Positive electrode active material and method for manufacturing the same, litium secondary battery comprising the same
The formation of island-shaped coating layers on high-nickel NCM cathode materials stabilizes the structure, addressing microcracks and gas generation, thereby improving electrochemical performance and energy density.
Patent Information
- Application Number
- KR1020240117615
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-30
AI Technical Summary
High-nickel NCM cathode materials suffer from microcracks, increased specific surface area, gas generation, and cation mixing due to structural instability, leading to degraded battery lifespan and electrochemical properties.
Manufacturing lithium metal oxides with single or pseudo-single particles by high-temperature calcination, followed by forming a controlled island-shaped coating layer on the surface to stabilize the structure and reduce oxygen vacancies.
Improves electrochemical performance by enhancing particle strength, reducing gas generation, and increasing energy density while maintaining structural stability and safety.
Smart Images

Figure 112024095368034-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The invention relates to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery containing the same. Background Technology
[0002] Driven by the recent explosive demand for electric vehicles and the need for increased driving range, the development of high-capacity, high-energy-density secondary batteries to meet these demands is actively underway worldwide. In particular, high-nickel NCM cathode materials with high nickel content are being used to satisfy these requirements.
[0003] However, while capacity characteristics improve as nickel content increases, microcracks occur during charging and discharging due to the decrease in particle strength. Furthermore, this leads to an increase in the specific surface area of the cathode material, resulting in increased gas generation as the reaction with the electrolyte intensifies. Additionally, unstable Ni due to structural instability 3+ stable Ni 2+ There is a problem in that the lifespan characteristics of the battery are degraded due to an increase in the cation mixing phenomenon, in which the cation is reduced and converted into stable NiO.
[0004] To solve the above problem, a method is proposed to increase the calcination temperature during the manufacture of lithium metal oxides (e.g., one or more metals including nickel) to form single particles or pseudo-single particles with the size of the primary particles maximized.
[0005] However, this method requires firing at a relatively high temperature for a long time compared to conventional processes, which results in oxygen vacancy. Consequently, defects in the layered structure of the final cathode active material occur, leading to a degradation of electrochemical properties such as capacity and output.
[0006] Therefore, there is a need to develop cathode active materials with improved electrochemical properties by controlling oxygen deficiency. The problem to be solved
[0007] The present invention aims to provide a positive electrode active material capable of securing improved cell characteristics and a method for manufacturing the same. means of solving the problem
[0008] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.
[0009] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.
[0010] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.
[0011] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.
[0012] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.
[0013] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.
[0014] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.
[0015] In this specification, “single particle” is a term used to distinguish it from cathode active material particles in the form of secondary particles formed by the aggregation of tens to hundreds of primary particles, which were conventionally used; it refers to a single particle composed of one primary particle, and “pseudo-single particle” refers to a composite particle of 30 or fewer primary particles. The “secondary particle” refers to an aggregate, or secondary structure, formed by the aggregation of tens to hundreds of primary particles through physical or chemical bonding between primary particles without an intentional aggregation or assembly process. Furthermore, “primary particle” refers to the smallest particle unit distinguished as a single mass when observing the cross-section of the cathode active material through a scanning electron microscope (SEM); it may consist of a single grain or multiple grains. Additionally, “grain” refers to a distinct region within the primary particle in which atoms form a lattice structure in a specific direction.
[0016] In the present invention, the term “particle” is a concept that includes one or more of a single particle, a pseudo-single particle, a primary particle, and a secondary particle.
[0017] In one embodiment of the present invention, a positive active material for a lithium secondary battery can be provided, wherein the positive active material comprises a form in which 1 to 20 single particles are aggregated, and an island-shaped coating particle is located on the surface of the positive active material, and the coating particle satisfies the following mathematical formula 1.
[0018] [Mathematical Formula 1]
[0019] Coating cover ratio ≤ 15 area%
[0020] The above coating cover ratio is the area occupied by the coating particles in the SEM image of the positive active material unit particles relative to the total area in the SEM image of the positive active material unit particles, for a certain proportion of the SEM image of the positive active material.
[0021] More specifically, the above positive active material can satisfy the following mathematical formula 2.
[0022] [Mathematical Formula 2]
[0023] 7 Area% ≤ Coating Cover Ratio ≤ 15 Area%
[0024] In one embodiment of the present invention, the coating layer may exist in an island form and may be positioned to cover a surface within 15% of the total surface area of the lithium metal oxide, specifically covering a surface within 7% to 15% of the total surface area.
[0025] In the present invention, the ratio of the coating area of the coating particles to the total surface area of the lithium metal oxide can be calculated as the ratio of the total area of the island-shaped coating particles observed in the SEM image to the total area of the lithium metal (total area of coating particles / total area of lithium metal particles). As can be seen in the examples described below, when this range is satisfied, the initial capacity, lifespan, efficiency characteristics, etc., can be improved.
[0026] Mid-Ni single crystals synthesized at relatively high temperatures may have an unstable layered structure due to oxygen vacancies near the surface.
[0027] To overcome this, we aim to improve rate characteristics by ensuring structural stability of the surface region through sufficient lithination in the unstable surface region.
[0028] When the coating temperature is low, numerous island-shaped coating materials exist on the surface, which can still destabilize the surface of the cathode active material. Therefore, we aim to improve electrochemical performance by controlling the island-shaped coating area on the surface through appropriate coating temperature control.
[0029] The single particle may include one or more crystal grains, specifically, it may include at least one of a structure that is distinguished as a single mass when the cross-section of the powder is observed through a scanning electron microscope (SEM), such as a single particle containing one crystal grain or a pseudo-single particle form in which 2 to 20 or 2 to 10 crystal grains are clustered together.
