Cathode active material for lithium secondary battery, manufacturing method of the same and lithium secondary battery comprising the same

By forming cobalt and boron coating layers on high-nickel cathode active materials through controlled heat treatments, the method addresses stability issues, resulting in improved capacity and electrochemical performance of lithium-ion batteries.

KR103046747B1Active Publication Date: 2026-11-11POSCO HLDG INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020250149882
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-10-16
Publication Date
2026-11-11
Estimated Expiration
2045-10-16

AI Technical Summary

Technical Problem

Conventional cathode active materials face challenges in maintaining structural stability as nickel content increases, limiting the capacity improvement of lithium-ion batteries used in electric vehicles.

Method used

A method involving the formation of a first coating layer with cobalt and a second coating layer with boron on the surface of a high-nickel metal oxide, optimized through specific heat treatment temperatures, to enhance capacity and stability.

Benefits of technology

The method results in a cathode active material with improved capacity characteristics and stability, enhancing electrochemical performance and reducing resistance, thereby increasing the lifespan and capacity retention of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025115791814-PAT00001_ABST
    Figure 112025115791814-PAT00001_ABST
Patent Text Reader

Abstract

The present embodiments relate to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same. A positive electrode active material for a lithium secondary battery according to one embodiment comprises a metal oxide containing elements lithium, nickel, cobalt, and manganese; a cobalt coating layer coated on the surface of the metal oxide, and a boron coating layer coated on the surface of the cobalt coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same. Background Technology

[0002] As the application range of lithium-ion batteries expands from small electronic devices to electric vehicles and power storage devices, there is a growing demand for cathode materials with excellent high energy density and high power characteristics.

[0003] In this regard, there is a demand for electric vehicles capable of long-distance driving, and high-energy-density lithium-ion batteries to meet this need. Among the components of lithium batteries, the cathode active material determines the energy density and price of the lithium-ion battery. Conventional cathode active materials exhibit capacity by storing lithium within the phase.

[0004] In particular, as technology advances in the EV market, high-capacity batteries and cathode active materials are essential for securing driving range. Therefore, nickel-based cathode active materials have traditionally been developed to enhance capacity, and further developments are underway to increase capacity by raising the nickel content or increasing the charging voltage. The problem to be solved

[0005] In this embodiment, we aim to provide a positive electrode active material for a lithium secondary battery having excellent capacity characteristics, a method for manufacturing the same, and a lithium secondary battery including the same. means of solving the problem

[0006] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment comprises the steps of: mixing a metal hydroxide containing nickel, cobalt, and manganese with a lithium raw material and then calcining to obtain a metal oxide; grinding the metal oxide; mixing the ground metal oxide and a cobalt raw material and then performing a first heat treatment to form a metal oxide having a first coating layer containing cobalt formed on the surface of the metal oxide; and mixing a raw material containing boron with the metal oxide having the first coating layer formed and then performing a second heat treatment to obtain a positive electrode active material having a second coating layer containing boron formed on the surface of the first coating layer; wherein the first heat treatment is performed at a temperature greater than 740°C and less than 850°C.

[0007] The above first heat treatment can be carried out at a temperature of 790℃ to 830℃.

[0008] The above cobalt raw material may include Co(OH)2.

[0009] The raw material containing the above boron may include at least one of H3BO3, B2O3, B4C, Li2B4O7, Li3BO3, W2B, WB, WB2, and WB4.

[0010] In the step of forming the first coating layer, the cobalt raw material may be mixed by adding it in a content range of 1.5g to 2.5g based on 100g of the crushed metal oxide.

[0011] The step of forming the first coating layer may be a step of coating the surface of the metal oxide obtained in the step of forming the first coating layer with cobalt in an amount of 1 mol% to 5 mol% based on the total number of moles (100 mol%) of atoms constituting the surface of the metal oxide.

[0012] In the step of forming the second coating layer, the raw material containing boron may be mixed by adding it in a content range of 0.1g to 1g based on 100g of the metal oxide on which the first coating layer is formed.

