Titanium oxide composition, dispersion, member having a titanium oxide composition on a surface layer
A titanium oxide composition with sepiolite and high silica zeolite improves decomposition and stability, addressing issues in existing deodorization technologies by enhancing adsorption and preventing re-release of odor-causing substances.
Patent Information
- Application Number
- KR1020237001706
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-19
- Filing Date
- 2021-06-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-06-04
AI Technical Summary
Existing deodorization technologies face challenges with low adsorption capacity, slow deodorization rates, re-release of odor-causing substances due to moisture adsorption, and poor particle dispersion stability, particularly in photocatalyst-based systems.
A titanium oxide composition comprising a mixture of titanium oxide particles, sepiolite or atapulgite, and high silica zeolite or hydrophobic silica, in specific mass ratios, enhances decomposition power and suppresses re-release of odor-causing substances while maintaining excellent particle dispersion stability.
The composition exhibits improved decomposition of odor-causing substances and maintains stability, effectively reducing harmful volatile organic compounds and unpleasant odors in various environments.
Smart Images

Figure 112023005419389-PCT00001 
Figure 112023005419389-PCT00002 
Figure 112023005419389-PCT00003
Abstract
Description
Technology Field
[0001] The present invention relates to a titanium oxide composition for adsorbing and decomposing odor-causing substances, a dispersion liquid comprising said composition, and a member having a titanium oxide composition on a surface layer. Background Technology
[0002] In recent years, due to the heightened health awareness of consumers, "safety and security" are required in addition to the comfort of living spaces. Consequently, materials with deodorizing effects are in demand to suppress harmful volatile organic compounds (VOCs) emitted from household products and buildings, as well as unpleasant odors closely related to daily life, such as sweat odor, body odor, cigarette smoke, and food waste odor.
[0003] Deodorization methods using deodorizers include chemical and physical deodorization, which are classified and used according to their purpose. Chemical deodorization renders odor-causing substances odorless by chemically reacting them with deodorizing components, enabling highly selective deodorization against specific odor-causing substances. Physical deodorization removes odor-causing substances from the air through physical adsorption, making it relatively easy to adsorb multiple odor-causing substances simultaneously using a single adsorbent. Activated carbon, zeolite, silica gel, alumina, titania, and cyclodextrin are commonly used as adsorbents. However, deodorization using adsorbents requires replacement because the adsorption capacity is lost once an adsorption equilibrium is reached with the odor-causing substances.
[0004] The odor removal method using photocatalysts relies on a mechanism based on the decomposition of odor-causing substances; consequently, the catalyst itself does not change, maintaining a fresh surface at all times, and thus eliminating the need for catalyst replenishment. Due to these advantages, research on decomposing odor-causing substances using photocatalysts has been actively conducted in recent years. However, since photocatalysts generally have low adsorption capacity, the deodorization rate is slow, and they cannot efficiently decompose odor-causing substances when their concentration is low. Therefore, there is a method to supplement the adsorption capacity of the photocatalyst by combining it with an adsorbent.
[0005] In the inventions described in Patent Document 1 or Patent Document 2, sepiolite or silica is used as an adsorbent. However, it is known that adsorbents with hydrophilic surfaces, such as sepiolite or silica, have a high affinity for water, and the adsorbent absorbs moisture from the air, thereby releasing the odor-causing substances that were once adsorbed.
[0006] In the inventions described in Patent Document 3 or Patent Document 4, hydrophobic high silica zeolite is used as an adsorbent to prevent the re-release of odor-causing substances. However, since the surface of the adsorbent is hydrophobic, the adsorption capacity of gases having hydrophilic groups is low. In addition, high silica zeolite generally has low dispersibility in water, and since the dispersion stability of particles in an aqueous dispersion is low, it is difficult to form a uniform composition, and the strength of the composition may be reduced.
