Alloy of having Dual-Phase interconnected Three-Dimensionally and Method of manufacturing the same

The multi-component alloy with a Cu-rich channel region addresses the limitations of conventional LMD by forming a three-dimensional structure with enhanced conductivity and stability, leveraging controlled miscibility and selective dissolution of elements.

KR103046543B1Active Publication Date: 2026-11-10DANKOOK UNIV CHEONAN CAMPUS IND ACADEMIC COOP FOUND
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250215941
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-12-31
Publication Date
2026-11-10
Estimated Expiration
2045-12-31

AI Technical Summary

Technical Problem

Conventional Liquid Metal Dealoying (LMD) processes struggle to produce multi-component alloys with a three-dimensional continuous linkage structure that satisfy various physical properties, as they distinguish between metal elements that remain and those that are leached, limiting the formation of alloys with diverse functionalities.

Method used

A multi-component alloy comprising a ligament structure formed by residual components of a precursor alloy after immersion in molten metal, with a channel region filled by a Cu-rich phase, achieved by controlling the miscibility and selective dissolution of elements like Co, Cr, Fe, Mn, Ni, and optionally Mo, through the LMD process.

Benefits of technology

The resulting alloy exhibits improved conductivity, hardness, and wear resistance due to its high specific surface area and chemical stability, with the Cu-rich channel regions enhancing electrical and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025149426041-PAT00006_ABST
    Figure 112025149426041-PAT00006_ABST
Patent Text Reader

Abstract

A multi-component alloy and a method for manufacturing the same are disclosed, wherein a liquid metal dealloying process is performed by introducing a multi-component precursor alloy into a molten metal. Due to differences in mixing enthalpy within the molten metal, specific metal elements are separated from the precursor alloy, and metal elements having a relatively large mixing enthalpy are separated from the precursor alloy slowly. Channel regions formed by filling the spaces between ligaments are also formed into a multi-component alloy, and Cu, etc. of the molten metal diffuses into the ligaments and participates in the multi-component alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an alloy having a double-phase heterostructure, and more specifically, to an alloy having a heterostructure in which a channel component fills the internal shape of a three-dimensional continuous connection structure formed by a ligament structure and a decomposition reaction of a high-entropy alloy, and a method for manufacturing the same. Background Technology

[0002] Liquid Metal Dealoying (LMD) is a process in which a pre-manufactured alloy is immersed in a specific liquid metal to selectively dissolve specific components within the alloy. After dissolution, the remaining components form a three-dimensional continuous-linked framework structure. The resulting three-dimensional continuous-linked framework structure is formed in nano- or micro-sized dimensions, and due to the high interfacial area and the three-dimensional continuous-linked structure, it offers the advantage of simultaneously securing strength and electrical conductivity.

[0003] The execution of the above process involves the manufacture of an alloy, the proceeding of dealloying by immersing the alloy in liquid metal, and the process of self-organization.

[0004] Figure 1 is a schematic diagram illustrating an LMD according to the prior art.

[0005] Referring to Fig. 1, an alloy composed of AB is first formed. Metal elements A and B have miscibility. Due to this miscibility, the formed alloy can have a specific crystal structure. Subsequently, the alloy with the composition of AB is introduced into a molten metal containing metal element C. It is assumed that in the alloy, metal element B has high solubility in C, while metal element A has low solubility. Due to solubility, metal element B escapes from the alloy. Consequently, most of the metal B escapes from the alloy, thereby forming a ligament with metal A as the main component. At this time, the molten C penetrates around the generated ligament, forming a complex network structure between the ligament and the liquid phase; the alloy then possesses a composite material structure with a high interfacial area and a three-dimensional continuous connection structure.

[0006] Alloys produced by LMD have a three-dimensional continuous structure in which two phases individually form a matrix, allowing both to function as a matrix. This enables multifunctionality by combining the advantages of each phase, making it applicable to various improvements in physical properties. Furthermore, if a nanoporous material with a three-dimensional continuous structure is created using a process that removes only specific phases, such as selective etching via acid treatment, it can be utilized as a catalyst or energy storage structure due to its continuous porous structure rather than isolated pores, which offers diverse applications.

[0007] Korean Registered Patent No. 10-2847746 discloses the manufacture of a porous Ti structure using LMD. First, a precursor alloy Ti-X is prepared, and X is a metal having a negative mixing enthalpy with Mg. Therefore, X can easily form a solid solution or a new compound with Mg. Through this process, a porous Ti structure is manufactured.

[0008] As mentioned above, conventional LMDs focus on the formation of porous structures, and technological development is proceeding in a direction that maximizes the pores of the porous structures.

[0009] In addition, we propose a porous structure composed solely of pure metal phases through LMD by utilizing the miscibility relationships between metal elements. However, porous structures composed of pure metals do not satisfy the requirements for various physical properties. This is due to the fact that the conventional LMD process distinguishes between metal elements that remain without clearly reacting with the molten metal and metal elements that are leached out through reaction. For this reason, three-dimensional continuous-linked composite materials or porous structures formed through the conventional LMD process have the disadvantage of not yet being able to be manufactured into multi-component alloys.

[0010] In other words, it is known that it is difficult to manufacture multi-component alloys in which various metal elements have miscibility and form a solid solution using the existing LMD process. On the other hand, there is a persistent demand in the industry for multi-component alloys that have a three-dimensional continuous linkage structure and satisfy various required physical properties. The problem to be solved

[0011] The first technical problem to be achieved by the present invention is to provide a multi-component alloy having a heterostructure having a channel region of molten metal that fills the region between the ligaments, which are the solid framework structure.

[0012] The second technical objective of the present invention is to provide a method for manufacturing a multi-component alloy to achieve the first technical objective. means of solving the problem

[0013] The present invention for achieving the first technical objective described above comprises: Co: 17.5 at.% to 20 at.%, Cr: 12.5 at.% to 20 at.%, Fe: 20.0 at.% to 55.0 at.%, Mn: 0 at.% to 20 at.%, Ni: 10 at.% to 20 at.%, Cu 100-x Ag x : x contains 0 at.% to 60 at.% of other impurities, and provides a multicomponent alloy comprising a channel region in which a liquid metal Cu-rich phase fills the space between the ligaments, which are interconnected solid framework structures. During the LMD process, the channel region, which is the liquid metal, solidifies into a solid state as the temperature decreases after the LMD process.

[0014] In addition, the first technical problem of the present invention is Co: 17.5 at.% to 20 at.%, Cr: 12.5 at.% to 20 at.%, Fe: 20.0 at.% to 55.0 at.%, Mo: 0 at.% to 5 at.%, Ni: 10 at.% to 20 at.%, Cu 100-x Ag x : x is also achieved by providing a multicomponent alloy containing 0 at.% to 60 at.% other impurities, a ligament which is a solid framework structure connected to each other, and a channel region which fills the region between the ligaments and is a Cu-rich phase.

[0015] The present invention, for achieving the second technical objective described above, provides a method for manufacturing a multi-component alloy comprising the steps of: preparing a precursor alloy of CoCrFeNiMn; immersing the precursor alloy in a molten metal; and forming a ligament having residual components of the precursor alloy through dealloying by immersion in the molten metal, and forming a channel region that fills the region between the ligaments through self-organization.

[0016] The second technical problem of the present invention is also achieved by providing a method for manufacturing a multi-component alloy comprising the steps of: preparing a precursor alloy of CoCrFeNiMo; immersing the precursor alloy in a molten metal; forming a ligament having residual components of the precursor alloy through dealloying by immersion in the molten metal and a channel region filling the area between the ligaments through self-organization; and selectively removing the channel region to leave the ligament having a needle-like shape. Effects of the invention

[0017] According to the present invention described above, ligaments can be formed through dealloying, and channels can be formed to fill the regions between the formed ligaments. The molten metal can be formed from Cu or an alloy of Cu, and the channels have a new alloy phase rich in Cu. Through this, at least two types of alloy forms appear, high conductivity can be obtained, and hardness and wear resistance are improved.

