Flame-retardant polyamide molding formulation for insulation of electrical components
The polyamide molding formulation with a specific flame-retardant composition addresses the challenge of achieving high flame retardancy, elongation, and minimal mass loss, providing excellent electrical insulation and mechanical stability.
Patent Information
- Application Number
- KR1020247002741
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-29
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Existing polyamide molding formulations face challenges in achieving excellent flame retardancy with low phosphorus content, while maintaining high elongation at break and minimizing mass loss at high temperatures, and they often suffer from migration issues.
A polyamide molding formulation comprising a polyamide matrix with specific carbon atoms per amide unit, combined with a flame-retardant composition containing metal-free aryl phosphate, aryl phosphonate, carbohydrate polyol, and melamine cyanurate, with a phosphorus content of 0.5% to 1.5% by weight, and optionally phosphorus-free flame retardants.
The formulation achieves a UL 94 fire resistance rating of V-0, minimal mass loss due to migration, high elongation at break, and excellent adhesion to metallic surfaces, ensuring effective electrical insulation and mechanical stability even at high temperatures.
Smart Images

Figure 112024009156461-PCT00001 
Figure 112024009156461-PCT00002 
Figure 112024009156461-PCT00003
Abstract
Description
Technology Field
[0001] The present invention relates to a flame-retardant polyamide molding formulation having a low phosphorus content. Background Technology
[0002] EP 150511 A1 discloses a powdered polyamide composition containing an alkyl phosphonate for use in 3D printing.
[0003] EP 3127937 A1 demonstrated the effectiveness of metal phosphinates in providing flame-retardant polyamides. According to the verbal evaluation of the examples, the addition of melamine cyanurate should be avoided.
[0004] EP 1731559 A1 proposed melamine cyanurate and phosphorus compounds combined with alcohols as flame retardants for polyamides. These achieve a UL 94 rating of V-0, but comparative testing of the present invention demonstrates increased mass loss due to migration. EP 1731559 A1 did not consider either such mass loss or the elongation at break of the composition.
[0005] US 2018 / 003771 A1 recommended providing flame retardancy of polyamides using only melamine cyanurate and polyols. Mechanical requirements were not disclosed.
[0006] The object of the present invention was to provide a polyamide molding formulation that exhibits excellent flame retardancy at low phosphorus content and undergoes only very little mass loss at high temperatures; such a molding formulation must also be characterized by a high elongation at break.
[0007] Surprisingly, it was found that flame retardants having a low content of phosphorus-containing compounds can be advantageously used for polyamide molding formulations.
[0008] The present invention relates to a polyamide molding formulation comprising:
[0009] (A) A polyamide matrix comprising one or more polyamides having at least 8 carbon atoms per amide unit,
[0010] (B) A flame-retardant composition comprising:
[0011] (B1) At least one metal-free aryl phosphate,
[0012] (B2) At least one aryl phosphonate,
[0013] (B3) Carbohydrate polyol,
[0014] (B4) Melamine cyanurate,
[0015] (B5) Optionally, phosphorus-free flame retardant,
[0016] Here, the phosphorus content in the total flame-retardant composition is 0.5% to 1.5% by weight, preferably 0.75% to 1.25% by weight, based on the polyamide molded formulation.
[0017] Provides a polyamide molding formulation.
[0018] Additionally, the present invention provides a use of the polyamide molding formulation of the present invention for the manufacture of parts.
[0019] Additionally, the present invention provides a method for insulating current-accompanied components.
[0020] Additionally, the present invention provides a hybrid part comprising a coated metal body, wherein the coating comprises a polyamide molding compound.
[0021] Additionally, the present invention provides a hybrid component for the transmission of electric current, preferably in high-voltage and low-voltage systems, more preferably in high-voltage systems.
[0022] The polyamide molding formulations of the present invention, hybrid parts comprising the molding formulations of the present invention, and uses according to the present invention are described below by exemplary examples, but there is no intention to limit the present invention to these exemplary embodiments. Where ranges, formulas, or classes of compounds are mentioned below, they are intended to encompass all sub-ranges and sub-groups of compounds that can be obtained by excluding individual values (ranges) or compounds, as well as the corresponding ranges or groups of compounds explicitly mentioned. Where literature is cited in the context describing the present invention, its entire contents are intended to be part of the disclosure of the present invention. Where % values are provided below, unless otherwise noted, they are values in weight %. Percentage values for composition are based on the total composition unless otherwise noted. Where average values are provided below, unless otherwise noted, they are mass averages (weight averages). Where measurements are provided below, unless otherwise noted, these measurements were determined at a pressure of 101325 Pa and a temperature of 25°C.
[0023] The scope of protection includes the product of the invention as itself, as well as finished and packaged forms commonly used in the commercial market, possibly in a crushed form, to the extent that they are not defined in the claims.
[0024] Arbitrarily different units of the polyamide follow a statistical distribution. The statistical distribution may have a block-type configuration with an arbitrary desired number of blocks and an arbitrary desired order, or they may follow a randomized distribution; they may also have an alternating configuration or otherwise form a gradient along the polymer chain; in particular, they may also form any mixed form in which groups having different distributions may be arbitrarily linked to one another. Specific embodiments may result in limitations on the statistical distribution as a result of such embodiments. In all areas not affected by such limitations, there is no change in the statistical distribution.