[0007] In the invention described in Patent Document 5, activated carbon with excellent adsorption capacity for numerous odor-causing substances is used, but since the activated carbon adsorbent absorbs light necessary for the exercise of photocatalytic function and inhibits the decomposition of odor-causing substances by the photocatalyst, combination with the photocatalyst is not suitable. Prior art literature
[0008] Japanese Patent Publication No. 2001-259003 Japanese Patent Publication No. 2002-136811 Japanese Patent Publication No. 2008-272651 Japanese Patent Publication No. 2018-158316 Japanese Patent Publication No. 2003-225572 The problem to be solved
[0009] The present invention aims to provide a titanium oxide composition having high decomposition power against odor-causing substances, low re-release of odor-causing substances due to moisture adsorption, and excellent particle dispersion stability, and a member having the titanium oxide composition on its surface. means of solving the problem
[0010] The inventors, having conducted diligent research to achieve the above objective, discovered that a mixture containing titanium oxide particles, component A (sepiolite, etc.), and component B (high silica zeolite, etc.) in a predetermined ratio exhibits high decomposition ability against odor-causing substances, suppresses the re-release of odor-causing substances due to the adsorption of moisture, and furthermore, the dispersion liquid has excellent particle dispersion stability, thereby completing the present invention.
[0011] [1]
[0012] titanium oxide particles and,
[0013] At least one component A selected from the group consisting of sepiolite and atapulgite, and
[0014] It is composed of at least one component B selected from the group consisting of high silica zeolite and hydrophobic silica, and
[0015] The mass ratio of component A to titanium oxide particles is 0.75 to 3.25, and also
[0016] Titanium oxide composition in which the mass ratio of component B to component A is 0.25 to 3.0.
[0017] [2]
[0018] Titanium oxide composition described in [1], wherein component A is sepiolite and component B is high silica zeolite.
[0019] [3]
[0020] Titanium oxide composition described in [1] or [2], wherein the average particle size of the titanium oxide particles is 5 to 30 nm.
[0021] [4]
[0022] In addition, a titanium oxide composition described in any one of claims [1] to [3] comprising an aqueous dispersion medium.
[0023] [5]
[0024] A member having a titanium oxide composition on its surface as described in any one of [1] to [3]. Effects of the invention
[0025] The composition of the present invention comprises titanium oxide particles and three types of particles, including component A (sepiolite, etc.) and component B (high silica zeolite, etc.), in a predetermined ratio, and exhibits higher decomposition ability than before for odor-causing substances and suppresses the re-release of odor-causing substances due to the adsorption of moisture.
[0026] In addition, the dispersion of the present invention is composed of titanium oxide particles and three types of particles, including component A (sepiolite, etc.) and component B (high silica zeolite, etc.), in a predetermined ratio, and has excellent dispersion stability of the particles, which provides excellent workability during coating and also suppresses a decrease in the strength of the composition.
[0027] Accordingly, by means of a member having a titanium oxide composition of the present invention on its surface, effects such as suppression of harmful volatile organic compounds (VOCs) emitted from household products or buildings, or unpleasant odors closely related to daily life such as sweat odor, body odor, cigarette odor, and food waste odor can be obtained. Specific details for implementing the invention
[0028] The present invention will be described in detail below.
[0029] Titanium oxide particles
[0030] As for the crystalline phases of titanium oxide particles, three types are generally known: rutile, anatase, and brookite, but it is preferable to use mainly anatase or rutile types. In addition, the term "mainly" as used here refers to at least 50 mass% of the total titanium oxide particle crystals, preferably at least 70 mass%, more preferably at least 90 mass%, and may be 100 mass%.
[0031] As for titanium oxide particles, in order to increase the performance of decomposing the odor-causing substances, titanium oxide particles supported with metal compounds such as platinum, gold, silver, palladium, iron, copper, zinc, and nickel, or titanium oxide particles doped with elements such as tin, nitrogen, sulfur, carbon, and transition metals may be used, and titanium oxide for photocatalysis may also be used.
[0032] Using titanium oxide for photocatalysis is more desirable because it yields stronger decomposition performance of odor-causing substances when irradiated with light.
[0033] Titanium oxide for photocatalysis is a general photocatalytic titanium oxide, and furthermore, it is preferably a visible light-responsive photocatalytic titanium oxide designed to respond to visible light of 400 to 800 nm.
[0034] Here, the odor-causing substances in this specification include, for example, odor components such as ammonia, acetic acid, hydrogen sulfide, methyl mercaptan, trimethylamine, formaldehyde, acetaldehyde, toluene, ethyl acetate, ethylene, benzene, acetone, pyridine, isovaleric acid, nonenal, indole, etc.
