Method for Manufacturing a Cement Admixture by Classification and Treatment with a Functional Additive, and a System for Producing Low-Carbon Blended Cement Utilizing CKD

The method of classifying and chemically treating CKD to enhance its reactivity addresses the industry's challenge of utilizing CKD as a high-performance admixture, improving strength and stability in cement production while reducing carbon emissions.

KR103045741B1Active Publication Date: 2026-11-06ASIA CEMENT +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020250197027
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-12-12
Publication Date
2026-11-06
Estimated Expiration
2045-12-12

AI Technical Summary

Technical Problem

The cement industry faces challenges in effectively utilizing Cement Kiln Dust (CKD) as a high-performance admixture due to its wide particle size distribution, low reactivity, and impurities that cause process instability and reduced productivity, despite its potential as a resource for carbon reduction.

Method used

A method involving classification of CKD to select fine particles with a D90 particle size of 15 to 20 μm and applying amine or polyol compounds as functional agents to enhance chemical reactivity, followed by integration into a low-carbon mixed cement production system.

Benefits of technology

Transforms CKD into a high-performance cement admixture that enhances strength and durability, reduces carbon emissions, and stabilizes the cement production process by optimizing particle size and chemical composition, while minimizing environmental and economic costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025140482459-PAT00030_ABST
    Figure 112025140482459-PAT00030_ABST
Patent Text Reader

Abstract

The present invention relates to a recycling technology for cement kiln byproducts (CKD), which are byproducts generated in the clinker manufacturing process. More specifically, it relates to a method and system for converting CKD into a cement admixture while stabilizing its quality and utilizing it through an external resource recovery method rather than internal kiln circulation. To solve the aforementioned problem, the present invention provides a method for manufacturing a cement admixture using cement kiln byproduct (CKD, Cement kiln dust) generated in a kiln, comprising: (a) a step of collecting CKD; (b) a step of classifying the collected CKD to select fine particle classifiers with a D90 particle size within the range of 15 to 20 μm; and (c) a step of spraying a functional agent containing one or more of amine compounds or polyol compounds onto the surface of the selected fine particle classifiers.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a mixed material subjected to classification and functional preparation treatment, and a CKD cement production system using the same. More specifically, the invention relates to a technology for utilizing CKD, which was conventionally reintroduced as a cement raw material, as a high-functional cement mixed material by applying a physical classification process to cement kiln byproduct (Cement Kiln Dust, hereinafter 'CKD') generated in a kiln to select fine powder favorable for reactivity, and improving the reactivity of the selected fine powder through chemical surface modification treatment. Furthermore, the present invention includes a technology for manufacturing a high-quality low-carbon mixed cement using the above-mentioned mixed material and a production system thereof. Background Technology

[0003] Recently, the cement industry has been actively encouraging the use of blended cement, in which a portion of cement clinker is replaced with other materials, to reduce carbon emissions and cut costs. One of the most widely used admixtures is finely ground limestone. Finely ground limestone is known to be inexpensive, readily available, and to have a positive effect on the physical and chemical performance of cement. However, the use of finely ground limestone is resource-intensive as it requires the mining and grinding of new natural resources, and it also has limitations in that additional grinding processes and energy are required to promote reaction with cement. Furthermore, it has the disadvantage of low reactivity and unfavorable conditions for strength development.

[0004] Meanwhile, in the clinker manufacturing process, large quantities of Cement Kiln Dust (hereinafter 'CKD') are continuously generated as the main raw material, limestone, is scattered and collected during the calcination process. Since CKD consists mainly of calcium carbonate (CaCO₃) and possesses characteristics very similar to fine limestone powder, its potential as an alternative admixture has been raised. In fact, CKD is recognized as an industrial byproduct with very high potential in terms of resource recycling and carbon reduction, with regions such as Europe allowing its use as an alternative admixture. However, despite this high potential, CKD has not been effectively utilized due to the following technical limitations and has been reused through an in-process recirculation method. This involves feeding the collected CKD back into the kiln without post-treatment for the purpose of recovering the raw material components contained within it. However, this method causes a phenomenon called 'circulation concentration,' which continuously accumulates volatile substances such as alkali, sulfur, and chlorine within the process. Concentrated impurities form a hard coating layer inside the kiln, causing serious problems that impair process stability and reduce productivity. In addition, if the CKD captured during kiln operation is not accurately reflected in the raw mix for clinker production during circulation, it can have a negative impact on the quality stability of the clinker.

[0005] To address these issues, the cement industry has recently been actively exploring ways to recover and refine CKD separately outside the kiln to utilize it as a resource. In particular, the resource value of CKD is recognized to some extent in international standards. ASTM C150 / C150M, the Portland cement standard of the American Society for Testing and Materials (ASTM), explicitly permits the use of inorganic processing additives during cement manufacturing, and states that CKD with ensured chemical and physical stability may be included in this category. Furthermore, the European cement standard EN 197-1 permits the use of inorganic materials generated during the clinker production process as auxiliary components of cement. Accordingly, CKD is evaluated not merely as a byproduct, but as an accredited resource capable of being recycled as a component of cement. However, to industrially maximize the carbon reduction potential of CKD, supplementary process technologies such as component homogenization, reduction of chlorine and alkali, and particle size control are required.

[0006] Therefore, there is an increasing need for technology that can effectively utilize CKD as a cement admixture by stabilizing its quality while utilizing it through an external resource recovery method rather than internal kiln circulation. Prior art literature

[0008] 1. Registered Patent 10-2311207 "Method for producing asphalt filler using chlorine bypass dust generated in a cement manufacturing process and asphalt filler" 2. Registered Patent 10-2094398 "Method for recycling chlorine bypass dust generated in a cement manufacturing process" 3. Registered Patent 10-1366835 "Cement composition using desulfurization dust" 4. Published Patent 10-2004-0078466 "Concrete manufactured using cement kiln dust" The problem to be solved

[0009] The present invention was devised to solve the aforementioned prior art, and aims to provide a method and system that can effectively utilize CKD generated in the clinker manufacturing process for the production of low-carbon mixed cement by converting it into a high-performance admixture. means of solving the problem

[0011] The present invention provides a method for manufacturing a cement admixture using cement kiln byproduct (CKD, Cement kiln dust) generated in a kiln (Klin, 10), comprising: (a) a step of collecting CKD; (b) a step of classifying the collected CKD to select fine particle classifiers with a D90 particle size within the range of 15 to 20 μm; and (c) a step of spraying a functional agent comprising one or more of amine compounds or polyol compounds onto the surface of the selected fine particle classifiers.