[0025] The advantage of the polyamide molded formulations of the present invention is that they have excellent fire resistance, where the UL 94 fire resistance rating is V-0.
[0026] An additional advantage of the polyamide molding formulations of the present invention is that they have a high elongation at break.
[0027] An additional advantage of the polyamide molding formulation of the present invention is that, after storage at high temperatures for a relatively long period, the migration (whitening, mass loss) of low molecular weight components on the surface occurs only very minimally.
[0028] An additional advantage of the polyamide molding formulation of the present invention is that there is no loss of flame retardancy due to mass loss caused by migration.
[0029] An additional advantage is the particularly excellent adhesion of the polyamide molding formulation of the present invention to metallic surfaces. Specific details for implementing the invention
[0030] Polyamide matrix (A)
[0031] Preferably, the polyamide of the polyamide matrix (A) has 8 to 16 carbon atoms per amide unit as a statistical average over the entire polymer, more preferably 9 to 14 carbon atoms, and particularly preferably 10 to 12 carbon atoms. More preferably, the polyamide of the polyamide matrix (A) has at least 8 carbon atoms per amide unit in all monomer units.
[0032] Polyamides can be homopolymers, copolymers, or blends of different polyamides. Differences in polyamides may appear, for example, in the use of different monomers in polymerization, different molar mass distributions (e.g., which may appear as different viscosities), or different terminal groups.
[0033] The polyamide is preferably selected from PA 8, PA 9, PA 10, PA 11, PA 12, PA 6.10, PA 6.12, PA 6.14, PA 8.10, PA 9.10, PA 9.12, PA 10.10, PA 10.12, PA 12.12, PA 6.16, PA 10.16; more preferably PA 6.12, PA 10.10, PA 10.12, PA 11 and PA 12; particularly preferably PA 11 and PA 12.
[0034] The polyamide molding formulation preferably does not contain any other polyamide other than the polyamide of the polyamide matrix (A).
[0035] Flame-retardant composition (B)
[0036] The flame-retardant composition of the polyamide molding formulation of the present invention preferably comprises the following:
[0037] 15% to 55% by weight, preferably 25% to 50% by weight, more preferably 30% to 45% by weight of melamine cyanurate (B4);
[0038] 10% to 30% by weight, preferably 15% to 25% by weight, more preferably 17% to 23% by weight of carbohydrate polyol (B3);
[0039] 5% to 30% by weight, preferably 7% to 25% by weight, more preferably 13% to 23% by weight of aryl phosphonate (B2);
[0040] 5 to 30 weight%, preferably 7 to 25 weight%, more preferably 13 to 23 weight% of metal-free aryl phosphate (B1);
[0041] 0 to 15 weight%, preferably 3 to 12 weight%, more preferably 5 to 10 weight% of phosphorus-free flame retardant (B5);
[0042] Here, the sum of (B1), (B2), (B3), (B4) and (B5) provides 100 weight% of component (B).
[0043] Preferably, the mass ratio of (B1) to (B2) in the flame-retardant composition of the polyamide molding formulation of the present invention is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5.
[0044] Phosphorus-free flame retardant (B5) is different from the flame retardants according to B3 and B4. Urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, and calcium hydroxide are preferred. Halogenated flame retardants may also be added.
[0045] Preferably, the phosphorus-free flame retardant (B5) does not contain halogenated material.
[0046] Melamine cyanurate(B4) is also understood to mean melamine condensation products such as melem, melam, and melon, but preferably to mean only melamine cyanurate (CA-RN 37640-57-6) itself.
[0047] Melamine cyanurate is used in powder form. It has a particle size D50, preferably 0.5 to 100 μm, more preferably 0.6 to 50 μm, particularly preferably 0.7 to 25 μm, very particularly preferably 0.8 to 5 μm, and particularly preferably 0.9 to 4 μm, measured by laser diffraction using a laser particle size analyzer in accordance with BS ISO 13320-1, version 2000-03-15. Preferably, measurements are performed using a Cilas 715 / 920 laser particle size analyzer.
[0048] Small particle size is desirable because it provides a smoother finish to the molded product.
[0049] Preferably, Carbohydrate polyols (B3) is a hydrocarbon that is substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally contains an ether group, preferably having at least 1 ether group.
[0050] Carbohydrate polyols are more preferably selected from triols, such as trimethylolpropane or glycerol or their derivatives, such as ditrimethylolpropane or diglycerol (formed through the monoetherification of two molecules of the mentioned compounds), or tetrols, such as erythritol, pentaerythritol or their ether-group-containing derivatives, such as di- or tripentaerythritol, pentols, such as xylitol or arabitol, hexols, such as mannitol, sorbitol, etc.; additionally, it is also possible to use higher adducts of the mentioned molecules, for example, branched or superbranched polyglycerols; and, of course, it is also possible to use mixtures of polyols. Erythritol, pentaerythritol, or di- or tripentaerythritol, particularly dipentaerythritol, are more preferred.
