comparative Example 1]

[0171] A copolymer was prepared in the same manner as in Example 1, except that the above alkali metal hydroxide was changed to lithium hydroxide.

[0173] [Comparative Example 2]

[0174] A copolymer was prepared in the same manner as in Example 1, except that the acrylic acid was changed to 60 parts by weight and the acrylonitrile to 20 parts by weight.

[0176] Table 1 below shows the composition and counter ion of the copolymers of Examples 1 to 6 and Comparative Examples 1 and 2.

[0177] In Table 1 below, AN, AA, MAM, AMPS, and HEMAM correspond to acrylonitrile (AN), acrylic acid (AA), acrylamide (MAM), 2-acrylamido-2-methylpropane sulfonic acid (AMPS), and hydroxyethyl acrylamide (N-(hydroxyethyl)acrylamide; 2-hydroxyethyl acrylamide, HEMAM), respectively.

[0179]

[0181] Preparation Example: Preparation of cathode slurry, cathode, and battery

[0182] A cathode slurry was prepared by mixing 65 parts by weight of graphite as a cathode active material, 1.6 parts by weight of the copolymer of Examples 1 to 6 and Comparative Examples 1 and 2, 30 parts by weight of silicon-carbon composite (Si-C), 2.4 parts by weight of styrene-butadiene rubber copolymer (SBR), 0.5 parts by weight of carboxymethylcellulose (CMC), and 0.5 parts by weight of carbon nanotubes (CNT) with triple distilled water.

[0183] The cathode slurry prepared above was uniformly coated onto a Cu thin film with a thickness of 10 μm using an applicator, and then dried at a temperature of 120°C for 10 minutes. The resulting dried mixture was rolled to a thickness of 57–60 μm using a roll press to achieve a compression density of 1.7 g / cm³, and then dried in a vacuum at 120°C for 4 hours to produce a high-content silicon cathode.

[0184] A positive electrode was prepared by mixing lithium nickel-manganese cobalt oxide as the positive active material, acetylene black as the conductive material, and polyvinylidene fluoride (PVDF) as the positive binder in a weight ratio of 92:4:4 and coating it onto an aluminum collector.

[0185] The cathode used was the cathode manufactured above.

[0186] The electrolyte was prepared by dissolving LiPF61M in a non-aqueous solvent of ethylene carbonate (EC): ethylmethyl carbonate (EMC): diethyl carbonate (DEC) = 3:5:2 (volume ratio) and using a composition containing 1.0% vinylene carbonate (VC) as an additive.

[0187] For the separator, a porous polyethylene film with a thickness of 18 μm was used, coated on both sides with an electrode adhesive layer and a ceramic heat-resistant layer.

[0188] The secondary battery was formed by winding, laminating, stacking, and aligning the positive electrode, separator, and negative electrode into a pouch shape, and then packaging it in an aluminum composite. After injecting the electrolyte, it was vacuum-sealed and left to stand at room temperature for 12 hours. Subsequently, a first formation process was performed at 0.1 C, and the generated gas was degassed. Then, the second and third formation processes were carried out to manufacture the battery.

[0189] Table 2 below shows the types of copolymers used for each battery.

[0191] Copolymer used Preparation Example 1 Example 1 Preparation Example 2 Example 2 Preparation Example 3 Example 3 Preparation Example 4 Example 4 Preparation Example 5 Example 5 Preparation Example 6 Example 6 Comparative Manufacturing Example 1 Comparative Example 1 Comparative Manufacturing Example 2 Comparative Example 2

[0193] [Evaluation Example]

[0194] Evaluation Example 1: Characteristics of the copolymer

[0195] The conversion rate was calculated as a percentage of the ratio of residual monomer to initial monomer, and the results are shown in Table 3 below.

[0196] Viscosity was measured using a Brookfield rotary cup viscometer (spindle SC4-34). Viscosity was measured at 25°C, and after maintaining the temperature for 30 minutes, the rotation speed was set to 50% torque to measure the stabilized indication. The measurement results are shown in Table 3 below.

[0197] pH was measured repeatedly using a pH meter, and the average value was calculated and the results are shown in Table 3 below.

[0198] The solid content was calculated using the loss on drying method, and the results are shown in Table 3 below.

[0199] At this time, the solid content was calculated according to the following mathematical formula 1.

