welded joint

By controlling the Al concentration in the plating layer to form a high η phase ratio, the welded joint effectively suppresses LME cracking and enhances corrosion resistance in spot welding of galvanized steel sheets.

KR103046918B1Active Publication Date: 2026-11-11NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020247021948
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-06
Filing Date
2022-12-21
Publication Date
2026-11-11
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing methods for suppressing Liquid Metal Embrittlement (LME) cracking in welded joints, particularly in spot welding of galvanized steel sheets, do not adequately address the plating structure prior to welding, leading to insufficient LME resistance.

Method used

A welded joint design utilizing plated steel sheets with a controlled Al concentration distribution in the plating layer, forming a high proportion of the η phase in the separation area outside the weld, thereby reducing the penetration of molten zinc during spot welding.

Benefits of technology

Significantly improves LME resistance and corrosion resistance by controlling the Al concentration in the plating layer, forming a new Fe-Al barrier layer to prevent zinc penetration and reduce crack formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024070972599-PCT00002_ABST
    Figure 112024070972599-PCT00002_ABST
Patent Text Reader

Abstract

A weld joint is provided having a plurality of overlapping steel plates, a nugget joining the plurality of steel plates, a spot weld portion having a pressure weld portion and a heat-affected portion formed around the nugget, and a separation portion located around the pressure weld portion; at least one of the plurality of steel plates is a plated steel plate having a base steel plate and a plating layer formed on a surface of the base steel plate corresponding to the overlapping surface of at least the plurality of steel plates, and the plating layer in the separation portion outside the heat-affected portion has a predetermined chemical composition, and in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a welded joint, and more specifically, to a welded joint obtained by spot welding plated steel plates. Background Technology

[0002] Steel sheets used in automobiles and the like require good weldability. Spot welding is primarily used in processes such as the assembly of automobile bodies and the installation of parts; however, particularly in spot welding between galvanized steel sheets or between galvanized steel and non-galvanized steel sheets, it is necessary to suppress Liquid Metal Embrittle (LME) cracking. This phenomenon is a crack that occurs when zinc, liquefied by welding heat input, penetrates into the interior of the steel sheet along grain boundaries and acts on the embrittled portions, which are then subjected to tensile stress generated by welding. In spot welding, if such LME cracking occurs, the strength of the welded joint cannot be secured, which may hinder the use of galvanized steel sheets.

[0003] In this regard, Patent Document 1 teaches that such LME cracks can be addressed by improving the spot welding method. More specifically, Patent Document 1 teaches that after the current flow between welding electrodes ends, the pressure holding support of the welding electrodes is continued (extending the post-welding holding time Ht), and by adjusting the post-welding holding time Ht as a function of the total plate thickness t of the workpiece, the molten zinc-based plating is solidified before the electrodes are opened, and as a result, the molten zinc-based plating does not penetrate into the grain boundaries of the steel plate at locations with high welding residual stress, thereby suppressing cracks.

[0004] Patent Document 2 describes a method for suppressing cracks by controlling the plating structure near the spot weld after spot welding. More specifically, Patent Document 2 describes a spot weld member having a spot weld formed by spot welding a plate set of multiple steel plates stacked together and supported by a pair of electrodes, wherein at least one of the multiple steel plates is a high-strength zinc-plated steel plate with a tensile strength of 780 MPa or more, and the Al content in the plating of the high-strength zinc-plated steel plate is 0.5 mass% or more, and the thermal shock region outside the corona bond end of the spot weld is described as having a plating layer having an average thickness of 0.3 μm or more and a zinc-plated layer having an average thickness of 2.0 μm or more formed on the FeAl alloy layer at the interface between the base steel plate of the high-strength zinc-plated steel plate and the plating. In addition, Patent Document 2 teaches that in order to suppress Zn penetration into the base steel plate, it is important to form a high-melting-point FeAl alloy layer at the interface between the steel plate and the plating of the steel plate by means of heat input during welding, by making the Al content in the plating 0.5 mass% or more. Prior art literature

[0005] Japanese Patent Publication No. 2017-047475, International Publication No. 2020 / 130079 The problem to be solved

[0006] In Patent Documents 1 and 2, the suppression of LME cracking in weld joints is examined from the perspective of improving the spot welding method or controlling the plating structure near the spot weld after spot welding. However, in Patent Documents 1 and 2, the suppression of LME cracking in weld joints in relation to the plating structure of the plated steel sheet prior to spot welding is not necessarily sufficiently examined. Therefore, in the inventions described in these patent documents, there is still room for improvement regarding the enhancement of LME resistance.

