Negative active material, manufacturing method thereof, negative electrode containing the same, and lithium secondary battery

A balanced mixture of natural graphites with controlled particle sizes and ratios addresses the challenges of adhesion and density in magnetic alignment, enhancing the performance of lithium secondary batteries in terms of charging speed, adhesion, and overall battery efficiency.

KR103046665B1Active Publication Date: 2026-11-11POSCO FUTURE M CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020240132625
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2026-11-11
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Existing negative electrode active materials for lithium secondary batteries face challenges in maintaining high-speed charging characteristics, electrode plate adhesion, and high electrode density, particularly when using magnetic alignment technology with natural graphite, which often results in poor adhesion and reduced density.

Method used

A negative electrode active material comprising a mixture of first and second natural graphites with specific weight and particle size ratios, controlled by equations to optimize adhesion, density, and magnetic alignment, ensuring a balanced distribution of particle sizes and sphericity to enhance electrode performance.

Benefits of technology

The solution achieves improved high-speed charging characteristics, increased electrode plate adhesion, and enhanced electrode density, leading to better battery lifespan, capacity, and output characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026012507029-PAT00001
    Figure 112026012507029-PAT00001
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material, a method for manufacturing the same, a negative electrode including the same, and a lithium secondary battery. Specifically, the invention relates to a negative electrode active material capable of preventing a decrease in electrode plate adhesion by controlling the mixing ratio of magnetically aligned bimodal natural graphite, a method for manufacturing the same, a negative electrode including the same, and a lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a negative electrode active material, a method for manufacturing the same, a negative electrode including the same, and a lithium secondary battery. Specifically, the invention relates to a negative electrode active material capable of preventing a decrease in electrode plate adhesion by controlling the mixing ratio of magnetically aligned bimodal natural graphite, a method for manufacturing the same, a negative electrode including the same, and a lithium secondary battery. Background Technology

[0002] A lithium secondary battery generally consists of a positive electrode containing a positive active material, a negative electrode containing a negative active material, a separator, and an electrolyte, and charging and discharging are performed through the intercalation and deintercalation of lithium ions. Since the lithium secondary battery possesses advantages such as high energy density, high electromotive force, and the ability to exhibit high capacity, it is being applied in various fields.

[0003] Furthermore, improving high-temperature performance, such as high-temperature storage and cycling characteristics, in lithium secondary batteries is a critical challenge. For example, there is a significant problem where the high-temperature performance of the anode is likely to deteriorate if the total internal pore volume is high after the anode active material is coated onto a current collector and rolled. Therefore, it is necessary to improve high-temperature characteristics when developing anode active materials for lithium secondary batteries, such as rapid-charge batteries, by minimizing changes in electrode structure and total internal pore volume that occur during electrode rolling.

[0004] Furthermore, as technology development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly rising. Among secondary batteries, lithium secondary batteries, which exhibit high energy density and operating potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0005] Furthermore, as interest in environmental issues grows, there is increasing interest in electric vehicles and hybrid electric vehicles that can replace fossil fuel-using vehicles, such as gasoline and diesel vehicles, which are one of the major causes of air pollution; consequently, research is actively underway to use lithium-ion batteries as a power source for the aforementioned electric vehicles and hybrid electric vehicles.

[0006] Recently, due to the rapid rise of electric vehicles (EVs), expectations for the aforementioned lithium-ion batteries are growing, and there is an increasing demand for improvements in rapid charging characteristics while preserving existing capacity. For the improvement of such rapid charging, the role of the negative electrode active material, which is responsible for storing lithium ions during charging, is becoming increasingly important.

[0007] Among carbon-based active materials, graphite-based materials such as artificial graphite and natural graphite have generally been used as negative electrode active materials for lithium-ion secondary batteries used in conventional small batteries. These materials reversibly accept or supply lithium ions while maintaining structural and electrical properties, and possess chemical potential characteristics nearly similar to metallic lithium during lithium ion insertion and extraction.

[0008] Artificial graphite has a higher charge-to-discharge efficiency than natural graphite and exhibits excellent lifespan characteristics due to less swelling during charging and discharging. However, it has a lower reversible capacity compared to natural graphite, and its hard grains make rolling difficult during electrode manufacturing. Additionally, it has the problem of poor orientation due to minimal shape change. In particular, it has the disadvantage of high manufacturing costs as it requires a high-temperature graphitization heat treatment of 3,000°C.

[0009] Meanwhile, natural graphite is widely used as a negative electrode active material because it is cheaper than synthetic graphite, has a high reversible capacity, and exhibits similar electrochemical properties.

[0010] Furthermore, various attempts have been made to improve the electrochemical properties of natural graphite, and in particular, magnetic alignment technology is sometimes introduced to enhance the fast charging characteristics of natural graphite anode active materials. Specifically, magnetic alignment technology involves adsorbing a paramagnetic material onto the graphite surface and then applying a magnetic field to control the graphite's orientation; this can improve fast charging characteristics by reducing tortuosity within the electrode. Additionally, it has the advantage of easily controlling the graphite's orientation even with a weak magnetic field.

[0011] However, applying magnetic alignment technology entails the inconvenience of having to separately remove metallic impurities such as iron (Fe), and has the disadvantage of lower electrode plate adhesion or electrode density compared to electrodes manufactured by conventional methods. Additionally, there may be difficulties in manufacturing electrodes with low loading levels.

[0012] Therefore, there is a need for a technology that can improve the high-speed charging characteristics of natural graphite by applying magnetic alignment while simultaneously maintaining good electrode plate adhesion when manufacturing electrodes. The problem to be solved

[0014] The technical problem that the present invention aims to solve is to provide a negative electrode active material that has excellent high-speed charging characteristics, electrode plate adhesion, and high electrode density even after electrode manufacturing.

[0015] Another technical problem that the present invention aims to solve is to provide a method for manufacturing a negative electrode active material having the aforementioned advantages.