[0013] The above first heat treatment may be performed for 10 to 30 hours.

[0014] The above secondary heat treatment may be performed at 200°C to 500°C for 3 to 18 hours.

[0015] The above metal oxide may be represented by the following chemical formula 1.

[0016] [Chemical Formula 1]

[0017] Li a (Ni b Co c Mn d )O2

[0018] In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤b≤0.99, 0.01≤c≤0.1, 0.01≤d≤0.1, and b+c+d = 1.

[0019] In the above chemical formula 1, b may be in the range of 0.85 ≤ b ≤ 0.99.

[0020] A positive active material for a lithium secondary battery according to another embodiment is a positive active material comprising Ni, Co, and Mn, wherein the positive active material comprises a first coating layer containing Co on its surface, and the first coating layer comprises a second coating layer containing B on its surface, and the positive active material exhibits a t1 value between 200 and 250 when exponential fitting is performed on a B1s XPS depth profile.

[0021] The above positive active material may have a nickel content of 80% or more.

[0022] A positive electrode for a lithium secondary battery according to another embodiment may include a positive electrode active material according to one embodiment.

[0023] A lithium secondary battery according to another embodiment may include a positive electrode comprising a positive electrode active material according to one embodiment. Effects of the invention

[0024] According to the present embodiment, through an optimized method of coating cobalt and boron on a high-nickel NCM cathode active material, a cathode active material with improved capacity characteristics can be realized while maintaining the stability of nickel. Brief explanation of the drawing

[0025] Figure 1 is B1s XPS depth profile data according to Example 1, Example 2 and Comparative Examples 1 to 3. Figure 2 is a scanning electron microscope (SEM) image of the positive electrode active material of Example 1. Figure 3 is a scanning electron microscope (SEM) image of the positive electrode active material of Example 2. Figure 4 is a scanning electron microscope (SEM) image of the positive electrode active material of Comparative Example 1. Figure 5 is a scanning electron microscope (SEM) image of the positive electrode active material of Comparative Example 2. Figure 6 is a scanning electron microscope (SEM) image of the positive electrode active material of Comparative Example 3. Specific details for implementing the invention

[0026] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0027] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0028] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0029] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0030] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.

[0031] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.

[0032] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0034] Method for manufacturing a positive electrode active material for a lithium secondary battery

[0035] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment comprises the steps of: mixing a metal hydroxide containing nickel, cobalt, and manganese with a lithium raw material and then calcining to obtain a metal oxide; grinding the metal oxide; mixing the ground metal oxide and a cobalt raw material and then performing a first heat treatment to form a metal oxide having a first coating layer containing cobalt formed on the surface of the metal oxide; and mixing a raw material containing boron with the metal oxide having the first coating layer formed and then performing a second heat treatment to obtain a positive electrode active material having a second coating layer containing boron formed on the surface of the first coating layer; wherein the first heat treatment is performed at a temperature greater than 740°C and less than 850°C.

[0036] That is, a method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment may include the steps of obtaining a metal oxide, washing the metal oxide with water, and forming a first coating layer and a second coating layer on the surface of the washed metal oxide.

[0037] High-nickel based cathode active materials have the advantage of being able to increase capacity as the nickel content is increased. However, as the nickel content increases, structural stability deteriorates due to the characteristic that nickel trivalent ions are unstable in the layered structure. Consequently, there are limits to improving capacity while increasing the nickel content. Therefore, it is important to develop technology to secure capacity within a nickel content range where stability is maintained.

[0038] One embodiment aims to present a Boron coating method to enhance the capacity of a high-nickel cathode active material through heterogeneous element coating rather than by increasing the nickel content, and to present a coating method for optimizing the said coating process.

[0039] Specifically, the step of obtaining the metal oxide can be carried out by mixing a metal hydroxide containing nickel, cobalt, and manganese with a lithium raw material and then calcining it.

