A method for producing recycled powder from waste thermal insulation by wet grinding and its applications
The wet-crushing method transforms waste insulation materials into recyclable powder, addressing inefficiencies in existing recycling methods by reducing costs and environmental impact, and improving the performance of construction materials.
Patent Information
- Application Number
- KR1020250189357
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-12-03
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-12-03
AI Technical Summary
Existing recycling methods for inorganic thermal insulation materials, such as glass wool and mineral wool, are inefficient, costly, and environmentally harmful, with limited recyclable volume and high energy consumption, and do not effectively convert waste into usable forms.
A wet-crushing method using a ball mill with alumina balls to produce a slurry, followed by stirring, filtering, and drying to create a recyclable powder, which is then used in waterproofing agents, cement mixtures, and fire beads.
The method efficiently converts waste insulation materials into recyclable powder form, minimizing environmental impact and processing costs, while enhancing water resistance, seismic performance, and mechanical properties of construction materials.
Smart Images

Figure 112025136397875-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for recycling waste inorganic thermal insulation materials, and more specifically, to a method for producing recyclable powder by wet crushing waste thermal insulation materials, and to applications such as waterproofing agents, cement mixtures, and fire beads produced using the powder. Background Technology
[0002] Inorganic thermal insulation materials such as glass wool, mineral wool, and Cerakwool, which are used in industrial sites, have excellent thermal insulation and heat resistance, so they are widely used for thermal insulation and insulation purposes in various heavy industrial plants, such as power plants, petrochemical plants, and marine and shipbuilding sectors.
[0003] However, these insulation materials are very difficult to recycle during the collection and disposal process after use. Currently, recycling technologies being attempted are extremely limited; reported methods include manufacturers melting unused or expired products to reuse some raw materials, or dry-crushing and sintering waste insulation materials to utilize them as aggregate for cement reinforcement.
[0004] However, these existing recycling methods are insufficient for effectively handling the large-scale thermal insulation waste generated across industries, as they involve high processing costs and lengthy processing times, and the recyclable volume is negligible compared to the initial usage. Furthermore, dry crushing processes entail environmental issues such as airborne dust, while melt-based recycling has low industrial applicability due to high energy costs and environmental burdens associated with high-temperature processes.
[0005] Therefore, there is a growing demand for recycling technologies that can process waste insulation materials economically and quickly, and convert them into practically recyclable forms and quantities while minimizing environmental burden. The problem to be solved
[0006] The present invention was created to solve the aforementioned problems, and more specifically, it relates to a method for manufacturing recycled powder that can process waste insulation material more economically and quickly to convert it into a recyclable powder form, and minimize environmental burden by reusing the solvent used in the process.
[0007] In addition, another objective is to provide a waterproofing composition capable of securing excellent water resistance and excellent seismic performance by utilizing the above-mentioned recycled powder.
[0008] In addition, another objective is to provide a cement mixture having improved strength characteristics by utilizing the above-mentioned recycled powder as a construction filler.
[0009] In addition, another objective is to provide digest beads that can be manufactured under non-heating conditions using a solid slurry containing the above-mentioned recycled powder. means of solving the problem
[0010] A method for manufacturing a wet-crushing recycled powder of waste thermal insulation material according to one embodiment of the present invention is characterized by comprising the following steps in a method for recycling waste thermal insulation material: (a) introducing waste thermal insulation material and water into a ball mill and wet-crushing to produce a slurry; (b) stirring to prevent sedimentation of the slurry; (c) filtering and dewatering the slurry to separate solids; and (d) drying and crushing the separated solids to produce a recycled powder.
[0011] More specifically, in step (a) above, the waste thermal insulation material is characterized by being crushed to a particle size of 1 to 100 μm and formed into a slurry.
[0012] More specifically, in step (a) above, the ball mill is characterized by using alumina balls of 10 to 40 mm as a grinding medium.
[0013] More specifically, in step (a) above, the grinding is characterized by being carried out at 40 to 60 rpm for 1 to 8 hours.
[0014] More specifically, in step (a) above, the crushing is characterized by being performed by repeating the process of adding waste insulation material after crushing for 30 minutes or more at least once.
