conductive paste

A conductive paste with a specific ionic radius ratio between metal and ABO3-type oxide ceramic powder improves electrode coverage in multilayer ceramic capacitors, ensuring high capacitance despite thin electrodes.

KR103046284B1Active Publication Date: 2026-11-11MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020257023176
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-02-27
Filing Date
2024-02-02
Publication Date
2026-11-11
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

Existing conductive pastes for forming internal electrodes in multilayer ceramic capacitors face challenges in maintaining high coverage when the electrodes are thinned, which hinders capacitance improvement.

Method used

A conductive paste comprising a specific ratio of ionic radii between the metal constituting the conductive metal powder and the A-site in ABO3-type oxide ceramic powder, within the range of 0.97 to 1.02, is used to enhance electrode coverage.

Benefits of technology

The solution maintains high coverage of internal electrodes even when they are thinned, preventing a decrease in capacitance of the multilayer ceramic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025078063320-PCT00017_ABST
    Figure 112025078063320-PCT00017_ABST
Patent Text Reader

Abstract

A conductive paste for internal electrodes is provided that can maintain a relatively high coverage even when the internal electrodes of a multilayer ceramic capacitor are thinned. A conductive paste for forming internal electrodes (4, 5) of a multilayer ceramic capacitor (1) manufactured through a firing process comprises a conductive metal powder, a ceramic powder, an organic solvent, and an organic binder, wherein at least a portion of the ceramic powder is a powder composed of an ABO3-type oxide of a specific ionic radius, wherein the ratio of the ionic radius of an element at the 6th coordination of the A-site in ABO3 to the ionic radius at the 6th coordination of a metal element included in the conductive metal powder is 0.97 or more and 1.02 or less. Preferably, the ABO3-type oxide of the specific ionic radius has an ilmenite crystal structure, and the conductive metal powder comprises one selected from nickel, copper, silver, and a silver / palladium alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a conductive paste, and in particular, to a conductive paste for forming internal electrodes of a multilayer ceramic capacitor. Background Technology

[0002] A multilayer ceramic capacitor typically comprises a plurality of stacked dielectric layers made of ceramic, a plurality of internal electrodes each disposed along a plurality of interfaces between the dielectric layers, and a plurality of external electrodes provided on the outer surface of the laminate and electrically connected to the internal electrodes. The internal electrodes include a plurality of first internal electrodes and a plurality of second internal electrodes alternately disposed in the stacking direction of the laminate, and the external electrodes include a first external electrode electrically connected to the first internal electrode and a second external electrode electrically connected to the second internal electrode.

[0003] In order to achieve a compact size and high capacitance of a multilayer ceramic capacitor with such a structure, it is required to thin the dielectric layer and internal electrodes, and at the same time, increase the coverage (electrode continuity) of the internal electrodes. Generally, during the firing process in the manufacturing of multilayer ceramic capacitors, the sintering temperature of the conductive metal particles contained in the conductive paste film that are to become the internal electrodes is lower than the sintering temperature of the ceramic constituting the dielectric layer; therefore, the metal particles contained in the internal electrodes sinter first. This causes a decrease in the coverage of the internal electrodes. In particular, there is a problem in that coverage is prone to decrease in the case of internal electrodes that are thinned, such as with a thickness of less than 1.0 μm, and such a decrease in coverage is likely to hinder the increase in capacitance.

[0004] Therefore, in order to form thin internal electrodes with high coverage, it is necessary to increase the sintering temperature of the conductive metal particles contained in the conductive paste film intended to serve as the internal electrode during the firing process of manufacturing multilayer ceramic capacitors. By doing so, the sintering temperature of the metal particles contained in the conductive paste film intended as the internal electrode can be brought closer to the temperature at which the ceramic constituting the dielectric layer begins sintering, thereby bringing the shrinkage timing during sintering closer to that between the internal electrode and the dielectric layer. As a result, the coverage of the internal electrode is increased, and a higher capacitance can be realized.

[0005] It is known that, in order to increase the coverage of the internal electrode and realize a high capacity by the method described above, a ceramic material having a composition similar to that of the ceramic constituting the dielectric layer, i.e., a co-material, is added to the conductive paste for forming the internal electrode, for example, as described in paragraph 0004 of Patent Document 1 (Japanese Patent Publication No. JP 2016-31807). By adding the co-material, the sintering timing of the metal particles included in the conductive paste film to become the internal electrode can be shifted toward a higher temperature, and the temperature at which the metal particles included in the conductive paste film are sintered can be brought closer to the temperature at which the ceramic constituting the dielectric layer is sintered. Prior art literature

[0006] Japanese Patent Publication No. JP2016-31807 The problem to be solved

[0007] However, even if a filler is added to the conductive paste for forming internal electrodes, it cannot be denied that the sintering temperature of the metal particles contained in the conductive paste is lower than the sintering temperature of the ceramic constituting the dielectric layer, and further improvement is desired. In particular, regarding thin internal electrodes, such as those with a thickness of less than 1.0 μm, for example, there is a strong demand for an effective solution to the problem of reduced coverage that hinders the increase in capacity.

[0008] Accordingly, the present invention has been made in light of these problems and aims to provide a conductive paste for forming internal electrodes that can maintain a relatively high coverage even when the internal electrodes are thinned. means of solving the problem

[0009] The present invention may provide a conductive paste for forming internal electrodes of a multilayer ceramic capacitor, comprising a conductive metal powder, a ceramic powder, an organic solvent, and an organic binder.

[0010] The ceramic powder included in the conductive paste is intended to suppress coverage degradation; however, the inventors discovered a correlation between the metal constituting the conductive metal powder included in the conductive paste and the elements of the A-site in the ABO3-type oxide constituting the ceramic powder, and thus arrived at the present invention. More specifically, the inventors focused on the ionic radius of the metal constituting the conductive metal powder and the ionic radius of the elements of the A-site in the ABO3-type oxide constituting the ceramic powder, and found that if the ratio of these ionic radii is within a predetermined range, it contributes more to the improvement of the coverage of the internal electrode.

[0011] Meanwhile, the ratio of appropriate ionic radii that can contribute to improving the coverage of the internal electrode is not universal and varies depending on the type of metal constituting the conductive metal powder. However, the inventors of the present invention noted that although the ratio of appropriate ionic radii varies depending on the type of metal constituting the conductive metal powder, there are common aspects regarding the ratio of appropriate ionic radii even if the metal types differ.

[0012] Accordingly, the present invention is characterized in that at least a portion of the ceramic powder is composed of an ABO3-type oxide in which the element at the A site has a specific ionic radius, and the ratio of the ionic radius at the 6th coordination of the element at the A site in ABO3 to the ionic radius at the 6th coordination of the metal included in the conductive metal powder is 0.97 or higher and 1.02 or lower. Effects of the invention

[0013] When the internal electrodes of a multilayer ceramic capacitor are formed using the conductive paste according to the present invention, the coverage of the internal electrodes can be improved regardless of the type of metal constituting the conductive metal powder. Therefore, even if the internal electrodes are thinned, the coverage of the internal electrodes is maintained at a high level, and the capacitance of the multilayer ceramic capacitor can be prevented from being hindered. Brief explanation of the drawing

[0014] FIG. 1 is a cross-sectional view schematically showing a multilayer ceramic capacitor (1) to which a conductive paste according to the present invention is applied. Specific details for implementing the invention

[0015] With reference to FIG. 1, the structure of a multilayer ceramic capacitor (1) to which a conductive paste according to the present invention is applied is described.

[0016] A multilayer ceramic capacitor (1) comprises a laminate (2). The laminate (2) comprises a plurality of stacked dielectric layers (3) made of ceramic and a plurality of internal electrodes (4 and 5) arranged along the interface between the plurality of dielectric layers (3). The internal electrodes (4 and 5) are classified into a plurality of first internal electrodes (4) and a plurality of second internal electrodes (5) arranged alternately in the stacking direction of the laminate (2). A first external electrode (6) and a second external electrode (7) are provided on the outer surface of the laminate (2), more specifically on each end face facing each other. The first external electrode (6) is electrically connected to the first internal electrode (4), and the second external electrode (7) is electrically connected to the second internal electrode (5).

[0017] The dielectric layer (3) is, for example, made of a ceramic having ABO3 as the main component (A is at least one of Ba, Ca, and Sr, and B is at least one of Ti and Zr). In addition, the ceramic may have ABO3 as the main component and additionally include at least one of Mn, Mg, Si, Y, Dy, and Gd as a minor component.

[0018] The internal electrodes (4 and 5) preferably comprise one selected from, for example, nickel, copper, silver, and silver / palladium alloys as a conductive component. Additionally, as a characteristic composition, the internal electrodes (4 and 5) comprise an ABO3-type oxide with a specific ionic radius as a ceramic component, wherein the ratio of the ionic radius of the element at the 6th coordination of the A-site in ABO3 to the ionic radius at the 6th coordination of the metal element that serves as the conductive component is 0.97 or more and 1.02 or less. This ABO3-type oxide preferably has an ilmenite crystal structure.

