Anode active material for lithium secondary battery, manufacturing method of the same and lithium secondary battery comprising the same

A carbon-silicon mixed active material with optimized shrinkage density addresses the volume expansion issue in silicon-based anodes, improving both capacity and lifespan of lithium secondary batteries.

KR103046671B1Active Publication Date: 2026-11-11POSCO FUTURE M CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020230051290
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2026-11-11
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face challenges in achieving high energy density and long-term lifespan due to the rapid volume expansion of silicon-based anode materials, which disrupt the conductive path and degrade battery characteristics.

Method used

A carbon-based and silicon-based mixed negative electrode active material with a specific shrinkage density range of 0.80 to 1.01 g/cm³ is developed, achieved by optimizing the carbon-based active material through oxidation and the silicon-based active material through multi-stage grinding, to absorb the volume expansion of silicon during charging and discharging.

Benefits of technology

The solution improves both the capacity and lifespan characteristics of lithium secondary batteries by reducing the volume expansion rate of the electrode, thereby enhancing the battery's overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023044068348-PAT00004_ABST
    Figure 112023044068348-PAT00004_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material for a lithium secondary battery comprising a mixture of a carbon-based active material and a silicon-based active material, wherein the shrinkage density is 0.80 g / cm3 or higher at a compression pressure in the range of 700 to 1300 kgf / cm2, and the shrinkage density is defined as the difference between the pellet density and the tap density.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a negative electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same. More specifically, it relates to a negative electrode active material for a lithium secondary battery including a carbon-based active material and a silicon-based active material, a method for manufacturing the same, and a lithium secondary battery including the same. Background Technology

[0003] With the increasing technological development and demand for mobile devices, the demand for rechargeable, miniaturized, and high-capacity secondary batteries is rapidly rising. Recently, the use of secondary batteries as a power source for hybrid electric vehicles (HEVs) and electric vehicles (EVs) is becoming a reality.

[0004] Accordingly, much research is being conducted on secondary batteries that can meet various requirements, and in particular, there is a growing demand for lithium secondary batteries that have high energy density, high discharge voltage, and high output. Furthermore, lithium secondary batteries used in electric vehicles and the like must possess high energy density and the ability to deliver high output in a short period of time, and must be able to be used for more than 10 years under harsh conditions where charging and discharging with high current is repeated in a short period of time; therefore, output characteristics and long-term life characteristics that are significantly superior to existing small lithium secondary batteries are inevitably required.

[0005] In particular, as the demand for high-density energy batteries has recently increased, research is actively being conducted on methods to increase capacity by using silicon-based materials such as Si / C or SiOx, which have a capacity more than 10 times greater than that of graphite-based materials, as anode active materials. However, in the case of silicon-based materials, which are high-capacity materials, although their capacity characteristics are superior compared to the graphite used conventionally, there is a problem in that their volume expands rapidly during the charging process, disrupting the conductive path and degrading battery characteristics, which in turn degrades the battery's lifespan.

[0006] Accordingly, there is a need for research on graphite and silicon-based negative electrode active materials that can adequately secure both battery capacity and lifespan characteristics. The problem to be solved

[0008] Accordingly, one objective of the present invention is to provide a carbon-based and silicon-based mixed negative electrode active material capable of improving both the capacity and lifespan characteristics of a battery, a method for manufacturing the same, and a lithium secondary battery including the same. means of solving the problem

[0010] One embodiment of the present invention comprises a mixture of a carbon-based active material and a silicon-based active material, and has a magnetic field of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The present invention provides a negative electrode active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.

[0011] The above negative electrode active material for a lithium secondary battery is 1000 kgf / cm² 2 The shrinkage density at a compression pressure is 0.90 g / cm³ 3 It could be more than that.

[0012] The above negative electrode active material for a lithium secondary battery is 1300 kgf / cm² 2 The shrinkage density at a compression pressure of 1.00 g / cm³ 3 It could be more than that.

[0013] The above carbon-based active material may be natural graphite.

[0014] The degree of sphericity of the above carbon-based active material may be 0.87 or higher.

[0015] The above carbon-based active material may be oxidized.

[0016] The above silicon-based active material may be silicon.

[0017] The above silicon-based active material may have a circularity of 0.931 or higher.

[0018] The above silicon-based active material may have a crystal grain size of 175 nm or less.

[0019] The above silicon-based active material has a strain of 10×10 -5 It could be more than that.

[0020] The content of the silicon-based active material may be 4 to 6 weight percent based on the total weight of the mixture.

[0022] Another embodiment of the present invention is a method for manufacturing a negative electrode active material, comprising the steps of: preparing a carbon-based active material; preparing a silicon-based active material by first grinding, second grinding, and third grinding a silicon-based active material raw material; and mixing the carbon-based active material and the silicon-based active material to form a mixture, wherein the negative electrode active material has a gravitational force of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The present invention provides a method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.

[0023] In the step of preparing the carbon-based active material, the carbon-based active material may be natural graphite.

[0024] In the step of preparing the carbon-based active material, the carbon-based active material may have a degree of sphericity of 0.87 or higher.

