Positive electrode active material, method for manufacturing the same, positive electrode containing the same AND lithium secondary battery containing the same

A three-stage calcination process addresses the structural instability of high-nickel lithium metal oxides by optimizing particle strength and distribution, resulting in improved energy density and lifespan for lithium secondary batteries.

KR103046661B1Active Publication Date: 2026-11-10POSCO FUTURE M CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020240057861
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2026-11-10
Estimated Expiration
2044-04-30

Smart Images

  • Figure 112024047559381-PAT00001_ABST
    Figure 112024047559381-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material, a method for manufacturing the same, a positive electrode containing the same, and a lithium secondary battery containing the same. Specifically, the invention relates to a positive electrode active material manufactured by mixing a ternary precursor and a lithium source followed by a tertiary calcination process, which improves the structural stability of particles, high temperature characteristics, and long life characteristics, a method for manufacturing the same, a positive electrode containing the same, and a lithium secondary battery containing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a positive electrode active material, a method for manufacturing the same, a positive electrode containing the same, and a lithium secondary battery containing the same. Specifically, the invention relates to a positive electrode active material manufactured by mixing a ternary precursor and a lithium source followed by a tertiary calcination process, which improves the structural stability of particles, high temperature characteristics, and long life characteristics, a method for manufacturing the same, a positive electrode containing the same, and a lithium secondary battery containing the same. Background Technology

[0002] To increase the utility of EVs and electronic devices, there is a simultaneous pursuit of miniaturization and high capacity in batteries. In particular, research on applying high-nickel lithium metal oxides as cathode active materials is ongoing to secure high energy density. However, the aforementioned high-nickel lithium metal oxides contain an excessive amount of nickel, which, while improving energy density, presents problems such as weak particle strength and low structural stability. Consequently, when rolled after being introduced into the electrode, the surface structure of the cathode active material frequently collapses, making lithiation and delithiation difficult and potentially leading to a significant reduction in capacity. Furthermore, during the pressurization process, particle breakage occurs simultaneously with the generation of a significant amount of fine particles, which can increase resistance and reduce lifespan characteristics.

[0003] Therefore, it is necessary to derive a high-nickel cathode active material capable of improving energy density, capacity, lifespan characteristics, and resistance characteristics while suppressing particle breakage, and a method for manufacturing the same. The problem to be solved

[0005] The technical problem that the present invention aims to solve is to provide a positive electrode active material with improved particle strength, structural stability, energy density, and lifespan characteristics.

[0006] Another technical problem that the present invention aims to solve is to provide a method for manufacturing a positive electrode active material having the aforementioned advantages, a positive electrode comprising the positive electrode active material, and a lithium secondary battery. means of solving the problem

[0007] A method for manufacturing a positive electrode active material according to one embodiment of the present invention comprises: a step of preparing a metal hydroxide precursor; a step of mixing the precursor, a lithium raw material, and a dopant to form a first mixture; and a step of calcining the first mixture in three stages in the order of a first temperature (T1) - a second temperature (T2) - a third temperature (T3); wherein T1, T2, and T3 may satisfy the following formula 1.

[0008] [Equation 1]

[0009] 55≤(|T1-T2|+|T2-T3|) / differential generation amount≤150

[0010] (The above fine particle generation amount is 67.8 kN / cm² after introducing 3.00g of cathode active material sample into a mold with a diameter of 1.3cm 2 It refers to the weight fraction of positive electrode active material particles having a particle size of less than 1 μm generated when a pellet formed by applying pressure with a certain force is crushed and then ultrasonically treated for 1 minute.

[0011] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, the T1 may be in the range of 800 to 840℃.

[0012] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, the T2 may be in the range of 850 to 1000℃.

[0013] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, the T3 may be in the range of 700 to 800℃.

[0014] A positive electrode active material according to another embodiment of the present invention may comprise a lithium transition metal oxide containing 80 to 100 mol% of nickel based on the total molar amount of the transition metal, and may satisfy Formula 2 below.

[0015] [Equation 2]

[0016] 0.6 < (Dv50 - Dn50) / Differential generation amount

[0017] (In Equation 2, Dv50 is the volume-averaged particle size of the 50% positive active material particles in the volume-based cumulative particle size distribution; Dn50 is the number-averaged particle size of the 50% positive active material particles in the number-based cumulative particle size distribution; the fine particle generation amount is 67.8 kN / cm² after introducing 3.00 g of positive active material sample into a mold with a diameter of 1.3 cm 2 It refers to the weight fraction of positive electrode active material particles having a particle size of less than 1 μm generated when a pellet formed by applying pressure with a certain force is crushed and then ultrasonically treated for 1 minute.

[0018] In a positive electrode active material according to another embodiment of the present invention, the Dv50 of the lithium transition metal oxide may be 3 to 4 μm.