[0030] In the case of a single-particle cathode active material of the aforementioned form, compared to a conventional cathode active material of secondary particles formed by the aggregation of tens to hundreds of primary particles, the specific surface area is smaller, which reduces the amount of gas generated due to side reactions with the electrolyte. Additionally, the particle strength is higher, which can suppress particle breakage during rolling and reduce the occurrence of cracks due to repeated charging and discharging. Accordingly, it has the advantage of superior lifespan and safety compared to secondary particles, and enables the realization of high energy density of the electrode.
[0031] As mentioned above, since cathode active materials in the form of single particles or pseudo-single particles are manufactured by firing at high temperatures compared to conventional cathode active materials in the form of secondary particles, crystal defects in a layered structure may occur. In this embodiment, by forming a coating layer containing a particle-shaped compound containing a coating element on the surface of a metal oxide, crystal defects such as an increase in the cation mixing ratio due to high-temperature firing can be prevented, and the crystal grain size within the single particles and the average particle size of the single particles can be efficiently increased during the firing process.
[0032] The content of the coating element included in the compound in the form of the coating particles may be in the range of 0.01 to 0.08 moles, more specifically in the range of 0.01 to 0.08 moles, 0.01 to 0.07 moles, 0.01 to 0.05 moles, 0.01 to 0.04 moles, or 0.01 to 0.03 moles, based on 1 mole of the total metal included in the lithium metal oxide core in which the coating particles are formed.
[0033] At this time, the coating element (metal element) within the coating particle may be introduced in a molar ratio similar to that of the additional lithium raw material introduced during coating, and the molar ratio of lithium among the lithium raw material to the metal material among the coating elements may be in the range of 0.5 to 2.0, 0.6 to 1.8, 0.7 to 1.6, 0.8 to 1.4, or 0.9 to 1.2.
[0034] In this embodiment, the coating element included in the particle-shaped compound may be cobalt. When the cobalt content satisfies the above range, the crystal grains can be grown to an appropriate size, and the production cost can be appropriately controlled, which has the advantage of excellent economic efficiency.
[0035] In the present invention, the coating particles in the form of particles containing the cobalt element are CoO, Co2O3, CO3O4, LiCoO2, Co(OH)2, CoCl2, CoF3, CoSO4·xH2O, CoSO4·7H2O, (CH3COO)2Co·4H2O, Co(NO3)2·6H2O, (CH3CO2)2Co, CoCO3· x It may include one or more selected from H2O and Co3(PO4)2.
[0036] Next, the coating layer containing the above-mentioned coating particles may further include additional coating elements, but the type and content of the additional coating elements are not particularly limited in the present invention.
[0037] Meanwhile, the average particle size (D50) of the positive active material according to one embodiment of the present invention may be 2 μm or more, more specifically in the range of 2 μm to 6 μm.
[0038] When the average particle size of the above particles and / or the average particle size of the positive electrode active material satisfies the above range, a lithium secondary battery with excellent electrochemical properties, such as lifespan characteristics and resistance growth rate, can be realized. Furthermore, since the energy density per unit volume can also be increased, it has a very excellent effect.
[0039] The diameter of the above-mentioned island-shaped coating particles may be 500 nm or less. More specifically, it may be 200 nm or less, or 100 nm or less.
[0040] The above positive active material can be represented by the following chemical formula 1.
[0041] [Chemical Formula 1]
[0042] Li a [Ni x Co y Mn z M w ]O2
[0043] In the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0≤z≤0.4, 0≤w≤0.2, x+y+z+w=1, and M is Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.
[0044] The nickel content may be 0.5 moles or more, more specifically 0.5 moles or more, 0.6 moles or more, 0.7 moles or less, or 0.65 moles or less, based on 1 mole of the total of nickel, cobalt, and manganese. Depending on the nickel content, performance characteristics such as capacity, output, and rate characteristics of a battery containing the active material of the present invention can be realized differently, and when the active material according to one embodiment of the present invention contains 0.6 moles to 0.7 moles of nickel, stability or thermal stability during rolling may be further improved.
[0046] In another embodiment of the present invention, a method for manufacturing a positive active material for a lithium secondary battery can be provided, comprising: a step of preparing a metal precursor; a step of mixing the metal precursor and a lithium raw material and then calcining to obtain a positive active material for a single-crystal lithium secondary battery; and a step of mixing the positive active material and a coating raw material and then heat-treating to obtain a positive active material having island-shaped coating particles located on the surface; wherein, in the step of mixing the positive active material and the coating raw material and then heat-treating to obtain a positive active material having island-shaped coating particles located on the surface, the heat-treating temperature is 730°C to 770°C.
[0047] The specific method is described in detail below, step by step.
[0048] First, a nickel-containing precursor is prepared. The nickel-containing precursor may be a nickel-containing metal hydroxide.
[0049] The above nickel-containing precursor can be manufactured by purchasing and using a commercially available cathode active material precursor, or by following a method for manufacturing a cathode active material precursor well known in the art.
[0050] For example, the above precursor may be prepared by co-precipitating a metal solution containing a nickel-containing raw material, a cobalt-containing raw material, and a manganese-containing raw material by adding a complex-forming agent and a pH-adjustable solution.
[0051] The above nickel raw material is not particularly limited as long as it is used in the industry for manufacturing a cathode active material precursor. For example, the above nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, it may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salt, nickel halide, or a combination thereof, but is not limited thereto.