[0013] At this time, the functional formulation may be characterized by being included in an amount of up to 0.5 wt% (excluding 0 wt%) relative to the total weight of the fine particle classifier.

[0015] In addition, the present invention provides a cement mixture prepared according to the above method.

[0017] In addition, the present invention provides a low-carbon mixed cement utilizing CKD comprising a clinker and the cement mixture.

[0019] At this time, the cement mixture may be characterized by containing 5 to 20 wt% relative to the total weight of the low-carbon mixed cement.

[0021] In addition, the present invention provides a low-carbon mixed cement production system utilizing CKD, characterized by comprising: a collection unit for collecting CKD generated in a kiln and preheated; a classification unit into which the CKD is introduced and which separates into fine particle classifiers with a D90 particle size within the range of 15 to 20 μm and coarse particle classifiers with a D90 particle size exceeding 20 μm; a processing unit for receiving the fine particle classifiers from the classification unit and spraying a functional agent containing one or more of amine compounds or polyol compounds onto the surface thereof to create a mixture; and a production unit for producing low-carbon mixed cement by operating one or more of the following: (a) a process line for mixing clinker powder crushed by a cement mill with the mixture; (b) a process line for crushing and discharging the clinker and the mixture together from the cement mill; and (c) a process line for including the mixture in an admixture and supplying it to the cement mill to crush and discharge it together with the clinker.

[0023] At this time, it may be characterized by further including a kiln supply line leading from the raw meal silo to the preheater and a recovery line for recovering the coarse particle classifier separated in the classifier to the kiln supply line.

[0025] In addition, the above-mentioned classifier may be characterized as being an air classifier equipped with a multi-stage cyclone.

[0027] At this time, the processing unit may be characterized by further including a spray nozzle for spraying the functional preparation. Effects of the invention

[0029] The present invention is,

[0030] 1) It can provide resource recovery and environmental and economic benefits for CKD.

[0031] The present invention enables the recycling of cement kiln dust (hereinafter 'CKD'), which caused instability when reused within existing processes, into a high-performance cement admixture that replaces admixtures such as fine limestone powder through a complex modification process described in detail below. This provides environmental and economic benefits that significantly contribute to reducing carbon emissions and enhancing sustainability in the cement industry by replacing the energy and resource consumption required for the mining and crushing of natural limestone—the raw material for the admixture—with industrial byproducts.

[0032] Furthermore, the mixture prepared according to the present invention can exhibit technical effects that surpass the performance of conventional limestone fine powder, along with these advantages. The present invention can achieve higher strength by contributing to the cement hydration reaction through a chemical activation mechanism by functional additives and potential pozzolanic reactivity not found in limestone fine powder, along with an intentionally optimized particle size distribution.

[0033] 2) Production process efficiency and stability can be maximized through selective recycling.

[0034] The coarse particles with low reactivity separated during the classification process are recycled back into raw materials for the kiln through a recovery line. At this time, since most impurities such as alkali and sulfur that cause process problems are separated together with the fine particles, the 'circulation concentration' phenomenon and the resulting decrease in equipment efficiency that occurred in the conventional CKD recirculation method can be prevented. Therefore, the present invention can have the effect of providing a sustainable solution that improves the stability of the cement production process as well as environmental protection and cost reduction.

[0035] 3) By organically combining physical modification and chemical activation, CKD can be converted into a high-performance mixture with complex reactivity.

[0036] First, the first stage, the classification process, goes beyond simply refining the particles and involves a chemical modification effect that relatively increases the content of active ingredients such as silica (SiO₂) and alumina (Al₂O₃), which are favorable for pozzolanic reactions, and sulfate (SO₃), which contributes to the promotion of initial hydration.

[0037] Next, the second step, treatment with amine or polyol functional additives, fundamentally improves the cement hydration reaction environment to maximize the potential of CKD. The functional additives form stable chelate complexes with aluminum and iron ions within the cement, thereby accelerating the hydration reaction of the cement particles themselves. This accelerated hydration environment provides conditions for the potential reactivity of fine calcium carbonate (CaCO₃) within the CKD, which was previously an inactive substance, to be realized. As a result, the activated cement aluminate phase (C₃A) and calcium carbonate react effectively to produce additional hydrates such as calcium carboaluminate, which densify the structure of the hardened cementitious body and play a key role in improving strength and durability.

[0038] Through the combined improvement of such physical and chemical properties, the admixture according to the present invention actively contributes to the hydration reaction of cement beyond a simple dilution effect, thereby exhibiting an effect that is equivalent to or greater than that of existing admixtures such as fine limestone powder.

[0039] 4) It is possible to achieve both strength enhancement and work improvement effects simultaneously.

[0040] The present invention secures a particle size base optimized for strength development through a classification process and improves fluidity by enhancing particle dispersibility through functional formulation treatment. Through this organic process, it is possible to achieve the effect of simultaneously maintaining or improving compressive strength while ensuring excellent workability.

[0041] 5) Process flexibility can be secured.

[0042] The system of the present invention can be flexibly applied to various production lines, such as grinding the final admixture before mixing, simultaneous grinding, or mixing with other admixtures before simultaneous grinding. This enables the easy introduction of the technology of the present invention while minimizing changes to the equipment of existing cement plants. Brief explanation of the drawing

[0045] [Fig. 1] is a photograph of an air classifier equipped with a multi-stage cyclone used in the present invention. [Figure 2] is a graph showing the change in chemical composition according to the classification stage of cement kiln byproduct (CKD). [Fig. 3] is a schematic diagram illustrating each process of the system and method of the present invention in comparison to a conventional method. [Fig. 4] is a schematic diagram showing process (a) of the production department. [Fig. 5] is a schematic diagram showing process (b) of the production department. [Fig. 6] is a schematic diagram showing the (c) process of the production department. Specific details for implementing the invention

[0046] The present invention aims to solve the problems of the aforementioned prior art by providing a method for recycling cement kiln byproduct (CKD) generated in a kiln (Klin, 10) as a high-performance cement admixture, a cement admixture produced by the said method, a method for producing low-carbon admixture cement using CKD, and a system for producing the said low-carbon admixture cement.