[0018] In addition, if the Cu-rich region forming the channel is selectively etched, needle- or nanorod-shaped alloys appear. The structure of the alloy has a high specific surface area and can possess excellent chemical stability due to the alloy's unique composition. Brief explanation of the drawing

[0019] Figure 1 is a schematic diagram illustrating an LMD according to the prior art. FIG. 2 shows FE-SEM images illustrating a multi-component alloy according to Manufacturing Example 1 of the present invention. Figure 3 is a graph showing the depth of the dealloyalization reaction of a sample according to Manufacturing Example 1 of the present invention. Figure 4 shows images illustrating the reaction interface state when the LMD process is carried out in Manufacturing Example 1 of the present invention and images of the prior art. Figure 5 shows images illustrating the microstructures of the multi-component alloy according to Manufacturing Example 1 of the present invention and the alloys according to the prior art of Figure 4. Figure 6 shows backscattered electron microscope (BSE) images of a multi-component alloy subjected to the LMD process according to Manufacturing Example 1 of the present invention. Figure 7 is a graph showing the change in composition according to LMD reaction time through point EDX in a multi-component alloy according to Manufacturing Example 1 of the present invention. Figure 8 is a graph showing the composition through point EDX of a specimen in which a 12-minute LMD reaction was performed according to Manufacturing Example 1 of the present invention. Figure 9 is an XRD graph of a specimen on which a 12-minute LMD reaction was performed according to Manufacturing Example 1 of the present invention. FIG. 10 is a schematic diagram illustrating the LMD reaction according to Manufacturing Example 1 of the present invention. Figure 11 is a graph showing the hardness of a specimen according to Manufacturing Example 1 of the present invention relative to the immersion time. Figure 12 shows Electron Backscatter Diffraction (EBSD) images of the multi-component alloy of Figure 11 according to the immersion time of the present invention. FIG. 13 is an orientation diagram showing the pole figure and grain orientation of the results of FIG. 12 of the present invention. FIG. 14 is a graph showing the electrical conductivity of a specimen according to Manufacturing Example 1 of the present invention. Figure 15 is a graph measuring the wear resistance of the specimen of Manufacturing Example 1 of the present invention. FIG. 16 is a BSE image of a multi-component alloy according to Manufacturing Examples 2 to 4 of the present invention. Figure 17 shows EDX mapping images of the multi-component alloy of Manufacturing Example 3 of the present invention. FIG. 18 is a graph showing the LMD reaction depth in Preparation Examples 2 to 4 of the present invention. FIG. 19 is an XRD graph of the multi-component alloys of Preparation Examples 3 and 4 of the present invention. FIG. 20 are EBSD images illustrating the multi-component alloy of Manufacturing Example 4 of the present invention. FIG. 21 is a table showing the composition of the multi-component alloy of Manufacturing Example 4 of the present invention through EDX analysis. FIG. 22 is a graph showing the thickness of the reaction layer according to the dealloying time of the specimen of Manufacturing Example 5 of the present invention. Figure 23 is an SEM image of the specimen of Preparation Example 5 of the present invention. FIG. 24 are enlarged images of the specimen of FIG. 23 of the present invention. FIG. 25 is an image for analyzing the ligament in a portion of FIG. 24 for the specimen of Manufacturing Example 5 of the present invention, and a graph showing the composition of constituent metal elements according to specific positions. FIG. 26 is an image showing the position of a selected ligament to investigate the content of the constituent metal in image (b) of FIG. 24 for the specimen of Manufacturing Example 5 of the present invention. FIG. 27 are images of the Cu-rich channel region removed from the specimen of Manufacturing Example 5 of the present invention. Specific details for implementing the invention

[0020] The present invention is susceptible to various modifications and may take various forms; therefore, specific embodiments are illustrated in the drawings and described in detail in the text. However, this is not intended to limit the invention to the specific disclosed forms, and it should be understood that the invention includes all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention. Similar reference numerals have been used for similar components in the description of each drawing.

[0021] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application.

[0022] Hereinafter, preferred embodiments of the present invention will be described in more detail with reference to the attached drawings.

[0024] Examples

[0025] The multi-component alloy having a heterostructure of the present embodiment consists of a combination or bonding of two types of phases. The first phase is the ligament remaining through the LMD process, and the second phase is a channel region that fills the area between the ligaments formed by the LMD process. When the two phases are numerically summed, the multi-component alloy of the present embodiment is Co a Cr b Fe c Mn d Ni e Cu f Cu 100-x Ag x It has the composition of.

[0026] In the above multi-component alloy, the sum of the at.% of the elements, a+b+c+d+e+f, is 100 at.% including other unavoidable impurities.

[0027] The content of the elements constituting the entire multi-component alloy is as follows.

[0028] Co : 17.5 at.% to 20 at.%

[0029] Cr : 12.5 at.% to 20 at.%

[0030] Fe : 20.0 at.% to 55.0 at.%

[0031] Mn : 0 at.% to 20 at.%

[0032] Ni : 10.0 at.% to 20 at.%

[0033] Cu 100-x Ag x : x is 0 at.% to 60 at.%

[0034] The above multicomponent alloy has two types of phases, namely ligament and channel regions. The ligament typically has a face-centered cubic structure relatively rich in Co, Cr, and Fe due to the leaching of Mn and Ni, while the channel region may have a region relatively rich in Cu.

[0035] Mn and Ni are elements in which selective dissolution occurs preferentially, so the sum of their ratios must be at least 20 at.% for a solid ligament framework structure to develop effectively. Even if Mn is 0 at.%, Ni replaces the role of Mn because selective dissolution of Ni occurs faster than that of other precursor elements.

[0036] In addition, in the multi-component alloy of the present invention, Mo may be included to replace Mn, and Mo may be contained in an amount of 0 at.% to 5 at.%. When Mo is substituted, rapid dissolution can be completely suppressed because Mo has much lower miscibility with Cu than other precursor elements, thereby providing the effect of maintaining the size of the precursor alloy after the LMD process. Even with the addition of a small amount of 5 at.% Mo, the ligament framework structure inside the precursor can be continuously maintained even if the LMD process time is prolonged, and the ligaments are formed as needle-like structures in the Mo-rich regions. In this case as well, the infiltrating channel regions become Cu-rich regions and fill the regions between the ligaments. Although the concentration of Mo was set to 5 at.% in the examples, increasing the concentration can further increase the fraction of Mo-rich ligaments.

[0037] In addition, in multicomponent alloys replaced with Mo, channel regions can be selectively removed to form ligaments composed of needles or nanorods.

[0038] Cu 100-x Ag x The fraction is important as it alters the reactivity with the precursor alloy, but it does not change the fundamental mechanism for fabricating ligaments with a three-dimensional continuous linkage structure. A higher Ag concentration can lower the LMD reaction temperature and allow for more effective control of selective dissolution phenomena. However, if the Ag concentration exceeds 60 at.%, the molten metal temperature must be raised again, and since the cost of the molten metal material increases, a concentration of 60 at.% or less is desirable.

[0039] The two types of phases formed in this embodiment are divided into a ligament forming a solid framework and a channel region filling the area between the ligaments, as described above. An alloy of CoCrFeMnNi is formed to perform the LMD process. This is referred to as a precursor alloy.

[0040] The above precursor alloy is introduced into a molten metal of Cu or CuAg. Due to the difference in miscibility with Cu or Ag, Mn and Ni are mixed with Cu, etc., in a relatively high proportion within the alloy, while Fe, Co, and Cr have relatively low miscibility and are therefore mixed with Cu, etc., in a low proportion.

[0041] The mechanism of the metal elements constituting the alloy is explained below.

[0042] Co has low miscibility with Cu, which is provided as molten metal, and due to this low miscibility, melting does not proceed smoothly in the beginning, forming solid ligaments.

[0043] Cr has the characteristic of not easily mixing with Cu together with Co, forms a solid ligament, and enhances corrosion resistance.