[0007] Accordingly, the present invention aims to provide a weld joint capable of suppressing or reducing the occurrence of LME cracks during spot welding through a novel configuration. means of solving the problem

[0008] The inventors conducted an investigation by focusing on the microstructure of the plating layer in plated steel sheets used for welded joints, in order to suppress or reduce the occurrence of LME cracking when manufacturing welded joints by spot welding. As a result, the inventors discovered that by using a plated steel sheet equipped with a plating layer containing a relatively small amount of Al and appropriately controlling the Al concentration distribution, the microstructure of the plating layer in the parts prone to LME cracking during spot welding can be improved, and in this regard, the LME resistance of the welded joint can be significantly improved, thereby completing the present invention.

[0009] The present invention, which was able to achieve the above objective, is as follows.

[0010] (1) Multiple overlapping steel plates, and

[0011] A nugget joining the plurality of steel plates, and a spot weld having a pressure weld and a heat-affected zone formed around the nugget, and

[0012] Separation part located around the above-mentioned pressure weld part

[0013] It is a welded joint equipped with,

[0014] One or more of the plurality of steel plates is a plated steel plate having a base steel plate and a plating layer formed on at least a surface of the base steel plate corresponding to the overlapping surface of the plurality of steel plates, and

[0015] The plating layer in the separation portion on the outer side of the heat-affected portion is, in mass %,

[0016] Al: 0.10 to 1.50%, and

[0017] Fe: 0.01 to 2.00%

[0018] Contains, and also

[0019] Mg: 0 to 1.500%,

[0020] Si: 0 to 1.000%,

[0021] Ni: 0 to 1.000%,

[0022] Ca: 0 to 4.000%,

[0023] Sb: 0 to 0.500%,

[0024] Pb: 0 to 0.500%,

[0025] Cu: 0 to 1.000%,

[0026] Sn: 0 to 1.000%,

[0027] Ti: 0 to 1.000%,

[0028] Cr: 0 to 1.000%,

[0029] Nb: 0 to 1.000%,

[0030] Zr: 0 to 1.000%,

[0031] Mn: 0 to 1.000%,

[0032] Mo: 0 to 1.000%,

[0033] Ag: 0 to 1.000%,

[0034] Li: 0 to 1.000%,

[0035] La: 0 to 0.500%,

[0036] Ce: 0 to 0.500%,

[0037] B: 0 to 0.500%,

[0038] Y: 0 to 0.500%,

[0039] P: 0 to 0.500%, and

[0040] Sr: 0 to 0.500%

[0041] Containing at least one of the following in total of 5.000% or less,

[0042] It has a chemical composition in which the remainder consists of Zn and impurities,

[0043] A welded joint characterized in that, in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%.

[0044] (2) The above-described weld joint, wherein the chemical composition contains Al: 0.30 to 1.50% in mass%, and the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion is 25 to 100%.

[0045] (3) The above-described weld joint, wherein the chemical composition contains Al: 0.30 to 1.50% in mass%, and the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion is 40 to 100%.

[0046] (4) A welded joint described in any one of claims (1) to (3), characterized in that the plating layer is a molten zinc plating (GI) layer.

[0047] (5) A welded joint described in any one of claims (1) to (4), characterized in that the plated steel plate has a tensile strength of 780 MPa or more. Effects of the invention

[0048] According to the present invention, a weld joint capable of suppressing or reducing the occurrence of LME cracks during spot welding can be provided. Brief explanation of the drawing

[0049] FIG. 1 is a schematic diagram illustrating a cross-section of a welded joint according to an embodiment of the present invention, (a) is an overall view of the welded joint, and (b) is an enlarged view of the end of the welded portion and the separation portion immediately outside thereof. FIG. 2 is a drawing illustrating the results of GDS analysis of a plated steel sheet, (a) illustrating the results of GDS analysis of an Al-containing plated steel sheet manufactured by a conventional method, and (b) illustrating the results of GDS analysis of a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention. Specific details for implementing the invention