[0019] In a positive electrode active material according to another embodiment of the present invention, the Dn50 of the lithium transition metal oxide may be 2.33 to 2.57 μm.

[0020] In a positive electrode active material according to another embodiment of the present invention, the volume-based cumulative particle size distribution of the lithium transition metal oxide may satisfy the following Equation 3.

[0021] [Equation 3]

[0022] 3.00≤(Dv,max-Dv,min) / Dv50≤3.50

[0023] (In Equation 3, Dv50 represents the volume-average particle size of the 50% positive active material particle in the volume-based cumulative particle size distribution, Dv,max represents the maximum particle size of the positive active material particle in the volume-based cumulative particle size distribution, and Dv,min represents the minimum particle size of the positive active material particle in the volume-based cumulative particle size distribution.)

[0024] In a positive electrode active material according to another embodiment of the present invention, the crystal grain size of the lithium transition metal oxide may be 150 to 190 nm.

[0025] In a positive electrode active material according to another embodiment of the present invention, the press density of the lithium transition metal oxide may be 2.10 to 2.50 g / cc.

[0026] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (003) plane may be 0.0735 to 0.0755.

[0027] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (101) plane may be 0.0845 to 0.0895.

[0028] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (104) plane may be 0.1005 to 0.1065.

[0029] In a positive electrode active material according to another embodiment of the present invention, the lithium transition metal oxide may include one represented by the following chemical formula 1.

[0030] [Chemical Formula 1]

[0031] Li a [Ni x Co y Mn z M w ]O2

[0032] In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤x≤1, 0≤y≤0.1, 0≤z≤0.2, 0≤w≤0.1, x+y+z+w=1, and M is Zr, Al, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.

[0033] A positive electrode according to another embodiment of the present invention may include at least one of the aforementioned positive electrode active materials.

[0034] A lithium secondary battery according to another embodiment of the present invention may include a positive electrode comprising at least one of the aforementioned positive electrode active materials. Effects of the invention

[0036] A method for manufacturing a positive electrode active material according to one embodiment of the present invention can provide a positive electrode active material exhibiting excellent particle strength, structural stability, energy density, and lifespan characteristics.

[0037] A positive electrode active material according to one embodiment of the present invention can exhibit excellent particle strength, structural stability, energy density, and lifespan characteristics.

[0038] A positive electrode and a lithium secondary battery according to another embodiment of the present invention may have excellent electrochemical characteristics such as capacity, energy density, lifespan characteristics, and resistance characteristics. Brief explanation of the drawing

[0040] Figure 1 shows the cumulative particle size distribution (number %) based on the number of particles according to the embodiments and comparative examples of the present invention. Figure 2 shows the cumulative particle size distribution (volume %) based on particle volume according to the embodiments and comparative examples of the present invention. Figure 3 shows an SEM image of the positive electrode active material according to Comparative Example 1. Figure 4 shows an SEM image of the positive electrode active material according to Comparative Example 2. Figure 5 shows an SEM image of the positive electrode active material according to Comparative Example 3. Figure 6 shows an SEM image of the positive electrode active material according to Comparative Example 4. Figure 7 shows an SEM image of the positive electrode active material according to Comparative Example 5. Figure 8 shows an SEM image of the positive electrode active material according to Example 1. Figure 9 shows an SEM image of the positive electrode active material according to Example 2. Specific details for implementing the invention

[0041] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0042] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of “comprising” specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0043] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0044] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0045] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.

[0046] A method for manufacturing a positive electrode active material according to one embodiment of the present invention will be described below.

[0047] Method for manufacturing positive electrode active material

[0048] A method for manufacturing a positive electrode active material according to one embodiment of the present invention comprises: a step of preparing a metal hydroxide precursor; a step of mixing the precursor, a lithium raw material, and a dopant to form a first mixture; and a step of calcining the first mixture in three stages in the order of a first temperature (T1) - a second temperature (T2) - a third temperature (T3); wherein T1, T2, and T3 may satisfy the following formula 1.

[0049] [Equation 1]

[0050] 55≤(|T1-T2|+|T2-T3|) / differential generation amount≤150

[0051] (The above fine particle generation amount is 67.8 kN / cm² after introducing 3.00g of cathode active material sample into a mold with a diameter of 1.3cm 2It refers to the weight fraction of positive electrode active material particles having a particle size of less than 1 μm generated when a pellet formed by applying pressure with a certain force is crushed and then ultrasonically treated for 1 minute.

[0052] Specifically, the above Equation 1 may be 70 ≤ (|T1-T2|+|T2-T3|) / differential generation amount ≤ 130, 80 ≤ (|T1-T2|+|T2-T3|) / differential generation amount ≤ 120, and 90 ≤ (|T1-T2|+|T2-T3|) / differential generation amount ≤ 110. More specifically, 90 ≤ (|T1-T2|+|T2-T3|) / differential generation amount ≤ 95.