[0040] The above metal hydroxide can be produced, for example, by preparing an aqueous metal salt solution containing nickel raw material, cobalt raw material, manganese raw material, and distilled water, and then supplying the aqueous metal salt solution to a co-precipitation reactor, and this can be carried out according to a method for producing metal hydroxides generally known in the art.

[0041] At this time, the nickel raw material may be, for example, a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide. More specifically, the nickel raw material may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salt, nickel halide, or a combination thereof.

[0042] The above cobalt raw material may be, for example, a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide. More specifically, the above cobalt raw material is CoSO 4,  It may be CoSO4ㆍ7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O, or a combination thereof.

[0043] The above manganese raw material may be, for example, a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof.

[0044] More specifically, the manganese raw material may be manganese salts such as MnSO4, MnSO4·H2O, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid salts, manganese oxides such as Mn2O3, MnO2, and Mn3O4, oxyhydroxides, manganese chloride, or combinations thereof.

[0045] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment first performs the step of mixing the metal hydroxide and the lithium raw material and then calcining to obtain a metal oxide.

[0046] At this time, the lithium raw material may be, for example, a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it is soluble in water. More specifically, the lithium raw material may include at least one of LiOH, Li2CO3, LiNO3, LiNO2, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof.

[0047] The calcination in the step of obtaining the metal oxide can be performed at 600°C to 1000°C, and more specifically, at 600°C to 990°C, 700°C to 970°C, or 720°C to 950°C.

[0048] The calcination in the step of obtaining the metal oxide can be performed for 5 to 20 hours, and more specifically, for 5 to 15 hours or 8 to 14 hours.

[0049] The calcination in the step of obtaining the above metal oxide can be performed by dividing it into preliminary calcination and main calcination as necessary.

[0050] Next, the step of grinding the obtained metal oxide can be performed.

[0051] Specifically, the obtained metal oxide can be ground through a jet-mill process so that aggregated particles can fall off during firing. For example, the particle size of the metal oxide ground in this way may be D50 = 2.5 to 6.0 μm.

[0052] Next, the step of washing the obtained metal oxide can be performed.

[0053] The above washing is intended to remove residual lithium present on the surface of the metal oxide and can be performed, for example, using distilled water. Specifically, the washing process can be performed by mixing 50 to 150 parts by weight of distilled water with respect to 100 parts by weight of the metal oxide.

[0054] Subsequently, the step of forming a metal oxide in which a first coating layer containing cobalt is formed on the surface of the metal oxide is performed by mixing the above-mentioned crushed (and washed) metal oxide and cobalt raw material and then performing a first heat treatment.

[0055] The above cobalt raw material may include Co(OH)2, and the aforementioned CoSO 4,  CoSO4·7H2O, Co(OH)2, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or combinations thereof may also be used.

[0056] The above first heat treatment must be performed at a temperature greater than 740°C and less than 850°C. Controlling the temperature range of the first heat treatment as described above ensures that the second coating layer containing boron, which is subsequently coated, is coated smoothly and sufficiently, allowing the boron to diffuse evenly across the surface of the first coating layer. Since the capacity characteristics of the positive electrode active material for a lithium secondary battery according to one embodiment can be improved only when the boron is evenly diffused across the surface of the first coating layer, controlling the temperature range of the first heat treatment is very important. If the temperature of the first heat treatment is 740°C or lower or 850°C or higher, it is not possible to improve the capacity characteristics while maintaining the stability of nickel.

[0057] For example, the above first heat treatment can be carried out at a temperature of 790°C to 830°C.

[0058] In this embodiment, the cobalt raw material may be obtained by grinding a raw material containing cobalt to produce a powder having an average particle size of 400 nm or less, more specifically in the range of 100 nm to 400 nm. When the average particle size of the cobalt raw material satisfies the above range, the surface resistance is significantly reduced, allowing for high electrochemical properties to be obtained and enabling homogeneous coating.