[0050] Welded Joint

[0051] A welded joint according to an embodiment of the present invention comprises a plurality of overlapping steel plates, and

[0052] A nugget joining the plurality of steel plates, and a spot weld having a pressure weld and a heat-affected zone formed around the nugget, and

[0053] Separation part located around the above-mentioned pressure weld part

[0054] It is a welded joint equipped with,

[0055] One or more of the plurality of steel plates is a plated steel plate having a base steel plate and a plating layer formed on at least a surface of the base steel plate corresponding to the overlapping surface of the plurality of steel plates, and

[0056] The plating layer in the separation portion on the outer side of the heat-affected portion is, in mass %,

[0057] Al: 0.10 to 1.50%, and

[0058] Fe: 0.01 to 2.00%

[0059] Contains, and also

[0060] Mg: 0 to 1.500%,

[0061] Si: 0 to 1.000%,

[0062] Ni: 0 to 1.000%,

[0063] Ca: 0 to 4.000%,

[0064] Sb: 0 to 0.500%,

[0065] Pb: 0 to 0.500%,

[0066] Cu: 0 to 1.000%,

[0067] Sn: 0 to 1.000%,

[0068] Ti: 0 to 1.000%,

[0069] Cr: 0 to 1.000%,

[0070] Nb: 0 to 1.000%,

[0071] Zr: 0 to 1.000%,

[0072] Mn: 0 to 1.000%,

[0073] Mo: 0 to 1.000%,

[0074] Ag: 0 to 1.000%,

[0075] Li: 0 to 1.000%,

[0076] La: 0 to 0.500%,

[0077] Ce: 0 to 0.500%,

[0078] B: 0 to 0.500%,

[0079] Y: 0 to 0.500%,

[0080] P: 0 to 0.500%, and

[0081] Sr: 0 to 0.500%

[0082] Containing at least one of the following in total of 5.000% or less,

[0083] It has a chemical composition in which the remainder consists of Zn and impurities,

[0084] In the plating layer of the separation portion in the region of 500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%.

[0085] As explained above, in spot welding between galvanized steel sheets or between galvanized steel sheets and non-galvanized steel sheets, it is necessary to suppress LME cracking. For example, when a joint is fabricated by spot welding two or more steel sheets, each containing at least one galvanized steel sheet, LME cracking may occur in the separation area (an area where the steel sheets are not joined) located inside or immediately outside the pressure weld (corona bond) formed on the outer side of the weld metal (nugget), for instance, around the pressure weld. LME cracking occurs when zinc, liquefied by the welding heat input during spot welding, penetrates into the interior of the steel sheet along the grain boundaries and acts on the steel sheet in the embrittled area; this tensile stress is generated by the welding process and is caused by many factors, such as pressure applied by the electrode, expansion and contraction of the weld area, and springback upon electrode release. Accordingly, in order to suppress or reduce the penetration of zinc into the interior of such steel sheets, the inventors focused on the structure of the plating layer in the plated steel sheets and conducted an examination from the perspective of making the structure of the plating layer more suitable.

[0086] First, the inventors have discovered that adding aluminum (Al) in a relatively small amount, namely 0.10 to 1.50 mass%, to a plating layer based on zinc (Zn) is effective in suppressing or reducing the penetration of Zn into the steel sheet. As the amount of Al added increases, the composition of the plating layer approaches the Zn-Al eutectic composition, and thus the melting point of the plating layer decreases. For this reason, the excessive addition of Al is likely to have an adverse effect in terms of improving LME resistance by suppressing or reducing the penetration of molten Zn into the steel sheet. In particular, when Al is added in amounts significantly exceeding 1.50 mass%, the negative effects based on the excessive addition of Al become pronounced, and it is thought that the effect of suppressing LME cracking by the addition of Al cannot be fully exerted. Furthermore, the inventors have discovered that by using a plated steel sheet in which the Al concentration distribution in the plating layer is controlled such that the Al concentration at the center of the plating layer is in a ratio of 0.10 to 1.50 with respect to the Al concentration near the interface between the base steel sheet and the plating layer—more specifically, the Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel sheet—the plating structure in the separation area directly outside the welded portion changes due to thermal effects during spot welding, and the occurrence of LME cracks around the welded portion is significantly suppressed or reduced. This will be explained in more detail below with reference to the drawings.