[0019] As can be seen from the experimental examples described below, in a preferred embodiment, the dielectric layer (3) is made of a ceramic having at least one selected from BaTiO3, SrTiO3, and CaZrO3 as the main component. In this case, the internal electrodes (4 and 5) may additionally include, as necessary, at least one selected from BaTiO3, SrTiO3, and CaZrO3 included in the dielectric layer (3), in addition to the ABO3-type oxide of the specific ionic radius described above as the ceramic component.

[0020] The content of the ceramic component in the internal electrodes (4 and 5) is preferably selected to be 5 mass% or more and 15 mass% or less. Meanwhile, the content is {(mass of ceramic component) / (mass of ceramic component + mass of conductive metal or alloy containing it)} × 100 (hereinafter the same).

[0021] The external electrodes (6 and 7) are formed by applying a conductive paste, for example, in which Ag or Cu is the main component of the conductive component, to a cross-section of the laminate (2) and baking it. If necessary, on the thick film formed by baking, for example, Ni plating and Sn plating thereon may be performed.

[0022] A multilayer ceramic capacitor (1) is manufactured, for example, through the following process. First, a ceramic slurry containing raw powder of ceramic having the composition as described above is prepared. Next, a ceramic green sheet is formed by applying a suitable sheet molding method to the ceramic slurry. Next, a conductive paste, which is to become each of the internal electrodes (4 and 5), is applied by printing or the like onto a predetermined ceramic green sheet among a plurality of ceramic green sheets. Next, a plurality of ceramic green sheets are stacked and then compressed to obtain a raw laminate. Next, the raw laminate is fired. In this firing process, the ceramic green sheet becomes a dielectric layer (3). After that, external electrodes (6 and 7) are formed on the cross-section of the laminate (2).

[0023] The conductive paste that is to be used as the internal electrodes (4 and 5) in the manufacture of the above-described multilayer ceramic capacitor (1) is preferably manufactured as follows.

[0024] In the production of a conductive paste, a first process of preparing a ceramic powder slurry comprising ceramic powder, an organic solvent, and a dispersant, a second process of preparing a metal powder slurry comprising conductive metal powder, an organic solvent, and a dispersant, a third process of preparing an organic vehicle comprising an organic resin component and an organic solvent, and a fourth process of mixing the ceramic powder slurry, the metal powder slurry, and the organic vehicle are carried out.

[0025] More specifically, in the first process, a ceramic powder slurry is produced by mixing ceramic powder and a dispersant in an organic solvent.

[0026] The ceramic powder described above is used to consist of an ABO3-type oxide of the aforementioned specific ionic radius. Additionally, there are cases where it is used as a co-material consisting of at least one selected from BaTiO3, SrTiO3, and CaZrO3. When a powder consisting of at least one selected from BaTiO3, SrTiO3, and CaZrO3 is used, it is preferable that at least 10 volume% of the ceramic powder consists of an ABO3-type oxide of the aforementioned specific ionic radius, and the remainder of the ceramic powder consists of a powder having at least one selected from BaTiO3, SrTiO3, and CaZrO3 as the main component.

[0027] The ABO3-type oxide of a specific ionic radius is determined by the type of metal constituting the conductive metal powder included in the metal powder slurry produced in the second process to be described later. That is, the ABO3-type oxide of a specific ionic radius is obtained by determining the ionic radius at the 6th coordination of the metal included in the conductive metal powder, and the ABO3-type oxide is an A-site element in which the ratio of the ionic radius at the 6th coordination to this ionic radius is 0.97 or higher and 1.02 or lower. Meanwhile, the range of the ratio of ionic radii, which is 0.97 or higher and 1.02 or lower, is derived from the results of the experiment to be described later.

[0028] As described above, according to the ceramic powder composed of an ABO3-type oxide of a specific ionic radius, the reaction that may occur between the conductive metal powder included in the metal powder slurry produced in the second process during firing can be suppressed. The ceramic powder included in the conductive paste may have the above-mentioned ABO3 oxide as a main component and additionally include at least one of Mn, Mg, Si, Y, Dy, and Gd as a minor component. When such minor components are included, the grain growth of the ceramic particles is suppressed, and the sintering of the metal particles can be effectively suppressed.

[0029] For example, an anionic polymer dispersant can be used as the dispersant mixed into the ceramic powder in the first process, and for example, dihydroterpineol can be used as the organic solvent.

[0030] In the second process, a metal powder slurry is prepared by mixing a conductive metal powder and a dispersant in an organic solvent. As the conductive metal powder, a powder consisting of one selected from nickel, copper, silver, and silver / palladium alloys is used, for example. The dispersant and organic solvent used in the second process may be the same as those used in the first process.

[0031] In the third process, an organic vehicle is produced by mixing an organic resin component with an organic solvent. For example, ethylcellulose resin can be used as the organic resin component. The same organic solvent used in the third process can also be used as the one used in the first process.

[0032] In the fourth process, the ceramic powder slurry, metal powder slurry, and organic vehicle described above are mixed. This results in a conductive paste that is to become the internal electrodes (4 and 5). This conductive paste contains the ceramic powder slurry, and since the ceramic powder slurry contains ceramic powder composed of ABO3 oxide of a specific ionic radius as described above, the internal electrodes (4 and 5) included in the multilayer ceramic capacitor (1) manufactured through the firing process contain ABO3 oxide of a specific ionic radius.

[0033] The content of ceramic powder in the conductive paste is preferably selected to be 5 mass% or more and 15 mass% or less.

[0034] Next, experimental examples conducted to determine the scope of the present invention and to verify the effects of the present invention will be described.

[0035] [Experimental Example 1] Conductive metal powder: Nickel powder

[0036] In Experimental Example 1, nickel powder was prepared as a conductive metal powder included in a conductive paste for forming an internal electrode.

[0037] Meanwhile, NiTiO3, MgTiO3, and MnTiO3 were prepared as ABO3 oxides of specific ionic radii constituting the ceramic powder included in the conductive paste for forming internal electrodes, and CuTiO3, BaTiO3, CaZrO3, and SrTiO3 were prepared as other ABO3 oxides. Table 1 shows the "crystal structure," "coordination number," "A-site element," and "ionic radius" for these ABO3 oxides. Meanwhile, Ba, Ca, and Sr are 12-coordinated when in the original perovskite structure, but since Ba, Ca, and Sr are 6-coordinated when dissolved into the sites of the 6-coordinated elements (Ni, Mg, Mn) of the ilmenite structure, the "ionic radius" in Table 1 represents the value at 6-coordinated.

[0038]

[0039] Below, Experimental Examples 1-1, 1-2, and 1-3, which were conducted by changing the ceramic raw materials constituting the dielectric layer, will be described.

[0040] (Experimental Example 1-1) Main component of the ceramic constituting the dielectric layer: BaTiO3

[0041] 1-1-1. Fabrication of BaTiO3-based ceramic raw materials constituting the dielectric layer

[0042] As starting materials, powders of the main components BaCO3 and TiO2 were weighed and mixed in a ball mill for 72 hours, then heat-treated at a top temperature of 1000°C for 2 hours to obtain heat-treated powder. Meanwhile, powders of MnO, Dy2O3, MgO, SiO2, and BaCO3 were prepared as minor components, and with respect to the heat-treated powder, the minor component powders were weighed so that the composition ratio was 100BaTiO3+0.5Mn+1.0Dy+1.0Mg+1.0Si+2.0Ba. These minor component powders were added to the heat-treated powder and mixed in a ball mill for 24 hours, then dried to obtain BaTiO3-based ceramic raw material powder.

[0043] 1-1-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0044] The powder of "ABO3 oxide" shown in Table 2 to be posted later and the BaTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0045] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 2, and these powders, dihydroterpineol as an organic solvent, and an anionic polymer dispersant as a dispersant were pre-mixed in a medium-free stirred mill, then dispersed in a medium-stirred mill to produce a ceramic powder slurry (Process 1).

[0046] Meanwhile, nickel powder as a conductive metal powder, dihydroterpineol as an organic solvent, and an anionic polymer dispersant as a dispersant were dispersed using a three-roll mill to produce a metal powder slurry (second process).

[0047] Additionally, ethylcellulose resin as an organic resin component and dihydroterpineol as an organic solvent were mixed to obtain an organic vehicle (Process 3).

[0048] After that, the metal powder slurry and the ceramic powder slurry were added to the organic vehicle and mixed and dispersed to produce a conductive paste for forming an internal electrode (4th process).

[0049] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0050] Table 2 shows the ratio of the ionic radius of the A-site element at the 6th coordination to the ionic radius of nickel to be included in the internal electrode, i.e., the "ionic radius ratio (A-site element / metallic nickel)." Meanwhile, for sample 8, the ratio of the ionic radius at the 6th coordination of Ba (1.35 Å) shown in Table 1 to the ionic radius at the 6th coordination of Ni (0.69 Å) is shown.