[0052] The above-mentioned cobalt raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above-mentioned cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO₄ 4, It may be CoSO4·7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or a combination thereof, but is not limited thereto.
[0053] The above manganese raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof. Specifically, it may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.
[0054] The above metal-containing solution may be prepared by adding a nickel raw material and optionally a cobalt raw material or a manganese raw material to a solvent, specifically water, or a mixture of water and an organic solvent that can be uniformly mixed with water (e.g., alcohol).
[0055] The above-mentioned complexing agent-containing solution performs the role of forming a complex, and may include, for example, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof as the complexing agent, but is not limited thereto. Meanwhile, the above-mentioned complexing agent-containing solution may be used in the form of an aqueous solution, and in this case, water or a mixture of water and an organic solvent that is uniformly miscible with water (e.g., alcohol, etc.) may be used as the solvent.
[0056] The above pH-adjustable solution may be an aqueous solution containing a basic compound, and the basic compound may be a hydroxide of an alkali metal or alkaline earth metal such as NaOH, KOH, or Ca(OH)2, a hydrate thereof, or a combination thereof. The basic compound may also be used in the form of an aqueous solution, in which case water or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.) may be used as the solvent.
[0057] The above basic compound is added to adjust the pH of the reaction solution, and may be added in an amount such that the pH of the metal solution becomes 11 to 13, but is not limited thereto.
[0058] Meanwhile, the above co-precipitation reaction may be carried out at a temperature of 40°C to 70°C under an inert atmosphere such as nitrogen or argon, but is not limited thereto.
[0059] By the process described above, nickel-cobalt-manganese hydroxide particles are generated and precipitated in the reaction solution. By controlling the concentrations of the nickel-containing raw material, the cobalt-containing raw material, and the manganese-containing raw material, a precursor can be prepared in which the nickel (Ni) content of the total metal content is 50 mol% or more, specifically 60 mol% or more and 70 mol% or less. The precipitated nickel-cobalt-manganese hydroxide particles can be separated by a conventional method and dried to obtain a nickel-cobalt-manganese precursor. The precursor may be a secondary particle formed by the aggregation of primary particles.
[0060] When the nickel (Ni) content in the above precursor satisfies the range, cell characteristics can be further improved when the positive electrode active material finally manufactured according to the embodiment of the present invention is applied to a battery. In the case of a positive electrode active material containing a nickel (Ni)-based metal oxide, the calcination temperature varies depending on the nickel (Ni) content during calcination; specifically, the higher the nickel (Ni) content, the lower the temperature required for calcination. More specifically, the lower the nickel (Ni) content, the higher the calcination temperature, and in this case, the surface of the active material may experience degradation due to high temperatures. In this case, it is common to reduce such degradation by coating the surface, and the heat treatment during coating also exhibits different coating element diffusion trends depending on the nickel (Ni) content. The heat treatment temperature of the embodiment can be controlled by the nickel (Ni) content of the above precursor according to the present invention, and thereby, the diffusion thickness of the coating element and the coating shape can be controlled.
[0061] Next, the above-mentioned positive active material precursor, lithium raw material, and optionally, doping raw material are mixed to form a mixture.
[0062] The above lithium raw material may include lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or oxyhydroxides, and is not particularly limited as long as it is soluble in water. Specifically, the above lithium raw material may be one or more selected from Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7.
[0063] The above lithium raw material can be mixed such that the molar ratio of lithium to metals other than lithium included in the final product lithium metal oxide is in the range of 1.0 to 1.20, specifically 1.01 to 1.10, or 1.02 to 1.07.
[0064] In one embodiment of the present invention, by mixing the lithium raw material within the above range, it is preferable that the lithium content remaining on the surface of the calcined product can be controlled to the range intended in the present invention during the subsequent step of manufacturing the calcined product.
[0065] Additionally, optionally, the doping element in the doping raw material may be mixed to have a content of 0.5 mol% or more, specifically 0.5 to 1.5 mol%, based on the total metal in the precursor.
[0066] Adding the above-mentioned doping raw material within the above range is desirable as it can improve the discharge capacity and charge / discharge efficiency performance of a lithium secondary battery using the finally manufactured cathode active material.
[0067] The above doping raw material may include one or more elements selected from Al, Zr, V, Co, Mg, Ti, Y, Sr, Nb, Ba, Ca, B, W, Sc, Si, Fe, Mo, Ce, Hf, Ta, and La, and more specifically, the above doping raw material may include an Al raw material, a Y raw material, and a Zr raw material.
[0068] The above doping raw material may be a sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide containing a doping element, and is not particularly limited in the present invention.
[0069] Next, the step of calcining the above mixture to obtain a calcined product is performed.
[0070] In the present invention, the step of obtaining the sintered product may be performed by maintaining the same sintering temperature within the same kiln or by changing the profile of the sintering temperature, for example, by performing a 1-step sintering process, performing a 1-step sintering process and a 2-step sintering process, or performing a 1-step sintering process, a 2-step sintering process, and a 3-step sintering process.
[0071] In one embodiment of the present invention, when firing is performed as a one-step process maintaining the same firing temperature, it may be performed in an oxygen atmosphere, an atmospheric atmosphere (air atmosphere), or an atmosphere mixed with oxygen and air, and the one-step firing may be performed for 10 to 30 hours at a temperature in the range of 880°C to 960°C, specifically 900°C to 955°C, or 920°C to 950°C in an oxygen atmosphere.