[0051] For the purposes of the present invention, aryl phosphonate (B2) is a polymer or oligomer having at least three repeating units, preferably three identical repeating units, and contains aromatic substituents in the backbone of the molecule.
[0052] The aryl phosphonate preferably contains the repeating unit presented in chemical formula (III):
[0053]
[0054] Here, R1 is an alkyl radical having 1 to 4 carbon atoms independently in each case, preferably methyl, and
[0055] Here, BAr is independently an aromatic radical in each case, preferably an aromatic radical having at least two rings, more preferably biphenylene or 4,4'-(propane-2,2-diyl)diphenylene.
[0056] Preferably, the aryl phosphonate contains an -BAr-OH group as a terminal group.
[0057] Particularly preferably, the aryl phosphonate contains the repeating unit presented in chemical formula (IV):
[0058]
[0059] Therefore, aryl phosphonates preferably contain bisphenol A terminal groups.
[0060] The aryl phosphonate preferably has an MVR (melt volume flow rate) of less than 100 ml / 10 min and, more preferably, at least 10 ml / 10 min, even more preferably at least 25 ml / 10 min, particularly preferably at least 50 ml / 10 min, and particularly preferably 65 to 90 ml / 10 min (measured according to ISO 1133 at 240°C and under a load of 1.2 kg).
[0061] metal-free Aryl Phosphate (B1) preferably contains at least two phosphate groups.
[0062] More preferably, the metal-free aryl phosphate comprises at least one unit of formula (I), preferably one or two units:
[0063]
[0064] and contains at least two units of formula (II), preferably two or three units:
[0065]
[0066] Here, the units of chemical formula (I) or (II) exist alternately, and
[0067] Here, the number of units according to chemical formula (II) is always one more than the number of units according to chemical formula (I), and
[0068] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, and
[0069] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical.
[0070] Preferably, the metal-free aryl group contains a phenyl radical as a terminal group, which can have any desired substitution by a C1 to C4 alkyl radical.
[0071] More preferably, the metal-free aryl phosphate contains a structural element of the formula (V):
[0072]
[0073] Particularly preferably, the metal-free aryl phosphate contains the structure of formula (VI):
[0074]
[0075] Here, Ar is meta- or para-phenylene, and Ph is phenyl.
[0076] Preferably, Ar is not a 4,4'-(propane-2,2-diyl)diphenylene radical.
[0077] The flame-retardant composition preferably does not contain any polyphosphate, any reaction product of melamine and polyphosphoric acid, or any derivative of phosphoric acid (III) and / or phosphoric acid (I).
[0078] The flame-retardant composition preferably does not contain any additional phosphorus-containing components other than components (B1) and (B2).
[0079] A preferred combination for the flame-retardant composition (B) is the following combination:
[0080] At least one unit of chemical formula (I), preferably one or two units:
[0081]
[0082] and at least one metal-free aryl phosphate (B1) containing at least two units of formula (II), preferably two or three units:
[0083]
[0084] Here, the units of chemical formula (I) or (II) exist alternately, and
[0085] Here, the number of units according to chemical formula (II) is always one more than the number of units according to chemical formula (I), and
[0086] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, but not the 4,4'-(propane-2,2-diyl)diphenylene radical,
[0087] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0088] Repeating unit of chemical formula (IV):
[0089]
[0090] and at least one aryl phosphonate (B2) containing bisphenol A as a terminal group;
[0091] A carbohydrate polyol (B3) substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally containing an ether group, preferably having at least 1 ether group;
[0092] Melamine cyanurate (B4);
[0093] and optionally, phosphorus-free flame retardants selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, calcium hydroxide (B5), optionally also halogenated flame retardants.
[0094] A more preferred combination for the flame-retardant composition (B) is the following combination:
[0095] At least one metal-free aryl phosphate (B1) containing a structural element of chemical formula (V):
[0096]
[0097] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, but not the 4,4'-(propane-2,2-diyl)diphenylene radical,
[0098] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0099] Repeating unit of chemical formula (IV):
[0100]
[0101] and at least one aryl phosphonate (B2) containing bisphenol A as a terminal group;
[0102] A carbohydrate polyol (B3) substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally containing an ether group, preferably having at least 1 ether group;
[0103] Melamine cyanurate (B4) having a particle size D50 of 0.5 to 100 μm, more preferably 0.6 to 50 μm, particularly preferably 0.7 to 25 μm, very particularly preferably 0.8 to 5 μm, and particularly preferably 0.9 to 4 μm, as measured by laser diffraction using a laser particle size analyzer according to BS ISO 13320-1, version 2000-03-15;
[0104] and optionally, phosphorus-free flame retardants (B5) selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, calcium hydroxide, optionally also halogenated flame retardants;
[0105] Here, the mass ratio of (B1) to (B2) is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5.