[0059] In the step of forming the first coating layer, the cobalt raw material can be added and mixed in a content range of 1.5g to 2.5g, more specifically 1.5g to 2.2g or 1.5g to 2.0g, based on 100g of the crushed (and washed) metal oxide. The cobalt raw material must be added in the above range so that the surface of the metal oxide obtained in the step of forming the first coating layer can be coated with cobalt in a range of 1 mol% to 5 mol% based on the total molar amount (100 mol%) of atoms constituting the surface of the metal oxide. When cobalt is coated in the above mol% range on the surface of the metal oxide obtained in the step of forming the first coating layer, the boron subsequently coated can be evenly diffused on the surface of the first coating layer.

[0060] Next, a step is performed to obtain an anode active material in which a second coating layer containing boron is formed on the surface of the first coating layer by mixing a raw material containing boron with the metal oxide on which the first coating layer is formed and then performing a second heat treatment.

[0061] The raw material containing the above boron may include at least one of H3BO3, B2O3, B4C, Li2B4O7, Li3BO3, W2B, WB, WB2, and WB4.

[0062] At this time, the raw material containing the boron can be added and mixed in such a way that the content ranges from 0.1g to 1g, more specifically from 0.2g to 0.8g or from 0.3g to 0.6g, based on 100g of the metal oxide on which the first coating layer is formed.

[0063] When the content of the cobalt raw material introduced in the first coating layer formation process and the content of the boron-containing raw material introduced in the second coating layer formation process satisfy the above range, it is possible to manufacture a positive electrode active material for a lithium secondary battery that has excellent resistance characteristics while having excellent initial charge and discharge capacity, initial efficiency, room temperature output, and high temperature capacity retention rate.

[0064] Meanwhile, in the step of forming the second coating layer, the heat treatment may be performed at 200°C to 500°C or 250°C to 400°C. Additionally, the heat treatment may be performed for 3 hours to 18 hours or 6 hours to 15 hours. If the heat treatment conditions for forming the second coating layer satisfy the above ranges, the initial efficiency can be further improved.

[0065] In this embodiment, the metal oxide may be represented by the following chemical formula 1.

[0066] [Chemical Formula 1]

[0067] Li a (Ni b Co c Mn d )O2

[0068] In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤b≤0.99, 0.01≤c≤0.1, 0.01≤d≤0.1, and b+c+d = 1.

[0069] At this time, b represents the molar ratio of nickel among all metal elements in the metal oxide, and may be in the range of 0.85 ≤ b ≤ 0.99. When the value of b in Equation 1 satisfies the above range, a positive electrode active material for a lithium secondary battery with excellent initial efficiency and room temperature output characteristics can be manufactured.

[0070] Meanwhile, the positive active material having a coating layer formed thereon, manufactured according to the method for manufacturing a positive active material for a lithium secondary battery according to one embodiment, may have a t1 value between 200 and 250 when exponential fitting is performed on the B1s XPS depth profile using an exponential decay model.

[0071] Specifically, when the depth is increased by sputtering from a coating layer formed on the surface of a positive electrode active material manufactured according to a method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment to a range of 100 nm at intervals of 20 nm and the B1s signal intensity is measured (wherein the x-axis is depth (or sputter time → depth conversion) and the y-axis is the B1s signal (usually normalized intensity)), the measurement results are exponentially fitted using a model represented by the following mathematical formula 1 to obtain the t1 value.

[0072] [Mathematical Formula 1]

[0073] y = e -x / t1 + y0

[0074] In the above mathematical formula 1,

[0075] y is the B1s signal (normalized strength), and

[0076] t1 is the attenuation length, which quantifies how slowly (or rapidly) the B signal decreases as the depth increases, and

[0077] y0 represents the offset, that is, the background signal remaining even after depth increase.

[0078] Therefore, as the above t1 value is smaller, the signal decreases quickly, indicating that boron is present shallowly on the surface of the first coating layer, and as the above t1 value is larger, the signal decreases slowly, indicating that boron is thickly and evenly diffused on the surface of the first coating layer.