[0072] In another embodiment of the present invention, when firing is performed in the two-step process, the first step firing may be performed in an oxygen atmosphere, an air atmosphere, or an atmosphere mixed with oxygen and air, and the first step firing may be performed in an oxygen atmosphere at a temperature in the range of 880°C to 930°C, specifically at a temperature in the range of 890°C to 920°C, 895°C to 915°C, or 900°C to 910°C for 3 to 6 hours. When firing is performed in the two-step process, the second step firing may be performed in the same atmosphere as the first step firing or in a different atmosphere at a temperature in the range of 760°C to 840°C, specifically at a temperature in the range of 780°C to 820°C or 800°C to 820°C for 7 to 9 hours.
[0073] In another embodiment of the present invention, when firing is performed using the 3-step process, similar to the 2-step process, a 2-step firing may be performed for 1 to 3 hours at a temperature in the range of 900°C to 950°C, specifically 910°C to 940°C, 915°C to 935°C, or 920°C to 930°C, in the same atmosphere or a different atmosphere as the 1-step firing, and a 2-step firing may be performed for 7 to 9 hours at a temperature in the range of 760°C to 840°C, specifically 780°C to 820°C or 800°C to 820°C, in the same atmosphere or a different atmosphere as the 2-step firing.
[0074] The total time for calcination to be performed in the step of obtaining the above-mentioned calcined product can be 10 to 30 hours, and this can be controlled according to the Ni content of the active material.
[0075] In the present invention, by performing calcination under the above conditions, it is desirable to be able to control the lithium content remaining on the surface of the calcined product to a range intended in the present invention.
[0076] In the present invention, the residual lithium compound content of the calcined product generated in the calcination step, that is, the lithium compound remaining on the surface of the calcined product, can be controlled to be 0.23 wt% or less based on the total weight of the calcined product, specifically in the range of 0.1 to 0.23 wt% or 0.14 wt% to 0.22 wt%.
[0077] When the residual lithium content of the calcined product is controlled within the above range as described above, for example, in the coating step described later, a coating layer is formed by reacting with a coating element on the surface of the calcined product, i.e., the lithium metal oxide, while simultaneously, a lithiation reaction occurs efficiently at the surface and / or particle boundaries of the lithium metal oxide, thereby recovering the oxygen-deficient (O2 vacancy) regions generated during the high-temperature manufacturing process of the lithium metal oxide. This is desirable as it can improve the electrochemical performance of the finally produced cathode active material.
[0078] In addition to controlling such residual lithium, additional lithium may be introduced during the coating step. The added lithium may be lithium hydroxide, lithium carbonate, or a combination thereof. The content of the additional lithium raw material introduced may be in the range of 0.01 to 0.08 moles, more specifically 0.01 to 0.07 moles, 0.01 to 0.06 moles, 0.01 to 0.05 moles, 0.01 to 0.04 moles, or 0.01 to 0.03 moles, based on 1 mole of the total metal contained in the lithium metal oxide into which the additional lithium raw material is introduced. Due to the introduction of such additional lithium, a reaction with the coating raw material particles can be effectively induced, thereby effectively forming a coating material on the surface of the single particle and controlling the area.
[0079] At this time, the metal element in the coating raw material may be introduced in a molar ratio similar to that of the additional lithium raw material introduced during coating, and the molar ratio of lithium in the lithium raw material to the metal material among the coating elements may be in the range of 0.5 to 2.0, 0.6 to 1.8, 0.7 to 1.6, 0.8 to 1.4, or 0.9 to 1.2.
[0080] Additionally, the method may further include a step of crushing the above-mentioned calcined product to form a desired particle size, but the present invention is not particularly limited to the crushing step, the crushing method, and the particle size after crushing.
[0081] Next, the step of mixing the above-mentioned calcined material and coating raw material to form a mixture, and then heat-treating to obtain a lithium metal oxide with a coating layer formed thereon.
[0082] In the present invention, the coating raw material may include a compound in the form of particles having an average particle size in the range of 150 nm to 300 nm or 200 nm to 280 nm.
[0083] The coating raw material containing the above-mentioned particulate compound is Co(OH)2, CoCl2, CoO, CoF3, CoSO4·xH2O, CoSO4·7H2O, (CH3COO)2Co·4H2O, Co(NO3)2·6H2O, (CH3CO2)2Co, CoCO3· x It may include one or more selected from H2O and Co3(PO4)2.
[0084] The coating raw material containing the above-mentioned particle-shaped compound can be introduced in a content range of 1 mol% to 4 mol%, specifically 2.0 mol% to 3.0 mol%, based on the total metal excluding lithium in the above-mentioned sintered product.
[0085] In the above heat treatment process, reactive lithium within the lithium remaining on the surface of the lithium metal oxide, additionally introduced lithium raw material; and cobalt contained in the coating raw material; react to form one or more coating materials selected from metal hydroxide, metal oxide, lithium metal hydroxide, and lithium metal oxide lithium cobalt compounds.
[0086] Specifically, cobalt oxide or lithium cobalt oxide can be produced alone or simultaneously.
[0087] At this time, the heat treatment can be performed in an oxygen atmosphere at a temperature in the range of 730°C to 770°C, specifically at a temperature of 740°C to 760°C or 750°C. The heat treatment can be performed for 3 to 10 hours.
[0088] The step of mixing the above-mentioned positive active material and coating raw material and then heat-treating to obtain a positive active material having island-shaped coating particles located on the surface can be performed under atmospheric conditions. The above-mentioned atmospheric conditions may be carbon dioxide-free atmospheric conditions (CO2-free air, CFA).
[0089] Generally, oxygen conditions are considered favorable for controlling residual lithium during the calcination of cathode active materials. This is because if oxygen is insufficient, lithium may revert to a form such as lithium carbonate, and there may be issues such as the failure to smoothly form the layered structure.