[0087] FIG. 1 is a schematic diagram illustrating a cross-section of a welded joint according to an embodiment of the present invention, (a) is an overall view of the welded joint, and (b) is an enlarged view of the pressure weld end and the separation portion immediately outside thereof. First, referring to FIG. 1 (a), the welded joint (1) according to an embodiment of the present invention comprises two overlapping steel plates (11), a nugget (12) joining the steel plates (11), a spot weld portion (16) having a pressure weld portion (13) and a heat-affected portion (15) formed around the nugget (12), and a separation portion (17) located around the pressure weld portion (13). In FIG. 1, as the two steel plates (11), plated steel plates are used, which have a plating layer on both sides of the base steel plate that is mainly composed of Zn and has an Al concentration distribution controlled within a predetermined range. In this regard, referring to FIG. 1(b), a plating layer (18) derived from a plating layer on a steel plate (11) prior to spot welding is formed in a separation portion (17) located directly outside the welded portion end (14). According to an embodiment of the present invention, in a separation portion (17) within a heat-affected portion (15) located directly outside the welded portion end (14), the structure of the initial plating layer is changed due to heat influence during spot welding, and a plating layer (18) with a relatively high proportion of the η phase is formed, more specifically, a plating layer (18) in which the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%. In the present invention, the η phase refers to a phase in which Zn is the main component and other elements such as Fe are included in a solid solution state. More specifically, it refers to a phase in which the Zn concentration is 97 atomic% or more, the Fe concentration is 3 atomic% or less, and other elements are 3 atomic% or less, as measured by a scanning electron microscope (SEM-EPMA) equipped with an electron probe microanalyzer. Likewise, the Γ phase refers to a phase in which the Zn concentration is 87 atomic% or more, the Fe concentration is 8 to 13 atomic%, and other impurities are 3 atomic% or less, as measured by SEM-EPMA.The change in the structure of such plating layers is greatly influenced by the chemical composition and structure of the initial plating layer before spot welding. In Zn-based plating, as the alloying of Zn in the plating layer proceeds due to the heat input of welding, the proportion of the Γ phase generally becomes high, and the proportion of the η phase becomes relatively low. However, according to an embodiment of the present invention, compared to the case of spot welding of a conventional Zn-based plated steel sheet, a plating layer (18) with a relatively high proportion of the η phase is formed in the separation portion (17) directly outside the pressure welding portion (13), and in this regard, the penetration of molten Zn into the steel sheet during spot welding is suppressed or reduced, and as a result, it is possible to significantly improve the LME resistance of the weld joint obtained.

[0088] In FIG. 1, for ease of understanding, only two steel plates (11) are overlapped and a plating layer is formed on both steel plates (11) to form a welded joint. However, the welded joint according to the embodiment of the present invention is not necessarily limited to such a welded joint and may include various welded joints in which a plating layer (18) having a predetermined amount of η phase is formed in the separation portion (17) within the heat-affected zone (15). For example, in a welded joint formed by spot welding two sets of steel plates (11) as described in FIG. 1, only one steel plate (11) may be a plated steel plate. In this case, the plating layer (18) may exist in the separation portion (17) outside the pressure welding portion (13) of at least the surface corresponding to the overlap surface of the two surfaces of the plated steel plate, and naturally, the plating layer (18) and / or an initial plating layer related to the plating layer (18) may exist on both surfaces. For example, if an initial plating layer related to the plating layer (18) exists on the surface opposite to the overlapping side of the steel plate, that is, on the electrode side, then even in the initial plating layer on the electrode side, the structure of the plating layer changes during spot welding in the region within the heat-affected zone (e.g., the contact area between the electrode and the steel plate and its periphery), and a plating layer (18) with a relatively high proportion of the η phase is formed. Because of this, it is possible to further improve LME resistance compared to the case where the plating layer (18) exists only on the surface corresponding to the overlapping side of the steel plate. Likewise, in the case of a welded joint made of three or more steel plates, various welded joints may be included in which a plating layer (18) having a predetermined amount of the η phase is formed in the separation portion (17) within the heat-affected zone (15). For example, in a welded joint formed by spot welding three sets of steel plates (11), a plating layer (18) may be present in a separation portion (17) outside the pressure weld portion (13) on the surface corresponding to at least one of the three steel plates (11).For example, if only the middle steel plate (11) among three overlapping steel plates (11) is a plated steel plate, the plating layer (18) may exist only in the separation portion (17) outside the pressure joint (13) of one of the two surfaces of the plated steel plate, or the plating layer (18) may exist in the separation portion (17) outside the pressure joint (13) of both surfaces. For example, the plating layer (18) may exist only in the separation portion (17) outside the pressure joint (13) of some steel plates (11), and a different Zn-based plating layer may exist in the separation portion (17) outside the pressure joint (13) of the other steel plate (11). Such embodiments are also included in the present invention. In this case, compared to the case of a welded joint where a plating layer (18) exists in the separation portion (17) outside the pressure joint portion (13) of all steel plates (11), there is a possibility that the joint strength may be slightly reduced in that the risk of LME cracking is increased on the surface where another Zn-based plating layer exists, but the specific number and arrangement of steel plates (11) on which a plating layer (18) having a predetermined amount of η phase is formed in the welded joint can be appropriately determined by considering the desired joint strength, etc.