[0053] However, when calculating the above Equation 1, the units of each factor constituting Equation 1 are not taken into account.

[0054] When the above-described Equation 1 is satisfied, the particle strength and structural stability of the manufactured cathode active material can be improved, and the amount of fine particles generated in the cathode active material can be reduced. If the amount of fine particles generated is reduced, the resistance can be maintained at a low level when applied to a battery, thereby improving lifespan characteristics. On the other hand, if the value is below the lower limit in the above-described Equation 1, the amount of fine particles generated in the cathode active material increases, which may lead to increased resistance and accelerated lifespan degradation when applied to a battery. If the value exceeds the upper limit in the above-described Equation 1, while there is the advantage of reducing the amount of fine particles generated, there may be a problem of increased energy costs incurred in the calcination process.

[0055] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, T1 may be in the range of 800 to 840°C. Specifically, T1 may be 810 to 830°C. More specifically, T1 may be 820 to 825°C.

[0056] If the above T1 falls within the aforementioned range, moisture present in the mixture or moisture generated during the reaction between the precursor and the lithium raw material can be sufficiently removed to minimize side reactions of the cathode active material, and lifespan characteristics can be improved when applied to a battery. On the other hand, if the above T1 is below the lower limit of the aforementioned range, a large amount of unformed particles may be generated, which may cause problems that reduce the quality or productivity of the cathode active material. If the above T1 exceeds the upper limit of the aforementioned range, there may be problems that increase the process costs of the manufacturing process more than necessary, and electrochemical performance may be degraded due to particle overgrowth during the formation of the single-crystal cathode active material.

[0057] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, the T2 may be in the range of 850 to 1000℃.

[0058] Specifically, the above T2 may be 850 to 950°C or 850 to 900°C. More specifically, the above T2 may be 850 to 870°C.

[0059] If the above T2 falls within the aforementioned range, the particle strength can be further improved. On the other hand, if the above T2 is below the lower limit of the aforementioned range, the particle strength may not increase sufficiently, and particle breakage may occur frequently, which may cause problems such as lifespan degradation and capacity reduction when applied to a battery. If the above T2 exceeds the upper limit of the aforementioned range, there may be a problem where the process cost is excessive compared to the effect of improving the particle strength of the cathode active material.

[0060] In the step of the three-stage calcination of the method for manufacturing a positive electrode active material according to one embodiment of the present invention, the T3 may be in the range of 700 to 800°C. Specifically, the T3 may be 720 to 780°C. More specifically, the T3 may be 740 to 750°C.

[0061] If the above T3 falls within the aforementioned range, the internal structure of the positive electrode active material is stabilized, thereby improving room temperature and high temperature life characteristics and mitigating the rate of increase in high temperature resistance. If the above T3 is below the lower limit of the aforementioned range, it may be difficult to improve the structural stability of the positive electrode active material due to abrupt changes in the calcination temperature. If the above T3 exceeds the upper limit of the aforementioned range, unexpected surface by-products may occur.

[0063] A positive active material according to another embodiment of the present invention will be described below.

[0064] positive electrode active material

[0065] A positive electrode active material according to another embodiment of the present invention comprises a lithium transition metal oxide containing 80 to 100 mol% of nickel based on the total molar amount of the transition metal, and

[0066] It may include satisfying the following Equation 2.

[0067] [Equation 2]

[0068] 0.6 < (Dv50 - Dn50) / Differential generation amount

[0069] (In Equation 2, Dv50 is the volume-averaged particle size of the 50% positive active material particles in the volume-based cumulative particle size distribution; Dn50 is the number-averaged particle size of the 50% positive active material particles in the number-based cumulative particle size distribution; the fine particle generation amount is 67.8 kN / cm² after introducing 3.00 g of positive active material sample into a mold with a diameter of 1.3 cm 2 It refers to the weight fraction of positive electrode active material particles having a particle size of less than 1 μm generated when a pellet formed by applying pressure with a certain force is crushed and then ultrasonically treated for 1 minute.

[0070] Specifically, the above Equation 2 may be 0.7 < (Dv50-Dn50) / differential generation amount and 0.8 < (Dv50-Dn50) / differential generation amount. More specifically, the above Equation 2 may be 0.8 < (Dv50-Dn50) / differential generation amount < 1.2.

[0071] However, when calculating the above Equation 2, the units of each factor constituting Equation 2 are not taken into account.

[0072] When the above Equation 2 is satisfied, a positive electrode active material with high particle strength and low fine particle generation is formed, which can improve capacity, efficiency, and lifespan characteristics when applied to a battery. On the other hand, if the above Equation 2 is not satisfied, not only is the particle distribution wide, but a large amount of secondary particles are formed in addition to single crystals, so particle breakage may occur frequently when the electrode is coated and rolled. Since the insertion and extraction of lithium are not smooth in a battery with such an electrode, the capacity may be low and the lifespan may also be significantly reduced.