[0025] After the step of preparing the carbon-based active material, the method may further include a step of oxidizing the prepared carbon-based active material by heat treating it under an air atmosphere.

[0026] The above heat treatment can be performed at a temperature of 500 to 700°C.

[0027] The above heat treatment can be performed for 30 minutes to 6 hours.

[0028] In the step of forming the above mixture, the content of the silicon-based active material may be 4 to 6 weight percent based on the total weight of the mixture.

[0030] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode; a negative electrode; an electrolyte; and a separator, wherein the negative electrode comprises the aforementioned negative electrode active material. Effects of the invention

[0032] A negative electrode active material for a lithium secondary battery according to one embodiment of the present invention can not only improve the capacity of the battery by including a silicon-based active material in addition to a carbon-based active material, but also minimize the deterioration of the battery's lifespan characteristics as the shrinkage density is sufficiently large. Brief explanation of the drawing

[0034] FIG. 1 is a schematic diagram of a negative electrode active material for a lithium secondary battery according to one embodiment of the present invention. Figure 2 is a graph showing the results of measuring the shrinkage density of the negative electrode active materials prepared according to Examples 1 to 3 and Comparative Examples 1 to 4. Figure 3 is a graph showing the results of the lifespan characteristics evaluation of lithium secondary batteries manufactured according to Examples 1 to 3 and Comparative Examples 1 to 4. Specific details for implementing the invention

[0035] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0036] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0037] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0038] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0039] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.

[0040] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.

[0041] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0043] 1. Cathode active material

[0044] FIG. 1 is a schematic diagram of a negative electrode active material for a lithium secondary battery according to one embodiment of the present invention. Hereinafter, a negative electrode active material for a lithium secondary battery according to one embodiment of the present invention will be described with reference to FIG. 1.

[0045] One embodiment of the present invention comprises a mixture of a carbon-based active material and a silicon-based active material, and has a magnetic field of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The present invention provides a negative electrode active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.

[0046] A negative electrode active material for a lithium secondary battery according to one embodiment of the present invention comprises a mixture of a carbon-based active material and a silicon-based active material. In addition to the carbon-based active material, the capacity characteristics of the battery can be improved by further including a silicon-based active material having a capacity at least 10 times greater. However, if the silicon-based active material is further included, the electrode volume expands rapidly during charging, thereby severing the conductive path and degrading the battery characteristics, and consequently, there is a problem in that the lifespan characteristics are significantly degraded as charging and discharging progress.

[0047] The inventors of the present invention have completed the present invention by conducting repeated research on a method to minimize the degradation of lifespan characteristics that occurs when the silicon-based active material is further included, and by discovering that if the shrinkage density of the active material is sufficiently large, the volume expansion rate of the electrode is reduced, thereby improving the battery lifespan characteristics.

[0049] A negative electrode active material for a lithium secondary battery according to one embodiment of the present invention has a polarity of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 That is the end, and more specifically, 0.805 g / cm³ 3 Above or 0.81 g / cm³ 3 It could be more than that.

[0050] In this specification, “shrinkage density” is defined as the difference between pellet density and tap density. Here, “pellet density” is a diameter of 2 cm 2 Pellet density is defined as the density measured after placing 2g of active material powder into a circular mold and applying a specific compression pressure. As can be seen from the definition above, this pellet density can vary depending on the value of the compression pressure applied to the active material powder, and generally increases as the compression pressure increases. "Tap density" is defined, based on ASTM-B527, as the density measured after placing 10g of active material powder into a 50mL container and tapping it at 3000 cycles @ 284 cycles / min. Unlike pellet density, tap density has a constant value. Pellet density has a higher value than tap density.

[0051] In the negative electrode active material for a lithium secondary battery according to one embodiment of the present invention, as the shrinkage density is sufficiently large as described above, the carbon-based active material absorbs the pressure generated by the volume expansion of the silicon negative electrode material during charging and discharging of the negative electrode as it shrinks, thereby reducing the volume expansion rate of the electrode during charging and discharging. Accordingly, the lifespan characteristics of the battery can be improved.

[0052] More specifically, the negative electrode active material for the lithium secondary battery is 700 kgf / cm² 2 The shrinkage density at a compression pressure is 0.80 g / cm³ 3 , 0.805 g / cm 3 or 0.81 g / cm³ 3 It could be more than that.

[0053] - More specifically, the negative electrode active material for the lithium secondary battery is 800 kgf / cm² 2 The shrinkage density at a compression pressure is 0.82 g / cm³ 3 , 0.835 g / cm 3 or 0.85 g / cm³ 3 It could be more than that.

[0054] More specifically, the negative electrode active material for the lithium secondary battery is 900 kgf / cm² 2 The shrinkage density at a compression pressure is 0.86 g / cm³ 3 , 0.875 g / cm 3 or 0.89 g / cm³ 3 It could be more than that.

