Light guide plate for image display

The laminate structure with a silicon oxynitride barrier layer in the light guide plate addresses hologram layer degradation by preventing moisture penetration, ensuring effective moisture barrier and maintaining optical properties in challenging environments.

KR103046629B1Active Publication Date: 2026-11-10MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020247043564
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-25
Filing Date
2021-09-28
Publication Date
2026-11-10
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Existing light guide plates for image display, particularly in VR and AR technologies, suffer from hologram layer degradation due to moisture absorption and corrosion in high-temperature and high-humidity environments, despite the use of aqueous polymer protective barriers.

Method used

A light guide plate design featuring a laminate structure with a resin substrate, an anchor coat layer, and a barrier layer, where the barrier layer is composed mainly of silicon oxynitride with a specific nitrogen element composition, and the total thickness of the anchor coat and barrier layers is limited, along with a hologram layer, to prevent moisture penetration and maintain optical properties.

Benefits of technology

The design effectively suppresses hologram layer degradation and maintains good optical properties, including low water vapor transmittance, high total light transmittance, and minimal haze, enhancing the longevity and performance of the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024146511334-PAT00014_ABST
    Figure 112024146511334-PAT00014_ABST
Patent Text Reader

Abstract

A light guide plate for image display having a first laminate (11) having a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order, and a hologram layer (4), wherein the first barrier layer (3) has silicon oxynitride as the main component and the nitrogen element composition in the first barrier layer (3) obtained by X-ray photoelectric molecular optics (XPS) is greater than 0 atm% and less than or equal to 25 atm%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a light guide plate for displaying images.

[0002] The present application claims priority based on Japanese patent applications No. 2020-162090 and No. 2020-162484 filed in Japan on September 28, 2020; Japanese patent application No. 2020-163145 filed in Japan on September 29, 2020; Japanese patent applications No. 2020-213349 and No. 2020-213350 filed in Japan on December 23, 2020; and Japanese patent application No. 2021-028831 filed in Japan on February 25, 2021, and incorporates the contents thereof herein. Background Technology

[0003] In display devices, a light guide plate for image display is sometimes used. For example, in a display device using VR (Virtual Reality) technology or AR (Augmented Reality) technology, a light guide plate for image display is used in which a holographic layer is supported on a transparent substrate. A hologram having various optical functions, such as wave guidance, reflection, and diffraction, is formed on the holographic layer.

[0004] The materials used for forming holographic layers often include photosensitive compositions containing radical polymerizable monomers, polyvalent acids, or bases such as amines, which can cause the resin substrate to deteriorate. It is also known that holographic materials deteriorate due to moisture absorption. For this reason, display devices that support a holographic layer on a resin substrate are prone to deterioration in high-temperature and high-humidity environments.

[0005] Patent Document 1 describes forming a photosensitive material layer that forms a hologram on an optically transparent resinous gaseous phase, and coating the photosensitive material layer with an aqueous polymer protective barrier. Patent Document 1 suggests that the aqueous polymer protective barrier is formed to withstand attacks caused by moisture. Prior art literature

[0006] Japanese Patent Publication No. Hei 5-181400 The problem to be solved

[0007] However, the technology described in Patent Document 1 has the following problems.

[0008] In the technology described in Patent Document 1, a resin-based gas is adhered to the surface opposite to the aqueous polymer protective barrier in the photosensitive material layer.

[0009] For this reason, there is a risk that the photosensitive material may corrode the resin gas under high-temperature environments.

[0010] Furthermore, since the interior of the resin gas contains moisture, the moisture diffuses into the photosensitive material layer through the contact surface with the photosensitive material layer. Additionally, because the gas is exposed to the outside, moisture from the outside continuously penetrates into the gas. As a result, since moisture penetrates into the photosensitive material layer via the resin gas, even if moisture is shielded by an aqueous polymer protective barrier, it is not possible to prevent the photosensitive material layer from deteriorating over time due to moisture from the gas side.

[0011] The present invention aims to provide a light guide plate for image display capable of suppressing the degradation of a hologram layer. means of solving the problem

[0012] <1> A light guide plate for image display having a laminate comprising a resin substrate, an anchor coat layer, and a barrier layer in this order, and a hologram layer, wherein the barrier layer is composed mainly of silicon oxynitride and the nitrogen element composition in the barrier layer obtained by X-ray photoelectric molecular optics (XPS) is greater than 0 atm% and less than or equal to 25 atm%.

[0013] <2> A light guide plate for image display, comprising a laminate having a resin substrate, an anchor coat layer, and a barrier layer in this order, and a hologram layer arranged in this order, wherein the thickness of the barrier layer is 150 nm or less, the total thickness of the anchor coat layer and the barrier layer is 300 nm or less, and furthermore, the tanδ peak temperature in the viscoelasticity measurement of the anchor coat layer is 80 ℃ or less.

[0014] <3> A light guide plate for image display having a laminate comprising a resin substrate, an anchor coat layer, and a barrier layer in this order, and a hologram layer, wherein when the thickness of the anchor coat layer is A nm and the tanδ peak temperature in the viscoelasticity measurement of the anchor coat layer is B ℃, A / B is 3 or less.

[0015] <4> A light guide plate for image display having a laminate comprising a resin substrate, an anchor coat layer, and a barrier layer in this order, and a hologram layer, wherein the anchor coat layer is composed of a resin composition containing a binder resin having hydroxyl groups and an isocyanate compound, and the molar ratio of the isocyanate group (NCO) of the isocyanate compound to the hydroxyl group (OH) of the binder resin, NCO / OH, is 0.8 or higher.

[0016] <5> A light guide plate for image display having a laminate comprising a resin substrate and a protective layer, and a hologram layer arranged in this order, wherein the surface roughness Sa of the side of the protective layer in contact with the hologram layer is less than 5.5 nm.

[0017] <6> A light guide plate for image display having a resin substrate, a barrier layer, and a hologram layer arranged in this order, and a mirror gloss of 120% or more at an incident angle of 60 degrees on the side of the laminate including the resin substrate and the barrier layer that contacts the hologram layer. Effects of the invention

[0018] According to the present invention, a light guide plate for image display capable of suppressing the degradation of the hologram layer can be provided. Brief explanation of the drawing

[0019] FIG. 1 is a schematic cross-sectional view showing an example of a light guide plate for image display according to the present invention. Specific details for implementing the invention

[0020] In the present invention, when a numerical range is indicated using “∼,” the numerical values ​​on both sides of “∼” are included in the numerical range.

[0021] In the present invention, “(meth)acrylic” includes “acrylic” and “methacrylic”. For example, “poly(meth)acrylic resin” includes “polyacrylic resin” and “polymethacrylic resin”. Likewise, “(meth)acrylate” includes “acrylate” and “methacrylate”, “(meth)acryloyl” includes “acryloyl” and “methacryloyl”, and “(meth)acryloyloxy” includes “acryloyloxy” and “methacryloyloxy”.

[0022] Embodiments of the present invention will be described below. However, the present invention is not limited to the embodiments described below, and various modifications are possible as long as they do not deviate from the essence of the invention.

[0023] <<First Embodiment>>

[0024] A light guide plate for image display related to the first embodiment of the present invention has a laminate having a resin substrate, an anchor coat layer, and a barrier layer in that order, and a hologram layer, wherein the barrier layer has silicon oxynitride as its main component and the nitrogen element composition in the barrier layer obtained by X-ray photoelectric molecular optics (XPS) is greater than 0 atm% and less than or equal to 25 atm%.

[0025] The light guide plate for image display according to the present embodiment can suppress the degradation of the hologram layer and also has good optical properties by having the barrier layer having the above characteristics.

[0026] The light guide plate for image display according to the present embodiment may include at least one resin selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin.

[0027] The light guide plate for image display according to the present embodiment may include at least one resin selected from the group consisting of acrylic resin, urethane resin, and polyester resin in the anchor coat layer.

[0028] In the image display light guide plate of the present embodiment, the laminate may have a hard coat layer on both surfaces of the resin substrate.

[0029] The light guide plate for image display according to the present embodiment may have a total light transmittance of 90% or more of the laminate.

[0030] The light guide plate for image display according to the present embodiment may have a haze of less than 0.1% of the laminate.

[0031] The light guide plate for image display of the present embodiment may have a b* value of the laminate measured by a spectrophotometric colorimeter of less than 0.5.

[0032] The light guide plate for image display according to the present embodiment may have a water vapor transmittance of the laminate of less than 0.01 g / m² / day.

[0033] Hereinafter, a light guide plate for image display related to the present embodiment will be described in detail.

[0034] Light guide plate for image display

[0035] The light guide plate for image display according to the present embodiment has a laminate comprising a resin substrate, an anchor coat layer, and a barrier layer, and a hologram layer. The resin substrate, the anchor coat layer, the barrier layer, and the hologram layer are arranged in this order in the thickness direction. The laminate may be placed on at least one surface of the hologram layer, but may also be placed on both surfaces of the hologram layer. When the laminate is placed on both surfaces of the hologram layer, the laminate placed on one surface of the hologram layer is called the first laminate, and the laminate placed on the other surface of the hologram layer is called the second laminate. In this case, the hologram layer is sandwiched between the first barrier layer of the first laminate and the second barrier layer of the second laminate, and the first anchor coat layer and the first resin substrate are laminated on the other side of the first barrier layer, and the second anchor coat layer and the second resin substrate are laminated on the other side of the second barrier layer. In the present embodiment, the first laminate and the second laminate may be collectively referred to simply as "laminated laminate" below. The first resin substrate and the second resin substrate may be collectively referred to simply as "resin substrate" below. Also, the first anchor coat layer and the second anchor coat layer may be collectively referred to simply as "anchor coat layer" below. Additionally, the first barrier layer and the second barrier layer may be collectively referred to simply as "barrier layer" below.

[0036] One or more transparent layers may be disposed between the resin substrate and the anchor coat layer, between the anchor coat layer and the barrier layer, and between the barrier layer and the hologram layer. For example, a hard coat layer may be used as the transparent layer.

[0037] In addition, the anchor coat layer, barrier layer, and transparent layer may be disposed on one surface of the resin substrate, but may also be disposed on both surfaces of the resin substrate. That is, the barrier layer, anchor coat layer, resin substrate, anchor coat layer, barrier layer, and hologram layer may be arranged in this order in the thickness direction, or the barrier layer, anchor coat layer, transparent layer, resin substrate, transparent layer, anchor coat layer, barrier layer, and hologram layer may be arranged in this order in the thickness direction.

[0038] The light guide plate for displaying an image has an incident part for incidenting image light and a display part for displaying an image by the image light.

[0039] The hologram layer is disposed between the incident portion and the display portion. The hologram layer has a diffraction grating pattern formed therein for guiding image light incident from the incident portion to the display portion and emitting it from the display portion.

[0040] The diffraction grating pattern in the above-mentioned display portion transmits at least a portion of external light incident from outside the light guide plate for image display. Additionally, the external light is incident from a surface opposite to the display portion.

[0041] The image light incident on the above-mentioned incident portion is guided into the hologram layer and emitted to the outside from the display portion. Meanwhile, as external light also passes through the resin substrate and the display portion, an observer of the display portion can observe both the image light and the external light within their field of view.

[0042] The light guide plate for image display according to the present embodiment can be used in display devices using VR (virtual reality) technology or AR (augmented reality) technology, etc., and, for example, can be used in automotive displays or sports sunglasses used outdoors.

[0043] In addition, the light guide plate for image display according to the present embodiment can be used in devices such as holographic optical elements (HOE), represented by a combiner for a head-up display (HUD) for automobiles or a reflector for a reflective liquid crystal display device, in addition to for display purposes.

[0044] Hereinafter, based on the example shown in FIG. 1, the detailed configuration of an example of a light guide plate for image display according to the present embodiment will be described. FIG. 1 is a schematic cross-sectional view showing an example of a light guide plate for image display according to the present embodiment.

[0045] In the light guide plate (8) for image display shown in Fig. 1, the first resin substrate (1), the first anchor coat layer (2), the first barrier layer (3), the hologram layer (4), the second barrier layer (5), the second anchor coat layer (6), and the second resin substrate (7) are arranged in this order in the thickness direction.

[0046] The shape of the light guide plate (8) for image display as seen from a flat surface is not particularly limited. For example, the light guide plate (8) for image display may be shaped into a form that can be mounted on the display device used.

[0047] For example, the light guide plate (8) for image display may be a rectangular plate larger than the shape mounted on the display device. In this case, the light guide plate (8) for image display is formed by cutting it into a shape that can be mounted on the display device before being assembled on the display device.

[0048] The light guide plate (8) for displaying images may be flat, or, if necessary, curved.

[0049] Below, an example is described in which the light guide plate (8) for displaying images is formed as a rectangular flat plate when viewed from a flat plane.

[0050] [First laminate (11)]

[0051] The first laminate (11) comprises a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order. The light guide plate (8) for image display can suppress the deterioration of the hologram layer and also obtain good optical properties by placing the first laminate (11) on the surface of the hologram layer (4).

[0052] (Optical properties)

[0053] The total light transmittance of the first laminate (11) is not particularly limited, but is preferably 90% or more, more preferably 91% or more, and even more preferably 92% or more. If the total light transmittance of the first laminate (11) is 90% or more, the brightness value of the light guide plate (8) for image display becomes better.

[0054] Also, from the same perspective, the haze of the first laminate (11) is preferably less than 0.1%, more preferably less than 0.08%, even more preferably less than 0.06%, and even more preferably less than 0.05%.

[0055] The absolute value of b* of the first laminate (11) measured by a spectrophotometer is preferably less than 0.8, more preferably less than 0.6, and even more preferably less than 0.5. Furthermore, among these, less than 0.4 is more preferably less than 0.3, and even more preferably less than 0.1. If the absolute value of b* of the first laminate (11) is less than 0.8, the brightness value and clarity of the light guide plate (8) for image display become better.

[0056] (Barrier)

[0057] The water vapor permeability of the first laminate (11) is preferably less than 0.01 g / m² / day, more preferably less than 0.008 g / m² / day, even more preferably less than 0.006 g / m² / day, and more preferably less than 0.004 g / m² / day. If the water vapor permeability of the first laminate (11) is less than 0.01 g / m² / day, the deterioration of the hologram layer (4) can be further suppressed.

[0058] [First resin entry (1)]

[0059] The first resin substrate (1) is placed at the outermost part in the thickness direction of the light guide plate (8) for image display. The first resin substrate (1) is placed on the surface of the light guide plate (8) for image display on the side of the image output.

[0060] The first resin substrate (1) has the same shape as the external shape of the light guide plate (8) for image display.

[0061] The first resin substrate (1) transmits image light emitted from the hologram layer (4) and external light that passes through the second resin substrate (7) and the hologram layer (4) described later.

[0062] The thickness of the first resin substrate (1) is not particularly limited, but is preferably 0.05 to 10 mm.

[0063] The lower limit of the thickness of the first resin substrate (1) is not particularly limited, but from the perspective of making scratch resistance good, it is preferable to have a thickness of 0.1 mm or more, and more preferable to have a thickness of 0.2 mm or more.

[0064] Also, the upper limit of the thickness of the first resin substrate (1) is not particularly limited, but from the viewpoint of improving moldability and light transmittance, it is preferable that it be 5 mm or less, more preferable that it be 3 mm or less, and even more preferable that it be 2 mm or less.

[0065] In addition, the thickness of the first resin substrate (1) in this specification can be measured using a dial gauge type or a micrometer using a stylus.

[0066] The total light transmittance of the first resin substrate (1) is not particularly limited, but is preferably 80% or more, and more preferably 90% or more. If the total light transmittance of the first resin substrate (1) is 80% or more, the brightness value of the light guide plate (8) for image display becomes better.

[0067] The first resin substrate (1) preferably includes a thermoplastic resin in order to improve optical properties, impact resistance, scratch resistance and moldability.

[0068] The above thermoplastic resins include, for example, polyolefin resins such as homopolymers or copolymers of alkenes such as ethylene, propylene, and butene; amorphous polyolefin resins such as cyclic polyolefin resins; polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN); cellulose resins such as triacetylcellulose, diacetylcellulose, and cellophane; polyamide resins such as nylon 6, nylon 66, nylon 12, and copolymer nylon; ethylene-vinyl acetate copolymer partial hydrolysate (EVOH); polyimide resins; polyetherimide resins; polysulfone resins; polyethersulfone resins; polyetheretherketone resins; polycarbonate resins; polyvinyl butyral resins; polyarylate resins; fluorine resins; poly(meth)acrylic resins; styrene resins such as polystyrene. Examples of organic materials include polyvinyl alcohol, ethylene vinyl alcohol copolymer, polyvinyl chloride, cellulose, acetylcellulose, polyvinylidene chloride, polyphenylene sulfide, polyurethane, phenolic resin, epoxy resin, polynorbornene, styrene-isobutylene-styrene block copolymer (SIBS), allyl diglyglycol carbonate, and biodegradable resin. These thermoplastic resins may be used as a single type or in combination of two or more types. Additionally, the first resin substrate (1) may be composed of a laminated layer made of two or more materials selected from the group consisting of the above thermoplastic resins.

[0069] In this embodiment, from the perspective of transparency, at least one type selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin is preferred.

[0070] Among these, poly(meth)acrylic resins are preferred due to their excellent scratch resistance and moldability.

[0071] (Poly(meth)acrylic resin)

[0072] As monomers constituting the above poly(meth)acrylic resin, for example, methyl methacrylate, methacrylic acid, acrylic acid, benzyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, Examples include dicyclofentanyl (meth)acrylate, dicyclofentenyloxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, acrylate (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, pentamethylpiperidyl (meth)acrylate, tetramethylpiperidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate. These monomers may be used by polymerizing them alone, or by polymerizing two or more types.

[0073] In addition, other monomers capable of copolymerizing with the monomers constituting the poly(meth)acrylic resin may be added. The other monomers may be monofunctional monomers, i.e., compounds having one polymerizable carbon-carbon double bond in the molecule, or polyfunctional monomers, i.e. compounds having at least two polymerizable carbon-carbon double bonds in the molecule.

[0074] Examples of the above monofunctional monomers include aromatic alkenyl compounds such as styrene, α-methylstyrene, and vinyltoluene, alkenyl cyanide compounds such as acrylonitrile and methacrylonitrile, acrylic acid, methacrylic acid, maleic anhydride, and N-substituted maleimide.

[0075] In addition, the above-mentioned polyfunctional monomers may include, for example, polyunsaturated carboxylic acid esters of polyhydric alcohols such as ethylene glycol dimethacrylate, butanediol dimethacrylate, and trimethylolpropane triacrylate; alkenyl esters of unsaturated carboxylic acids such as allyl acrylate, allyl methacrylate, and allyl cinnamate; polyalkenyl esters of polybasic acids such as diallyl phthalate, diallyl maleate, trialyl cyanurate, and trialyl isocyanurate; and aromatic polyalkenyl compounds such as divinylbenzene.

[0076] The above monofunctional monomer and the above polyfunctional monomer may be used as a single type or in combination of two or more types.

[0077] The above poly(meth)acrylic resin can be manufactured by polymerizing the aforementioned monomer components using known methods such as suspension polymerization, emulsion polymerization, or bulk polymerization.

[0078] [First Anchor Coat Layer (2)]

[0079] The first anchor coat layer (2) is placed between the first resin substrate (1) and the first barrier layer (3).

[0080] By forming the first anchor coat layer (2), the adhesion between the first resin substrate (1) and the first barrier layer (3) is improved, and the barrier properties are improved.

[0081] The first anchor coat layer (2) also serves to relieve residual stress that occurs when the first barrier layer (3), described later, is formed by dry film formation. Furthermore, it can suppress deformation of the first barrier layer (3) in a humid heat environment (e.g., 40°C, 90%RH) to prevent the rise of haze in the light guide plate (8) for image display.

[0082] In order to sufficiently relieve residual stress of the first barrier layer (3), the thickness of the first anchor coat layer (2) is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more.

[0083] Meanwhile, in order to prevent the first barrier layer (3) from being excessively deformed by residual stress, the thickness of the first anchor coat layer (2) is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.

[0084] In addition, in order to sufficiently relieve the residual stress of the first barrier layer (3) so that the first barrier layer (3) is not excessively deformed by the residual stress, the thickness of the first anchor coat layer (2) is preferably 1 to 200 nm, more preferably 3 to 150 nm, and even more preferably 5 to 100 nm.

[0085] In addition, the thickness of the first anchor coat layer (2) can be measured by observing the cross-section of the light guide plate (8) for image display via TEM.

[0086] When the first resin substrate (1) is formed from a highly hygroscopic resin such as a poly(meth)acrylic resin, the first resin substrate (1) may expand under a moist heat environment. In order to accommodate the expansion of the first resin substrate (1) under a moist heat environment, the tanδ peak temperature in the measurement of the viscoelasticity of the first anchor coat layer (2) is preferably 80°C or lower, and more preferably 75°C or lower.

[0087] Meanwhile, in order to prevent the first anchor coat layer (2) from being excessively deformed due to residual stress of the first barrier layer (3), the tanδ peak temperature in the viscoelasticity measurement of the first anchor coat layer (2) is preferably 10°C or higher, more preferably 15°C or higher, and even more preferably 20°C or higher.

[0088] In addition, in order to allow the first anchor coat layer (2) to follow the expansion of the first resin substrate (1) under a moist heat environment, so that the first anchor coat layer (2) is not excessively deformed by the residual stress of the first barrier layer (3), the tanδ peak temperature in the measurement of the viscoelasticity of the first anchor coat layer (2) is preferably 10 to 80 ℃, more preferably 15 to 80 ℃, and even more preferably 20 to 75 ℃.