[0090] The inventors have discovered that oxygen conditions are not essential during the coating step following the manufacture of lithium metal oxides, and that in some aspects, general atmospheric conditions are actually more advantageous. More specifically, regarding the aforementioned nickel (Ni) content range, a higher temperature than in an atmospheric atmosphere is required for grain growth and subsequent single crystallization during calcination in an oxygen-rich, stable atmosphere. In this case, since the required reaction temperature under atmospheric conditions is actually lower than under oxygen conditions, favorable results can be expected, such as the suppression of various side reactions (e.g., changes in crystal structure) that may occur at high temperatures and economic benefits. These characteristics can be similarly realized through heat treatment during coating; more specifically, under atmospheric conditions, the diffusion of coating elements into the core is further promoted, and the structural stability of the core's surface can be significantly improved.
[0091] However, even in such cases, atmospheric conditions free of carbon dioxide may be desirable to prevent the loss of lithium raw materials due to carbon dioxide.
[0092] In one embodiment of the present invention, when heat treatment is performed under the above conditions, a coating layer is formed on the surface of the sintered product, i.e., the lithium metal oxide, and at the same time, a lithiation reaction occurs efficiently at the surface and / or particle boundaries of the lithium metal oxide, thereby forming coating particles in the coating layer within a range that allows for the recovery of the oxygen-deficient (O2 vacancy) region generated during the high-temperature manufacturing process of the lithium metal oxide, while also stabilizing the structure up to the depth range of the surface portion of the internal core. This is desirable because it can improve the electrochemical performance of the cathode active material finally produced.
[0093] In addition, by performing the calcination and heat treatment steps under the above conditions in the present invention, a separate washing process is not required to remove lithium remaining on the surface of the final-produced positive electrode active material.
[0095] In another embodiment, a positive electrode is provided comprising a current collector and a positive electrode active material layer located on one side of the current collector and comprising a positive electrode active material manufactured according to the above-described embodiment.
[0096] The characteristics of the positive active material constituting the above positive active material layer are the same as those previously described. Therefore, a detailed description of the positive active material will be omitted.
[0097] The above current collector may be, for example, made of stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treated with carbon, nickel, titanium, silver, etc.
[0098] Meanwhile, the above positive active material layer may include a binder and a conductive material.
[0099] At this time, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.
[0100] In addition, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used, but is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the positive electrode active material layer.
[0101] The above-mentioned anode can be manufactured according to a conventional anode manufacturing method, except for using the above-mentioned anode active material.
[0102] Specifically, the anode can be manufactured by applying a composition for forming an anode active material layer, comprising the aforementioned anode active material and optionally a binder, conductive material, or solvent as needed, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.
[0103] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that allows for the dissolution or dispersion of the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.
[0104] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.
[0106] In another embodiment of the present invention, a lithium secondary battery may be provided comprising: a positive electrode including a positive active material; a negative electrode; and an electrolyte located between the positive electrode and the positive electrode, wherein the positive active material comprises the positive active material according to the aforementioned embodiment of the present invention.
[0107] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly comprising the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.
[0108] In the above lithium secondary battery, the negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0109] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0110] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a composition for forming a cathode active material layer, comprising a cathode active material and optionally a binder and a conductive material, onto a cathode current collector and drying it, or by casting the composition for forming a cathode onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.
[0111] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the above-mentioned negative electrode active material. Furthermore, the carbon material may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0112] The binder and conductive material mentioned above may be the same as those previously described in the anode.
[0113] Next, depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used, and a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.
[0114] In addition, regarding the above lithium secondary battery, the electrolyte may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing a lithium secondary battery, but is not limited to these.
[0115] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0116] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.
[0117] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.
[0118] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs). Effects of the invention
[0119] When a cell is constructed using a positive electrode active material according to one embodiment of the present invention, improved cell characteristics can be secured. Specifically, initial capacity, efficiency, resistance characteristics, and lifespan characteristics can be improved. Brief explanation of the drawing
[0120] Figures 1 to 4 are SEM images of positive electrode active materials according to examples and comparative examples. Specific details for implementing the invention
[0121] Preferred embodiments and comparative examples of the present invention are described below. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0122] Examples and Comparative Examples
[0123] 1. Preparation of cathode active material
[0124] (Mixed) Ni 0.69 Co 0.06 Mn 0.25 A precursor of (OH)2 composition was mixed with LiOH such that the molar ratio of lithium to the transition metal of the precursor (Li / M) was 1.05.
[0125] After (calcination and disintegration), the mixture was heated to 950°C through heat treatment in an oxygen atmosphere, subjected to primary calcination for 12 hours, and then naturally cooled to form a lithium metal oxide. Subsequently, the lithium metal oxide was disintegrated using an air jet mill to obtain a single-crystal cathode active material. The composition of the obtained single-crystal cathode active material is Li 1.05 Ni 0.69 Co 0.06 Mn 0.25 It was O2.
[0126] (1st Coating and Heat Treatment) The single-crystal cathode active material, which has undergone 1st calcination, is prepared. Here, coating particles are formed on the surface of the single-crystal cathode active material under conditions as shown in Tables 1 to 3 below by mixing the coating raw material Co(OH)2, optionally additional lithium raw material LiOH or Li2CO3, in a predetermined ratio. The coating heat treatment time was fixed at 6 hours.