[0016] Another technical problem that the present invention aims to solve is to provide a cathode comprising a cathode active material having the aforementioned advantages, and a lithium secondary battery having excellent lifespan and output characteristics including said cathode. means of solving the problem

[0018] A negative electrode active material according to one embodiment of the present invention comprises: a first natural graphite; and a second natural graphite having an average particle size (D50) smaller than that of the first natural graphite; wherein the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than or equal to 100 weight% based on 100 weight% of the total negative electrode active material, and may satisfy Formula 1 below.

[0019] [Equation 1]

[0020] A = 1.16*B +7.66*I +6.79 +ε (-4.8≤ε≤4.8)

[0021] (In the above Equation 1, A is the electrode plate adhesion strength of the negative active material expressed in units of gf / cm, B is the weight mixing ratio of the first natural graphite expressed in units of weight%, and I is m 2 They each represent the reciprocal of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 1 above, the units of each variable are not considered and are calculated as dimensionless values.)

[0022] In a negative electrode active material according to one embodiment of the present invention, the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite may be 0.1 to 0.5.

[0023] In one embodiment of the present invention, the average particle size (D50) of the first natural graphite may be 18 to 30 μm.

[0024] In one embodiment of the present invention, the average particle size (D50) of the second natural graphite may be 3 to 9 μm.

[0025] In one embodiment of the present invention, the negative electrode active material may have a SPAN ((D90-D10) / D50) value of the first natural graphite of 0.7 to 1.3.

[0026] In one embodiment of the present invention, the negative electrode active material may have a SPAN ((D90-D10) / D50) value of the second natural graphite of 0.6 to 1.2.

[0027] A negative electrode active material according to one embodiment of the present invention has a compressed density of 1.0 to 1.5 g / cm³. 3 It could be.

[0028] A negative electrode active material according to one embodiment of the present invention has a BET specific surface area of ​​1.8 to 2.5 g / cm² 3 It could be.

[0029] In one embodiment of the present invention, the degree of sphericity of the first natural graphite and the second natural graphite in the negative electrode active material may be 0.4 to 1.0.

[0030] A method for manufacturing a negative electrode active material according to another embodiment of the present invention comprises: a step of preparing a first natural graphite and a second natural graphite; and a step of mixing the first natural graphite and the second natural graphite; wherein, in the mixing step, the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than or equal to 100 weight% based on 100 weight% of the total negative electrode active material, and may satisfy Formula 2 below.

[0031] [Equation 2] 0.25≤B*D p *I≤0.6

[0032] (In the above Equation 2, B is the weight mixing ratio (weight%) of the first natural graphite expressed in weight% units, D p is g / cm 3 The compressed density I of the above-mentioned cathode active material, expressed in units of m 2 They respectively represent the reciprocals of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 2 above, the units of each variable are not considered and are calculated as dimensionless values.)

[0033] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the average particle size (D50) of the first natural graphite to a range of 18 to 30 μm in the preparation step.

[0034] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the average particle size (D50) of the second natural graphite to a range of 3 to 9 μm in the preparation step.

[0035] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite in the preparation step to a range of 0.1 to 0.5.

[0036] A method for manufacturing a cathode active material according to another embodiment of the present invention may include controlling the degree of sphericity of the first natural graphite and the second natural graphite to a range of 0.4 to 1.0 in the preparation step.

[0037] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include a magnetic field strength of 0.5 to 2.0 T applied to the first natural graphite and the second natural graphite after the mixing step.

[0038] A cathode according to another embodiment of the present invention comprises a current collector; and a cathode active material layer located on the current collector; wherein the cathode active material layer may comprise at least one of the aforementioned cathode active materials.

[0039] A lithium secondary battery according to another embodiment of the present invention may include the aforementioned negative electrode. Effects of the invention

[0041] A negative electrode active material according to one embodiment of the present invention can exhibit excellent high-speed charging characteristics, electrode plate adhesion, and high electrode density.

[0042] A method for manufacturing a negative electrode active material according to another embodiment of the present invention can provide a negative electrode active material having the aforementioned advantages.

[0043] According to another embodiment of the present invention, the negative electrode and lithium secondary battery may have improved output and lifespan characteristics of the battery by including a negative electrode active material having the aforementioned advantages. Specific details for implementing the invention

[0045] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0046] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of “comprising” specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0047] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0048] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0049] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.

[0050] In this specification, specifically, D10, D50, and D90 average particle sizes refer to particle sizes when active material particles with various particle sizes are accumulated in volume ratios of 10%, 50%, and 90%, respectively.

[0051] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.

[0052] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0054] A negative electrode active material according to one embodiment of the present invention will be described below.

[0055] 1. Cathode active material

[0056] A negative electrode active material according to one embodiment of the present invention comprises: a first natural graphite; and a second natural graphite having an average particle size (D50) smaller than that of the first natural graphite; wherein the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than or equal to 100 weight% based on 100 weight% of the total negative electrode active material, and may satisfy Formula 1 below.

[0057] [Equation 1]

[0058] A = 1.16*B +7.66*I +6.79 +ε (-4.8≤ε≤4.8)

[0059] (In the above Equation 1, A is the electrode plate adhesion strength of the negative active material expressed in units of gf / cm, B is the weight mixing ratio of the first natural graphite expressed in units of weight%, and I is m 2 They each represent the reciprocal of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 1 above, the units of each variable are not considered and are calculated as dimensionless values.)

[0060] Preferably, the weight mixing ratio of the first natural graphite may be 70 weight% or more and 90 weight% or less. More preferably, the weight mixing ratio of the first natural graphite may be 90 weight%.

[0061] Preferably, in the above Equation 1, ε can be -1≤ε≤1, -0.1≤ε≤0.1, or -0.01≤ε≤0.01.

[0062] More preferably, in the above Equation 1, ε can be -0.003≤ε≤0.003.