[0051] 1-1-3. Fabrication of Multilayer Ceramic Capacitors

[0052] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in 1-1-1 above was prepared, and then a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a conductive paste for forming an internal electrode prepared in 1-1-2 above was applied by screen printing onto a predetermined ceramic green sheet among a plurality of ceramic green sheets. Subsequently, a plurality of ceramic green sheets were stacked and then compressed to obtain a raw laminate. Subsequently, the raw laminate was sintered. After that, an external electrode was formed on the cross-section of the sintered laminate, and a multilayer ceramic capacitor serving as a sample was manufactured.

[0053] 1-1-4. Evaluation

[0054]

[0055] The internal electrode and dielectric layer located in the center of the laminate in the height direction of the sample multilayer ceramic capacitor were separated from each other by electric field peeling.

[0056] Next, the area near the center of the exposed internal electrode (at the halfway point in the width direction and halfway point in the length direction) was observed using a microscope at a magnification of 100x. By analyzing the obtained image, the ratio of the area occupied by the conductive film as the internal electrode in the exposed part was calculated as the "coverage" shown in Table 2. If the "coverage" exceeded 80%, it was judged as good and "○" was entered in the "Evaluation" column, and if the "coverage" was 80% or less, it was judged as poor and "×" was entered in the "Evaluation" column.

[0057] 1-1-5. Discussion

[0058] Samples 1–3 and 5–7 in Table 2 have an "Evaluation" of "○". In these samples 1–3 and 5–7, the internal electrode contains one of NiTiO3, MgTiO3, and MnTiO3 as an ABO3 oxide. Additionally, the internal electrode contains nickel as a conductive component.

[0059] Here, attention is paid to the ionic radius. First, as indicated in the "NiTiO3" section of Table 1, the ionic radius of nickel at the 6th coordination is 0.69 Å. Meanwhile, as shown in Table 1, the ionic radii at the 6th coordination of the elements at the A-site of NiTiO3, MgTiO3, and MnTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 1 to 3 and 5 to 7, are 0.69 Å, 0.72 Å, and 0.67 Å, ​​respectively.

[0060] In samples 1 to 3 and 5 to 7 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of the metal element contained in the conductive metal particle, i.e., the "ionic radius ratio," is 0.97 or higher and 1.04 or lower.

[0061] As such, NiTiO3, MgTiO3, and MnTiO3 as ABO3 oxides in samples 1-3 and 5-7 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of nickel, which is the conductive metal to be included in the internal electrode. Since the energy difference with nickel in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 1-3 and 5-7 has increased to 84% or higher.

[0062] In addition, as with samples 5 to 7, the addition ratio of NiTiO3, MgTiO3, and MnTiO3 is not necessarily 100%, but if it is 10% or more, the effect of improving coverage is recognized compared to the case where none of NiTiO3, MgTiO3, and MnTiO3 are included. Meanwhile, it is also noted that in Experimental Example 1-1, the coverage of samples 5 to 7, in which the addition ratio of NiTiO3, MgTiO3, and MnTiO3 is 10%, shows the same value as the coverage of samples 1 to 3, in which the addition ratio is 100%.

[0063] In contrast, in Sample 4, which was evaluated as "×", CuTiO3 was used as the ABO3 oxide, and the ionic radius of Cu at the 6th coordination, which is the element of the A-site in ABO3, is 0.73 Å as shown in Table 1. Therefore, the ratio of the ionic radius of Cu at the 6th coordination to the ionic radius of nickel at the 6th coordination, i.e., the "ionic radius ratio," is 1.06. That is, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was lowered to 75%.

[0064] In addition, in Sample 8, which was evaluated as "×", only BaTiO3 was added to the internal electrode as a co-material. In this case, Ba, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius at 6-coordinated Ba is 1.35 Å as shown in Table 1. Therefore, the ratio of the ionic radius at 6-coordinated Ba to the ionic radius at 6-coordinated Nickel, i.e., the "ionic radius ratio," is 1.96. Consequently, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was reduced to 74%.

[0065] In these samples 4 and 8, the "ionic radius ratio" is outside the range of 0.97 or higher and 1.04 or lower, and it is presumed that CuTiO3 and BaTiO3 are ejected from the internal electrode portion, respectively, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0066] (Experimental Example 1-2) Main component of the ceramic constituting the dielectric layer: CaZrO3

[0067] 1-2-1. Fabrication of CaZrO3-based ceramic raw materials constituting the dielectric layer

[0068] As starting materials, powders of the main components CaCO3 and ZrO2, and powders of the minor components MnO, SiO2, and MgO were weighed, mixed for 72 hours using a ball mill, and then heat-treated at a top temperature of 1000℃ for 2 hours to obtain CaZrO3-based ceramic raw material powder.

[0069] 1-2-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0070] The powder of "ABO3 oxide" shown in Table 3 to be posted later and the CaZrO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0071] The powders of these "ABO3 oxides" and the CaZrO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 3, and a conductive paste for forming internal electrodes was prepared by following the same process as in Experimental Example 1-1.

[0072] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0073] Table 3 shows the "ionic radius ratio (A-site element / metallic nickel)" as in Table 2. Meanwhile, for sample 18, the ratio of the ionic radius at the 6th coordination of Ca (1.00 Å) shown in Table 1 to the ionic radius at the 6th coordination of Ni (0.69 Å) is shown.

[0074] 1-2-3. Fabrication of Multilayer Ceramic Capacitors

[0075] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 1-1.

[0076] 1-2-4. Evaluation

[0077]

[0078] Following the same procedure as in Experimental Example 1-1, "coverage" was calculated as shown in Table 3 and evaluated in the same way.

[0079] 1-2-5. Discussion

[0080] Samples 11–13 and 15–17 in Table 3 have an "Evaluation" of "○". In these samples 11–13 and 15–17, the internal electrode contains one of NiTiO3, MgTiO3, and MnTiO3 as an ABO3 oxide. Additionally, the internal electrode contains nickel as a conductive component.

[0081] Here, attention is paid to the ionic radius. First, as indicated in the "NiTiO3" section of Table 1, the ionic radius of nickel at the 6th coordination is 0.69 Å. Meanwhile, as shown in Table 1, the ionic radii at the 6th coordination of the elements at the A-site of NiTiO3, MgTiO3, and MnTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 11–13 and 15–17, are 0.69 Å, 0.72 Å, and 0.67 Å, ​​respectively.

[0082] In samples 11–13 and 15–17 evaluated as “○”, the ratio of the ionic radius of the element at the A-site in ABO3 to the ionic radius at the 6-coordinate of the metal element contained in the conductive metal particle, i.e., the “ionic radius ratio,” is 0.97 or higher and 1.04 or lower.

[0083] As such, NiTiO3, MgTiO3, and MnTiO3 as ABO3 oxides in samples 11–13 and 15–17 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of nickel, which is a conductive metal to be included in the internal electrode. Since the energy difference with nickel in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is presumed that the coverage in samples 11–13 and 15–17 is increased to 81% or higher.

[0084] In addition, as with samples 15 to 17, the addition ratio of NiTiO3, MgTiO3, and MnTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of NiTiO3, MgTiO3, and MnTiO3 are included.

[0085] In contrast to these, in sample 14 evaluated as "×", CuTiO3 was used as the ABO3 oxide, and the ionic radius of Cu at the 6th coordination, which is the element of the A-site in ABO3, is 0.73 Å as shown in Table 1. Therefore, the ratio of the ionic radius of Cu at the 6th coordination to the ionic radius of nickel at the 6th coordination, i.e., the "ionic radius ratio," is 1.06. That is, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was lowered to 75%.

[0086] In addition, in Sample 18, which was evaluated as "×", only CaZrO3 was added to the internal electrode as a co-material. In this case, Ca, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Ca at 6-coordinated is 1.00 Å as shown in Table 1. Therefore, the ratio of the ionic radius of Ca at 6-coordinated to the ionic radius of nickel at 6-coordinated, i.e., the "ionic radius ratio," is 1.45. Consequently, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was reduced to 72%.

[0087] In these samples 14 and 18, the "ionic radius ratio" is outside the range of 0.97 or higher and 1.04 or lower, and it is presumed that CuTiO3 and CaZrO3 are ejected from the internal electrode portion, respectively, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0088] (Experimental Example 1-3) Main component of the ceramic constituting the dielectric layer: SrTiO3

[0089] 1-3-1. Fabrication of SrTiO3-based ceramic raw materials constituting the dielectric layer

[0090] As starting materials, each powder of the main components SrCO3 and TiO2, and each powder of the minor components MnO, SiO2, and MgO were weighed, mixed for 72 hours using a ball mill, and then heat-treated at a top temperature of 1000℃ for 2 hours to obtain SrTiO3-based ceramic raw material powder.

[0091] 1-3-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0092] The powder of "ABO3 oxide" shown in Table 4 to be posted later and the SrTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0093] The powders of these "ABO3 oxides" and SrTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 4, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 1-1.

[0094] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0095] Table 4 shows the "ionic radius ratio (A-site element / metallic nickel)" as in Table 2. Meanwhile, for sample 28, the ratio of the ionic radius at 6-coordinate of Sr (1.18 Å) shown in Table 1 to the ionic radius at 6-coordinate of Ni (0.69 Å) is shown.

[0096] 1-3-3. Fabrication of Multilayer Ceramic Capacitors

[0097] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 1-1.