[0044] Fe forms ligaments just like Co and Cr, and provides strength and ductility to the alloy.

[0045] Since Mn has high miscibility with Cu, it is selectively melted by Cu and others, leaches out from the initial alloy, and self-organizes together with Cu and others to form channel regions.

[0046] Ni has the second-highest miscibility with Cu, etc., after Mn, selectively melts into the molten metal of Cu, etc., and can remain on the ligament through various control techniques. Therefore, it can act as a key element in forming a face-centered cubic structure as an alloying element.

[0047] Mo is used selectively and is useful for forming ligament phases because it does not react with molten metal such as Cu.

[0048] The mechanism regarding the composition of the molten metal is explained below.

[0049] Cu is contained in the molten metal in an amount of 40.0 at.% to 100.0 at.%, selectively reacts with the precursor alloy, and penetrates into the precursor alloy to form a molten phase through the selective reaction of the metal elements constituting the precursor alloy. Subsequently, the solidified Cu-rich phase forms channel regions. The formed channel regions have high thermal and electrical conductivity and reduce the coefficient of friction of the entire alloy.

[0050] Ag is used selectively in the molten metal and can be contained in an amount ranging from 0.0 at.% to 60.0 at.%; it is used to control reactivity with precursor alloys. Ag is an element with much lower miscibility than Cu with precursor alloy elements such as Co, Cr, Fe, Mn, and Ni; essentially, Co, Cr, Fe, and Ni have very low solubility in molten Ag. Therefore, it acts as a molten metal alloying element that completely controls selective reactions. Like Cu, Ag also improves electrical and thermal conductivity. The channel regions that solidify due to the use of Ag form a microstructure and deepen the heterostructure.

[0051] Cu and Ag are elements with lower melting points than precursor elements, and they are molten metal elements that enable the LMD process, in which solid ligaments are maintained. When Cu and Ag are mixed through process reactions, the temperature of the molten metal can be lowered. Lowering the temperature of the molten metal reduces the unit size of the resulting ligament structure and the size of the internal crystal grains, which helps improve strength and wear resistance.

[0052] The manufacture of multi-component alloys having a heterostructure follows the following procedure.

[0053] Precursor metals constituting the precursor alloy are prepared, and homogenization heat treatment is performed.

[0054] The precursor metals are mixed in the specified at.% ratio, placed in a crucible, and melted and cast by heating. Through this, a precursor alloy is manufactured.

[0055] Homogenization heat treatment is performed on the precursor alloy after casting, and this needs to be carried out at a temperature of 1,000°C to 1,200°C. Through homogenization heat treatment, non-uniformity of the components within the precursor alloy is eliminated, and the metal structure is made uniform.

[0056] Subsequently, cold rolling is performed on the precursor alloy. Grains that have grown excessively or coarsely during the homogenization heat treatment process are plastically deformed through cold rolling, thereby increasing the strength of the precursor alloy. In the case of a multi-component precursor alloy, a reduction ratio of 70% or more is preferable, but the reduction ratio can be changed by those skilled in the art and is not a critical factor in securing the physical properties of the multi-component alloy of the present invention. Therefore, those skilled in the art may appropriately change the reduction ratio when implementing the present invention.

[0057] Subsequently, a post-heat treatment is performed on the precursor alloy that has undergone the rolling process. The post-heat treatment is a process that removes internal stress generated through rolling and induces recrystallization. Through recrystallization, the ductility of the precursor alloy is restored, and a stable alloy state is obtained. In this embodiment, it is preferable that the post-heat treatment be performed at 1,000°C to 1,100°C for 6 to 18 hours. Through this, a precursor alloy in a stable alloy state is produced.

[0058] When the precursor alloy is completed, the precursor alloy is immersed in a molten metal. The molten metal is composed mainly of Cu with Ag optionally added. In addition, the molten metal has a temperature range of 800°C to 1,100°C, and the time required for dealloying and self-organization when the precursor alloy is immersed is set differently depending on the size of the precursor alloy.

[0059] When a precursor alloy is immersed in a molten metal, selective melting occurs between the metal elements constituting the precursor alloy due to differences in mixing enthalpy.

[0060] Table 1 shows the mixing enthalpy between Cu and the metal elements constituting the precursor alloy.

[0061] Metal elements of precursor alloys ΔH mix with Cu (kJ / mol) Co 6 Cr 12 Fe 13 Mn 4 Ni 4

[0062] Among the metallic elements, Mn and Ni have the relatively lowest mixing enthalpy values; therefore, within the precursor alloy, Mn and Ni dissolve into Cu at a relatively high rate to form an alloy with Cu, while other metallic elements dissolve at a relatively low rate. Due to the selective dissolution or leaching of metallic elements, the precursor alloy has a ligament structure with a three-dimensional continuous connection structure into which the molten CuAg has penetrated.

[0063] In addition, when Cu is incorporated into the elements constituting the solid ligament, it lowers the free energy of the ligament alloy, causing the Cu metal in the molten metal to diffuse and penetrate into the ligament structure. However, the ligament, which is the structure remaining after the selective melting of the precursor alloy, has a relatively low concentration of Cu. Furthermore, the regions between the three-dimensional continuous ligament structures formed by selective melting are melted by Cu and filled with a molten phase containing miscible Ni and Mn.

[0065] Preparation Example 1: Preparation of a heterostructured multicomponent alloy using a CoCrFeMnNi precursor alloy 1

[0066] Co, Cr, Fe, Mn, and Ni metal powders were each melted and cast in a uniform ratio of 20 at.%, and a homogenization heat treatment was performed at 1,100°C for 6 hours, followed by water cooling. Additionally, the alloy was cold-rolled with a reduction rate of 77%. The final thickness of the manufactured precursor alloy is 1.5 mm.

[0067] The proportions of constituent metal elements in the precursor alloy are uniform at 20 at.% each. However, a small loss of at.% may occur due to various causes during the manufacturing process.

[0068] The prepared molten metal consists of Cu with a purity of 99.9%, and 427.4g of Cu is melted. The manufactured precursor alloy is immersed in the Cu molten metal at 1,095℃. The immersion times are 2, 5, 10, and 12 minutes, respectively, and the immersion of the precursor alloy in the Cu molten metal is carried out in a pure Ar atmosphere.

[0069] The LMD process is carried out in a precursor alloy immersed in a molten Cu bath. In the present invention, the term LMD process refers to the dealloying and self-organization of metal elements in the precursor alloy. Additionally, for convenience of explanation, the time during which dealloying and self-organization proceed is expressed as the LMD process time or immersion time.

[0070] In the LMD process, the channel region that fills the region from which metal elements have been leached is not removed and remains. That is, the alloy that has elapsed for a set time in the molten metal is recovered from the molten metal, and a heterostructure is formed in which the ligament and the channel region each have a network structure. In the present invention, this is referred to as a heterostructure multi-component alloy or a multi-component alloy.

[0072] FIG. 2 shows FE-SEM images illustrating a multi-component alloy according to Manufacturing Example 1 of the present invention.

[0073] Referring to FIG. 2, image (a) illustrates an alloy with an immersion time of 2 minutes. In the cut specimen, the dissolution of Mn occurs actively by the LMD process up to a predetermined depth, and a heterostructure formed by alloying with Cu appears. The heterostructure refers to a structure in which ligament and channel regions are formed, as previously described. However, due to the short immersion time, the structure is not sufficiently converted into a heterostructure, and the structure of the precursor alloy appears significantly.

[0074] Image (b) shows an alloy with an immersion time of 5 minutes. Although the heterostructure in the specimen is more deeply developed, the precursor alloy, in which the LMD process was not carried out, still appears at the cross-section of the specimen.

[0075] Image (c) shows an alloy with an immersion time of 10 minutes. In the cut specimen, the heterostructure progressed to a significant depth in the cut plane, but in the center of the specimen, the LMD process did not proceed, and a precursor alloy that did not react with Cu remained.