[0047] A method for manufacturing a cement admixture according to one aspect of the present invention for achieving the above-mentioned purpose may include: (a) collecting cement kiln byproduct (CKD) generated in a kiln (Klin, 10); (b) classifying the collected CKD to select fine particle classifiers with a D90 particle size within the range of 15 to 20 μm; and (c) spraying a functional agent comprising one or more of amine compounds or polyol compounds onto the surface of the selected fine particle classifiers.

[0048] In addition, the CKD cement production system of the present invention comprises: a collection unit (100) for collecting CKD generated in a kiln (10); a classification unit (200) into which the CKD is introduced and which separates into fine particle classifiers with a D90 particle size within the range of 15 to 20 μm and coarse particle classifiers with a D90 particle size exceeding 20 μm; and a treatment unit (300) which receives the fine particle classifiers from the classification unit (200) and sprays a functional agent containing one or more of an amine compound or a polyol compound onto the surface thereof to create a mixture. The production unit (400) may include one or more of the following: (a) a process line for mixing the clinker powder crushed by a cement mill (410) with the mixture; (b) a process line for crushing and discharging the clinker and the mixture together from the cement mill; and (c) a process line for including the mixture in the mixture and supplying it to the cement mill to crush and discharge it together with the clinker.

[0050] Conventionally, CKD was processed by reintroducing it into a kiln (Klin, 10) at the cost of reduced production efficiency. To solve the aforementioned problems, the present invention aims to improve both the physical and chemical properties of CKD to provide it with the function of a high-performance mixture that can replace mixtures such as limestone fine powder. To this end, the core technology of the present invention is to 1) maximize physical performance by precisely classifying CKD to a particle size smaller than a specific size, and 2) chemically enhance potential hydration reactivity by treating the classified fine particles with a functional agent.

[0052] First, the major roles that fine limestone powder, currently widely used as a cement admixture and supplementary cementitious material (SCM), plays in contributing to cement performance are as follows.

[0053] 1) Filler Effect

[0054] Fine limestone powder is finer than cement particles, so it exerts a 'filling effect' by filling the voids between the particles. This improves the density of the cement and provides 'nucleation sites' for the formation of cementitious hydrates (CSH), thereby promoting the initial hydration reaction and positively influencing the development of early strength.

[0055] 2) Chemical Effect

[0056] Calcium carbonate (CaCO₃), the main component of fine limestone powder, reacts with the aluminate phase (C₃A) of cement to additionally form carboaluminate hydrates. The carboaluminate hydrates thus formed increase the total amount of hydrates and stabilize the internal structure, thereby improving strength and durability.

[0058] In addition, since the D90 particle size of the limestone fine powder typically used as a mixture is within 15 to 20 μm, in order to have a filling effect equivalent to that of the limestone fine powder, CKD can undergo a classification step and be selected to have a D90 particle size within 15 to 20 μm.

[0060] The present invention will be described below with specific test and analysis examples.

[0062] The starting material of the present invention, CKD, is prepared by collecting airborne dust generated during the kiln (10) calcination process of combined raw materials such as limestone in the cement clinker manufacturing process, using a dust collection device such as a bag filter (110).

[0065] 1. Analysis of CKD Characteristics and Limitations

[0066] The present invention compared and analyzed CKD and limestone fine powder used as a cement admixture.

[0067] 1) Chemical and mineralogical properties

[0068] As a result of chemical composition analysis using XRF (X-ray fluorescence analysis), as shown in [Table 1] below, CKD showed a chemical composition that was very similar to that of limestone fine powder, although the calcium oxide (CaO) component accounted for the largest portion at approximately 49% and the alkali (Na₂O, K₂O) content was slightly higher than that of limestone fine powder.

[0069]

[0070] [Graph 1] and [Graph 2] below show the X-ray diffraction (XRD) analysis results of CKD and limestone fine powder. The results of the mineral phase analysis using XRD also confirmed that the main constituent mineral is calcite, a crystalline phase of calcium carbonate (CaCO₃), confirming that the two materials are mineralogically based on the same material.

[0071] [Graph 1] - XRD Analysis Results of CKD

[0072]

[0073] [Graph 2] - XRD Analysis Results of Fine Limestone Powder

[0074]

[0076] 2) Physical properties

[0077] As a result of analyzing the physical properties, as shown in [Table 2] below, the density of CKD was 2.55 g / cm³, which was similar to that of limestone fine powder (2.50 g / cm³), but the fineness (Blaine) was 7,239 cm² / g, which was significantly higher than that of limestone fine powder (4,152 cm² / g). This suggests that the fine particles were particularly scattered and captured during the clinker manufacturing process.

[0078]

[0079] In addition, the results of the particle size analysis of CKD before classification using laser diffraction are as shown in [Table 3] below.

[0080]

[0081] First, D10, D50, and D90 are commonly used in particle size analysis indicators that refer to specific points on the cumulative volume distribution measured by methods such as laser diffraction, and each has the following technical meanings.

[0082] - D10: Particle size corresponding to the bottom 10% of the cumulative distribution, meaning that 10% of the particles in the sample are smaller than this size.

[0083] - D50: This is the particle size corresponding to the 50% point of the cumulative distribution, i.e., the median.

[0084] - D90: Corresponds to the top 90% of the cumulative distribution, meaning that 90% of the particles in the sample are smaller than this size.

[0085] - D[4,3]: Volume average particle size, which is a weighted average value calculated in proportion to the volume of individual particles; it has the characteristic that this value can increase even if only a small amount of coarse particles are present.

[0086] Analyzing [Table 3] above, the D10 value for CKD before classification is 1.50 μm and the D90 value is 22.20 μm. The large deviation between the D10 and D90 values ​​indicates that the particle size distribution is widely spread and not homogeneous. Although the volume average particle size (D[4,3]) is 9.49 μm, which is a relatively fine average particle size, this does not adequately reflect the state in which different particle size ranges are mixed within the sample due to the characteristics of the volume weighting value.

[0087] Among them, D90 is an indicator reflecting the fraction of upper coarse particles in the sample, and the fact that the D90 value of the sample is 22.20 μm suggests that a significant amount of coarse particles are included that can impede the packing effect or reduce reactivity.

[0088] In conclusion, CKD before classification is in a heterogeneous state in which fine particles and coarse particles are inefficiently mixed.

[0090] 3) Limitations of CKD

[0091] As mentioned above, if the above-mentioned CKD with a wide and non-uniform particle size distribution is used as a cement admixture without post-treatment, it causes the following problems.