[0098] 1-3-4. Evaluation

[0099]

[0100] Following the same procedure as in Experimental Example 1-1, "coverage" was calculated as shown in Table 4 and evaluated in the same way.

[0101] 1-3-5. Discussion

[0102] Samples 21–23 and 25–27 in Table 4 have an "Evaluation" of "○". In these samples 21–23 and 25–27, the internal electrode contains one of NiTiO3, MgTiO3, and MnTiO3 as an ABO3 oxide. Additionally, the internal electrode contains nickel as a conductive component.

[0103] Here, attention is paid to the ionic radius. First, as indicated in the "NiTiO3" section of Table 1, the ionic radius of nickel at the 6th coordination is 0.69 Å. Meanwhile, as shown in Table 1, the ionic radii at the 6th coordination of the elements at the A-site of NiTiO3, MgTiO3, and MnTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 21–23 and 25–27, are 0.69 Å, 0.72 Å, and 0.67 Å, ​​respectively.

[0104] In samples 21–23 and 25–27 evaluated as “○”, the ratio of the ionic radius of the element at the A-site in ABO3 to the ionic radius at the 6-coordinate of the metal element contained in the conductive metal particle, i.e., the “ionic radius ratio,” is 0.97 or higher and 1.04 or lower.

[0105] As such, NiTiO3, MgTiO3, and MnTiO3 as ABO3 oxides in samples 21–23 and 25–27 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of nickel as the conductive metal to be included in the internal electrode. Since the energy difference with nickel in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 21–23 and 25–27 exceeds 80%.

[0106] In addition, as with samples 25 to 27, the addition ratio of NiTiO3, MgTiO3, and MnTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of NiTiO3, MgTiO3, and MnTiO3 are included.

[0107] In contrast, in sample 24 evaluated as "×", CuTiO3 was used as the ABO3 oxide, and the ionic radius of Cu at the 6th coordination, which is the element of the A-site in ABO3, is 0.73 Å as shown in Table 1. Therefore, the ratio of the ionic radius of Cu at the 6th coordination to the ionic radius of nickel at the 6th coordination, i.e., the "ionic radius ratio," is 1.06. That is, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was lowered to 72%.

[0108] In addition, in Sample 28, which was similarly evaluated as "×", only SrTiO3 as a co-material was added to the internal electrode. In this case, Sr, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Sr at 6-coordinated is 1.18 Å as shown in Table 1. Therefore, the ratio of the ionic radius of Sr at 6-coordinated to the ionic radius of nickel at 6-coordinated, i.e., the "ionic radius ratio," is 1.71. Consequently, the "ionic radius ratio" falls outside the range of 0.97 or higher and 1.04 or lower, and the coverage was reduced to 70%.

[0109] In these samples 24 and 28, the "ionic radius ratio" is outside the range of 0.97 or higher and 1.04 or lower, and it is presumed that CuTiO3 and SrTiO3 are ejected from the internal electrode portion, respectively, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0110] [Experimental Example 2] Conductive metal powder: Copper powder

[0111] In Experimental Example 2, copper powder was prepared as a conductive metal powder included in a conductive paste for forming an internal electrode.

[0112] Meanwhile, CuTiO3, CoTiO3, and CrTiO3 were prepared as ABO3 oxides of specific ionic radii constituting the ceramic powder included in the conductive paste for forming internal electrodes, and BaTiO3, CaZrO3, and SrTiO3 were prepared as other ABO3 oxides. Table 5 shows the "crystal structure," "coordination number," "A-site element," and "ionic radius" for these ABO3 oxides. Meanwhile, Ba, Ca, and Sr are 12-coordinated when in the conventional perovskite structure, but since Ba, Ca, and Sr are 6-coordinated when incorporated into the sites of 6-coordinated elements (Cu, Co, Cr) of the ilmenite structure, the "ionic radius" in Table 5 represents the value at 6-coordinated.

[0113]

[0114] Below, Experimental Examples 2-1, 2-2, and 2-3, which were conducted by changing the ceramic raw materials constituting the dielectric layer, will be described.

[0115] (Experimental Example 2-1) Main component of the ceramic constituting the dielectric layer: BaTiO3

[0116] 2-1-1. Fabrication of BaTiO3-based ceramic raw materials constituting the dielectric layer

[0117] BaTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-1.

[0118] 2-1-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0119] The powder of "ABO3 oxide" shown in Table 6 to be posted later and the BaTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0120] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 6, and a conductive paste for forming internal electrodes was prepared by following the same process as in Experimental Example 1-1.

[0121] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0122] Table 6 shows the ratio of the ionic radius of the A-site element in the 6th coordination to the ionic radius of copper to be included in the internal electrode, i.e., the "ionic radius ratio (A-site element / metallic copper)." Meanwhile, for sample 37, the ratio of the ionic radius in the 6th coordination of the Ba element (1.35 Å) shown in Table 5 to the ionic radius in the 6th coordination of copper (0.77 Å) is shown.

[0123] 2-1-3. Fabrication of Multilayer Ceramic Capacitors

[0124] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 1-1.

[0125] 2-1-4. Evaluation

[0126]

[0127] Following the same procedure as in Experimental Example 1-1, "coverage" was calculated as shown in Table 6 and evaluated in the same way.

[0128] 2-1-5. Discussion

[0129] Samples 31 to 36 in Table 6 have an "Evaluation" of "○". In these samples 31 to 36, the internal electrode contains one of CuTiO3, CoTiO3, and CrTiO3 as an ABO3 oxide. Additionally, the internal electrode contains copper as a conductive component.

[0130] Here, attention is paid to the ionic radius. First, as indicated in the "CuTiO3" section of Table 5, the ionic radius of copper at the 6th coordination is 0.77 Å. Meanwhile, as shown in Table 5, the ionic radii at the 6th coordination of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 31 to 36, are 0.77 Å, 0.74 Å, and 0.80 Å, respectively.

[0131] In samples 31 to 36 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of copper, i.e., the "ionic radius ratio," is 0.96 or higher and 1.04 or lower.

[0132] As such, CuTiO3, CoTiO3, and CrTiO3 as ABO3 oxides in samples 31 to 36 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of copper, which is the conductive metal to be included in the internal electrode. Since the energy difference with copper in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 31 to 36 has increased to 84% or higher.

[0133] In addition, as with samples 34 to 36, the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is not necessarily 100%, but if it is 10% or more, the effect of improving coverage is recognized compared to the case where none of CuTiO3, CoTiO3, and CrTiO3 are included. Meanwhile, it is also noted that in Experimental Example 2-1, the coverage of samples 34 to 36, in which the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is 10%, shows the same value as the coverage of samples 31 to 33, in which the addition ratio is 100%.

[0134] In contrast, in sample 37, which was evaluated as "×", only BaTiO3 was added to the internal electrode as a co-material. In this case, Ba, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius at 6-coordinated Ba is 1.35 Å, as shown in Table 5. Therefore, the ratio of the ionic radius at 6-coordinated Ba to the ionic radius at 6-coordinated copper, i.e., the "ionic radius ratio," is 1.75. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.04 or lower, and the coverage was reduced to 74%.

[0135] In sample 37, the "ion radius ratio" is outside the range of 0.96 or higher and 1.04 or lower, and it is presumed that BaTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0136] (Experimental Example 2-2) Main component of the ceramic constituting the dielectric layer: CaZrO3

[0137] 2-2-1. Fabrication of CaZrO3-based ceramic raw materials constituting the dielectric layer

[0138] CaZrO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-2.

[0139] 2-2-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0140] The powder of "ABO3 oxide" shown in Table 7 to be posted later and the CaZrO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0141] The powders of these "ABO3 oxides" and the CaZrO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 7, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 2-1.

[0142] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0143] Table 7 shows the "ionic radius ratio (A-site element / metallic copper)" as in Table 6. Meanwhile, for sample 47, the ratio of the ionic radius at the 6th coordination of the Ca element (1.00 Å) shown in Table 5 to the ionic radius at the 6th coordination of copper (0.77 Å) is shown.

[0144] 2-2-3. Fabrication of Multilayer Ceramic Capacitors

[0145] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 2-1.

[0146] 2-2-4. Evaluation

[0147]

[0148] Following the same procedure as in Experimental Example 2-1, "coverage" was calculated as shown in Table 7 and evaluated in the same way.

[0149] 2-2-5. Discussion

[0150] Samples 41 to 46 in Table 7 have an "Evaluation" of "○". In these samples 41 to 46, the internal electrode contains one of CuTiO3, CoTiO3, and CrTiO3 as an ABO3 oxide. Additionally, the internal electrode contains copper as a conductive component.

[0151] Here, focusing on the ionic radius, first, as indicated in the "CuTiO3" section of Table 5, the ionic radius of copper at the 6th coordination is 0.77 Å. Meanwhile, as shown in Table 5, the ionic radii at the 6th coordination of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 41 to 46, are 0.77 Å, 0.74 Å, and 0.80 Å, respectively.

[0152] In samples 41 to 46 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of copper, i.e., the "ionic radius ratio," is 0.96 or higher and 1.04 or lower.