[0055] More specifically, the negative electrode active material for the lithium secondary battery is 1000 kgf / cm² 2 The shrinkage density at a compression pressure is 0.90 g / cm³ 3 , 0.915 g / cm 3 or 0.92 g / cm³ 3 It could be more than that.

[0056] More specifically, the negative electrode active material for the lithium secondary battery is 1200 kgf / cm² 2 The shrinkage density at a compression pressure is 0.96 g / cm³ 3 , 0.975 g / cm 3 or 0.98 g / cm³ 3 It could be more than that.

[0057] More specifically, the negative electrode active material for the lithium secondary battery is 1300 kgf / cm² 2 The shrinkage density at a compression pressure of 1.00 g / cm³ 3 or 1.01 g / cm³ 3 It could be more than that.

[0058] More specifically, the negative electrode active material for the lithium secondary battery has a tap density of 0.80 to 0.95 g / cm³ 3 It could be.

[0060] The above carbon-based active material may be natural graphite. When the carbon-based active material is natural graphite, the shrinkage density of the active material can be more easily realized within the aforementioned numerical range, and the resulting improvement in battery performance can be realized more preferably.

[0061] The above carbon-based active material may have a sphericity of 0.87 or higher. When the sphericity of the carbon-based active material satisfies the above range, the adhesion between the active material and the current collector is improved, providing advantages in the manufacturing process and further enhancing the capacity and output characteristics of the battery. In this specification, “sphericity” refers to a numerical expression of the degree to which a particle is close to being spherical, and is defined as the value obtained by dividing the circumference of a circle having the same area as the projected shape of the particle by the actual circumference of the projected shape of the particle using a flow-type particle analysis device. Such sphericity can be measured using an analyzer for obtaining optical images (Fluid Imaging Technologies, Flowcam 8100) and analysis software (visual spreadsheet).

[0063] In particular, the carbon-based active material may be oxidized. Conventionally, to improve the lifespan characteristics of carbon-based active materials, low-crystallinity carbon materials, such as soft carbon or hard carbon, were generally coated onto the carbon-based active material. However, the carbon-based active material according to the present invention may be oxidized rather than coated with a low-crystallinity carbon material. As the carbon-based active material undergoes oxidation treatment, the internal pores increase, and the hardness of the graphite weakens. Consequently, a difference in density due to tapping of the powder and density due to compression occurs. Since this difference implies that the expansion pressure generated during charging and discharging of the mixed silicon can be absorbed, the shrinkage density of the active material can be more easily realized within the aforementioned numerical range, and the resulting improvement in battery performance can be more desirablely realized. On the other hand, if the carbon-based active material is coated with a low-crystallinity carbon material, the shrinkage density of the active material cannot be easily obtained within the aforementioned numerical range, making it unsuitable.

[0065] The silicon-based active material may be silicon particles. When the silicon-based active material is selected as the material, the shrinkage density of the active material can be more easily realized within the aforementioned numerical range, and the resulting improvement in battery performance can be more preferably realized.

[0067] Meanwhile, the silicon-based active material may have a circularity of 0.931 or higher.

[0068] In this specification, “circularity” refers to a numerical expression of the degree to which a particle is close to being circular, and is represented by collecting and analyzing data to divide the circumference of the particle shape into the circumference of a circle having an equivalent area using an individual 2D image of each particle through an image analysis device. Such circularity can be measured using an analyzer (Malvernpanalytical, Morphologi 4) for obtaining optical images.

[0070] In addition, the silicon-based active material may have a crystal grain size of 175 nm or less, and more specifically, 170 nm or less.

[0071] In this specification, the “grain size” can be measured by analyzing X-ray diffraction data of the cross-section of the active material using the Rietveld refinement method. For example, the grain size can be obtained by performing X-ray diffraction analysis under the following conditions using a Bruker D8 Discover with GADDS XRD instrument to acquire XRD data, and then processing the XRD data using Bruker’s DIFFRAC.TOPAS program. At this time, the full width at half maximum (FWHM) is set to be measured using the Caglioti equation.

[0072] <X-선 회절 분석 조건>

[0073] Light source: Cu-target, 45kV, 40mA output, wavelength=1.54Å

[0074] Detector: GaliPIX3D

[0075] Sample preparation: Approximately 2g of sample was filled into a 2cm diameter holder and loaded onto a rotation stage (ratiation stage).

[0076] Measurement time: Approx. 20 minutes

[0077] Measurement range: 2θ = 10° ~ 90°

[0079] In addition, the silicon-based active material has a strain of 10×10 -5 It may be more than, more specifically 10.3 × 10 -5- It could be.

[0080] In this specification, “strain” refers to a value measured through Rietveld refinement analysis of X-ray diffraction data, and the grating spacing It represents the average deviation of and is a value indicating the degree of deformation of the crystal lattice, satisfying the following equation.

[0081]

[0082] At this time, represents the full width of half the maximum value of the profile component associated with micro-strain expansion.

[0084] When the circularity, grain size, and strain of the silicon-based active material satisfy the above ranges, the stiffness and volume expansion characteristics with respect to the compression pressure of the powder are determined, so that the shrinkage density of the active material can be more easily realized within the aforementioned numerical range, and the resulting improvement in battery performance can be more preferably realized.

