Manufacturing method of high hardness austenitic stainless steel using 3D printing and high hardness austenitic stainless steel by the method

The method addresses the challenge of achieving high hardness in austenitic stainless steel through controlled 3D printing composition and process conditions, reducing nickel content and using manganese, resulting in improved mechanical properties and cost-effectiveness without post-processing.

KR103046733B1Active Publication Date: 2026-11-10FOUND FOR RES & BUSINESS SEOUL NAT UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230057170
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2026-11-10
Estimated Expiration
2043-05-02

AI Technical Summary

Technical Problem

Existing metal 3D printing technologies for austenitic stainless steel face challenges in achieving high hardness without post-processing, which can lead to issues like difficulty in maintaining corrosion resistance and non-magnetism due to austenite-to-martensite transformation and increased manufacturing costs due to high nickel content.

Method used

A method for manufacturing high-hardness austenitic stainless steel using 3D printing with a controlled composition of carbon, manganese, chromium, nickel, and nitrogen, and optimized direct energy deposition process conditions, reducing nickel content and replacing it with manganese, to achieve hardness without post-processing.

Benefits of technology

The method results in high-hardness austenitic stainless steel with improved mechanical properties, reduced material loss, and lower costs, expanding its industrial application while avoiding issues associated with post-processing transformations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023049005838-PAT00006_ABST
    Figure 112023049005838-PAT00006_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing high-hardness austenitic stainless steel using 3D printing and high-hardness austenitic stainless steel produced thereby, comprising a process of manufacturing an additively formed body by a 3D printing method using a powder material comprising, based on total weight, 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities. The high-hardness austenitic stainless steel produced by 3D printing according to the present invention is not only economical as it replaces expensive nickel with manganese, but also has higher hardness than austenitic stainless steel produced by conventional processes without post-processing by using 3D printing, which can expand the scope of industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing austenitic stainless steel and austenitic stainless steel, and more specifically, to a method for manufacturing austenitic stainless steel having high hardness without post-processing technology by utilizing 3D printing technology, and to high-hardness austenitic stainless steel produced by the same. Background Technology

[0002] 3D printing technology is a technology that manufactures products with three-dimensional structures by stacking various forms of materials, such as powder, liquid, and wire, layer by layer, and has recently been receiving worldwide attention.

[0003] In particular, metal 3D printing technology is recognized as an innovative technology that can change the paradigm of existing manufacturing, as it can drastically reduce the time required for product development compared to traditional metal processing technologies such as casting, forging, welding, and extrusion, and further reduce the loss of raw materials because chips generated during cutting are not formed, and it can meet the demand for shapes and functions required by consumers.

[0004] However, research on metal 3D printing technology is still lacking globally. This is because, in order for metal 3D printing technology to move beyond the existing level of prototyping and become commercialized, the mechanical properties of products manufactured using metal 3D printing technology must be secured.

[0005] In addition, research on metal 3D printing is not progressing smoothly because metal 3D printing equipment is very expensive compared to conventional plastic 3D printing equipment, and manufacturing the materials (powder) used also requires additional research.

[0006] Meanwhile, austenitic stainless steel, which possesses excellent properties such as good corrosion resistance and non-magnetic characteristics, is utilized in various fields including aerospace, automotive, shipbuilding, and households.

[0007] However, recently, as the cost of nickel (Ni), a major element of austenitic stainless steel, has risen, there has been a problem of increasing manufacturing costs for austenitic stainless steel. To address this, there has been a need to develop a new composition of austenitic stainless steel that has properties equivalent to or better than existing austenitic stainless steel while lowering the nickel content.

[0008] In particular, high hardness is considered among various properties in order to take advantage of the beautiful surface of austenitic stainless steel. Since austenitic stainless steel manufactured through conventional processes generally has a hardness of 220 Hv or less, post-processing steps such as cold rolling (deep drawing, press forming, etc.) are added to improve hardness depending on the purpose.