[0089] In addition, in the present specification, the tanδ peak temperature is the peak temperature of the loss tangent (tanδ) when a sheet with a thickness of 200 μm is manufactured from the first anchor coat layer (2), and viscoelasticity is measured using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) under conditions of a frequency of 1 Hz, a heating rate of 3 ℃ / min, and a measurement temperature of -50 to 200 ℃.

[0090] The total light transmittance of the first anchor coat layer (2) is not particularly limited, but is preferably 80% or more, and more preferably 90% or more. If the total light transmittance of the first anchor coat layer (2) is 80% or more, the brightness value of the light guide plate (8) for image display becomes good.

[0091] Also, when the average refractive index of the first resin substrate (1) and the first barrier layer (3) is n1, the refractive index n2 of the first anchor coat layer (2) is preferably within the range of n1 ± 0.20, more preferably within the range of n1 ± 0.15, and even more preferably within the range of n1 ± 0.10. If the refractive index n2 of the first anchor coat layer (2) is within the range of n1 ± 0.20, the brightness value of the light guide plate (8) for image display becomes good, and color non-uniformity can be prevented.

[0092] In addition, the refractive index is the refractive index measured by an Abbe refractometer (NAR-4T, manufactured by Atago).

[0093] The material of the first anchor coat layer (2) is not particularly limited, but, for example, may be a thermoplastic resin or a curable resin.

[0094] Examples of thermoplastic resins include fluorine resins, polyethersulfone resins, polycarbonate resins, acrylic resins, silicone resins, cycloolefin resins, thermoplastic polyimide resins, polyamide resins, polyamideimide resins, polyarylate resins, polysulfone resins, polyetherimide resins, polyetheretherketone resins, polyethersilicone resins, polyester resins, and polyphenylenesulfide resins.

[0095] Examples of curable resins include acrylic resins, urethane resins, epoxy resins, and silicone resins.

[0096] Among them, acrylic resin or polyester resin as a thermoplastic resin is preferred from the perspective of water vapor barrier properties.

[0097] In the resin composition constituting the first anchor coat layer (2), a silane coupling agent, a sensitizer, a crosslinking agent, a UV absorber, a polymerization inhibitor, a surfactant, a filler, a release agent, and a thermoplastic resin other than those listed above may be added. These additives may be used as a single type or in combination of two or more types.

[0098] Among these, the first anchor coat layer (2) preferably includes a crosslinking agent. Examples of crosslinking agents include isocyanate-based crosslinking agents, peroxide-based crosslinking agents, epoxy-based crosslinking agents, and imine-based crosslinking agents, and isocyanate-based crosslinking agents are preferred. The content of the crosslinking agent is preferably 0 to 20 parts by mass and more preferably 5 to 15 parts by mass per 100 parts by mass of the thermoplastic resin or the curable resin.

[0099] As a method for forming the first anchor coat layer (2), for example, a resin composition for forming the first anchor coat layer (2) can be applied to the first resin substrate (1), and a first barrier layer (3) can be laminated thereon, and the laminate can be formed by processing the laminate using a press, nip roll, thermal lamination, etc. If the first anchor coat layer (2) is made of a curable resin, a curing process may be included when forming the first anchor coat layer (2).

[0100] [First barrier layer (3)]

[0101] The first barrier layer (3) is placed between the first anchor coat layer (2) and the hologram layer (4) described later.

[0102] The first barrier layer (3) prevents gases such as water vapor and oxygen from penetrating from the outside of the light guide plate (8) for image display and the first resin substrate (1) from penetrating into the hologram layer (4) and causing deterioration.

[0103] Therefore, the oxygen permeability and water vapor permeability of the first barrier layer (3) are more desirable the smaller they are.

[0104] The oxygen permeability of the first barrier layer (3) is preferably 1 cm³ / m² / day / atm or less.

[0105] Also, the water vapor permeability of the first barrier layer (3) is preferably 1 g / m² / day or less, more preferably 0.5 g / m² / day or less, and even more preferably 0.1 g / m² / day or less.

[0106] Here, oxygen permeability is the oxygen permeability measured using an oxygen permeability measuring device (OX-TRAN 2 / 21, manufactured by MOCON). Also, water vapor permeability is the water vapor permeability measured using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox).

[0107] The first barrier layer (3) is composed mainly of silicon oxynitride. Here, "main component of the first barrier layer (3)" refers to a component that accounts for 50 mass% or more of the total components constituting the first barrier layer (3). The proportion of silicon oxynitride in the first barrier layer (3) is not particularly limited as long as it is 50 mass% or more with respect to the total mass of the first barrier layer, but 60 mass% or more is preferred, 70 mass% or more is more preferred, and 80 mass% or more is even more preferred.

[0108] The nitrogen element composition in the first barrier layer (3), obtained by X-ray Photoelectron Spectroscopy (XPS), is greater than 0 atm% and less than or equal to 25 atm%, preferably greater than or equal to 2 atm% and less than or equal to 23 atm%, more preferably greater than or equal to 5 atm% and less than or equal to 20 atm%, and even more preferably greater than or equal to 10 atm% and less than or equal to 17 atm%. If the nitrogen element composition is within the above range, the transparency of the first barrier layer (3) is increased, so the optical properties of the light guide plate (8) for image display are improved.

[0109] When the first barrier layer (3) is formed by dry film formation, residual stress may occur in the direction of curling the first barrier layer (3) outward. In order to prevent this residual stress from becoming excessive, the thickness of the first barrier layer (3) is preferably 150 nm or less, and more preferably 130 nm or less.

[0110] Meanwhile, from the perspective of improving barrier properties, the thickness of the first barrier layer (3) is preferably 5 nm or more, and more preferably 10 nm or more.

[0111] Also, in order to prevent deformation caused by residual stress of the first barrier layer (3), the total thickness of the first anchor coat layer (2) and the first barrier layer (3) is preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less.

[0112] Meanwhile, in order to sufficiently relieve the above residual stress with the first anchor coat layer (2) and to ensure good barrier properties by the first barrier layer (3), the total thickness of the first anchor coat layer (2) and the first barrier layer (3) is preferably 30 nm or more, and more preferably 50 nm or more.

[0113] It is preferable that the first barrier layer (3) has a higher refractive index than the first resin substrate (1). For example, when an acrylic resin is used as the first resin substrate (1), the refractive index of the first barrier layer (3) is preferably 1.48 or higher, and more preferably 1.48 or higher and 3.0 or lower. If the first barrier layer (3) has a higher refractive index than the first resin substrate (1), light passing through the first barrier layer (3) and through the first resin substrate (1) is incident from the optically dense first barrier layer (3) to the optically sparse first resin substrate (1), and the angle of emission of light from the first barrier layer (3) toward the first resin substrate (1) increases according to the difference in refractive index between the first barrier layer (3) and the first resin substrate (1). Thus, the Field of View (FOV) of the light guide plate for image display can be widened.

[0114] The first barrier layer (3) can be formed by conventionally known film formation methods, such as vacuum deposition, sputtering, ion plating, or plasma CVD. Among these, sputtering is preferred as the film formation method in order to obtain good barrier properties and improve the clarity of the light guide plate (8) for image display.

[0115] In order to improve the adhesion between the first anchor coat layer (2) and the first barrier layer (3), surface treatments such as corona discharge treatment or low-temperature plasma treatment may be performed on the surface of the first anchor coat layer (2), a silane coupling agent may be applied, or a mixture of saturated polyester and isocyanate may be applied.

[0116] When forming the first barrier layer (3), for example, by vacuum deposition, silicon, silicon monoxide, silicon dioxide, silicon oxynitride, or a mixture thereof is used as the evaporation material, 1.0 × 10-3 ~ 2.0 × 10 -1 Under a vacuum of Pa, heat and evaporate using an electron beam, resistance heating, or high-frequency heating method.

[0117] In addition, as a film deposition method, a reaction deposition method carried out while supplying oxygen gas or nitrogen gas can also be employed.

[0118] In addition, when forming a film by the sputtering method, for example, silicon, silicon monoxide, silicon dioxide, silicon oxynitride, or a mixture thereof is used as a target, 1.0 × 10 -2 ~ 5.0 × 10 -1 Under a vacuum of Pa, the tabernacle can be consecrated.

[0119] In addition, as the sputtering method mentioned above, a reactive sputtering method carried out while supplying oxygen gas, nitrogen gas, or argon gas may also be employed.

[0120] The nitrogen element composition in the first barrier layer (3) can be adjusted by the nitrogen flow rate, power, and film pressure during film formation.

[0121] In particular, to make the nitrogen element composition greater than 0 atm% and less than or equal to 25 atm%, the ratio of oxygen flow rate O2 [sccm] to nitrogen flow rate N2 [sccm], O2 / N2, is preferably 0.10 to 1.5, more preferably 0.12 to 1.0, and even more preferably 0.15 or higher.

[0122] Also, the power is preferably 1000 to 2000 W. Since O2 / N2 and power influence each other, when O2 / N2 is 0.10 or higher and less than 0.15, it is preferable to set the power to 1000 W or higher and less than 1500 W, and when O2 / N2 is 0.15 or higher and less than 1.5, it is preferable to set the power to 1500 W or higher and less than 2000 W.

[0123] Also, the pressure of the tabernacle is 1.0 × 10⁻⁶ -2 ~ 2.0 × 10-1 Pa is desirable, and 5.0 × 10 -2 ~ 1.5 × 10 -1 Pa is desirable.

[0124] The silicon oxynitride forming the first barrier layer (3) may contain 10 mass% or less of calcium, magnesium, or their oxides as impurities.

[0125] In addition, the first barrier layer (3) may include an inorganic material in addition to the silicon oxynitride. Examples of the inorganic material include silicon oxide, diamond-like carbon (DLC), and aluminum oxide.

[0126] [Hologram layer (4)]

[0127] The hologram layer (4) is placed on the surface opposite to the surface of the first barrier layer (3) to which the first anchor coat layer (2) is in close contact. A diffraction grating corresponding to the function that the light guide plate (8) for image display must have is appropriately formed on the hologram layer (4).

[0128] The material of the hologram layer (4) is not particularly limited and any known resin material for forming holograms can be used.

[0129] For the material of the hologram layer (4), for example, a hologram recording material comprising a thermosetting resin having at least one solvent-soluble cation-polymerizable ethylene oxide ring among its structural units and a radical-polymerizable ethylene monomer (see Japanese Patent Publication No. Hei 9-62169, Japanese Patent Publication No. Hei 11-161141 and Japanese Patent Publication No. 2002-310932).

[0130] Specifically, the hologram layer (4) is preferably formed from a photosensitive material comprising an epoxy resin such as bisphenol-based epoxy resin, a (meth)acrylate such as triethylene glycol diacrylate, a photopolymerization initiator such as 4,4'-bis(tert-butylphenyl)iodonium hexafluorophosphate, a wavelength sensitizer such as 3,3'-carbonylbis(7-diethylamino)coumarin, and an organic solvent such as 2-butanone.

[0131] [Second laminate (12)]

[0132] The second laminate (12) comprises a second barrier layer (5), a second anchor coat layer (6), and a second resin substrate (7) in this order. The various physical properties of the second laminate (12) may be different from those of the first laminate (11).

[0133] [Second barrier layer (5)]

[0134] The second barrier layer (5) is laminated on the opposite side of the first barrier layer (3) via a hologram layer (4). The second barrier layer (5) uses the same configuration as exemplified in the description of the first barrier layer (3). However, the thickness and material of the second barrier layer (5) may be different from those of the first barrier layer (3).

[0135] [Second Anchor Coat Layer (6)]

[0136] The second anchor coat layer (6) is disposed between the second barrier layer (5) and the second resin substrate (7). The second anchor coat layer (6) uses the same configuration as exemplified in the description of the first anchor coat layer (2). However, the thickness and material of the second anchor coat layer (6) may be different from those of the first anchor coat layer (2).

[0137] [2nd Substantiation (7)]

[0138] The second resin substrate (7) is laminated on the surface of the second barrier layer (5). The second resin substrate (7) uses the same configuration as exemplified in the description of the first resin substrate (1). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image emission side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0139] [Light guide plate for image display (8)]

[0140] In the image display light guide plate (8), a first anchor coat layer (2) and a first barrier layer (3), and a second barrier layer (5) and a second anchor coat layer (6) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0141] Gas from the outside of the light guide plate (8) for image display passes through the first resin substrate (1) and the second resin substrate (7) to some extent, or accumulates inside. At this time, moisture is particularly likely to accumulate in the first resin substrate (1) and the second resin substrate (7).

[0142] However, according to the configuration of the present embodiment, moisture that has penetrated from the outside into the first resin substrate (1) and the second resin substrate (7) can be shielded by the first barrier layer (3) and the second barrier layer (5), so that the penetration of water vapor into the hologram layer (4) is suppressed, and thus the deterioration of the hologram layer (4) can be prevented.

[0143] In addition, the chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0144] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) and a decrease in clarity are likely to occur.

[0145] However, according to the configuration of the present embodiment, by forming a first barrier layer (3) and a second barrier layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, thereby preventing deterioration of the first resin substrate (1) and the second resin substrate (7).

[0146] [Hard Coat Layer]

[0147] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0148] The hard coat layer is preferably formed from a curable resin composition. The curable resin composition is not particularly limited, but is preferably cured by irradiation with energy rays such as electron beams, radiation, or ultraviolet rays, or by heating; and, from the perspective of molding time and productivity, an ultraviolet-curable resin composition is more preferable.

[0149] Examples of curable resins constituting the above curable resin composition include acrylate compounds, urethane acrylate compounds, epoxy acrylate compounds, carboxyl group-modified epoxy acrylate compounds, polyester acrylate compounds, copolymerized acrylates, alicyclic epoxy resins, glycidyl ether epoxy resins, vinyl ether compounds, and oxetane compounds. The above curable resins may be used as a single type or in combination of two or more types.

[0150] Among these curable resins, a curable compound of the radical polymerization system, such as a polyfunctional acrylate compound, a polyfunctional urethane acrylate compound, or a polyfunctional epoxy acrylate compound, or a curable compound of the thermal polymerization system, such as an alkoxysilane or an alkylalkoxysilane, is preferred in that it can impart excellent surface hardness to the hard coat layer.

[0151] The curable resin composition forming the hard coat layer may include a leveling agent as a surface conditioning component. Examples of the leveling agent include fluorine-based leveling agents, silicone-based leveling agents, and acrylic-based leveling agents. Among these leveling agents, acrylic-based leveling agents are preferred in that they can ensure excellent adhesion when a barrier layer is laminated onto the surface of the hard coat layer.

[0152] When the above-mentioned curable resin composition is cured with ultraviolet light, a photopolymerization initiator is used. Examples of the above-mentioned photopolymerization initiators include benzyl, benzophenone and its derivatives, thioxantones, benzyldimethylketals, α-hydroxyalkylphenones, hydroxyketones, aminoalkylphenones, and acylphosphine oxides. The amount of the above-mentioned photopolymerization initiator added is typically 0.1 to 8 parts by mass per 100 parts by mass of the above-mentioned curable resin composition.

[0153] The curable resin composition forming the hard coat layer may include a refractive index adjusting component. Examples of the refractive index adjusting component include fine particles of a high-refractive-index metal compound such as zinc oxide, zirconium oxide, or titanium oxide, or fine particles of a low-refractive-index metal compound such as magnesium fluoride. Here, it is preferable that the size of the fine particles of the refractive index adjusting component be 5 to 50 nm, as this does not impair the transparency and total light transmittance of the hard coat layer. Alternatively, the fine particles of the refractive index adjusting component may be mixed with the curable resin composition in advance and included in the curable resin composition forming the hard coat layer. Alternatively, the fine particles of the refractive index adjusting component, which have been mixed with the curable resin composition in advance, may be used as the curable resin composition forming the hard coat layer. Commercially available products exist for which the fine particles of the refractive index adjusting component have been mixed with the curable resin composition in advance. Examples of such commercially available products include Rioduras TYZ, Rioduras TYT, and Rioduras TYM (all manufactured by Toyochem Co., Ltd.).

[0154] The curable resin composition forming the hard coat layer may include, in addition to the components described above, additives such as lubricants, silicon-based compounds, fluorine-based compounds, or mixtures thereof, antioxidants, ultraviolet absorbers, antistatic agents, flame retardants, silicone-based compounds, fillers, glass fibers, and silica. These additives may be used individually or in combination of two or more types.

[0155] The thickness of the hard coat layer is not particularly limited, but is preferably 1 to 20 μm. If the thickness of the hard coat layer is 1 μm or more, sufficient hardness can be imparted to the surface of the resin substrate. In addition, if the thickness of the hard coat layer is 20 μm or less, moldability and cutability can be further secured for the resin substrate. Furthermore, it is also desirable in that the curing shrinkage of the hard coat layer is further suppressed and does not cause warping or bending of the resin substrate.

[0156] When the refractive index of the resin substrate is set to na, the refractive index nb of the hard coat layer is preferably within the range of na ± 0.20, more preferably within the range of na ± 0.15, and even more preferably within the range of na ± 0.10. If the refractive index nb of the hard coat layer is within the range of na ± 0.20, the brightness value of the light guide plate (8) for image display becomes better, and color non-uniformity can be further prevented.

[0157] A method for forming a hard coat layer may include, for example, a method of forming and laminating the hard coat layer on the surface of a resin substrate by coating the surface of the resin substrate with a curable resin composition and then curing it into a film, but is not limited to this method.

[0158] A known method is used for lamination with a resin substrate. Examples of the known methods include the dip coat method, natural coat method, reverse coat method, comma coater method, roll coat method, spin coat method, wire bar method, extrusion method, curtain coat method, spray coat method, and gravure coat method. In addition, for example, a method of laminating a hard coat layer onto a resin substrate may be adopted by using a transfer sheet in which a hard coat layer is formed on a release layer.

[0159] In addition, for the purpose of improving the adhesion between the hard coat layer and the resin substrate, a primer layer may be formed on the surface of the resin substrate in advance.

[0160] Method for manufacturing a light guide plate for image display

[0161] As an example of a method for manufacturing a light guide plate for image display according to the present embodiment, a method for manufacturing a light guide plate (8) for image display shown in FIG. 1 will be described.

[0162] A first resin substrate (1) and a second resin substrate (7) are prepared ([substrate preparation process]), and a first barrier layer (3) and a second barrier layer (5) are formed respectively on the surfaces of the first resin substrate (1) and the second resin substrate (7) by interposing a first anchor coat layer (2) and a second anchor coat layer (6) ([barrier layer formation process]). As for the manufacturing method of the first barrier layer (3) and the second barrier layer (5), an appropriate manufacturing method is selected according to the material of the first barrier layer (3) and the second barrier layer (5).

[0163] For example, a photosensitive material for forming a hologram is applied to the surface of the first barrier layer (3) in the first resin substrate (1) on which the first barrier layer (3) is formed. At this time, a transparent seal layer having the same thickness as the hologram layer (4) may be formed on the outer periphery of the first barrier layer (3). The seal layer seals the outer periphery of the hologram layer (4) after the hologram layer (4) is formed with the photosensitive material. The seal layer is made of a transparent material, and for example, epoxy resin, silicone resin, or ethiol resin, etc. are used.

[0164] Afterwards, a second resin substrate (7) having a second barrier layer (5) formed thereon is placed on the photosensitive material with the second barrier layer (5) facing toward the photosensitive material ([light guide plate manufacturing process]).

[0165] However, the manufacturing sequence described above is an example. For example, after a photosensitive material is applied to a second resin substrate (7) on which a second barrier layer (5) is formed, a first resin substrate (1) on which a first barrier layer (3) is formed may be placed on a hologram layer (4).

[0166] Afterwards, by a pressure press, each layer of the first resin substrate (1), the first anchor coat layer (2), the first barrier layer (3), the hologram layer (4), the second barrier layer (5), the second anchor coat layer (6), and the second resin substrate (7) is laminated to obtain a light guide plate (8) for image display.

[0167] Afterwards, an interference pattern corresponding to the diffraction pattern is formed on the photosensitive material, and a diffraction grating is formed within the photosensitive material.

[0168] <<Second Embodiment>>

[0169] A light guide plate for image display related to the second embodiment of the present invention comprises a laminate having a resin substrate, an anchor coat layer, and a barrier layer in this order, and a hologram layer arranged in this order, wherein the thickness of the barrier layer is 150 nm or less, the total thickness of the anchor coat layer and the barrier layer is 300 nm or less, and additionally, the tanδ peak temperature in the viscoelasticity measurement of the anchor coat layer is 80 ℃ or less.

[0170] If the thickness of the barrier layer is 150 nm or less, the residual stress in the barrier layer does not become excessively large, so cracks in the barrier layer can be prevented.

[0171] In addition, if the total thickness of the anchor coat layer and the barrier layer is 300 nm or less, it is possible to prevent the barrier layer from being excessively deformed by residual stress.

[0172] In addition, if the tanδ peak temperature in the measurement of the viscoelasticity of the anchor coat layer is 80°C or lower, cracks are unlikely to occur because the anchor coat layer follows the expansion of the resin substrate even when it expands in a moist heat environment.

[0173] Therefore, by providing the above configuration, cracks or deformations caused by residual stress in the barrier layer, and furthermore, cracks caused by expansion of the resin substrate under a moist and hot environment, can be prevented, so the barrier properties are improved and the deterioration of the hologram layer can be suppressed.

[0174] The light guide plate for image display according to the present embodiment may include one or more resins selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin.

[0175] The light guide plate for image display according to the present embodiment may have the barrier layer comprising an inorganic material.

[0176] The light guide plate for image display according to the present embodiment may include one or more inorganic materials selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, and aluminum oxide in the barrier layer.