[0015] More specifically, in step (b) above, the stirring is performed continuously until step (c) begins in order to prevent sedimentation of the slurry and maintain a uniform state.
[0016] More specifically, in step (c) above, the solids are separated and the remaining filtrate is reused in step (a).
[0017] In addition, the recycled powder according to one embodiment of the present invention is characterized by being manufactured by a method for manufacturing recycled powder by wet crushing of the waste thermal insulation material.
[0018] In addition, a waterproofing agent composition according to one embodiment of the present invention is characterized by including the recycled powder.
[0019] More specifically, the waterproofing agent composition is characterized by containing cement, water glass, and the recycled powder in a ratio of about 1:1.5:3.
[0020] In addition, a cement mixture according to one embodiment of the present invention is characterized by including the recycled powder.
[0021] More specifically, the cement mixture is composed of 20 to 50 weight% cement and 50 to 80 weight% filler, and the filler is characterized by being composed of 40 to 95 weight% sand and 5 to 60 weight% recycled powder.
[0022] In addition, the ceramic bead slurry for fire extinguishing according to one embodiment of the present invention is characterized by including the recycled powder.
[0023] More specifically, the above-described ceramic bead slurry for extinguishing fires is characterized by having a composition ratio of 45 to 73 weight% distilled water, 25 to 53 weight% solid composition, and 0.1 to 5 weight% sodium alginate, wherein the solid composition is composed of 35 to 85 weight% recycled powder and 15 to 65 weight% extinguishing capsule.
[0024] In addition, a fire extinguishing ceramic bead according to one embodiment of the present invention is manufactured by dropping the fire extinguishing ceramic bead slurry into a molding water, solidifying it for 24 hours or more, and then drying it for 24 hours or more, wherein the molding water is composed of 90% by weight of water and 10% by weight of calcium chloride. Effects of the invention
[0025] A method for manufacturing recycled powder according to one embodiment of the present invention has the technical effect of being able to process waste insulation material more economically and quickly to convert it into a recyclable powder form.
[0026] In addition, the above-mentioned method for manufacturing recycled powder has the effect of minimizing wastewater generation and significantly reducing environmental burden by recirculating the solvent used in the wet grinding process.
[0027] A waterproofing agent composition according to one embodiment of the present invention can secure excellent water resistance and seismic performance by including the recycled powder, thereby effectively suppressing corrosion caused by moisture penetration and condensation (CUI) occurring in industrial facility piping, etc.
[0028] A cement mixture according to one embodiment of the present invention has the effect of improving mechanical properties, such as compressive strength, by utilizing the recycled powder as a construction filler.
[0029] In addition, the above cement mixture has the effect of high applicability at construction sites because it can secure stable performance without cracking even when replacing a portion of the sand.
[0030] Digestion beads according to one embodiment of the present invention have the effect of being easily manufactured even under non-heating conditions using a solid slurry containing the recycled powder.
[0031] In addition, since the above-mentioned fire extinguishing beads are formed by a reaction-based gelation method of sodium alginate and calcium chloride, they have the effect of simultaneously ensuring physical stability and fire extinguishing performance when dropped into high-temperature environments such as wildfires. Brief explanation of the drawing
[0032] FIG. 1 is a flowchart illustrating the sequence of a recycling method through wet crushing of waste thermal insulation material according to one embodiment of the present invention. Figure 2 is a figure showing the difference in volume of the slurry before and after drying in a recycling method of waste thermal insulation material through wet crushing according to one embodiment of the present invention. Figure 3 is a figure showing the ion exchange of a fire extinguishing ceramic bead slurry prepared according to one embodiment of the present invention by dropping it into molding water (left) and drying the gelled fire extinguishing ceramic beads (right). Figure 4 is a graph showing the particle size distribution of the crushed material according to the size of the ball mill soft medium in a recycling method of waste thermal insulation material through wet crushing according to one embodiment of the present invention. Figure 5 is a graph showing the particle size distribution of the crushed material according to the crushing time of a recycling method through wet crushing of waste thermal insulation material according to one embodiment of the present invention. Figure 6 is an SEM image of the crushed material of a recycling method through wet crushing of waste insulation material according to one embodiment of the present invention. Specific details for implementing the invention
[0033] The following detailed description of the present invention refers to the accompanying drawings, which illustrate specific embodiments in which the present invention may be practiced. These embodiments are described in sufficient detail to enable those skilled in the art to understand and practice the present invention. Various embodiments of the present invention may differ from one another, but this does not mean that they must be mutually exclusive. For example, specific shapes, structures, and characteristics described herein may be modified or applied to other embodiments without departing from the technical spirit of the present invention.