[0009] However, when austenitic stainless steel is processed through post-treatment, the austenite transforms into martensite, which presents several problems, such as difficulty in maintaining corrosion resistance and non-magnetism, and the occurrence of delayed cracking. Prior art literature

[0010] Korean Registered Patent No. 10-2020507 (Published September 10, 2019) The problem to be solved

[0011] The present invention was developed to solve the above-mentioned necessities and problems, and aims to provide a method for manufacturing high-hardness austenitic stainless steel using 3D printing, which controls the nickel content of austenitic stainless steel and has excellent hardness without special post-processing by utilizing 3D printing technology, and to provide high-hardness austenitic stainless steel produced thereby. means of solving the problem

[0012] To achieve the above objective, the present invention provides a technical gist of a method for manufacturing high-hardness austenitic stainless steel using 3D printing, comprising a process of manufacturing an additively formed body by 3D printing using a powder material containing, based on total weight, 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities.

[0013] Here, it is preferable that the diameter of the powder material is less than 90 μm.

[0014] In addition, the 3D printing method is characterized by a direct energy deposition (DED) method, and the process conditions of the direct energy deposition method include a laser output of 350 to 450 W, a hatch spacing of 0.010 to 0.020 inch, and a laser speed of 30 to 50 inch / min.

[0015] In addition, based on the total weight, the high-hardness austenitic stainless steel produced by 3D printing using a direct energy deposition method comprises 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities. Effects of the invention

[0016] Since the present invention utilizes a 3D printing method, it has the effect of reducing the loss of raw materials compared to existing processes, and at the same time, it is more economical than conventional austenitic stainless steel by adding manganese to replace expensive nickel.

[0017] In addition, process conditions obtained through process optimization of the direct energy deposition method, a 3D printing method, can be used as basic data for the future development of 3D printing materials and parts.

[0018] In addition, since the austenitic stainless steel of the present invention has higher hardness than austenitic stainless steel manufactured by conventional processes, the scope of industrial application can be expanded.

[0019] In addition, since the austenitic stainless steel of the present invention does not require post-processing, it has the effect of eliminating problems such as the difficulty in maintaining corrosion resistance and non-magnetism due to the austenite-to-martensite transformation and the occurrence of delayed cracking that may occur during post-processing. Brief explanation of the drawing

[0020] FIG. 1 - A graph showing the X-ray diffraction analysis of a laminated body made of high-hardness austenitic stainless steel according to an embodiment of the present invention. FIG. 2 - An optical microscope image showing the microstructure of a laminated body made of high-hardness austenitic stainless steel according to an embodiment of the present invention. Fig. 3 - A figure showing optical microscope images of a laminated body made of austenitic stainless steel according to the diameter of the powder material and the specimen orientation. Fig. 4 - A figure showing the relationship between the porosity of an austenitic stainless steel laminate and the diameter of the powder material. Fig. 5 - A figure showing the relationship between the micro-Vickers hardness of an austenitic stainless steel additive body and the diameter of the powder material. Specific details for implementing the invention

[0021] The present invention relates to a method for manufacturing high-hardness austenitic stainless steel using 3D printing and high-hardness austenitic stainless steel produced thereby, and aims to provide a method for manufacturing high-hardness austenitic stainless steel using 3D printing with improved hardness without a post-processing step by reducing a portion of the nickel (Ni) content and replacing it with manganese (Mn), and adjusting the content of carbon (C) and nitrogen (N).

[0023] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0024] FIG. 1 is a graph showing X-ray diffraction analysis of an additive body made of high-hardness austenitic stainless steel according to an embodiment of the present invention, FIG. 2 is an optical microscope image showing the microstructure of an additive body made of high-hardness austenitic stainless steel according to an embodiment of the present invention, FIG. 3 is an optical microscope image showing the diameter of the powder material and the specimen direction of the additive body made of austenitic stainless steel, FIG. 4 is a figure showing the relationship between the porosity of an additive body made of austenitic stainless steel and the diameter of the powder material, FIG. 5 is a figure showing the relationship between the micro-Vickers hardness of an additive body made of austenitic stainless steel and the diameter of the powder material.

[0026] First, I would like to describe a method for manufacturing high-hardness austenitic stainless steel using 3D printing according to one embodiment of the present invention.

[0027] More specifically, the method for manufacturing a high-hardness austenitic stainless steel using 3D printing comprises a process of manufacturing an additively formed body by 3D printing using a powder material containing, based on total weight, 0.2 to 1.0 wt% carbon (C), 7.0 to 10.0 wt% manganese (Mn), 15.0 to 20.0 wt% chromium (Cr), 1.0 to 3.0 wt% nickel (Ni), 0.1 to 1.0 wt% nitrogen (N), and the remainder being iron (Fe) and unavoidable impurities.

[0028] First, the design of the composition of the above powder material will be explained.