[0177] The light guide plate for image display according to the present embodiment may include one or more resins selected from the group consisting of acrylic resin, urethane resin, and polyester resin in the anchor coat layer.

[0178] In the image display light guide plate of the present embodiment, the laminate may have a hard coat layer on both surfaces of the resin substrate.

[0179] Hereinafter, a light guide plate for image display related to the present embodiment will be described.

[0180] Light guide plate for image display

[0181] The outline of the laminated configuration of the light guide plate for image display in this embodiment is the same as the light guide plate for image display related to the first embodiment.

[0182] [First laminate (11)]

[0183] The first laminate (11) comprises a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order. The light guide plate (8) for image display can suppress the deterioration of the hologram layer by placing the first laminate (11) on the surface of the hologram layer (4).

[0184] (Barrier)

[0185] The water vapor permeability of the first laminate (11) is preferably less than 0.1 g / m² / day, more preferably less than 0.08 g / m² / day, even more preferably less than 0.05 g / m² / day, even more preferably less than 0.03 g / m² / day, even more preferably less than 0.01 g / m² / day, and even more preferably less than 0.005 g / m² / day.

[0186] If the water vapor permeability of the first laminate (11) is within the above range, the deterioration of the hologram layer (4) can be further suppressed.

[0187] [First resin entry (1)]

[0188] The preferred thickness, total light transmittance, and material of the first resin substrate (1) are the same as those of the first resin substrate (1) related to the first embodiment.

[0189] The surface roughness Sa of the first resin substrate (1) is not particularly limited, but with 0 nm as the lower limit, it is preferably 10 nm or less, more preferably 8 nm or less, and even more preferably 6 nm or less. If the surface roughness Sa is 10 nm or less, the surface roughness Sa of the first laminate (11) can be reduced, and the brightness value of the light guide plate (8) for image display becomes good.

[0190] In addition, in this specification, surface roughness Sa is a surface roughness measured using a white interferometer (VertScan, manufactured by Ryoka Systems Co., Ltd.).

[0191] [First Anchor Coat Layer (2)]

[0192] The preferred thickness, tanδ peak temperature, total light transmittance, refractive index, material, and formation method of the first anchor coat layer (2) are the same as those of the first anchor coat layer (2) related to the first embodiment.

[0193] [First barrier layer (3)]

[0194] The preferred oxygen permeability, water vapor permeability, thickness, and refractive index of the first barrier layer (3) are the same as those of the first barrier layer (3) related to the first embodiment.

[0195] The first barrier layer (3) preferably comprises an inorganic material. Among these, it is more preferable to include one or more selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon (DLC), and aluminum oxide. Furthermore, from the viewpoint of improving total light transmittance and barrier properties, it is even more preferable for the first barrier layer (3) to include silicon oxide or silicon oxynitride.

[0196] When the first barrier layer (3) is made of silicon oxide or silicon oxynitride, the first barrier layer (3) can be formed by conventionally known methods such as vacuum deposition, sputtering, ion plating, or plasma CVD. Among these, sputtering is preferred in order to obtain good barrier properties and to improve the clarity of the light guide plate (8) for image display.

[0197] In order to improve the adhesion between the first anchor coat layer (2) and the first barrier layer (3), surface treatments such as corona discharge treatment or low-temperature plasma treatment may be performed on the surface of the first anchor coat layer (2), or a silane coupling agent may be applied, or a mixture of saturated polyester and isocyanate may be applied.

[0198] For example, when forming a film by vacuum deposition, silicon, silicon monoxide, silicon dioxide, silicon oxynitride, or a mixture thereof is used as the evaporation material, 1.0 × 10 -3 ~ 2.0 × 10 -1 Under a vacuum of Pa, heat and evaporate using an electron beam, resistance heating, or high-frequency heating method.

[0199] In addition, a reaction deposition method carried out while supplying oxygen and nitrogen gases can also be employed.

[0200] Also, for example, when forming a film by the sputtering method, silicon, silicon monoxide, silicon dioxide, silicon oxynitride, or a mixture thereof is used as a target, 1.0 × 10 -2 ~ 5.0 × 10 -1 Under a vacuum of Pa, the tabernacle can be consecrated.

[0201] In addition, a reactive sputtering method carried out while supplying oxygen gas, nitrogen gas, and argon gas can also be employed.

[0202] In the silicon oxide or silicon oxynitride forming the first barrier layer (3), calcium, magnesium, or their oxides may be mixed in as impurities if the amount is 10 mass% or less.

[0203] Diamond-like carbon (DLC) is an amorphous carbon material that is generally composed of a ternary structure consisting of a diamond-like structure, a graphite-like structure, and a polyethylene-type polymer structure containing hydrogen atoms in its structure. When hydrocarbons such as ethylene, acetylene, or benzene are used as carbon sources in the production of DLC, the structure is typically a ternary structure containing hydrogen.

[0204] DLC has excellent hardness, lubricity, wear resistance, chemical stability, heat resistance, and surface smoothness. Because DLC forms the dense polymer structure described above, it also has excellent gas barrier and water vapor barrier properties.

[0205] When forming the first barrier layer (3) by DLC, well-known appropriate coating methods such as physical vapor deposition methods like plasma CVD, ion plating, or ion beam sputtering can be used.

[0206] When the first barrier layer (3) is made of aluminum oxide, the first barrier layer (3) may be formed, for example, only with Al2O3, or may be formed by mixing two or more types selected from the group consisting of Al, AlO, and Al2O3. The atomic ratio of Al to O in the aluminum oxide layer varies depending on the manufacturing conditions of the aluminum oxide layer. The aluminum oxide layer that can be used as the first barrier layer (3) may contain a small amount of other components (at most up to 3% of the total components) within a range where the barrier performance is not impaired.

[0207] When forming the first barrier layer (3) with aluminum oxide, it is not particularly limited. For example, as a method for forming the first barrier layer (3), PVD (physical vapor deposition) or CVD (chemical vapor deposition) methods such as vacuum deposition, sputtering, or ion plating may be used.

[0208] For example, in vacuum deposition, materials such as Al and Al2O3 are used as deposition source materials, and resistance heating, high-frequency induction heating, or electron beam heating may be used as the heating method for the deposition source. In vacuum deposition, oxygen, nitrogen, or water vapor may be introduced as a reactive gas, or reactive deposition using means such as ozone addition or ion assist may be used. Additionally, bias may be applied to the deposited surface, or the temperature of the deposited surface may be raised or lowered. The same applies to other film deposition methods other than vacuum deposition, such as sputtering, PVD, and CVD.

[0209] [Hologram layer (4)]

[0210] The preferred material of the hologram layer (4) is the same as the hologram layer (4) related to the first embodiment.

[0211] [Second laminate (12)]

[0212] The second laminate (12) comprises a second barrier layer (5), a second anchor coat layer (6), and a second resin substrate (7) in this order. The various physical properties of the second laminate (12) may be different from those of the first laminate (11).

[0213] [Second barrier layer (5)]

[0214] The second barrier layer (5) is laminated on the opposite side of the first barrier layer (3) via a hologram layer (4). The second barrier layer (5) uses the same configuration as exemplified in the description of the first barrier layer (3). However, the thickness and material of the second barrier layer (5) may be different from those of the first barrier layer (3).

[0215] [Second Anchor Coat Layer (6)]

[0216] The second anchor coat layer (6) is disposed between the second barrier layer (5) and the second resin substrate (7). The second anchor coat layer (6) uses the same configuration as exemplified in the description of the first anchor coat layer (2). However, the thickness and material of the second anchor coat layer (6) may be different from those of the first anchor coat layer (2).

[0217] [2nd Substantiation (7)]

[0218] The second resin substrate (7) is laminated on the surface of the second barrier layer (5). The second resin substrate (7) uses the same configuration as exemplified in the description of the first resin substrate (1). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image emission side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0219] [Light guide plate for image display (8)]

[0220] In the image display light guide plate (8), a first anchor coat layer (2) and a first barrier layer (3), and a second barrier layer (5) and a second anchor coat layer (6) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0221] Gas from the outside of the light guide plate (8) for image display passes through the first resin substrate (1) and the second resin substrate (7) to some extent, or accumulates inside. At this time, moisture is particularly likely to accumulate in the first resin substrate (1) and the second resin substrate (7).

[0222] However, according to the configuration of the present embodiment, moisture that has penetrated from the outside into the first resin substrate (1) and the second resin substrate (7) can be shielded by the first barrier layer (3) and the second barrier layer (5), so that the penetration of water vapor into the hologram layer (4) is suppressed, and thus the deterioration of the hologram layer (4) can be prevented.

[0223] In addition, the chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0224] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) or a decrease in clarity is likely to occur.

[0225] However, according to the configuration of the present embodiment, by forming a first barrier layer (3) and a second barrier layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, thereby preventing deterioration of the first resin substrate (1) and the second resin substrate (7).

[0226] [Hard Coat Layer]

[0227] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0228] The preferred material, thickness, refractive index, and method of forming the hard coat layer are the same as the hard coat layer related to the first embodiment.

[0229] Method for manufacturing a light guide plate for image display

[0230] The method for manufacturing a light guide plate for image display according to the present embodiment is the same as the method for manufacturing a light guide plate for image display related to the first embodiment.

[0231] <<Third Embodiment>>

[0232] A light guide plate for image display related to the third embodiment of the present invention has a laminate having a resin substrate, an anchor coat layer, and a barrier layer in that order, and a hologram layer, wherein the thickness of the anchor coat layer is A nm and the tanδ peak temperature in the measurement of the viscoelasticity of the anchor coat layer is B °C, and A / B is 3 or less.

[0233] The light guide plate for image display according to the present embodiment can suppress the deterioration of the hologram layer by having the above configuration, and since deformation caused by residual stress of the barrier layer is unlikely to occur in a humid and hot environment, the optical properties are unlikely to change even in a humid and hot environment.

[0234] The light guide plate for image display according to the present embodiment may have an anchor coat layer thickness of 1 nm or more and 200 nm or less.

[0235] In the image display light guide plate of the present embodiment, the tanδ peak temperature in the measurement of the viscoelasticity of the anchor coat layer may be 10°C or higher and 80°C or lower.

[0236] The light guide plate for image display according to the present embodiment may include one or more resins selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin.

[0237] The light guide plate for image display according to the present embodiment may include one or more resins selected from the group consisting of acrylic resin, urethane resin, and polyester resin in the anchor coat layer.

[0238] The light guide plate for image display according to the present embodiment may have the barrier layer comprising an inorganic material.

[0239] The light guide plate for image display according to the present embodiment may include one or more inorganic materials selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, and aluminum oxide in the barrier layer.

[0240] In the image display light guide plate of the present embodiment, the laminate may have a hard coat layer on both surfaces of the resin substrate.

[0241] The light guide plate for image display according to the present embodiment may have a water vapor transmittance of the laminate of less than 0.01 g / m² / day.

[0242] Hereinafter, a light guide plate for image display related to the present embodiment will be described.

[0243] Light guide plate for image display

[0244] The outline of the laminated configuration of the light guide plate for image display in this embodiment is the same as the light guide plate for image display related to the first embodiment.

[0245] [First laminate (11)]

[0246] The first laminate (11) comprises a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order. The light guide plate (8) for image display can suppress the deterioration of the hologram layer by placing the first laminate (11) on the surface of the hologram layer (4).

[0247] The preferred water vapor permeability of the first laminate (11) is the same as that of the first laminate (11) related to the first embodiment.

[0248] (Optical properties)

[0249] The haze of the first laminate (11) is preferably less than 0.1%, more preferably less than 0.08%, even more preferably less than 0.06%, and even more preferably less than 0.05%. If the haze of the first laminate (11) is less than 0.1%, the brightness value of the light guide plate (8) for image display becomes better.

[0250] Also, the haze after storing the first laminate (11) at 40°C and 90°F for 10 days is preferably less than 2%, more preferably less than 1%, even more preferably less than 0.5%, even more preferably less than 0.2%, and particularly preferably less than 0.1%.

[0251] [First resin entry (1)]

[0252] The preferred thickness, total light transmittance, and material of the first resin substrate (1) are the same as those of the first resin substrate (1) related to the first embodiment.

[0253] [First Anchor Coat Layer (2)]

[0254] The preferred thickness, tanδ peak temperature, total light transmittance, refractive index, material, and formation method of the first anchor coat layer (2) are the same as those of the first anchor coat layer (2) related to the first embodiment.

[0255] When the tanδ peak temperature of the first anchor coat layer (2) is lower than the ambient temperature, if the light guide plate (8) for image display is placed in a humid heat environment, the elastic modulus of the first anchor coat layer (2) decreases. And, if the first anchor coat layer (2) becomes soft, the residual stress of the first barrier layer (3) cannot be suppressed, so the first barrier layer (3) deforms, and haze tends to rise. Even if the first anchor coat layer (2) is thick, it tends to deform significantly due to the residual stress of the first barrier layer (3) in a humid heat environment, so haze tends to rise.

[0256] Meanwhile, when the tanδ peak temperature of the first anchor coat layer (2) is higher than the ambient temperature, the elastic modulus is less likely to decrease even in a humid heat environment, so deformation due to residual stress in the first barrier layer (3) is less likely to occur, and thus the rise in haze is suppressed. Even when the first anchor coat layer (2) is thin, deformation due to residual stress in the first barrier layer (3) is less likely to occur, so the rise in haze is suppressed.

[0257] From the above perspective, when the thickness of the first anchor coat layer (2) is set to A [nm] and the tanδ peak temperature in the viscoelasticity measurement of the first anchor coat layer (2) is set to B [℃], A / B is 3 or less, preferably 2.5 or less, and more preferably 2 or less.

[0258] [First barrier layer (3)]

[0259] The preferred oxygen permeability, water vapor permeability, thickness, and refractive index of the first barrier layer (3) are the same as those of the first barrier layer (3) related to the first embodiment.

[0260] Also, the preferred material and method of forming the first barrier layer (3) are the same as the first barrier layer (3) related to the second embodiment.

[0261] [Hologram layer (4)]

[0262] The preferred material of the hologram layer (4) is the same as the hologram layer (4) related to the first embodiment.

[0263] [Second laminate (12)]

[0264] The second laminate (12) comprises a second barrier layer (5), a second anchor coat layer (6), and a second resin substrate (7) in this order. The various physical properties of the second laminate (12) may be different from those of the first laminate (11).

[0265] [Second barrier layer (5)]

[0266] The second barrier layer (5) is laminated on the opposite side of the first barrier layer (3) via a hologram layer (4). The second barrier layer (5) uses the same configuration as exemplified in the description of the first barrier layer (3). However, the thickness and material of the second barrier layer (5) may be different from those of the first barrier layer (3).

[0267] [Second Anchor Coat Layer (6)]

[0268] The second anchor coat layer (6) is disposed between the second barrier layer (5) and the second resin substrate (7). The second anchor coat layer (6) uses the same configuration as exemplified in the description of the first anchor coat layer (2). However, the thickness and material of the second anchor coat layer (6) may be different from those of the first anchor coat layer (2).

[0269] [2nd Substantiation (7)]

[0270] The second resin substrate (7) is laminated on the surface of the second barrier layer (5). The second resin substrate (7) uses the same configuration as exemplified in the description of the first resin substrate (1). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image emission side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0271] [Light guide plate for image display (8)]

[0272] In the image display light guide plate (8), a first anchor coat layer (2) and a first barrier layer (3), and a second barrier layer (5) and a second anchor coat layer (6) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0273] Gas from the outside of the light guide plate (8) for image display passes through the first resin substrate (1) and the second resin substrate (7) to some extent, or accumulates inside. At this time, moisture is particularly likely to accumulate in the first resin substrate (1) and the second resin substrate (7).

[0274] However, according to the configuration of the present embodiment, moisture that has penetrated from the outside into the first resin substrate (1) and the second resin substrate (7) can be shielded by the first barrier layer (3) and the second barrier layer (5), so that the penetration of water vapor into the hologram layer (4) is suppressed, and thus the deterioration of the hologram layer (4) can be prevented.

[0275] In addition, the chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0276] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) or a decrease in clarity is likely to occur.

[0277] However, according to the configuration of the present embodiment, by forming a first barrier layer (3) and a second barrier layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, thereby preventing deterioration of the first resin substrate (1) and the second resin substrate (7).

[0278] [Hard Coat Layer]

[0279] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0280] The preferred material, thickness, refractive index, and method of forming the hard coat layer are the same as the hard coat layer related to the first embodiment.

[0281] Method for manufacturing a light guide plate for image display

[0282] The method for manufacturing a light guide plate for image display according to the present embodiment is the same as the method for manufacturing a light guide plate for image display related to the first embodiment.

[0283] <<Fourth Embodiment>>

[0284] A light guide plate for image display related to the fourth embodiment of the present invention has a laminate having a resin substrate, an anchor coat layer, and a barrier layer in that order, and a hologram layer, wherein the anchor coat layer is composed of a resin composition containing a binder resin having hydroxyl groups and an isocyanate compound, and the molar ratio of the isocyanate group (NCO) of the isocyanate compound to the hydroxyl group (OH) of the binder resin, NCO / OH, is 0.8 or higher.

[0285] The light guide plate for image display according to the present embodiment has the above characteristics, so that the deterioration of the hologram layer can be suppressed and good solvent resistance is also present.

[0286] The light guide plate for image display according to the present embodiment may include at least one resin selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin.

[0287] The light guide plate for image display according to the present embodiment may have the anchor coat layer comprising at least one resin selected from the group consisting of acrylic resin, urethane resin, and polyester resin as the binder resin.

[0288] The light guide plate for image display according to the present embodiment may have the barrier layer comprising an inorganic material.

[0289] The light guide plate for image display according to the present embodiment may include at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, and aluminum oxide in the barrier layer.

[0290] In the image display light guide plate of the present embodiment, the barrier layer may have silicon oxynitride as the main component, and the nitrogen element composition in the barrier layer obtained by X-ray photoelectric molecular optics (XPS) may be 7 atm% or more.

[0291] In the image display light guide plate of the present embodiment, the laminate may have a hard coat layer on both surfaces of the resin substrate.

[0292] The light guide plate for image display according to the present embodiment may have a water vapor transmittance of the laminate of less than 0.01 g / m² / day.

[0293] Hereinafter, a light guide plate for image display related to the present embodiment will be described.

[0294] Light guide plate for image display

[0295] The outline of the laminated configuration of the light guide plate for image display in this embodiment is the same as the light guide plate for image display related to the first embodiment.

[0296] [First laminate (11)]

[0297] The first laminate (11) comprises a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order. The light guide plate (8) for image display can suppress the deterioration of the hologram layer and also obtain good solvent resistance by placing the first laminate (11) on the surface of the hologram layer (4).

[0298] In addition, "solvent resistance" in the present invention refers to the fact that when a solvent such as isopropyl alcohol is applied to the surface of the first barrier layer (3) and wiped off with a wipe, the first barrier layer (3) does not peel off from the first resin substrate (1). More specifically, it is evaluated by the method described in the example.

[0299] The preferred total light transmittance and water vapor transmittance of the first laminate (11) are the same as those of the first laminate (11) related to the first embodiment.

[0300] [First resin entry (1)]

[0301] The preferred thickness, total light transmittance, and material of the first resin substrate (1) are the same as those of the first resin substrate (1) related to the first embodiment.

[0302] [First Anchor Coat Layer (2)]

[0303] The preferred thickness, total light transmittance, refractive index, and formation method of the first anchor coat layer (2) are the same as those of the first anchor coat layer (2) related to the first embodiment.

[0304] The first anchor coat layer (2) is composed of a resin composition including a binder resin having hydroxyl groups and an isocyanate compound. As the binder resin is crosslinked by the isocyanate compound, the solvent resistance is improved.

[0305] Binder resins having hydroxyl groups are not particularly limited, but examples include acrylic resins, urethane resins, polycarbonate resins, polyether resins, and polyester resins, and at least one type selected from the group consisting of acrylic resins, urethane resins, and polyester resins is preferred. The binder resin is preferably a polyol having two or more hydroxyl groups in one molecule.

[0306] The hydroxyl group value of the binder resin is preferably 0.1 to 300 mgKOH / g, more preferably 1 to 200 mgKOH / g, and even more preferably 5 to 150 mgKOH / g from the perspective of increasing the crosslinking density.

[0307] The isocyanate compound is preferably an aromatic or aliphatic diisocyanate or a polyisocyanate with three or more valences. Examples of isocyanate compounds include tetramethylene diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, cyclohexane diisocyanate, dicyclohexyl diisocyanate, or trimers thereof.

[0308] The molar ratio of the isocyanate group (NCO) of the isocyanate compound to the hydroxyl group (OH) of the binder resin, NCO / OH, is 0.8 or higher, preferably 0.9 or higher, and more preferably 1 or higher. The upper limit is not particularly limited, but is preferably 10 or lower.

[0309] If the isocyanate group of the isocyanate compound is contained in greater quantities than the hydroxyl group of the binder resin, some of the isocyanate compound reacts with the functional group on the surface of the first resin substrate (1) to form a bond, so the adhesion between the first resin substrate (1) and the first anchor coat layer (2) is improved.

[0310] In the resin composition constituting the first anchor coat layer (2), resins other than the binder resin having hydroxyl groups, silane coupling agents, sensitizers, crosslinking agents other than isocyanate compounds, ultraviolet absorbers, polymerization inhibitors, surfactants, fillers, release agents, and thermoplastic resins other than those above may be added. These additives may be used as a single type or in combination of two or more types.