[0063] When the weight mixing ratio of the first natural graphite mentioned above falls within the aforementioned range, the adhesion of the negative electrode active material to the electrode plate can be maintained well even after magnetic alignment. Specifically, both the bonding between negative electrode active material particles and the adhesion between the negative electrode active material and the electrode plate are excellent, and changes in expansion caused by the insertion and extraction of lithium ions can be minimized even when charge-discharge cycles are repeated. Accordingly, the lifespan characteristics of the battery can be improved.

[0064] On the other hand, if the weight mixing ratio of the first natural graphite is below the lower limit of the aforementioned range, the content of the first natural graphite is significantly low, so a large amount of binder is used when forming the electrode. Consequently, there may be a problem in which the capacity and output characteristics of the battery are degraded.

[0065] Furthermore, if the weight mixing ratio of the first natural graphite exceeds the upper limit of the aforementioned range, the content of the second natural graphite becomes significantly lower, which may lead to a problem of reduced adhesion between the negative electrode active material particles. In addition, the adhesion between the negative electrode active material and the electrode plate decreases, and the volume change due to lithium-ion charging and discharging becomes significant, which may cause a problem of a rapid decrease in the battery's lifespan.

[0066] When the above Equation 1 satisfies the aforementioned range, the adhesion strength of the negative electrode active material to the electrode plate can be improved, and when applied to a battery, the peel strength of the negative electrode active material layer is increased, thereby increasing the durability of the negative electrode. Accordingly, the lifespan of the lithium secondary battery can be improved. In addition, the capacity, output, and energy density of the battery can also be improved.

[0067] On the other hand, if the above Equation 1 is below the lower limit of the aforementioned range, it may correspond to a case where the content of the first natural graphite is low or the BET specific surface area is significantly increased. In the former case, using a large amount of binder during electrode formation reduces not only the capacity and output characteristics of the battery but also the adhesion of the electrode plate, which may cause a problem of simultaneously degrading the capacity and lifespan characteristics of the lithium secondary battery. In the latter case, the electrolyte wettability is excellent during battery formation, resulting in high lithium ion mobility, and consequently, the capacity efficiency or output characteristics of the battery may be excellent. However, as the contact area of ​​the negative electrode active material layer with the electrolyte increases, side reactions may increase, leading to the generation of a large amount of gas and electrode delamination. In other words, there may be a problem of a rapid decrease in the battery's lifespan.

[0068] In addition, if the above Equation 1 exceeds the upper limit of the aforementioned range, it may correspond to a case where the BET specific surface area is excessively small. In such a case, since there are almost no voids between particles due to pressure during electrode formation, the permeability of the electrolyte is reduced and the lithium ion mobility decreases, which may result in a problem where the output characteristics are significantly reduced.

[0069] In a negative electrode active material according to one embodiment of the present invention, the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite may be 0.1 to 0.5.

[0070] When the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite falls within the aforementioned range, the expansion of the negative electrode active material due to lithium ion charging is suppressed, and the adhesion of the negative electrode active material to the electrode plate can be maintained well. Accordingly, the lifespan characteristics of the battery can be improved.

[0071] On the other hand, if the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite is less than the lower limit of the aforementioned range, the difference in average particle size between the bimodal natural graphite particles becomes excessively large, which may result in a problem of reduced capacity or output characteristics of the battery.

[0072] In addition, if the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite exceeds the upper limit of the aforementioned range, most of the particles constituting the negative electrode active material become coarse, so the orientation index increases, which may result in a problem where the high-speed charging characteristics are inferior. Furthermore, the void volume between particles becomes large, and the volume change due to lithium ion insertion and extraction becomes large, which may lower the electrode plate adhesion of the negative electrode active material.

[0073] In one embodiment of the present invention, the average particle size (D50) of the first natural graphite may be 18 to 30 μm.

[0074] Preferably, the average particle size (D50) of the first natural graphite may be 20 to 25 μm or 20 to 23 μm.

[0075] More preferably, the average particle size (D50) of the first natural graphite may be 21.7 μm.

[0076] In one embodiment of the present invention, the average particle size (D50) of the second natural graphite may be 3 to 9 μm.

[0077] Preferably, the average particle size (D50) of the second natural graphite may be 5 to 7 μm.

[0078] More preferably, the average particle size (D50) of the second natural graphite may be 6.8 μm.

[0079] When the average particle size (D50) of the first natural graphite and the average particle size (D50) of the second natural graphite fall within the aforementioned range, magnetic alignment can be easily performed during electrode manufacturing. In addition, the bonding between the first natural graphite and the second natural graphite particles can be maximized, and since an appropriate amount of binder is used, the adhesion to the electrode plate is maintained well, thereby improving the lifespan characteristics of the battery. Furthermore, the mobility of lithium ions can be improved, thereby improving the capacity and output characteristics of the battery.

[0080] On the other hand, if the average particle size (D50) of the first natural graphite and the second natural graphite is less than the lower limit of the aforementioned range, there may be an advantage in minimizing expansion caused by lithium ion charging by causing a decrease in the orientation degree and an increase in disorder of the natural graphite. However, since the number of natural graphite particles per unit volume of the negative electrode active material layer increases significantly, more binder is required when forming the electrode. As a result, there may be a problem in that the capacity and output characteristics of the manufactured battery are degraded. In addition, there may be a problem in that the capacity is lowered as the orientation index of the negative electrode active material decreases significantly.

[0081] Furthermore, if the average particle size (D50) of the first natural graphite and the second natural graphite exceeds the upper limit of the aforementioned range, the rate of change in expansion and contraction due to lithiation / delithiation during charging and discharging of the battery increases significantly, which can lead to rapid degradation of the negative electrode and a reduction in the battery's lifespan. Additionally, the void volume between natural graphite particles is large, and both the bonding between negative electrode active material particles and the adhesion between the negative electrode active material and the electrode plate are reduced, which may decrease the battery's lifespan. Moreover, there may be a problem where the orientation index of the negative electrode active material increases significantly, resulting in poor high-speed charging performance.