[0106] A particularly preferred combination for the flame-retardant composition (B) is the following combination:
[0107] At least one metal-free aryl phosphate (B1) having a structure of formula (VI) in an amount of 5% to 30% by weight:
[0108]
[0109] Here, Ar is meta- or para-phenylene, and
[0110] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0111] Repeating unit of formula (IV), 5% to 30% by weight:
[0112]
[0113] and at least one aryl phosphonate (B2) containing bisphenol A as a terminal group;
[0114] A carbohydrate polyol (B3) having at least 10% to 30% by weight, substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, and preferably having at least 1 ether group;
[0115] Melamine cyanurate (B4) having a particle size D50 of 0.5 to 100 μm, more preferably 0.6 to 50 μm, particularly preferably 0.7 to 25 μm, very particularly preferably 0.8 to 5 μm, and particularly preferably 0.9 to 4 μm, as measured by laser diffraction using a laser particle size analyzer according to BS ISO 13320-1, version 2000-03-15, in an amount of 15 wt% to 55 wt%;
[0116] and 0 to 15 weight% of a phosphorus-free flame retardant (B5) selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, and calcium hydroxide;
[0117] Here, the sum of (B1), (B2), (B3), (B4) and (B5) provides 100 weight% of component (B);
[0118] Here, the mass ratio of (B1) to (B2) is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5.
[0119] Preferably, the polyamide molding formulation of the present invention contains phosphorus from sources other than phosphorus-containing flame retardants, such as stabilizers, processing aids, or catalysts, in an amount of 5,000 ppm or less, preferably 1,000 ppm or less, more preferably 500 ppm or less, and particularly preferably 250 ppm or less.
[0120] Optionally, the polyamide molding formulation of the present invention comprises conventional processing aids, such as stabilizers, oxidation retardants, other agents that prevent thermal decomposition and degradation by ultraviolet rays, lubricants and release agents, coloring agents such as dyes and pigments, nucleating agents, plasticizers, etc.
[0121] Optionally, the polyamide molding formulation of the present invention, in addition to the described components, may optionally include two or more additional additives selected from one or more representative examples, such as stabilizers, other polymers, impact modifiers, plasticizers, coloring agents such as pigments and dyes, and processing aids, of the same type.
[0122] good oxidation stabilizer These include aromatic amines, sterically hindered phenols, hydroquinones, phosphites, phosphonites, thio-synergists, hydroxylamines, benzofuranone derivatives, acryloyl-modified phenols, etc. A very large number of these oxidation stabilizers are commercially available, for example, under the trade names Naugard 445, Irganox 1010, Irganox 1098, Irgafos 168, P-EPQ, or Lowinox DSTDP. Generally, the molded formulation contains about 0.01 wt% to about 2 wt%, preferably about 0.1 wt% to about 1.5 wt% of an oxidation stabilizer.
[0123] Additionally, the molding formulation may also include a UV stabilizer or a light stabilizer. Suitable UV stabilizer These are organic UV absorbers, e.g., benzophenone derivatives, benzotriazole derivatives, resorcinol, salicylates, oxalanilide, and phenyltriazine. Tetramethylpiperidine derivatives are HALS-type light stabilizers. UV stabilizers and light stabilizers may advantageously be used in combination. A very large number of types of both are commercially available; regarding dosage, the manufacturer's instructions may be followed.
[0124] Additionally, the molding formulation may include a hydrolysis stabilizer, for example, a monomeric, oligomeric, or polymeric carbodiimide or bisoxazolin.
[0125] Examples of other polymers that may be present in the molding composition as additives are polyetheramide or polytetrafluoroethylene (PTFE).
[0126] Shock modifier These are known to those skilled in the art. They contain functional groups derived from unsaturated functional compounds that are incorporated into the main chain polymer or grafted onto the main chain. The most commonly used are EPM or EPDM rubbers in which free-radical grafting of maleic anhydride has occurred. Rubbers of this type may also be used with unfunctionalized polyolefins, such as isotactic polypropylene, as described in EP-A-0 683 210.
[0127] plasticizer This is known to those skilled in the art from the literature [Gaechter / Mueller, Kunststoffadditive [Plastics additives], C. Hanser Verlag, 2nd edition, p. 296]. Examples of common compounds suitable for use as plasticizers are esters of p-hydroxybenzoic acid having 2 to 20 carbon atoms in the alcohol component or amides of arylsulfonic acid having 2 to 12 carbon atoms in the amine component, preferably amides of benzenesulfonic acid. Useful plasticizers include ethyl p-hydroxybenzoate, octyl p-hydroxybenzoate, i-hexadecyl p-hydroxybenzoate, Nn-octyltoluenesulfonamide, Nn-butylbenzenesulfonamide, or N-2-ethylhexylbenzenesulfonamide.
[0128] good pigment and / or dyes Examples of are mixed oxides, titanium dioxide, iron oxide, zinc sulfide, ultramarine, nigrosine, organic pigments such as phthalocyanine, quinacridone, perylene, nigrosine, anthraquinone, and pearlescent pigments.
[0129] good Processing aidsExamples of are paraffin, fatty alcohol, fatty acid amide, stearate such as calcium stearate, paraffin wax, montanate, or polysiloxane.
[0130] The polyamide molding formulation of the present invention preferably does not contain halogenated material.