[0311] Examples of resins other than the binder resin having the above hydroxyl group include fluorine-based resins, polyethersulfone-based resins, silicone-based resins, cycloolefin-based resins, thermoplastic polyimide-based resins, polyamide-based resins, polyamideimide-based resins, polyarylate-based resins, polysulfone-based resins, polyetherimide-based resins, polyetheretherketone-based resins, polyethersilicone-based resins, and polyphenylenesulfide-based resins.

[0312] Examples of crosslinking agents other than the above isocyanate compounds include peroxide-based crosslinking agents, epoxy-based crosslinking agents, and imine-based crosslinking agents.

[0313] [First barrier layer (3)]

[0314] The preferred oxygen permeability, water vapor permeability, thickness, and refractive index of the first barrier layer (3) are the same as those of the first barrier layer (3) related to the first embodiment.

[0315] Also, the preferred material and method of forming the first barrier layer (3) are the same as the first barrier layer (3) related to the second embodiment.

[0316] Among them, in terms of barrier properties and solvent resistance, it is preferable that the first barrier layer (3) contains silicon oxynitride as a main component.

[0317] When the first barrier layer (3) contains silicon oxynitride, the nitrogen element composition in the first barrier layer (3) obtained by X-ray Photoelectron Spectroscopy (XPS) is preferably 7 atm% or more, more preferably 8 atm% or more, even more preferably 9 atm% or more, and even more preferably 10 atm% or more. If the nitrogen element composition is 7 atm% or more, the solvent resistance of the first barrier layer (3) is improved.

[0318] Also, the nitrogen element composition in the first barrier layer (3) is preferably 40 atm% or less, more preferably 30 atm% or less, and even more preferably 25 atm% or less from the perspective of optical properties.

[0319] The nitrogen element composition in the first barrier layer (3) can be adjusted by the nitrogen flow rate, power, and film pressure during film formation.

[0320] In particular, to make the nitrogen element composition 7 atm% or more, the ratio of oxygen flow rate O2 [sccm] to nitrogen flow rate N2 [sccm] O2 / N2 is preferably 0.10 to 1.5, more preferably 0.12 to 1.0, and even more preferably 0.15 to 1.0 or more.

[0321] Also, the power is preferably 1000 to 2000 W. Since O2 / N2 and power influence each other, when O2 / N2 is 0.10 or higher and less than 0.15, it is preferable to set the power to 1000 W or higher and less than 1500 W, and when O2 / N2 is 0.15 or higher and less than 1.5, it is preferable to set the power to 1500 W or higher and less than 2000 W.

[0322] Also, the pressure of the tabernacle is 1.0 × 10⁻⁶ -2 ~ 2.0 × 10 -1 Pa is desirable, and 5.0 × 10 -2 ~ 1.5 × 10 -1 Pa is desirable.

[0323] [Hologram layer (4)]

[0324] The preferred material of the hologram layer (4) is the same as the hologram layer (4) related to the first embodiment.

[0325] [Second laminate (12)]

[0326] The second laminate (12) comprises a second barrier layer (5), a second anchor coat layer (6), and a second resin substrate (7) in this order. The various physical properties of the second laminate (12) may be different from those of the first laminate (11).

[0327] [Second barrier layer (5)]

[0328] The second barrier layer (5) is laminated on the opposite side of the first barrier layer (3) via a hologram layer (4). The second barrier layer (5) uses the same configuration as exemplified in the description of the first barrier layer (3). However, the thickness and material of the second barrier layer (5) may be different from those of the first barrier layer (3).

[0329] [Second Anchor Coat Layer (6)]

[0330] The second anchor coat layer (6) is disposed between the second barrier layer (5) and the second resin substrate (7). The second anchor coat layer (6) uses the same configuration as exemplified in the description of the first anchor coat layer (2). However, the thickness and material of the second anchor coat layer (6) may be different from those of the first anchor coat layer (2).

[0331] [2nd Substantiation (7)]

[0332] The second resin substrate (7) is laminated on the surface of the second barrier layer (5). The second resin substrate (7) uses the same configuration as exemplified in the description of the first resin substrate (1). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image emission side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0333] [Light guide plate for image display (8)]

[0334] In the image display light guide plate (8), a first anchor coat layer (2) and a first barrier layer (3), and a second barrier layer (5) and a second anchor coat layer (6) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0335] Gas from the outside of the light guide plate (8) for image display passes through the first resin substrate (1) and the second resin substrate (7) to some extent, or accumulates inside. At this time, moisture is particularly likely to accumulate in the first resin substrate (1) and the second resin substrate (7).

[0336] However, according to the configuration of the present embodiment, moisture that has penetrated from the outside into the first resin substrate (1) and the second resin substrate (7) can be shielded by the first barrier layer (3) and the second barrier layer (5), so that the penetration of water vapor into the hologram layer (4) is suppressed, and thus the deterioration of the hologram layer (4) can be prevented.

[0337] In addition, the chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0338] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) or a decrease in clarity is likely to occur.

[0339] However, according to the configuration of the present embodiment, by forming a first barrier layer (3) and a second barrier layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, thereby preventing deterioration of the first resin substrate (1) and the second resin substrate (7).

[0340] [Hard Coat Layer]

[0341] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0342] The preferred material, thickness, refractive index, and method of forming the hard coat layer are the same as the hard coat layer related to the first embodiment.

[0343] Method for manufacturing a light guide plate for image display

[0344] The method for manufacturing a light guide plate for image display according to the present embodiment is the same as the method for manufacturing a light guide plate for image display related to the first embodiment.

[0345] <<Fifth Embodiment>>

[0346] A light guide plate for image display related to the fifth embodiment of the present invention comprises a laminate having a resin substrate and a protective layer in this order, and a hologram layer arranged in this order, wherein the surface roughness Sa of the side of the protective layer in contact with the hologram layer is less than 5.5 nm.

[0347] The light guide plate for image display according to the present embodiment can suppress the deterioration of the hologram layer by having the protective layer configured as described above.

[0348] The light guide plate for image display according to the present embodiment may include one or more resins selected from the group consisting of acrylic resin, polycarbonate resin, polyester resin, and cycloolefin resin.

[0349] The light guide plate for image display according to the present embodiment may have a resin layer (A) comprising a hard resin (a) having a hard dispersed phase in the matrix, wherein the resin substrate comprises the hard resin (a) having a hard dispersed phase in the matrix.

[0350] In the image display light guide plate of the present embodiment, the resin substrate may have the resin layer (A) and the resin layer (B), which has a different main component from the resin layer (A), laminated together.

[0351] The light guide plate for image display according to the present embodiment may have a resin substrate thickness of 0.05 to 5 mm.

[0352] The light guide plate for image display according to the present embodiment may have a pencil hardness of 3 H or higher on the surface opposite to the side facing the protective layer of the resin substrate.

[0353] In the light guide plate for image display according to the present embodiment, the laminate may have an adhesive layer between the resin substrate and the protective layer.

[0354] Hereinafter, a light guide plate for image display related to the present embodiment will be described.

[0355] Light guide plate for image display

[0356] The light guide plate for image display according to the present embodiment has at least a laminate having a resin substrate and a protective layer, and a hologram layer. The resin substrate, the protective layer, and the hologram layer are arranged in this order in the thickness direction. The resin substrate and the protective layer may be arranged on at least one surface of the hologram layer, but may also be arranged on both surfaces of the hologram layer. When the laminate is arranged on both surfaces of the hologram layer, the laminate arranged on one surface of the hologram layer is called the first laminate, and the laminate arranged on the other surface of the hologram layer is called the second laminate. In this case, the hologram layer is sandwiched between the first protective layer of the first laminate and the second protective layer of the second laminate, and the first resin substrate is laminated on the other side of the first protective layer, and the second resin substrate is laminated on the other side of the second protective layer. In the present embodiment, the first laminate and the second laminate may be collectively referred to as "laminated laminate" below. The first resin substrate and the second resin substrate may be collectively referred to as "resin substrate" below. Also, the first protective layer and the second protective layer may be collectively referred to as "protective layer" below.

[0357] One or more transparent layers may be disposed between the resin substrate and the protective layer, and between the protective layer and the hologram layer. Examples of transparent layers include an adhesive layer, a hard coat layer, etc.

[0358] In addition, the protective layer and the transparent layer may be disposed on one surface of the resin substrate, but may also be disposed on both surfaces of the resin substrate. That is, the configuration may be such that the protective layer, the resin substrate, the protective layer, and the hologram layer are arranged in this order in the thickness direction, or the configuration may be such that the protective layer, the transparent layer, the resin substrate, the transparent layer, the protective layer, and the hologram layer are arranged in this order in the thickness direction.

[0359] [First laminate (11)]

[0360] The first laminate (11) comprises a first resin substrate (1) and a first protective layer (3) in this order. The first laminate (11) may have a first adhesive layer (2) between the first resin substrate (1) and the first protective layer (3). The light guide plate (8) for image display can suppress the deterioration of the hologram layer by placing the first laminate (11) on the surface of the hologram layer (4).

[0361] (Barrier)

[0362] The water vapor permeability of the first laminate (11) is preferably less than 1 g / m² / day, more preferably less than 0.5 g / m² / day, even more preferably less than 0.3 g / m² / day, even more preferably less than 0.1 g / m² / day, even more preferably less than 0.08 g / m² / day, and even more preferably less than 0.05 g / m² / day.

[0363] If the water vapor permeability of the first laminate (11) is within the above range, the deterioration of the hologram layer (4) can be further suppressed.

[0364] [First resin entry (1)]

[0365] The thickness of the first resin substrate (1) is not particularly limited, but is preferably 0.05 to 5 mm.

[0366] The lower limit of the thickness of the first resin substrate (1) is not particularly limited, but from the perspective of making scratch resistance good, it is preferable to have a thickness of 0.1 mm or more, and more preferable to have a thickness of 0.2 mm or more.

[0367] Also, the upper limit of the thickness of the first resin substrate (1) is not particularly limited, but from the viewpoint of improving moldability and light transmittance, it is preferable to have a thickness of 3 mm or less, and more preferable to have a thickness of 2 mm or less.

[0368] The pencil hardness of the surface of the first resin substrate (1) on the side opposite to the first protective layer (3) (hereinafter simply referred to as "pencil hardness of the surface of the first resin substrate (1)") is not particularly limited, but is preferably 3 H or higher, more preferably 4 H or higher, and even more preferably 5 H or higher. By having a high pencil hardness (high hardness) of the surface of the first resin substrate (1), excellent scratch resistance can be imparted to the light guide plate (8) for image display.

[0369] Also, the surface roughness Sa of the first resin substrate (1) on the side facing the first protective layer (3) (hereinafter simply referred to as "surface roughness Sa of the first resin substrate (1)") is not particularly limited, but is preferably less than 5.5 nm. As the surface roughness Sa of the first resin substrate (1) is small, the first protective layer (3) described later becomes easier to form more uniformly, and the surface roughness Sa of the first protective layer (3) also becomes smaller. As a result, the water vapor barrier properties of the first protective layer (3) are improved, and the deterioration of the hologram layer (4) can be suppressed. In this regard, the surface roughness Sa of the first resin substrate (1) is preferably less than 5.5 nm with 0 nm as the lower limit, more preferably 5.0 nm or less, even more preferably 4.5 nm or less, even more preferably 4.0 nm or less, even more preferably 3.0 nm or less, even more preferably 2.5 nm or less, even more preferably 2.0 nm or less, and particularly preferably 1.5 nm or less.

[0370] The total light transmittance of the first resin substrate (1) is not particularly limited, but is preferably 80% or more, and more preferably 90% or more. If the total light transmittance of the first resin substrate (1) is 80% or more, the brightness value of the light guide plate (8) for image display becomes better.

[0371] The first resin substrate (1) preferably includes a thermoplastic resin in order to improve optical properties, impact resistance, scratch resistance and moldability.

[0372] The thermoplastic resin is not particularly limited as long as it is a thermoplastic resin capable of forming a film, sheet, or plate by melt extrusion. Preferred examples of thermoplastic resins include aromatic polyesters such as polyethylene terephthalate, polyethylene naphthalate, polypropylene terephthalate, polybutylene terephthalate, and poly-1,4-cyclohexylenedimethylene terephthalate; polyester resins represented by aliphatic polyesters such as polylactic acid-based polymers; and polyolefin resins such as polyethylene, polypropylene, and cycloolefin resins. Examples include polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyether resin, polyurethane resin, polyphenylene sulfide resin, polyesteramide resin, polyether ester resin, vinyl chloride resin, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, modified polyphenylene ether resin, polyarylate resin, polysulfone resin, polyetherimide resin, polyamideimide resin, polyimide resin, and copolymers thereof. These thermoplastic resins may be used as a single type or in combination of two or more types. Additionally, the first resin substrate (1) may be composed of a laminated layer made of two or more materials selected from the group consisting of the above thermoplastic resins.

[0373] In the present invention, one or more types selected from the group consisting of acrylic resin, polycarbonate resin, polyester resin, and cycloolefin resin are preferred, with respect to the fact that there is almost no absorption in the visible light range.

[0374] Among these, acrylic resins are preferred in terms of excellent transparency, scratch resistance, and moldability.

[0375] In addition, polycarbonate resin is preferred in terms of excellent transparency, impact resistance, and moldability.

[0376] (Acrylic resin)

[0377] The preferred monomer constituting the above acrylic resin is the same as the monomer constituting the poly(meth)acrylic resin related to the first embodiment.

[0378] In addition, other monomers copolymerizable with the monomers constituting the acrylic resin may be added. Preferred compounds as other monomers are the same as the monofunctional monomers and polyfunctional monomers related to the first embodiment.

[0379] Among the above acrylic resins, a methyl methacrylate-styrene copolymer is preferred in terms of improving environmental resistance (bending due to moisture absorption).

[0380] The methyl methacrylate-styrene copolymer resin preferably has 30 to 95 mass% of methyl methacrylate units and 5 to 70 mass% of styrene units based on the total monomer units, more preferably has 40 to 95 mass% of methyl methacrylate units and 5 to 60 mass% of styrene units, and even more preferably has 50 to 90 mass% of methyl methacrylate units and 10 to 50 mass% of styrene units. Since the ratio of methyl methacrylate units is above the above lower limit, the strength and surface hardness of the first resin substrate (1) are improved, and a light guide plate for image display with good scratch resistance is obtained. On the other hand, since the ratio of methyl methacrylate units is below the above upper limit, the environmental resistance is improved.

[0381] The above acrylic resin can be manufactured by polymerizing the aforementioned monomer components using known methods such as suspension polymerization, emulsion polymerization, or bulk polymerization.

[0382] (Polycarbonate resin)

[0383] There are no particular limitations on the above polycarbonate-based resin, and aromatic polycarbonate, aliphatic polycarbonate, or cycloaliphatic polycarbonate may be used.

[0384] Examples of the above aromatic polycarbonates include i) those obtained by reacting a divalent phenol with a carbonylating agent via interfacial polycondensation or melt ester exchange, ii) those obtained by polymerizing a carbonate prepolymer via solid ester exchange, iii) those obtained by polymerizing a cyclic carbonate compound via ring-opening polymerization. Among these, i) those obtained by reacting a divalent phenol with a carbonylating agent via interfacial polycondensation or melt ester exchange are preferred in terms of productivity.

[0385] As the divalent phenol in i) above, for example, hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)methane, bis{(4-hydroxy-3,5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, 2,2-bis{(4-hydroxy-3,5-dimethyl)phenyl}propane, 2,2-bis{(4-hydroxy-3,5-dibromo)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, Examples include 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantan, 4,4'-dihydroxydiphenylsulfone, 4,4'-dihydroxydiphenylsulfoxide, 4,4'-dihydroxydiphenylsulfide, 4,4'-dihydroxydiphenylketone, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ester, etc. These divalent phenols can be used either alone or in combination of two or more types.

[0386] Among the above-described divalent phenols, it is preferable to use a divalent phenol selected from the group consisting of bisphenol A, 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, either alone or in combination of two or more types.

[0387] Among these, the use of bisphenol A alone, or in combination with 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and one or more divalent phenols selected from the group consisting of bisphenol A, 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane and α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene is preferred.

[0388] Examples of carbonylating agents in i) above include carbonyl halides such as phosgene, carbonate esters such as diphenyl carbonate, and haloformates such as dihaloformate of divalent phenol. These carbonylating agents may be used individually or in combination of two or more types.

[0389] [Preferred embodiment of the first resin substrate (1)]

[0390] A first preferred embodiment of the first resin substrate (1) consists of a resin layer (A) comprising a hard resin (a) having a hard dispersed phase in the matrix.

[0391] A second preferred embodiment of the first resin substrate (1) is formed by laminating a resin layer (A) comprising a hard resin (a) having a hard dispersed phase in a matrix, and a resin layer (B) having a different main component from the resin layer (A).

[0392] (Resin layer (A))

[0393] The hard resin (a) forming the resin layer (A) comprises a matrix resin and a hard dispersion phase (hereinafter also referred to as "hard dispersion phase").

[0394] By forming the resin layer (A) with the hard resin (a), the scratch resistance of the first resin substrate (1) can be improved.

[0395] In addition, by being formed with the hard resin (a) above, the surface roughness of the resin layer (A) can be reduced. Therefore, since the surface roughness Sa of the first protective layer (3) described later is reduced, the water vapor barrier properties are improved, and the deterioration of the hologram layer (4) can be suppressed.

[0396] As the matrix resin of the resin layer (A), it is preferable to use one or more selected from the group consisting of the acrylic resin, polycarbonate resin, polyester resin, and cycloolefin resin described above.

[0397] Among these, acrylic resins are preferred due to their excellent transparency, scratch resistance, and moldability.

[0398] The hard dispersion phase included in the hard resin (a) forming the resin layer (A) should have at least one of the heat resistance and scratch resistance superior to the acrylic resin, and among these, a thermosetting resin is preferred.

[0399] Examples of thermosetting resins include polycondensation or addition condensation resins such as phenolic resin, amino resin, epoxy resin, silicone resin, thermosetting polyimide resin, and thermosetting polyurethane resin, as well as addition polymerization resins obtained by radical polymerization of unsaturated monomers such as thermosetting acrylic resin, vinyl ester resin, unsaturated polyester resin, and diallyl phthalate resin. These thermosetting resins may be used individually or in combination of two or more types.

[0400] Among these, if the unsaturated monomer is polyfunctional, it is desirable because the properties of a hard material (insoluble in acrylic resin, high glass transition temperature) are obtained through polymerization crosslinking. Examples of unsaturated monomers include polyesters of polyols and acrylic acid and / or methacrylic acid, and furthermore, crosslinkable monomers such as polyaryls and polyvinyl ethers of these polyols.

[0401] Examples of unsaturated monomers include, specifically, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, trimethylolpropane ethoxylate (di-, tri-)acrylate, trimethylolpropane diallyl ether, pentaerythritol trimallyl ether, pentaerythritol tetraallyl ether, di(trimethylolpropane)tetraacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate, ethoxylated pentaerythritol tetraacrylate, and mixtures thereof. Among these, trimethylolpropane triacrylate (TMPTA) and trimethylolpropane trimethacrylate (TMPTMA) are preferred as the unsaturated monomers, considering their affinity with acrylic resins.

[0402] In order to improve the scratch resistance of the first resin substrate (1), the pencil hardness of the hard resin (a) forming the resin layer (A) is preferably 3 H or higher, more preferably 4 H or higher, and even more preferably 5 H or higher.

[0403] A method for making the pencil hardness of the hard resin (a) above 3 H or higher includes a hard dispersion phase (hereinafter also referred to as "hard dispersion phase") in the matrix of the hard resin (a).

[0404] Examples of shapes of the hard dispersed phase include granular, spherical, linear, or fibrous forms, and spherical shapes are preferred from the viewpoint that they are easy to disperse evenly in the matrix of the hard resin (a), but are not limited to this.

[0405] The particle size of the hard dispersed phase is appropriately set, but 0.1 to 1000 μm is preferred.

[0406] If the particle size of the hard dispersed phase is 0.1 μm or larger, hardness can be imparted to the hard resin (a). In this regard, the particle size of the hard dispersed phase is more preferably 0.5 μm or larger, and even more preferably 1 μm or larger.

[0407] In addition, if the particle size is 1000 μm or less, the surface roughness of the resin layer (A) formed from the hard resin (a) can be reduced. Accordingly, since the surface roughness Sa of the first protective layer (3) described later is reduced, the water vapor barrier properties are improved, and the deterioration of the hologram layer (4) can be suppressed. From this perspective, the particle size of the hard dispersed phase is more preferably 500 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0408] In addition, the particle size of the hard dispersed phase can be measured, for example, by reading from an SEM image or by image analysis methods.

[0409] In addition, the amount of hard resin (a) in the hard dispersed phase is preferably 0.1 to 60 mass% of the total mass of the hard resin (a).

[0410] If the amount of hard dispersed phase is 0.1 mass% or more of the total mass of hard resin (a), hardness can be imparted to the hard resin (a). In this regard, the amount of hard dispersed phase is more preferably 0.5 mass% or more of the total mass of hard resin (a), and even more preferably 1 mass% or more.

[0411] In addition, if the amount of hard dispersed phase is 60 mass% or less of the total mass of hard resin (a), the surface roughness of the resin layer (A) formed from hard resin (a) can be reduced. In this regard, it is more preferable that the amount of hard dispersed phase is 50 mass% or less of the total mass of hard resin (a).

[0412] The method of including a hard dispersed phase in the hard resin (a) is not particularly limited, but, for example, the following methods may be used.

[0413] a) A material constituting a hard dispersed phase is added to the matrix resin material of the hard resin (a).