[0082] In one embodiment of the present invention, the negative electrode active material may have a SPAN ((D90-D10) / D50) value of the first natural graphite of 0.7 to 1.3.

[0083] Preferably, the SPAN((D90-D10) / D50) value of the first natural graphite may be 0.8 to 1.1.

[0084] More preferably, the SPAN((D90-D10) / D50) value of the first natural graphite may be 0.95.

[0085] In one embodiment of the present invention, the negative electrode active material may have a SPAN ((D90-D10) / D50) value of the second natural graphite of 0.6 to 1.2.

[0086] Preferably, the SPAN((D90-D10) / D50) value of the second natural graphite may be 0.7 to 0.9.

[0087] More preferably, the SPAN((D90-D10) / D50) value of the second natural graphite may be 0.81.

[0088] When the SPAN value of the first natural graphite and the SPAN value of the second natural graphite fall within the aforementioned range, a uniform negative electrode active material can be formed, and a lithium secondary battery containing the negative electrode active material can exhibit uniform electrochemical characteristics.

[0089] On the other hand, if the SPAN values ​​of the first natural graphite and the second natural graphite do not fall within the aforementioned range, there may be a problem with the quality of the battery being non-uniform. In addition, during electrode manufacturing, the bonding between negative electrode active material particles is low, and the adhesion of the negative electrode active material layer stacked on the current collector is also low, which may cause the battery life to decrease rapidly.

[0090] A negative electrode active material according to one embodiment of the present invention has a compressed density of 1.0 to 1.5 g / cm³. 3 It could be.

[0091] Preferably, the compressed density of the cathode active material is 1.08 to 1.3 g / cm³ 3 It could be.

[0092] More preferably, the compressed density of the cathode active material is 1.08 to 1.19 g / cm³ 3 It could be.

[0093] When the above-mentioned compression density falls within the aforementioned range, the expansion of the electrode due to repeated charge-discharge cycles can be minimized, and there may be advantages such as improved electrode density and increased capacity.

[0094] On the other hand, if the above-mentioned compression density is below the lower limit of the aforementioned range, there is a disadvantage that the electrode density is low and the capacity is reduced. In addition, if the above-mentioned compression density exceeds the upper limit of the aforementioned range, the penetration of the electrolyte into the negative electrode active material is not easy, which may significantly reduce lithium ion mobility. Consequently, the output and high-speed charge / discharge characteristics of the battery may be degraded.

[0095] A negative electrode active material according to one embodiment of the present invention has a BET specific surface area of ​​1.8 to 2.5 g / cm² 3 It could be.

[0096] Preferably, the BET specific surface area of ​​the cathode active material is 1.89 to 2.5 g / cm² 3 It could be.

[0097] More preferably, the BET specific surface area of ​​the cathode active material is 1.89 to 2.47 g / cm² 3 It could be.

[0098] When the above BET specific surface area falls within the aforementioned range, the negative electrode active material and the electrolyte come into proper contact, allowing for excellent lithium ion mobility. By including the above negative electrode active material, the capacity, efficiency, and high-speed charge / discharge characteristics of the battery can be improved.

[0099] If the above BET specific surface area is less than the lower limit of the aforementioned range, the penetration rate and contact of the electrolyte with respect to the negative electrode active material are reduced, so the lithium ion mobility may be significantly reduced.

[0100] Furthermore, if the above BET specific surface area exceeds the upper limit of the aforementioned range, the electrolyte wettability of the negative electrode active material may be excellent, but side reactions may also increase significantly. Consequently, there may be a problem in which the battery life characteristics rapidly deteriorate due to the generation of large amounts of gas and electrode delamination caused by repeated charge-discharge cycles.

[0101] In one embodiment of the present invention, the degree of sphericity of the first natural graphite and the second natural graphite in the negative electrode active material may be 0.4 to 1.0.

[0102] When the degree of sphericity of the first natural graphite and the second natural graphite falls within the aforementioned range, the electrode plate adhesion of the negative electrode active material is improved, and by forming a high-density electrode, there may be an advantage of improving the capacity, energy density, and lifespan characteristics of the battery.

[0103] On the other hand, if the degree of sphericity of the first natural graphite and the second natural graphite exceeds the aforementioned range, the anisotropy of the negative electrode active material increases, leading to an uneven distribution of voltage and current and an increase in resistance. In the case of a battery containing such a negative electrode active material, there may be a problem of reduced capacity and a rapid decline in lifespan.

[0105] A method for manufacturing a negative electrode active material according to another embodiment of the present invention will be described below.

[0106] 2. Method for manufacturing negative electrode active material

[0107] A method for manufacturing a negative electrode active material according to another embodiment of the present invention comprises: a step of preparing a first natural graphite and a second natural graphite; and a step of mixing the first natural graphite and the second natural graphite; wherein, in the mixing step, the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than or equal to 100 weight% based on 100 weight% of the total negative electrode active material, and may satisfy Formula 2 below.

[0108] [Equation 2] 0.25≤B*D p *I≤0.6

[0109] (In the above Equation 2, B is the weight mixing ratio (weight%) of the first natural graphite expressed in weight% units, D p is g / cm 3 The compressed density I of the above-mentioned cathode active material, expressed in units of m 2 They respectively represent the reciprocals of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 2 above, the units of each variable are not considered and are calculated as dimensionless values.)

[0110] Preferably, the weight mixing ratio of the first natural graphite may be 70 weight% or more and 90 weight% or less. More preferably, the weight mixing ratio of the first natural graphite may be 90 weight%.

[0111] Preferably, Equation 2 is 0.3 ≤ B*D p *I≤0.6, 0.33≤B*Dp I≤0.58 can be.