[0035] Titanium oxide particles, 50% cumulative distribution diameter D on a volume basis measured by dynamic light scattering using laser light 50(Hereinafter referred to as "average particle size") is preferably 5 to 30 nm, and more preferably 5 to 20 nm. This is because if the average particle size is less than 5 nm, the deodorizing performance may be insufficient, and if it exceeds 30 nm, the dispersion may become opaque when dispersed in an aqueous dispersion medium. In addition, as a device for measuring the average particle size, for example, the ELSZ-2000ZS (manufactured by Otsuka Denshi Co., Ltd.), Nanotrack UPA-EX150 (manufactured by Nikkiso Co., Ltd.), LA-910 (manufactured by Horiba Seisakusho Co., Ltd.) may be used.
[0036] Ingredient A
[0037] Component A is at least one selected from the group consisting of sepiolite and atapulgite, and may be used alone or in combination with multiple types.
[0038] Sepiolite is a clayey mineral containing hydrated magnesium silicate and having numerous active hydroxyl groups on its surface. Unlike two-dimensional crystal structures such as talc, sepiolite adopts a 2:1 ribbon structure, which is a three-dimensional chain structure. In the present invention, in addition to sepiolite, attapulgite (magnesium-aluminum silicate (Mg,Al)2Si4O), a holmite-based clay mineral having a structure similar to sepiolite, is used. 10 You may use a chain structure salt of (OH)·6H2O (CAS registration number: 12174-11-7), and preferably use sepiolite.
[0039] In terms of the adsorption and decomposition rate of odor-causing substances, it is desirable that the specific surface area of component A be 100 m² / g or more and 1000 m² / g or less, more preferably 120 m² / g or more and 500 m² / g or less. Furthermore, it is not limited in shape at all, and lumps and granules other than fibrous can all be used. In addition, the specific surface area is a value measured by the gas adsorption method.
[0040] Ingredient B
[0041] Component B is at least one selected from the group consisting of high silica zeolite and hydrophobic silica, and may be used alone or in combination with multiple types.
[0042] High silica zeolite is composed of crystalline hydrated aluminum silicate with a higher proportion of silica than alumina, and the internal cavities of the crystal are hydrophobic. Generally, zeolites with a SiO2 / Al2O3 ratio of 10 or more by weight are referred to as high silica zeolites. The general formula for high silica zeolite is A 2 / n O·Al2O 3z It is represented as ·xSiO2·yH2O (A=metal cations such as Na, Ca, K, etc., n=valence)), and when the SiO2 / Al2O3 ratio of the zeolite framework is low, hydrophilicity is strong, and when the SiO2 / Al2O3 ratio is high, hydrophobicity is strong. Since the boundary is generally said to be about 30, the SiO2 / Al2O3 ratio of the high silica zeolite used as component B is preferably 30 or higher and 80 or lower. In addition, the SiO2 / Al2O3 ratio can be calculated from the quantitative analysis of elements by inductively coupled plasma emission spectroscopy (ICP-AES).
[0043] As component B, a material in which exchangeable hydrogen ions present in high silica zeolite are exchanged with metal ions such as copper ions may be used. In the present invention, hydrophobic silica, such as which has a hydrophobic adsorbent surface similar to high silica zeolite, may be used as component B, and preferably, high silica zeolite is used.
[0044] Hydrophobic silica is a silicon oxide compound that has undergone hydrophobic treatment using a trimethylsilylating agent. The hydrophobicity of the hydrophobic silica used as component B is preferably 20 or higher, and a higher degree of hydrophobicity is preferable, with no specific upper limit. Furthermore, the degree of hydrophobicity in this specification refers to a concentration expressed in methanol volume% at which the treated powder begins to swell in a mixed solution of water and methanol, and refers to the value measured under the following conditions.
[0045] Method for Measuring Degree of Hydrophobicity
[0046] 50 mL of pure water is placed in a 200 mL beaker, 0.2 g of sample is added, and the mixture is stirred with a magnetic stirrer. The tip of a burette containing methanol is placed in the liquid, and methanol is added dropwise under stirring. When the amount of methanol required to be added until the sample is completely dispersed in water is denoted as Y mL, the following formula is obtained.
[0047] Primeness M={Y / (50+Y)}×100
[0048] In addition, the average particle size of component B is preferably 50 μm or less, more preferably 20 μm or less, and even more preferably 5 μm or less. This is because if the average particle size exceeds 50 μm, the dispersion stability of the particles in the dispersion is reduced, and there is concern that the strength of the composition may decrease. In addition, the average particle size is measured by dynamic light scattering using laser light.