[0085] Various physical properties of these silicon-based active materials can be easily obtained by performing a multi-stage grinding process of first, second, and third grinding on the silicon-based active material raw materials during the manufacturing process. This will be explained in more detail in the method for manufacturing the negative electrode active material described later.

[0087] The content of the silicon-based active material may be 3 to 7 weight percent based on the total weight of the mixture, and more specifically, 4 to 6 weight percent. When the content of the silicon-based active material satisfies the above range, the effect of simultaneously realizing the capacity and lifespan characteristics of the battery can be more preferably realized. More specifically, if the content of the silicon-based active material is too low, the effect of improving battery capacity characteristics may be negligible, and if the content of the silicon-based active material is too high, the electrode expansion rate due to charging and discharging becomes too large, so the effect of improving battery lifespan characteristics may be negligible.

[0089] The above-described cathode active material may have an average particle size (D50) of 10 to 30 μm. In this specification, the average particle size (D50) may be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. The average particle size (D50) may be measured, for example, using a laser diffraction method.

[0090] The above-mentioned negative electrode active material has a specific surface area of ​​3 to 6 m² 2 It may be / g. In this specification, the specific surface area of ​​the active material may be measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020) for the active material powder.

[0091] Battery performance can be more preferably realized when the average particle size and specific surface area of ​​the negative electrode active material satisfy the above range.

[0093] 2. Method for manufacturing negative electrode active material

[0094] Another embodiment of the present invention is a method for manufacturing a negative electrode active material, comprising the steps of: preparing a carbon-based active material; preparing a silicon-based active material by first grinding, second grinding, and third grinding a silicon-based active material raw material; and mixing the carbon-based active material and the silicon-based active material to form a mixture, wherein the negative electrode active material has a gravitational force of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The present invention provides a method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.

[0095] A method for manufacturing a negative electrode active material according to another embodiment of the present invention is described in more detail step by step.

[0097] First, prepare a carbon-based active material.

[0098] The above carbon-based active material may be natural graphite.

[0099] At this time, the carbon-based active material may be obtained through a spheroidization process.

[0100] The above spheroidization may be performed using a general method in the industry for spheroidizing plate-shaped or flake-shaped carbon-based active material raw material powder.

[0102] In particular, after the step of preparing the carbon-based active material, the method may further include a step of oxidizing the prepared carbon-based active material by heat-treating it under an air atmosphere. The technical significance of oxidizing the carbon-based active material is as described above and is therefore omitted.

[0103] At this time, the heat treatment can be performed at a temperature of 500 to 700°C, and more specifically, at a temperature of 550 to 650°C. When the heat treatment temperature satisfies the above range, the effect of the aforementioned oxidation treatment can be more preferably realized. More specifically, if the heat treatment temperature is too low, the oxidation reactivity by oxygen is reduced, which may result in a lower shrinkage density of the active material, and if the heat treatment temperature is too high, there may be problems such as deterioration of battery characteristics due to structural collapse of spherical graphite caused by a violent oxidation reaction and increased costs due to low yield.

[0104] In addition, the heat treatment can be performed for 30 minutes to 6 hours, and more specifically, for 1 hour to 5 hours. When the heat treatment time satisfies the above range, the effects of the aforementioned oxidation treatment can be more preferably realized. More specifically, if the heat treatment time is too short, the natural graphite is oxidized less, the increase in internal pores is reduced, and consequently, the effect of absorbing the expansion of silicon is reduced, which may cause the battery lifespan to deteriorate. If the heat treatment time is too long, the high BET of the active material results in high viscosity during the electrode manufacturing process, leading to low processability and reduced yield, which may increase manufacturing costs, or severe adverse reactions with the electrolyte may cause the battery life characteristics to deteriorate.

[0106] Next, a silicon-based active material is prepared by sequentially grinding the silicon-based active material raw material in the first, second, and third stages. By grinding the silicon-based active material in the first, second, and third stages, the circularity, grain size, and strain of the silicon-based active material are controlled to an appropriate range, thereby allowing the shrinkage density of the active material to be more preferably realized.

[0107] More specifically, the silicon-based active material raw material may be metallic silicon powder, wherein the metallic silicon powder may contain 98% or more of silicon and other impurities based on the total weight.

[0108] The first crushing described above may be performed using crushing equipment commonly used in the industry and is not particularly limited. For example, the first crushing may be performed using a jaw crusher, but is not limited thereto.

[0109] The second grinding described above may be performed using grinding equipment commonly used in the industry and is not particularly limited. For example, the second grinding may be performed using one or more selected from a jet mill, ball mill, stirred media mill, roll mill, hammer mill, pin mill, disk mill, colloid mill, and atomizer mill, but is not limited thereto.

[0110] At this time, the second grinding can be performed two or more times. By performing the second grinding multiple times in this manner, the circularity and strain of the silicon-based active material can be further improved, and the grain size can be reduced, thereby maximizing the effect of improving battery performance.