[0127] (Optional secondary coating and heat treatment) When mixing the single-crystal positive active material with coating raw materials Al2O3 and WO3, Al and W were added at 1500 ppm and 3000 ppm of the total mixture weight, respectively, mixed in a mixer, and then heat-treated at 430°C for 6 hours to obtain a single-crystal positive active material having a coating layer containing Al and W formed on its surface. A secondary coating may be performed optionally.
[0128] 2. Cell manufacturing
[0129] To evaluate the physical properties and electrochemistry of the positive electrode active materials according to the examples and comparative examples, coin cells were manufactured as follows.
[0130] Specifically, a positive active material, a polyvinylidene fluoride binder (product name: KF9700), and a carbon black conductive material were mixed in a weight ratio of 95:3:2, and this mixture was added to an N-methyl-2-pyrrolidone solvent so that the solid content was about 60 wt% to prepare a positive active material slurry.
[0131] The above slurry was coated onto an anode current collector aluminum foil (Al foil, thickness: 20 μm) using a doctor blade, dried, and then rolled to manufacture an anode. The loading amount of the anode was approximately 16 mg / cm², and the rolling density was approximately 3.5 g / cm³. 3 It was.
[0132] A 2032 coin cell was manufactured by a conventional method using the above-mentioned anode, a lithium metal cathode (thickness 200 μm, Welcos), an electrolyte, and a polyethylene separator. The electrolyte used was a mixed solution in which 1M LiPF6 was dissolved in a mixed solvent of 2% VC (vinylene carbonate), ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) (mixing ratio EC:DMC:DEC = 1:2:1 volume%).
[0133] 3. Analysis of coating particles on the cathode active material via SEM images
[0134] Images of the positive electrode active material prepared according to the above examples and comparative examples were obtained using Scanning Electron Microscopy (SEM) analysis equipment under conditions of 20,000x magnification, 3 kV, and 5,000x magnification, 5 kV.
[0135] At this time, the coating particles formed on the surface of the active material were marked on the SEM image, and the area ratio of the coating particles was calculated as follows.
[0136] Using the Image J program, the total 2D area of the primary particle was calculated from SEM images obtained under conditions of 20K and 3kV, and then the area of the island-shaped coating layer within the particle was calculated. (Island coating layer area / Total area) * 100%
[0137] 4. Evaluation of Initial Capacity and Initial Efficiency
[0138] After fabricating the coin cell, it was aged at 25°C for 12 hours, and then a charge / discharge test was conducted at 25°C. To evaluate the discharge capacity, the reference capacity was set to 200 mAh / g, and the cell was charged to 4.45V with a constant current of 0.1C. Then, the voltage was switched to a constant voltage, and charging continued until the termination current reached 0.05C. After a 10-minute rest time following charging, the cell was discharged until it reached 2.5V with a constant current of 0.1C and a reference capacity of 200 mAh / g.
[0139] 4. Room Temperature Resistance Evaluation
[0140] In the initial capacity evaluation, the initial resistance value was calculated using the current and voltage figures corresponding to the 60-second interval when charging to 4.45V at 0.1C and discharging to 2.5V at 0.1C. R = ΔV(60s - 0s) / ΔI(60s - 0s)
[0141] 5. High-temperature life evaluation (45℃, 50 cycles)
[0142] After fabricating a lithium secondary battery half cell, it was charged to 4.45V at 45℃ with a constant current of 0.5C, then switched to a constant voltage and charged until the termination current reached 0.05C. After a 10-minute rest time following charging, it was discharged with a constant current of 1.0C until it reached 2.5V. Fifty charge-discharge cycles were performed under these conditions, and the capacity retention rate of the 50th cycle was calculated relative to the first cycle.
[0143] 6. Evaluation of Residual Lithium
[0144] In the present invention, the residual lithium content can be obtained through the following method.
[0145] 5g of the above calcined material was dispersed in 100mL of distilled water for 5 minutes to prepare a mixed solution, and then only the solution containing dissolved Li was extracted from the mixed solution using a vacuum filter. A pH titration curve was obtained by measuring the change in pH value while titrating the extracted solution with 0.1M HCl. Using the above pH titration curve, the residual amount of LiOH and the residual amount of Li2CO3 in each calcined material were calculated, for example, as weight relative to the total weight of the active material.
[0146] In addition, the content of reactive lithium reacting in the post-calcination step within the above residual lithium, that is, the content of only the lithium (Li) element (e.g., by weight) among the residual LiOH and residual Li2CO3 remaining on the surface of the calcined product, can be calculated using the following formula.
[0147] Reacted Lithium (ppm) = Residual LiOH (ppm) * (Molecular Weight of Li / Molecular Weight of LiOH) + Residual Li2CO3 (ppm) * (Molecular Weight of Li / Molecular Weight of Li2CO3)
[0148] 7. Analysis Results
[0149] (1) Analysis based on calcination temperature, atmosphere, and type of additional lithium raw material
[0150] The characteristics of a positive electrode active material and a cell using the same were evaluated without performing a secondary coating under the conditions of the above examples and comparative examples, and without performing a secondary coating, and are shown in Table 1 below.
[0151] Figures 1 and 2 are SEM images of Examples 1 to 4 and Comparative Examples 1 to 4. Figure 2 is an enlarged image of Example 2 of Figure 1. In Figures 1 and 2, small particles located on the surface of the single-particle positive electrode active material are island-shaped coating particles.
[0152] Based on the two-dimensional SEM images, we checked the ratio of difference with respect to the area of the single-particle cathode active material. We compared the relative values with the comparative example using the area % ratio.