[0076] Image (d) shows an alloy with an immersion time of 12 minutes. With the LMD process sufficiently advanced, no unreacted precursor alloy is observed. Due to the difference in mixing enthalpy, Mn is selectively leached from the precursor alloy to form inter-ligate regions within the precursor alloy, and these regions are filled with Cu and leached metal elements. The Cu-rich regions filling the inter-ligate regions form channel regions, while the regions where Mn and Ni are predominantly dissolved are converted into the ligament phase.

[0077] The above ligament has a structure formed by the infiltration of Cu through diffusion or some degree of miscibility, with a reduced proportion of Mn compared to the initial precursor alloy. Additionally, the ligament has a three-dimensional network structure.

[0078] The regions between the ligaments within the three-dimensional network structure formed by the ligaments are filled with channel regions. The regions between the ligaments secured by the dissolution of Mn are rapidly filled by Cu in the molten metal, and due to the low mixing enthalpy, Mn forms an alloy with Cu, but with a compositional ratio different from that of the ligament phase.

[0079] Figure 3 is a graph showing the depth of the dealloyalization reaction of a sample according to Manufacturing Example 1 of the present invention.

[0080] Referring to Fig. 3, the reaction depth over time represents the distance from the surface to the point where dealolysis and self-organization are completed.

[0081] Furthermore, in Preparation Example 1, the dealolysis time is expressed as the immersion time. The dealolysis time and the reaction depth exhibit a linear proportional relationship. This corresponds to a very unusual phenomenon. In a conventional LMD process, the reaction depth is not proportional to the increase in time but exhibits a constant saturation point at a specific time. This is a phenomenon similar to diffusion behavior, where the reaction depth appears in proportion to the square root of time.

[0082] However, in the multi-component alloy of the present embodiment, the reaction depth is proportional to time. This is presumed to be because Mn is actively dissolved into the Cu matrix, and the dissolved Mn and Cu are evenly distributed within a relatively abundant amount of Cu.

[0083] In Figure 3 above, the coefficient of determination R 2 It has a value of 0.99758. That is, the straight line connecting the points in Figure 3 above shows near-perfect agreement with the experimental data, and it can be seen that the reaction depth is exactly proportional to the immersion time.

[0084] Figure 4 shows images illustrating the reaction interface state when the LMD process is carried out in Manufacturing Example 1 of the present invention and images of the prior art.

[0085] Referring to FIG. 4, images (a), (b), and (c) illustrate reaction interfaces as the immersion time or reaction time increases. In the present invention, the term reaction interface refers to a region where dealloying and self-organization are initiated, and to a boundary surface where the dissolution of a specific component metal from a precursor metal is initiated. In this embodiment, the reaction interface forms a continuous melting channel.

[0086] In the image (a) after 2 minutes of LMD process, the image (b) after 5 minutes, and the image (c) after 10 minutes, the reaction interface is clearly visible and melting channels are observed. Additionally, it is observed that the reaction interface extends into the bulk region of the sample as the reaction time progresses.

[0087] Image (d) is a conventional (FeCo) 0.7 Ni 0.3 The reaction interface is illustrated when the precursor alloy is immersed in a molten Mg bath at 800°C, and image (e) is a conventional (FeCo) 0.5 Ni 0.5 The reaction interface when the precursor alloy is immersed in a molten Mg bath at 800°C is illustrated. In images (d) and (e), the structure of the ligaments from the precursor alloy is formed in a filament shape, which is caused by the dissolution of Ni. However, the regions between the ligaments formed by the dissolution of metal elements dissolved in the molten Mg bath do not form continuous channels.

[0088] Image (f) is a conventional (FeCo) 0.3 Ni 0.7 The reaction interface when the precursor alloy is immersed in a molten Mg bath at 800°C is illustrated. In the enlarged image, a reaction interface in the form of a continuous channel appears. This is presumed to be the result of the relatively abundant Ni in the precursor alloy being actively leached out, while the leaching of Co proceeded slowly. In other words, it is predicted that a significant fraction of the leached metal within the precursor alloy is required for the leached metal to form a continuous channel.

[0089] However, in the present invention, it is observed that continuous channels of the leached metal are formed even though the fraction of the leached metal is not significantly high. This is presumed to be due to the phenomenon in which Mn is evenly distributed within the precursor alloy of the present invention and Cu, which forms the molten metal, diffuses into the precursor metal.

[0090] Figure 5 shows images illustrating the microstructures of the multi-component alloy according to Manufacturing Example 1 of the present invention and the alloys according to the prior art of Figure 4.

[0091] Image (a) is an image of a multi-component alloy separated from the molten metal after being immersed for at least 12 minutes in Preparation Example 1. The light color represents the channel region, and the dark color represents the ligament. As metal elements are selectively dissolved from the precursor alloy by the LMD process, regions between ligaments are formed within the precursor alloy, and the leached metal elements form an alloy phase different from Cu. This forms a channel region and has a form in which they are roughly physically connected to each other. In addition, the remaining ligaments form a frame that includes the regions between ligaments.

[0092] Image (b) is the existing (Fe 0.8 Cr 0.2 ) 0.7 Ni 0.3 This is an image of an alloy formed by immersing a precursor alloy in a molten Mg bath to perform the LMD process and recovering it from the bath. In the image above, Ni is dissolved into the molten bath by the LMD process, and bright-colored Fe 0.8 Cr 0.2 Ligaments appear. Additionally, the dark color is an alloy region where Ni has leached out and mixed with Mg, failing to form interconnected channels, and separate island shapes appear.

[0093] Image (c) is the existing (Fe 0.5 Cr 0.5 ) 0.7 Ni 0.3 This shows the result of performing the LMD process on a precursor alloy in a molten Mg bath. The bright area is Fe 0.5 Co 0.5 The image shows a ligament structure, and the dark area represents the region where Ni is leached out and forms an alloy with Mg. Fine channels are formed, or a type of flow path shape resulting from leaching appears. Looking at images (b) and (c), it can be seen that as the content of Co, which has a larger mixing enthalpy than Ni, increases, the region between the ligaments fills the area, and the self-organized region is prone to having a channel phase.

[0094] Figure 6 shows backscattered electron microscope (BSE) images of a multi-component alloy subjected to the LMD process according to Manufacturing Example 1 of the present invention.

[0095] Referring to FIG. 6, image (a) is a photograph of the area where phase separation or the structure of the ligament / channel region is formed after 2 minutes of immersion. Image (b) is an image of a sample that underwent a 5-minute immersion process, image (c) is an image of a sample that underwent a 10-minute immersion process, and image (d) is an image of a sample that underwent a 12-minute immersion process.

[0096] Dealoying due to immersion proceeds from the top to the bottom of the images. Additionally, as the immersion time progresses, the coarsening of the ligaments progresses, and the volume of the channels due to the molten Cu and leached metal elements increases.

[0097] It is a very unusual phenomenon for ligament coarsening to occur as the LMD process time increases. It was predicted that the size of the ligaments would decrease as metal elements were leached from the precursor alloy during the LMD process, but in the multi-component alloy of the present invention, the size of the ligaments actually tends to increase. This is presumed to be due to the removal of small-sized ligaments as the LMD process progresses, recrystallization occurring on the surface of the remaining large-sized ligaments, or due to the diffusion and recrystallization of Cu constituting the molten metal.

[0098] Figure 7 is a graph showing the change in composition according to LMD reaction time through point EDX in a multi-component alloy according to Manufacturing Example 1 of the present invention.

[0099] Referring to FIG. 7, graph (a) illustrates the composition within the solid ligament in the region where the LMD reaction is performed and which is close to the reaction interface. In the solid ligament where metal elements are leached out and reconstituted with the remaining metal elements, no significant change in composition is observed even when the LMD reaction proceeds.

[0100] Graph (b) illustrates the composition within the solid ligament adjacent to the molten Cu. No significant change in composition is observed even as the LMD reaction proceeds. However, a slight increase in Cu is observed within the ligament. This phenomenon indicates that the diffusion of Cu from the molten Cu is proceeding.