[0131] The molding formulation of the present invention has a UL 94 fire resistance rating of V0. This rating is in accordance with UL guidelines, but preferably in accordance with DIN EN 60695-11-10:2014 for a test specimen having dimensions of 125 mm * 13 mm * 0.8 mm, taking into account Revision 1 (October 2015) of the said standard.
[0132] Preferably, the molding formulation of the present invention has an elongation at break of at least 50%, preferably at least 100%, more preferably at least 150%, and particularly preferably at least 200%. The elongation at break is measured for a tensile specimen of type 1A (DIN EN ISO 527-2) according to DIN EN ISO 527-1.
[0133] Preferably, the molding formulation of the present invention exhibits only very small migration of low molecular weight components after storage at high temperatures for a relatively long period. To this end, a test specimen having dimensions of 125 mm * 13 mm * 0.8 mm was stored at 150°C for 24 hours, and the amount of migrated material was determined. The method of determination is described in more detail in the examples. The mass loss due to migration is, based on the total molding formulation, preferably less than 1.1 wt%, more preferably less than 1.0 wt%, and particularly preferably less than 0.9 wt%.
[0134] Preferably, the molding formulation of the present invention has a UL 94 grade of V-0, a mass loss due to movement of less than 1.1 weight%, and an elongation at break of at least 50%.
[0135] The polyamide molding formulation of the present invention preferably does not contain additives that increase electrical conductivity, in particular conductive carbon black or carbon nanotubes.
[0136] A preferred polyamide molding formulation comprises the following:
[0137] (A) A polyamide matrix comprising one or more polyamides having, as a statistical average for the entire polymer, 8 to 16 carbon atoms per amide unit, more preferably 9 to 14 carbon atoms, and particularly preferably 10 to 12 carbon atoms;
[0138] (B) A flame-retardant composition comprising:
[0139] (B1) At least one metal-free aryl phosphate containing a structural element of chemical formula (V):
[0140]
[0141] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, but not the 4,4'-(propane-2,2-diyl)diphenylene radical,
[0142] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0143] (B2) Repeating unit of chemical formula (IV):
[0144]
[0145] and at least one aryl phosphonate containing bisphenol A as a terminal group;
[0146] (B3) A carbohydrate polyol substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally containing an ether group, preferably having at least 1 ether group;
[0147] (B4) Melamine cyanurate having a particle size D50 of 0.5 to 100 μm, more preferably 0.6 to 50 μm, particularly preferably 0.7 to 25 μm, very particularly preferably 0.8 to 5 μm, and particularly preferably 0.9 to 4 μm, as measured by laser diffraction using a laser particle size analyzer in accordance with BS ISO 13320-1, version 2000-03-15;
[0148] (B5) Optionally, phosphorus-free flame retardants selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, calcium hydroxide, optionally also halogenated flame retardants;
[0149] Here, the mass ratio of (B1) to (B2) is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5;
[0150] Here, the phosphorus content from the total flame-retardant composition is 0.5% to 1.5% by weight based on the polyamide molded formulation.
[0151] Likewise, a desirable polyamide molding formulation comprises the following:
[0152] (A) a polyamide matrix comprising one or more polyamides selected from PA 8, PA 9, PA 10, PA 11, PA 12, PA 6.10, PA 6.12, PA 6.14, PA 8.10, PA 9.10, PA 9.12, PA 10.10, PA 10.12, PA 12.12, PA 6.16, PA 10.16; more preferably PA 6.12, PA 10.10, PA 10.12, PA 11 and PA 12; particularly preferably a polyamide matrix comprising one or more polyamides selected from PA 11 and PA 12;
[0153] (B) A flame-retardant composition comprising:
[0154] (B1) At least one unit of formula (I), preferably one or two units:
[0155]
[0156] and at least one metal-free aryl phosphate containing at least two units of formula (II), preferably two or three units:
[0157]
[0158] Here, the units of chemical formula (I) or (II) exist alternately, and
[0159] Here, the number of units according to chemical formula (II) is always one more than the number of units according to chemical formula (I), and
[0160] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, but not the 4,4'-(propane-2,2-diyl)diphenylene radical,
[0161] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0162] (B2) Repeating unit of chemical formula (IV):
[0163]
[0164] and at least one aryl phosphonate containing bisphenol A as a terminal group;
[0165] (B3) A carbohydrate polyol substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally containing an ether group, preferably having at least 1 ether group;
[0166] (B4) Melamine cyanurate;
[0167] (B5) Optionally, phosphorus-free flame retardants selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, calcium hydroxide, optionally also halogenated flame retardants;
[0168] Here, the mass ratio of (B1) to (B2) is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5;
[0169] Here, the phosphorus content from the total flame-retardant composition is 0.5% to 1.5% by weight based on the polyamide molded formulation.