[0029] According to one embodiment of the present invention, the composition of the powder material comprises, based on the total weight, 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities.

[0030] Hereinafter, since the microstructure and physical properties of austenitic stainless steel can change depending on the content of alloying elements, the roles of each alloying element added in the present invention will be explained.

[0031] Carbon (C)

[0032] The carbon mentioned above is a powerful austenite-stabilizing element and an element that increases the strength of the material through solid solution strengthening.

[0033] According to one embodiment of the present invention, the carbon may be 0.2 to 1.0 weight% based on 100 weight% of austenitic stainless steel, and is preferably 0.35 weight%. If it is less than 0.2 weight%, the strengthening of material strength due to solid solution strengthening may be insufficient, and if it is 1.0 weight% or more, deterioration of toughness and deterioration of weldability may occur due to an excessive increase in hardness.

[0034] Manganese (Mn)

[0035] The aforementioned manganese can improve the solubility of nitrogen as an austenite-stabilizing element, similar to carbon and nickel. Recently, manganese has been attracting attention as an alloying element that can replace nickel.

[0036] According to one embodiment of the present invention, the manganese may be 7.0 to 10.0 weight% based on 100 weight% of austenitic stainless steel, and among them, 8.50 weight% is preferred. If it is less than 7.0 weight%, it is difficult to obtain the effect of replacing nickel, and if it exceeds 10.0 weight%, weldability and toughness may be reduced.

[0037] chrome( Cr )

[0038] The aforementioned chromium is the most abundant element among the corrosion-resistant elements in stainless steel and is added as a basic component. However, if the chromium content is increased without limitation, hot workability may deteriorate, and the formation of phases other than austenite may cause a decline in mechanical properties and corrosion resistance.

[0039] According to one embodiment of the present invention, the chromium may be 15.0 to 20.0 weight% based on 100 weight% of austenitic stainless steel, and is preferably 17.50 weight%. If it is less than 15.0 weight%, it may not be easy to secure corrosion resistance, and if it is more than 20.0 weight%, the ferrite fraction increases, which hinders austenite stabilization and may increase manufacturing costs.

[0040] nickel( Ni )

[0041] Although the aforementioned nickel is the most important austenite-stabilizing element added to austenitic stainless steel, an increase in nickel content is directly linked to a rise in raw material prices; therefore, alloying elements capable of replacing nickel are currently being researched.

[0042] According to one embodiment of the present invention, the nickel may be 1.0 to 3.0 weight% based on 100 weight% of austenitic stainless steel, and among them, 2.20 weight% is preferred. If it is less than 1.0 weight%, it is difficult to obtain sufficient strength improvement, and if it exceeds 3.0 weight%, there is a disadvantage that manufacturing costs increase.

[0043] Nitrogen (N)

[0044] The aforementioned nitrogen can improve the strength and corrosion resistance of stainless steel in a chlorine atmosphere and expand the austenite region. However, since adding large amounts reduces hot workability and lowers the yield, it is limited to a specific weight percent.

[0045] According to one embodiment of the present invention, the nitrogen may be 0.1 to 1.0 weight% based on 100 weight% of the austenitic stainless steel, and is preferably 0.13 weight%. If it is less than 0.1 weight%, it is difficult to contribute to the stabilization of the austenite phase, and if it is more than 1.0 weight%, there is a problem of increasing the possibility of defects occurring in the steel.

[0046] In addition, the powder material according to one embodiment of the present invention may contain some unavoidable impurities, and the content of such impurities may be 10 weight% or less based on 100 weight% of the powder material. For example, alloying elements not listed above may be present up to 10 weight%, and the corresponding content of iron (Fe) may be reduced by 10 weight%. As unavoidable impurities, elements such as sulfur (S) may be included.

[0047] As such, in one embodiment of the present invention, 1.0 to 3.0 weight% of nickel is included relative to 100 weight% of the powder material, whereas the nickel content generally included in austenitic stainless steel is 7.0 weight% or more relative to 100 weight% of the total alloy. In one embodiment of the present invention, in order to control the content of expensive nickel, a portion of the nickel is replaced with manganese by including 7.0 to 10.0 weight% of manganese, and an alloy capable of improving corrosion resistance, strength, and hardness is designed by including 0.2 to 1.0 weight% of carbon and 0.1 to 1.0 weight% of nitrogen.