[0414] b) Next, when the matrix resin material is melt-kneaded and molded into a predetermined shape, the material constituting the hard dispersed phase is phase-separated and cross-linked, thereby forming a hard dispersed phase in the matrix of the hard resin (a).

[0415] Alternatively, a method may be used in which a material constituting the hard dispersed phase is cross-linked in the form of particles or the like beforehand, added to the matrix resin material, and molded into a predetermined shape by melt-kneading, thereby dispersing the hard dispersed phase in the matrix of the hard resin (a).

[0416] The hard resin (a) forming the resin layer (A) may include, in addition to the matrix resin and the hard dispersion phase, various additives such as plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, lubricants, flame retardants such as silicone compounds, fillers, glass fibers, impact-resistant modifiers, etc., to the extent that they do not impede the effects of the present invention.

[0417] The method of forming the resin layer (A) is not particularly limited as long as it can form a film, sheet, or plate, but examples include melt extrusion molding, press molding, injection molding, calendering, etc.

[0418] The thickness of the resin layer (A) forming the first resin substrate (1) is not particularly limited, but is preferably 0.05 to 5 mm.

[0419] If the thickness of the resin layer (A) is 0.05 mm or more, an improvement in scratch resistance is obtained. In this regard, the thickness of the resin layer (A) is more preferably 0.1 mm or more, and even more preferably 0.2 mm or more.

[0420] In addition, if the thickness of the resin layer (A) is 5 mm or less, the moldability becomes good. From this perspective, the thickness of the resin layer (A) is more preferably 3 mm or less, and even more preferably 2 mm or less.

[0421] (Resin layer (B))

[0422] The resin layer (B) has a different main component from the resin layer (A). By laminating the resin layer (A) and the resin layer (B), the secondary processing properties, such as impact resistance and stamping ability of the first resin substrate (1), are improved.

[0423] For the resin layer (B), it is preferable to use one or more selected from the group consisting of the acrylic resin, polycarbonate resin, polyester resin, and cycloolefin resin described above.

[0424] Among these, polycarbonate resin is preferred due to its excellent transparency, impact resistance, and moldability.

[0425] The resin layer (B) serves to impart excellent impact resistance and secondary processability, such as stamping ability, to the first resin substrate (1) by laminating it with the resin layer (A). In this regard, it is preferable to set the thickness of the resin layer (B) based on the ratio to the thickness of the resin layer (A) (or the ratio to the total thickness if there are two or more layers of the resin layer (A)).

[0426] The ratio of the thickness of the resin layer (B) to the total thickness of the resin layer (A) (thickness of resin layer (B) / total thickness of resin layer (A)) (hereinafter also simply referred to as the “thickness ratio”) is not particularly limited, but is preferably 2 or more, and more preferably 4 or more. If the thickness ratio is 2 or more, excellent impact resistance and secondary processability such as stamping can be imparted to the first resin substrate (1).

[0427] In addition, the thickness ratio is preferably 40 or less, and more preferably 20 or less. If the thickness ratio is 40 or less, deformation and bending of the first resin substrate (1) can be suppressed under usage conditions.

[0428] The laminated configuration of the resin layer (A) and the resin layer (B) is not particularly limited, but a configuration in which the resin layer (A) is laminated on both sides of the resin layer (B) is preferred.

[0429] If the laminated configuration of the resin layer (A) and the resin layer (B) is configured such that the resin layer (A) is laminated on both sides of the resin layer (B), the resin layer (A) with good scratch resistance is placed on the surface of the first resin substrate (1), thereby improving the scratch resistance of the first resin substrate (1). In addition, if the configuration is configured such that the resin layer (A) is laminated on both sides of the resin layer (B), it is desirable because bending and deformation of the first resin substrate (1) can be easily suppressed even when the first resin substrate (1) is exposed to high temperature or high temperature and high humidity for a long time.

[0430] [First adhesive layer (2)]

[0431] It is preferable to form a first adhesive layer (2) between the first resin substrate (1) and the first protective layer (3) in order to improve the adhesion between the first resin substrate (1) and the first protective layer (3) and to make the water vapor barrier properties better. In addition, if the adhesion between the first resin substrate (1) and the first protective layer (3) is good, the first adhesive layer (2) is not essential.

[0432] The preferred material, light transmittance and refractive index of the first adhesive layer (2) and the method of forming it are the same as the first anchor coat layer (2) related to the first embodiment.

[0433] The thickness of the first adhesive layer (2) is not particularly limited, but is preferably 1 to 700 μm.

[0434] Among them, in order to improve the adhesion between the first resin substrate (1) and the first protective layer (3), the thickness of the first adhesive layer (2) is more preferably 3 μm or more.

[0435] Also, from the perspective of suppressing color non-uniformity of the light guide plate (8) for image display, the thickness of the first adhesive layer (2) is more preferably 100 μm or less.

[0436] [First protective layer (3)]

[0437] The preferred oxygen permeability, water vapor permeability, and refractive index of the first protective layer (3) are the same as those of the first protective layer (3) related to the first embodiment.

[0438] The surface roughness Sa of the first protective layer (3) on the side in contact with the hologram layer (4) is less than 5.5 nm. Since the surface roughness Sa is small, the first protective layer (3) is formed uniformly, so the water vapor barrier properties are improved, and the deterioration of the hologram layer (4) can be suppressed. In this regard, the surface roughness Sa of the first protective layer (3) on the side in contact with the hologram layer (4) is preferably 5.0 nm or less with 0 nm as the lower limit, more preferably 4.5 nm or less, and even more preferably 4.0 nm or less.

[0439] The thickness of the first protective layer (3) is not particularly limited, but is preferably 10 to 200 μm.

[0440] Among them, in order to improve the mechanical strength and barrier properties of the first protective layer (3), the thickness of the first protective layer (3) is more preferably 30 μm or more.

[0441] In addition, from the perspective of improving optical properties such as total light transmittance, the thickness of the first protective layer (3) is more preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less.

[0442] The first protective layer (3) preferably comprises an inorganic material. Examples of inorganic materials include silicon oxide, silicon oxynitride, diamond-like carbon (DLC), aluminum oxide, and glass. These inorganic materials may be used individually or in combination of two or more types. In terms of ensuring good barrier properties, the first protective layer (3) preferably comprises one or more selected from the group consisting of silicon oxide and silicon oxynitride, and more preferably comprises silicon oxynitride.

[0443] If the first protective layer (3) includes silicon oxide, silicon oxynitride, DLC, or aluminum oxide, the preferred material and method of formation are the same as the first barrier layer (3) of the first embodiment.

[0444] When the first protective layer (3) is made of silicon oxide or silicon oxynitride, the thickness of the first protective layer (3) is preferably 10 to 300 nm.

[0445] Among them, in order to improve the barrier properties of the first protective layer (3), the thickness of the first protective layer (3) is more preferably 20 nm or more.

[0446] Also, in order to improve the film-forming properties of the first protective layer (3), the thickness of the first protective layer (3) is more preferably 200 nm or less.

[0447] When the first protective layer (3) is made of aluminum oxide, the thickness of the first protective layer (3) is preferably 5 to 800 nm.

[0448] When glass is used as the first protective layer (3), the material of the glass may be, for example, borosilicate glass, alkali-free glass, low-alkali glass, soda-lime glass, sol-gel glass, or glass that has undergone heat treatment or surface treatment. Alkali-free glass is particularly preferred as the glass in order to avoid discoloration caused by impurities in the glass material.

[0449] When glass is used as the first protective layer (3), the thickness of the first protective layer (3) is preferably 10 to 200 μm.

[0450] Among them, in order to improve the mechanical strength and barrier properties of the first protective layer (3), the thickness of the first protective layer (3) is more preferably 30 μm or more.

[0451] In addition, from the perspective of improving optical properties such as light transmittance, the thickness of the first protective layer (3) is more preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less.

[0452] When glass is used as the first protective layer (3), the method of forming the first protective layer (3) can be appropriately selected, and, for example, the slot-down draw method, fusion method, float method, etc. may be adopted. In addition, commercially available glass may be used as is, or commercially available glass may be polished to a desired thickness and used. Examples of commercially available glass include EAGLE2000 (manufactured by Corning), AN100 (manufactured by AGC), OA10G (manufactured by Nippon Electric Glass Co.), D263 (manufactured by Schott).

[0453] [Hologram layer (4)]

[0454] The preferred material of the hologram layer (4) is the same as the hologram layer (4) related to the first embodiment.

[0455] [Second laminate (12)]

[0456] The second laminate (12) comprises a second protective layer (5) and a second resin substrate (7) in this order. The second laminate (12) may have a second adhesive layer (6) between the second protective layer (5) and the second resin substrate (7). The various physical properties of the second laminate (12) may be different from those of the first laminate (11).

[0457] [Second adhesive layer (6)]

[0458] It is preferable to form a second adhesive layer (6) between the second protective layer (5) and the second resin substrate (7) in order to improve the adhesion between the second protective layer (5) and the second resin substrate (7) and to make the barrier properties better. In addition, if the adhesion between the second protective layer (5) and the second resin substrate (7) is good, the second adhesive layer (6) is not essential. For the second protective layer (5), the same configuration as exemplified in the description of the first protective layer (3) is used. However, the thickness and material of the second protective layer (5) may be different from those of the first protective layer (3).

[0459] [2nd Substantiation (7)]

[0460] The second resin substrate (7) is laminated on the surface of the second protective layer (5) with or without the second adhesive layer (6). The same configuration as exemplified in the description of the first resin substrate (1) is used for the second resin substrate (7). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image emission side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0461] [Light guide plate for image display (8)]

[0462] In the image display light guide plate (8), a first adhesive layer (2) and a first protective layer (3), and a second protective layer (5) and a second adhesive layer (6) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0463] Gas from the outside of the light guide plate (8) for image display passes through the first resin substrate (1) and the second resin substrate (7) to some extent, or accumulates inside. At this time, moisture is particularly likely to accumulate in the first resin substrate (1) and the second resin substrate (7).

[0464] However, according to the configuration of the present embodiment, moisture that has penetrated into the first resin substrate (1) and the second resin substrate (7) from the outside can be shielded by the first protective layer (3) and the second protective layer (5), so that the penetration of water vapor into the hologram layer (4) is suppressed, and thus the deterioration of the hologram layer (4) can be prevented.

[0465] In addition, the chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0466] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) or a decrease in clarity is likely to occur.

[0467] However, according to the configuration of the present embodiment, by forming a first protective layer (3) and a second protective layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, thereby preventing deterioration of the first resin substrate (1) and the second resin substrate (7).

[0468] [Hard Coat Layer]

[0469] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0470] The preferred material, thickness, refractive index, and method of forming the hard coat layer are the same as the hard coat layer related to the first embodiment.

[0471] In addition, the above-mentioned curable resin composition may be an organic-inorganic hybrid curable resin composition in which an inorganic component is included in the above-mentioned curable resin. Examples of the above-mentioned organic-inorganic hybrid curable resin composition include a curable resin composition in which an inorganic component having a reactive functional group is included in the above-mentioned curable resin. It is preferable to use such an inorganic component having a reactive functional group, for example, by copolymerizing and crosslinking this inorganic component with a radical polymerizable monomer, so that curing shrinkage is less likely to occur and high surface hardness can be exhibited compared to an organic-inorganic composite curable resin composition in which an inorganic component is simply included in an organic binder. Furthermore, from the perspective of reducing curing shrinkage, an organic-inorganic hybrid curable resin composition comprising UV-reactive colloidal silica as the inorganic component having a reactive functional group may be cited as a more preferred example.

[0472] Method for manufacturing a light guide plate for image display

[0473] The method for manufacturing a light guide plate for image display according to the present embodiment is the same as the method for manufacturing a light guide plate for image display related to the first embodiment.

[0474] <<6th Embodiment>>

[0475] A light guide plate for image display related to the 6th embodiment of the present invention comprises a resin substrate, a barrier layer, and a hologram layer arranged in this order, and has a mirror glossiness of 120% or more at an incident angle of 60 degrees on the side of the laminate comprising the resin substrate and the barrier layer that contacts the hologram layer.

[0476] The light guide plate for image display according to the present embodiment can suppress the deterioration of the hologram layer by providing a barrier layer. In addition, by increasing the mirror gloss of the laminate, the clarity of the light guide plate for image display is improved.

[0477] The light guide plate for image display according to the present embodiment may include at least one resin substrate selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin.

[0478] The light guide plate for image display according to the present embodiment may have the barrier layer comprising an inorganic material.

[0479] The light guide plate for image display according to the present embodiment may have at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, aluminum oxide, and glass.

[0480] The light guide plate for image display according to the present embodiment may have an anchor coat layer between the resin substrate and the barrier layer, wherein the laminate has an anchor coat layer.

[0481] The light guide plate for image display according to the present embodiment may include at least one type selected from the group consisting of acrylic resin, urethane resin, and polyester resin in the anchor coat layer.

[0482] Hereinafter, a light guide plate for image display related to the present embodiment will be described.

[0483] Light guide plate for image display

[0484] The light guide plate for image display according to the present embodiment has at least a resin substrate, a barrier layer, and a hologram layer. The resin substrate, the barrier layer, and the hologram layer are arranged in this order in the thickness direction. The resin substrate and the barrier layer may be arranged on at least one surface of the hologram layer, but may also be arranged on both surfaces of the hologram layer. When the resin substrate and the barrier layer are arranged on both surfaces of the hologram layer, the resin substrate and the barrier layer arranged on one surface of the hologram layer are respectively referred to as the first resin substrate and the first barrier layer, and the resin substrate and the barrier layer arranged on the other surface of the hologram layer are respectively referred to as the second resin substrate and the second barrier layer. In this case, the hologram layer is sandwiched between the first barrier layer and the second barrier layer, the first resin substrate is laminated on the other side of the first barrier layer, and the second resin substrate is laminated on the other side of the second barrier layer. In the present embodiment, the first resin substrate and the second resin substrate may be collectively referred to as "resin substrate" below. Also, the first barrier layer and the second barrier layer may be collectively referred to as "barrier layer" below.

[0485] One or more transparent layers may be disposed between the resin substrate and the barrier layer, and between the barrier layer and the hologram layer. Examples of transparent layers include an anchor coat layer, a hard coat layer, etc.

[0486] From the perspective of improving the adhesion between the resin substrate and the barrier layer, it is desirable to form an anchor coat layer between the resin substrate and the barrier layer. That is, it is desirable for the resin substrate, the anchor coat layer, the barrier layer, and the hologram layer to be arranged in this order.

[0487] The anchor coat layer, barrier layer, and transparent layer may be disposed on one surface of the resin substrate, but may also be disposed on both surfaces of the resin substrate. That is, the barrier layer, anchor coat layer, resin substrate, anchor coat layer, barrier layer, and hologram layer may be arranged in this order in the thickness direction, or the barrier layer, anchor coat layer, transparent layer, resin substrate, transparent layer, anchor coat layer, barrier layer, and hologram layer may be arranged in this order in the thickness direction.

[0488] [First laminate (11)]

[0489] The first laminate (11) comprises a first resin substrate (1), a first anchor coat layer (2), and a first barrier layer (3) in this order. The light guide plate (8) for image display can suppress the deterioration of the hologram layer by placing the first laminate (11) on the surface of the hologram layer (4). Additionally, if the adhesion between the first resin substrate (1) and the first barrier layer (3) is good, the first anchor coat layer (2) is not required.

[0490] The first laminate (11) transmits image light emitted from the hologram layer (4) and external light that passes through the second laminate and the hologram layer (4) described later.

[0491] The inventors have discovered that by increasing the mirror-like gloss of the first laminate (11), optical defects in the first laminate (11) are reduced, and the factors that diffuse light are reduced, so the clarity of the light guide plate (8) for image display can be improved.

[0492] In order to improve the clarity of the light guide plate (8) for image display, the mirror glossiness at an incident angle of 60 degrees on the side in contact with the hologram layer (4) of the first laminate (11) is 120% or more, preferably 130% or more, more preferably 140% or more, and even more preferably 150% or more.

[0493] In addition, the mirror glossiness in the present invention is a measured value when the angle of incidence of the light source is 60 degrees in accordance with JIS Z 8741:1997.

[0494] The total light transmittance of the first laminate (11) is not particularly limited, but is preferably 80% or more, and more preferably 90% or more. If the total light transmittance is 80% or more, the clarity and brightness values ​​of the light guide plate (8) for image display become better.

[0495] The transmittance b* value in the CIE1976 L*a*b* color space specified in JIS Z 8781-4:2013 of the first laminate (11) is not particularly limited, but is preferably 0.90 or less, more preferably 0.50 or less, even more preferably 0.40 or less, and even more preferably 0.30 or less.

[0496] The refractive index of the first laminate (11) is not particularly limited, but is preferably 1.48 or higher. If the refractive index of the first laminate (11) is 1.48 or higher, the viewing angle can be further expanded when used as a light guide plate for image display. In addition, the upper limit of the refractive index of the first laminate (11) is not particularly limited, but is typically 3.00 or lower.

[0497] In addition, the refractive index in the present invention can be measured, for example, by a refractive index measuring device (Model 2010 / M prism coupler, manufactured by Metricon Co.).

[0498] The surface roughness Sa of the side in contact with the hologram layer (4) of the first laminate (11) is not particularly limited, but is preferably 5 nm or less, more preferably 3 nm or less, even more preferably 2 nm or less, and even more preferably 1.5 nm or less. The smaller the surface roughness Sa of the side in contact with the hologram layer (4) of the first laminate (11), the more the diffusion of light due to surface irregularities can be suppressed, and the clarity of the image can be further improved.

[0499] In addition, the surface roughness Sa in the present invention is a surface roughness measured using a white interferometer (VertScan, manufactured by Ryoka Systems Co., Ltd.).

[0500] The pencil hardness of the surface on the side not in contact with the hologram layer (4) of the first laminate (11) is not particularly limited, but is preferably 3 H or higher, more preferably 4 H or higher, and even more preferably 5 H or higher. The higher the pencil hardness of the surface on the side not in contact with the hologram layer (4) of the first laminate (11), the better the scratch resistance can be imparted to the light guide plate (8) for image display.

[0501] The parallelism of the first laminate (11) in a 50 mm × 100 mm area is not particularly limited, but is preferably 0.01 to 5 μm. As the parallelism increases, the reflection angle of light becomes distorted, and as the wavelength dependence of luminance increases, the image contrast changes, causing a problem in which the image clarity is reduced. If the parallelism is within the above range, the reduction in image clarity caused by changes in image contrast can be further suppressed. The evaluation of the parallelism is performed by measurement using a Fizeau interferometer (laser interferometer).

[0502] The first laminate (11) is preferably to have at least one of oxygen barrier properties and water vapor barrier properties, and more preferably to have both, in order to prevent deterioration of the hologram layer (4).

[0503] The oxygen permeability of the first laminate (11) is not particularly limited, but is preferably 1 cm³ / m² / day / atm or less.

[0504] Also, the water vapor permeability of the first laminate (11) at 40°C and 90% is preferably 1 g / m² / day or less, more preferably 0.5 g / m² / day or less, and even more preferably 0.1 g / m² / day or less.

[0505] [First resin entry (1)]

[0506] The preferred thickness, total light transmittance, and material of the first resin substrate (1) are the same as those of the first resin substrate (1) related to the first embodiment.

[0507] The surface roughness Sa of the first resin substrate (1) is not particularly limited, but is preferably 10 nm or less, and more preferably 5 nm or less. The smaller the surface roughness Sa, the smaller the surface roughness Sa of the first laminate (11) can be, and the brightness value of the light guide plate (8) for image display becomes better.

[0508] The mirror gloss of the first resin substrate (1) is not particularly limited, but is preferably 120% or more, and more preferably 130% or more. The greater the mirror gloss, the greater the mirror gloss of the first laminate (11) can be, and the brightness value of the light guide plate (8) for image display becomes better.

[0509] The transmittance b* value in the CIE1976 L*a*b* color space specified in JIS Z 8781-4:2013 of the first resin substrate (1) is not particularly limited, but is preferably 0.50 or less, and more preferably 0.40 or less. The smaller the transmittance b* value, the smaller the transmittance b* value of the first laminate (11) can be made.

[0510] [First Anchor Coat Layer (2)]

[0511] In order to improve the adhesion between the first resin substrate (1) and the first barrier layer (3), it is preferable to form a first anchor coat layer (2) between the first resin substrate (1) and the first barrier layer (3).

[0512] The preferred material, light transmittance and refractive index of the first anchor coat layer (2) and the method of forming it are the same as the first anchor coat layer (2) related to the first embodiment.

[0513] As for the material of the first anchor coat layer (2), an acrylic resin as a thermoplastic resin is preferred in terms of water vapor barrier properties. Also, as for the material of the first anchor coat layer (2), a urethane resin or a polyester resin is preferred in terms of improving the mirror gloss of the first laminate (11).

[0514] The thickness of the first anchor coat layer (2) is not particularly limited, but, for example, may be 5 to 500 nm.

[0515] In order to improve the adhesion between the first resin substrate (1) and the first barrier layer (3), the thickness of the first anchor coat layer (2) is preferably 5 nm or more, and more preferably 10 nm or more.

[0516] Also, in order to suppress color non-uniformity of the light guide plate (8) for image display, the thickness of the first anchor coat layer (2) is preferably 500 nm or less, and more preferably 200 nm or less.

[0517] [First barrier layer (3)]

[0518] The preferred oxygen permeability, water vapor permeability, and refractive index of the first barrier layer (3) are the same as those of the first barrier layer (3) related to the first embodiment.