[0111] The third grinding described above may be performed using grinding equipment commonly used in the industry and is not particularly limited. For example, the third grinding may be performed using one or more selected from a jet mill, a spiral jet mill, a ball mill, a stirred media mill, a roll mill, a hammer mill, a pin mill, a disk mill, a colloid mill, and an atomizer mill, but is not limited thereto.

[0113] Next, the carbon-based active material and the silicon-based active material are mixed to form a mixture. The negative electrode active material according to the present invention, which is the mixture formed thereby, has a polarity of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 That is all. The technical significance of the shrinkage density of the negative electrode active material according to the present invention satisfying the above range and a more detailed shrinkage density range are omitted as they are as described above.

[0114] At this time, the content of the silicon-based active material may be 3 to 7 weight% based on the total weight of the mixture, and more specifically, 4 to 6 weight%.

[0116] 3. Lithium secondary battery

[0117] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode; a negative electrode; a separator; and an electrolyte, wherein the negative electrode comprises the aforementioned negative electrode active material.

[0118] Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly of a positive electrode, a negative electrode, and a separator, and a sealing member sealing the battery container.

[0120] More specifically, the above-mentioned cathode may include a cathode current collector; and a cathode active material layer located on the cathode current collector and comprising the aforementioned cathode active material for a lithium secondary battery.

[0121] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0122] The above-mentioned cathode active material layer may optionally include a binder and / or a conductive material together with the cathode active material.

[0123] The above binder serves to improve adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The above binder may be included in an amount of 1 to 30 weight% based on the total weight of the negative electrode active material layer.

[0124] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special restrictions as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The above conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the negative electrode active material layer.

[0125] A negative electrode for a lithium secondary battery according to one embodiment of the present invention can be manufactured according to a conventional negative electrode manufacturing method, except for using the negative electrode active material described above.

[0126] Specifically, it can be manufactured by applying a composition for forming a negative electrode active material layer, comprising the aforementioned negative electrode active material and optionally a binder, a conductive material, and a solvent, onto a negative electrode current collector, followed by rolling and drying. At this time, the types and contents of the negative electrode active material, binder, and conductive material are as described above.

[0127] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that dissolves or disperses the cathode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for cathode manufacturing.

[0128] Alternatively, the cathode may be manufactured by casting the composition for forming the cathode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto a cathode current collector.

[0130] The above positive electrode may include a positive current collector and a positive active material layer disposed on the positive current collector, and the positive active material layer may include a positive active material.

[0131] The above-mentioned positive active material may be used without special restrictions as long as it is commonly used in the industry.

[0133] The above separator separates the positive and negative electrodes and provides a pathway for the movement of lithium ions. It can be used without special restrictions as long as it is typically used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0135] The above electrolytes may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which can be used in the manufacture of lithium secondary batteries, but are not limited thereto.

[0136] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0137] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.

[0138] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0139] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds like difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.

[0141] The embodiments of the present invention will be described in more detail below through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited by the following examples.

[0143] Example 1

[0144] (1) Manufacturing of cathode active material

[0145] (Preparation of carbon-based active material) Spherical natural graphite particles with an average particle size (D50) of 17 μm were heat-treated in a continuous rotary kiln under an air atmosphere at 600°C for 3 hours to undergo oxidation treatment, and then subjected to a classification process on a 45 μm sieve.

[0146] (Preparation of silicon-based active material) Metallurgical silicon powder was first ground using conventional grinding equipment. Subsequently, a second grinding and a second grinding were performed using a different type of conventional grinding equipment. Subsequently, a third grinding was performed using a different type of conventional grinding equipment. Afterward, silicon particles were prepared by ultrasonic classification.

[0147] (Mixing) The carbon-based active material and silicon-based active material prepared above were mixed to form a mixture, and a negative electrode active material was prepared with the content of the silicon-based active material being 5% by weight based on the total weight of the mixture.

[0148] (2) Cathode manufacturing

[0149] The above-mentioned cathode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethylcellulose (CMC) as a thickener were prepared. These were mixed in a mass ratio of 98.0:1.0:1.0 (cathode active material:binder:thickener) and dispersed in deionized distilled water to prepare a cathode active material composition. The composition was coated onto a Cu-foil current collector, followed by drying and rolling. During rolling, pressure conditions were varied to obtain an electrode density of 1.60 ± 0.05 g / cm³. 3 The cathode of was prepared.

[0150] (3) Lithium secondary battery manufacturing

[0151] A coin-type 2032 half-cell was fabricated using the above-mentioned negative electrode as the working electrode and metallic lithium as the counter electrode. At this time, a separator made of a porous polypropylene film was inserted between the working electrode and the counter electrode, and as the electrolyte, a mixed solution of diethyl carbonate (DEC) and ethylene carbonate (EC) with a mixed volume ratio of 7:3 and 1 M concentration of LiPF6 dissolved in it was used.