[0092] First, it results in an inefficient filler effect. The coarse particles included in the above CKD before classification cannot fill the fine pores between the cement particles, and instead only occupy space with a size similar to that of the cement particles.

[0093] Second, the nucleation effect is reduced. The nucleation effect refers to the fact that numerous fine particles provide a large surface area and act as 'nucleation sites' where cementitious hydrate (CSH) can adhere and grow; the more nuclei there are, the faster and more uniform the hydration reaction occurs. The nucleation effect depends on the 'specific surface area,' but the coarse particles in the CKD only occupy volume, and the number of effective nucleation sites per gram of the total mixture is significantly reduced, thereby lowering the nucleation effect.

[0094] Third, it causes a decrease in strength. Coarse CKD particles, which have almost no reactivity within the hardened cement structure, have weak adhesion to the surrounding cement paste, so when external force is applied, microcracks easily form, causing a decrease in overall strength.

[0095] Fourth, quality prediction is impossible. The ratio of fine particles to coarse particles can vary depending on which part of the CKD pile the sample is taken from. This results in inconsistent and large deviations in the quality (strength, fluidity, etc.) of the final product, making it difficult to use in construction sites where stable quality control is essential.

[0096] In conclusion, despite its high potential, CKD cannot fully demonstrate its performance if used as is due to the technical problem of a wide particle size distribution.

[0097] Therefore, in order to solve the above problems and maximize the potential of CKD, it is desirable for the present invention to remove coarse particles within CKD and uniformly control the particle size distribution through a classification process in terms of improving material properties.

[0099] 2. Classification stage

[0100] To overcome the aforementioned limitations, it is desirable to remove the group of coarse particles and simultaneously make the particle size distribution uniform by subjecting the captured CKD to a particle size classification process. At this time, the classification process can effectively remove coarse particles, minimize the loss of fine particles, and precisely make the particle size distribution uniform by using an air separator (210) having a multi-stage cyclone structure as shown in [Fig. 1].

[0102] 1) Optimization of physical properties

[0103] The above classification step is a key step for effectively separating coarse particles with low reactivity from the aforementioned wide particle size distribution and securing raw materials having a narrow and uniform particle size distribution composed solely of highly reactive fine particles.

[0104] The aforementioned selected fine particles can effectively serve as filling sites that fill the voids between cement particles and as nucleation sites that promote the cement hydration reaction.

[0105]

[0106] [Graph 3]

[0107]

[0108] Table 4 above shows the results of analyzing the particle size of CKD samples classified at each stage after the CKD samples collected and prepared in the kiln (10) were fed into a three-stage cyclone air classifier (210). Meanwhile, Graph 3 is a visual representation of the results of Table 4 above.

[0109] Referring to [Table 4] above, the D90 particle size of the first stage was 23.80 μm, whereas the D90 values ​​of the second and third stage classifiers were measured as 8.05 μm and 5.52 μm, respectively. This indicates that the proportion of relatively fine particles increases significantly as the classification stage progresses.

[0110] In addition, referring to [Graph 3], it can be seen that the particle size distribution curve of the 2nd and 3rd stage samples, which underwent the classification process, shifts to the left compared to the 1st stage, and at the same time, the width of the distribution becomes significantly narrower. From the above results, it can be seen that compared to the 1st stage classifier, the 2nd and 3rd stage classifiers show a significant decrease in the proportion of coarse particles and an improvement in the uniformity of the particle size distribution.

[0111] Therefore, through the above classification step, coarse particles are removed and the particle size distribution is reconfigured to be narrow and uniform, mainly consisting of fine particles, so that the physical properties of CKD can be optimized for the purpose.

[0113] 2) Optimization of chemical composition

[0114] The classification step of the present invention is a chemical modification process that not only has a physical effect of simply controlling particle size but also increases the chemically highly reactive components.

[0115] [Table 5] below shows the results of the chemical composition analysis of CKD samples before and at each classification stage.

[0116]

[0117] First, potential pozzolanic reactivity that enhances long-term strength can be secured.

[0118] The clay minerals (kaolinite, illite, etc.) contained in the CKD undergo a thermal history of about 500 to 900°C inside the preheater (20), which destroys their crystal structure and transforms them into a highly reactive amorphous state. When this CKD is classified, the amorphous clay mineral components, which are relatively fine particles, become concentrated as they progress to the later stages. In fact, as the classification stage progresses, the content of the main component CaO (50.0% → 47.3% → 46.5%) decreases, while the content of SiO₂ (6.2% → 6.8% → 7.6%) and Al₂O₃ derived from clay increases significantly. Therefore, the classified CKD, which has increased SiO₂ (silica) and Al₂O₃ (alumina), can react with calcium hydroxide (Ca(OH)₂) generated during cement hydration to form secondary hydrates such as CSH and CAH. This effect enhances long-term strength and durability, a unique advantage not found in ordinary limestone powder.

[0119] Second, it can have a hydration-promoting function that compensates for the reduction in initial strength. As the classification stage progresses, the SO₃ (sulfate) content increases significantly from 0.6% to 1.5%. Sulfate ions (SO₄²⁻) can contribute to the development of the cement's initial strength by reacting with the aluminate component (C₃A) in the cement to promote the formation of initial hydrates such as ettringite.

[0121] 3) Mineral phase changes according to particle size classification

[0122] XRD analysis was performed on classified samples to analyze changes in mineral phases according to particle size classification.

[0123] [Graph 4] - XRD by Classification Sample

[0124]

[0125] As a result of the analysis, as shown in [Graph 4] above, no change in the major mineral phases according to the classification stage was observed, which suggests that the major mineral types of CKD are maintained even during the classification process. However, subtle differences were observed in the relative XRD peak intensity of the major minerals, and in particular, the peak intensity of calcite showed a tendency to decrease as the classification stage progressed. This suggests a decrease in the crystallinity of calcite or an increase in the proportion of the amorphous phase, and acts as a factor contributing to the enhancement of the material's reactivity, as confirmed in the performance evaluation described later.

[0127] 4) Conclusion

[0128] Consequently, the above classification step physically removes coarse particles with low reactivity to secure an optimal particle size distribution that maximizes packing and nucleation effects, while chemically concentrating pozzolanic reactive materials (SiO₂, Al₂O₃) that contribute to long-term strength and hydration-promoting components (SO₃) that complement initial strength, and mineralogically reducing the crystallinity of the main component, calcite, to increase the proportion of the amorphous state.