[0519] The first barrier layer (3) preferably comprises an inorganic material. Examples of inorganic materials include silicon oxide, silicon oxynitride, diamond-like carbon (DLC), aluminum oxide, and glass. These inorganic materials may be used individually or in combination of two or more types. In order to improve the mirror gloss and barrier properties of the first laminate (11), the first barrier layer (3) preferably comprises one or more selected from the group consisting of silicon oxide and silicon oxynitride, and it is more preferable to include silicon oxide.

[0520] If the first barrier layer (3) includes silicon oxide, silicon oxynitride, DLC, or aluminum oxide, the preferred material and method of formation are the same as the first barrier layer (3) of the first embodiment.

[0521] If the first barrier layer (3) includes silicon oxide, silicon oxynitride, or aluminum oxide, the preferred thickness is the same as the first protective layer (3) of the fifth embodiment.

[0522] In addition, when the first barrier layer (3) is formed by reactive sputtering with silicon oxide or silicon oxynitride, the total gas flow rate is preferably 150 sccm or less, more preferably 120 sccm or less, and even more preferably 90 sccm or less. If the total gas flow rate is within the above range, the mirror glossiness at an incident angle of 60 degrees on the side in contact with the hologram layer (4) of the first laminate (11) can be made higher.

[0523] If the first barrier layer (3) includes glass, the preferred material and method of formation are the same as the first protective layer (3) of the fifth embodiment.

[0524] Also, when the first barrier layer (3) is formed by glass, it may be formed on the outer side of the first resin substrate (1), that is, on the side opposite to the hologram layer (4).

[0525] [Hologram layer (4)]

[0526] The preferred material of the hologram layer (4) is the same as the hologram layer (4) related to the first embodiment.

[0527] [Second laminate]

[0528] The second laminate comprises a second barrier layer (5), a second anchor coat layer (6), and a second resin substrate (7) in this order. Additionally, if the adhesion between the second barrier layer (5) and the second resin substrate (7) is good, the second anchor coat layer (6) is not required. The various physical properties of the second laminate may be different from those of the first laminate (11).

[0529] [Second barrier layer (5)]

[0530] The second barrier layer (5) is laminated on the opposite side of the first barrier layer (3) via a hologram layer (4). The second barrier layer (5) uses the same configuration as exemplified in the description of the first barrier layer (3). However, the thickness and material of the second barrier layer (5) may be different from those of the first barrier layer (3).

[0531] [Second Anchor Coat Layer (6)]

[0532] In order to improve the adhesion between the second barrier layer (5) and the second resin substrate (7), it is preferable to form a second anchor coat layer (6) between the second barrier layer (5) and the second resin substrate (7). Additionally, if the adhesion between the second barrier layer (5) and the second resin substrate (7) is good, the second anchor coat layer (6) is not essential. For the second anchor coat layer (6), the same configuration as exemplified in the description of the first anchor coat layer (2) is used. However, the thickness, material, etc. of the second anchor coat layer (6) may be different from that of the first anchor coat layer (2).

[0533] [2nd Substantiation (7)]

[0534] The second resin substrate (7) is laminated on the surface of the second barrier layer (5) with or without the second anchor coat layer (6). The same configuration as exemplified in the description of the first resin substrate (1) is used for the second resin substrate (7). However, the thickness and material of the second resin substrate (7) may be different from that of the first resin substrate (1). In particular, since the second resin substrate (7) is placed on the surface of the external light incident side located opposite to the display image output side of the light guide plate (8) for image display, a material with a higher surface hardness than that of the first resin substrate (1) may be used.

[0535] [Light guide plate for image display (8)]

[0536] In the image display light guide plate (8), a first barrier layer (3) and a second barrier layer (5) are disposed between the first resin substrate (1) and the hologram layer (4) and between the second resin substrate (7) and the hologram layer (4), respectively.

[0537] The chemical resistance of the first resin substrate (1) and the second resin substrate (7) varies in degree depending on the type of resin material, but is significantly lower than that of glass. For this reason, the first resin substrate (1) and the second resin substrate (7) have lower solvent resistance and holographic resistance than glass.

[0538] When the first resin substrate (1) and the second resin substrate (7) are in contact with the hologram layer (4), the hologram agent, which is a component of the hologram layer (4), is likely to penetrate the first resin substrate (1) and the second resin substrate (7), or accumulate inside the first resin substrate (1) and the second resin substrate (7). When the first resin substrate (1) and the second resin substrate (7) are exposed to the hologram agent, the first resin substrate (1) and the second resin substrate (7) deteriorate, and a decrease in the FOV (Field of View) or a decrease in clarity is likely to occur.

[0539] However, according to the configuration of the present embodiment, by forming a first barrier layer (3) and a second barrier layer (5) between the first resin substrate (1) and the second resin substrate (7) and the hologram layer (4), respectively, penetration of the hologram agent into the first resin substrate (1) and the second resin substrate (7) is suppressed, so deterioration of the first resin substrate (1) and the second resin substrate (7) is prevented.

[0540] [Hard Coat Layer]

[0541] The light guide plate for image display according to the present embodiment may have a hard coat layer on one or both surfaces of the resin substrate for the purpose of increasing the pencil hardness of the surface of the resin substrate or for the purpose of reducing the surface roughness Sa of the barrier layer.

[0542] The preferred material, thickness, refractive index, and method of forming the hard coat layer are the same as the hard coat layer related to the first embodiment.

[0543] Method for manufacturing a light guide plate for image display

[0544] The method for manufacturing a light guide plate for image display according to the present embodiment is the same as the method for manufacturing a light guide plate for image display related to the first embodiment.

[0545] Examples

[0546] The present invention will be explained in more detail below through test examples and manufacturing examples. However, the present invention is not limited to the test examples and manufacturing examples described below, and various modifications are possible as long as they do not deviate from the gist of the present invention.

[0547] <<Test Example and Manufacturing Example of the First Embodiment>>

[0548] Hereinafter, the test example and manufacturing example of the first embodiment will be described.

[0549] <Test Example 1>

[0550] PMMA (polymethyl methacrylate, trade name "Acrylite" (registered trademark), manufactured by Mitsubishi Chemical Co., Ltd.) is used as the material for the resin substrate. The resin substrate is made of a rectangular plate with a width of 200 mm × a length of 200 mm × a thickness of 1 mm.

[0551] As the material for the hard coat layer, an acrylic UV-curing resin (product name "Jikou UV1700B", manufactured by Mitsubishi Chemical Co.) is used.

[0552] As the material for the anchor coat layer, an anchor coat solution 1-1 (indicated as "AC1-1" in Table 1, tanδ peak temperature: 78°C) is used, which is a mixture of an acrylic resin 1-1 and an isocyanate compound in a mass ratio of 10:1.

[0553] Silicon oxynitride is used as the material for the barrier layer.

[0554] Using the above material, a laminate is manufactured by carrying out the substrate preparation process and the barrier layer formation process described below.

[0555] [Material Preparation Process]

[0556] In the substrate preparation process, after cleaning and drying the resin substrate, a hard coat layer is formed on the resin substrate.

[0557] The resin substrate is cut into a rectangular shape of 200 mm × 200 mm and ultrasonically cleaned for 5 minutes while immersed in a 5% aqueous surfactant solution of a neutral cleaning agent (product name "Semiclean (registered trademark) M-LO", manufactured by Yokohama Yuji Kogyo Co., Ltd.).

[0558] Afterwards, the resin substrate is ultrasonically cleaned for 5 minutes while immersed in ultrapure water. Additionally, the resin substrate is rinsed with ultrapure water, and after air drying, the resin substrate is dried in an oven at 80°C under a nitrogen atmosphere. Afterwards, the air-dried evaluation sample is UV ozone cleaned in a UV ozone cleaner for 1 minute.

[0559] Next, an acrylic UV-curing resin, which is the material of the hard coat layer, is applied to both surfaces of the resin substrate using a bar coater, dried at 90°C for 1 minute, and then both surfaces are exposed to light with an integrated light intensity of 500 mJ / ㎠ to form a hard coat layer with a thickness of 5 μm.

[0560] [Barrier layer formation process]

[0561] In the barrier layer formation process, an anchor coat layer is interposed on the surface of the hard coat layer to form a barrier layer.

[0562] Anchor coat liquid 1-1 is applied to the surface of the hard coat layer using a bar coater and dried at 60°C for 1 minute to form an anchor coat layer with a thickness of 200 nm.

[0563] A silicon oxynitride film with a thickness of 100 nm is formed by a reactive sputtering method using silicon (manufactured by High Purity Chemical Research Institute Co., Ltd.) as a target, while supplying oxygen gas, nitrogen gas, and argon gas under the conditions listed in Table 1.

[0564] By the above operation, a laminate of Test Example 1 is obtained, consisting of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-1, 200 nm) / barrier layer (silicon oxynitride, 100 nm).

[0565] <Test Example 2>

[0566] In Test Example 2, the material of the anchor coat layer is an anchor coat liquid 1-2 (indicated as "AC1-2" in Table 1, tanδ peak temperature: 56°C) prepared by mixing an acrylic resin 1-2 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 1, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0567] That is, the laminate of Test Example 2 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-2, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0568] <Test Example 3>

[0569] In Test Example 3, a laminate is manufactured in the same manner as Test Example 2, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0570] That is, the laminate of Test Example 3 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-2, 50 nm) / barrier layer (silicon oxynitride, 30 nm).

[0571] <Test Example 4>

[0572] In Test Example 4, the material of the anchor coat layer is an anchor coat liquid 1-3 (indicated as "AC1-3" in Table 1, tanδ peak temperature: 32°C) prepared by mixing a polyester resin 1-1 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 1, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0573] That is, the laminate of Test Example 4 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-3, 50 nm) / barrier layer (silicon oxynitride, 40 nm).

[0574] <Test Example 5>

[0575] In Test Example 5, the material of the anchor coat layer is an anchor coat liquid 1-4 (indicated as "AC1-4" in Table 1, tanδ peak temperature: 20°C) prepared by mixing a polyester resin 1-2 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 1, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0576] That is, the laminate of Test Example 5 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-4, 25 nm) / barrier layer (silicon oxynitride, 130 nm).

[0577] <Test Example 6>

[0578] In Test Example 6, the material of the anchor coat layer is an anchor coat liquid 1-5 (indicated as "AC1-5" in Table 1, tanδ peak temperature: 72°C) prepared by mixing an acrylic resin 1-3 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 1, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0579] That is, the laminate of Test Example 6 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-5, 150 nm) / barrier layer (silicon oxynitride, 50 nm).

[0580] <Test Example 7>

[0581] In Test Example 7, a laminate is manufactured in the same manner as Test Example 4, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Table 1.

[0582] That is, the laminate of Test Example 7 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC1-3, 100 nm) / barrier layer (silicon oxynitride, 210 nm).

[0583] Table 1 shows the resin substrate material (resin substrate material), hard coat layer material (hard coat layer material), anchor coat layer material (AC layer material), barrier layer film deposition pressure (film deposition pressure [Pa]), power during film deposition (power [W]), flow rate of Ar (Ar [sccm]), flow rate of O2 (O2 [sccm]) and flow rate of N2 (N2 [sccm]), and thickness of the barrier layer (thickness [nm]) of the laminates of Test Examples 1 to 7.

[0584] Measurement and Evaluation Methods

[0585] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 1 to 7 are described.

[0586] (tanδ peak temperature)

[0587] Anchor coat liquids 1-1 to 1-5 of Test Examples 1 to 7 are dried at 80°C to produce a sheet with a thickness of 200 μm.

[0588] For the manufactured sheet, viscoelasticity measurements are performed using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) under conditions of a frequency of 1 Hz, a heating rate of 3 ℃ / min, and a measurement temperature of -50 to 200 ℃, to obtain the peak temperature [℃] of the loss tangent (tanδ).

[0589] (Elemental composition of the barrier layer)

[0590] For the laminates of Test Examples 1 to 7, the binding energy is measured by XPS (X-ray photoelectron spectroscopy) using an X-ray photoelectron spectroscopy device (K-Alpha, manufactured by Thermo Fisher Scientific), and the composition of each element [atm%] is calculated by converting from the area of ​​the peaks corresponding to Si2P, O1S, N1S, and C1S.

[0591] In the columns for “Si [atm%]”, “O [atm%]”, “N [atm%]”, and “C [atm%]” of “Barrier Layer Composition” in Table 2, the measured values ​​of each element composition [atm%] are shown.

[0592] (Total light transmittance and haze)

[0593] For the laminates of Test Examples 1 to 7, a haze meter (NDH 7000II, manufactured by Nippon Denk Industry) is installed so that the barrier layer side of the laminate becomes the light source side, and the total light transmittance [%] and haze [%] are measured using the JIS measurement method (total light transmittance: JIS K7361-1, haze: JIS 7136).

[0594] In addition, the laminates of Test Examples 1 to 7 are placed in a constant temperature and humidity chamber set to a temperature of 40 ℃ and a relative humidity of 90 %RH, and the total light transmittance [%] and haze [%] are measured in the same way after 10 days.

[0595] In the “Immediately after film formation” column of “Total light transmittance [%]” and “Haze [%]” in Table 2, the measured values ​​of total light transmittance [%] and haze [%] immediately after forming the barrier layer are shown, respectively. In addition, in the “40°C 90% 10 days later” column of “Total light transmittance [%]” and “Haze [%]”, the measured values ​​of total light transmittance [%] and haze [%] after 10 days have passed since placing the laminate in a constant temperature and humidity chamber set to conditions of a temperature of 40°C and a relative humidity of 90%RH are shown.

[0596] (b*)

[0597] For the laminates of Test Examples 1 to 7, a spectrophotometer (SD 6000, manufactured by Nippon Denk Kogyo) is used to install the laminate so that the barrier layer side is the light source side, and b* is measured under the following conditions (measurement method: transmission, specular reflection treatment: SCI, light source: C, field of view: 2°).

[0598] In addition, the laminates of Test Examples 1 to 7 are placed in a constant temperature and humidity chamber set to a temperature of 40 ℃ and a relative humidity of 90 %RH, and b* is measured in the same way after 10 days.

[0599] In the columns “Immediately after film formation” and “40°C 90% 10 days later” of “b*” in Table 2, the measured value of b* immediately after film formation of the barrier layer and the measured value of b* after 10 days have passed since placing the laminate in a constant temperature and humidity chamber set to conditions of 40°C and 90% RH relative humidity are shown, respectively.

[0600] (Water vapor barrier properties)

[0601] Using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox), the barrier layer side of the laminates of Test Examples 1 to 7 is set so that the detector side (the resin substrate side is the water vapor exposure side), and the water vapor permeability [g / m² / day] is measured under conditions of a temperature of 40°C and a relative humidity of 90%RH.

[0602] The measured value of water vapor permeability is shown in the column “Water vapor permeability [g / ㎡ / day]” of Table 2.

[0603]

[0604]

[0605] <Explanation of Results>

[0606] The laminates of Test Examples 1 to 5 have a nitrogen element composition of the barrier layer of greater than 0 atm% and less than or equal to 25 atm%, thereby obtaining good optical properties in terms of total light transmittance, haze, and b*. These laminates also have a high effect in preventing degradation caused by the hologram layer due to their low water vapor transmittance.

[0607] In addition, these laminates do not deteriorate in optical properties even when stored at 40°C and 90°F for 10 days.

[0608] <Preparation Example 1>

[0609] Below, an example of manufacturing a light guide plate (8) for image display using the laminate of Test Example 1 is shown.

[0610] In addition, as a photosensitive material for forming a hologram layer (4), 100 parts by mass of bisphenol-based epoxy resin jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical, degree of polymerization n = 10.8, epoxy equivalent: 1750 to 2200), 50 parts by mass of triethylene glycol diacrylate, 5 parts by mass of 4,4'-bis(tert-butylphenyl)iodonium hexafluorophosphate, and 0.5 parts by mass of 3,3'-carbonylbis(7-diethylamino)coumarin are mixed and dissolved in 100 parts by mass of 2-butanone (hereinafter also referred to as "photosensitive material A").

[0611] (Light guide plate manufacturing process)

[0612] In the manufacturing process of the light guide plate of Manufacturing Example 1, a light guide plate (8) for image display is manufactured using two laminates of Test Example 1.

[0613] A seal layer with a width of 5 mm and a thickness of 5 μm is applied to the perimeter edge of the barrier layer of one laminate.

[0614] The seal layer is made of a transparent material and is not particularly limited as long as it is a material capable of bonding the barrier layers of the laminate together, but in Example 1 of preparation, a photo-adhesive (manufactured by Denka Co., Ltd., product name “Hardlock (registered trademark) OP-1045K”) is used.

[0615] Thus, an intermediate body is formed in which an opening surrounded by a seal layer has a seal layer step with a size of 50 mm × 50 mm.

[0616] Afterwards, a photosensitive material A forming a hologram layer (4) is applied to the intermediate by spin coating. The photosensitive material A is applied such that its thickness after drying is 5 μm.

[0617] Afterwards, the other laminate is laminated onto the hologram layer (4) with a seal layer interposed, such that the barrier layer faces the barrier layer of the intermediate body in which the seal layer step is formed, and press-laminated under reduced pressure. The conditions for press-lamination are an absolute pressure of 5 kPa, a temperature of 70°C, and a press pressure of 0.04 MPa.

[0618] Afterwards, a diffraction grating is recorded on the press-bonded hologram layer (4). In this process, the temperature of the laminate containing the hologram layer (4) is maintained at 20°C. The diffraction grating is formed by irradiating the laminate with two laser lights and adjusting the respective irradiation angles and intensities to form an interference pattern that creates the required diffraction pattern. Thus, the diffraction grating is recorded on the hologram layer (4).

[0619] This diffraction grating is a color display diffraction grating that diffracts each of the red, green, and blue wavelength regions incident as image light in the incident section and emits them from the display section at a position corresponding to the pixel of the image light.

[0620] Afterwards, while maintaining the laminate containing the hologram layer (4) at 20°C, ultraviolet light (wavelength 365 nm, irradiance 80 W / cm²) is irradiated over the entire surface for 30 seconds from the direction of one side of the laminate. A high-pressure mercury lamp is used as the light source for the ultraviolet light.

[0621] Thus, the seal layer is hardened, and the light guide plate (8) for image display of Manufacturing Example 1 is manufactured.

[0622] <<Test Example and Manufacturing Example of the Second Embodiment>>

[0623] Hereinafter, test examples and manufacturing examples of the second embodiment will be described.

[0624] <Test Example 8>

[0625] The materials of the resin substrate, hard coat layer, and barrier layer are the same as those in Test Example 1 above.

[0626] As the material for the anchor coat layer, Anchor Coat Solution 2-1 (indicated as "AC2-1" in Table 3, tanδ peak temperature: 20°C), which is a mixture of an amorphous polyester resin and an isocyanate compound in a mass ratio of 10:1, is used.

[0627] After performing a substrate preparation process in the same manner as Test Example 1 above, a barrier layer formation process described below is performed to manufacture a laminate.

[0628] [Barrier layer formation process]

[0629] In the barrier layer formation process, an anchor coat layer is interposed on the surface of the hard coat layer to form a barrier layer.

[0630] Anchor coat liquid 2-1 is applied to the surface of the hard coat layer using a bar coater and dried at 60°C for 1 minute to form an anchor coat layer with a thickness of 25 nm.

[0631] A silicon oxynitride film with a thickness of 130 nm is formed by a reactive sputtering method using silicon (manufactured by High Purity Chemical Research Institute Co., Ltd.) as a target, while supplying oxygen gas, nitrogen gas, and argon gas under the conditions listed in Tables 3 and 4.

[0632] By the above operation, a laminate of Test Example 8 is obtained, consisting of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-1, 25 nm) / barrier layer (silicon oxynitride, 130 nm).

[0633] <Test Example 9>

[0634] In Test Example 9, a laminate is manufactured in the same manner as Test Example 8, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0635] That is, the laminate of Test Example 9 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-1, 100 nm) / barrier layer (silicon oxynitride, 50 nm).

[0636] <Test Example 10>

[0637] In Test Example 10, the material of the anchor coat layer is an anchor coat liquid 2-2 (indicated as "AC2-2" in Table 3, tanδ peak temperature: 56°C) in which an acrylic resin and an isocyanate compound are mixed in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 8, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0638] That is, the laminate of Test Example 8 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-2, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0639] <Test Example 11>

[0640] In Test Example 11, a laminate is manufactured in the same manner as Test Example 10, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0641] That is, the laminate of Test Example 11 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-2, 50 nm) / barrier layer (silicon oxynitride, 20 nm).

[0642] <Test Example 12>

[0643] In Test Example 12, the material of the anchor coat layer is an anchor coat liquid 2-3 (indicated as "AC2-3" in Table 3, tanδ peak temperature: 72°C) in which an acrylic resin and an isocyanate compound are mixed in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 8, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0644] That is, the laminate of Test Example 12 is composed of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-3, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0645] <Test Example 13>

[0646] In Test Example 13, a laminate is manufactured in the same manner as Test Example 12, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0647] That is, the laminate of Test Example 13 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-3, 50 nm) / barrier layer (silicon oxynitride, 70 nm).

[0648] <Test Example 14>

[0649] In Test Example 14, a laminate is manufactured in the same manner as Test Example 8, except that the thickness of the anchor coat layer is changed as shown in Table 3.

[0650] That is, the laminate of Test Example 14 is composed of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-1, 200 nm) / barrier layer (silicon oxynitride, 130 nm).

[0651] <Test Example 15>

[0652] In Test Example 15, a laminate is manufactured in the same manner as Test Example 11, except that the thickness of the barrier layer is changed as shown in Table 4.

[0653] That is, the laminate of Test Example 15 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-3, 100 nm) / barrier layer (silicon oxynitride, 160 nm).