[0079] That is, in the above mathematical formula 1, the t1 value represents the slope of the exponential function, and the accuracy (R) of the fitting 2 ), that is, R representing the accuracy of the above exponential decay model 2The closer the value is to 1, the closer the above model is to actual data. More specifically, the above t1 value can be viewed as the "characteristic length of the boron concentration distribution," and can serve as an indirect indicator of the thickness and penetration depth of the second coating layer or the degree of boron ablation.

[0080] As such, since the exponential decay model represented by the above Equation 1 assumes a simple diffusion / decrease form that is “large at the surface and monotonically decreases with depth,” if an exponential decay pattern of the B1s signal decreasing exponentially with depth does not hold even when exponential fitting is performed using the exponential decay model represented by the above Equation 1, then the above t1 value and R 2 It is impossible to calculate the value. This is because there is almost no signal, or it exhibits non-monotonic or complex distributions.

[0081] A positive electrode active material having a coating layer formed according to a method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment may have a t1 value between 200 and 250, and this is because the t1 value must be in the above range so that the second coating layer (boron coating layer) is optimally coated on the surface of the first coating layer (cobalt coating layer) and the improvement of the capacity characteristics of the positive electrode active material can be maximized.

[0083] Cathode active material for lithium secondary batteries

[0084] A positive electrode active material for a lithium secondary battery according to another embodiment is a positive electrode active material comprising Ni, Co and Mn, wherein the positive electrode active material comprises a first coating layer containing cobalt on its surface, and the first coating layer comprises a second coating layer containing boron on its surface, and the positive electrode active material exhibits a t1 value between 200 and 250 when exponential fitting is performed on a B1s XPS depth profile.

[0085] For example, the above t1 value may be between 215 and 305, or between 220 and 305, or between 235 and 305, or between 215 and 250.

[0086] For example, the above positive active material may have a nickel content of 80% or more.

[0087] In this way, by continuously forming the first coating layer and the second coating layer on the surface of the metal oxide, direct contact between the positive electrode active material and the electrolyte can be prevented, and the decomposition or oxidation of the electrolyte can be prevented. That is, by manufacturing a positive electrode active material with such a coating layer formed thereon, the lifespan and capacity retention rate of the positive electrode can be improved, and there is an advantage of reducing heat dissipation of high-nickel NCM positive electrode active materials with a high nickel content.

[0088] However, when cobalt raw materials are used alone in high-nickel cathode materials with high nickel content, there is a problem in that electrochemical performance is degraded due to increased contact resistance between the metal oxide and the cobalt element.

[0089] However, in this embodiment, by forming a first coating layer containing cobalt and forming a second coating layer containing boron on the surface of the first coating layer, the problem of increased contact resistance of the positive electrode active material manufactured according to this embodiment can be resolved.

[0090] In addition, the above-mentioned positive active material may have a layered structure. In this layered unit cell structure, the lengths in the horizontal and vertical directions can be represented by 'a', and the height can be represented by 'c'; the physical properties of the material change significantly depending on variations in the values ​​of 'a' and 'c' representing this crystal structure.

[0091] The cathode active material of the present embodiment can further increase the length of the c-axis of the unit cell structure by manufacturing a cathode active material having a first coating layer containing cobalt and a second coating layer containing boron formed on the surface of the first coating layer. Accordingly, the mobility of Li within the crystal structure of the cathode active material can be increased, and consequently, a cathode active material with excellent electrochemical and resistance characteristics can be manufactured even when using cobalt.

[0092] At this time, the total average thickness of the coating layer, which is the sum of the thickness of the first coating layer and the thickness of the second coating layer, may be in the range of 20 nm to 200 nm or 20 nm to 100 nm. When the thickness of the coating layer satisfies the above range, the resistance characteristics are reduced and high electrochemical properties can be secured. In addition, the cycle characteristics due to the coating are excellent.