[0153] Example 2

[0154] A negative electrode active material and a lithium secondary battery were prepared in the same manner as in Example 1, except that in the carbon-based active material preparation step, natural graphite particles were heat-treated in a continuous rotary kiln under an air atmosphere at 600°C for 1 hour.

[0156] Example 3

[0157] A negative electrode active material and a lithium secondary battery were prepared in the same manner as in Example 1, except that in the carbon-based active material preparation step, natural graphite particles were heat-treated in a continuous rotary kiln under an air atmosphere at 600°C for 5 hours.

[0159] Comparative Example 1

[0160] A negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the carbon-based active material preparation step, a low-crystallinity carbon material was coated instead of oxidizing natural graphite particles. Specifically, the coating treatment was carried out by the following method.

[0161] Natural graphite particles and petroleum-based pitch were mixed in a weight ratio of 100:5, then mechanically mixed at 2000 rpm for 10 minutes in a high-speed stirrer to form a homogeneous mixture, heat-treated at 1200°C for 5 hours under a nitrogen atmosphere, and then classified through a 75 μm sieve.

[0163] Comparative Example 2

[0164] A negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the carbon-based active material preparation step, instead of oxidizing the natural graphite particles, the natural graphite particles and petroleum-based pitch were mixed in a weight ratio of 100:8 and then heat-treated.

[0166] Comparative Example 3

[0167] A negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the natural graphite particles were not oxidized during the carbon-based active material preparation step.

[0169] Comparative Example 4

[0170] A negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the silicon-based active material preparation step, the second grinding was applied only once.

[0172] Experimental Example 1: Evaluation of Active Material Properties

[0173] The physical properties of the cathode active materials prepared according to the examples and comparative examples were evaluated, and the results are shown in Tables 1 and 2 and Figure 2 below. The specific experimental methods are as follows.

[0174] (1) Evaluation of the degree of sphericity of carbon-based active materials

[0175] The degree of sphericity of carbon-based active material powder was evaluated by dividing the circumference of a circle having the same area as the particle projection shape by the actual circumference of the particle projection shape using a flow-type particle analysis device. This degree of sphericity can be measured using an analyzer for obtaining optical images (Fluid Imaging Technologies, Flowcam 8100) and analysis software (visual spreadsheet).

[0176] (2) Evaluation of the prototype of silicon-based active material

[0177] The circularity of silicon-based active material powders was evaluated by dividing the perimeter of the particle shape into the perimeter of a circle having an equivalent area, using an image analysis device to obtain individual 2D images of each particle. This circularity can be measured using an analyzer (Malvernpanalytical, Morpholgi 4) for obtaining optical images.

[0178] (3) Evaluation of silicon-based active material grain size and strain

[0179] XRD data of silicon-based active materials were measured using Bruker’s D8 Discover with GADDS XRD instrument, and crystal size and microstrain were measured using the Reitveld refinement method embedded in Bruker’s DIFFRAC.TOPAS program.

[0180] (4) Evaluation of active material (mixture) tap density

[0181] Based on ASTM-B527, 10g of active material powder was placed in a 50mL container and tapped at 3000 cycles @ 284 cycles / min to measure the packing density.

[0182] (5) Evaluation of shrinkage density of active material (mixture)

[0183] Diameter 2 cm 2 2g of active material powder is introduced into a circular mold at 700 kgf / cm² 2 , 800 kgf / cm 2 , 900 kgf / cm 2 , 1000 kgf / cm 2 , 1200 kgf / cm 2 , 1300 kgf / cm 2 The pellet density was measured by applying a compressive pressure and then measuring the density. Subsequently, the shrinkage density was derived by calculating the difference between the measured pellet density and the tap density.

[0184] (5) Evaluation of active material (mixture) particle size

[0185] The active material powder was measured using the laser diffraction method.

[0186] At this time, particle size (D10), particle size (D50), particle size (D90) and particle size (Dmax) each represent particle sizes corresponding to 10%, 50%, 90%, and 100% of the cumulative volume in the particle size distribution curve, and SPAN means (particle size (D90) - particle size (D10)) / particle size (D50).

[0187] (6) Evaluation of the specific surface area of ​​the active material (mixture)

[0188] The specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0189] Types of carbon-based active materials Surface treatment characteristics Sphericity of carbon-based active materials Types of silicon-based active materials Prototype of silicon-based active material Silicon-based active material grain size (nm) Silicon-based active material strain (×10 -5 ) Active material tab density (g / cm³) 3 ) Example 1 Oxidized natural graphite 3 hours of oxidation 0.88 silicone 0.931 168 10.5 0.89 Example 2 Oxidized natural graphite 1 hour of oxidation 0.89 silicone 0.931 168 10.5 0.89 Example 3 Oxidized natural graphite 5 hours of oxidation 0.87 silicone 0.931 168 10.5 0.89 Comparative Example 1 Coated natural graphite 3% coating 0.87 silicone 0.931 168 10.5 1.10 Comparative Example 2 5% coating 0.88 silicone 0.931 168 10.5 1.05 Comparative Example 3 natural graphite Micoting 0.91 silicone 0.931 168 10.5 0.97 Comparative Example 4 Oxidized natural graphite 3 hours of oxidation 0.88 silicone 0.93 180 9 0.93