[0153] As such, CuTiO3, CoTiO3, and CrTiO3 as ABO3 oxides in samples 41 to 46 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of copper, which is a conductive metal to be included in the internal electrode. Since the energy difference with copper in the internal electrode becomes zero or small, they remain without being discharged from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is presumed that the coverage in samples 41 to 46 is increased to 81% or higher.

[0154] In addition, as with samples 44 to 46, the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of CuTiO3, CoTiO3, and CrTiO3 are included.

[0155] In contrast, in sample 47, which was evaluated as "×", only CaZrO3 was added to the internal electrode as a co-material. In this case, Ca, the element of the A-site in the perovskite structure ABO3, is 12-coordinated, but when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Ca at 6-coordinated is 1.00 Å as shown in Table 5. Therefore, the ratio of the ionic radius of Ca at 6-coordinated to the ionic radius of copper at 6-coordinated, i.e., the "ionic radius ratio," is 1.30. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.04 or lower, and the coverage was reduced to 72%.

[0156] In sample 47, the "ion radius ratio" is outside the range of 0.96 or higher and 1.04 or lower, and it is presumed that CaZrO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0157] (Experimental Example 2-3) Main component of the ceramic constituting the dielectric layer: SrTiO3

[0158] 2-3-1. Fabrication of SrTiO3-based ceramic raw materials constituting the dielectric layer

[0159] SrTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Examples 1-3.

[0160] 2-3-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0161] The powder of "ABO3 oxide" shown in Table 8 to be posted later and the SrTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0162] The powders of these "ABO3 oxides" and the SrTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 8, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 2-1.

[0163] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0164] Table 8 shows the "ionic radius ratio (A-site element / metallic copper)" as in Table 6. Meanwhile, for sample 57, the ratio of the ionic radius at 6-coordinate of Sr element (1.18 Å) shown in Table 5 to the ionic radius at 6-coordinate of copper (0.77 Å) is shown.

[0165] 2-3-3. Fabrication of Multilayer Ceramic Capacitors

[0166] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 2-1.

[0167] 2-3-4. Evaluation

[0168]

[0169] Following the same procedure as in Experimental Example 2-1, "coverage" was calculated as shown in Table 8 and evaluated in the same way.

[0170] 2-3-5. Discussion

[0171] Samples 51 to 56 in Table 8 have an "Evaluation" of "○". In these samples 51 to 56, the internal electrode contains one of CuTiO3, CoTiO3, and CrTiO3 as an ABO3 oxide. Additionally, the internal electrode contains copper as a conductive component.

[0172] Here, attention is drawn to the ionic radius. First, as indicated in the "CuTiO3" section of Table 5, the ionic radius of copper at the 6th coordination is 0.77 Å. Meanwhile, as shown in Table 5, the ionic radii at the 6th coordination of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 51 to 56, are 0.77 Å, 0.74 Å, and 0.80 Å, respectively.

[0173] In samples 51 to 56 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of copper, i.e., the "ionic radius ratio," is 0.96 or higher and 1.04 or lower.

[0174] As such, CuTiO3, CoTiO3, and CrTiO3 as ABO3 oxides in samples 51 to 56 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of copper, which is a conductive metal to be included in the internal electrode. Since the energy difference with copper in the internal electrode becomes zero or small, they remain without being discharged from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 51 to 56 exceeds 80%.

[0175] In addition, as with samples 54 to 56, the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of CuTiO3, CoTiO3, and CrTiO3 are included.

[0176] In contrast, in sample 57, which was evaluated as "×", only SrTiO3 as a co-material was added to the internal electrode. In this case, Sr, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Sr at 6-coordinated is 1.18 Å as shown in Table 5. Therefore, the ratio of the ionic radius of Sr at 6-coordinated to the ionic radius of copper at 6-coordinated, i.e., the "ionic radius ratio," is 1.53. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.04 or lower, and the coverage was reduced to 70%.

[0177] In sample 57, the "ionic radius ratio" is outside the range of 0.96 or higher and 1.04 or lower, and it is presumed that SrTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0178] [Experimental Example 3] Conductive metal powder: Silver powder

[0179] In Experimental Example 3, silver powder was prepared as a conductive metal powder included in a conductive paste for forming an internal electrode.

[0180] Meanwhile, AgTiO3, EuTiO3, and NaTiO3 were prepared as ABO3 oxides of specific ionic radii constituting the ceramic powder included in the conductive paste for forming internal electrodes, and CuTiO3, SrTiO3, BaTiO3, and CaZrO3 were prepared as other ABO3 oxides. Table 9 shows the "crystal structure," "coordination number," "A-site element," and "ionic radius" for these ABO3 oxides. On the other hand, Sr, Ba, and Ca are 12-coordinated when in the conventional perovskite structure, but since Sr, Ba, and Ca are 6-coordinated when incorporated into the sites of 6-coordinated elements (Ag, Eu, Na) of the ilmenite structure, the "ionic radius" in Table 9 represents the value at 6-coordinated.

[0181]

[0182] Below, Experimental Examples 3-1, 3-2, and 3-3, which were conducted by changing the ceramic raw materials constituting the dielectric layer, will be described.

[0183] (Experimental Example 3-1) Main component of the ceramic constituting the dielectric layer: BaTiO3

[0184] 3-1-1. Fabrication of BaTiO3-based ceramic raw materials constituting the dielectric layer

[0185] BaTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-1.

[0186] 3-1-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0187] The powder of "ABO3 oxide" shown in Table 10 to be posted later and the BaTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0188] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 10, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 1-1.

[0189] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0190] Table 10 shows the ratio of the ionic radius of the A-site element in the 6th coordination to the ionic radius of silver in the 6th coordination to be included in the internal electrode, i.e., the "ionic radius ratio (A-site element / metallic silver)". Meanwhile, for sample 68, the ratio of the ionic radius in the 6th coordination of Ba element (1.35 Å) shown in Table 9 to the ionic radius in the 6th coordination of silver (1.15 Å) is shown.

[0191] 3-1-3. Fabrication of Multilayer Ceramic Capacitors

[0192] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 1-1.

[0193] 3-1-4. Evaluation

[0194]

[0195] Following the same procedure as in Experimental Example 1-1, "coverage" was calculated as shown in Table 6 and evaluated in the same way.

[0196] 3-1-5. Discussion

[0197] Samples 61–63 and 65–67 in Table 10 have an "Evaluation" of "○". In these samples 61–63 and 65–67, the internal electrode contains one of AgTiO3, EuTiO3, and NaTiO3 as an ABO3 oxide. Additionally, the internal electrode contains silver as a conductive component.

[0198] Here, attention is drawn to the ionic radius. First, as indicated in the "AgTiO3" section of Table 9, the ionic radius of silver at the 6th coordination is 1.15 Å. Meanwhile, as indicated in Table 9, the ionic radii at the 6th coordination of the elements at the A-site of AgTiO3, EuTiO3, and NaTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 61–63 and 65–67, are 1.15 Å, 1.17 Å, and 1.02 Å, respectively.

[0199] In samples 61–63 and 65–67 evaluated as “○”, the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of silver, i.e., the “ionic radius ratio,” is 0.89 or higher and 1.02 or lower.

[0200] As such, AgTiO3, EuTiO3, and NaTiO3 as ABO3 oxides in samples 61–63 and 65–67 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of silver, which is the conductive metal to be included in the internal electrode. Since the energy difference with silver in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 61–63 and 65–67 has increased to 82% or more.

[0201] In addition, as with samples 65 to 67, the addition ratio of AgTiO3, EuTiO3, and NaTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of AgTiO3, EuTiO3, and NaTiO3 are included.

[0202] In contrast, in sample 64 evaluated as "×", SrTiO3 was used as the ABO3 oxide, and the ionic radius of Sr, the element of the A-site in ABO3, at the 6th coordination is 1.18 Å, as shown in Table 9. Therefore, the ratio of the ionic radius of Sr at the 6th coordination to the ionic radius of silver at the 6th coordination, i.e., the "ionic radius ratio," is 1.03. That is, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was reduced to 76%.

[0203] In addition, in sample 68, which was similarly evaluated as "×", only BaTiO3 was added to the internal electrode as a co-material. In this case, Ba, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when incorporated into the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius at 6-coordinated Ba is 1.35 Å as shown in Table 9. Therefore, the ratio of the ionic radius at 6-coordinated Ba to the ionic radius at 6-coordinated silver, i.e., the "ionic radius ratio," is 1.17. Consequently, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was reduced to 75%.

[0204] In these samples 64 and 68, the "ionic radius ratio" is outside the range of 0.89 or higher and 1.02 or lower, and it is presumed that BaTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0205] (Experimental Example 3-2) Main component of the ceramic constituting the dielectric layer: CaZrO3

[0206] 3-2-1. Fabrication of CaZrO3-based ceramic raw materials constituting the dielectric layer

[0207] CaZrO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-2.

[0208] 3-2-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0209] The powder of "ABO3 oxide" shown in Table 11 to be posted later and the CaZrO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0210] The powders of these "ABO3 oxides" and the CaZrO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 11, and a conductive paste for forming internal electrodes was prepared by following the same process as in Experimental Example 3-1.