[0048] Accordingly, the preferred composition of the powder material according to one embodiment of the present invention may be a composition comprising 0.35 wt% carbon, 8.50 wt% manganese, 17.50 wt% chromium, 2.20 wt% nickel, and 0.13 wt% nitrogen based on the total weight of the powder material, and the remainder being iron and unavoidable impurities.

[0049] Meanwhile, the diameter distribution of the above powder material was prepared in four types: less than 45 μm, 45 μm or more and less than 63 μm, 63 μm or more and less than 90 μm, and 90 μm or more and less than 150 μm. As a result of analyzing the phase using an X-ray diffraction analyzer, it was confirmed that the above powder material has a complete austenite phase.

[0050] The following is a process for manufacturing an additively built body using the above powder material and the above 3D printing method.

[0051] 3D printing is a method that produces three-dimensional objects using an additive method rather than milling or cutting, so the shapes are more diverse compared to existing processes, and since chips generated during milling or cutting are not formed, it is a method that can reduce raw materials.

[0052] Generally, 3D printing can be classified into direct energy deposition (DED) and powder bed fusion (PBF) methods, and the 3D printing method of high-hardness austenitic stainless steel according to one embodiment of the present invention was carried out using the direct energy deposition method.

[0053] The above direct energy deposition method is a method of depositing materials by melting and bonding them using energy such as a high-power laser, electron beam, or plasma arc while spraying metal powder or wire directly onto the surface of an object. For example, a laser beam is irradiated onto a metal surface to temporarily create a molten pool, and metal powder is supplied to form a cladding layer.

[0054] However, no matter how excellent a material may be, if it is not controlled by appropriate process conditions when fed into a 3D printer, isolation or delamination may occur during 3D printing, and the layering may not proceed smoothly, so it may be important to find optimal printing process conditions.

[0055] According to one embodiment of the present invention, the 3D printing was performed on the powder material using a LENS device with a direct energy deposition method. The process conditions of the direct energy deposition method may include a laser output of 350 to 450 W, a hatch spacing of 0.010 to 0.020 inch, and a laser speed of 30 to 50 inch / min.

[0056] The output of the laser used for the 3D printing according to one embodiment of the present invention may be 350 to 450 W, and preferably 400 W. If the output of the laser is less than 350 W, sufficient melting may not occur, and if it exceeds 450 W, it may have an unintended effect on the underlying layer.

[0057] In addition, the hatch spacing used in the 3D printing according to one embodiment of the present invention may be 0.010 to 0.020 inches, and preferably 0.015 inches. This is because if the hatch spacing is less than 0.010 inches, the melting zones of the powder material may overlap, and if it is 0.020 inches or more, heat transfer to the applied powder material may be insufficient.

[0058] In addition, the laser speed used for the 3D printing according to one embodiment of the present invention may be 30 to 50 inch / min, and preferably 40 inch / min. This is because when the laser speed is less than 30 inch / min, it is not efficient, and when it exceeds 50 inch / min, there is a possibility that partial melting will occur and peeling will occur.

[0059] Accordingly, the 3D printing process according to one embodiment of the present invention may include process conditions such as a laser output of 400 W, a hatch spacing of 0.015 inch, and a laser speed of 40 inch / min, using the direct energy deposition method.

[0060] The process conditions obtained through process optimization of the direct energy deposition method, which is the 3D printing method mentioned above, can be used as basic data for the future development of 3D printing materials and parts.

[0061] Accordingly, one embodiment of the present invention comprises, based on total weight, 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities, and provides a method for manufacturing high-hardness austenitic stainless steel using direct energy deposition 3D printing and high-hardness austenitic stainless steel produced thereby.

[0063] The present invention will be described below with reference to embodiments and comparative examples, but the following embodiments are intended to illustrate the invention and the scope of the invention is not limited thereto.

[0064] <Example 1>

[0065] Based on 100 wt% of the powder material, the composition includes 0.35 wt% carbon, 8.50 wt% manganese, 17.50 wt% chromium, 2.20 wt% nickel, 0.13 wt% nitrogen, and the remainder being iron and unavoidable impurities. The diameter distribution of the powder material is less than 45 μm. The 3D printing process conditions are a direct energy deposition method, and 3D printing is performed with a laser output of 400 W, a hatch spacing of 0.015 inch, and a laser speed of 40 inch / min to manufacture an additively manufactured body.