[0034] In addition, it should be understood that the location or arrangement of components in each embodiment may be changed without departing from the spirit and scope of the invention. Accordingly, the following detailed description is not intended to be taken in a limiting sense, and the scope of the invention is limited by the appended claims and only by equivalents. Similar reference numerals in the drawings refer to the same or similar functions across various aspects.
[0035] Hereinafter, in order to enable a person skilled in the art to easily practice the present invention, preferred embodiments of the present invention will be described in detail with reference to the attached drawings.
[0037] First, with reference to FIG. 1, a recycling method through wet crushing of waste thermal insulation material according to one embodiment of the present invention will be described.
[0038] FIG. 1 is a flowchart illustrating the sequence of a recycling method through wet crushing of waste thermal insulation material according to one embodiment of the present invention.
[0039] The recycling method of waste insulation material through wet crushing according to the present invention corresponds to a method for converting waste insulation material into a powder form that can be recycled economically and efficiently.
[0040] As illustrated in FIG. 1, the recycling method (S1000) of the present invention through wet crushing of waste thermal insulation material comprises: (a) step (S100) of introducing waste thermal insulation material and water into a ball mill and wet crushing to produce a slurry; (b) step (S200) of stirring to prevent sedimentation of the slurry; (c) step (S300) of filtering and dewatering the slurry to separate solids; and (d) step (S400) of drying and crushing the separated solids to produce a recycled powder.
[0042] First, step (a), which involves feeding the waste insulation material and water into a ball mill and wet-grinding to produce a slurry, is a type of pretreatment process in which the waste insulation material is fed into a ball mill together with water and wet-grinded to produce a slurry with uniform particle size.
[0043] The ball mill described above is a crusher containing steel balls or stones inside a cylinder that crushes objects through collision and friction when the object to be crushed is introduced and operated. Since the ball mill crushes materials using various crushing mechanisms such as collision, friction, and crushing, it is characterized by its ability to crush materials into particles of uniform size. This characteristic helps to uniformly crush waste insulation materials that are irregular and difficult to crush due to their fibrous structure. In addition, the ball mill is highly suitable for the present invention because it enables large-scale crushing, allowing for mass processing, and can perform wet crushing by introducing water, thereby enabling the immediate production of crushed material in the form of a slurry.
[0045] In addition, step (a) above involves feeding waste insulation material and water together into a ball mill to perform wet grinding, thereby fundamentally preventing the scattering of glass fibers, fine powder, and fiber fragments generated during the grinding of waste insulation material. In a wet environment, dust does not float into the air, which reduces the risk of inhalation by workers and allows for more stable compliance with environmental regulations required in industrial sites. While conventional technology suppressed dust generation by spraying a small amount of water, the present invention creates a complete slurry state by grinding with sufficient water; this not merely suppresses dust but fundamentally prevents the generation of dust itself, thereby enhancing work safety and environmental suitability.
[0046] Unlike dry grinding, this wet grinding method has the advantage of maintaining stable grinding efficiency without generating excessive heat and preventing particle aggregation, thereby enabling uniform grinding up to the target particle size range. Additionally, water cushions the impact, reducing equipment wear and increasing process stability.
[0047] Furthermore, in the present invention, water is sufficiently added to produce a crushed material in a slurry state, so it can be continuously linked with subsequent stirring, filtration, and drying steps, and the recovered filtrate can be reused in step (a), thereby reducing the environmental burden and operating costs of the entire process simultaneously.