[0211] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0212] Table 11 shows the "ionic radius ratio (A-site element / metal silver)" as in Table 10. Meanwhile, for sample 78, the ratio of the ionic radius at 6-coordinate of the Ca element (1.00 Å) shown in Table 9 to the ionic radius at 6-coordinate of silver (1.15 Å) is shown.

[0213] 3-2-3. Fabrication of Multilayer Ceramic Capacitors

[0214] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 3-1.

[0215] 3-2-4. Evaluation

[0216]

[0217] Following the same procedure as in Experimental Example 3-1, "coverage" was calculated as shown in Table 11 and evaluated in the same way.

[0218] 3-2-5. Discussion

[0219] Samples 71–73 and 75–77 in Table 11 have an "Evaluation" of "○". In these samples 71–73 and 75–77, the internal electrode contains one of AgTiO3, EuTiO3, and NaTiO3 as an ABO3 oxide. Additionally, the internal electrode contains silver as a conductive component.

[0220] Here, attention is paid to the ionic radius. First, as indicated in the "AgTiO3" section of Table 9, the ionic radius of silver at the 6th coordination is 1.15 Å. Meanwhile, as indicated in Table 9, the ionic radii at the 6th coordination of the elements at the A-site of AgTiO3, EuTiO3, and NaTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 71–73 and 75–77, are 1.15 Å, 1.17 Å, and 1.02 Å, respectively.

[0221] In samples 71–73 and 75–77 evaluated as “○”, the ratio of the ionic radius of the element at the A-site in ABO3 to the ionic radius at the 6-coordinate of silver, i.e., the “ionic radius ratio,” is 0.89 or higher and 1.02 or lower.

[0222] As such, AgTiO3, EuTiO3, and NaTiO3 as ABO3 oxides in samples 71–73 and 75–77 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of silver, which is a conductive metal to be included in the internal electrode. Since the energy difference with silver in the internal electrode becomes zero or small, they remain without being ejected from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is presumed that the coverage in samples 71–73 and 75–77 is increased to 81% or more.

[0223] In addition, as with samples 75 to 77, the addition ratio of AgTiO3, EuTiO3, and NaTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of AgTiO3, EuTiO3, and NaTiO3 are included.

[0224] In contrast, in sample 74 evaluated as "×", CuTiO3 was used as the ABO3 oxide, and the ionic radius of Cu at the 6th coordination, which is the element of the A-site in ABO3, is 0.73 Å as shown in Table 9. Therefore, the ratio of the ionic radius at the 6th coordination of Cu to the ionic radius at the 6th coordination of silver, i.e., the "ionic radius ratio," is 0.63. That is, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was lowered to 75%.

[0225] In addition, in sample 78, which was similarly evaluated as "×", only CaZrO3 was added to the internal electrode as a co-material. In this case, although Ca, the element of the A-site in the perovskite structure ABO3, is 12-coordinated, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Ca at 6-coordinated is 1.00 Å as shown in Table 9. Therefore, the ratio of the ionic radius of Ca at 6-coordinated to the ionic radius of silver at 6-coordinated, i.e., the "ionic radius ratio," is 0.87. Consequently, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was reduced to 72%.

[0226] In these samples 74 and 78, the "ionic radius ratio" is outside the range of 0.89 or higher and 1.02 or lower, and it is presumed that CaZrO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0227] (Experimental Example 3-3) Main component of the ceramic constituting the dielectric layer: SrTiO3

[0228] 3-3-1. Fabrication of SrTiO3-based ceramic raw materials constituting the dielectric layer

[0229] SrTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Examples 1-3.

[0230] 3-3-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0231] The powder of "ABO3 oxide" shown in Table 12 to be posted later and the SrTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0232] The powders of these "ABO3 oxides" and SrTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 12, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 3-1.

[0233] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0234] Table 12 shows the "ionic radius ratio (A-site element / metal silver)" as in Table 10. Meanwhile, for sample 88, the ratio of the ionic radius at 6-coordinate of the Sr element (1.18 Å) shown in Table 9 to the ionic radius at 6-coordinate of silver (1.15 Å) is shown.

[0235] 3-3-3. Fabrication of Multilayer Ceramic Capacitors

[0236] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 3-1.

[0237] 3-3-4. Evaluation

[0238]

[0239] Following the same procedure as in Experimental Example 3-1, "coverage" was calculated as shown in Table 12 and evaluated in the same way.

[0240] 3-3-5. Discussion

[0241] Samples 81–83 and 85–87 in Table 12 have an “Evaluation” of “○”. In these samples 81–83 and 85–87, the internal electrode contains one of AgTiO3, EuTiO3, and NaTiO3 as an ABO3 oxide. Additionally, the internal electrode contains silver as a conductive component.

[0242] Here, attention is drawn to the ionic radius. First, as indicated in the "AgTiO3" section of Table 9, the ionic radius of silver at the 6th coordination is 1.15 Å. Meanwhile, as indicated in Table 9, the ionic radii at the 6th coordination of the elements at the A-site of AgTiO3, EuTiO3, and NaTiO3, respectively, which are ABO3 oxides included in the internal electrodes of samples 81–83 and 85–87, are 1.15 Å, 1.17 Å, and 1.02 Å, respectively.

[0243] In samples 81–83 and 85–87 evaluated as “○”, the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of silver, i.e., the “ionic radius ratio,” is 0.89 or higher and 1.02 or lower.

[0244] As such, AgTiO3, EuTiO3, and NaTiO3 as ABO3 oxides in samples 81–83 and 85–87 have an ionic radius at the 6th coordination of the element at the A-site in ABO3 that is equal to or close to the ionic radius at the 6th coordination of silver as the conductive metal to be included in the internal electrode. Since the energy difference with silver in the internal electrode becomes zero or small, they remain without being discharged from the internal electrode portion and act to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 81–83 and 85–87 exceeds 80%.

[0245] In addition, as with samples 85 to 87, the addition ratio of AgTiO3, EuTiO3, and NaTiO3 is not necessarily 100%, but is 10% or more, and the effect of improved coverage was recognized compared to the case where none of AgTiO3, EuTiO3, and NaTiO3 are included.

[0246] In contrast, in sample 84 evaluated as "×", CuTiO3 was used as the ABO3 oxide, and the ionic radius of Cu at the 6th coordination, which is the element of the A-site in ABO3, is 0.73 Å as shown in Table 9. Therefore, the ratio of the ionic radius at the 6th coordination of Cu to the ionic radius at the 6th coordination of silver, i.e., the "ionic radius ratio," is 0.63. That is, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was reduced to 72%.

[0247] In addition, in sample 88, which was similarly evaluated as "×", only SrTiO3 as a co-material was added to the internal electrode. In this case, Sr, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Sr at 6-coordinated is 1.18 Å as shown in Table 9. Therefore, the ratio of the ionic radius of Sr at 6-coordinated to the ionic radius of silver at 6-coordinated, i.e., the "ionic radius ratio," is 1.03. Consequently, the "ionic radius ratio" falls outside the range of 0.89 or higher and 1.02 or lower, and the coverage was reduced to 70%.

[0248] In these samples 84 and 88, the "ionic radius ratio" is outside the range of 0.89 or higher and 1.02 or lower, and it is presumed that SrTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0249] [Experimental Example 4] Conductive metal powder: Silver / palladium alloy powder

[0250] In Experimental Example 4, a silver / palladium alloy powder consisting of an alloy of 70 atm% silver and 30 atm% palladium was prepared as a conductive metal powder to be included in a conductive paste for forming an internal electrode.

[0251] Meanwhile, as an ABO3 oxide of a specific ionic radius constituting the ceramic powder included in the conductive paste for forming internal electrodes (Ag 0.7 , Pd 0.3 Along with preparing TiO3, NaTiO3, and EuTiO3, BaTiO3, CaZrO3, and SrTiO3 were prepared as other ABO3 oxides. Table 13 shows the "crystal structure," "coordination number," "A-site element," and "ionic radius" for these ABO3 oxides. Meanwhile, Ba, Ca, and Sr are 12-coordinated when in the conventional perovskite structure, but since Ba, Ca, and Sr are also 6-coordinated when incorporated into the sites of 6-coordinated elements (Ag / Pd, Na, Eu) of the ilmenite structure, the "ionic radius" in Table 13 represents the value at 6-coordinated.

[0252]

[0253] Below, Experimental Examples 4-1, 4-2, and 4-3, which were conducted by changing the ceramic raw materials constituting the dielectric layer, will be described.

[0254] (Experimental Example 4-1) Main component of the ceramic constituting the dielectric layer: BaTiO3

[0255] 4-1-1. Fabrication of BaTiO3-based ceramic raw materials constituting the dielectric layer

[0256] BaTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-1.

[0257] 4-1-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0258] The powder of "ABO3 oxide" shown in Table 14 to be posted later and the BaTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0259] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 14, and a conductive paste for forming internal electrodes was prepared through the same process as in Experimental Example 1-1.