[0049] Titanium Oxide Composition
[0050] The titanium oxide composition of the present invention comprises titanium oxide particles and components A and B, wherein the mass ratio of component A to titanium oxide particles is 0.75 to 3.25 and the mass ratio of component B to component A is 0.25 to 3.0.
[0051] If the mass ratio of component A to titanium oxide particles is less than 0.75, the adsorption effect on odor-causing substances is not sufficiently obtained, resulting in a decrease in the decomposition rate of odor-causing substances; if it is greater than 3.25, it hinders the propagation of light necessary for the exercise of photocatalytic activity of titanium oxide, which leads to a decrease in the decomposition rate of odor-causing substances and makes it impossible to ignore the re-release of odor-causing substances due to the adsorption of moisture, which is undesirable. Furthermore, if the mass ratio of component B to component A is less than 0.25, the adsorption effect on odor-causing substances is not sufficiently obtained, resulting in a decrease in the decomposition rate of odor-causing substances; and if it is greater than 3.0, it hinders the propagation of light necessary for the exercise of photocatalytic activity of titanium oxide, which leads to a decrease in the decomposition rate of odor-causing substances, which is undesirable. From the perspective of improving the adsorption effect on odor-causing substances and the decomposition rate of odor-causing substances, the mass ratio of component B to component A is more preferably 1.25 to 2.5.
[0052] Titanium Oxide Dispersion
[0053] As one embodiment of the titanium oxide composition of the present invention, a titanium oxide composition (titanium oxide dispersion) containing an aqueous dispersion medium in addition to the titanium oxide particles, component A, and component B may also be provided. Since the titanium oxide dispersion of the present invention has excellent particle dispersion stability, a uniform surface layer of titanium oxide can be formed when applied to the member described below. Therefore, it is preferable to use it as a titanium oxide dispersion.
[0054] As an aqueous dispersion medium for a titanium oxide dispersion, an aqueous solvent is typically used, and while it is preferable to use water, a water-soluble organic solvent that is miscible with water, or a mixed solvent in which water and a water-soluble organic solvent are mixed in any ratio, may also be used. As for water, deionized water, distilled water, pure water, etc., are preferred. In addition, as for water-soluble organic solvents, alcohols such as methanol, ethanol, and isopropanol; glycols such as ethylene glycol and propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and propylene glycol-n-propyl ether are preferred. One or more of these types of aqueous dispersion media may be used in combination. When a mixed solvent is used, it is preferable that the proportion of the water-soluble organic solvent in the mixed solvent be greater than 0 mass% and 50 mass% or less, more preferably 20 mass% or less, and even more preferably 10 mass% or less.
[0055] The titanium oxide dispersion of the present invention comprises titanium oxide particles and components A and B, wherein the mass ratio of component A to titanium oxide particles is 0.75 to 3.25 and the mass ratio of component B to component A is 0.25 to 3.0.
[0056] If the mass ratio of component A to titanium oxide particles is less than 0.75, the dispersion stability of the dispersion is poor, raising concerns about a decrease in the strength of the composition; if it is greater than 3.25, the decomposition rate of the odor-causing substance in the composition is reduced, which is undesirable. Additionally, if the mass ratio of component B to component A is less than 0.25, the decomposition rate of the odor-causing substance in the composition is reduced; if it is greater than 3.0, the dispersion stability of particles within the dispersion is poor, raising concerns about a decrease in the strength of the composition, which is undesirable. From the perspective of the adsorption effect on the odor-causing substance, the improvement of the decomposition rate of the odor-causing substance, and the dispersion stability of particles in the dispersion, the mass ratio of component B to component A is more preferably 1.25 to 2.5.
[0057] The concentration of titanium oxide particles in the titanium oxide dispersion is preferably 0.01 to 30 mass%, and particularly 0.5 to 20 mass%, from the perspective of ease of manufacturing the titanium oxide composition (surface layer) of the required thickness described later.
[0058] The method for preparing the titanium oxide composition of the present invention involves mixing titanium oxide particles, component A, and component B in the ratio described above, and is not particularly limited.
[0059] In addition, for a titanium oxide composition containing an aqueous dispersion medium, the titanium oxide particle dispersion, component A, and component B can be mixed in the ratio described above. Although not particularly limited, a method for preparing a titanium oxide composition containing an aqueous dispersion medium is preferably to add component A and component B to a titanium oxide particle dispersion obtained by crystal growth of an aqueous solution of a titanium oxide precursor, such as titanium peroxide, through hydrothermal treatment.