[0190] Shrinkage density according to compression pressure Compression pressure (kg / cm²) 2 ) 700 800 900 1000 1200 1300 Example 1 0.89 0.93 0.97 1.00 1.06 1.09 Example 2 0.81 0.85 0.89 0.92 0.98 1.01 Example 3 0.99 1.03 1.07 1.10 1.16 1.19 Comparative Example 1 0.41 0.46 0.51 0.54 0.62 0.65 Comparative Example 2 0.34 0.39 0.44 0.47 0.55 0.58 Comparative Example 3 0.51 0.56 0.61 0.64 0.72 0.75 Comparative Example 4 0.61 0.64 0.66 0.70 0.75 0.78

[0191] D10(μm) D50(μm) D90(μm) Dmax(μm) SPAN Specific surface area (m²) 2 / g) Example 1 9.6 18.0 31.2 73.4 1.20 4.95 Example 2 9.5 17.8 29.0 62.0 1.10 4.10 Example 3 9.8 18.2 32.1 74.0 1.23 4.45 Comparative Example 1 10.4 18.1 27.6 61.7 0.95 1.68 Comparative Example 2 10.8 19.0 28.6 62.0 0.94 1.81 Comparative Example 3 9.4 18.4 29.7 52.0 1.1 4.41 Comparative Example 4 9.7 18.2 32 74 1.23 4.96

[0192] Referring to Tables 1 and 2 and Figure 2, in the case of Examples 1 to 3, oxidation-treated graphite was used as the carbon-based active material, and silicon particles with appropriately controlled roundness, grain size, and strain were used as the silicon-based active material through first, second, and third grinding, and it was confirmed that the shrinkage density was appropriately achieved within the target range.

[0193] On the other hand, in Comparative Examples 1 to 3, which used coated or uncoated natural graphite rather than oxidized natural graphite as a carbon-based active material, it was confirmed that the shrinkage density was too small.

[0194] In addition, in the case of Comparative Example 4, which was performed only once during the second silicon grinding process, it was confirmed that the silicon had a small circularity, a large grain size, and a small shrinkage density as the strain decreased.

[0196] Experimental Example 2: Evaluation of Cathode Volume Expansion Rate

[0197] The negative electrode volume expansion rate was evaluated after 30 cycles of charge and discharge in lithium secondary batteries prepared according to the examples and comparative examples, and the results are shown in Table 4 below.

[0198] More specifically, the thickness of the negative electrodes prepared according to the examples and comparative examples was measured, and after fabricating a lithium secondary battery CR2032 half-cell and aging it at 25°C for 30 hours, a charge-discharge test was conducted. To evaluate the expansion characteristics, the reference capacity was set to 500 mAh / g, and the battery was charged to 5 mV using a constant current of 0.5 C, then switched to a constant voltage and charged until the terminal current reached 0.005 C. After a 10-minute rest time following charging, the battery was discharged for 30 cycles using a constant current of 0.5 C with a reference capacity of 500 mAh / g until it reached 1.2 V. Subsequently, the battery was charged again to 5 mV using a constant current of 0.5 C, then switched to a constant voltage and charged until the terminal current reached 0.005 C. The battery was then disassembled, the electrodes were washed with DMC solvent for 5 minutes, and the electrode thickness was measured to calculate the negative electrode thickness expansion rate using the following formula.

[0199] <Equation 1>

[0200] Volume expansion rate (%) = (Decomposed electrode thickness after 30 cycles - Electrode thickness before assembly) / (Electrode thickness before assembly) X 100

[0201] Volume expansion rate (%) Example 1 41.6 Example 2 42.5 Example 3 38.4 Comparative Example 1 46.8 Comparative Example 2 50.6 Comparative Example 3 44.9 Comparative Example 4 43.8

[0202] Referring to Table 4, it was confirmed that the volume expansion rate of Examples 1 to 3 was significantly reduced compared to Comparative Examples 1 to 4. This can be interpreted as a result of controlling the shrinkage density of the cathode active material to an appropriate range.

[0204] Experimental Example 3: Evaluation of Battery Electrochemical Characteristics

[0205] The electrochemical characteristics of lithium secondary batteries prepared according to the examples and comparative examples were evaluated, and the results are shown in Table 5 and Figure 3 below. The specific experimental methods are as follows.

[0206] (1) Evaluation of initial discharge capacity and initial efficiency

[0207] After fabricating a CR2032 lithium secondary battery half-cell, a charge-discharge test was performed after aging it at 25°C for 30 hours. To evaluate the initial capacity, the reference capacity was set to 500 mAh / g, and the battery was charged to 5 mV with a constant current of 0.1 C. Then, the voltage was switched to a constant voltage, and charging continued until the terminal current reached 0.005 C. After a 10-minute rest time following charging, the battery was discharged until it reached 1.0 V with a constant current of 0.1 C and a reference capacity of 500 mAh / g.