[0170] Additional desirable polyamide molding formulations include the following:
[0171] (A) A polyamide matrix comprising one or more polyamides having, as a statistical average for the entire polymer, 8 to 16 carbon atoms per amide unit, more preferably 9 to 14 carbon atoms, and particularly preferably 10 to 12 carbon atoms;
[0172] (B) A flame-retardant composition comprising:
[0173] (B1) At least one unit of formula (I), preferably one or two units:
[0174]
[0175] and at least one metal-free aryl phosphate containing at least two units of formula (II), preferably two or three units:
[0176]
[0177] Here, the units of chemical formula (I) or (II) exist alternately, and
[0178] Here, the number of units according to chemical formula (II) is always one more than the number of units according to chemical formula (I), and
[0179] Here, Ar is ortho-, meta-, para-phenylene, naphthylene, or biphenylene, but not the 4,4'-(propane-2,2-diyl)diphenylene radical,
[0180] Here, Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical;
[0181] (B2) Repeating unit of chemical formula (IV):
[0182]
[0183] and at least one aryl phosphonate containing bisphenol A as a terminal group;
[0184] (B3) A carbohydrate polyol substituted with at least 3, preferably at least 4, more preferably at least 5, and more preferably at least 6 hydroxyl groups, optionally containing an ether group, preferably having at least 1 ether group;
[0185] (B4) Melamine cyanurate;
[0186] (B5) Optionally, phosphorus-free flame retardants selected from urea and urea derivatives, magnesium hydroxide, aluminum hydroxide, aluminum sulfate, borax, boric acid and borate salts (e.g., zinc borate), ammonium sulfate, calcium hydroxide, optionally also halogenated flame retardants;
[0187] Here, the mass ratio of (B1) to (B2) is 0.25 to 4, preferably 0.33 to 3, more preferably 0.5 to 2, and particularly preferably 0.75 to 1.5;
[0188] Here, the phosphorus content from the total flame-retardant composition is 0.5% to 1.5% by weight based on the polyamide molded formulation;
[0189] Here, the molding formulation has a UL 94 rating of V-0, a mass loss due to movement of less than 1.1 wt%, and an elongation at break of at least 50%.
[0190] The present invention relates to the use of the polyamide molding formulation of the present invention for the manufacture of parts, and to parts, electrical parts, and electronic parts, such as preferably current-accompanied metal members, for use as fire-retardants, particularly in the automotive sector, preferably as coatings, covers, films, profiles, tubes, corrugated tubes, hollow bodies, sealants, exterior materials, brackets, housings, and covering materials.
[0191] In the method of the present invention for insulating a current-accompanying component, the component is preferably manufactured by compression molding, foaming, extrusion, co-extrusion, blow molding, 3D blow molding, co-extrusion blow molding, co-extrusion 3D blow molding, co-extrusion suction blow molding, extrusion coating, powder coating, or injection molding. These types of processes are known to those skilled in the art.
[0192] Preferably, the hybrid component of the present invention comprises a coated metal body, wherein the coating comprises a polyamide molding compound comprising:
[0193] (A) A polyamide matrix comprising one or more polyamides having at least 8 carbon atoms per amide unit,
[0194] (B) A flame-retardant composition comprising:
[0195] (B1) At least one metal-free aryl phosphate,
[0196] (B2) At least one aryl phosphonate,
[0197] (B3) Carbohydrate polyol,
[0198] (B4) Melamine cyanurate,
[0199] (B5) Optionally, phosphorus-free flame retardant,
[0200] Here, the phosphorus content from the total flame-retardant composition is 0.5% to 1.5% by weight, preferably 0.75% to 1.25% by weight, based on the polyamide molded formulation. The components of the polyamide molded formulation are described above.
[0201] Preferably, the phosphorus-free flame retardant (B5) does not contain halogenated flame retardants. More preferably, the entire coating does not contain halogenated materials. This is associated with the advantages of better corrosion protection and also better environmental friendliness; also, halogen-containing materials cannot be emitted even in the event of extreme heating such as metal fires.
[0202] The present invention also relates to a method for manufacturing this type of part. The method is characterized by forming a polyamide molding compound into a part by an extrusion process, a blow extrusion process, an injection-molding process, or an insert molding process.
[0203] Particularly in the case of hybrid parts, these can be formed after coating the metal body. It is also possible to mount additional attachments to the hybrid parts, such as plugs and sockets, screw connections, and connecting elements.
[0204] The polyamide molding formulation of the present invention has the advantageous characteristic of excellent moldability during formation, which means that delamination, cracking, shrinkage wrinkles, and similar effects do not occur in the coating of the polyamide molding formulation (also briefly referred to as polyamide coating below) during the formation of a hybrid part.
[0205] In particular, its excellent moldability ensures that the polyamide coating provides effective electrical insulation, especially in the high voltage range. In the high voltage range, a large amount of electric charge is transported over a long period. In this regard, a notable feature of the coating using the molding formulation of the present invention is its excellent temperature stability. This manifests in two ways: firstly, no significant mass loss occurs due to movement. This maintains excellent insulation properties (prevention of leakage current) between the external and current-accompanied metals, as well as on the surface of the polyamide coating. Secondly, the polyamide coating maintains mechanical stability even after a long time at high temperatures, for example, against vehicle vibrations, which means that cracks—particularly in the aforementioned molded body—do not occur, which would particularly reduce the insulation effect.