[0060]
[0061] The above titanium oxide dispersion can be used for the purpose of forming a composition having the ability to decompose odor-causing substances on the surface of a component. The component may have various shapes according to its respective purpose and use.
[0062] Herein, the term "material" in this specification includes, for example, indoor building materials such as wall materials, wallpaper, ceiling materials, floor materials, tiles, bricks, wooden boards, resin boards, metal boards, tatami mats, bathroom materials; interior materials for vehicles such as automobiles or trains, such as wall materials, ceiling materials, floor materials, seats, handrails, and leather handles; furniture or household products such as curtains, blinds, rugs, partitions, glass, mirrors, films, desks, chairs, beds, and storage shelves; and home appliances such as deodorizing filters, air purifiers, air conditioners, refrigerators, washing machines, personal computers, printers, tablets, touch panels, and telephones, and are particularly suitable for deodorizing filters.
[0063] Here, as the material of the component, examples include organic materials and inorganic materials.
[0064] Organic materials may include synthetic resin materials such as vinyl chloride resin (PVC), polyethylene (PE), polypropylene (PP), polycarbonate (PC), acrylic resin, polyacetal, fluoropolymer, silicone resin, ethylene-vinyl acetate copolymer (EVA), acrylonitrile-butadiene rubber (NBR), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyvinyl butyral (PVB), ethylene-vinyl alcohol copolymer (EVOH), polyimide resin, polyphenylene sulfide (PPS), polyetherimide (PEI), polyetheretherimide (PEEI), polyetheretherketone (PEEK), polyamide resin (PA), melamine resin, phenolic resin, acrylonitrile-butadiene-styrene (ABS) resin, etc.; natural materials such as natural rubber; and semi-synthetic materials of the above synthetic resin materials and natural materials. These may be processed into the necessary shapes and configurations, such as films, sheets, fiber materials, fiber products, other molded articles, laminates, etc.
[0065] Inorganic materials include, for example, non-metallic inorganic materials and metallic inorganic materials.
[0066] Examples of non-metallic inorganic materials include glass, ceramics, stone, and gypsum. These may be processed into various forms such as tiles, glass, mirrors, walls, filters, and decorative materials.
[0067] Examples of metallic inorganic materials include cast iron, steel, iron, iron alloy, stainless steel, aluminum, aluminum alloy, aluminum nitride, zirconia, silicon carbide, silicon nitride, clay minerals, alumina, titania, silica, nickel, nickel alloy, zinc die casting, etc. These may be plated with the above-mentioned metallic inorganic material, may have the above-mentioned organic material applied, or may be a plating applied to the surface of the above-mentioned organic material or non-metallic inorganic material.
[0068] As a method for forming a titanium oxide composition on the surface of a member, a titanium oxide dispersion may be applied to the surface of the member, for example, by a method such as spray coating, flow coating, dip coating, spin coating, Meyer bar coating, reverse roll coating, gravure coating, knife coating, kiss coating, die coating, etc., and then dried or film transferred.
[0069] The drying temperature after coating can be determined in various ways depending on the member to be coated, but preferably it is 0 to 1000°C, more preferably 10 to 800°C, and even more preferably 20 to 700°C. This is because if the temperature is below 0°C, there is a risk that the dispersion and / or coating solution will freeze and become unusable. Since the crystal water of sepiolite or zeolite is completely dehydrated at 600°C or higher, sintering at a temperature higher than 700°C is not only uneconomical but also tends to reduce the strength of the composition.
[0070] The drying time after application can be appropriately selected by the application method and drying temperature, but is preferably 10 minutes to 72 hours, more preferably 20 minutes to 48 hours. This is because if it is less than 10 minutes, the adhesion of the composition to the surface of the member may be insufficient, and if it exceeds 3 days, the economic efficiency in manufacturing is poor and undesirable.
[0071] The thickness of the composition (surface layer) on the surface of the above-mentioned member can be appropriately selected, but preferably 100 nm to 50 µm, more preferably 200 nm to 50 µm, and even more preferably 500 nm to 30 µm. This is because if the layer thickness is less than 100 nm, the decomposition of the odor-causing substance may become insufficient, and if it exceeds 50 µm, the surface layer may easily peel off from the surface of the member.