[0129] Therefore, through the classification process of the present invention, optimization can be simultaneously achieved in various aspects ranging from particle size, chemical composition, and mineral phase for utilizing CKD as a mixed material.

[0131] 3. Verification of classification effect through performance evaluation

[0132] To verify the effect of the CKD classified as above on the actual performance of cement, the physical properties of mortar to which samples from each classification stage were applied were evaluated.

[0134] 1) Mixing

[0135] Table 6 below is a mortar mix design for performance evaluation. Based on the Plain mix (100% ordinary Portland cement), samples were prepared by replacing the samples before classification and the samples classified at each stage (Stage 1, Stage 2, Stage 3) with 5%, 10%, and 15% of the cement weight, respectively.

[0136]

[0138] 2) Evaluation of compressive strength (activity index)

[0139] [Graph 5] below shows the results of mortar compressive strength tests according to the classification stage and replacement rate mentioned above. As shown in [Graph 5], under all replacement rate conditions, as the classification stage increases (before classification → 1st stage → 2nd stage → 3rd stage), both the initial and long-term compressive strengths tend to increase proportionally.

[0140] In particular, when using 2-stage and 3-stage classified samples, early and long-term strength development was superior compared to 1-stage classified samples.

[0141] [Graph 5]

[0142]

[0144] 3) Liquidity (Flow) Assessment

[0145] Next, a flow test was performed to evaluate the effect of classified CKD on the workability of cement mortar, and the results are shown in [Graph 6] below.

[0146] [Graph 6]

[0147]

[0148] As a result of the analysis, when CKD is substituted for cement before classification, the flow value shows a continuous increasing trend compared to the standard mix (Plain) as the substitution rate increases from 5% to 15%. This is considered to be due to the characteristic flow-increasing effect of CKD replacing cement.

[0149] However, the most noteworthy point is that in the case of the above 2-stage and 3-stage classified samples, which effectively improved compressive strength, fluidity was secured at a level substantially equivalent to the standard mix (186 mm) even when the substitution rate was increased to 15%.

[0150] This indicates that the classification step of the present invention is a highly efficient method that improves compressive strength without significantly reducing workability, which is directly related to constructability.

[0152] 4) Conclusion

[0153] When the above compressive strength and fluidity evaluation results are combined, it is proven that the classification step of the present invention is a key process for modifying CKD to be suitable for use as a cement admixture.

[0154] As a result of the performance evaluation, the 2-stage and 3-stage classifiers showed a higher improvement in compressive strength compared to the 1-stage classifier, while maintaining fluidity equivalent to that of the standard mix. This means that the classified CKD can function as a mixture that simultaneously satisfies both strength and workability.

[0155] Therefore, the present invention aims to further improve chemical reactivity by adopting two-stage and three-stage classifiers (hereinafter, 'fine particle classifiers') composed of performance-proven fine particles as target raw materials for a subsequent process (functional formulation treatment).

[0157] 4. Functional formulation processing step

[0158] This step can be applied to enhance the chemical reactivity of the above-mentioned fine particle classifier.

[0160] Generally, the 'grinding aids' used in the cement industry are primarily intended to improve the grinding efficiency of clinker. However, the present invention focuses on improving dispersibility and reactivity by forming a uniform coating layer on the particle surface rather than grinding fine particle classifiers, so this is referred to as a 'functional aid'.

[0162] 1) Types and Processing Methods of Functional Formulas

[0163] In the present invention, the functional additive may include one or more of amine compounds or polyol compounds. Representative amine compounds include amines such as TEA (triethanolamine), TIPA (triisopropanolamine), and DEG (diethylene glycol), which mainly form chelate complexes with metal ions in cement to directly promote the hydration reaction.

[0164] In addition, a representative polyol compound is DEG (Diethylene Glycol), and [Equation 1] below is the chemical structural formula of DEG. The above polyol compound forms an adsorption layer on the surface of the cement and the fine particle classifier through a large number of polar hydroxyl groups (-OH) within the molecule, thereby suppressing aggregation between particles and uniformly dispersing them through steric hindrance and electrostatic repulsion. This dispersion effect improves the overall fluidity of the paste and increases the effective reaction surface area of ​​the particles, thereby improving the efficiency and uniformity of the hydration reaction and ultimately enhancing physical performance.

[0165] [Equation 1]

[0166]

[0168] In the following, cases in which amine compounds such as TEA and TIPA are applied are described in detail as representative examples, but the rights of the present invention are not limited thereto.

[0169] [Equation 2] and [Equation 3] below are the chemical structural formulas of TEA and TIPA, respectively.

[0170] [Equation 2]

[0171]

[0172] [Equation 3]

[0173]

[0174] The processing method may be carried out by spraying a liquid functional additive on the surface of the particles in a transfer stage before the fine particle classifiers, which have undergone the classification step through an air classifier (210) as shown in [Fig. 3], are mixed with other cement materials. The amount of the functional additive added may be within 0.5 wt% (excluding 0 wt%) of the total weight of the fine particle classifiers. If the amount added exceeds 0.5 wt%, the additive molecules may cross-link between the particle surfaces to cause re-aggregation, or form excessive complex compounds with metal ions required for the cement hydration reaction, thereby causing a negative effect that delays the initial hydration reaction.

[0176] 2) Principle of performance improvement through functional formulation

[0177] The amine functional additive used in the present invention directly participates in the cement hydration process to induce a chemical environment that allows calcium carbonate (CaCO₃), the main component of the fine particle classifier, to actively participate in the hydration reaction, thereby contributing to the improvement of cement strength development. The principle is as follows.

[0178] ① Acceleration of hydration reaction through chelate complex formation

[0179] In the cement paste, aluminum ions (Al³⁺) and iron ions (Fe³⁺) dissolved from C₃A and C₄AF form hydroxide complex ions ([Al(OH)₄]-, [Fe(OH)₄]-) as shown in [Equation 4].

[0180] [Equation 4]

[0181]

[0182] However, when TEA or TIPA applied in the present invention is present, they act as strong chelate ligands and react with Al³⁺ and Fe³⁺ ions preferentially over the reaction of [Equation 4] to form a very stable water-soluble chelate complex ([Al(TEA)]³⁺, [Fe(TEA)]³⁺) as shown in [Equation 5].

[0183] [Equation 5]

[0184]

[0185] The formation of these chelate complexes promotes the dissolution of C₃A and C₄AF, and consequently plays a role in accelerating the hydration reaction of cement.