[0101] Graph (c) illustrates the change in composition within the molten channel adjacent to the reaction interface. As the LMD reaction proceeds, the Cu content decreases slightly, while an increase in Mn and Ni is observed. This indicates that as Mn and Ni from the precursor alloy continuously leaches and diffuses into the channel through the reaction interface, the leaching rate of Mn and Ni slows down, causing a change in the concentration within the molten channel.

[0102] Graph (d) illustrates the compositional change within the melting channel adjacent to the Cu molten metal. Significant changes in the content of constituent elements are not observed in the Cu molten metal, which corresponds to a bulk region.

[0103] It is worth noting that the constant dissolution of Mn and Ni at the reaction interface means that a heterostructure is fabricated in a local equilibrium state, and the fact that there is no change in the concentration of the ligament and molten channel in the region adjacent to the molten Cu over time also means that the reaction of the present invention is a process that can be controlled in a local equilibrium state.

[0104] Figure 8 is a graph showing the composition through point EDX of a specimen in which a 12-minute LMD reaction was performed according to Manufacturing Example 1 of the present invention.

[0105] Referring to Fig. 8, almost no compositional changes in Co, Cr, and Fe are observed in the ligament. However, a sharp decrease in Mn and a small decrease in Ni are observed. Additionally, Cu, which was not included in the initial precursor alloy, appears. This indicates that Cu from the molten metal has diffused into the ligament structure and is included in the composition of the alloy constituting the ligament.

[0106] Furthermore, the channel region contains a very high fraction of Cu, and has a relatively high composition of Mn and Ni. Additionally, it is confirmed that trace amounts of Co, Cr, and Fe are present. This is attributed to the fact that Mn and Ni, which have relatively low mixing enthalpies, are rapidly leached from the precursor alloy, while Co, Cr, and Fe, which have relatively high mixing enthalpies, are slowly leached from the precursor alloy.

[0107] Table 2 below discloses the measured compositional ratios of constituent metal elements within the ligament and channel, based on the compositional graph shown in Figure 8 above.

[0108] area Metal elements (at.%) Co Cr Fe Mn Ni Cu Multicomponent alloy specimen 21.3 ± 0.4 20.6 ± 0.5 20.9 ± 0.4 3.9 ± 0.7 13.4 ± 0.7 19.9 ± 0.6 Ligament 24.7 ± 0.8 23.5 ± 1.2 24.1 ± 0.7 3.9 ± 1.1 16.0 ± 1.2 7.6 ± 1.1 channel 2.9 ± 0.4 1.4 ± 0.3 2.4 ± 0.3 3.4 ± 0.9 3.1 ± 0.7 86.5 ± 2.7

[0109] In Table 2 above, the content of Mn within the ligament is significantly reduced compared to that of Ni, whereas Mn and Ni exhibit a similar content ratio within the channel region. This phenomenon is attributed to the difference in the diffusivity of the two types of metals within the Cu matrix. Since the mixing enthalpy of Mn and Ni is similar, the probability of forming an alloy with Cu is similar. However, Mn has a higher diffusion coefficient within the Cu matrix compared to Ni. Consequently, Mn diffuses rapidly into the molten Cu outside the channel region. Due to this phenomenon, the content of Mn in the ligament and channel regions is significantly reduced compared to the initial precursor alloy.

[0110] In addition, it is confirmed in Table 2 above that Cu also flows into the ligament.

[0111] Figure 9 is an XRD graph of a commercial product in which a 12-minute LMD reaction was performed according to Manufacturing Example 1 of the present invention.

[0112] Referring to Fig. 9, a single-phase face-centered cubic crystal peak is observed in the initial precursor alloy. However, in the specimen subjected to the LMD reaction, two types of face-centered cubic structures appear, which have the same or similar crystallinity and differ in minute azimuthal angles. Therefore, their peaks indicate that different FCC crystal structures are continuously connected to each other in adjacent states.

[0113] In the graph above, fcc1 represents the crystal structure of the ligament, and fcc2 illustrates the crystal structure of the channel region.

[0114] FIG. 10 is a schematic diagram illustrating the LMD reaction according to Manufacturing Example 1 of the present invention.

[0115] Referring to FIG. 10, when a precursor alloy is immersed in a molten Cu, Mn and Ni are leached from the surface of the precursor alloy. Due to the leaching of Mn and Ni, regions between the ligaments are formed, and Cu, Mn, and Ni in the molten metal fill or penetrate these regions between the ligaments, forming a melting channel. Along with the formation of the melting channel, Co, Cr, and Fe are also dissolved to some extent. Through this process, metals are ejected from the precursor alloy into the melting channel, and the remaining regions are formed as ligaments. In the melting channel, self-organization occurs through the molten metal elements other than Cu, forming a new crystal phase with a face-centered cubic structure, which is then formed into a channel region.

[0116] The above process intensifies as the LMD reaction time progresses.

[0117] In the LMD reaction, Cu in the molten channel diffuses into the ligament structure and alloys.

[0118] Through the above process, two types of face-centered cubic structures are formed, and each phase forms ligament and channel regions. These form a heterostructure.

[0119] Figure 11 is a graph showing the hardness of a specimen according to Manufacturing Example 1 of the present invention relative to the immersion time.

[0120] Referring to Fig. 11, after the precursor alloy is introduced into the Cu molten metal, the Vickers hardness is measured for the unreacted region where the LMD process was not performed and the region where the LMD process was performed and a heterostructure was formed.

[0121] For both types of cases, hardness increases as the immersion time progresses. However, a decrease in hardness was measured in specimens after 12 minutes of immersion in the area where the LMD process was performed and a heterostructure was formed, which is attributed to a slight increase in the fraction of the Cu molten metal channels.

[0122] The increase in hardness over time due to immersion is attributed to the penetration of Cu from the molten metal into the grain boundaries of unreacted regions and the formation of a microstructure.

[0123] Figure 12 shows Electron Backscatter Diffraction (EBSD) images of the multi-component alloy of Figure 11 according to the immersion time of the present invention.

[0124] Referring to Fig. 12, images (a) and (c) are Inverse Pole Figure (IPF) maps, where the orientation of the grains is represented by specific colors. This allows for the identification of different orientations of the grains and the determination of their sizes based on their classification. Additionally, images (b) and (d) are grain boundary maps of the specimens in images (a) and (b), respectively. Grain boundary maps distinguish the boundaries between grains and mark them with lines. Boundaries are classified by Δg, which is the difference in azimuth angle between two grains. Red represents low-angle boundaries where 3° < Δg < 5°, which are practically identical grains with only slight differences. Green represents medium-angle boundaries where 5° < Δg < 15°. Furthermore, blue represents high-angle boundaries with an azimuth difference of 15° < Δg < 180°, and the grain boundaries marked in blue are typical.

[0125] Images (a) and (b) illustrate the microstructural changes after 5 minutes of immersion. Due to the LMD process, coarse grains are converted into fine grains as the reaction time progresses. This phenomenon is the result of the diffusion of liquid Cu, the dissolution of constituent metal elements, and self-organization. In the reaction region where the multi-component alloy is formed, the hardness improves over time due to the fine grains. Additionally, in the grain boundary map of image (b), yellow represents ∑3, a commonly referred to twin boundary, and cyan represents ∑9, a boundary more complex than ∑3. Furthermore, the white arrows in images (b) and (c) indicate wavy ∑3 boundaries and Cu-rich phase grains.

[0126] Images (c) and (d) show images of the reaction zone immersed for 12 minutes. Over time, the grain size becomes finer, and an improvement in hardness is observed. In other words, as the LMD reaction intensifies, the grain size becomes finer.

[0127] FIG. 13 is an orientation diagram showing the pole figure grain orientations analyzed from the results of FIG. 12 of the present invention.