[0072] Examples
[0073] The present invention will be specifically described below by presenting examples and comparative examples, but the present invention is not limited to the following examples. Performance tests in the present invention were performed as follows.
[0074] (1) 50% cumulative distribution diameter of titanium oxide dispersion (D 50 )
[0075] D of titanium oxide dispersion 50 It was calculated as the 50% cumulative distribution diameter based on volume measured by dynamic light scattering using laser light, using a particle size distribution measuring device (ELSZ-2000ZS (manufactured by Otsuka Denshi Co., Ltd.)).
[0076] (2) Re-emission test of acetaldehyde gas
[0077] An evaluation sample was placed in a 1L gas bag, and 300mL of acetaldehyde gas with a concentration of 100 ppm was injected into the gas bag. After standing for 45 minutes, the acetaldehyde gas concentration was measured upon reaching adsorption equilibrium. The sample was removed after adsorption equilibrium, placed in a new 1L gas bag, and 300mL of air with a relative humidity of 100% was injected into the gas bag. After standing for 15 minutes, the concentration of acetaldehyde emitted from the evaluation sample was measured. The ratio of re-emitted acetaldehyde was calculated using Equation 1. At this time, a Tedla bag (As One Co., Ltd.) equipped with a single-port stopcock was used for the 1L gas bag, and the acetaldehyde gas concentration was measured using a 92L acetaldehyde detector tube (Gas Tech Co., Ltd.), and evaluated according to the following criteria.
[0078] · Good (indicated by ○)···Ratio of re-released acetaldehyde less than 5%
[0079] · Slightly poor (indicated by △)···Ratio of re-released acetaldehyde is 5 to 10%
[0080] · Defective (marked with ×)···Ratio of re-released acetaldehyde exceeds 10%
[0081] Equation 1: Percentage of re-released acetaldehyde [%] = Re-released acetaldehyde concentration / (Initial concentration - Acetaldehyde concentration at adsorption equilibrium) × 100
[0082] (3) Acetaldehyde gas decomposition performance evaluation test
[0083] An evaluation sample that had reached adsorption equilibrium was placed in a 1L gas bag, 700mL of acetaldehyde gas at a concentration of 20 ppm was injected into the gas bag, and the initial acetaldehyde gas concentration was measured. After irradiating with ultraviolet light of 2.0 (mW / cm²) for 20 minutes, the acetaldehyde gas concentration was measured. A UVLED lamp (product model number "HLDL-600×480U6-PSC" CCS Co., Ltd.) was used as the test light source. The decomposition rate of the malodorous gas was calculated by Equation 2 and evaluated according to the following criteria.
[0084] · Good (marked with ○)···Decomposition rate exceeding 90%
[0085] · Slightly defective (indicated by △)··· Decomposition rate 70 to 90%
[0086] · Defective (marked with ×)··· Decomposition rate less than 70%
[0087] Equation 2: Decomposition rate [%] = (Initial concentration - Residual concentration) / Initial concentration × 100
[0088] (4) Evaluation of dispersion stability of titanium oxide dispersion
[0089] The dispersion stability of the prepared titanium oxide dispersion was measured using a multi-sample dispersion stability evaluation particle distribution measuring device (LUMiSiZER 610, manufactured by Nippon Lufto Co., Ltd.). 0.4 mL of the prepared titanium oxide dispersion was placed into a cell (PC 2 mm cell, manufactured by Nippon Lufto Co., Ltd.), and the cycle setting parameters were set to 2500 rpm, 300 profiles, a measurement interval of 10 seconds, 25°C, and a light count of 1. The transmittance was measured 60 seconds after the start of centrifugation at a measurement position of 115 mm and evaluated according to the following criteria.
[0090] · Good (indicated by ○)··· Transmittance of less than 0 to 50% at measurement position 115 mm 60 seconds after the start of centrifugation
[0091] · Defective (marked with ×)··· Transmittance of 50% or more at measurement position 115 mm 60 seconds after the start of centrifugation
[0092] (5) Overall evaluation
[0093] Based on the results of the acetaldehyde gas re-emission test, the acetaldehyde gas decomposition performance evaluation test, and the titanium oxide dispersion stability evaluation test, a comprehensive evaluation was conducted according to the following criteria.