[0153] division Additional lithium raw material (content 0.02 mol) Heat treatment temperature (°C) Firing atmosphere Coating particle area ratio (%) Residual LH (wt%) Residual LC (wt%) Total residual lithium (wt%) 0.1C Initial capacity (mAh / g) Initial efficiency (%) 2C / 0.1C (%) Comparative Example 1 LiOH 650 O2 20.22% 0.08 0.16 0.24 206.3 90.4 87.8 Comparative Example 2 LiOH 700 O2 17.26% 0.09 0.11 0.19 206.9 90.2 88.3 Example 1 LiOH 750 O2 14.67% 0.08 0.09 0.17 207.7 91.3 89.0 Example 2 Li 2 CO 3 750 O2 9.58% 0.09 0.08 0.17 208.3 91.3 89.3 Comparative Example 3 LiOH 650 Air 21.50% 0.08 0.22 0.31 205.8 90.2 88.1 Comparative Example 4 LiOH 700 Air 15.58% 0.08 0.16 0.25 207.6 90.7 88.8 Example 3 Li 2 CO 3 750 Air 7.55% 0.08 0.14 0.22 208.7 91.2 89.1 Example 4 LiOH 750 Air 7.12% 0.07 0.14 0.22 209.8 91.4 89.3
[0154] As can be seen from Table 1, the initial capacity and efficiency are excellent only when the area of the Co-coated particles satisfies a predetermined range.
[0155] The surface area of these primary coating particles can be partially controlled by the heat treatment temperature and firing atmosphere of the primary coating. Specifically, while an O2 atmosphere is very important for forming a layered structure during the manufacturing stage of the cathode active material, it can be seen that the active material coated in an atmospheric atmosphere actually exhibits superior cell characteristics during the primary coating.
[0156] This can reduce oxygen usage in the actual commercialization process, offering significant advantages in terms of facility investment and raw materials.
[0157] Furthermore, when dry-coating Co, adding a portion of lithium raw material not only compensates for lithium loss occurring during the process due to residual lithium but also secures electrical properties by partially converting the coating material into a lithium-containing oxide form. In this case, both lithium hydroxide and lithium carbonate can be used as the input lithium raw material, and it can be seen that residual lithium issues do not occur significantly even when lithium carbonate is used.
[0158] (2) Analysis of whether to perform 1st and 2nd coatings simultaneously
[0159] Table 2 below shows the results of verifying whether the effect of the Co coating confirmed in Table 1 above can be obtained even when the first and second coatings are performed simultaneously. As mentioned in the above example, the Co coating was performed first, and then Al and W coatings were additionally performed.
[0160] Specifically, the temperature of the secondary coating selected in Table 1 was controlled to 430℃, and Al and W were added at 1500 ppm and 3000 ppm of the total mixture weight, respectively, mixed in a mixer, and heat-treated for 6 hours.
[0161] division Co Coating Co coating temperature (°C) Co firing atmosphere Al / W Coating Residual LH (wt%) Residual LC (wt%) Total residual lithium (wt%) 0.1C Initial capacity (mAh / g) Initial efficiency (%) Room temperature resistance (Ω) 2C / 0.1C (%) High-temperature resistance increase rate (%) High temperature lifespan (%) Comparative Example 5 X X X O 0.08 0.22 0.31 206.1 90.1 49.8 86.9 79.0 94.7 Comparative Example 6 0.08 0.21 0.29 207.7 90.4 44.6 88.1 79.0 94.8 Comparative Example 7 0.10 0.52 0.62 204.1 89.1 58.7 86.0 69.0 94.5 Comparative Example 8 0.08 0.22 0.29 206.3 90.3 46.9 87.9 81.0 94.6 Example 5 O 750 LC Air 0.04 0.19 0.22 209.8 91.7 27.9 89.7 59.0 94.9 Example 6 LC O 2 0.03 0.18 0.21 210.0 91.6 28.9 89.8 61.0 94.5 Example 7 LH Air 0.02 0.21 0.23 209.5 91.7 28.1 89.7 60.0 94.9 Example 8 LH O 2 0.03 0.19 0.22 210.1 91.7 28.2 89.3 63.0 94.7
[0162] As can be seen in Table 2, it can be confirmed that the battery characteristics of the example are superior in all aspects compared to Comparative Examples 5 to 8, in which only Al and W secondary coatings were performed.
[0163] Looking at Examples 5 and 7 among the examples, it can be seen that cell characteristics are actually improved when the atmosphere condition is atmospheric rather than when it is O2. This means that although residual lithium may be somewhat higher under atmospheric conditions, this does not lead to the predicted results in cell characteristics.
[0164] (3) Whether to add lithium and control of calcination temperature
[0165] Ni different from the precursor of the aforementioned example 0.64 Co0.04 Mn 0.32 Lithium carbonate was used as the lithium source for the (OH)2 precursor.
[0166] At this time, the molar ratio of lithium carbonate to metal in the precursor was controlled to 1.07. Subsequently, a single-particle cathode active material was prepared by calcining at 950°C for 6 hours under atmospheric conditions. The total residual lithium content of the prepared cathode active material was 9,400 ppm.
[0167] Unlike the previously described example, 0.02 mol of Co(OH)2 was added without adding additional lithium raw material, and a first coating was performed under the conditions of Table 3 below. At this time, a second coating was not performed.
[0168] Figures 3 and 4 are SEM images of the positive electrode active material according to the example and comparative example. Specifically, Figure 4 is an enlarged image of a portion of the SEM image in Figure 3.