[0112] More preferably, Equation 2 above is 0.33725 ≤ B*D p *I≤0.57143 can be.

[0113] When the weight mixing ratio of the first natural graphite mentioned above falls within the aforementioned range, the adhesion of the negative electrode active material to the electrode plate can be maintained well even after magnetic alignment. Specifically, both the bonding between negative electrode active material particles and the adhesion between the negative electrode active material and the electrode plate are excellent, and changes in expansion caused by the insertion and extraction of lithium ions can be minimized even when charge-discharge cycles are repeated. Accordingly, the lifespan characteristics of the battery can be improved.

[0114] On the other hand, if the weight mixing ratio of the first natural graphite is below the lower limit of the aforementioned range, the content of the first natural graphite is significantly low, so a large amount of binder is used when forming the electrode. Consequently, there may be a problem in which the capacity and output characteristics of the battery are degraded.

[0115] Furthermore, if the weight mixing ratio of the first natural graphite exceeds the upper limit of the aforementioned range, the content of the second natural graphite becomes significantly lower, which may lead to a problem of reduced adhesion between the negative electrode active material particles. In addition, the adhesion between the negative electrode active material and the electrode plate decreases, and the volume change due to lithium-ion charging and discharging becomes significant, which may cause a problem of a rapid decrease in the battery's lifespan.

[0116] When the above Equation 2 satisfies the aforementioned range, the adhesion strength of the negative electrode active material to the electrode plate can be improved, and when applied to a battery, the peel strength of the negative electrode active material layer is increased, thereby increasing the durability of the negative electrode. Accordingly, the lifespan of the lithium secondary battery can be improved. In addition, the capacity, output, and energy density of the battery can also be improved.

[0117] On the other hand, if the above Equation 2 is below the lower limit of the aforementioned range, it may correspond to a case where the content of the first natural graphite is low or the BET specific surface area is significantly increased. In the former case, using a large amount of binder during electrode formation reduces not only the capacity and output characteristics of the battery but also the adhesion of the electrode plate, which may cause a problem of simultaneously degrading the capacity and lifespan characteristics of the lithium secondary battery. In the latter case, the electrolyte wettability is excellent during battery formation, resulting in high lithium ion mobility, and consequently, the capacity efficiency or output characteristics of the battery may be excellent. However, as the contact area of ​​the negative electrode active material layer with the electrolyte increases, side reactions may increase, leading to the generation of a large amount of gas and electrode delamination. In other words, there may be a problem of a rapid decrease in the battery's lifespan. Additionally, if the compression density is low, the above Equation 2 may fall below the lower limit of the aforementioned range, which may result in a problem of low energy density.

[0118] In addition, if the above Equation 2 exceeds the upper limit of the aforementioned range, it may correspond to a case where the compression density is excessively high or the BET specific surface area is excessively small. In such cases, since there are almost no voids between particles due to pressure during electrode formation, the permeability of the electrolyte is reduced and the lithium ion mobility decreases, which may result in a problem where the output characteristics are significantly reduced.

[0119] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the average particle size (D50) of the first natural graphite to a range of 18 to 30 μm in the preparation step.

[0120] Preferably, the average particle size (D50) of the first natural graphite may be 20 to 25 μm or 20 to 23 μm.

[0121] More preferably, the average particle size (D50) of the first natural graphite may be 21.7 μm.

[0122] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the average particle size (D50) of the second natural graphite to a range of 3 to 9 μm in the preparation step.

[0123] Preferably, the average particle size (D50) of the second natural graphite may be 5 to 7 μm.

[0124] More preferably, the average particle size (D50) of the second natural graphite may be 6.8 μm.

[0125] When the average particle size (D50) of the first natural graphite and the average particle size (D50) of the second natural graphite fall within the aforementioned range, magnetic alignment can be easily performed during electrode manufacturing. In addition, the bonding between the first natural graphite and the second natural graphite particles can be maximized, and since an appropriate amount of binder is used, the adhesion to the electrode plate is maintained well, thereby improving the lifespan characteristics of the battery. Furthermore, the mobility of lithium ions can be improved, thereby improving the capacity and output characteristics of the battery.

[0126] On the other hand, if the average particle size (D50) of the first natural graphite and the second natural graphite is less than the lower limit of the aforementioned range, there may be an advantage in minimizing expansion caused by lithium ion charging by causing a decrease in the orientation degree and an increase in disorder of the natural graphite. However, since the number of natural graphite particles per unit volume of the negative electrode active material layer increases significantly, more binder is required when forming the electrode. As a result, there may be a problem in that the capacity and output characteristics of the manufactured battery are degraded. In addition, there may be a problem in that the capacity is lowered as the orientation index of the negative electrode active material decreases significantly.

[0127] Furthermore, if the average particle size (D50) of the first natural graphite and the second natural graphite exceeds the upper limit of the aforementioned range, the rate of change in expansion and contraction due to lithiation / delithiation during charging and discharging of the battery increases significantly, which can lead to rapid degradation of the negative electrode and a reduction in the battery's lifespan. Additionally, the void volume between natural graphite particles is large, and both the bonding between negative electrode active material particles and the adhesion between the negative electrode active material and the electrode plate are reduced, which may decrease the battery's lifespan. Moreover, there may be a problem where the orientation index of the negative electrode active material increases significantly, resulting in poor high-speed charging performance.

[0128] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include controlling the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite in the preparation step to a range of 0.1 to 0.5.

[0129] When the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite falls within the aforementioned range, the expansion of the negative electrode active material due to lithium ion charging is suppressed, and the adhesion of the negative electrode active material to the electrode plate can be maintained well. Accordingly, the lifespan characteristics of the battery can be improved.

[0130] On the other hand, if the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite is less than the lower limit of the aforementioned range, the difference in average particle size between the bimodal natural graphite particles becomes excessively large, which may result in a problem of reduced capacity or output characteristics of the battery.