[0208] (2) Evaluation of life characteristics

[0209] For the life characteristics, the device was charged to 5mV with a constant current of 0.5C at 25℃, then switched to a constant voltage and charged until the termination current reached 0.005C. After a 10-minute rest time following charging, the device was discharged with a constant current of 0.5C until it reached 1.2V. Thirty charge-discharge cycles were performed under these conditions, and the capacity retention rate of the 30th cycle was calculated relative to the first cycle.

[0210] Initial discharge capacity (mAh / g) Initial efficiency (%) Life characteristics (30 cycles, %) Example 1 498.8 90.1 78.8 Example 2 498.7 90.0 74.8 Example 3 489.7 89.2 81.8 Comparative Example 1 479.3 87.5 65.5 Comparative Example 2 469.1 84.2 63.0 Comparative Example 3 485.2 87.3 67.8 Comparative Example 4 495.5 90.0 68.5

[0211] Referring to Table 5, it was confirmed that the capacity and lifespan characteristics of the batteries in Examples 1 to 3 were significantly improved compared to Comparative Examples 1 to 4. This can be interpreted as a result of controlling the shrinkage density of the negative electrode active material to an appropriate range.

[0213] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.

[0214] Therefore, the substantive scope of the present invention shall be defined by the appended claims and their equivalents.

Claims

Claim 1 It comprises a mixture of carbon-based active material and silicon-based active material, and 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The above is as follows, wherein the shrinkage density is defined as the difference between the pellet density and the tap density, and the tap density is 0.80 to 0.95 g / cm³ 3 A negative electrode active material for a lithium secondary battery that is within the range. Claim 2 In paragraph 1, 1000 kgf / cm² 2 The shrinkage density at a compression pressure is 0.90 g / cm³ 3 Negative electrode active material for lithium secondary batteries. Claim 3 In paragraph 1, 1300 kgf / cm² 2 The shrinkage density at a compression pressure of 1.00 g / cm³ 3 Negative electrode active material for lithium secondary batteries. Claim 4 In claim 1, the carbon-based active material is a negative electrode active material for a lithium secondary battery, which is natural graphite. Claim 5 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the degree of sphericity of the carbon-based active material is 0.87 or higher. Claim 6 In claim 1, the carbon-based active material is an oxidized negative electrode active material for a lithium secondary battery. Claim 7 In claim 1, the silicon-based active material is a negative electrode active material for a lithium secondary battery, which is a silicon particle. Claim 8 In claim 1, the silicon-based active material is a negative electrode active material for a lithium secondary battery having a circularity of 0.931 or higher. Claim 9 In claim 1, the silicon-based active material is a negative electrode active material for a lithium secondary battery having a crystal grain size of 175 nm or less. Claim 10 In claim 1, the silicon-based active material has a strain of 10×10 -5 Negative electrode active material for lithium secondary batteries. Claim 11 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the content of the silicon-based active material is 4 to 6 weight% based on the total weight of the mixture. Claim 12 A method for manufacturing a negative electrode active material comprising: a step of preparing a carbon-based active material; a step of preparing a silicon-based active material by sequentially grinding a silicon-based active material raw material in a first grinding, a second grinding, and a third grinding; and a step of mixing the carbon-based active material and the silicon-based active material to form a mixture, wherein the negative electrode active material has a gravitational force of 700 to 1300 kgf / cm² 2 Shrinkage density at compression pressures in the range of 0.80 g / cm³ 3 The above is as follows, wherein the shrinkage density is defined as the difference between the pellet density and the tap density, and the tap density is 0.80 to 0.95 g / cm³ 3 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the second grinding is performed two or more times. Claim 13 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in the step of preparing the carbon-based active material, the carbon-based active material is natural graphite. Claim 14 In claim 12, a method for manufacturing a negative electrode active material for a lithium secondary battery in the step of preparing the carbon-based active material, wherein the carbon-based active material has a degree of sphericity of 0.87 or higher. Claim 15 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 12, after the step of preparing the carbon-based active material, the step of heat-treating the prepared carbon-based active material under an air atmosphere to oxidize it further comprises the step of oxidizing the prepared carbon-based active material. Claim 16 In claim 15, the method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the heat treatment is performed at a temperature of 500 to 700°C. Claim 17 In claim 16, the method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the heat treatment is performed for 1 to 5 hours. Claim 18 A method for manufacturing a negative electrode active material for a lithium secondary battery according to claim 12, wherein, in the step of forming the mixture, the content of the silicon-based active material is 4 to 6 weight percent based on the total weight of the mixture. Claim 19 A lithium secondary battery comprising a positive electrode; a negative electrode; an electrolyte; and a separator, wherein the negative electrode comprises a negative electrode active material according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Carbon material for nonaqueous secondary battery negative electrode and nonaqueous secondary battery

    JP2015185444A

  • Negative electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing negative electrode active material for nonaqueous electrolyte secondary battery, and negative electrode material for nonaqueous electrolyte secondary battery

    JP2017062974A

  • Negative electrode material of electrode and preparing method therefor

    KR1020130046423A