[0260] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0261] Table 14 shows the ratio of the ionic radius at the 6th coordination of the A-site element to the ionic radius at the 6th coordination of the silver / palladium alloy to be included in the internal electrode, i.e., the "ionic radius ratio (A-site element / Ag 0.7 Pd 0.3 The alloy” is indicated. Meanwhile, for sample 97, the ratio of the ionic radius at 6th coordination (1.06 Å) of the silver / palladium alloy to the ionic radius at 6th coordination (1.35 Å) of the Ba element shown in Table 13 is indicated.

[0262] 4-1-3. Fabrication of Multilayer Ceramic Capacitors

[0263] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 1-1.

[0264] 4-1-4. Evaluation

[0265]

[0266] Following the same procedure as in Experimental Example 1-1, "coverage" was calculated as shown in Table 6 and evaluated in the same way.

[0267] 4-1-5. Discussion

[0268] Samples 91–96 in Table 14 have an "Evaluation" of "○". In these samples 91–96, the internal electrode is ABO3 oxide (Ag 0.7 , Pd0.3 It contains one of TiO3, NaTiO3, and EuTiO3. In addition, the internal electrode contains a silver / palladium alloy as a conductive component.

[0269] Here, focusing on the ionic radius, first, as indicated in the "(Ag, Pd)TiO3" section of Table 13, the ionic radius at the 6th coordination of the silver / palladium alloy is 1.06 Å. Meanwhile, as for the ABO3 oxide contained in the internal electrodes of samples 91–96 (Ag 0.7 , Pd 0.3 The ionic radii at the 6-coordinate of the elements at the A-site of TiO3, NaTiO3, and EuTiO3, respectively, are 1.06 Å, 1.02 Å, and 1.17 Å, respectively, as shown in Table 13.

[0270] In samples 91 to 96 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of the metal element contained in the conductive metal particle, i.e., the "ionic radius ratio," is 0.96 or higher and 1.10 or lower.

[0271] Thus, as ABO3 oxide in samples 91–96 (Ag 0.7 , Pd 0.3 Since the ionic radius at the 6th coordination of the element at the A-site in ABO3 of TiO3, NaTiO3, and EuTiO3 is equal to or close to the ionic radius at the 6th coordination of the silver / palladium alloy as the conductive metal to be included in the internal electrode, the energy difference with the silver / palladium alloy in the internal electrode becomes zero or small, so it remains without being discharged from the internal electrode portion and acts to improve the heat resistance of the internal electrode. As a result, it is estimated that the coverage in samples 91 to 96 increased to 82% or higher.

[0272] In addition, as with samples 94–96, (Ag 0.7 , Pd 0.3The addition ratio of )TiO3, NaTiO3, and EuTiO3 is not necessarily 100%, and if it is 10% or more, (Ag 0.7 , Pd 0.3 Compared to cases that do not contain any of TiO3, NaTiO3, or EuTiO3, the effect of improved coverage was recognized.

[0273] In contrast, in sample 97, which was evaluated as "×", only BaTiO3 was added to the internal electrode as a co-material. In this case, Ba, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Ba at 6-coordinated is 1.35 Å, as shown in Table 13. Therefore, the ratio of the ionic radius at 6-coordinated Ba to the ionic radius at 6-coordinated silver / palladium alloy, i.e., the "ionic radius ratio," is 1.27. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.10 or lower, and the coverage was reduced to 75%.

[0274] In sample 97, the "ionic radius ratio" is outside the range of 0.96 or higher and 1.10 or lower, and it is presumed that BaTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0275] (Experimental Example 4-2) Main component of the ceramic constituting the dielectric layer: CaZrO3

[0276] 4-2-1. Fabrication of CaZrO3-based ceramic raw materials constituting the dielectric layer

[0277] CaZrO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Example 1-2.

[0278] 4-2-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0279] The powder of "ABO3 oxide" shown in Table 15 to be posted later and the CaZrO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0280] The powders of these "ABO3 oxides" and the CaZrO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 15, and a conductive paste for forming internal electrodes was prepared by following the same process as in Experimental Example 4-1.

[0281] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0282] In Table 15, as in Table 14, "ionic radius ratio (A-site element / Ag 0.7 Pd 0.3 "Alloy" is indicated. Meanwhile, for sample 107, the ratio of the ionic radius at 6th coordination (1.00 Å) of the Ca element shown in Table 13 to the ionic radius at 6th coordination (1.06 Å) of the silver / palladium alloy is indicated.

[0283] 4-2-3. Fabrication of Multilayer Ceramic Capacitors

[0284] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 4-1.

[0285] 4-2-4. Evaluation

[0286]

[0287] Following the same procedure as in Experimental Example 4-1, "coverage" was calculated as shown in Table 15 and evaluated in the same way.

[0288] 4-2-5. Discussion

[0289] Samples 101–106 in Table 15 have an "Evaluation" of "○". In these samples 101–106, the internal electrode is ABO3 oxide (Ag 0.7 , Pd 0.3 It contains one of TiO3, NaTiO3, and EuTiO3. In addition, the internal electrode contains a silver / palladium alloy as a conductive component.

[0290] Here, focusing on the ionic radius, first, as indicated in the "(Ag, Pd)TiO3" section of Table 13, the ionic radius at the 6th coordination of the silver / palladium alloy is 1.06 Å. Meanwhile, as the ABO3 oxide contained in the internal electrodes of samples 101–106 (Ag 0.7 , Pd 0.3 The ionic radii at the 6-coordinate of the elements at the A-site of TiO3, NaTiO3, and EuTiO3, respectively, are 1.06 Å, 1.02 Å, and 1.17 Å, respectively, as shown in Table 13.

[0291] In samples 101 to 106 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 to the ionic radius at the 6th coordination of the metal element contained in the conductive metal particle, i.e., the "ionic radius ratio," is 0.96 or higher and 1.10 or lower.

[0292] Thus, as (Ag as ABO3 oxide in samples 101–106 0.7 , Pd 0.3 Since the ionic radius at the 6th coordination of the element at the A-site in ABO3 of TiO3, NaTiO3, and EuTiO3 is equal to or close to the ionic radius at the 6th coordination of the silver / palladium alloy as the conductive metal to be included in the internal electrode, the energy difference with the silver / palladium alloy in the internal electrode becomes zero or small, so it remains without being discharged from the internal electrode portion and acts to improve the heat resistance of the internal electrode, and as a result, it is presumed that the coverage in samples 101 to 106 increased to 81% or more.

[0293] In addition, as with samples 104–106, (Ag 0.7 , Pd 0.3 The addition ratio of )TiO3, NaTiO3, and EuTiO3 is not necessarily 100%, and if it is 10% or more, (Ag 0.7 , Pd 0.3 Compared to cases that do not contain any of TiO3, NaTiO3, or EuTiO3, the effect of improved coverage was recognized.

[0294] In contrast, in sample 107, which was evaluated as "×", only CaZrO3 was added to the internal electrode as a co-material. In this case, Ca, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Ca at 6-coordinated is 1.00 Å, as shown in Table 13. Therefore, the ratio of the ionic radius at 6-coordinated Ca to the ionic radius at 6-coordinated silver / palladium alloy, i.e., the "ionic radius ratio," is 0.94. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.10 or lower, and the coverage was reduced to 72%.

[0295] In sample 107, the "ion radius ratio" is outside the range of 0.96 or higher and 1.10 or lower, and it is presumed that CaZrO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0296] (Experimental Example 4-3) Main component of the ceramic constituting the dielectric layer: SrTiO3

[0297] 4-3-1. Fabrication of SrTiO3-based ceramic raw materials constituting the dielectric layer

[0298] SrTiO3-based ceramic raw material powder was obtained by undergoing the same process as in Experimental Examples 1-3.

[0299] 4-3-2. Fabrication of Conductive Paste for Internal Electrode Formation

[0300] The powder of "ABO3 oxide" shown in Table 16 to be posted later and the SrTiO3-based ceramic raw material powder for the dielectric layer were used as ceramic powders included in the conductive paste for forming internal electrodes.

[0301] The powders of these "ABO3 oxides" and SrTiO3-based ceramic raw material powders were weighed to the "addition ratio" shown in Table 16, and a conductive paste for forming internal electrodes was prepared by following the same process as in Experimental Example 4-1.

[0302] Here, the content of ceramic powder in the conductive paste for forming internal electrodes was set to 10 mass%.

[0303] In Table 16, as in Table 14, "ionic radius ratio (A-site element / Ag 0.7 Pd 0.3 "Alloy" is indicated. Meanwhile, for sample 117, the ratio of the ionic radius at 6th coordination (1.18 Å) of the Sr element shown in Table 13 to the ionic radius at 6th coordination (1.06 Å) of the silver / palladium alloy is indicated.

[0304] 4-3-3. Fabrication of Multilayer Ceramic Capacitors

[0305] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in 1 above was prepared, and then, a ceramic green sheet was formed by applying the doctor blade method to the ceramic slurry. Subsequently, a multilayer ceramic capacitor serving as a sample was prepared by undergoing the same process as in Experimental Example 4-1.