[0067] <Example 2>

[0068] It is the same as Example 1, except that the diameter distribution of the powder material is 45 μm or more and less than 63 μm.

[0070] <Example 3>

[0071] It is the same as Example 1, except that the diameter distribution of the powder material is 63 μm or more and less than 90 μm.

[0073] <Comparative Example 1>

[0074] Except for the diameter distribution of the powder material being 90 μm or more and less than 150 μm, it is the same as Example 1.

[0076] Below, we will examine the X-ray diffraction analysis results, optical microscope observation results, and hardness measurement results of the laminated bodies manufactured according to the embodiments and comparative examples of the present invention.

[0077] FIG. 1 is a graph showing the X-ray diffraction analysis of a laminated body made of high-hardness austenitic stainless steel according to an embodiment of the present invention. According to one embodiment of the present invention, the laminated body manufactured under the above conditions was confirmed to have a complete austenite phase as a result of analyzing the phase through an X-ray diffraction analyzer as shown in FIG. 1.

[0078] In addition, FIG. 2 is an optical microscope image showing the microstructure of an additive body made of high-hardness austenitic stainless steel according to an embodiment of the present invention. As shown in FIG. 2, the additive body manufactured by 3D printing according to an embodiment of the present invention can exhibit a wide variety of microstructures depending on melting, solidification, and phase transformation by a laser.

[0079] In addition, Fig. 3 is a diagram showing optical microscope images according to the diameter of the powder material and the direction of the specimen of the additive body made of austenitic stainless steel. As shown in Fig. 3, optical microscope observation results show that pores exist inside all of the additive bodies, which are created by the gas introduced during the 3D printing process and are generally spherical in shape.

[0080] Meanwhile, some pores are formed by cracks caused by thermal stress and incompletely melted powder material, have irregular shapes, and can act as crack initiation points, which can cause a decrease in mechanical properties.

[0081] According to Figure 3, as the diameter of the powder material increases, the pores increase, and when the diameter of the powder material is 90 μm or more and less than 150 μm, the diameter of the pores reaches about 100 μm, so it does not meet the suitable conditions.

[0082] In addition, Figure 4 is a figure showing the relationship between the porosity of an austenitic stainless steel laminate and the diameter of the powder material. As the diameter of the powder material increases, the porosity tends to increase. When the diameter of the powder material is 90 μm or more and less than 150 μm, the porosity deteriorates rapidly, so the diameter of the powder material being less than 90 μm is an appropriate range.

[0083] In addition, to measure the hardness of the laminated bodies manufactured according to the embodiments and comparative examples of the present invention, the surface hardness was measured using a Vickers hardness tester.

[0084] Vickers hardness is a hardness value obtained by lightly pressing a pyramid-shaped diamond indenter with a face angle of 136° against the surface of a material to create a pit, and then dividing the load by the surface area of ​​the permanent pit remaining after the load is removed. By making the load very small, the hardness can be measured directly on the surface of the product.

[0085] In addition, a testing machine that can be used with a load of 1 kg or less is specifically called a microhardness tester, and since the pit is very small, it is also used to determine the hardness distribution of a test surface or to measure the hardness of a small part of a metal structure. The hardness obtained in this case is called micro-Vickers hardness.

[0086] Accordingly, in the present invention, micro-Vickers hardness was measured to measure the surface hardness of the laminated body. At this time, the indentation force was 50gf and the dwell time was 15 seconds.

[0087] [Table 1]

[0088]

[0089] Table 1 shows the measurement results of the porosity and micro-Vickers hardness of the laminated body with respect to the diameter of the powder material. As described above with respect to FIG. 4, regarding the porosity of the laminated body, Examples 1 to 3 showed a value of less than 1%, while Comparative Example 1 showed a value of 2.5%.

[0090] In addition, Figure 5 is a graph showing the relationship between the micro-Vickers hardness of an austenitic stainless steel laminated body and the diameter of the powder material. As shown in Table 1 and Figure 5, Examples 1 to 3 showed a micro-Vickers hardness of 300 Hv or higher, whereas Comparative Example 1 showed 299 Hv. Although the micro-Vickers hardness measurement results showed similar values ​​in the Examples and Comparative Examples, the porosity of the Comparative Example increased rapidly compared to the Examples.