[0206] The hybrid component of the present invention may preferably be used in a vehicle, wherein the term "vehicle" is understood to mean any means of transport, namely water, land, and aerospace transport. The hybrid component is used, for example, within a current generating component as well as for transfer to a receiving source and for charge transfer in a power supply. Preferred use is in an electric drive vehicle, for example, in the series or parallel connection of an electric storage system or an electric generator, charge transfer from the electric storage system or generator system to a driving unit, and charge transfer to an additional electric-consuming system, preferably in a high-voltage system.
[0207] The hybrid component of the present invention may additionally be preferably used in fixed systems, such as power plants: wind turbines, fuel cells or electrolytic cells, hydroelectric power plants or other power plants, or in intermediate processing units such as substations, or in transmission facilities such as underground or seabed, or in cable systems and line systems buried in structures, such as bridges (which are particularly exposed to vibrations caused by climate and use).
[0208] The phosphorus content value in the article of the present invention represents the content of phosphorus as an element.
[0209] method
[0210] Differential Scanning Calorimetry (DSC):
[0211] DSC measurements were performed according to DIN EN ISO 11357-1: 2016.
[0212] Relative solution viscosity (η) rel ):
[0213] The sample was dissolved in m-cresol at 30°C (0.005 g / ml) and measured at 25.00°C using a viscosity measuring system (LAUDA PVS or Schott AVS Pro).
[0214] The molding formulation of the present invention has a UL 94 fire resistance rating of V-0. The rating is in accordance with the UL guidelines, but preferably in accordance with DIN EN 60695-11-10:2014 for a test specimen having dimensions of 125 mm * 13 mm * 0.8 mm, taking into account Revision 1 (October 2015) of the said standard.
[0215] For the determination of mass loss due to migration, a specimen (125 mm * 13 mm * 0.8 mm) was weighed at 23°C and subsequently heat-treated in an oven at 150°C for 24 hours according to IEC 60216-4. Subsequently, the rod was cooled at 23°C for 30 minutes and mechanically cleaned with an acetone-soaked wipe until no wipeable coating remained (mirror-finished sample). Then, the rod was dried at 23°C for 15 minutes and any electrostatic charge was removed using an ionization device. Mass loss is calculated as the average value of three samples weighed repeatedly. A negative value indicates mass loss due to migration.
[0216] The elongation at break was measured according to DIN EN ISO 527-1. Dumbbell-shaped specimen A1 according to Part 2 of the aforementioned standard was used. Measurements were performed at 23°C at a speed of 50 mm / min.
[0217] Elongation at break is particularly important in relation to the present invention, as the use of electrical insulators for covering electrical conductors must meet particularly demanding requirements, especially in high voltage ranges. It must be ensured that these conductors are bent up to 180° and that the insulator does not exhibit cracks, because such cracks would act as current bridges. For example, in automotive applications, it is evident that these requirements must be met with maximum certainty to avoid endangering people working in the engine compartment.
[0218] ingredient:
[0219] PA 6.10: Medium viscosity
[0220] PA 6.12: Medium viscosity
[0221] PA 10.12: Medium viscosity
[0222] PA 12: High viscosity
[0223] PA 12 / 6: Medium viscosity
[0224] Melamine Cyanurete (MC), Melapur MC 25 (BASF)
[0225] Dipentaerythritol from Perstorp
[0226] Fyrolflex® Sol-DP and ~RDP, trademarks of ICL IP America Inc., based in the United States.
[0227] ADK STAB FP-600, a product of Adeka, Polymer Additives Europe, based in France
[0228] Disflamoll® DPK, a trademark of Lanxess, Germany
[0229] Aflammit® PCO 900, a trademark of Thor Specialities Limited, based in the UK
[0230] Amgard® CU, a trademark of Lancet, Germany
[0231] Nofia® HM7000, a trademark of FRX Polymers, Inc., based in the United States.
[0232] The stabilizer mixture included an impact modifier, a stabilizer (thermal and / or oxidation), and a dye / pigment.
[0233] Example 1: General formulation procedure for polyamide molding formulations
[0234] The molded mixture was prepared on a co-rotating twin-screw extruder. The solid component was metered in through the main feeder, and the liquid component was metered in as a melt downstream thereof. The housing temperatures are listed in Table 1. Pelletization was performed by strand pelletization, and then dried for 12 hours in a drying-air-chamber dryer at 80°C.
[0235] Example 2: Preparation of test specimens
[0236] Test specimens were prepared by injection-molding according to DIN EN ISO 294-1 and DIN EN ISO 16396-2. The injection speed was 200 mm / s, the temperature of the mixture was 240°C in all cases, and the corresponding mold temperatures are shown in Table 1.
[0237] The following sample was implemented to determine typical material properties:
[0238] Multipurpose test specimen according to DIN EN ISO 527-2 Type 1A for mechanical testing
[0239] UL 94V and UL 94 test specimen for mass loss due to movement 172 mm x 12.7 mm x 0.8 mm
[0240] Electrical measuring plate 130 mm x 130 mm x 1 mm.