[0654] <Test Example 16>

[0655] In Test Example 16, the material of the anchor coat layer is an anchor coat liquid 2-4 (indicated as "AC2-4" in Table 3, tanδ peak temperature: 82°C) in which an acrylic resin and an isocyanate compound are mixed in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 8, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 3 and 4.

[0656] That is, the laminate of Test Example 16 is composed of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC2-4, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0657] Tables 3 and 4 show the resin substrate material, hard coat layer material, anchor coat layer material and anchor coat layer thickness, barrier layer material, barrier layer deposition pressure, power during deposition, flow rates of Ar, O2 and N2, and barrier layer thickness of the laminates of Test Examples 8 to 16.

[0658] Measurement and Evaluation Methods

[0659] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 8 to 16 are described.

[0660] (tanδ peak temperature)

[0661] Anchor coat liquids 2-1 to 2-4 of Test Examples 8 to 16 are dried at 80°C to produce a sheet with a thickness of 200 μm.

[0662] For the manufactured sheet, viscoelasticity measurements are performed using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) under conditions of a frequency of 1 Hz, a heating rate of 3 ℃ / min, and a measurement temperature of -50 to 200 ℃, to obtain the peak temperature [℃] of the loss tangent (tanδ).

[0663] In the column “tanδ peak temperature [°C]” of “Anchor Coat Layer” in Table 3, the measured value of the peak temperature [°C] of the loss tangent (tanδ) is shown.

[0664] (Appearance evaluation)

[0665] For the laminates of Test Examples 8 to 16, the appearance immediately after forming the barrier layer in the barrier layer formation process is observed and evaluated according to the following criteria.

[0666] In addition, the laminates of Test Examples 8 to 16 are placed in a constant temperature and humidity chamber set to a temperature of 40°C and a relative humidity of 90%RH, and after one day, the appearance is observed and evaluated again according to the following criteria.

[0667] A (good): No cracks are visible on the surface of the barrier layer.

[0668] B (poor): Cracks are occurring on the surface of the barrier layer.

[0669] In the columns “Immediately after film formation” and “40°C 90% 1 day later” of “Appearance evaluation” in Table 4, the appearance evaluation immediately after forming the barrier layer and the appearance evaluation after 1 day have passed after placing the laminate in a constant temperature and humidity chamber set to conditions of 40°C and 90% RH are shown, respectively.

[0670] (Water vapor barrier properties)

[0671] Using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox), the barrier layer side of the laminates of Test Examples 8 to 16 is set so that the detector side (the resin substrate side is the water vapor exposure side), and the water vapor permeability [g / m² / day] is measured under conditions of a temperature of 40°C and a relative humidity of 90%RH.

[0672] The measured value of water vapor permeability is shown in the column “Water vapor permeability [g / ㎡ / day]” of Table 4.

[0673]

[0674]

[0675] <Explanation of Results>

[0676] The laminates of Test Examples 8 to 13 have a barrier layer thickness of 150 nm or less, a total thickness of the anchor coat layer and the barrier layer of 300 nm or less, and also a tanδ peak temperature in the measurement of viscoelasticity of the anchor coat layer of 80 ℃ or less.

[0677] Since the thickness of the barrier layer and the total thickness of the anchor coat layer and the barrier layer are within the above range, cracks or deformation caused by residual stress due to the barrier layer formation are unlikely to occur in these laminates, so the appearance immediately after formation is good.

[0678] In addition, since the tanδ peak temperature in the measurement of the viscoelasticity of the anchor coat layer is within the above range, cracks caused by the expansion of the resin substrate in a moist heat environment are unlikely to occur in these laminates, so the appearance after 1 day at 40°C and 90°C is also good.

[0679] <Preparation Example 2>

[0680] By using the laminate of Test Example 8 and carrying out the light guide plate manufacturing process in the same way as Manufacturing Example 1, the image display light guide plate (8) of Manufacturing Example 2 is manufactured.

[0681] <<Test Example and Manufacturing Example of the Third Embodiment>>

[0682] Hereinafter, the test example and manufacturing example of the third embodiment will be described.

[0683] <Test Example 17>

[0684] The materials of the resin substrate, hard coat layer, and barrier layer are the same as those in Test Example 1 above.

[0685] As the material for the anchor coat layer, an anchor coat solution 3-1 (indicated as "AC3-1" in Table 5, tanδ peak temperature: 78°C) is used, which is a mixture of an acrylic resin 3-1 and an isocyanate compound in a mass ratio of 10:1.

[0686] After performing a substrate preparation process in the same manner as Test Example 1 above, a barrier layer formation process described below is performed to manufacture a laminate.

[0687] [Barrier layer formation process]

[0688] In the barrier layer formation process, an anchor coat layer is interposed on the surface of the hard coat layer to form a barrier layer.

[0689] Anchor coat liquid 3-1 is applied to the surface of the hard coat layer using a bar coater and dried at 60°C for 1 minute to form an anchor coat layer with a thickness of 200 nm.

[0690] A silicon oxynitride film with a thickness of 100 nm is formed by a reactive sputtering method using silicon (manufactured by High Purity Chemical Research Institute Co., Ltd.) as a target, while supplying oxygen gas, nitrogen gas, and argon gas under the conditions described in Tables 5 and 6.

[0691] By the above operation, a laminate of Test Example 17 is obtained, consisting of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-1, 200 nm) / barrier layer (silicon oxynitride, 100 nm).

[0692] <Test Example 18>

[0693] In Test Example 18, the material of the anchor coat layer is an anchor coat liquid 3-2 (indicated as "AC3-2" in Table 5, tanδ peak temperature: 56°C) prepared by mixing an acrylic resin 3-2 and an isocyanate compound in a mass ratio of 10:1, and a laminate is manufactured in the same manner as Test Example 17, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0694] That is, the laminate of Test Example 18 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-2, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0695] <Test Example 19>

[0696] In Test Example 19, a laminate is manufactured in the same manner as Test Example 18, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0697] That is, the laminate of Test Example 19 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-2, 50 nm) / barrier layer (silicon oxynitride, 30 nm).

[0698] <Test Example 20>

[0699] In Test Example 20, the material of the anchor coat layer is an anchor coat liquid 3-3 (indicated as "AC3-3" in Table 5, tanδ peak temperature: 32°C) prepared by mixing a polyester resin 3-1 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 17, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0700] That is, the laminate of Test Example 20 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-3, 50 nm) / barrier layer (silicon oxynitride, 40 nm).

[0701] <Test Example 21>

[0702] In Test Example 21, the material of the anchor coat layer is an anchor coat liquid 3-4 (indicated as "AC3-4" in Table 5, tanδ peak temperature: 20°C) prepared by mixing a polyester resin 3-2 and an isocyanate compound in a mass ratio of 10:1, and the laminate is manufactured in the same manner as Test Example 17, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0703] That is, the laminate of Test Example 21 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-4, 25 nm) / barrier layer (silicon oxynitride, 130 nm).

[0704] <Test Example 22>

[0705] In Test Example 22, a laminate is manufactured in the same manner as Test Example 20, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0706] That is, the laminate of Test Example 22 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-3, 100 nm) / barrier layer (silicon oxynitride, 210 nm).

[0707] <Test Example 23>

[0708] In Test Example 23, a laminate is manufactured in the same manner as Test Example 17, except that the thickness of the anchor coat layer, the thickness of the barrier layer, and the film formation conditions are changed as shown in Tables 5 and 6.

[0709] That is, the laminate of Test Example 23 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC3-3, 100 nm) / barrier layer (silicon oxynitride, 40 nm).

[0710] Tables 5 and 6 show the resin substrate material, hard coat layer material, anchor coat layer material and anchor coat layer thickness, barrier layer material, barrier layer deposition pressure, power during deposition, flow rates of Ar, O2 and N2, and barrier layer thickness of the laminates of Test Examples 17 to 23.

[0711] Measurement and Evaluation Methods

[0712] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 17 to 23 are described.

[0713] (tanδ peak temperature)

[0714] Anchor coat liquids 3-1 to 3-4 of Test Examples 17 to 23 are dried at 80°C to produce a sheet with a thickness of 200 μm.

[0715] For the manufactured sheet, viscoelasticity measurements are performed using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) under conditions of a frequency of 1 Hz, a heating rate of 3 ℃ / min, and a measurement temperature of -50 to 200 ℃, to obtain the peak temperature [℃] of the loss tangent (tanδ).

[0716] In the column “tanδ peak temperature [°C]” of “Anchor Coat Layer” in Table 5, the measured value of the peak temperature [°C] of the loss tangent (tanδ) is shown. Also, in the column “(A) / (B)”, the calculated value of “Anchor Coat Layer Thickness [nm] / Peak Temperature of Loss Tangent (tanδ) [°C]” is shown.

[0717] (Heize)

[0718] For the laminates of Test Examples 17 to 23, a haze meter (NDH 7000II, manufactured by Nippon Denk Industry) is installed so that the barrier layer side of the laminate becomes the light source side, and the haze [%] is measured using the JIS measurement method (Total light transmittance: JIS K7361-1, Haze: JIS 7136).

[0719] In addition, the laminates of Test Examples 17 to 23 are placed in a constant temperature and humidity chamber set to a temperature of 40°C and a relative humidity of 90%RH, and the haze [%] after 10 days is measured in the same way.

[0720] In addition, for the laminates of Test Examples 17 to 23, the change in haze (Δhaze) before and after storage is calculated.

[0721] In the column “Immediately after film formation” of “Haze [%]” in Table 6, the measured value immediately after forming the barrier layer is indicated. In addition, in the column “40°C 90% 10 days later”, the laminate is placed in a constant temperature and humidity chamber set to conditions of 40°C and 90% RH relative humidity, and the measured value is indicated after 10 days have elapsed. Furthermore, in the column “Δhaze”, the amount of change in haze before and after the above storage is indicated.

[0722] (Water vapor barrier properties)

[0723] Using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox), the barrier layer side of the laminates of Test Examples 17 to 23 is set so that the detector side (the resin substrate side is the water vapor exposure side), and the water vapor permeability [g / m² / day] is measured under conditions of a temperature of 40°C and a relative humidity of 90%RH.

[0724] The measured value of water vapor permeability is shown in the column “Water vapor permeability [g / ㎡ / day]” of Table 6.

[0725]

[0726]

[0727] <Explanation of Results>

[0728] The laminates of Test Examples 17 to 21 have an anchor coat thickness [nm] / tanδ peak temperature [°C] of 3 or less, so that deformation caused by residual stress in the barrier layer is suppressed even after 10 days at 40°C 90%, and thus optical properties do not deteriorate. These laminates also have a high effect in preventing degradation caused by the hologram layer due to their low water vapor transmittance.

[0729] <Preparation Example 3>

[0730] By using the laminate of Test Example 17 and carrying out the light guide plate manufacturing process in the same way as Manufacturing Example 1, the image display light guide plate (8) of Manufacturing Example 3 is manufactured.

[0731] <<Test Example and Manufacturing Example of the 4th Embodiment>>

[0732] Hereinafter, the test example and manufacturing example of the fourth embodiment will be described.

[0733] <Test Example 24>

[0734] The materials of the resin substrate, hard coat layer, and barrier layer are the same as those in Test Example 1 above.

[0735] As the material for the anchor coat layer, an anchor coat solution 4-1 (indicated as “AC4-1” in Table 7) is used, which is formulated by mixing polyester resin 4-1 (product name “Vylon 63SS”, manufactured by Toyobo Co., Ltd., hydroxyl group: 5 mgKOH / g) and isocyanate compound 4-1 (product name “Colonate HX”, manufactured by Tosho Co., Ltd., isocyanurate structure trimer of hexamethylene diisocyanate) such that NCO (number of isocyanate groups of isocyanate compound 4-1) / OH (number of hydroxyl groups of polyester resin 4-1) = 1 (molar ratio).

[0736] After performing a substrate preparation process in the same manner as Test Example 1 above, a barrier layer formation process described below is performed to manufacture a laminate.

[0737] [Barrier layer formation process]

[0738] In the barrier layer formation process, an anchor coat layer is interposed on the surface of the hard coat layer to form a barrier layer.

[0739] Anchor coat liquid 4-1 is applied to the surface of the hard coat layer using a bar coater and dried at 60°C for 1 minute to form an anchor coat layer with a thickness of 25 nm.

[0740] A silicon oxynitride film with a thickness of 130 nm is formed by a reactive sputtering method using silicon (manufactured by High Purity Chemical Research Institute Co., Ltd.) as a target, while supplying oxygen gas, nitrogen gas, and argon gas under the conditions listed in Table 7.

[0741] By the above operation, a laminate of Test Example 24 is obtained, consisting of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC4-1, 25 nm) / barrier layer (silicon oxynitride, 130 nm).

[0742] <Test Example 25>

[0743] In Test Example 25, the material of the anchor coat layer is an acrylic resin 4-1 (product name "Acrite 6AN-6000", manufactured by Taisei Fine Chemical Co., Ltd., hydroxyl group: 108 mgKOH / g) and an isocyanate compound 4-1, and an anchor coat liquid 4-2 (indicated as "AC4-2" in Table 7) is prepared by mixing NCO (number of isocyanate groups of isocyanate compound 4-1) / OH (number of hydroxyl groups of acrylic resin 4-1) so that NCO = 1 (molar ratio), and the thickness of the anchor coat layer is 150 nm, and the thickness of the barrier layer and the film formation conditions are changed as shown in Table 7, except that a laminate is manufactured in the same manner as Test Example 24.

[0744] That is, the laminate of Test Example 25 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC4-2, 150 nm) / barrier layer (silicon oxynitride, 100 nm).

[0745] <Test Example 26>

[0746] In Test Example 26, the material of the anchor coat layer is an anchor coat solution 4-3 (indicated as “AC4-3” in Table 7) prepared by mixing acrylic resin 4-2 (product name “Acrite 6BF-400”, manufactured by Taisei Fine Chemical Co., Ltd., hydroxyl group: 59 mgKOH / g) and isocyanate compound 4-1 such that NCO (number of isocyanate groups of isocyanate compound 4-1) / OH (number of hydroxyl groups of acrylic resin 4-2) = 1 (molar ratio), the thickness of the anchor coat layer is 100 nm, and the thickness of the barrier layer and the film formation conditions are changed as shown in Table 7, except that the laminate is manufactured in the same manner as Test Example 24.

[0747] That is, the laminate of Test Example 26 is composed of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC4-3, 100 nm) / barrier layer (silicon oxynitride, 100 nm).

[0748] <Test Example 27>

[0749] In Test Example 27, the material of the anchor coat layer is an anchor coat liquid 4-4 (indicated as "AC4-4" in Table 7) in which acrylic resin 4-1 and isocyanate compound 4-1 are mixed such that NCO (number of isocyanate groups in isocyanate compound 4-1) / OH (number of hydroxyl groups in acrylic resin 4-1) = 0.5 (molar ratio), and the laminate is manufactured in the same manner as Test Example 24, except that the thickness of the barrier layer and the film formation conditions are changed as shown in Table 7.

[0750] That is, the laminate of Test Example 27 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC4-4, 25 nm) / barrier layer (silicon oxynitride, 100 nm).

[0751] <Test Example 28>

[0752] In Test Example 28, an anchor coat solution 4-5 (indicated as “AC4-5” in Table 7) is prepared by mixing acrylic resin 4-1 and isocyanate compound 4-1 such that NCO (number of isocyanate groups in isocyanate compound 4-1) / OH (number of hydroxyl groups in acrylic resin 4-1) = 0.75 (molar ratio), and a laminate is manufactured in the same manner as Test Example 24, except that the thickness of the barrier layer and the film formation conditions are changed as shown in Table 7.

[0753] That is, the laminate of Test Example 28 consists of a hard coat layer / resin substrate / hard coat layer / anchor coat layer (AC4-5, 25 nm) / barrier layer (silicon oxynitride, 100 nm).

[0754] Table 7 shows the resin base material (resin base material), hard coat layer material (hard coat layer material), anchor coat layer material (AC layer material), molar ratio of isocyanate groups of the isocyanate compound to hydroxyl groups of the binder resin in the anchor coat layer (NCO / OH), film formation pressure of the barrier layer (film formation pressure [Pa]), power during film formation (power [W]), flow rate of Ar (Ar [sccm]), flow rate of O2 (O2 [sccm]) and flow rate of N2 (N2 [sccm]), and thickness of the barrier layer (thickness [nm]).

[0755] Measurement and Evaluation Methods

[0756] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 24 to 28 are described.

[0757] (Elemental composition of the barrier layer)

[0758] For the laminates of Test Examples 24 to 28, the binding energy is measured by XPS (X-ray photoelectron spectroscopy) using an X-ray photoelectron spectroscopy device (K-Alpha, manufactured by Thermo Fisher Scientific), and the composition of each element [atm%] is calculated by converting from the area of ​​the peaks corresponding to Si2P, O1S, N1S, and C1S.

[0759] In the columns for “Si [atm%]”, “O [atm%]”, “N [atm%]”, and “C [atm%]” of “Barrier Layer Composition” in Table 8, the measured values ​​of each element composition [atm%] are shown.

[0760] (Content)

[0761] The solvent resistance test is performed using the RT-300 friction fastness tester manufactured by Daiei Kagaku Seikisakusho. A flat test stand is installed on the test machine, and the laminates of Test Examples 24 to 28, cut into a short sheet shape with a width of 2 cm and a length of 20 cm, are set on the test stand with the barrier layer side facing upward. One wiping cloth (Hashimoto Cloth Co., Ltd. N2325) is set to cover the friction surface of the friction element of the test machine, and an 800 g load weight is attached to the friction element (a total load of 1 kg, consisting of 200 g for the friction element and 800 g for the weight). Isopropyl alcohol (IPA) is applied to the barrier layer surface of a laminated structure, a friction element is lowered onto the barrier layer surface, and the barrier layer surface is observed after 10 reciprocating movements using a scanning white interference microscope (VertScan) manufactured by Hitachi High-Tech Science Co., Ltd., and the solvent resistance is evaluated according to the following criteria.

[0762] A (good): No peeling of the barrier layer is visible.

[0763] B (poor): Delamination of the barrier layer is visible.

[0764] The evaluation results are shown in the column "Content Quality" of Table 8.

[0765] (Water vapor barrier properties)

[0766] Using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox), the barrier layer side of the laminates of Test Examples 24 to 28 is set so that the detector side (the resin substrate side is the water vapor exposure side), and the water vapor permeability [g / m² / day] is measured under conditions of a temperature of 40°C and a relative humidity of 90%RH.

[0767] The measured value of water vapor permeability is shown in the column “Water vapor permeability [g / ㎡ / day]” of Table 8.

[0768]

[0769]

[0770] <Explanation of Results>

[0771] The laminates of Test Examples 24 to 26 have an NCO / OH ratio of 0.8 or higher in the anchor coat layer, which increases the crosslinking density of the anchor coat layer and thus increases resistance to solvents, thereby suppressing peeling of the barrier layer during the solvent resistance test. Since these laminates have a low water vapor permeability, they also have a high effect in preventing degradation caused by the hologram layer.

[0772] <Preparation Example 4>

[0773] By using the laminate of Test Example 24 and carrying out the light guide plate manufacturing process in the same way as Manufacturing Example 1, the light guide plate (8) for image display of Manufacturing Example 4 is manufactured.

[0774] <<Test Example and Manufacturing Example of the 5th Embodiment>>

[0775] Hereinafter, the test example and manufacturing example of the 5th embodiment will be described.

[0776] <Test Example 29>

[0777] (Manufacture of resin substrate A-1)

[0778] Pellet of an acrylic resin (manufactured by Arkema, trade name “Altuglas HT121”, matrix resin: methyl methacrylate-methyl acrylate-styrene copolymer, hard dispersed phase: TMPTA-TMPTMA polymerized cross-linked resin, hard dispersed phase diameter: 5 to 10 μm) is used as is as resin composition a-1.

[0779] The above resin composition a-1 is supplied to extruder A, melt-kneaded at 240°C in the extruder, then supplied to a T die for single layer heated to 250°C to be extruded into a sheet, and cooled and solidified to obtain a resin substrate A-1 with a thickness of 0.5 mm.

[0780] (Manufacturing of protective layer E-1)

[0781] A resin substrate A-1 is cut into a rectangular shape of 200 mm × 300 mm, and by the following operation, a protective layer E-1 is manufactured by interposing an adhesive layer D-1 on one surface of the resin substrate A-1, thereby obtaining a laminate consisting of resin substrate A-1 / adhesive layer D-1 / protective layer E-1.

[0782] An ethyl acetate solution of an acrylic resin (manufactured by Taisei Fine Chemical Co., Ltd., trade name "Acrite 6BF-400"), which is the material for adhesive layer D-1, is applied using a bar coater to one surface of the resin substrate A-1, and dried at 60°C for 1 minute to produce an adhesive layer D-1 with a thickness of 100 nm. In addition, a protective layer E-1 with a thickness of 100 nm formed of silicon nitrate oxide is produced on the surface of this adhesive layer D-1 by a reactive sputtering method. The reactive sputtering method uses silicon as a target and 1.0 × 10⁻⁶ -1 The process is carried out under a vacuum of Pa while supplying oxygen gas, nitrogen gas, and argon gas. In addition, the total gas flow rate at this time is set to 70 sccm.

[0783] Table 9 shows the materials and thicknesses of the resin substrate, adhesive layer, and protective layer.

[0784] (Measurement and Evaluation)

[0785] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of resin substrate A-2 and protective layer E-1.

[0786] <Test Example 30>

[0787] (Manufacture of resin substrate A-1 / B-1 / A-1)

[0788] In Test Example 30, resin substrate A-1 and resin substrate B-1 are laminated in the order A-1 / B-1 / A-1 and used as the resin substrate.