[0131] In addition, if the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite exceeds the upper limit of the aforementioned range, most of the particles constituting the negative electrode active material become coarse, so the orientation index increases, which may result in a problem where the high-speed charging characteristics are inferior. Furthermore, the void volume between particles becomes large, and the volume change due to lithium ion insertion and extraction becomes large, which may lower the electrode plate adhesion of the negative electrode active material.

[0132] A method for manufacturing a cathode active material according to another embodiment of the present invention may include controlling the degree of sphericity of the first natural graphite and the second natural graphite to a range of 0.4 to 1.0 in the preparation step.

[0133] Preferably, the degree of sphericity of the first natural graphite and the second natural graphite may be controlled to a range of 0.8 to 1.0.

[0134] When the degree of sphericity of the first natural graphite and the second natural graphite falls within the aforementioned range, the electrode plate adhesion of the negative electrode active material is improved, and by forming a high-density electrode, there may be an advantage of improving the capacity, energy density, and lifespan characteristics of the battery.

[0135] On the other hand, if the degree of sphericity of the first natural graphite and the second natural graphite exceeds the aforementioned range, the anisotropy of the negative electrode active material increases, leading to an uneven distribution of voltage and current and an increase in resistance. In the case of a battery containing such a negative electrode active material, there may be a problem of reduced capacity and a rapid decline in lifespan.

[0136] A method for manufacturing a negative electrode active material according to another embodiment of the present invention may include a magnetic field strength of 0.5 to 2.0 T applied to the first natural graphite and the second natural graphite after the mixing step.

[0137] When the strength of the magnetic field mentioned above falls within the aforementioned range, the mobility of lithium ions can be improved by appropriately controlling the alignment degree of the first natural graphite and the second natural graphite. Accordingly, the capacity and high-speed charge / discharge characteristics of the battery can be improved.

[0138] On the other hand, if the strength of the magnetic field is below the lower limit of the aforementioned range, the alignment of the first natural graphite and the second natural graphite is very low and disoriented, which may result in low lithium ion mobility and increased resistance of the negative electrode. Consequently, problems may arise regarding the battery's capacity, charge / discharge speed, and initial efficiency. Furthermore, there may be a problem where the battery's safety is low and its lifespan is rapidly reduced due to high heat generation.

[0139] Furthermore, if the strength of the magnetic field exceeds the upper limit of the aforementioned range, the alignment degree of the first natural graphite and the second natural graphite may be increased, but the contact angle between the negative electrode active material and the electrode plate may increase excessively, thereby reducing the contact area and the adhesion strength to the electrode plate. As a result, the negative electrode active material layer may easily peel off from the electrode plate, which may lead to a problem of reduced battery life.

[0141] A negative electrode and a lithium secondary battery according to another embodiment of the present invention will be described below.

[0142] 3. Cathode and Lithium Secondary Battery

[0143] A cathode according to another embodiment of the present invention comprises a current collector; and a cathode active material layer located on the current collector; wherein the cathode active material layer may comprise at least one of the aforementioned cathode active materials.

[0144] A lithium secondary battery according to another embodiment of the present invention may include the aforementioned negative electrode.

[0146] The following describes embodiments, comparative examples, and experimental examples of the present invention. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited by the following examples. Furthermore, it is possible to implement the invention with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and such modifications may also fall within the scope of the present invention.

[0147] Example 1

[0148] (1) Manufacturing of cathode active material

[0149] First natural graphite powder with an average particle size (D50) of 21.7 μm and second natural graphite powder with an average particle size (D50) of 6.8 μm were prepared. Subsequently, the first natural graphite and the second natural graphite were mixed in a weight ratio of 9:1. The mixed natural graphite powder was processed in a spheronizer at 1,000 rpm for 15 minutes to produce a high-density spherical bimodal natural graphite negative electrode active material.

[0150] (2) Cathode manufacturing

[0151] A negative electrode active material powder produced by the above method, a conductive material, a binder (styrene butadiene rubber - SBR), and a thickener (carboxymethylcellulose - CMC) were mixed in a mass ratio of 96.3:1:1.5:1.2, and water was added to prepare a negative electrode active material slurry. The negative electrode active material slurry was coated onto a copper (Cu) foil current collector, and then dried and rolled to manufacture a negative electrode. At this time, the loading of the negative electrode was 3.6 mAh / cm² 2 It was manufactured to be this way.

[0152] (3) Lithium secondary battery manufacturing

[0153] As a positive electrode active material, NCM (Ni 65 wt%), a conductive material, and KF1100 as a binder were mixed in a weight ratio of 96:2:2, and water was added to prepare a positive electrode slurry. The positive electrode slurry was coated onto aluminum foil, and the electrode was manufactured by vacuum drying and rolling at approximately 120°C for 12 hours. At this time, the loading of the positive electrode was 3.3 mAh / cm² 2 It was manufactured to be this way.

[0154] At this time, a separator made of a porous polypropylene film was inserted between the working electrode and the counter electrode, and as the electrolyte, a mixed solvent was used in which 0.5 wt% of vinylene carbonate (VC) and 1.5 wt% of propane sulfone (PS) were added to the solvent and 1.2 M concentration of LiPF6 was dissolved, with the mixed volumes of ethylene carbonate (EC), propylene carbonate (PC), ethylmethyl carbonate (EMC), and dimethyl carbonate (DMC) having a mixture volume ratio of 25:5:30:35.

[0155] Example 2

[0156] (1) A negative electrode active material, a negative electrode, and a lithium secondary battery were prepared in the same manner as in Example 1, except that the weight ratio of the first natural graphite and the second natural graphite was mixed at 7:3.

[0157] Comparative Example 1

[0158] (1) A negative electrode active material, a negative electrode, and a lithium secondary battery were prepared in the same manner as in Example 1, except that the weight ratio of the first natural graphite and the second natural graphite was mixed at 5:5.