[0128] Referring to FIG. 13, (a) shows the normal coordinate system on the crystal plane {101}, which is the pole figure of the reaction region of the sample immersed for 5 minutes. Green indicates the orientation of the crystal grains in the unreacted region, and blue indicates the orientation of the solid ligaments. It is confirmed that the orientation of the ligaments is changed compared to the unreacted region through the LMD process.

[0129] (b) shows the orientation derived by rotating the grains of the unreacted region by 4 degrees around the [1 -2 -1] axis. The red dots indicate the orientation of the rotated grains.

[0130] (c) shows the orientation of the grains rotated 109.47 degrees around the

[0101] axis. Blue indicates the orientation of the grains of the ligand.

[0131] Through the above pole figure data, it can be seen that the LMD reaction does not occur along the conventional crystal orientation relationship where close-packed planes are parallel to each other, but rather that heterostructures and grain refinement occur along non-close-packed planes.

[0132] FIG. 14 is a graph showing the electrical conductivity of a specimen according to Manufacturing Example 1 of the present invention.

[0133] Referring to Fig. 14, the precursor alloy is indicated by ◇, and the conductivity of the specimen after 12 minutes of immersion in Preparation Example 1 is indicated by ○. After the LMD process, it is confirmed that the electrical conductivity increased by approximately 2 times at room temperature.

[0134] In addition, it is confirmed that the specimen of the present invention has excellent conductivity compared to existing alloys having a high copper content compared to the specimen of Manufacturing Example 1.

[0135] To verify the aforementioned causes, the atomic structure of each phase was simulated using Density Functional Theory (DFT), and electrical conductivity was predicted based on this. It is predicted that when trace alloying of Cu occurs in the specimen of Preparation Example 1, the ligament exhibits higher conductivity compared to the precursor alloy in which the LMD process was not performed. Furthermore, very high conductivity is observed in the channel region where Cu is relatively abundant and self-organized.

[0136] Figure 15 is a graph measuring the wear resistance of the specimen of Manufacturing Example 1 of the present invention.

[0137] Referring to Fig. 15, the y-axis plots the wear depth, representing the depth to which the surface of the specimen is gouged out due to wear after the wear resistance test. In other words, it plots the vertical distance between the original surface before wear and the lowest point of wear. The precursor specimen (As-cast) before the LMD process exhibited the highest amount of wear, while the specimen after 3 minutes of the LMD process exhibited the lowest amount of wear. The specimen after the 6-minute LMD process was also confirmed to possess improved wear resistance compared to the precursor specimen. This is because the wear resistance was enhanced by the hardness increased by the LMD process and the lubricating effect caused by the addition of Cu. The reason the 6-minute LMD specimen exhibits lower wear resistance than the 3-minute LMD specimen is believed to be due to the increased fraction of Cu molten metal channels in the precursor surface region during the 6-minute LMD process.

[0139] Preparation Example 2: Preparation of a heterostructured multicomponent alloy using a CoCrFeMnNi precursor alloy 2

[0140] A specimen of the precursor alloy is prepared in the same manner as in Preparation Example 1 above. However, compared to Preparation Example 1, Cu is used instead of molten Cu. 0.8 Ag 0.2A molten metal is used, and the temperature of the molten metal is 950℃. The precursor alloy is immersed in the molten metal, and after the LMD process is carried out, it is separated from the molten metal. Through this, a multi-component alloy having a heterostructure is manufactured.

[0142] Preparation Example 3: Preparation of a heterostructured multicomponent alloy using a CoCrFeMnNi precursor alloy 3

[0143] A specimen of the precursor alloy is prepared in the same manner as in Preparation Example 1 above. Compared to Preparation Example 1, at 800°C, Cu 0.6 Ag 0.4 The molten metal is used, and the precursor alloy undergoes the LMD process within the molten metal and is separated from the molten metal.

[0145] Preparation Example 4: Preparation of a heterostructured multi-component alloy using a CoCrFeMnNi precursor alloy 4

[0146] A specimen of the precursor alloy is prepared in the same manner as in Preparation Example 1 above. Compared to Preparation Example 1, at 950°C, Cu 0.6 Ag 0.4 The molten metal is used, and the precursor alloy undergoes the LMD process within the molten metal and is separated from the molten metal.

[0148] FIG. 16 is a BSE image of a multi-component alloy according to Manufacturing Examples 2 to 4 of the present invention.

[0149] Referring to FIG. 16, image (a) shows the multi-component alloy of Preparation Example 2, image (b) shows the multi-component alloy of Preparation Example 3, and image (c) shows the multi-component alloy of Preparation Example 4. For all three types of samples, the LMD process is performed for 20 minutes.

[0150] It is confirmed that when the Cu content in the molten metal is high, the ligament coarsening proceeds, and under conditions of low Cu content, the size of the ligament structure becomes finer. In addition, a continuously connected heterostructure resulting from self-organization in the channels is commonly observed. Furthermore, even with molten metal of the same composition, it is observed that if the temperature of the molten metal is high, the ligament structure becomes finer due to the smooth dissolution of metal elements.

[0151] Figure 17 shows EDX mapping images of the multi-component alloy of Manufacturing Example 3 of the present invention.

[0152] Referring to Fig. 17, the LMD process time is set to 20 minutes. The ligament and channel are visible in the overall image. Additionally, Mn preferentially reacts with the molten metal and is selectively dissolved, and the difference in density between the channel and the ligament is clearly visible. Furthermore, it is confirmed that Cu and Ag diffuse into the ligament. However, Ag diffuses into the ligament at a lower concentration compared to Cu.

[0153] FIG. 18 is a graph showing the LMD reaction depth in Preparation Examples 2 to 4 of the present invention.

[0154] Referring to Fig. 18, graph (a) illustrates the depth of dealolysis in the grains of the precursor alloy. As the immersion time increases, the depth of dealolysis increases, and also, as the content of Ag in the molten metal increases, the depth of reaction also tends to increase.

[0155] Graph (b) illustrates the dealloying depth at the grain boundaries of the precursor alloy. Compared to Graph (a), it is confirmed that the reaction depth increased even at the same immersion time. In other words, it is confirmed that the LMD reaction occurs preferentially through the grain boundaries of the precursor alloy.

[0156] FIG. 19 is an XRD graph of the multi-component alloys of Preparation Examples 3 and 4 of the present invention.

[0157] Referring to FIG. 19, in Preparation Example 3, the precursor alloy is immersed in the molten metal for 135 minutes to form a multi-component alloy. In addition, in Preparation Example 4, the precursor alloy is immersed in the molten metal for 60 minutes to form a multi-component alloy.

[0158] The multi-component alloys of Preparation Examples 3 and 4 exhibit three types of face-centered cubic structures. This is because, as the molten channel solidifies, the molten metal is in a state mixed with Cu and Ag, and two types of face-centered cubic structures appear in the channel region due to the phase separation of Cu and Ag within the molten metal during the solidification process. Additionally, three types of face-centered cubic structures appear overall due to the ligaments formed by the infiltration of Cu and Ag and the dissolution of some metal elements. That is, a face-centered cubic structure appears in the ligaments, and a Cu-rich face-centered cubic structure and an Ag-rich face-centered cubic structure appear within the molten channel.

[0159] FIG. 20 are EBSD images illustrating the multi-component alloy of Manufacturing Example 4 of the present invention.

[0160] Referring to FIG. 20, images (a) and (b) show images of the precursor alloy, images (c) and (d) show images of the reaction interface after 20 minutes of immersion, and images (e) and (f) show images of the reaction interface after 60 minutes of immersion. It is confirmed that grain refinement occurs at the reaction interface as the immersion time increases.

[0161] FIG. 21 is a table showing the composition of the multi-component alloy of Manufacturing Example 4 of the present invention through EDX analysis.

[0162] Referring to Fig. 21, the composition of the ligament, the composition of the Ag-rich region within the channel region, the composition of the Cu-rich region within the channel region, and the composition of the entire multi-component alloy are investigated. The LMD process is performed for 60 minutes. Significant dissolution of Mn occurs in the ligament, and due to the diffusion of Cu, Cu is contained in the ligament at a rate of approximately 4%. In addition, it is confirmed that Ag has diffused in trace amounts.