[0073] In a positive electrode active material according to another embodiment of the present invention, the Dv50 of the lithium transition metal oxide may be 3 to 4 μm. Specifically, the Dv50 may be 3.5 to 4 μm or 3.58 to 3.67 μm.

[0074] If the above Dv50 falls within the aforementioned range, a high-nickel single-crystal cathode active material with high particle strength is formed, thereby ensuring high energy density and high capacity characteristics when applied to a battery. On the other hand, if the above Dv50 is below the lower limit of the aforementioned range, a large amount of fine particles is generated, which increases the resistance of the cathode active material and may lead to a problem of reduced capacity. If the above Dv50 exceeds the upper limit of the aforementioned range, secondary particles may be formed in addition to single crystals, and the probability of particle breakage may increase when rolled after coating on the electrode. Consequently, there may be a problem of reduced capacity and lifespan characteristics. Furthermore, since a large amount of coarse particles are generated, numerous large voids are distributed between particles, which may also lower the energy density.

[0075] In a positive electrode active material according to another embodiment of the present invention, the Dn50 of the lithium transition metal oxide may be 2.33 to 2.57 μm.

[0076] When the above Dn50 falls within the aforementioned range, a high-nickel single-crystal cathode active material with high particle strength can be formed. Accordingly, a battery with excellent electrochemical characteristics can be formed. If the above Dn50 is below the lower limit of the aforementioned range, a large amount of fine particles is generated, which increases the resistance of the cathode active material and may result in a problem of reduced capacity. If the above Dn50 exceeds the upper limit of the aforementioned range, secondary particles may be formed in addition to single crystals, and the probability of particle breakage may increase when rolled after coating on the electrode. Consequently, there may be a problem of reduced capacity and lifespan characteristics. Furthermore, since a large amount of coarse particles are generated, numerous large voids are distributed between particles, which may also lower the energy density.

[0077] In a positive electrode active material according to another embodiment of the present invention, the volume-based cumulative particle size distribution of the lithium transition metal oxide may satisfy the following Equation 3.

[0078] [Equation 3]

[0079] 3.00≤(Dv,max-Dv,min) / Dv50≤3.50

[0080] (In Equation 3, Dv50 represents the volume-average particle size of the 50% positive active material particle in the volume-based cumulative particle size distribution, Dv,max represents the maximum particle size of the positive active material particle in the volume-based cumulative particle size distribution, and Dv,min represents the minimum particle size of the positive active material particle in the volume-based cumulative particle size distribution.)

[0081] Specifically, the above Equation 3 may be 3.00 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.40, 3.00 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.36, 3.23 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.36, and 3.00 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.20. More specifically, the above Equation 3 may be 3.01 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.20.

[0082] When the above Equation 3 is satisfied, a positive electrode active material with a uniform particle size distribution can be obtained. On the other hand, if the upper limit of the above Equation 3 is exceeded, the particle size distribution of the positive electrode active material is uneven, and a large amount of secondary particles may be included. As a result, when applied to a battery, there may be a problem in that many particle breakages occur due to rolling, which significantly reduces capacity and lifespan.

[0083] In a positive electrode active material according to another embodiment of the present invention, the crystal grain size of the lithium transition metal oxide may be 150 to 190 nm. Specifically, the crystal grain size may be 160 to 180 nm, 165 to 178 nm, 170 to 176 nm, or 172 to 176 nm. More specifically, the crystal grain size may be 172 to 174 nm.

[0084] When the above-mentioned grain size falls within the aforementioned range, the yield strength of the grain increases, and plastic deformation can be suppressed. On the other hand, when the above-mentioned grain size is below the lower limit of the aforementioned range, it is difficult to form a single-crystal positive active material. In addition, the contact interface area between the positive active material and the electrolyte increases, which may increase the probability of side reactions occurring in the electrolyte. When the above-mentioned grain size exceeds the upper limit of the aforementioned range, there may be a problem where the capacity decreases due to the grains becoming coarse.

[0085] In a positive electrode active material according to another embodiment of the present invention, the press density of the lithium transition metal oxide may be 2.10 to 2.50 g / cc. Specifically, the press density may be 2.10 to 2.30 g / cc, 2.15 to 2.30 g / cc, 2.17 to 2.30 g / cc, or 2.17 to 2.25 g / cc. More specifically, the press density may be 2.17 to 2.20 g / cc.

[0086] If the above rolling density falls within the aforementioned range, the energy density of the positive active material may be high. On the other hand, if the above rolling density is below the lower limit of the aforementioned range, the energy density may decrease.