[0093] Meanwhile, the metal oxide of the present embodiment may be a secondary particle formed by the aggregation of a plurality of primary particles.

[0094] In this specification, “secondary particle” means an aggregate, i.e., a secondary structure, formed by the aggregation of tens to hundreds of primary particles by physical or chemical bonding between primary particles without an intentional aggregation or assembly process of the primary particles.

[0095] In addition, “primary particle” refers to the smallest particle unit that is distinguished as a single mass when the cross-section of the positive active material is observed through a scanning electron microscope (SEM), and it may consist of a single crystal grain or multiple crystal grains.

[0097] anode

[0098] In another embodiment, a positive electrode is provided comprising a current collector and a positive electrode active material layer located on one side of the current collector and comprising the positive electrode active material of the aforementioned embodiment.

[0099] The characteristics of the positive active material constituting the above positive active material layer are the same as those previously described. Therefore, a detailed description of the positive active material will be omitted.

[0100] The above current collector may be, for example, made of stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treated with carbon, nickel, titanium, silver, etc.

[0101] Meanwhile, the above positive active material layer may include a binder and a conductive material.

[0102] At this time, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.

[0103] In addition, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used, but is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the positive electrode active material layer.

[0104] The above-mentioned anode can be manufactured according to a conventional anode manufacturing method, except for using the above-mentioned anode active material.

[0105] Specifically, the anode can be manufactured by applying a composition for forming an anode active material layer, comprising the aforementioned anode active material and optionally a binder, conductive material, or solvent as needed, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.

[0106] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that dissolves or disperses the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.

[0107] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0109] lithium secondary battery

[0110] In another embodiment, a lithium secondary battery including the anode is provided.

[0111] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly comprising the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0112] In the above lithium secondary battery, the negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0113] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0114] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a composition for forming a cathode active material layer, comprising a cathode active material and optionally a binder and a conductive material, onto a cathode current collector and drying it, or by casting the composition for forming a cathode onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.

[0115] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ βExamples include metal oxides capable of doping and dedoping lithium, such as (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, the carbon material may include low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0116] The binder and conductive material mentioned above may be the same as those previously described in the anode.

[0117] Next, depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used, and a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.

[0118] In addition, regarding the above lithium secondary battery, the electrolyte may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing a lithium secondary battery, but is not limited to these.

[0119] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0120] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.

[0121] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0123] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).

[0125] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0127] Example 1

[0128] Preparation of anode active material with Boron coating applied after 790℃ surface modification heat treatment

[0129] (Ni) having a particle size of 5 to 15 μm 0.86 Co 0.06 Mn 0.08160g of a precursor of )(OH)2 composition and 73.48g of LiOH·H2O were fed into a mixer and mechanically mixed, and then calcined for 13 hours at 850 to 950℃ in an O2 atmosphere.

[0130] The manufactured cathode active material was ground using a Jet-mill process so that aggregated particles could fall off during calcination. 250g of the obtained cathode active material was mixed with 24.8g of Co(OH)2 and calcined at 790℃ for 20 hours to produce a cathode active material coated with 2 mol% Co on the surface of the cathode active material.

[0131] 1.06 g of H3BO3 was mixed with 250 g of Co-coated cathode active material and calcined at 350°C for 12 hours to prepare a cathode active material coated with Boron on the surface.

[0132] Example 2

[0133] Preparation of anode active material with Boron coating applied after 830℃ surface modification heat treatment

[0134] Synthesis and grinding were performed in the same manner as in Example 1. 250g of the obtained positive active material was mixed with 24.8g of Co(OH)2 and calcined at 830℃ for 20 hours to produce a positive active material coated with 2 mol% of Co on the surface of the positive active material.

[0135] 1.06 g of H3BO3 was mixed with 250 g of Co-coated cathode active material and calcined at 350°C for 12 hours to prepare a cathode active material coated with Boron on the surface.