[0186] ② Generation of additional hydrates through activation of calcium carbonate in fine particle classifiers

[0187] As described above, the activated C₃A and C₄AF react with fine calcium carbonate (CaCO₃) contained in the fine particle classifier, and produce carboaluminate as shown in [Equation 6]. ) and carboferrite, forms ).

[0188] [Equation 6]

[0189]

[0190]

[0191] These hydrates form a dense structure within the cement hydration product, resulting in an increase in the strength of the hardened cementitious body.

[0193] In conclusion, the functional formulation of the present invention exhibits the effect of maximizing the overall strength development of the hardened cementitious body by ① promoting the hydration reaction of the aluminate phase (C₃A) and ferrite phase (C₄AF) of cement through the formation of chelate complexes, and ② inducing calcium carbonate (CaCO₃) in the fine particle classifier to participate in the reaction for the formation of additional hydrates such as carboaluminates within the active environment thus formed, thereby increasing the total amount of hydrates produced.

[0195] 3) Verification of effectiveness through performance evaluation

[0196] A. Mixing

[0197] For the test in this stage, fine particle classifiers were obtained from Company A and Company U, respectively (hereinafter CA and CU). For 100 parts by weight of the obtained fine particle classifiers, 0.04 parts by weight (400 ppm, based on solid content) of the functional preparations TEA and TIPA were sprayed on each to pre-treat the particles so that they were uniformly dispersed and coated on the surface of the preparation particles.

[0198] Table 7 below is a mortar mix design for performance evaluation. A mix (R50G50) using 50% cement and 50% blast furnace slag fine powder (GGBS) was set as the standard (Plain). The test mix was prepared by replacing a portion of the blast furnace slag fine powder in the standard mix with 10% and 20%, respectively, of fine particle classifiers (CA or CU) pretreated with the above functional additive, and the water-to-binder ratio (W / B) was fixed at 0.5.

[0199] [Table 7]

[0200]

[0202] B. Liquidity (Flow) Assessment

[0203] [Graph 7] below is the result of a flow test evaluating the effect of the functionally formulated fine particle classifier on the workability of the mortar under the above mixing conditions.

[0204] [Graph 7]

[0205]

[0206] The results of [Graph 7] show that the functionally formulated fine particle classifier has a combined effect of increasing strength and simultaneously improving workability.

[0207] All formulations using fine particle classifiers (CA, CU) treated with functional agents exhibited excellent fluidity equivalent to or better than the standard formulation (R50G50). This means that the amine functional agents effectively suppressed the re-aggregation of the classified fine particles, thereby improving the workability of the paste.

[0209] C. Evaluation of Compressive Strength and Activity Index

[0210] [Graph 8] below shows the results of evaluating the effect of functional formulation treatment on the strength development of fine particle classifiers.

[0211] [Graph 8] - Compressive strength of mortar with functional formulation

[0212]

[0213] As a result of analyzing [Graph 8] above, from 7 days of age onwards, all formulations to which the functional additive was applied exhibited compressive strength equal to or greater than that of formulations without the additive (R50G40A10, R50G30A20, etc.). This indicates that the functional additive effectively promoted the reactivity of the fine particle classifiers. This trend was consistently observed regardless of the substitution rate (10%, 20%) and type (CA, CU) of the fine particle classifiers.

[0214] [Graph 9] below shows the results of evaluating the effect of functionally formulated fine particle classifiers on strength development. The activity index represents the relative strength development level of each experimental formulation when the compressive strength of the standard formulation (R50G50) is set to 100%.

[0215] [Graph 9] - Activity of mortar with applied functional formulation (Replacement rate 10%, 20%)

[0216]

[0217] As a result of a comprehensive analysis considering long-term strength up to 28 days, when 10% was replaced, strength from 7 to 28 days of age achieved an equivalent or greater level than the standard mix, and when 20% was replaced, although the long-term strength at 28 days decreased slightly compared to the standard (activity 90~98%), it still exhibited a high level of strength, making it suitable for specific applications.

[0219] D. Conclusion

[0220] The performance evaluation performed as an embodiment of the present invention demonstrates that the amine-based functional additive treatment step is an efficient method that improves fluidity by exhibiting a complex effect: ① promoting the reaction of the aluminate phase (C₃A) and the like during the cement hydration process to improve compressive strength, and ② acting as a dispersant that adsorbs to the surface of fine particle classifiers to prevent aggregation between particles, thereby improving the fluidity of the mortar. Through this, it can be proven that the admixture of the present invention has value as a high-performance admixture that satisfies both strength and workability.

[0222] 5. Particle size conditions and desirable content of the mixture

[0223] Prior to this test, considering that the D90 particle size of the limestone fine powder used as a representative mixture is within 15 to 20 μm, the fine particle classifier of the present invention was also selected to have a D90 particle size within 15 to 20 μm. As a result of synthesizing all the preceding characteristic analyses and performance evaluations, it was proven that the first-stage classifier with a D90 particle size larger than 20 μm had poor performance. On the other hand, the fine particle classifier (second and third-stage classifiers, D90≤20 μm) clearly showed an improvement in strength and workability. Therefore, by controlling the D90 particle size to within 15 to 20 μm, it is possible to stably secure performance by including the fine particle classifier with proven performance (second and third-stage classifiers) while excluding the first-stage classifier with poor performance (D90>20 μm). In particular, as in the embodiment of the present invention, it is more preferable to sort the D90 particle size of the 2-stage and 3-stage classifiers to be within 5 to 8 μm.

[0224] In addition, from the results of '4. Functional Preparation' above, it can be confirmed that the functionally prepared CKD admixture functions effectively as an admixture within a range of 5 to 20 wt% relative to the total weight of the cement. If the content of the cement admixture is less than 5 wt%, the effect of replacing natural resources by recycling CKD, which is the main objective of the present invention, may be relatively insignificant. On the other hand, if it exceeds 20 wt%, the compressive strength may be significantly reduced compared to the standard mix (Plain) due to the cement dilution effect, and an excessive amount of fine particles may act as a negative factor that hinders paste fluidity. Therefore, it is determined that the optimal range is 5 to 20 wt% to minimize the reduction in compressive strength and economically achieve the resource recycling effect while maintaining workability equivalent to that of the standard mix (Plain).