[0091] Accordingly, based on the measurement results of the porosity and the micro-Vickers hardness, it is preferable that the diameter of the powder material used for the 3D printing be less than 90 μm, where the porosity is 1% or less. At this time, it can be confirmed that the porosity is 1% or less and the micro-Vickers hardness is 300 Hv or more. In addition, the diameter of the powder material used for the 3D printing may more preferably be less than 45 μm, where the porosity is lowest.

[0092] In addition, while the Vickers hardness of general forged austenitic stainless steels such as STS316 and STS304 is 220 Hv or less, the Vickers hardness of the embodiment of the present invention is 300 Hv or more, so it can be said that the embodiment of the present invention exhibits significantly superior characteristics in terms of hardness.

[0093] Accordingly, in the embodiments of the present invention, by reducing the nickel content compared to general austenitic stainless steel and controlling the carbon and nitrogen content, it can be confirmed that measurement results superior to the hardness of general austenitic stainless steel can be obtained using only a 3D printing process without a post-processing process.

[0094] Thus, the present invention can provide a high-hardness austenitic stainless steel manufactured by a 3D printing method having a porosity of 1% or less and a micro-Vickers hardness of 300 Hv or more.

[0096] Accordingly, while the nickel content in general austenitic stainless steel is 7.0 wt% or more relative to 100 wt% of the total alloy, the present invention reduces costs by controlling the content of expensive nickel to 1.0 to 3.0 wt% and including 7.0 to 10.0 wt% of manganese instead of nickel, thereby replacing some of the nickel with manganese.

[0097] In addition, austenitic stainless steel generally undergoes post-processing steps such as cold rolling to increase hardness. However, in such cases, as austenite transforms into martensite, the elongation decreases, it becomes difficult to maintain corrosion resistance and non-magnetism, and problems such as delayed cracking may occur. However, the present invention improves hardness without post-processing by controlling the carbon and nitrogen content and optimizing process conditions using a 3D printing method. This resolves the problems associated with post-processing, thereby increasing industrial utility. Furthermore, the optimized process conditions obtained can be utilized as basic data for the future development of 3D printing materials and parts.

[0098] Therefore, the high-hardness austenitic stainless steel produced by 3D printing according to the present invention reduces costs by controlling the nickel content, controls the carbon and nitrogen content, and maintains high hardness without additional post-processing by using 3D printing, so it is economically advantageous and the scope of industrial application can be expanded.

Claims

Claim 1 A method for manufacturing high-hardness austenitic stainless steel using 3D printing, comprising a process of manufacturing an additively formed body on the surface of an object by a 3D printing method using a powder material comprising, based on total weight, 0.2 to 1.0 wt% carbon (C), 7.0 to 10.0 wt% manganese (Mn), 15.0 to 20.0 wt% chromium (Cr), 1.0 to 3.0 wt% nickel (Ni), 0.1 to 1.0 wt% nitrogen (N), and the remainder being iron (Fe) and unavoidable impurities, wherein the manganese replaces nickel by lowering the nickel content to 3.0 wt% or less based on 100 wt% of the powder material, and the 3D printing method comprises irradiating a laser beam onto a metal surface to create a molten pool on the metal surface, supplying a powder material to the molten pool on the metal surface to melt and cool the powder material in the molten pool on the metal surface. A method for manufacturing high-hardness austenitic stainless steel using 3D printing, characterized in that the direct energy deposition (DED) method includes forming a cladding layer, the laser beam is irradiated with a laser output of 350 to 450 W, a hatch spacing of 0.010 to 0.020 inch, and a laser speed of 30 to 50 inch / min, and the diameter of the powder material is less than 90 μm. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 A high-hardness austenitic stainless steel, manufactured on the surface of an object by 3D printing of a powder material having a diameter of less than 90 μm and containing 0.2 to 1.0 wt% carbon, 7.0 to 10.0 wt% manganese, 15.0 to 20.0 wt% chromium, 1.0 to 3.0 wt% nickel, 0.1 to 1.0 wt% nitrogen, and the remainder being iron and unavoidable impurities based on total weight, wherein the manganese replaces nickel by lowering the nickel content to 3.0 wt% or less based on 100 wt% of the powder material, and wherein the powder material has a porosity of less than 1.0% when the diameter is maintained at less than 90 μm, and exhibits a micro-Vickers hardness of 300 Hv or higher.

Citation Information

Patent Citations

  • Mold steel powder and method of preparing the same

    KR1020200080371A

  • Stainless steel powder for molding

    KR1020200104288A