[0306] 4-3-4. Evaluation

[0307]

[0308] Following the same procedure as in Experimental Example 4-1, "coverage" was calculated as shown in Table 16 and evaluated in the same way.

[0309] 4-3-5. Discussion

[0310] Samples 111–116 in Table 16 have an "Evaluation" of "○". In these samples 111–116, the internal electrode is ABO3 oxide (Ag 0.7 , Pd 0.3 It contains one of TiO3, NaTiO3, and EuTiO3. In addition, the internal electrode contains a silver / palladium alloy as a conductive component.

[0311] Here, focusing on the ionic radius, first, as indicated in the "(Ag, Pd)TiO3" section of Table 13, the ionic radius at the 6th coordination of the silver / palladium alloy is 1.06 Å. Meanwhile, as the ABO3 oxide contained in the internal electrodes of samples 111–116 (Ag 0.7 , Pd 0.3 The ionic radii at the 6-coordinate of the elements at the A-site of TiO3, NaTiO3, and EuTiO3, respectively, are 1.06 Å, 1.02 Å, and 1.17 Å, respectively, as shown in Table 13.

[0312] In samples 111 to 116 evaluated as "○", the ratio of the ionic radius of the element at the A-site in ABO3 to the ionic radius at the 6-coordinate of the silver / palladium alloy, i.e., the "ionic radius ratio," is 0.96 or higher and 1.10 or lower.

[0313] Thus, as (Ag as ABO3 oxide in samples 111–116 0.7 , Pd 0.3 Since the ionic radius at the 6th coordination of the element at the A-site in ABO3 of TiO3, NaTiO3, and EuTiO3 is equal to or close to the ionic radius at the 6th coordination of the silver / palladium alloy as the conductive metal to be included in the internal electrode, the energy difference with the silver / palladium alloy in the internal electrode becomes zero or small, so it remains without being discharged from the internal electrode portion and acts to improve the heat resistance of the internal electrode, and as a result, it is estimated that the coverage in samples 111 to 116 exceeds 80%.

[0314] In addition, as with samples 114–116, (Ag 0.7 , Pd 0.3 The addition ratio of )TiO3, NaTiO3, and EuTiO3 is not necessarily 100%, and if it is 10% or more, (Ag 0.7 , Pd 0.3 Compared to cases that do not contain any of TiO3, NaTiO3, or EuTiO3, the effect of improved coverage was recognized.

[0315] In contrast, in sample 117, which was evaluated as "×", only SrTiO3 as a co-material was added to the internal electrode. In this case, Sr, the element of the A-site in the perovskite structure ABO3, is 12-coordinated; however, when dissolved in the A-site of the ilmenite structure, it is necessary to compare it with the ionic radius at 6-coordinated, which is the coordination number of the A-site in the ilmenite structure, and the ionic radius of Sr at 6-coordinated is 1.18 Å, as shown in Table 13. Therefore, the ratio of the ionic radius of Sr at 6-coordinated to the ionic radius at 6-coordinated of the silver / palladium alloy, i.e., the "ionic radius ratio," is 1.11. Consequently, the "ionic radius ratio" falls outside the range of 0.96 or higher and 1.10 or lower, and the coverage was reduced to 70%.

[0316] In sample 117, the "ionic radius ratio" is outside the range of 0.96 or higher and 1.10 or lower, and it is presumed that SrTiO3 is ejected from the internal electrode portion, so the heat resistance of the internal electrode is not improved and the coverage is lowered.

[0317] [organize]

[0318] As a result of the above-described experimental examples 1 to 4, the following preferred range was found regarding the ratio of the ionic radius at the 6th coordination of the element at the A-site in ABO3 to the ionic radius at the 6th coordination of the metal contained in the conductive metal powder.

[0319] (1) Experimental Example 1: 0.97~1.04

[0320] (2) Experimental Example 2: 0.96~1.04

[0321] (3) Experimental Example 3: 0.89~1.02

[0322] (4) Experimental Example 4: 0.96~1.10

[0323] The types of metals constituting the conductive metal powder differ, as shown in Experimental Example 1 as nickel, Experimental Example 2 as copper, Experimental Example 3 as silver, and Experimental Example 4 as a silver / palladium alloy. However, even though the types of metals differ in this way, there is a common aspect regarding the range of the ratio of appropriate ionic radii. By having this common aspect, the scope of the present invention is defined. That is, the present invention is characterized by a powder composed of an ABO3-type oxide in which the ratio of the ionic radius at the 6th coordination of the element at the A-site in ABO3 to the ionic radius at the 6th coordination of the metal included in the conductive metal powder is 0.97 or higher and 1.02 or lower.

[0324] In the experimental examples described above, nickel powder, copper powder, silver powder, and silver / palladium alloy powder were used as the conductive metal powders included in the conductive paste for forming internal electrodes. However, it is also possible to use materials other than the above powders as the conductive metal powders. In addition, any ABO3-type oxide of a specific ionic radius may be any ABO3-type oxide as long as the ratio of the ionic radius of the element at the 6th coordination of the A-site in ABO3 to the ionic radius at the 6th coordination of the metal element included in the conductive metal powder included in the conductive paste is 0.97 or higher and 1.02 or lower.

[0325] Embodiments of the present invention include the following:

[0326] <1>

[0327] A conductive paste for forming internal electrodes of a multilayer ceramic capacitor, comprising a conductive metal powder, a ceramic powder, an organic solvent, and an organic binder,

[0328] A conductive paste, wherein at least a portion of the ceramic powder is a powder composed of an ABO3-type oxide having a specific ionic radius, wherein the ratio of the ionic radius at the 6th coordination of an element at the A-site in ABO3 to the ionic radius at the 6th coordination of a metal included in the conductive metal powder is 0.97 or more and 1.02 or less.

[0329] <2>

[0330] In paragraph 1,

[0331] The above ABO3 type oxide of a specific ionic radius is a conductive paste having an ilmenite crystal structure.

[0332] <3>

[0333] In paragraph 1 or 2,

[0334] A conductive paste comprising one type selected from nickel, copper, silver, and silver / palladium alloy, wherein the conductive metal powder is the conductive paste.

[0335] <4>

[0336] In any one of paragraphs 1 through 3,

[0337] A conductive paste in which at least 10 volume% of the ceramic powder is a powder composed of an ABO3-type oxide of the specific ionic radius, and the remainder of the ceramic powder is a powder having at least one selected from BaTiO3, SrTiO3, and CaZrO3 as a main component.

[0338] <5>

[0339] A laminate comprising a plurality of stacked dielectric layers made of ceramic and a plurality of internal electrodes each disposed along a plurality of interfaces between the dielectric layers, and

[0340] A multilayer ceramic capacitor, wherein the internal electrode comprises a conductive component and a ceramic component, and at least a portion of the ceramic component comprises an ABO3-type oxide of a specific ionic radius, wherein the ratio of the ionic radius of an element at the A-site in ABO3 to the ionic radius at the 6-coordinate of a metal included in the conductive component is 0.97 or more and 1.02 or less. Explanation of the symbols

[0341] 1: Multilayer ceramic capacitor 2: Laminate 3: Dielectric layer 4, 5: Internal electrodes 6, 7: External electrodes

Claims

Claim 1 A conductive paste for forming internal electrodes of a multilayer ceramic capacitor comprising a conductive metal powder, a ceramic powder, an organic solvent, and an organic binder, wherein at least a portion of the ceramic powder is a powder composed of an ABO3-type oxide having a specific ionic radius, wherein the ratio of the ionic radius of an element at the A-site in ABO3 to the ionic radius at the 6-coordinate of a metal included in the conductive metal powder is 0.97 or more and 1.02 or less. Claim 2 In claim 1, the ABO3 type oxide of the specific ionic radius is a conductive paste having an ilmenite crystal structure. Claim 3 A conductive paste according to claim 1, wherein the conductive metal powder comprises one selected from nickel, copper, silver, and silver / palladium alloy. Claim 4 A conductive paste according to any one of claims 1 to 3, wherein 10 volume percent or more of the ceramic powder is a powder composed of an ABO3-type oxide of the specific ionic radius, and the remainder of the ceramic powder is a powder having at least one selected from BaTiO3, SrTiO3, and CaZrO3 as a main component. Claim 5 A multilayer ceramic capacitor comprising a plurality of stacked dielectric layers made of ceramic and a plurality of internal electrodes each disposed along a plurality of interfaces between the dielectric layers, wherein the internal electrodes comprise a conductive component and a ceramic component, and at least a portion of the ceramic component comprises an ABO3-type oxide of a specific ionic radius such that the ratio of the ionic radius of an element at the 6th coordination of ABO3 to the ionic radius at the 6th coordination of a metal included in the conductive component is 0.97 or more and 1.02 or less.

Citation Information

Patent Citations

  • Conductive paste for via conductor and ceramic wiring board using it and its manufacturing method

    JP2005276826A

  • Paste for internal electrode

    KR1019990000612A

  • Dielectric ceramic composition, multilayer complex electronic device, multilayer common mode filter, multilayer ceramic coil and multilayer ceramic capacitor