[0089] Next, a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention will be described. FIG. 2 is a diagram showing the results of GDS analysis of a plated steel sheet, FIG. 2(a) shows the results of GDS analysis of an Al-containing plated steel sheet manufactured by a conventional method, and FIG. 2(b) shows the results of GDS analysis of a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention. First, referring to FIG. 2(a), in an Al-containing plated steel sheet in which 0.20% Al is contained in a Zn-based plating layer by a conventional method, as the depth increases from 0 μm, which corresponds to the plating surface, it can be seen that the Al concentration has a relatively high peak near the interface between the base steel sheet and the plating layer, that is, near the plating layer position where the Fe concentration is 50% of that of the base steel sheet. This peak in Al concentration suggests that an Fe-Al barrier layer containing an alloy of Fe and Al is formed at the interface between the base steel sheet and the plating layer. As is evident from the relatively high peak in Al concentration, in Al-containing plated steel sheets manufactured by conventional methods, more Al in the plating layer is consumed in the formation of the Fe-Al barrier layer, resulting in the formation of a relatively thick Fe-Al barrier layer. Therefore, in Figure 2(a), as the Al concentration progresses from near the interface between the base steel sheet and the plating layer toward the plating surface, it decreases significantly and then becomes a very low value that is almost constant. It can be seen that the Al concentration is about 0.1% at the center of the plating layer, which corresponds to the intermediate position between the plating layer where the Fe concentration is 50% of the base steel sheet and the plating surface.

[0090] In contrast, referring to FIG. 2(b), it can be seen that in the plated steel sheet of FIG. 2(b), even though the plating layer has the same Al content as in FIG. 2(a), the Al concentration near the interface between the base steel sheet and the plating layer is very low compared to FIG. 2(a). Therefore, in the plated steel sheet of FIG. 2(b), a thin Fe-Al barrier layer is formed compared to FIG. 2(a). In this regard, in FIG. 2(b), even as the process proceeds from near the interface between the base steel sheet and the plating layer toward the plating surface, the Al concentration in the plating layer does not decrease significantly but decreases relatively gradually and then becomes almost constant, and it can be seen that the Al concentration at the center of the plating layer exceeds about 0.2%, showing a very high value of about twice as high as in FIG. 2(a). From the GDS analysis results of FIG. 2(a) and (b), it is believed that in the plated steel sheet of FIG. 2(b), most of the Al in the plating layer is not consumed in the formation of the Fe-Al barrier layer, but exists as an Al phase, for example, in a solid solution state, within the plating layer other than the Fe-Al barrier layer. Based on the GDS analysis results of these plated steel sheets and the fact that the weld joint obtained by spot welding the plated steel sheet of FIG. 2(b) experimentally exhibited higher LME resistance compared to the weld joint obtained by spot welding the plated steel sheet of FIG. 2(a), the inventors considered that the Al phase existing within the plating layer other than the Fe-Al barrier layer plays a very important role in suppressing or reducing the penetration of molten Zn into the steel sheet during spot welding, and conducted further investigations. As a result, the inventors determined that the total amount of Al added is 1.It was found that by controlling the amount to a relatively low amount of 50 mass% or less to suppress the deterioration of LME resistance based on the decrease in the melting point in the plating layer, and by controlling the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” when the plating layer is measured by GDS to within the range of 0.10 to 1.50, the effect of adding Al to the plating layer can be fully exerted. In addition, the inventors have discovered that by using such a plated steel sheet, the structure of the initial plating layer changes in the separation area within the heat-affected zone immediately outside the weld during spot welding, more specifically in the separation area of ​​500 μm from the end of the weld, and a plating layer is formed in which the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%, and in this regard, the penetration of molten Zn into the steel sheet during spot welding can be significantly suppressed or reduced. In addition to this improvement in LME resistance, the inventors have discovered that the corrosion resistance of the weld can also be significantly improved by increasing the relative proportion of the η phase, which is mainly Zn, in the plating layer of the weld.