[0048] More specifically, in step (a) above, the waste insulation material is characterized by being crushed to an average particle size of 1 to 100 μm and formed into a slurry. If the waste insulation material is crushed to a particle size larger than 100 μm, fiber fragments remain intact, making powdering impossible. Furthermore, if the particle size is too large, sedimentation accelerates, and when the slurry is subsequently filtered, it quickly accumulates on the surface of the filter, hindering the drainage of the filter. On the other hand ,When waste insulation is crushed to a size smaller than 1 μm, it is not filtered out by the filtration filter and passes through the filter, resulting in powder loss. It also becomes a colloidal state, which reduces dehydration ability and consequently significantly prolongs the drying time.
[0049] More specifically, the waste thermal insulation material is characterized by being crushed to an average particle size of 10 to 100 μm and formed into a slurry. If the particle size is larger than 100 μm, the applicability of the waterproofing agent is reduced when the recycled powder is used in a waterproofing agent, and the surface becomes rough after application. On the other hand, if the particle size is smaller than 10 μm, the viscosity of the waterproofing agent increases excessively, making application difficult. Furthermore, when the recycled powder is used in a cement mixture, particles that are too small or too large cannot sufficiently perform the role of a cement filler. Also, when the recycled powder is used in digestion beads, if the particle size is too large, gelation does not occur, making it impossible to manufacture digestion beads; and if the particles are too small, the surface area becomes excessively large, causing gel to form rapidly, which prevents the formation of spherical beads and results in a decrease in digestion function.
[0050] More specifically, in step (a) above, the ball mill is characterized by using alumina balls of 10 to 40 mm as the grinding medium. To find the optimal grinding medium capable of obtaining recycled powder with a desired particle size of 1 to 100 μm, Cerakwool and mineral wool were fed into a ball mill and wet-ground with 160 L of water. At this time, the grinding was carried out at 50 rpm for 24 hours, and the grinding was performed using alumina balls of 10, 20, 30, 40, and 50 mm as the grinding medium, respectively. As shown in FIG. 4, it was observed that the size of the ball mill should be 10 to 40 mm to ensure that the 1 to 100 μm range predominates in the grinding results. In particular, it was confirmed that using a ball mill of 20 to 40 mm was the most suitable.
[0051] More specifically, in step (a) above, the ball mill is characterized by performing grinding at 40 to 60 rpm. If the ball mill rotation speed is less than 40 rpm, the falling motion of the balls is not sufficiently formed, so the waste insulation material is not effectively cut or ground, and problems may occur where long fibers remain or large particles remain intact. In addition, the grinding efficiency decreases, increasing the process time, and sedimentation occurs rapidly within the slurry, which may result in a decrease in the uniformity of dispersion. Conversely, if the ball mill rotation speed is greater than 60 rpm, the impact force of the balls becomes excessively large, which may lead to over-grinding of the material or uneven particle size distribution, and increased wear on the liners and balls inside the equipment, which may result in a decrease in the lifespan of the device and an increase in energy consumption. Furthermore, there is a possibility that heat generation due to excessive impact may increase, causing changes in the viscosity of the slurry or aggregation.
[0052] More specifically, in step (a) above, the grinding is characterized by being carried out for 1 to 8 hours. To find the optimal grinding time to obtain recycled powder with a desired particle size of 1 to 100 μm, Cerakwool and mineral wool were fed into a ball mill and wet-ground with 160 L of water. At this time, grinding was carried out at 50 rpm using 20 mm alumina balls, and the results of grinding for 2 hours, 4 hours, 6 hours, 8 hours, and 12 hours were analyzed. As shown in Fig. 5, when grinding for more than 12 hours, the particles of the ground material were excessively small, while similar particle size results were obtained when grinding for 2 hours, 4 hours, 6 hours, and 8 hours. That is, it was confirmed that powder with an optimal particle size could be obtained when ground for 1 to 8 hours, and among them, grinding for 2 hours was the most efficient in terms of time.