[0201] [Mathematical Formula 1]

[0202] Solid content [%] = [Mass of solids remaining after drying / Total mass of sample added initially] x 100

[0204] Conversion rate (%) Viscosity (cps@25℃) pH Solids (%) Example 1 80 8,000 7 6 - 7 Example 2 90 10,000 7 6 - 7 Example 3 80 4,000 7 6 - 7 Example 4 80 4,000 7 6 - 7 Example 5 90 8,000 7 6 - 7 Example 6 90 7,000 7 6 - 7 Comparative Example 1 80 13,000 7 6 - 7 Comparative Example 2 80 12,000 7 6 - 7

[0206] As a result of measurement, as shown in Table 3 above, the conversion rate of the copolymer (binder) prepared in Examples 2, 5, and 6 was high at 90%, while the copolymers prepared in the remaining examples and comparative examples were all 80%.

[0207] It was confirmed that the copolymers prepared in Examples 3 and 4, in which AMPS or HEMAM was introduced alone, had the lowest viscosity at 25 °C at 4,000 cps, indicating the best slurry workability. Additionally, when AMPS and HEMAM were introduced in combination, it was confirmed that the viscosity (at 25 °C) of the copolymer prepared in Example 6 was 7,000 cps, which was lower than that of the copolymer prepared in Example 5.

[0208] In contrast, the copolymers prepared in Comparative Examples 1 and 2 had viscosity ranges of 13,000 cps and 12,000 cps, respectively, so it was confirmed that the processability was poor.

[0209] From the perspective of ionic resistance, it was confirmed that the case using K (Examples 1, 3, 4, 6) showed overall lower viscosity than the case using Na (Example 2) or Li (Comparative Example 1).

[0210] In other words, it was confirmed that the effect of the composition (introduction of AMPS / HEMAM, AA:AN ratio) on viscosity was greater than the effect of the anti-ion alone.

[0211] Meanwhile, pH and solid content were the same at pH 7 and 6–7%, respectively, under all conditions.

[0213] Evaluation Example 2: Measurement of Electrode Adhesion (UTM)

[0214] A specimen was prepared by cutting the cathodes of Preparation Examples 1 to 6 and Comparative Preparation Examples 1 and 2, which were prepared using the copolymers of Examples 1 to 6 and Comparative Examples 1 and 2, into pieces 25 mm wide and 100 mm long.

[0215] A double-sided tape with a width of 20 mm and a length of 40 mm was attached to a acrylic plate with a width of 40 mm and a length of 100 mm. After attaching the prepared electrode to the double-sided tape, it was lightly pressed 5 times with a hand roller and mounted on a universal testing machine (UTM) (20 kgf Load cell). After peeling off approximately 25 mm of one side of the cathode, the cathode was fixed to the upper clip of the universal testing machine (UTM), and the tape attached to one side of the cathode was fixed to the lower clip. The electrode was then peeled off at a speed of 100 mm / min, and the force of the electrode falling in the 180° direction was measured. At least 5 specimens were prepared and measured per sample, and the average value was calculated. The results are shown in Table 4 below.

[0217] cathode Electrode adhesion (gf / cm) (UTM) Preparation Example 1 15.0 Preparation Example 2 13.0 Preparation Example 3 14.2 Preparation Example 4 14.9 Preparation Example 5 15.0 Preparation Example 6 14.5 Comparative Manufacturing Example 1 12.6 Comparative Manufacturing Example 2 10.9

[0219] As a result of the measurement, as shown in Table 4 above, it was confirmed that the cathodes of Preparation Examples 1 to 6 had a high peel strength of 13.0 gf / cm or higher. In particular, it was confirmed that the cathodes of Preparation Examples 1 and 5 had the highest peel strength of 15.0 gf / cm.

[0220] That is, in the case of the cathodes of Manufacturing Examples 1 to 6 prepared using the copolymers of Examples 1 to 6, it was confirmed that they had higher binding strength compared to the cathodes of Comparative Manufacturing Examples 1 and 2 prepared using the copolymers of Comparative Examples 1 and 2.

[0221] In addition, it was confirmed that the low viscosity of Example 3 (14.2 gf / cm) and the copolymer of Example 3 also had sufficient binding strength, so the decrease in viscosity did not lead to a decrease in binding strength.