[0226] 6. Composition and Operating Principle of a Low-Carbon Blended Cement Production System Using CKD

[0227] The low-carbon blended cement production system utilizing CKD according to the present invention aims to improve the inefficient aspects of the existing cement manufacturing process, convert the CKD into a high-performance cement admixture, and ultimately produce CKD cement.

[0228] Below, as an embodiment of the present invention, I will explain the comparison between the existing cement process and the improved process according to the present invention, as shown in [Fig. 3].

[0230] 1) Problems with the existing system

[0231] In the existing process (blue line), raw materials are generated in the kiln (10), and the CKD that has passed through the preheater (20) is collected in a collector such as a bag filter (110), and then re-introduced into the top of the preheater (20), having a circulation structure.

[0232] However, when the above CKD is simply reused, the alkali, sulfur, and other components concentrated in the above CKD form an adhesive coating layer inside the kiln (10), which reduces the efficiency of the equipment and hinders stable operation.

[0234] 2) Improved system according to the present invention

[0235] To solve the problems of the existing system described above, the present invention provides a new system as shown in the improved process (red line) in [Fig. 3]. The system of the present invention includes a collection unit (100), a classification unit (200), a processing unit (300), a generation unit (400), etc., and the specific roles and operating principles of each component are as follows.

[0237] a. Collection unit (100)

[0238] The collection unit (100) collects CKD generated in the kiln (10) and passed through the preheater (20). The CKD that has passed through the preheater (20) undergoes a certain level of thermal history, and there is a high possibility that clay minerals, etc., will be activated in an amorphous state. The present invention provides a basis for maximizing the quality of the final mixture by selectively collecting the CKD having such potential reactivity and using it as a raw material.

[0239] The collection unit (100) can typically be implemented as a bag filter (110) or an electrostatic precipitator, and is located at the rear of a preheater (20) and a cooling tower (30) connected to a kiln (10) to collect CKD particles with an efficiency of 99% or more. As shown in [Fig. 3], the bag filter (110) used as the collection unit (100) in one embodiment of the present invention can collect even fine CKD particles of several micrometers (μm) or less with high efficiency using a high-performance fiber filter, which has the advantage of having superior dust collection efficiency compared to an electrostatic precipitator and is also advantageous for the selective collection of fine particles.

[0241] b. Distribution Department (200)

[0242] Next, the CKD collected in the collection unit (100) is transferred to the classification unit (200). At this time, the classification unit (200) may be an air classifier (210), a centrifugal classifier, an electrostatic classifier, etc. As shown in [Fig. 1], the air classifier (210) used as an embodiment in the present invention is composed of a three-stage cyclone air classifier (210), and each stage is configured to effectively separate CKD of different particle size ranges using centrifugal force and air flow.

[0243] The above-mentioned classifier (200) is one of the core components of the present invention and is responsible for precisely separating CKD of non-uniform particle size supplied from the above-mentioned collection unit (100) so as to maximize its performance as a cement mixture.

[0244] The above classification unit (200) can be implemented as an air classifier (210) with a multi-stage cyclone structure utilizing aerodynamic principles, as shown in [Fig. 3]. The input CKD is separated by particle size due to the difference in centrifugal force and fluid resistance within a strong swirling airflow. Coarse particles with relatively large mass are pushed out to the outer wall and discharged downwards due to the influence of centrifugal force, while fine particles with small mass rise along the airflow and move to the next stage cyclone or are finally separated and collected.

[0245] The above classification unit (200) can separate CKD into fine particle classifiers with a D90 particle size within the range of 15 to 20 μm and coarse particle classifiers with a D90 particle size exceeding 20 μm. More preferably, it can be separated into D90 particle sizes of 5 to 8 μm or less (levels of 2nd and 3rd stage classifiers) that showed excellent performance in '3. Performance Evaluation'. The classified fine particles contribute decisively to improving the final strength and durability of the cement through a combination of effects: ① enhancement of nucleation effects due to maximized specific surface area, ② optimization of filling effects due to removal of coarse particles, and ③ increase in the relative content of reactive substances (SiO₂, Al₂O₃, etc.). The highly active fine particle classifiers selected from the classification unit (200) are transferred to the processing unit (300), and the coarse particle classifiers with relatively low reactivity can be discharged to the kiln supply line (50) through the recovery line (60) described later. In addition, the coarse particle classifier discharged in this way and supplied to the kiln supply line (50) can be recycled again as a raw material for the kiln (10).

[0247] c. Processing unit (300)

[0248] The processing unit (300) is a device that completes a final high-performance mixture by imparting chemical activity to fine particle classifiers with optimized physical properties after passing through the classification unit (200). The processing unit (300) performs the function of uniformly spraying a functional agent containing one or more of amine or polyol compounds onto the surface of the classified fine particles.

[0249] In one embodiment, as illustrated in FIG. 3, the processing unit (300) may include one or more spray nozzles (310) installed inside a closed conduit or chute through which fine particle classifiers are transported. A liquid functional agent, such as triethanolamine (TEA) or triisopropanolamine (TIPA), is sprayed in an aerosol state through the spray nozzles (310). The aerosolized functional agent particles collide with fine particle classifiers scattered in the air and are adsorbed or coated on their surface in the form of a thin film. This method can enable efficient surface treatment in a continuous process without separate mixing power.

[0250] As previously described in '4. Functional Preparation Treatment Step,' the surface-treated admixture acts as a dispersant by ① promoting the reaction of the aluminate phase (C₃A) and the like during the cement hydration process, and simultaneously ② adsorbing to the surface of cement particles to prevent aggregation between particles, which effectively improves the fluidity of the mortar, as confirmed by actual flow test results.

[0252] D. Production Department (400)

[0253] The production unit (400) is a part that produces final CKD cement by mixing the high-performance admixture produced in the processing unit (300) with clinker, and is characterized by being designed to flexibly respond to various process conditions of an actual cement plant. The present invention can produce CKD cement by selectively or in combination operating at least one of the following process lines (a), (b), and (c).

[0254] ① (a) Process line (post-mixing method): As shown in [Fig. 4], the clinker is crushed to a target fineness in a cement mill (410) and then mixed with the admixture of the present invention in a separate blender (not shown). This allows for precise control of the amount of admixture added, which is advantageous for producing various types of customized cement.

[0255] ② (b) Process line (simultaneous grinding method): As shown in [Fig. 5], this is a method in which clinker and the mixture of the present invention are fed together into a cement mill (410) to be ground and mixed simultaneously. This has the advantage of being simple because no separate mixing equipment is required, and the homogeneity of the two materials is maximized during the grinding process.