[0094] · Very Good (marked as A)···Total score of each evaluation is 6 points
[0095] ·Good (marked as B)···Total score of each evaluation is 5 points
[0096] · Slightly Poor (marked as C)···Total score of each evaluation is 3 to 4 points
[0097] ·Poor (marked as D)···Total score of each evaluation is 0 to 2 points
[0098] Calculated as ○···2 points, △···1 point, ×···0 points
[0099] Preparation of Titanium Oxide Particle Dispersion
[0100] [Preparation Example 1]
[0101] A 36 mass% aqueous solution of titanium chloride (IV) was diluted 10 times with pure water, and then 10 mass% ammonia water was slowly added to neutralize and hydrolyze the solution, thereby obtaining a precipitate of titanium hydroxide. The pH of the solution at this time was 8. The obtained precipitate of titanium hydroxide was deionized by repeating the addition of pure water and decanting. After deionization, 35 mass% hydrogen peroxide water was added to the titanium hydroxide precipitate so that the hydrogen peroxide / titanium hydroxide (molar ratio) was 10, and then the mixture was reacted sufficiently at 60°C for 2 hours to obtain a peroxotitanic acid solution (1a) (solid content concentration 1 mass%).
[0102] 400 mL of peroxo-titanium solution (1a) was added to an autoclave with a volume of 500 mL, and the solution was hydrothermally treated for 90 minutes under conditions of 150°C, and then pure water was added to adjust the concentration, thereby obtaining a dispersion of titanium oxide particles (1A) (solid content concentration 2.0 mass%).
[0103] D of titanium oxide particles in the dispersion 50 It was 18nm.
[0104] [Example 1]
[0105] Preparation of Titanium Oxide Dispersion
[0106] 20 mL of titanium oxide particle dispersion (1A) and sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD: Si 12 Mg8O 30 0.8 g of (OH)4(OH2)4·8H2O (CAS63800-37-3)) and 1.0 g of high silica zeolite (Union Showa Corporation USKY-700) were mixed and dispersed to obtain a titanium oxide dispersion. The composition of the dispersion is shown in Table 1, and the average particle size and specific surface area of the materials used are shown in Table 2.
[0107] <Production of Evaluation Samples>
[0108] A titanium oxide dispersion was applied to a plasma-surface-treated PET film (Toray Corporation Lumirror T60) using a bar coater (Daiichi Ricca Corp. No. 7) to a thickness of 16.0 μm. The film was dried in an oven set to 80°C for 30 minutes, and the coated area was cut into a square with sides of 10 cm to obtain an evaluation sample having a titanium oxide composition formed on the film.
[0109] Acetaldehyde gas re-emission test (Table 3) and acetaldehyde gas decomposition performance evaluation test (Table 4) were performed on the obtained evaluation samples, and the results are shown in each table.
[0110] In addition, a dispersion stability evaluation test (Table 5) was performed on the titanium oxide dispersion, and the results are shown in the table. In addition, the overall evaluation is shown in Table 6.
[0111] [Example 2]
[0112] The titanium oxide dispersion was evaluated in the same manner as in Example 1, except that 0.4 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.5 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain the titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-release test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0113] [Example 3]
[0114] Except for the fact that 1.2 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 1.5 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion, the results were evaluated in the same manner as in Example 1 (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-release test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0115] [Example 4]
[0116] The evaluation was conducted in the same manner as in Example 1, except that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.4 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0117] [Example 5]
[0118] Except for the fact that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 2.0 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion, the results were evaluated in the same manner as in Example 1 (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-release test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0119] [Example 6]
[0120] The results were evaluated in the same manner as in Example 1, except that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANSIL) and 2.0 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0121] [Example 7]
[0122] The results were evaluated in the same manner as in Example 1, except that 0.8 g of atapulgite (BASF Attagel 40) and 2.0 g of high silica zeolite (Union Showa Corp. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0123] [Example 8]
[0124] The results were evaluated in the same manner as in Example 1, except that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 2.0 g of hydrophobic silica (Asahi Kasei Wacker Silicon Co., Ltd. HDK (registered trademark) H30, M value 52) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-release test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0125] [Example 9]
[0126] Except for the fact that 1.2 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 3.0 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion, the results were evaluated in the same manner as in Example 1 (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0127] [Example 10]
[0128] Except for the fact that 0.4 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.2 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion, the evaluation was conducted in the same manner as in Example 1 (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0129] [Comparative Example 1]
[0130] The titanium oxide dispersion was evaluated in the same manner as in Example 1, except that 0.2 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.5 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain the titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0131] [Comparative Example 2]
[0132] Except for the fact that 1.4 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.7 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion, the results were evaluated in the same manner as in Example 1 (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0133] [Comparative Example 3]
[0134] The results were evaluated in the same manner as in Example 1, except that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 0.1 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0135] [Comparative Example 4]
[0136] The results were evaluated in the same manner as in Example 1, except that 0.8 g of sepiolite (Kusumoto Kasei Co., Ltd. PANGEL AD) and 2.8 g of high silica zeolite (Union Showa Co., Ltd. USKY-700) were mixed and dispersed in 20 mL of titanium oxide particle dispersion (1A) to obtain a titanium oxide dispersion (Table 1). For the obtained titanium oxide dispersion or evaluation sample, an acetaldehyde gas re-emission test (Table 3), an acetaldehyde gas decomposition performance evaluation test (Table 4), and a dispersion stability test (Table 5) were performed, and the results are shown in each table. In addition, the overall evaluation is shown in Table 6.