[0091] Although it is not intended to be bound by any specific theory, in the welded joint according to the embodiment of the present invention, it is thought that Al in the initial plating layer acts as follows to suppress or reduce the penetration of Zn, which is liquefied by welding heat input during spot welding, into the interior of the steel plate along the grain boundaries. To explain in more detail, first, the Fe-Al barrier layer formed at the interface between the base steel plate and the plating layer in the plated steel plate is relatively fragile, so it is thought to fracture relatively easily due to the stress loaded on the steel plate caused by the pressure applied by the electrode during spot welding. Since the molten Zn comes into direct contact with the base steel plate due to the fracture of this Fe-Al barrier layer during spot welding, the risk of the molten Zn penetrating into the interior of the steel plate along the grain boundaries increases. However, when a plated steel sheet having a plating layer with an Al concentration distribution as shown in Fig. 2 is used, the Al present in a relatively large amount in the portion of the plating layer other than the Fe-Al barrier layer comes into direct contact with the base steel sheet together with Zn due to the rupture of the Fe-Al barrier layer. In this case, it is believed that the Al in the plating layer reacts with Fe in the base steel sheet due to the heat input during spot welding to form a new Fe-Al barrier layer, and consequently, the ruptured Fe-Al barrier layer is repaired. That is, because there is a large amount of Al in the plating layer other than the Fe-Al barrier layer, even if Zn comes into direct contact with the base steel sheet due to the rupture of the Fe-Al barrier layer during spot welding, a new Fe-Al barrier layer is immediately formed at the rupture site by the Al present right nearby.For this reason, the frequency and duration of direct contact between molten Zn and the base steel sheet are reduced, and the alloying of Zn in the plating layer is suppressed or delayed by the heat input during spot welding. It is believed that, compared to the case of spot welding of conventional Zn-based plated steel sheets, a plating layer with a relatively high proportion of the η phase is formed in the region directly outside the weld area. Furthermore, regarding the formation of this new Fe-Al barrier layer, it is believed that the penetration of molten Zn into the steel sheet during spot welding can be significantly suppressed or reduced, thereby making it possible to reliably suppress or reduce the occurrence of LME cracks. Conventionally, plated steel sheets in which Al is added to a Zn-based plating layer are known. However, it is not conventionally known that by considering the reduction in the melting point of the plating layer, the amount of Al in the entire plating layer is kept relatively low, while at the same time the amount of Al in the plating layer other than the Fe-Al barrier layer is increased, the plating structure of the plated steel sheet in the separation part outside the pressure weld can be changed to a structure with a relatively high proportion of the η phase, and in this regard, the penetration of molten Zn into the steel sheet during spot welding can be suppressed or reduced, and furthermore, the corrosion resistance of the weld can be improved. This fact has been revealed for the first time by the inventors of the present invention.

[0092] Hereinafter, each component of the welded joint according to the embodiments of the present invention will be described in more detail. In the following description, "%", which is the unit of the content of each element, means "mass%" unless otherwise specified. Furthermore, in this specification, "to" indicating a numerical range is used to mean that the values ​​described before and after it are included as lower and upper limits, unless otherwise specified.