[0136] Comparative Example 1

[0137] Preparation of anode active material with Boron coating applied after 680℃ surface modification heat treatment

[0138] Synthesis and grinding were performed in the same manner as in Example 1. 250g of the obtained positive active material was mixed with 24.8g of Co(OH)2 and calcined at 680°C for 20 hours to produce a positive active material coated with 2 mol% of Co on the surface of the positive active material.

[0139] 1.06 g of H3BO3 was mixed with 250 g of Co-coated cathode active material and calcined at 350°C for 12 hours to prepare a cathode active material coated with Boron on the surface.

[0140] Comparative Example 2

[0141] Preparation of positive electrode active material with Boron coating after 740℃ surface modification heat treatment

[0142] Synthesis and grinding were performed in the same manner as in Example 1. 250g of the obtained positive active material was mixed with 24.8g of Co(OH)2 and calcined at 740℃ for 20 hours to produce a positive active material coated with 2 mol% of Co on the surface of the positive active material.

[0143] 1.06 g of H3BO3 was mixed with 250 g of Co-coated cathode active material and calcined at 350°C for 12 hours to prepare a cathode active material coated with Boron on the surface.

[0144] Comparative Example 3

[0145] Preparation of anode active material with Boron coating applied after 850℃ surface modification heat treatment

[0146] Synthesis and grinding were performed in the same manner as in Example 1. 250g of the obtained positive active material was mixed with 24.8g of Co(OH)2 and calcined at 850°C for 20 hours to produce a positive active material coated with 2 mol% Co on the surface of the positive active material.

[0147] 1.06 g of H3BO3 was mixed with 250 g of Co-coated cathode active material and calcined at 350°C for 12 hours to prepare a cathode active material coated with Boron on the surface.

[0149] (Experimental Example 1) B1s XPS depth profile of the prepared cathode active material

[0150] The B1s XPS depth profiles of the cathode active materials prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were measured and are shown as graphs in Fig. 1. Depth analysis was performed using an XPS sputter to approximately 0 to 100 nm from the surface, with intervals of 20 nm. The XPS etching conditions are as follows.

[0151] * Ar ion etching: 1keV, 2mm x 2mm raster

[0152] * Calculated as 20 nm depth per 200 sec etching

[0154] (Experimental Example 2) Exponential fitting data and electrochemical characteristics of XPS depth profile (Coin cell)

[0155] Exponential fitting was performed using the depth profile analyzed in Experimental Example 1, and the necessary factors are shown in Table 1 below. The fitting formula is Equation 1, y = e -x / t1 + y0 was used, through which t1, representing the slope of the exponential function, and R, representing the accuracy of the fitting, were obtained. 2 The values ​​were calculated. For the Comparative Example 1 sample, which did not show the shape of the Exponential function, t1, R 2 I couldn't find the value.

[0156] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Surface modification heat treatment temperature (°C) 790 830 680 740 850 t1 236.4 304.7 - 202.0 214.4 R 2 0.9989 0.9998 - 0.9981 0.9976 Charging (mAh / g) 214.1 240.2 235.4 234.9 238.4 Discharge (mAh / g) 217.4 213.9 208.8 208.5 210.1 efficiency 90.2% 89.1% 88.7% 88.8% 88.1%

[0157] The cathode active materials prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were applied to coin half-cells to evaluate their electrochemical characteristics. The slurry for electrode manufacturing consisted of cathode active material : conductive material (acetylene black) : binder (PVDF, KF1120) = 96.5 : 1.5 : 2 wt%, and additional NMP (N-Methyl-2-pyrrolidone) was added to adjust the solid content and slurry viscosity. The prepared slurry was coated onto an Al foil using a doctor blade, and electrode plates were manufactured by drying and rolling. At this time, the electrode loading amount was 15 to 16 mg / cm². 2 was, and the density of the electrode mixture was 3.5 g / cm³ 3 The above was the result. The electrolyte used in the coin cell was 1M LiPF6 in EC : DMC : EMC = 3:4:3 (vol%) + VC 3.0 wt%, and the coin cell was fabricated using a PP separator and a lithium anode (300 μm). After fabrication, the cell was aged at room temperature for 10 hours, and then a charge-discharge test was performed. To evaluate the initial capacity, 200 mAh / g was set as the reference capacity, and the cell was charged to 4.3 V with a constant current of 0.1 C, then switched to a constant voltage, and charging continued until the terminal current reached 0.05 C.