[0163] Since the molten metal is an alloy of Cu and Ag, the channel region is divided into a Cu-rich phase and an Ag-rich phase through phase separation of the molten metal alloy. In the Cu-rich phase, the dissolution of Mn and Ni from the precursor alloy occurs relatively actively, while in the Ag-rich phase, the dissolution of metals from the precursor alloy occurs relatively low. The proportion of Mn in the resulting multi-component alloy appears relatively low, which is the result of Mn rapidly migrating to the bulk region of the molten metal outside the channel region due to its high dissolution and diffusion capabilities.

[0165] Preparation Example 5: Preparation of a heterostructured multi-component alloy using a CoCrFeNiMo precursor alloy

[0166] Weigh Co, Cr, Fe, Ni, and Mo, and melt them in a crucible. Through casting, Co 17.5 Cr 12.5 Fe 55 Ni 10 A precursor alloy of Mo5 is prepared. Afterwards, homogenization heat treatment is performed at 1,200°C for 6 hours, and after cold rolling, annealing is performed at 900°C for 1 hour.

[0167] Specimens of the annealed precursor alloy are placed into a Cu molten metal at 1,200°C, and LMD processes are carried out for 15 minutes, 30 minutes, 45 minutes, and 60 minutes, respectively. After the LMD process is performed for the set time, the alloy is separated from the molten metal and formed into a multi-component alloy through cooling.

[0169] FIG. 22 is a graph showing the thickness of the reaction layer according to the dealloying time of the specimen of Manufacturing Example 5 of the present invention.

[0170] Referring to Fig. 22, the dealosite thickness increases as the LMD process progresses. The dealosite thickness refers to the distance between the surface of the precursor alloy and the region where the molten metal channel is formed. Rather than a linear increase in dealosite thickness, the thickness of the dealosite layer shows a tendency to saturate to some extent with increasing time.

[0171] The specimen of Manufacturing Example 5 above has a different composition of precursor alloy compared to the prior manufacturing examples, and in particular, the precursor alloy is substituted with Mo instead of Mn. As Mo is substituted for Mn, which has a relatively low mixing enthalpy, dealloying may proceed in a different manner.

[0172] Figure 23 is an SEM image of the specimen of Preparation Example 5 of the present invention.

[0173] Referring to FIG. 23, the multicomponent alloy undergoing dealloying and self-assembly for 60 minutes forms channel regions that fill the spaces between ligaments. In FIG. 24, the bright areas represent ligaments, and the dark areas represent channel regions. The channel regions appear in a matrix form, while the ligaments appear spaced apart and dispersed within the matrix. However, subsequent analysis confirms that the ligaments have elongated nanorod or needle-like structures. Additionally, the channel regions appear to fill adjacent ligaments.

[0174] At the surface of the formed multicomponent alloy, the density of ligaments is high, and the ligaments have a point shape or a short column shape. On the other hand, as one moves toward the center of the multicomponent alloy, the ligaments appear in a needle-like shape with long lengths.

[0175] FIG. 24 are enlarged images of the specimen of FIG. 23 of the present invention.

[0176] Referring to FIG. 24, image (a) is an enlarged view of a in FIG. 23 showing the surface area of ​​the multi-component alloy. Image (b) is an enlarged view of b in FIG. 23 showing the center area of ​​the multi-component alloy.

[0177] In image (a), needle-shaped ligaments are visible, along with numerous short, column-shaped ligaments that are not fully developed. Additionally, dot-shaped ligaments are visible. On the other hand, in image (b), it is confirmed that the needle-shaped ligaments have grown further and the density of the ligaments is low.

[0178] In the images above, the bright areas show a ligament structure in which a Mo-rich phase with Mo as the main component is formed, and the dark areas show a channel structure in which a Cu-rich region rich in Cu is formed.

[0179] FIG. 25 is an image for analyzing the ligament in a portion of FIG. 24 for the specimen of Manufacturing Example 5 of the present invention, and a graph showing the composition of constituent metal elements according to specific positions.

[0180] Referring to FIG. 25, image (a) indicates the locations where four ligaments were selected from image (a) of FIG. 24 and EDX analysis was performed. Locations 1 and 2 are columnar or dot-shaped ligaments with short lengths, and locations 3 and 4 are needle-shaped ligaments with long lengths. That is, in a multi-component alloy, the constituent metal elements are analyzed according to the type of ligament in the surface area.

[0181] Graph (b) shows the composition of each selected ligament. A very high Mo content is observed in the short columnar ligaments. On the other hand, the Fe and Co content is significantly reduced. Conversely, in the needle-shaped ligaments at positions 3 and 4, a relatively small amount of Mo is observed, and relatively high amounts of Fe and Co are observed. This is shown in Table 3 below.

[0182] constituent elements Ingredient content at.% by ligament position 1 2 3 4 Cr 3.43 3.05 5.94 7.21 Fe 6.27 7.86 33.1 32.5 Co 1.25 2.37 13.7 13.2 Mo 70.9 71.8 38.8 36.6 Ni 0.16 0.49 0.73 0.24 Cu 18 14.4 7.73 10.2

[0183] In Table 3 above, very high Mo content and relatively high Cu content are observed in short columnar or dot-shaped ligaments. That is, in short columnar ligaments, the leaching of Mo occurs relatively very little, and the diffusion of Cu occurs significantly. In addition, structures formed as leaching of Co and others occurs actively.

[0184] On the other hand, in the needle-shaped ligament, the amount of Mo decreases relatively significantly, and the amount of Cu also decreases. Conversely, the amount of Co shows a relatively increasing trend. In particular, the amount of Fe increases relatively significantly.

[0185] When looking at the above Fig. 25, in the multi-component alloy undergoing dealloying, a number of short columnar ligaments appear in the surface region, and needle-shaped ligaments occupy the majority as you go further in.

[0186] In other words, the short columnar ligaments formed in the surface region are dominated by a Mo-rich phase, which is a result of the initial reaction. That is, in the initial reaction, the leaching of Mo does not occur actively, but the leaching of Fe occurs, and along with the leaching of Fe, the inflow of Cu due to diffusion is predicted.

[0187] On the other hand, the needle-shaped ligaments appearing towards the center are predicted to be the result of the recomposition of residual metal elements following the leaching of Mo by continuously supplied thermal energy.

[0188] That is, in the multi-component alloy of Manufacturing Example 5, the pattern of dealloying varies depending on the location, and selective retention and rearrangement of metal elements occur.

[0189] FIG. 26 is an image showing the position of a selected ligament to investigate the content of the constituent metal in image (b) of FIG. 24 for the specimen of Manufacturing Example 5 of the present invention.

[0190] Referring to FIG. 26, the composition of metal elements at various locations in the central part of the self-assembled alloy is analyzed via EDX, corresponding to the disclosed image (b) of FIG. 24.

[0191] The content of the constituent metal elements by position is summarized in Table 4 below.

[0192] Bed-type ligament Channel area Dot-shaped or short columnar ligands 1 2 3 4 5 6 7 8 9 Cr 9.23 6.28 7.45 0.37 0.3 0.28 5.94 9.8 8.59 Fe 36.61 28.07 36.07 3.06 2.38 2.07 18.49 36.4 35.31 Co 14.09 11.07 13.85 1.22 0.72 0.69 6.48 12.6 12.83 Ni 0.39 0.34 0.6 0.46 0.15 0.25 0.33 0.47 0.18 Cu 3.48 23.54 6.95 94.82 96.32 96.58 52.61 7.63 8.52 Mo 36.2 30.71 35.07 0.07 0.13 0.13 16.14 33.1 34.58

[0193] Referring to Table 4, three main types of regions appear.

[0194] First, it corresponds to positions 1 through 3 as an acicular ligament. In the acicular ligament, Fe, Co, and Cr have relatively high content, and Mo also appears at a high level. However, Cu is included in small amounts.