[0789] The material of resin substrate A-1 uses the resin composition a-1 of Test Example 29.

[0790] The material of resin substrate B-1 is a resin composition b-1 obtained by mixing pellets of polycarbonate resin A (manufactured by Sumika Styron Co., Ltd., product name "CALIBRE301-4"), pellets of polycarbonate resin B (manufactured by Sumika Styron Co., Ltd., product name "SD Polycar SP3030"), and pellets of polyester resin (manufactured by SK Chemicals Co., Ltd., product name "SKYGREEN J2003") in a mass ratio of 55:25:20, and then pelletizing them using a twin-screw extruder heated to 260°C.

[0791] Resin composition a-1 and resin composition b-1 are supplied to extruders A and B, respectively, and in each extruder, after melt-kneading at 240°C and 260°C, are joined to a T die for 2 types and 3 layers heated to 250°C, extruded into a sheet to form A-1 / B-1 / A-1, and cooled and solidified to produce a resin substrate A-1 / B-1 / A-1 with a thickness of 0.8 mm (A-1: 100 μm, B-1: 600 μm).

[0792] (Manufacturing of protective layer E-1)

[0793] A resin substrate A-1 / B-1 / A-1 is cut into a rectangular shape of 200 mm × 300 mm, and a protective layer E-1 is prepared by interposing an adhesive layer D-1 on one of the resin substrates A-1 in the same manner as in Example 1, thereby obtaining a laminate consisting of resin substrate A-1 / B-1 / A-1 / adhesive layer D-1 / protective layer E-1.

[0794] Table 9 shows the materials and thicknesses of the resin substrate, adhesive layer, and protective layer.

[0795] (Measurement and Evaluation)

[0796] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of resin substrate A-1 / B-1 / A-1 / adhesive layer D-1 / protective layer E-1.

[0797] <Test Example 31>

[0798] (Manufacture of Hard Coat Layer C-1 / Resin Substrate A-1 / Hard Coat Layer C-1)

[0799] In Test Example 31, a hard coat layer C-1 is laminated on both surfaces of a resin substrate A-1.

[0800] The material of resin substrate A-1 uses the resin composition a-1 of Test Example 29.

[0801] The material for the hard coat layer C-1 is a UV-curable resin composition c-1, which is prepared by mixing 4 parts by mass of photopolymerization initiator A (manufactured by BASF, product name "Omnirad 184") and 0.5 parts by mass of leveling agent A (manufactured by Kyoei Chemical, product name "Polyflow No. 75") with 100 parts by mass of UV-curable resin composition A (manufactured by Mitsubishi Chemical, product name "Jikou UV1700B"), and dissolving and diluting the mixture with PGM (propylene glycol monomethyl ether) so that the solid content of the mixture is 40% by mass.

[0802] UV-curable resin composition c-1 is applied to both surfaces of resin substrate A-1 using a bar coater, dried at 90°C for 1 minute, and then both surfaces are exposed to an integrated light intensity of 500 mJ / ㎠ to form a hard coat layer C-1 with a thickness of 10 μm, thereby obtaining hard coat layer C-1 / resin substrate A-1 / hard coat layer C-1.

[0803] (Manufacturing of protective layer E-1)

[0804] A hard coat layer C-1 / resin substrate A-1 / hard coat layer C-1 is cut into a rectangular shape of 200 mm × 300 mm, and a protective layer E-1 is prepared by interposing an adhesive layer D-1 on one of the hard coat layers C-1 in the same manner as in Example 1, thereby obtaining a laminate consisting of a hard coat layer C-1 / resin substrate A-1 / hard coat layer C-1 / adhesive layer D-1 / protective layer E-1.

[0805] Table 9 shows the materials and thicknesses of the resin substrate, hard coat layer, adhesive layer, and protective layer.

[0806] (Measurement and Evaluation)

[0807] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of hard coat layer C-1 / resin substrate A-1 / hard coat layer C-1 / adhesive layer D-1 / protective layer E-1.

[0808] <Test Example 32>

[0809] (Manufacturing of hard coat layer C-2 / resin substrate A-1 / B-1 / A-1 / hard coat layer C-2)

[0810] In Test Example 32, resin substrate A-1 and resin substrate B-1 are laminated in the order A-1 / B-1 / A-1, and a hard coat layer C-2 is laminated on both surfaces.

[0811] Resin material A-1 / B-1 / A-1 is used as the same as Test Example 30.

[0812] The material for the hard coat layer C-2 is a UV-curable resin composition c-2, which is prepared by mixing a UV-curable resin composition A (manufactured by Mitsubishi Chemical, trade name "Jikou UV1700B") and a silica dispersion containing reactive functional groups (manufactured by Nissan Chemical, trade name "Organosilicol PGM-AC-2140Y") in a mass ratio of curable resin : silica = 50 : 50, mixing 4 parts by mass of photopolymerization initiator A (manufactured by BASF, trade name "Omnirad 184") and 0.5 parts by mass of leveling agent A (manufactured by Kyoei Chemical, trade name "Polyflow No. 75") with respect to 100 parts by mass of the solid content of the mixture, and dissolving and diluting the mixture with PGM (propylene glycol monomethyl ether) so that the solid content of the mixture is 40% by mass.

[0813] UV-curable resin composition c-2 is applied to both surfaces of resin substrate A-1 / B-1 / A-1 using a bar coater, dried at 90°C for 1 minute, and then both surfaces are exposed to an integrated light intensity of 500 mJ / ㎠ to form a hard coat layer C-2 with a thickness of 15 μm, thereby obtaining hard coat layer C-2 / resin substrate A-1 / B-1 / A-1 / hard coat layer C-2.

[0814] (Manufacturing of protective layer E-1)

[0815] Hard coat layer C-2 / resin substrate A-1 / B-1 / A-1 / hard coat layer C-2 is cut into a rectangular shape of 200 mm × 300 mm, and in the same manner as Test Example 29, an adhesive layer D-1 is interposed on one of the hard coat layers C-2 to produce a protective layer E-1, thereby obtaining a laminate consisting of hard coat layer C-2 / resin substrate A-1 / B-1 / A-1 / hard coat layer C-2 / adhesive layer D-1 / protective layer E-1.

[0816] Table 9 shows the materials and thicknesses of the resin substrate, hard coat layer, adhesive layer, and protective layer.

[0817] (Measurement and Evaluation)

[0818] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of hard coat layer C-2 / resin substrate A-1 / B-1 / A-1 / hard coat layer C-2 / adhesive layer D-1 / protective layer E-1.

[0819] <Test Example 33>

[0820] (Manufacture of resin substrate A-2)

[0821] An acrylic resin plate with a thickness of 1.5 mm (manufactured by Mitsubishi Chemical, product name "Acrylite L") is used as resin substrate A-2.

[0822] (Manufacturing of protective layer E-1)

[0823] A resin substrate A-2 is cut into a rectangular shape of 200 mm × 300 mm, and a protective layer E-1 is prepared by interposing an adhesive layer D-1 on one surface of the resin substrate A-2 in the same manner as in Test Example 29, thereby obtaining a laminate consisting of resin substrate A-2 / adhesive layer D-1 / protective layer E-1.

[0824] Table 9 shows the materials and thicknesses of the resin substrate, adhesive layer, and protective layer.

[0825] (Measurement and Evaluation)

[0826] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of resin substrate A-2 / adhesive layer D-1 / protective layer E-1.

[0827] <Test Example 34>

[0828] (Manufacture of resin substrate A-2)

[0829] An acrylic resin plate with a thickness of 1.5 mm (manufactured by Mitsubishi Chemical, product name "Acrylite L") is used as resin substrate A-2.

[0830] (Manufacturing of protective layer E-1)

[0831] A resin substrate A-2 is cut into a rectangular shape of 200 mm × 300 mm, and by the following operation, a protective layer E-1 is manufactured on one surface of the resin substrate A-2 to obtain a laminate consisting of resin substrate A-2 and protective layer E-1.

[0832] A protective layer E-1 with a thickness of 100 nm, formed of silicon nitride oxide, is prepared on one surface of the resin substrate A-2 by a reactive sputtering method. The reactive sputtering method uses silicon as a target and 1.0 × 10⁻⁶ -1 The process is carried out under a vacuum of Pa while supplying oxygen gas, nitrogen gas, and argon gas. In addition, the total gas flow rate at this time is set to 70 sccm.

[0833] Table 9 shows the material and thickness of the resin substrate and protective layer.

[0834] (Measurement and Evaluation)

[0835] Table 10 shows the pencil hardness of the resin substrate surface, the surface roughness of the resin substrate, the surface roughness of the protective layer, and the water vapor barrier properties for a laminate composed of resin substrate A-2 and protective layer E-1.

[0836] Measurement and Evaluation Methods

[0837] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 29 to 34 are described.

[0838] (Pencil hardness of the resin substrate surface)

[0839] The pencil hardness of the surface opposite to the side facing the protective layer of the resin substrate obtained in Test Examples 29 to 34 is measured in accordance with JIS K 5600-5-4: 1999. The load during the test is 750 gf.

[0840] (Surface roughness Sa)

[0841] The surface roughness Sa of the resin substrate used in Test Examples 29 to 34 and the surface roughness Sa of the side in contact with the hologram layer of the protective layer (surface roughness Sa of the protective layer) are measured using a VertScan.

[0842] Device: VertScan (Manufactured by Ryoka Systems Co., Ltd.)

[0843] Observation conditions

[0844] Objective: 5x

[0845] Wavelength Filter: 530 white

[0846] Measurement mode: wave

[0847] Field of view: 640 × 480 pixels

[0848] Scan range: 7 µm (start)

[0849] -7 µm (stop)

[0850] Lamp aperture: 50%

[0851] Contrast: 62%

[0852] Brightness: 0%

[0853] Interpretation conditions

[0854] Interpolation: Complete

[0855] Surface correction: 4th-order approximation

[0856] (Water vapor barrier properties)

[0857] The water vapor barrier properties of the laminates of Test Examples 29 to 34 are measured using a water vapor permeability measuring device (DELTAPERM, manufactured by Technolox).

[0858] Set the laminate so that the protective layer side becomes the detector side (the resin substrate side becomes the water vapor exposure side), and measure under conditions of a temperature of 40°C and a relative humidity of 90%RH.

[0859]

[0860]

[0861] <Explanation of Results>

[0862] The laminates of Test Examples 29 to 33 have a surface roughness Sa of the protective layer of less than 5.5 nm and good water vapor barrier properties. Among them, when comparing Test Example 29 and Test Example 33, the laminate of Test Example 29 uses a resin layer (A) containing a hard resin (a) having a hard dispersed phase in the matrix as the resin substrate, so the surface roughness Sa of the resin substrate is smaller and the surface roughness Sa of the protective layer is also smaller, thereby further improving the water vapor barrier properties.

[0863] In addition, the laminates of Test Examples 29 to 32 have a higher pencil hardness on the surface of the resin substrate compared to the laminate of Test Example 33, so they also have excellent scratch resistance.

[0864] <Preparation Example 5>

[0865] By using the laminate of Test Example 29 and carrying out the light guide plate manufacturing process in the same way as Manufacturing Example 1, the image display light guide plate (8) of Manufacturing Example 5 is manufactured.

[0866] <<Test Example and Manufacturing Example of the 6th Embodiment>>

[0867] Hereinafter, the test example and manufacturing example of the 6th embodiment will be described.

[0868] <Test Example 35>

[0869] The materials of the resin substrate, hard coat layer, and barrier layer are the same as those in Test Example 1 above.

[0870] As the material for the anchor coat layer, an acrylic resin ("Acrylate 6BF-400" manufactured by Taisei Fine Chemical Co., Ltd.) is used.

[0871] After performing a substrate preparation process in the same manner as Test Example 1 above, a barrier layer formation process described below is performed to manufacture a laminate.

[0872] [Barrier layer formation process]

[0873] In the barrier layer formation process, an anchor coat layer is interposed on the surface of the hard coat layer to form a barrier layer.

[0874] An acrylic resin, which is the material of the anchor coat layer, is applied to the surface of the hard coat layer using a bar coater and dried at 60°C for 1 minute to form an anchor coat layer with a thickness of 100 nm.

[0875] By reactive sputtering using silicon (manufactured by High Purity Chemical Research Institute Co., Ltd.) as a target, 1.0 × 10 -1 Under a vacuum of Pa, a silicon-nitrogen oxide film with a thickness of 100 nm is deposited while supplying oxygen gas, nitrogen gas, and argon gas. The total gas flow rate is set to 70 sccm.

[0876] <Test Example 36>

[0877] In Test Example 36, a laminate is manufactured in the same manner as in Test Example 35, except that the total gas flow rate when forming the barrier layer is 105 sccm.

[0878] <Test Example 37>

[0879] In Test Example 37, a laminate is manufactured in the same manner as Test Example 35, except that the material of the anchor coat layer is a urethane-based resin (Toyobo Corporation’s “Vylon UR-1350”).

[0880] <Test Example 38>

[0881] In Test Example 38, a laminate is manufactured in the same manner as Test Example 37, except that the total gas flow rate when forming the barrier layer is 105 sccm.

[0882] <Test Example 39>

[0883] In Test Example 39, a laminate is manufactured in the same manner as in Test Example 37, except that the drying temperature of the anchor coat layer is 40°C.

[0884] <Test Example 40>

[0885] In Test Example 40, a laminate is manufactured in the same manner as Test Example 35, except that the material of the anchor coat layer is a polyester resin (Toyobo Corporation’s “Vylon 63SS”).

[0886] <Test Example 41>

[0887] In Test Example 41, a laminate is manufactured in the same manner as Test Example 40, except that the total gas flow rate when forming the barrier layer is 105 sccm.

[0888] <Test Example 42>

[0889] In Test Example 42, a laminate is manufactured in the same manner as Test Example 40, except that the drying temperature of the anchor coat layer is 40°C.

[0890] <Test Example 43>

[0891] In Test Example 43, a laminate is manufactured in the same manner as Test Example 35, except that the drying temperature of the anchor coat layer is 40°C.

[0892] Tables 11 and 12 show the resin substrate material and plate thickness, hard coat layer material, anchor coat layer material, film thickness and drying temperature, and barrier layer material, film thickness, total gas flow rate and batch during film formation for Test Examples 35 to 43.

[0893] Measurement and Evaluation Methods

[0894] The measurement and evaluation methods for various physical property values ​​of the laminates obtained in Test Examples 35 to 43 are described.

[0895] (Measurement of surface roughness Sa)

[0896] The laminates of Test Examples 35 to 43 are used as measurement samples, and the surface roughness Sa is measured using the butt scan method.

[0897] Device: White Interferometer (VertScan, manufactured by Ryoka Systems)

[0898] Observation conditions

[0899] Objective: 5x

[0900] Wavelength Filter: 530 white

[0901] Measurement mode: wave

[0902] Field of view: 640 × 480 pixels

[0903] Scan range: 7 µm (start)

[0904] -7 µm (stop)

[0905] Lamp aperture: 50%

[0906] Contrast: 62%

[0907] Brightness: 0%

[0908] Interpretation conditions

[0909] Interpolation: Complete

[0910] Surface correction: 4th-order approximation

[0911] The measurement results of Test Examples 35 to 43 are shown in the column “Surface Roughness Sa” of Table 12.

[0912] (Measurement of mirror gloss)

[0913] The laminates of Test Examples 35 to 43 are used as measurement samples, and the specular gloss is measured using a gloss meter (manufactured by Suga Testing Machine Co., Ltd., product name: GS-4K) with the incident angle of the light source set to 60 degrees and the receiving angle of the light receiver set to 60 degrees. In addition, prior to the measurement, the device is calibrated so that the specular gloss of the black flat optical polished glass No. 2012-015-B, which serves as a gloss standard plate, is 92.2%.

[0914] The measurement results of Test Examples 35 to 43 are shown in the “Glossiness” column of Table 12.

[0915] (Measurement of transmission b* value)

[0916] The laminates of Test Examples 35 to 43 are used as measurement samples, and the transmittance b* value is measured using the spectrophotometer “SD6000” manufactured by Nippon Denk Industry Co., Ltd. with a light source of C and a viewing angle of 2 degrees.

[0917] The measurement results of Test Examples 35 to 43 are shown in the “Transmission b* Value” column of Table 12.

[0918]

[0919]

[0920] <Explanation of Results>

[0921] The laminates of Test Examples 35 to 42 have a mirror gloss of 120% or more. Since these laminates have low transmittance b*, it can be seen that they also have low yellowness.

[0922] Meanwhile, the laminate of Test Example 43 uses an acrylic resin as the anchor coat layer, and by setting the drying temperature of the anchor coat layer to 40°C, the mirror gloss becomes 100%. It can be seen that the laminate of Test Example 43 has a high transmittance b* and a strong yellowish tint.

[0923] In Test Example 43, it is believed that the acrylic resin used as the anchor coat layer does not sufficiently cure under drying conditions of 40°C for 1 minute, and since the anchor coat layer cures while being formed during the sputtering of the barrier layer, non-uniformity of the film formation occurs within the film, resulting in a decrease in mirror gloss.

[0924] <Preparation Examples 6 to 14>

[0925] By using the laminates of Test Examples 35 to 43 and carrying out the light guide plate manufacturing process in the same way as Manufacturing Example 1, the image display light guide plates (8) of Manufacturing Examples 6 to 14 are manufactured.

[0926] <Evaluation of Display Image Clarity>

[0927] The light guide plates for image display of Manufacturing Examples 6 to 14 are mounted on an image display device. The image display device is formed with an optical system that directs image light for displaying to the incident part of the light guide plate (8), a driving power source, and a circuit system that supplies image information for obtaining image light.

[0928] White images and character display images are used as input images for evaluation.

[0929] Evaluation is performed by visually determining how the white image and the character display image are seen. As for the character image, "ABCDE" within a size of 10 mm × 100 mm is displayed.

[0930] If no rainbow colors are visible in a white image and the characters are clearly visible in a character display image, it is judged as good (indicated as “A” in Table 2).

[0931] If a slight rainbow color is visible in a white image but the text is clearly visible in a text display image, it is judged as possible (fair, indicated as “B” in Table 2).

[0932] If rainbow colors are visible in at least part of the white image, and the outline of the characters is faint in the character display image, it is judged as unsuitable (no good, indicated as “C” in Table 2).

[0933] The “Sharpness” column of Table 13 shows the results of the sharpness evaluation for Preparation Examples 6 to 14.

[0934]

[0935] <Explanation of Results>

[0936] As shown in Table 13, the light guide plates for image display of Manufacturing Examples 6 to 13 can be judged to have "good" or "possible" clarity by having a mirror gloss of the laminate of 120% or more.

[0937] Meanwhile, the light guide plate for image display of Manufacturing Example 14 may be judged to have "unclear" clarity because the mirror gloss of the laminate is low at 100%.

[0938] Industrial applicability

[0939] The light guide plate for image display according to the present invention is useful for display devices for, for example, VR applications and AR applications, and is useful for display devices such as, for example, head-up displays, wearable displays, and head-mounted displays. Explanation of the symbols

[0940] 1 : First resin material 2: 1st Anchor Coat Layer 3: First barrier layer (first protective layer) 4: Holographic layer 5 : Second barrier layer (second protective layer) 6: Second anchor coat layer 7 : Second resin material 8: Light guide plate for image display 11: First laminate 12: Second laminate

Claims

Claim 1 A light guide plate for image display, comprising a first laminate having a first resin substrate, a first anchor coat layer, and a first barrier layer in this order, and a hologram layer, wherein silicon oxynitride accounts for 50 mass% or more of the total components constituting the first barrier layer, and the nitrogen element composition of the first barrier layer obtained by X-ray photoelectric molecular optics (XPS) is greater than 0 atm% and less than or equal to 25 atm%, wherein the material of the first anchor coat layer includes an acrylic resin, and furthermore, the tanδ peak temperature in the viscoelasticity measurement of the first anchor coat layer is 56 to 80 ℃. Claim 2 A light guide plate for image display according to claim 1, wherein the first resin substrate comprises at least one resin selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin resin, and polycarbonate resin. Claim 3 A light guide plate for image display according to claim 1 or 2, wherein the first laminate has a first hard coat layer on both surfaces of the first resin substrate. Claim 4 A light guide plate for image display according to claim 1 or 2, wherein the total light transmittance of the first laminate is 90% or more. Claim 5 A light guide plate for image display according to claim 1 or 2, wherein the haze of the first laminate is less than 0.1%. Claim 6 A light guide plate for image display according to claim 1 or 2, wherein the b* of the first laminate measured by a spectrophotometer is less than 0.

5. Claim 7 A light guide plate for image display according to claim 1 or 2, wherein the water vapor transmittance of the first laminate is less than 0.01 g / m² / day. Claim 8 A light guide plate for image display according to claim 1 or 2, wherein the nitrogen element composition in the first barrier layer is 2 atm% or more and 23 atm% or less. Claim 9 A light guide plate for image display according to claim 1 or 2, wherein the thickness of the first barrier layer is 130 nm or less. Claim 10 A light guide plate for image display according to claim 1 or 2, wherein the thickness of the first barrier layer is 5 nm or more. Claim 11 A light guide plate for image display according to claim 1 or 2, wherein the thickness of the first anchor coat layer is 1 to 200 nm. Claim 12 A light guide plate for image display according to claim 1 or 2, wherein the total thickness of the first anchor coat layer and the first barrier layer is 300 nm or less. Claim 13 A light guide plate for image display according to claim 1 or 2, wherein the total thickness of the first anchor coat layer and the first barrier layer is 50 nm or more.

Citation Information