[0087] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (003) plane may be 0.0735 to 0.0755. More specifically, the diffraction peak full width at half maximum (FWHM) of the (003) plane may be 0.0745 to 0.0750.

[0088] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (101) plane may be 0.0845 to 0.0895. More specifically, the diffraction peak full width at half maximum (FWHM) of the (101) plane may be 0.0874 to 0.0875.

[0089] In a positive electrode active material according to another embodiment of the present invention, when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (104) plane may be 0.1005 to 0.1065. More specifically, the diffraction peak full width at half maximum (FWHM) of the (104) plane may be 0.1035 to 0.1050.

[0090] If the full width at half maximum (FWHM) of the diffraction peaks of the above (003), (101), and (104) planes falls within the aforementioned range, it may be a single-crystal anode active material with high particle strength.

[0091] In a positive electrode active material according to another embodiment of the present invention, the lithium transition metal oxide may include one represented by the following chemical formula 1.

[0092] [Chemical Formula 1]

[0093] Li a [Ni x Co y Mn z M w ]O2

[0094] In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤x≤1, 0≤y≤0.1, 0≤z≤0.2, 0≤w≤0.1, x+y+z+w=1, and M is Zr, Al, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.

[0096] A positive electrode and a lithium secondary battery according to another embodiment of the present invention will be described below.

[0097] Positive electrode and lithium secondary battery

[0098] A positive electrode according to another embodiment of the present invention may include at least one of the aforementioned positive electrode active materials.

[0099] A lithium secondary battery according to another embodiment of the present invention may include a positive electrode comprising at least one of the aforementioned positive electrode active materials.

[0101] The following describes embodiments, comparative examples, and experimental examples of the present invention. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited by the following examples. Furthermore, it is possible to implement the invention with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and such modifications may also fall within the scope of the present invention.

[0103] 1. Precursor preparation

[0104] Preparation Example 1

[0105] Water was placed in a batch reactor and stirred, the internal temperature was set to 50°C, and nitrogen gas was introduced into the reaction vessel to adjust the atmosphere to an inert atmosphere. Subsequently, an aqueous sulfate solution mixed with nickel sulfate, cobalt sulfate, manganese sulfate, and aluminum sulfate in a molar ratio of 95.5% : 2.0% : 2.0% : 0.5% was prepared, along with sodium hydroxide and ammonia water. The sodium hydroxide solution and ammonia water were introduced into the reactor to form an initial reaction atmosphere, after which the flow rate of the ammonia water was adjusted to a ratio of 1.2 to the flow rate of the metal sulfate solution. Subsequently, the dosage of the sodium hydroxide (NaOH) solution was adjusted so that the hydrogen ion concentration (pH) inside the reactor was approximately 11.8. Then, the reactants were introduced while stirring, and the inert atmosphere was maintained after introducing nitrogen gas. After the reaction was completed, the formed solution was washed and solid-liquid separated using a pressure filter (Filter Press), and a drying process was carried out.

[0107] 2. Preparation of small-particle cathode active material

[0108] Comparative Example 1 - Application of 2-stage firing (1st: 820℃ / 2nd: 740℃)

[0109] 21.81 kg of the precursor prepared in Preparation Example 1 was mixed with 10.19 kg of LiOH·H2O and 31.06 g of ZrO2, respectively, and then uniformly mixed using a mixer. The mixture was then calcined in an RHK calcination furnace where an O2 atmosphere was maintained. The mixture was recovered and placed in a mullite crucible. In an RHK calcination furnace supplied with oxygen at a flow rate of approximately 2800 L / min, the temperature was raised at 4.5 ℃ / min and maintained for 4 hours at the 820°C range, which corresponds to the first calcination temperature range. Afterward, the temperature was lowered to 740°C, which corresponds to the second calcination temperature range, at a cooling rate of 1.3°C / min and maintained for 8 hours. Subsequently, the temperature was lowered at 4.0 ℃ / min. The obtained sample was crushed using a Rotor-Mill and Jet-Mill equipment to produce a single-crystal cathode active material with a central particle size of approximately 3.6 μm.

[0110] Approximately 0.14g of Al(OH)3 and 1.95g of Co(OH)2 were mixed per 100g of single-crystal cathode active material that had undergone a disintegration process, and heat treatment was carried out in a box-shaped kiln where an O2 atmosphere was maintained. In a box-shaped kiln where O2 gas was introduced at a flow rate of 25 L / min, the temperature was raised at 3.5 ℃ / min and maintained at 680℃ for 6 hours, after which it was naturally cooled to produce a single-crystal cathode active material with a central particle size of 3.8㎛ with Al and Co coating layers formed.

[0111] Comparative Example 2 - Application of 2-stage firing (1st: 830℃ / 2nd: 740℃)

[0112] A small particle size cathode active material was prepared using the same method as Comparative Example 1, except that the first calcination temperature was 830℃.