[0222] In contrast, the peel strength of Comparative Example 1, prepared using the copolymer of Comparative Example 1, and Comparative Example 2, prepared using the copolymer of Comparative Example 2, was low at 12.6 gf / cm and 10.9 gf / cm, respectively, confirming that the adhesive strength decreases when the viscosity is excessive or the composition is outside the range of the present invention.

[0224] Evaluation Example 3: Measurement of battery capacity retention rate and verification of negative electrode surface after battery cycling

[0225] For the batteries prepared in Preparation Examples 1 to 6 and Comparative Preparation Examples 1 and 2, the charge termination voltage was set to 4.3V and the discharge termination voltage to 2.5V at 25°C, and the charge / discharge current density was changed sequentially to 0.1C, 0.2C, and 0.5C, and a total of 3 charge / discharge cycles were performed once each.

[0226] Afterwards, 300 charge and discharge cycles were performed with a charge / discharge current density of 1C, a charge termination voltage of 4.3V, and a discharge termination voltage of 2.5V.

[0227] All discharges were performed under constant current / constant voltage conditions, and the termination current of the constant voltage discharge was set to 0.005C.

[0228] At this time, the capacity retention rate was calculated according to the following mathematical formula 2.

[0230] [Mathematical Formula 2]

[0231] Capacity retention rate [%] = [Discharge capacity of the 300th cycle / Discharge capacity of the 1st cycle] x 100

[0233] The results of measuring the capacity retention rate of the batteries prepared in Preparation Examples 1 to 6 and Comparative Preparation Examples 1 and 2 are shown in Table 5 below.

[0234] At this time, five pouch-type secondary batteries were fabricated and measured for each binder, and the average value was calculated and the results are shown in Table 5 below.

[0235] In addition, the battery that had completed cycle performance operation using the above method was completely discharged with a 1C current, disassembled, deactivated by leaving it in ethanol for 1 hour, and then the surface of the negative electrode was visually inspected.

[0236] After disassembling the battery that had completed the cycle and removing the negative electrode, the following three items were observed: (1) whether the negative active material had detached from the electrode, (2) whether surface non-uniformity (irregularity, peeling marks, etc.) was observed, and (3) whether the surface had detached when lightly rubbed with a gloved finger.

[0237] As a result of the observation, the results were judged as 'very good', 'good', and 'partially delaminated'. As a judgment criterion, 'very good' is defined as a case where no delamination of the negative active material is observed from the electrode, no surface non-uniformity is observed, and no delamination occurs even when lightly rubbed with a gloved finger. 'Good' is defined as a case where no delamination of the active material is observed from the electrode, but surface non-uniformity is observed, and no delamination occurs during the rubbing test. 'Partially delaminated' is defined as a case where delamination of the active material is observed from the electrode, surface non-uniformity is observed, and delamination occurs during the rubbing test.

[0239] The results of observing the negative electrode surface after cycling of the batteries prepared in Preparation Examples 1 to 6 and Comparative Preparation Examples 1 and 2 are shown in Table 5 below.

[0241] cathode Capacity retention rate (%, @300 cycles) Post-cycle cathode surface condition Preparation Example 1 82.0 (Good) ○ Preparation Example 2 81.8 (Good) ○ Preparation Example 3 82.3 (Good) ○ Preparation Example 4 83.3 (Good) ○ Preparation Example 5 83.3 (Good) ○ Preparation Example 6 84.4 (Very good) ◎ Comparative Manufacturing Example 1 81.5 (Partial Tali) △ Comparative Manufacturing Example 2 80.8 (Partial Tali) △

[0243] As a result of measurement, it was confirmed that the batteries of Preparation Examples 1 to 6, prepared using the copolymers of Examples 1 to 6 as shown in Table 5 and Figures 1 and 3 above, exhibited a high capacity retention rate of 81.8% or higher, and the negative electrode surface condition evaluation results after cycling were all rated as “good.”

[0244] In particular, the battery of Preparation Example 6 showed the highest capacity retention rate at 84.4% and the best result with an evaluation of the negative electrode surface condition after cycling as “very good.” In addition, the batteries of Preparation Examples 4 and 5 each showed a capacity retention rate of 83.3%, and the batteries of Preparation Examples 1 to 3 showed a capacity retention rate of 81.8–82.3%, and all of Preparation Examples 1 to 5 showed an evaluation of the negative electrode surface condition after cycling as “good.”