[0053] More specifically, in step (a) above, the grinding is characterized by repeating the process of grinding for at least 30 minutes and then adding waste insulation material at least once. By adopting this grinding method, the basic material is sufficiently fined for 30 minutes to form a stable grinding environment inside the ball mill, and then new waste insulation material is added stepwise. This prevents problems such as increased load on the ball mill, clumping, and uneven grinding that occur when large initial fiber lumps or long fibers are excessively added at once. Furthermore, the repeated grinding process gradually homogenizes the particle size distribution and induces all inputs to converge to the same level of fine particle size, thereby ensuring a uniform slurry quality. In addition, stepwise addition suppresses a rapid increase in slurry viscosity and solid content concentration, which has the effect of improving the stability of the entire process leading up to the stirring and filtration processes.
[0055] Next, step (b) is a stirring step to prevent sedimentation of the slurry, and the slurry is continuously stirred at a constant speed to maintain a uniform suspension state. Since waste thermal insulation materials contain fibrous particles, they may settle in water; if sedimentation occurs, non-uniformity of concentration occurs within the slurry, which may reduce the efficiency of subsequent filtration and dewatering processes. In other words, some parts may contain a large amount of solids, resulting in a slow filtration speed, while others may contain less solids, resulting in a faster filtration speed and thus uneven filtration quality. Therefore, step (b) is a step that maintains the viscosity and concentration of the slurry at a constant level and prevents the aggregation of solids, thereby enabling stable filtration and drying processes.
[0056] More specifically, the stirring step is performed to prevent the slurry obtained by wet grinding from settling rapidly in a stationary state and to maintain a state in which the solids are uniformly dispersed. By continuing the stirring until step (c), which involves filtration and dewatering of the slurry, begins, the concentration and viscosity of the slurry can be stably maintained, and a solid of a certain quality can be secured in subsequent processes.
[0058] Step (c) above is a step of separating solids by filtering and dewatering the slurry uniformly stirred in Step (b), and is a process of recovering solids by passing them through a filter mesh or filter paper while simultaneously separating the filtrate. Since the crushed waste insulation material contains fine fibrous particles, moisture must be effectively removed through the filtration and dewatering process to produce a uniform and high-quality powder after the subsequent drying step.
[0059] More specifically, the filtrate separated in step (c) above is water used for wet crushing of waste insulation material, and since the slurry is completely filtered, it can be reused in step (a). Therefore, by recirculating the filtrate separated in step (c) back to step (a) for reuse, the amount of solvent input into the entire process can be reduced, thereby reducing operating costs, and the amount of wastewater generated can be reduced, thereby reducing the environmental burden.
[0060] In addition, waste insulation material is wet-crushed and crushed in a state where long fibers and short fibers are mixed, as shown in Fig. 6. At this time, since the long fibers are heavier than other particles, they settle first to form a primary filter layer on the surface of the filter paper, while the short fibers and fine particles are layered on top to naturally form a secondary filter layer. This multi-layered filter structure has the effect of increasing filtration efficiency and improving the separation of solids. In particular, since even fine particles can be stably filtered out, the recovery rate of recycled powder increases, and high-quality powder with a more uniform particle size distribution can be manufactured.
[0062] It is characterized by performing drying until the moisture content is lower than 0.5 weight%. If drying is performed until the moisture content is lower than 0.5 weight%, the solids become too hard, making it difficult to crush and difficult to secure uniform particles. In addition, if over-dried, dust is easily generated in the powder state, posing a risk of inhalation by workers. On the other hand, if drying is completed with a moisture content higher than 5 weight%, step (d) above is a step of manufacturing recycled powder by drying and crushing the solids separated in step (c). Since waste insulation material contains some moisture due to its fibrous structure, a stable powder form is manufactured through a sufficient drying process. Furthermore, as the solids in the form of a slurry are converted into actual powder through drying, the volume can be reduced by more than 90% as shown in FIG. 2, thereby reducing waste disposal costs and improving the economic efficiency of the recycling process.
[0063] More specifically, the above step (d) may be in the form of a paste rather than a powder when the moisture content of the solid is 0.5 to 5 weight%, and when the recycled powder is subsequently combined with cement or a waterproofing agent, the remaining moisture in the powder may cause the overall composition ratio to become unstable, thereby reducing reproducibility.