[0113] Comparative Example 3 - Application of 2-stage firing (1st: 830℃ / 2nd: 750℃)

[0114] A small particle size cathode active material was prepared using the same method as Comparative Example 1, except that the first calcination temperature was 830℃ and the second calcination temperature was 750℃.

[0115] Comparative Example 4 - Application of 2-stage firing (1st: 840℃ / 2nd: 750℃)

[0116] A small particle size cathode active material was prepared using the same method as Comparative Example 1, except that the first calcination temperature was 840℃ and the second calcination temperature was 750℃.

[0117] Comparative Example 5 - Application of 2-stage firing (1st: 850℃ / 2nd: 750℃)

[0118] A small particle size cathode active material was prepared using the same method as Comparative Example 1, except that the first calcination temperature was 850℃ and the second calcination temperature was 750℃.

[0119] Example 1 - Application of 3-stage firing (1st: 820℃ / 2nd: 850℃ / 2nd: 740℃)

[0120] A small particle size active material was prepared using the same method as Comparative Example 1, except that the temperature was increased at a rate of 4.5 ℃ / min, maintained at 820℃ (corresponding to the first calcination temperature range) for 4 hours, then increased to 850℃ (the second calcination temperature) at a rate of 0.5 ℃ / min, and then decreased to 740℃ (the third calcination temperature) at a rate of 2 ℃ / min.

[0121] Example 2 - Application of 3-stage firing (1st: 825℃ / 2nd: 850℃ / 2nd: 745℃)

[0122] A small particle size active material was prepared using the same method as in Example 1, except that the first calcination temperature was 825℃ and the third calcination temperature was 745℃.

[0124] Experimental Example 1 - Measurement of Physical Properties

[0125] (1) Particle size measurement

[0126] The particle size distribution of the cathode active material according to the examples and comparative examples was measured using a Microtrac (S3000) instrument utilizing the laser diffraction method. The average particle size based on volume (Dv50) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. The average particle size based on the number of particles (Dn50) can be defined as the particle size corresponding to 50% of the cumulative number in the particle size distribution curve.

[0127] (2) Measurement of Press Density

[0128] The rolled density of the positive electrode active materials according to the examples and comparative examples was measured using a GEOPYC 1365 (Micromeritics) instrument. Specifically, 10 g of the positive electrode active material was placed into a cylindrical vessel, and then the mold containing the positive electrode active material was pressurized at a pressure of 108 N. Subsequently, the rolled density was calculated through the height of the pressurized sample.

[0129] (3) XRD measurement

[0130] For the cathode active materials according to the examples and comparative examples, FWHM was analyzed by extracting X-ray diffraction patterns using a D8 ENDEAVOR (BRUKER) instrument utilizing X-ray diffraction (XRD). Specifically, the cathode active material was uniformly loaded in powder form into a sample holder, and XRD analysis was performed in the 2θ region between 10 and 90 degrees at a speed of 10.7° / min, with the X-ray tube set to 45kV and 200mA. The extracted X-ray diffraction patterns were used to calculate FWHM values ​​for each crystal size and peaks (003), (101), and (104).

[0131] (4) 9 ton press measurement

[0132] After introducing 3.00g of cathode active material sample into a mold with a diameter of 1.3cm, 67.8 kN / cm 2 Pressurization was applied using force. Subsequently, the pressurized pellet-shaped cathode active material was placed in a mortar and pestle and ground to break up the clumped particles. Then, 0.01 g of the cathode active material was added to 61 mL of 10 wt% (NaPO3) as a dispersant, and ultrasonic treatment was performed for 1 minute. Afterward, a particle size distribution curve was obtained by analyzing the particle size using a Malvern (MS3000) instrument. Subsequently, the amount of fine particles generated was calculated by verifying the Dv50 value and summing the fraction of particles smaller than 1 μm based on the results.

[0134] Experimental Example 2 - Evaluation of Battery Characteristics

[0135] (1) Manufacturing of coin-type half-cells

[0136] To evaluate the physical properties and electrochemistry of the positive electrode active materials according to the examples and comparative examples, coin-type half-cells were manufactured as follows.

[0137] Specifically, a positive electrode active material slurry was prepared by adding a positive electrode active material, a polyvinylidene fluoride binder (product name: KF1120), and a carbon black conductive material to an N-methyl-2-pyrrolidone solvent in a weight ratio of 96.5:1.5:2.0.

[0138] The above slurry was coated onto an aluminum foil (Al foil, thickness: 20 μm), which serves as an anode current collector, using a doctor blade, and an anode was manufactured by drying and rolling. The loading amount of the anode was approximately 17.0 mg / cm², and the anode density after rolling was approximately 3.7 g / cm³. 3 It was.