[0137]
[0138]
[0139]
[0140]
[0141]
[0142]
[0143] As can be seen from Examples 1 to 10, a titanium oxide composition in which the mass ratio of component A to titanium oxide particles is 0.75 to 3.25 and the mass ratio of component B to component A is 0.25 to 3.0 has excellent decomposition properties for odor-causing substances, is difficult to re-release odor-causing substances that have been adsorbed once, and also has excellent dispersion stability of the particles in the dispersion liquid.
[0144] As can be seen from Example 6, even when using sepiolites with different specific surface areas, the decomposition of odor-causing substances is excellent, it is difficult to re-release odor-causing substances that have been adsorbed once, and the dispersion liquid has excellent particle dispersion stability.
[0145] As can be seen from Example 7, even when using atapulgite, the decomposition of odor-causing substances is excellent, it is difficult to re-release odor-causing substances that have been adsorbed once, and the dispersion has excellent particle dispersion stability.
[0146] As can be seen from Example 8, even when hydrophobic silica is used, the decomposition of odor-causing substances is excellent, it is difficult to re-release odor-causing substances that have been adsorbed once, and the dispersion has excellent particle dispersion stability.
[0147] As can be seen from Comparative Example 1, when the amount of component A in the composition is small, the effect obtained from the adsorbent is small, so the decomposition of the odor-causing substance is low, and the particle dispersion stability of the dispersion is also poor.
[0148] As can be seen from Comparative Example 2, when the amount of component A in the composition is in excess, the acetaldehyde adsorbed to component A is likely to be released again.
[0149] As can be seen from Comparative Example 3, when the amount of component B in the composition is small, the adsorption capacity for acetaldehyde is weak, so the decomposition of acetaldehyde is low, and also the rate of re-releasing acetaldehyde that has been adsorbed once is large.
[0150] As can be seen from Comparative Example 4, when the amount of component B in the composition is excessive, the particle dispersion stability of the dispersion is reduced.
[0151] From the above results, the composition of the present invention is capable of efficiently decomposing odor-causing substances, suppressing the re-release of odor-causing substances, and the dispersion liquid has excellent particle dispersion stability.
Claims
Claim 1 A titanium oxide composition comprising titanium oxide particles, at least one component A selected from the group consisting of sepiolite and attapulgite, at least one component B selected from the group consisting of high silica zeolite and hydrophobic silica, and an aqueous dispersion medium, wherein the mass ratio of component A to titanium oxide particles is 0.75 to 3.25, the mass ratio of component B to component A is 0.25 to 3.0, and the average particle size of the titanium oxide particles is 5 to 30 nm. Claim 2 Titanium oxide composition according to claim 1, wherein component A is sepiolite and component B is high silica zeolite. Claim 3 A titanium oxide composition according to claim 2, wherein the composition of the high-silica zeolite of component B has a SiO2 / Al2O3 ratio of 30 or more and 80 or less, calculated from the quantitative analysis of elements by inductively coupled plasma emission spectroscopy (ICP-AES). Claim 4 A titanium oxide composition according to any one of claims 1 to 3, wherein the concentration of titanium oxide is 0.01 to 30 mass%. Claim 5 A member having a surface layer formed by a titanium oxide composition described in any one of claims 1 to 3.
Citation Information
Patent Citations
Photocatalyst deodorizing filter
JP2000210534A
Photocatalyst deodorizing filter
JP2002136811A