[0245] In contrast, as shown in Table 5 and Figures 1 to 3 above, the batteries of Comparative Examples 1 and 2, prepared using the copolymers of Comparative Examples 1 and 2, had capacity retention rates of 81.5% and 80.8%, respectively, which were lower than the capacity retention rates of the batteries of Examples 1 to 6, prepared using the copolymers of Examples 1 to 6, and some delamination was observed on the negative electrode surface after cycling.

[0246] That is, it was confirmed that the cycle durability of the battery and the surface stability of the electrode were simultaneously improved when AMPS and HEMAM were mixed and the AA:AN content ratio was maintained at 40:40, as in the battery of Preparation Example 6 prepared using the copolymer of Example 6.

[0247] Consequently, it was confirmed that the introduction of AMPS or HEMAM can improve processability by lowering viscosity while maintaining the conversion rate. In particular, it was confirmed that the mixed introduction of the two functional monomers (Example 6, Preparation Example 6) could simultaneously achieve a medium viscosity (7,000 cps), a high conversion rate (90%), and excellent binding strength (14.5 gf / cm), as well as the best capacity retention rate and electrode surface stability. On the other hand, in the case of Comparative Example 2, where the AA:AN content ratio is 60:20, which is outside the scope of the present invention, and in the case of using MAM alone and Li + In Comparative Example 1 under anti-ionic conditions, it was confirmed that the electrode binding strength, electrode surface condition, and battery cycle performance all deteriorated along with the copolymer's excessive viscosity. Furthermore, anti-ionic selection has a secondary effect on viscosity, and K + Although the use showed an overall favorable trend, it was confirmed that the final performance was primarily influenced by adjusting the combination of functional monomers and the AA:AN content ratio to the present invention range.

[0248] Therefore, to ensure a balanced combination of processability (viscosity), conversion rate, binding strength, and long-term cycle performance, the AA:AN content ratio is maintained within the range of the present invention, AMPS and HEMAM are introduced in combination, and K is used as the anti-ion. + It was confirmed that a configuration adopting [it] is desirable.

[0250] The scope of the present invention is defined by the claims set forth below rather than by the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention.