[0139] A 2032 coin-type half-cell was manufactured by a conventional method using the above-mentioned positive electrode, a lithium metal negative electrode (thickness 200 μm, NEBA), an electrolyte, and a polyethylene separator. The electrolyte used was a mixed solution in which 1M LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethylmethyl carbonate (EMC) (mixing ratio EC:DMC:EMC = 3:4:3 volume%) together with a mixed solvent of VC (vinylene carbonate), PS (propane sulfone), and ESA (ethylene sulfate) (3.0:0.5:1 wt%).

[0140] (2) Capacity evaluation

[0141] After fabricating a lithium secondary battery half cell, a charge-discharge test was performed after aging it at 25°C for 10 hours. To evaluate the initial capacity, the reference capacity was set to 200 mAh / g, and the battery was charged to 4.3V with a constant current of 0.1C. Then, the voltage was switched to a constant voltage, and charging continued until the terminal current reached 0.05C. After charging, the battery was discharged with a constant current of 0.1C with a reference capacity of 200 mAh / g until it reached 3.0V.

[0142] (3) High temperature life evaluation

[0143] After fabricating a lithium secondary battery half cell at 45°C, it was charged to 4.3V with a constant current of 0.1C, then switched to a constant voltage and charged until the terminal current reached 0.05C. After charging, it was discharged with a constant current of 0.1C until it reached 3.0V. After the initial charge and discharge, it was charged to 4.3V with a constant current of 0.5C, then switched to a constant voltage and charged until the terminal current reached 0.05C. After charging, it was discharged with a constant current of 1.0C until it reached 3.0V, and 50 charge and discharge cycles were performed under these cycle conditions, and the capacity retention rate of the 50th cycle compared to the first cycle was calculated.

[0144]

[0145] Table 1 above shows the physical properties of the cathode active materials according to the examples and comparative examples, such as particle size, XRD measurement results, crystal grain size, rolling density, and amount of fine particles generated. According to Table 1, it was confirmed that the amount of fine particles generated in the cathode active materials prepared by Examples 1 and 2 was significantly reduced compared to the cathode active materials of Comparative Examples 1 to 5. In addition, it was confirmed that the degree of consolidation in Example 2 was slightly increased compared to Comparative Examples 1 to 5.

[0147]

[0148] Table 2 above shows the calcination conditions (temperature) and electrochemical characteristics of the examples and comparative examples. According to Table 2, it was confirmed that Examples 1 and 2, which underwent three-stage calcination, had a higher high-temperature lifespan at 45°C and a lower rate of increase in high-temperature resistance compared to Comparative Examples 1 to 5, which underwent only two-stage calcination. According to Tables 1 and 2, it can be inferred that the positive electrode active material according to the examples of the present invention has low fine particle generation and excellent high-temperature characteristics, and thus can exhibit excellent lifespan characteristics when applied to a battery.

[0149] Figure 1 shows the cumulative particle size distribution (number %) based on the number of particles according to the embodiments and comparative examples of the present invention.

[0150] Figure 2 shows the cumulative particle size distribution (volume %) based on particle volume according to the embodiments and comparative examples of the present invention.

[0151] Figure 3 shows an SEM image of the positive electrode active material according to Comparative Example 1.

[0152] Figure 4 shows an SEM image of the positive electrode active material according to Comparative Example 2.

[0153] Figure 5 shows an SEM image of the positive electrode active material according to Comparative Example 3.

[0154] Figure 6 shows an SEM image of the positive electrode active material according to Comparative Example 4.

[0155] Figure 7 shows an SEM image of the positive electrode active material according to Comparative Example 5.

[0156] Figure 8 shows an SEM image of the positive electrode active material according to Example 1.

[0157] Figure 9 shows an SEM image of the positive electrode active material according to Example 2.

[0158] According to Figure 1 above, when comparing the graphs of Comparative Examples 1 to 5, it was confirmed that the fine powder region (1 μm) tended to decrease as the firing temperature increased. Furthermore, it was confirmed that Examples 1 and 2, which applied three-stage firing, showed a significantly reduced fine powder region compared to Comparative Examples 1 to 5, which applied only two-stage firing. In other words, it was found that Examples 1 and 2 had lower fine powder generation compared to Comparative Examples 1 to 5, and therefore had higher particle strength.

[0159] According to Figure 2 above, as the firing temperature increases, the particle size distribution tends to shift slightly to the right, so it was confirmed that the particles grow significantly as the firing temperature increases. In addition, the examples with three-stage firing showed a tendency for the particle size around 10 μm to decrease and the peak intensity around Dv50 to increase compared to the comparative examples with only two-stage firing, indicating that three-stage firing is advantageous in terms of particle size control. On the other hand, in the comparative examples with two-stage firing, it was confirmed that the particle size distribution widened as the particle size around 10 μm increased with increasing firing temperature.