[0159] Comparative Example 2

[0160] (1) A negative electrode active material, a negative electrode, and a lithium secondary battery were prepared in the same manner as in Example 1, except that the weight ratio of the first natural graphite and the second natural graphite was mixed at 3:7.

[0161] Comparative Example 3

[0162] (1) A negative electrode active material, a negative electrode, and a lithium secondary battery were prepared in the same manner as in Example 1, except that the weight ratio of the first natural graphite and the second natural graphite was mixed at 1:9.

[0163] Comparative Example 4

[0164] (1) A negative electrode active material, a negative electrode, and a lithium secondary battery were prepared in the same manner as in Example 1, except that the negative electrode active material was prepared using 100% of the fine particle second natural graphite without mixing the allele first natural graphite.

[0166]

[0167] division Electrochemical properties Charging capacity Discharge capacity Initial efficiency [mAh / g] [mAh / g] [%] Example 1 380.8 368.1 96.7 Example 2 386.1 357.2 92.5 Comparative Example 1 387.0 357.9 92.5 Comparative Example 2 388.4 354.1 91.2 Comparative Example 3 390.4 353.8 90.6 Comparative Example 4 396.8 361.1 91.0

[0168] Table 1 above is a table showing the physical properties, weight mixing ratio, ε value of Equation 1, and value of Equation 2 of bimodal natural graphite in the embodiments and comparative examples of the present invention.

[0169] According to Table 1 above, it was confirmed that Examples 1 and 2, in which the proportion of the first natural graphite (opponent) among the negative electrode active materials exceeded 50 wt%, exhibited significantly higher electrode plate adhesion compared to Comparative Examples 1 to 4, in which the proportion of the first natural graphite was less than or equal to the proportion of the second natural graphite. In addition, the BET specific surface area was 2.47 m² 2 Examples 1 and 2, controlled to / g or less, have a BET specific surface area of ​​2.49 m² 2 It was confirmed that the electrode plate adhesion was improved compared to Comparative Examples 1 to 4, which were greater than / g. In other words, it was confirmed that the improvement in electrode plate adhesion can be achieved by controlling the mixing ratio of large and small natural graphite and / or the BET specific surface area of ​​the negative electrode active material within a predetermined range.

[0170] In addition, regarding the above Equation 1, it was confirmed that the error ε in Examples 1 and 2 was very small at -0.003, while the error ε in Comparative Examples 1 to 4 was large at -4.827 to -7.205. That is, the correlation of Equation 1 can be satisfied when the mixing ratio of the first natural graphite (large) and the second natural graphite (small) is controlled as in Examples 1 and 2.

[0171] In addition, it was confirmed that when the natural graphite mixing ratio of Examples 1 and 2 is satisfied, Equation 2 can be satisfied simultaneously.

[0172] Table 2 above shows the charge / discharge capacity and initial efficiency of the embodiments and comparative examples of the present invention.

[0173] According to Table 2 above, it was confirmed that the charge / discharge capacity and initial efficiency of Examples 1 and 2 and Comparative Example 1 were relatively high. In particular, it was confirmed that the charge / discharge capacity and initial efficiency of Example 1 were significantly higher. It can be seen that setting a high mixing ratio of the first natural graphite has the advantage of improving capacity and efficiency, and considering the electrode plate adhesion and the improvement of battery life together, it may be desirable to control the mixing ratio of the first natural graphite within the range of Examples 1 and 2. Furthermore, in order to maximize the improvement of battery life, capacity, and initial efficiency evenly, it may be more desirable to control the mixing ratio of the first natural graphite to around 90 weight%.

[0174] Experimental Example 1 - Evaluation of Physical Properties of Cathode Active Material

[0175] (1) Evaluation of average particle size (D10, D50, D90)

[0176] The particle sizes corresponding to 10%, 50%, and 90% of the cumulative volume of the negative electrode active material were measured using the laser diffraction method.

[0177] (2) Evaluation of compressive density

[0178] Compressed density (g / cm³) 3The compressive density is calculated from the volume measured after filling a mold (a cylindrical mold with a diameter of 25 mm) with the cathode active material powder and pressurizing it to a pressure of 0.22 MPa, and the mass of the cathode active material powder introduced into the mold. This compressive density can be measured and calculated using conventional density analysis equipment (for example, a GeoPyc 1360 density analyzer, Micromeritics).

[0179] (3) Specific surface area evaluation

[0180] The specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0182] Experimental Example 2 - Evaluation of Electrochemical Properties

[0183] (1) Evaluation of initial capacity and initial efficiency

[0184] After fabricating the lithium secondary battery half-cell, it was aged at 25°C for 48 hours, and then a charge-discharge test was conducted at 25°C. To evaluate the initial capacity, the reference capacity was set to 360 mAh / g, and the battery was charged to 0.005V with a constant current of 0.1C. Then, the voltage was switched to a constant voltage, and charging continued until the terminal current reached 0.05C. After a 10-minute rest time following charging, the battery was discharged until it reached 1.5V with a constant current of 0.1C and a reference capacity of 360 mAh / g.

[0185] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

[0187] Experimental Example 3 - Correlation analysis between electrode plate adhesion (A), mixing ratio of first natural graphite (B), and reciprocal of BET specific surface area (I)

[0188] The correlation between the electrode plate adhesion (A), BET specific surface area, and the mixing ratio of the first natural graphite (B) measured from the cathode active materials of the embodiments and comparative examples of the present invention was analyzed.