[0241] Example 3: Mechanical and Electrical Tests
[0242] The elongation at break was determined according to DIN EN ISO 527-1.
[0243] Dielectric strength was determined according to DIN EN 60243-1, AC K20 / K20.
[0244] Table 1: Manufacturing parameters for Example 2 (temperature in °C)
[0245]
[0246] Table 2: Results of the test according to Example 3 for the test specimen according to Example 2
[0247]
[0248] *nd: Undetermined
[0249]
[0250]
[0251] Examples Ex. 2, Ex. 7, Ex. 9, Ex. 14 and Ex. 18 This is an embodiment of the present invention.
[0252] Surprisingly, the examples suggest that when using the aryl phosphate of the present invention, particularly when using an aryl phosphate containing a phenylene group, the mass loss due to migration is less than when using a high molecular weight aryl phosphate containing a 4,4'-(propane-2,2-diyl)diphenylene group.
[0253] From the examples, it can be seen that the desired properties in terms of flame retardancy and mass loss due to migration can be achieved only by a combination of metal-free aryl phosphates and aryl phosphonates. In this regard, a combination of metal-free aryl phosphates and alkyl phosphonates is not effective.
Claims
Claim 1 A polyamide molding formulation comprising: (A) a polyamide matrix comprising one or more polyamides having at least 8 carbon atoms per amide unit; (B) a flame-retardant composition comprising: (B1) at least one metal-free aryl phosphate; (B2) at least one aryl phosphonate; (B3) a carbohydrate polyol; (B4) melamine cyanurate; (B5) optionally, a phosphorus-free flame retardant, wherein the metal-free aryl phosphate (B1) is at least one unit of formula (I): and containing at least two units of formula (II): Herein, the units of formula (I) or (II) exist alternately, wherein the number of units according to formula (II) is always one greater than the number of units according to formula (I), wherein Ar is ortho-, meta-, para-phenylene, naphthylene or biphenylene, wherein Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical, wherein the phosphorus content in the total flame-retardant composition is 0.5% to 1.5% by weight based on the polyamide molding formulation, and the mass loss is less than 1.1% by weight. Claim 2 A polyamide molding formulation according to claim 1, wherein the polyamide is selected from PA 8, PA 9, PA 10, PA 11, PA 12, PA 6.10, PA 6.12, PA 6.14, PA 8.10, PA 9.10, PA 9.12, PA 10.10, PA 10.12, PA 12.12, PA 6.16, and PA 10.
16. Claim 3 A polyamide molded formulation according to claim 1 or 2, wherein the mass ratio of (B1) to (B2) is 0.25 to 4, 0.33 to 3, 0.5 to 2, or 0.75 to 1.
5. Claim 4 In claim 1 or 2, the metal-free aryl phosphate (B1) is one or two units of formula (I): and a polyamide molding formulation containing two or three units of chemical formula (II): Here, the units of formula (I) or (II) exist alternately, where the number of units according to formula (II) is always one greater than the number of units according to formula (I), where Ar is ortho-, meta-, para-phenylene, naphthylene or biphenylene, and where Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical. Claim 5 A polyamide molding formulation according to claim 1 or 2, wherein the aryl phosphonate (B2) contains repeating units as defined in formula (III): Here, R1 is an alkyl radical having 1 to 4 carbon atoms, and BAr is, in each case, independently an aromatic radical, an aromatic radical having at least 2 rings, or biphenylene or 4,4'-(propane-2,2-diyl)diphenylene. Claim 6 A polyamide molding compound for use in the manufacture of parts according to claim 1 or 2. Claim 7 A method for insulating a current-carrying component, characterized by forming a component from a polyamide molding compound according to claim 1 or 2 by an extrusion process or a blow extrusion process, an injection-molding process or an insert molding process. Claim 8 A hybrid component comprising a coated metal body, wherein the coating comprises a polyamide molding formulation comprising: (A) a polyamide matrix comprising one or more polyamides having at least 8 carbon atoms per amide unit; (B) a flame-retardant composition comprising: (B1) at least one metal-free aryl phosphate; (B2) at least one aryl phosphonate; (B3) a carbohydrate polyol; (B4) melamine cyanurate; (B5) optionally, a phosphorus-free flame retardant, wherein the metal-free aryl phosphate (B1) is at least one unit of formula (I): and containing at least two units of formula (II): Herein, the units of formula (I) or (II) exist alternately, wherein the number of units according to formula (II) is always one greater than the number of units according to formula (I), wherein Ar is ortho-, meta-, para-phenylene, naphthylene or biphenylene, wherein Ph is a phenyl radical having any desired substitution by a C1 to C4 alkyl radical, wherein the phosphorus content in the total flame-retardant composition is 0.5 wt% to 1.5 wt% based on the polyamide molding formulation, and the mass loss is less than 1.1 wt%. Claim 9 In paragraph 8, a hybrid component for use in transmitting electric current.
Citation Information
Patent Citations
Composite flame retardant for non-halogen-based resin
JP2000351906A
Flame-retardant resin composition
JP2005162912A
Plastic fastener composed of polyamide resin composition
JP2017082203A
Flame-retardant polyamide molding composition