[0065] The recycled thermal insulation powder produced by the above method has a uniform particle size due to wet grinding, resulting in excellent dispersibility when mixed with various binders and resins. Furthermore, because it undergoes dehydration and drying processes to achieve a low moisture content and stability, precise mixing ratios can be achieved when utilizing it as a waterproofing agent, cement, or ceramic beads for fire extinguishing. Additionally, since the form of the waste thermal insulation is altered solely through physical treatment, its heat resistance and non-flammability are maintained, making it suitable for use as fire extinguishing beads or fillers for reinforcing insulation.
[0067] A waterproofing agent composition containing the above-mentioned recycled thermal insulation powder can improve the recycling rate of existing waste thermal insulation while simultaneously enhancing waterproofing performance by including the recycled powder as a main component. Since the recycled powder is an SiO2-based powder obtained by crushing inorganic fibers such as waste glass wool and waste mineral wool, it acts as an aggregate within the waterproofing agent and exhibits excellent bonding strength with the binder due to its large surface area.
[0068] In addition, the waterproofing agent composition of the present invention has the advantage of being able to be mixed and used at a composition ratio suitable for the work site by adjusting the content of recycled powder, and carbon emissions can be reduced through the active utilization of recycled powder from waste insulation materials. At this time, the content of the recycled powder can be adjusted to 30 to 60 weight percent, and as the viscosity changes according to the content of the recycled powder, it has the effect of being easily applied using various methods such as brushes, rollers, and air sprays.
[0069] More specifically, the waterproofing agent composition is characterized by containing cement, water glass, and the recycled powder in a ratio of approximately 1:1.5:3. When mixed in this ratio and applied as a waterproofing agent, it was confirmed that the adhesion was excellent and almost no cracks occurred.
[0071] Next, a cement mixture containing recycled powder prepared according to one embodiment of the present invention will be described. The cement mixture is prepared by utilizing the recycled powder of the present invention as a filler, and has the effect of improving the strength and durability of the cement matrix.
[0072] More specifically, the cement mixture is composed of 20 to 50 weight% cement and 50 to 80 weight% filler, and the filler is characterized by being composed of 40 to 95 weight% sand and 5 to 60 weight% recycled powder. If the cement content is less than 20 weight%, it does not sufficiently function as a binder, and cracks may occur after construction; if the cement content is greater than 50 weight%, shrinkage deformation increases, which may also cause cracks and make construction difficult. When the recycled powder in the filler is less than 5 weight%, almost no improvement in strength and water resistance is observed after cement construction; conversely, when the recycled powder is more than 60 weight%, there is a problem that the viscosity of the mixture increases and the binding strength decreases.
[0074] Next, a ceramic bead slurry for fire extinguishing comprising recycled powder prepared according to one embodiment of the present invention will be described. The ceramic bead slurry for fire extinguishing is a composition in the form of a slurry prepared by including the recycled powder of the present invention as a main component, and is used as a base material for producing fire extinguishing beads through a gelation reaction under non-heating conditions. The recycled powder is an inorganic-based fine particle that serves as a filler and a heat resistance reinforcing agent for the beads, and is uniformly dispersed in the slurry state to contribute to the formation of a stable gel structure.
[0075] More specifically, the above-mentioned ceramic bead slurry for fire extinguishing is composed of 45 to 73 weight% distilled water, 25 to 53 weight% solid composition, and 0.1 to 5 weight% sodium alginate, and the above-mentioned solid composition is composed of 35 to 85 weight% recycled powder and 15 to 65 weight% fire extinguishing capsule. The above-mentioned fire extinguishing capsule is a microcapsule containing a fire extinguishing agent component in advance, and means that the component is solidified, such as bicarbonate, phosphate-based fire extinguishing agent, pyrolytic coolant such as ammonium sulfate / ammonium nitrate, endothermic substance such as magnesium / aluminum hydroxide, or flame retardant / fire extinguishing agent composite powder.
[0076] In the solid composition of the above-mentioned ceramic bead slurry composition for fire extinguishing, if the content of recycled powder is less than 35 weight%, the inorganic filling effect inside the bead is not sufficiently expressed, which may result in a decrease in the strength and heat resistance of the bead and a reduction in fire extinguishing performance. On the other hand, if the content of recycled powder is more than 85 weight%, the proportion of fine particles increases, leading to increased viscosity, and consequently, the gelation reaction of sodium alginate does not occur well, resulting in a problem where the shape of spherical beads is not properly formed.