[0195] The above structure is formed after dealolysis, with Mo and other metallic elements remaining.

[0196] Locations 4 through 6 are channel regions that are relatively rich in Cu. In these channel regions, Cu appears in very high proportions, while the content of other metal elements appears low. That is, since Cu forms the molten metal, it is confirmed that the Cu constituting the molten metal penetrates into the alloy structure to form the main component of the channel regions, and other metal elements are leached out in trace amounts.

[0197] Positions 6 through 9 are measurements of point-shaped or column-shaped ligaments; however, in the case of position 6, it is difficult to confirm meaningful data as it corresponds to the boundary surface between the round ligament and the channel area.

[0198] In the point form, it exhibits a composition ratio similar to that of needle-shaped ligaments. However, since the shape appears closer to a sphere, this is considered to be the result of the re-aggregation of the alloy during the stabilization of the interface and the formation of the Cu-rich phase.

[0199] In addition, regardless of shape, it is confirmed that the ligaments have a composition ratio of similar component metals among themselves, and the ligaments are formed as a Mo-rich phase, while the channel regions are formed as a Cu-rich phase.

[0200] FIG. 27 are images of the Cu-rich channel region removed from the specimen of Manufacturing Example 5 of the present invention.

[0201] Referring to FIG. 27, image (a) is an upper image showing the Cu-rich channel region being selectively etched and the remaining ligaments. The remaining ligaments have a needle-like shape and are Mo-rich regions. Additionally, voids or gaps appear between the ligaments.

[0202] Images (b) and (c) are images observed by cutting the specimen shown in image (a) in a lateral direction. Long, longitudinally formed ligaments are shown and form a network. Additionally, they extend into the interior of the alloy.

[0203] That is, by removing the channel region through selective etching, a Mo-rich needle-shaped ligament structure can be obtained, and said structure has a very large specific surface area and chemical stability.

[0205] In the present invention described above, ligaments can be formed through dealloying, and channels can be formed to fill the regions between the ligaments. The molten metal can be formed from Cu or an alloy of Cu, and the channels have a new alloy phase rich in Cu. Through this, at least two types of alloy forms appear, and high conductivity and excellent wear resistance are ensured.

[0206] In addition, if the Cu-rich region forming the channel is selectively etched, needle- or nanorod-shaped alloys appear. The structure of the alloy has a high specific surface area and can possess excellent chemical stability due to the alloy's unique composition. Explanation of the symbols delete

Claims

Claim 1 Co: 17.5 at.% to 20 at.%, Cr: 12.5 at.% to 20 at.%, Fe: 20.0 at.% to 55.0 at.%, Mn: 0 at.% to 20 at.%, Ni: 10 at.% to 20 at.%, and Cu which is a molten metal 100-x Ag x (x contains Cu or Ag introduced from 0 at.% to 60 at.%) and other unavoidable impurities, and said Co, Cr, Fe, Mn, Ni, Cu 100-x Ag x A multicomponent alloy in which the sum of the at.% of Cu or Ag introduced from and other unavoidable impurities is 100 at.%, and which includes ligaments, which are interconnected solid framework structures, and channel regions of a Cu-rich phase that fill the regions between the ligaments. Claim 2 A multi-component alloy according to claim 1, characterized in that the ligament is composed of residual metal elements in which Mn or Ni is dissolved into the molten metal. Claim 3 A multi-component alloy according to claim 2, characterized in that the channel region undergoes alloying through self-assembly by the eluted Mn or Ni and has a face-centered cubic crystal structure. Claim 4 A multi-component alloy characterized in that, in paragraph 3, the channel region is a Cu-rich phase. Claim 5 A multi-component alloy according to claim 1, wherein when the molten metal is Cu alone, the channel region has a Cu-rich face-centered cubic structure and has a composition different from the ligament due to the preferential dissolution of Mn and Ni. Claim 6 A multi-component alloy according to claim 5, wherein when the molten metal is an alloy of CuAg, the channel region has a face-centered cubic structure of a Cu-rich phase and an Ag-rich phase by phase separation, and the phase-separated face-centered cubic structures have a composition different from the ligament. Claim 7 A multi-component alloy according to claim 1, characterized in that Cu diffuses into the ligament and the ligament has a face-centered cubic structure. Claim 8 A multi-component alloy according to claim 1, characterized in that the channel region fills the region between the ligaments and has an interconnected network shape. Claim 9 A multi-component alloy according to claim 1, characterized in that the multi-component alloy has twin boundaries in a grain boundary map. Claim 10 A step of preparing a CoCrFeNiMn precursor alloy in which the ratio of constituent metal elements is uniformly 20 at.% each; and preparing the said precursor alloy as Cu 100-x Ag x A method for manufacturing a multi-component alloy comprising: a step of immersing in a molten metal (where x is 0 at.% to 60 at.%); and a step of forming a channel region that fills the region between the ligaments through self-organization and a ligament having residual components of the precursor alloy through dealolysis by immersion in the molten metal. Claim 11 A method for manufacturing a multi-component alloy according to claim 10, wherein the molten metal contains Cu. Claim 12 A method for manufacturing a multi-component alloy according to claim 11, wherein the dealolysis is characterized by dissolving Mn or Ni of the precursor alloy into the molten metal and forming a Cu-rich channel region that fills the region between the ligaments formed by the dissolution to complete the self-organization. Claim 13 A method for manufacturing a multi-component alloy according to claim 12, characterized in that, during the dealloying and self-organization process, Cu of the molten metal diffuses into the ligament. Claim 14 A method for manufacturing a multi-component alloy according to claim 10, wherein the molten metal comprises an alloy of CuAg. Claim 15 A method for manufacturing a multi-component alloy according to claim 14, wherein the channel region has a face-centered cubic structure of a Cu-rich phase and an Ag-rich phase by phase separation, and the phase-separated face-centered cubic structures have a composition different from that of the ligament. Claim 16 A multicomponent alloy comprising Co: 17.5 at.% to 20 at.%, Cr: 12.5 at.% to 20 at.%, Fe: 20.0 at.% to 55.0 at.%, Mo: 0 at.% to 5 at.%, Ni: 10 at.% to 20 at.%, Cu and other unavoidable impurities introduced from the molten metal Cu, wherein the sum of the at.% of Co, Cr, Fe, Mo, Ni, Cu and other unavoidable impurities is 100 at.%, and comprising a ligament, which is a solid framework structure connected to one another, and a channel region that fills the region between the ligaments and is a Cu-rich phase. Claim 17 A multi-component alloy according to claim 16, wherein the above ligaments have a point shape, a short-length column shape, or a needle shape, and the point shape or column shape occupies the majority in the region adjacent to the surface of the multi-component alloy. Claim 18 In claim 17, the multi-component alloy is characterized in that the ligands occupy a majority of the central region of the multi-component alloy. Claim 19 A multi-component alloy according to claim 16, characterized in that the ligament has a Mo-rich phase, the channel region has a matrix form between the ligaments, and has a Cu-rich phase. Claim 20 Co 17.5 Cr 12.5 Fe 55 Ni 10 A method for manufacturing a multi-component alloy comprising: a step of preparing a precursor alloy of Mo5; a step of immersing the precursor alloy in a molten Cu; a step of forming a ligament having residual components of the precursor alloy through dealloying by immersion in the molten Cu and a step of forming a channel region that fills the region between the ligaments through self-organization; and a step of selectively removing the channel region to leave the ligament having a needle-like shape.

Citation Information

Patent Citations

  • High entropy alloy having complex microstructure and method for manufacturing the same

    KR101744102B1

  • METHOD FOR MANUFACTURING METALLIC COMPOSITE MATERIAL THROUGH LIQUID METAL DEALLOYING TECHNIQUE USING Mg-Ca ALLOY MOLTEN METAL AND Ti-BASED PRECURSOR ALLOY AND METALLIC COMPOSITE MATERIAL MANUFACTURED THEREBY

    KR1020240157397A