[0169] division lithium raw materials Coating temperature (°C) Coating atmosphere Residual LH (wt%) Residual LC (wt%) Total residual lithium (wt%) 0.1C Initial capacity (mAh / g) Initial efficiency (%) Room temperature resistance (Ω) 2C / 0.1C (%) Comparative Example 9 Li2CO3 710 Air 0.11 0.15 0.26 199.1 89.3 32.0 84.1 Example 9 730 0.10 0.16 0.27 200.4 89.4 31.0 84.1 Example 10 750 0.10 0.15 0.25 200.5 89.7 30.3 84.8 Example 11 770 0.09 0.16 0.25 199.3 89.3 30.5 84.6 Comparative Example 10 790 0.08 0.16 0.24 199.5 89.2 31.6 84.7
[0170] As can be seen from Table 3 above, there are differences in cell characteristics depending on the primary coating temperature range. It can be observed that residual lithium decreases slightly as the coating temperature increases, but this reduction in residual lithium does not necessarily equate to an improvement in cell characteristics. Due to factors independent of residual lithium, it can be seen that optimal cell characteristics are secured only when the heat treatment temperature meets the appropriate temperature. One of these factors is believed to be the area ratio of coating particles, which can be confirmed in Table 1 above.
[0171] Conventional solid-state coatings are performed at excessively low temperatures (e.g., around 700°C), thereby maintaining the island coating area at a certain high level. Recognizing that this is not advantageous for improving cell characteristics, the inventors have proposed an optimal coating range.
[0172] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
Claims
Claim 1 A positive active material for a single-crystal lithium secondary battery, wherein the positive active material is represented by the following chemical formula 1, the positive active material comprises a form in which 1 to 20 single particles are aggregated, an island-shaped coating particle is located on the surface of the positive active material, and the coating particle satisfies the following mathematical formula 1. [Chemical Formula 1] Li a [Ni x Co y Mn z M w ]O2(In the above Chemical Formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0≤z≤0.4, 0≤w≤0.2, x+y+z+w=1, and M is Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.)[Mathematical Formula 1] Coating Cover Ratio ≤ 15 Area % (The above coating cover ratio is the area occupied by the coating particles within the SEM image of the positive active material unit particles relative to the total area within the SEM image of the positive active material unit particles, for a certain proportion of SEM images of the positive active material.) Claim 2 A positive electrode active material for a lithium secondary battery according to claim 1, satisfying the following mathematical formula 2. [Mathematical Formula 2] 7 Area % ≤ Coating Cover Ratio ≤ 15 Area % Claim 3 A positive electrode active material for a lithium secondary battery according to claim 1, wherein the coating particles comprise one or more selected from metal hydroxide, metal oxide, lithium metal hydroxide, and lithium metal oxide. Claim 4 A positive electrode active material for a lithium secondary battery according to claim 1, wherein the diameter of the island-shaped coating particles is 500 nm or less. Claim 5 delete Claim 6 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, comprising: a step of preparing a metal precursor; a step of mixing the metal precursor and a lithium raw material and calcining to obtain a positive electrode active material for a single-crystal lithium secondary battery; and a step of mixing the positive electrode active material and a coating raw material and heat-treating to obtain a positive electrode active material having island-shaped coating particles located on the surface; wherein the obtained positive electrode active material for a single-crystal lithium secondary battery is represented by the following chemical formula 1, and in the step of mixing the positive electrode active material and the coating raw material and heat-treating to obtain a positive electrode active material having island-shaped coating particles located on the surface, an additional lithium raw material is added, and the heat-treating temperature is 730℃ to 770℃. [Chemical Formula 1] Li a [Ni x Co y Mn z M w ]O2(in the above chemical formula 1, 0.8≤a≤1.2, 0.5≤x≤0.7, 0.05≤y≤0.2, 0≤z≤0.4, 0≤w≤0.2, x+y+z+w=1, and M is Zr, Y, B, Al, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.) Claim 7 A method for manufacturing a positive active material for a lithium secondary battery according to claim 6, wherein the step of mixing the positive active material and the coating raw material and then heat-treating to obtain a positive active material having island-shaped coating particles located on the surface is performed under atmospheric conditions. Claim 8 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 7, the above atmospheric conditions are carbon dioxide-free atmospheric conditions (CO2-free air, CFA). Claim 9 delete Claim 10 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 6, the additional lithium raw material is lithium hydroxide. Claim 11 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 6, the additional lithium raw material is lithium carbonate. Claim 12 A method for manufacturing a positive active material for a lithium secondary battery, wherein, in claim 6, the positive active material obtained by the step of mixing the positive active material and the coating raw material and then heat-treating to obtain a positive active material having island-shaped coating particles located on the surface, has a residual lithium of 0.23 weight% or less. Claim 13 delete Claim 14 A method for manufacturing a positive active material for a lithium secondary battery, wherein, in claim 6, the step of mixing the metal precursor and the lithium raw material and then calcining to obtain a positive active material for a single-crystal lithium secondary battery comprises: the step of mixing the metal precursor and the lithium raw material and then calcining to obtain a lithium metal oxide; and the step of dissolving the lithium metal oxide to obtain a positive active material for a single-crystal lithium secondary battery. Claim 15 A lithium secondary battery comprising: a positive electrode including a positive active material; a negative electrode; and an electrolyte located between the positive electrode and the positive electrode, wherein the positive active material includes the positive active material according to claim 1.
Citation Information
Patent Citations
Positive electrode active material and manufacturing method of the same
KR1020230162572A
Positive electrode active material and preparing method for the same
KR1020230162575A
Multi-element positive electrode material, preparation method thereof and lithium ion battery
CN116504979A
Positive electrode active material, producing method thereof, positive electrode and lithium secondary battery comprising the same