[0159] (Experimental Example 3) Analysis of the shape of the manufactured cathode active material

[0160] The morphology of the cathode active materials prepared in Example 1, Example 2 and Comparative Examples 1 to 3 was observed using a scanning electron microscope (SEM) and is shown in FIGS. 2 to 6. Through the images presented in FIGS. 2 to 6, it can be seen that all examples and comparative examples have a structure in which 5 to 10 primary particles aggregate to form secondary particles.

[0162] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.

[0163] Therefore, the actual scope of the rights of the present invention shall be defined by the appended claims and their equivalents.

Claims

Claim 1 A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising: a step of obtaining a metal oxide by mixing a metal hydroxide containing nickel, cobalt, and manganese with a lithium raw material and then calcining; a step of grinding the metal oxide; a step of forming a metal oxide in which a first coating layer containing cobalt is formed on the surface of the metal oxide by mixing the ground metal oxide and a cobalt raw material and then performing a first heat treatment; and a step of obtaining a positive electrode active material in which a second coating layer containing boron is formed on the surface of the first coating layer by mixing a raw material containing boron with the metal oxide in which the first coating layer is formed and then performing a second heat treatment; wherein the first heat treatment is performed at a temperature of 790°C to 830°C. Claim 2 delete Claim 3 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the cobalt raw material comprises Co(OH)2. Claim 4 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the raw material containing boron comprises at least one of H3BO3, B2O3, B4C, Li2B4O7, Li3BO3, W2B, WB, WB2, and WB4. Claim 5 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein in the step of forming the first coating layer, the cobalt raw material is added and mixed in a content range of 1.5g to 2.5g based on 100g of the crushed metal oxide. Claim 6 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the step of forming the first coating layer is a step of coating the surface of the metal oxide obtained in the step of forming the first coating layer with cobalt in an amount of 1 mol% to 5 mol% based on the total number of moles of atoms constituting the surface of the metal oxide. Claim 7 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein in the step of forming the second coating layer, the raw material containing boron is added and mixed in a content range of 0.1g to 1g based on 100g of the metal oxide on which the first coating layer is formed. Claim 8 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the first heat treatment is performed for 10 to 30 hours. Claim 9 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the secondary heat treatment is performed at 200°C to 500°C for 3 hours to 18 hours. Claim 10 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the metal oxide is represented by the following chemical formula 1: [Chemical Formula 1]Li a (Ni b Co c Mn d In the above chemical formula 1, 0.8≤a≤1.2, 0.80≤b≤0.99, 0.01≤c≤0.1, 0.01≤d≤0.1, and b+c+d = 1. Claim 11 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein b is in the range of 0.85 ≤ b ≤ 0.99 in claim 10. Claim 12 A positive active material comprising Ni, Co and Mn, wherein the positive active material comprises a first coating layer containing Co on its surface, the first coating layer comprises a second coating layer containing B on its surface, and the positive active material exhibits a t1 value between 235 and 305 when exponential fitting is performed on a B1s XPS depth profile. Claim 13 In Clause 12, the above-mentioned positive active material is a positive active material having a nickel content of 80% or more. Claim 14 A positive electrode for a lithium secondary battery comprising a positive electrode active material manufactured according to the manufacturing method of claim 1. Claim 15 A positive electrode for a lithium secondary battery comprising the positive electrode active material of claim 12. Claim 16 A lithium secondary battery comprising a positive electrode for a lithium secondary battery according to claim 14 or 15.

Citation Information

Patent Citations

  • Positive electrode active material, positive electrode and lithium secondary battery