[0189] At this time, regression analysis was used among the data analysis tools in Excel for correlation analysis. First, a scatter plot was generated from the data of electrode plate adhesion (A) - mixing ratio of first natural graphite (B) and electrode plate adhesion (A) - reciprocal of BET specific surface area (I), and it was confirmed that the correlation between each factor generally followed a linear pattern. Next, multiple regression analysis was performed by setting the mixing ratio of first natural graphite (B) as the independent variable (x1), the reciprocal of BET specific surface area (I) as the independent variable (x2), and electrode plate adhesion (A) as the dependent variable (y). Specifically, the mixing ratio of first natural graphite (B) and the reciprocal of BET specific surface area (I) were entered as the x-axis input range, and the electrode plate adhesion (A) data was entered as the y-axis input range, respectively, and the above multiple regression analysis was performed with the confidence level set to 95%.

[0190] By the above multiple regression analysis, the correlation between the electrode plate adhesion (A) of the natural graphite cathode active material of the present invention, the mixing ratio (B) of the first natural graphite, and the reciprocal of the BET specific surface area (I) was derived as Equation 1 below.

[0191] [Equation 1]

[0192] A = 1.16*B +7.66*I +6.79 +ε (-4.8≤ε≤4.8)

[0193] (In the above Equation 1, A is the electrode plate adhesion strength of the negative active material expressed in units of gf / cm, B is the weight mixing ratio of the first natural graphite expressed in units of weight%, and I is m 2 They each represent the reciprocal of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 1 above, the units of each variable are not considered and are calculated as dimensionless values.)

[0194] In the above Equation 1, B and I correspond to independent variables (x1 and x2), and A corresponds to dependent variable (y), respectively.

[0195] Also, the multiple correlation coefficient (R value) for the above Equation 1 is 1, and the coefficient of determination (R 2 It was confirmed that ) is 1, indicating a very high correlation. That is, the reliability of Equation 1 derived by regression analysis is high, and it can be confirmed that the negative electrode active material according to the embodiment of the present invention satisfies Equation 1, thereby improving the adhesion to the electrode plate.

Claims

Claim 1 A negative electrode active material comprising: a first natural graphite; and a second natural graphite having an average particle size (D50) smaller than that of the first natural graphite; wherein the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than 100 weight% based on 100 weight% of the total negative electrode active material, and satisfies the following Equation 1. [Equation 1] A = 1.16*B + 7.66*I + 6.79 + ε (-4.8≤ε≤4.8) (wherein Equation 1, A is the electrode plate adhesion strength of the negative electrode active material expressed in units of gf / cm, B is the weight mixing ratio of the first natural graphite expressed in units of weight%, and I is m 2 They each represent the reciprocal of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 1 above, the units of each variable are not considered and are calculated as dimensionless values.) Claim 2 A negative electrode active material according to claim 1, wherein the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite is 0.1 to 0.

5. Claim 3 A negative electrode active material according to claim 1, wherein the average particle size (D50) of the first natural graphite is 18 to 30 μm. Claim 4 A negative electrode active material according to claim 1, wherein the average particle size (D50) of the second natural graphite is 3 to 9 μm. Claim 5 A negative electrode active material according to claim 1, wherein the SPAN ((D90-D10) / D50) value of the first natural graphite is 0.7 to 1.

3. Claim 6 A negative electrode active material according to claim 1, wherein the SPAN ((D90-D10) / D50) value of the second natural graphite is 0.6 to 1.

2. Claim 7 In claim 1, the compressed density of the negative electrode active material is 1.0 to 1.5 g / cm³ 3 Phosphorus, cathode active material. Claim 8 In claim 1, the BET specific surface area of ​​the negative electrode active material is 1.8 to 2.5 g / cm² 3 Phosphorus, cathode active material. Claim 9 A cathode active material according to claim 1, wherein the degree of sphericity of the first natural graphite and the second natural graphite is 0.4 to 1.

0. Claim 10 A method for manufacturing a negative electrode active material, comprising: a step of preparing a first natural graphite and a second natural graphite having an average particle size (D50) smaller than that of the first natural graphite; and a step of mixing the first natural graphite and the second natural graphite; wherein, in the mixing step, the weight mixing ratio of the first natural graphite is greater than 50 weight% and less than 100 weight% based on 100 weight% of the total negative electrode active material, and satisfies the following Equation 2. [Equation 2] 0.25≤B*D p *I≤0.6(in Equation 2 above, B is the weight mixing ratio (weight%) of the first natural graphite expressed in weight% units, D p is g / cm 3 The compressed density I of the above-mentioned cathode active material, expressed in units of m 2 They respectively represent the reciprocals of the BET specific surface area of ​​the cathode active material expressed in units of / g, and in the calculation of Equation 2 above, the units of each variable are not considered and are calculated as dimensionless values.) Claim 11 A method for manufacturing a cathode active material according to claim 10, wherein the preparation step comprises controlling the average particle size (D50) of the first natural graphite to a range of 18 to 30 μm. Claim 12 A method for manufacturing a cathode active material according to claim 10, wherein the preparation step comprises controlling the average particle size (D50) of the second natural graphite to a range of 3 to 9 μm. Claim 13 A method for manufacturing a cathode active material according to claim 10, wherein the preparation step comprises controlling the ratio of the average particle size (D50) of the second natural graphite to the average particle size (D50) of the first natural graphite to a range of 0.1 to 0.

5. Claim 14 A method for manufacturing a cathode active material according to claim 10, wherein the preparation step comprises controlling the degree of sphericity of the first natural graphite and the second natural graphite to a range of 0.4 to 1.

0. Claim 15 A method for manufacturing a negative electrode active material according to claim 10, further comprising a magnetic field strength of 0.5 to 2.0 T applied to the first natural graphite and the second natural graphite after the mixing step. Claim 16 A cathode comprising: a current collector; and a negative active material layer located on the current collector; wherein the negative active material layer comprises a negative active material according to any one of claims 1 to 9. Claim 17 A lithium secondary battery comprising the negative electrode of claim 16.

Citation Information

Patent Citations

  • Negative electrode, secondary battery, battery module and battery pack comprising the same

    KR1020180029919A

  • An active material for an anode, an anode comprising the same and an electrochemical device comprising the same

    KR1020190049585A