Claims

Claim 1 It is composed of an acrylic acid-based monomer unit, an acrylonitrile-based monomer unit, and an acrylamide-based monomer unit, wherein the acrylamide-based monomer unit is formed by polymerizing a nonionic acrylamide, an acrylamide containing a hydroxyl group, an acrylamide containing a sulfonic acid group, or a combination thereof, and at least one of the acrylic acid-based monomer units is a lithium ion (Li + ), sodium ions (Na + ), potassium ions (K + A copolymer comprising ) or a combination thereof and ionically bonded, and based on 100% by weight of the total copolymer, 30-50% by weight of the acrylic acid-based monomer unit, 35-60% by weight of the acrylonitrile-based monomer unit, and 10-30% by weight of the acrylamide-based monomer unit. Claim 2 In claim 1, the copolymer is polymerized using a degrading initiator or a water-soluble azo initiator, wherein the degrading initiator is potassium persulfate (K₂S₂O₅), ammonium persulfate ((NH₄)₂S₂O₅), sodium persulfate (Na₂S₂O₅), or a combination thereof, and the water-soluble azo initiator is 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (VA-057), 2,2′-azobis(2-methylpropionamidine) dihydrochloride (V-50). 4,4′-Azobis(4-cyanovaleric acid), ACVA / ACPA, 2,2′-Azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, VA-044, 2,2′-Azobis[2-methyl-N-(2-hydroxyethyl)propionamide], VA-086, or a copolymer of a combination thereof. Claim 3 delete Claim 4 A copolymer according to paragraph 2, wherein 0.01 to 5 parts by weight of the decomposition-type initiator or water-soluble azo initiator is used based on 100 parts by weight of the total monomer (solid content) during the polymerization of the copolymer. Claim 5 In claim 1, the acrylic acid series monomer unit is formed by polymerizing acrylic acid and (meth)acrylic acid, or a combination thereof, and the acrylonitrile series monomer unit is formed by polymerizing acrylonitrile, methacrylonitrile, or a combination thereof, and the acrylamide series monomer unit (i) the nonionic acrylamide is formed by polymerizing acrylamide, methacrylamide, N-isopropylacrylamide, N-tert-butylacrylamide, N-dodecylacrylamide, or a combination thereof, and (ii) the acrylamide containing a hydroxyl group (iii) a copolymer formed by polymerizing N-(hydroxymethyl)acrylamide, N-(hydroxyethyl)acrylamide, N-(2-hydroxypropyl)acrylamide, 2-hydroxyethyl methacrylamide, or a combination thereof, wherein the acrylamide containing the sulfonic acid group is formed by polymerizing 2-acrylamido-2-methylpropanesulfonic acid (AMPS). Claim 6 The copolymer of claim 1, comprising repeating units represented by the following chemical formula 1. [Chemical Formula 1] In the above Chemical Formula 1, R1 is each independently hydrogen, a linear or branched hydrocarbon having 1 to 10 carbon atoms, or a combination thereof, and R2 is hydrogen, lithium ion (Li + ), sodium ions (Na + ), potassium ions (K + ) or a combination thereof, where R3 is each independently hydrogen, a saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms, a saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms substituted with a hydroxyl group (-OH), a sulfonic acid group (-SO₃H), or an acyl group (-CO-R4), or a combination thereof, and R4 of the acyl group (-CO-R4) is a linear or branched hydrocarbon group having 1 to 8 carbon atoms, and a+b+c=1. Claim 7 In claim 6, R1 of Formula 1 is each independently selected from the group consisting of hydrogen, methyl, ethyl, n-propyl, and iso-propyl, and R2 of Formula 1 is each independently hydrogen, lithium ion (Li + ), sodium ions (Na + ), or potassium ions (K + ) any one selected from the group consisting of, and R3 of the above chemical formula 1 is each independently hydrogen, methyl, ethyl, n-propyl, iso-propyl, n-butyl, iso-butyl, sec-butyl, tert-butyl, n-pentyl, allyl, phenyl, cyclohexyl, hydroxymethyl, 2-hydroxyethyl, 1-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, 4-hydroxybutyl, methylsulfonic group, ethylsulfonic group, propylsulfonic group, butylsulfonic group, isopropylmethylsulfonic group, isobutylmethylsulfonic group, sec-butylmethylsulfonic group, tert-butylmethylsulfonic group, tert-butylethylsulfonic group, (2,2,3,3-tetramethylpropyl)methylsulfonic group, methyl acetyl group, ethyl acetyl group, propyl acetyl group, butyl acetyl group, isopropylmethyl acetyl group,Any one selected from the group consisting of isobutylmethylacetyl group, sec-butylmethylacetyl group, tert-butylmethylacetyl group, and (2,2,3,3-tetramethylpropyl)methylacetyl group, and R4 of Formula 1 is each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl (2-methylpropyl), tert-butyl (1,1-dimethylethyl), n-pentyl, isopentyl (3-methylbutyl), neopentyl; A copolymer selected from the group consisting of 2,2-dimethylpropyl), n-hexyl, 2-methylpentyl, 3-methylpentyl, n-heptyl, 2-methylhexyl, 3-methylhexyl, n-octyl, and 2-ethylhexyl. Claim 8 In claim 1, the copolymer is a random or block copolymer. Claim 9 A copolymer according to claim 1, having a viscosity of 3,000 to 11,000 cps at 25°C. Claim 10 A cathode slurry comprising: a copolymer of any one of claims 1, 2, and 4 to 9; and a cathode active material. Claim 11 A cathode comprising: a current collector; and a cathode active material layer comprising a copolymer of any one of claims 1, 2, and 4 to 9 formed on the current collector. Claim 12 A secondary battery comprising the negative electrode of claim 11.

Citation Information

Patent Citations

  • Thermal crosslinking binder aqueous solution for lithium ion battery, thermal crosslinking slurry for lithium ion battery negative electrode, negative electrode for lithium ion battery, and lithium ion battery

    JP2021036519A

  • Porous membrane for secondary battery, slurry for secondary battery porous membrane and secondary battery

    KR1020140004156A

  • Binder for Anode of lithium secondary batteries and Anode for lithium secondary batteries comprising the binder

    KR1020210034966A

  • Copolymer for separator and secondary battery using thereof

    KR1020250075968A

  • Binder comprising copolymer composition, anode for secondary battery comprising the same, and secondary battery comprising the anode

    KR102661818B1