[0256] ③ (c) Process line (simultaneous grinding method after mixing with admixture): As shown in [Fig. 6], the admixture of the present invention is first mixed with other admixtures such as gypsum, and then supplied to a cement mill (410) along with clinker for grinding. At this time, the term 'admixture' as used in this specification is defined in a broad sense to include not only setting retarders such as gypsum, which are typically added during cement manufacturing, but also other existing cement admixtures (or binders) such as fly ash or blast furnace slag fine powder. This is intended to allow the implementation of the present invention by flexibly utilizing the input system of various types of materials (gypsum, fly ash, etc.) present in existing facilities, and is a very practical method that allows the system of the present invention to be applied while minimizing equipment changes.

[0257] At this time, regardless of whether the production unit (400) produces CKD cement by selectively or in combination with at least one of the process lines (a), (b), and (c), it is preferable that the admixture of the present invention be controlled to be included within the range of 5 to 15% relative to the total weight of the finally produced CKD cement. As proven by the performance evaluation above, this content range is the most optimized technical range that can maximize workability and resource recycling effects while minimizing strength reduction. The production unit (400) can precisely control the content through a quantitative supply device (not shown), such as a weighing feeder installed at the raw material input section of each process line.

[0259] E. Recovery line (60)

[0260] The recovery line serves to stably recover the coarse particle classifier separated from the classifier (200) into the kiln supply line (50) leading from the raw meal silo to the preheater (20).

[0261] The system of the present invention may further include a recovery line (60) that recovers the coarse particle classifier separated from the classification unit (200) and recirculates it into the process. As shown in [Fig. 2], the recovery line (60) connects the discharge port of the coarse particle classifier of the classification unit (200) with a kiln supply line (50) that supplies raw materials. The coarse particle classifier contains a large amount of useful raw material components (CaCO₃), but the concentration of volatile impurities (alkali, sulfur, etc.) that cause process problems is relatively low. Therefore, recycling it as a raw material can reduce the amount of raw material used, and at the same time, it is a very efficient and eco-friendly process design that can fundamentally prevent the 'circulation concentration' phenomenon inside the kiln (10), which was a chronic problem of the existing CKD recirculation method.

[0263] Through the configurations described above, the system of the present invention can effectively achieve multiple objectives of resource recycling, energy saving, and high-performance cement production by converting CKD into a high-performance resource and perfectly integrating it into the actual production process.

[0265] For the time being, this specification describes the relevant contents focusing on embodiments of the present invention. The terms used in this specification are used merely in a general sense to facilitate the explanation of the technical content of the present invention and to aid in understanding the invention, and the scope of the present invention is not limited to the dictionary meanings of the terms. In addition to the embodiments disclosed in this specification, other variations based on the technical concept of the present invention are also possible. Explanation of the symbols

[0267] 10: Kiln 20: Preheater 30: Cooling Tower 40: Raw mill silo 50: Kiln supply line 60: Recovery line 100 : Collection unit 110: Bag filter 200 : Classification Department 210 : Air classifier 300 : Processing unit 310 : Spray nozzle 400 : Production Department 410 : Cement Mill

Claims

Claim 1 A method for manufacturing a cement admixture using cement kiln byproduct (CKD, Cement kiln dust) generated in a kiln (Klin, 10), comprising: (a) a step of collecting CKD; (b) a step of classifying the collected CKD to select fine particle classifiers with a D90 particle size in the range of 15 to 20 μm, in which silica (SiO2), alumina (Al2O3), and sulfate (SO3) components are concentrated; and (c) a step of treating the surface of the selected fine particle classifiers with a functional agent that promotes a hydration reaction by inducing the formation of a chelate complex by spraying a functional agent containing one or more of amine compounds or polyol compounds. Claim 2 A method for manufacturing a mixture according to claim 1, characterized in that the functional additive is included in an amount of up to 0.5 wt% (excluding 0 wt%) relative to the total weight of the fine particle classifier. Claim 3 A cement mixture manufactured by the method of any one of paragraphs 1 to 2. Claim 4 A low-carbon blended cement utilizing CKD comprising clinker; and the cement admixture of claim 3. Claim 5 In claim 4, the low-carbon mixed cement utilizing CKD is characterized in that the cement admixture is included in an amount of 5 to 20 wt% relative to the total weight of the low-carbon mixed cement. Claim 6 A collection unit (100) for collecting CKD generated in a kiln (10) and passed through a preheater (20); a classification unit (200) into which the CKD is introduced and which separates into fine particle classifiers with a D90 particle size within the range of 15 to 20 μm and coarse particle classifiers with a D90 particle size exceeding 20 μm; a processing unit (300) for producing a mixture that promotes a hydration reaction by receiving the fine particle classifiers from the classification unit (200) and spraying a functional agent containing one or more of amine compounds or polyol compounds onto the surface thereof to induce the formation of a chelate complex; and among (a) a process line for mixing the mixture with clinker powder crushed by a cement mill (410), (b) a process line for crushing and discharging the clinker and the mixture together from the cement mill, and (c) a process line for including the mixture in an admixture and supplying it to the cement mill to crush and discharge it together with the clinker. A low-carbon mixed cement production system utilizing CKD, characterized by comprising: a production unit (400) that produces low-carbon mixed cement through one or more operations; and a recovery line (60) that maintains the stability of the cement production process by recovering the coarse particle classifier separated from the classification unit (200) into a kiln supply line (50) leading from a raw meal silo (40) to a preheater (20) and recycling it as a kiln raw material. Claim 7 delete Claim 8 A low-carbon mixed cement production system utilizing CKD, characterized in that, in claim 6, the classifying unit (200) is an air classifier (210) equipped with a multi-stage cyclone. Claim 9 A low-carbon mixed cement production system utilizing CKD, characterized in that, in either claim 6 or claim 8, the processing unit (300) further comprises a spray nozzle (310) for spraying the functional agent.

Citation Information

Patent Citations

  • High-early strength type cement supporting early form removal produced by classified fine particle cement and manufacturing method using the same

    KR100865848B1

  • Method and apparatus for recovering co2 gas in cement production equipment

    KR101586107B1

  • CKD-based carbon dioxide storage cement manufacturing systems and methods

    KR1020220157600A

  • Modified Mixture for Manufacturing Blended Cement, Its Manufacturing Method and Blended Cement Using The Modified Mixture

    KR102805085B1