[0160] According to the above Figures 3 to 9, it can be observed that there is a tendency for particles to grow as the calcination temperature increases, and when comparing Comparative Examples 1 to 5, it was observed that particle growth was most severe in Comparative Example 5, which had the highest calcination temperature. However, it was confirmed that when applying three-stage calcination, it is advantageous to form a cathode active material in the form of single particles of uniform size even as the calcination temperature increases.

[0161] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

Claims

Claim 1 The method comprises the steps of: preparing a metal hydroxide precursor; mixing the precursor, a lithium raw material, and a dopant to form a first mixture; and performing a three-stage calcination of the first mixture in the order of a first temperature (T1) - a second temperature (T2) - a third temperature (T3); wherein, in the three-stage calcination step, T1 is in the range of 800 to 840℃, and T1, T2, and T3 satisfy the following Equation 1: [Equation 1] 55 ≤ (|T1-T2|+|T2-T3|) / amount of fine particles generated ≤ 150 (the amount of fine particles generated is 67.8 kN / cm² after introducing 3.00g of a positive electrode active material sample into a mold with a diameter of 1.3cm 2 A method for manufacturing a positive electrode active material, wherein the weight fraction of positive electrode active material particles having a particle size of less than 1 μm is generated when a pellet formed by applying pressure with a force is crushed and then ultrasonically treated for 1 minute. Claim 2 delete Claim 3 A method for manufacturing an anode active material according to claim 1, wherein in the step of the three-stage calcination, T2 is in the range of 850 to 1000℃. Claim 4 A method for manufacturing an anode active material according to claim 1, wherein in the step of the three-stage calcination, T3 is in the range of 700 to 800℃. Claim 5 A lithium transition metal oxide containing 80 to 100 mol% nickel based on the total molar amount of the transition metal, satisfying the following Equation 2: [Equation 2] 0.6 < (Dv50 - Dn50) / fine particle generation amount (wherein Dv50 is the volume average particle size of 50% of the positive electrode active material particles in the volume-based cumulative particle size distribution; Dn50 is the number average particle size of 50% of the positive electrode active material particles in the number-based cumulative particle size distribution; the fine particle generation amount is 67.8 kN / cm² after introducing 3.00 g of positive electrode active material sample into a mold with a diameter of 1.3 cm 2 (Refers to the weight fraction of positive active material particles having a particle size of less than 1 μm generated when a pellet formed by applying pressure with a force is crushed and then ultrasonically treated for 1 minute.) Positive active material. Claim 6 A positive active material according to claim 5, wherein the Dv50 of the lithium transition metal oxide is 3 to 4 μm. Claim 7 In claim 5, the positive active material, wherein the Dn50 of the lithium transition metal oxide is 2.33 to 2.57 μm. Claim 8 In claim 5, a positive electrode active material satisfying the following Equation 3 for the volume-based cumulative particle size distribution of the lithium transition metal oxide, [Equation 3] 3.00 ≤ (Dv,max - Dv,min) / Dv50 ≤ 3.50 (wherein Dv50 represents the volume average particle size of 50% of the positive electrode active material particles in the volume-based cumulative particle size distribution, Dv,max represents the maximum particle size of the positive electrode active material particles in the volume-based cumulative particle size distribution, and Dv,min represents the minimum particle size of the positive electrode active material particles in the volume-based cumulative particle size distribution). Claim 9 A positive active material according to claim 5, wherein the crystal grain size of the lithium transition metal oxide is 150 to 190 nm. Claim 10 A positive active material according to claim 5, wherein the press density of the lithium transition metal oxide is 2.10 to 2.50 g / cc. Claim 11 A positive active material according to claim 5, wherein when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the full width at half maximum (FWHM) of the diffraction peak of the (003) plane is 0.0735 to 0.0755. Claim 12 A positive active material according to claim 5, wherein when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the full width at half maximum (FWHM) of the diffraction peak of the (101) plane is 0.0845 to 0.0895. Claim 13 A positive active material according to claim 5, wherein when X-ray diffraction analysis (XRD) is performed on the lithium transition metal oxide, the diffraction peak full width at half maximum (FWHM) of the (104) plane is 0.1005 to 0.1065. Claim 14 In claim 5, the lithium transition metal oxide is a positive active material represented by the following chemical formula 1. [Chemical Formula 1] Li a [Ni x Co y Mn z M w ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤x≤1, 0≤y≤0.1, 0≤z≤0.2, 0≤w≤0.1, x+y+z+w=1, and M is Zr, Al, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof. Claim 15 A positive electrode comprising a positive electrode active material according to any one of paragraphs 5 to 14. Claim 16 A lithium secondary battery comprising the positive electrode of claim 15.

Citation Information

Patent Citations

  • Method for manufacturing positive electrode active material for nonaqueous electrolyte secondary battery

    JP2017188444A