[0077] The above-mentioned ceramic bead slurry for fire extinguishing is uniformly stirred and then dropped into a molding solution composed of water and calcium chloride to gel into a bead shape. This is because sodium alginate, a component of the ceramic bead slurry for fire extinguishing, undergoes an ion exchange reaction with calcium chloride inside the molding solution to form a gel structure and solidify. More specifically, the alginate chains on the outer edge of the slurry are connected by calcium ions to form a membrane, thereby gelling and forming a fire extinguishing bead shape. As shown in FIG. 3, the ceramic bead for fire extinguishing of the present invention is manufactured by undergoing a substitution and gelation process in the molding solution for 24 hours, followed by a drying step of at least 24 hours.
[0078] Although the present invention has been described above with specific details such as specific components, limited embodiments, and drawings, this is provided only to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments, and a person skilled in the art to which the invention belongs can make various modifications and variations from this description.
[0079] Accordingly, the technical concept of the present invention should not be limited to the embodiments described above, and not only the claims set forth below, but also equivalents and equivalent variations thereof shall be considered to fall within the scope of the technical concept of the present invention.
Claims
Claim 1 A method for recycling waste insulation material comprises: (a) a step of introducing waste insulation material and water into a ball mill and wet-grinding to produce a slurry; (b) a step of stirring to prevent sedimentation of the slurry; and (c) a step of filtering and dewatering the slurry to separate solids. A method for recycling waste thermal insulation through wet grinding, comprising: (d) a step of drying and grinding the separated solids to produce recycled powder; wherein, in step (a), the waste thermal insulation is ground to a particle size of 1 to 100 μm to form a slurry, the ball mill uses alumina balls of 10 to 40 mm as a grinding medium, the grinding is carried out at 40 to 60 rpm for 1 to 8 hours, and the operation of adding waste thermal insulation after grinding for 30 minutes or more is repeated at least once; in step (b), the stirring is continuously performed until step (c) begins to prevent sedimentation of the slurry and maintain a uniform state, and in step (c), the filtered liquid remaining after separating the solids is reused from step (a). Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 Recycled powder manufactured by the method of claim 1 above Claim 9 Waterproofing agent composition comprising the recycled powder of claim 8 above Claim 10 In claim 9, the waterproofing agent composition is characterized by comprising cement, water glass, and the recycled powder in a ratio of 2:3:
6. Claim 11 A cement mixture comprising the recycled powder of claim 8 above Claim 12 A cement mixture according to claim 11, characterized in that it is composed of a composition ratio of 20 to 50 weight% cement and 50 to 80 weight% filler, wherein the filler is composed of 40 to 95 weight% sand and 5 to 60 weight% recycled powder. Claim 13 A ceramic bead slurry for fire extinguishing comprising the recycled powder of claim 8 above Claim 14 The fire extinguishing ceramic bead slurry according to claim 13 above is characterized in that the fire extinguishing ceramic bead slurry comprises a composition ratio of 45 to 73 wt% distilled water; 25 to 53 wt% solid composition; and 0.1 to 5 wt% sodium alginate, wherein the solid composition comprises a composition ratio of 35 to 85 wt% recycled powder; and 15 to 65 wt% fire extinguishing capsules in which a fire extinguishing component has been solidified. Claim 15 A fire extinguishing ceramic bead slurry according to claim 13 above is prepared by dropping it into molding water, solidifying it for at least 24 hours, and then drying it for at least 24 hours, wherein the molding water is composed of 90% by weight of water and 10% by weight of calcium chloride.
Citation Information
Patent Citations
Environment-friendly type baking-free building blocks and manufacturing method thereof
CN101362640A
Microbead-wrapped foam slow-release stopping agent for fire prevention and extinguishing of coal mine
CN112127936A
Treatment of industrial waste containing glass fiber
JP1998053451A
Process for the recovery of high purity carbon fromwaste carbon sludge
KR1020020037532A
Manufacturing method of insulation board using glass fiber insulation waste
KR102714632B1