[0093] [Plated Steel Sheet]

[0094] In a welded joint according to an embodiment of the present invention, one or more of a plurality of overlapping steel plates are plated steel plates having a base steel plate and a plating layer formed on a surface of the base steel plate corresponding to at least the overlapping surface of the plurality of steel plates. The plating layer of the plated steel plate has the following chemical composition, which is identical to the initial chemical composition prior to spot welding, in the separation portion outside the heat-affected zone.

[0095] [Chemical composition of the plating layer]

[0096] [Al: 0.10 to 1.50%]

[0097] Al is an effective element for inhibiting molten Zn from penetrating into the steel sheet along grain boundaries. To sufficiently obtain this effect, the Al content is set to 0.10% or more. The Al content may be 0.12% or more, 0.15% or more, 0.18% or more, 0.20% or more, 0.25% or more, 0.30% or more, 0.35% or more, 0.40% or more, exceeding 0.50%, 0.52% or more, 0.55% or more, exceeding 0.60%, 0.62% or more, 0.65% or more, or 0.70% or more. On the other hand, if Al is contained excessively, the composition of the plating layer approaches the Zn-Al eutectic composition, causing the melting point of the plating layer to decrease. Consequently, during spot welding, Zn in the plating layer becomes prone to melting, which may accelerate LME cracking. Therefore, the Al content is set to 1.50% or less. The Al content may be 1.45% or less, 1.40% or less, 1.30% or less, 1.20% or less, 1.10% or less, 1.00% or less, 0.90% or less, or 0.80% or less.

[0098] [Fe: 0.01 to 2.00%]

[0099] Fe is an element that is inevitably included in the plating layer, for example, by dissolving from the base steel sheet in the plating bath or by reacting with Al during the plating process to form an Fe-Al barrier layer at the interface between the base steel sheet and the plating layer. For this reason, in the embodiments of the present invention, the Fe content in the plating layer is 0.01% or more. The Fe content may be 0.04% or more, 0.05% or more, 0.10% or more, 0.15% or more, 0.20% or more, 0.25% or more, 0.30% or more, 0.40% or more, or 0.50% or more. On the other hand, if the Fe content in the plating layer is too high, there may be cases where Al in the plating layer combines with Fe, or where a large amount of Al is consumed in the formation of the Fe-Al barrier layer. As a result, there are cases where the effect of adding Al—that is, by the Al in the plating layer—cannot be fully exerted, which suppresses or reduces direct contact between molten Zn and the base steel sheet during spot welding, thereby suppressing the alloying of Zn in the plating layer and suppressing or reducing the occurrence of LME cracks. Therefore, the Fe content is 2.00% or less. The Fe content may be 1.80% or less, 1.60% or less, 1.50% or less, 1.30% or less, 1.20% or less, 1.00% or less, 0.90% or less, 0.80% or less, 0.70% or less, or 0.60% or less.

[0100] The basic chemical composition of the plating layer is as described above. In addition, the plating layer is optionally composed of Mg: 0 to 1.500%, Si: 0 to 1.000%, Ni: 0 to 1.000%, Ca: 0 to 4.000%, Sb: 0 to 0.500%, Pb: 0 to 0.500%, Cu: 0 to 1.000%, Sn: 0 to 1.000%, Ti: 0 to 1.000%, Cr: 0 to 1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0 to 1.000%, Ag: 0 to 1.000%, Li: 0 to 1.000%, La: 0 to 0.500%, Ce: 0 to It may contain at least one of 0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500%, and Sr: 0 to 0.500%. These optional elements shall be present in a total amount of 5.000% or less, from the viewpoint of fully utilizing the action and function of the basic components constituting the plating layer, particularly Al. The optional elements may be present in a total amount of 4.500% or less, 4.000% or less, 3.500% or less, 3.000% or less, 2.500% or less, 2.000% or less, 1.500% or less, or 1.000% or less. These optional elements will be described in detail below.

[0101] [Mg: 0 to 1.500%]

[0102] Mg is an element effective for improving the corrosion resistance of the plating layer. The Mg content may be 0%, but to obtain this effect, it is preferable that the Mg content be 0.001% or more. The Mg content may be 0.010% or more, 0.050% or more, or 0.100% or more. On the other hand, if Mg is contained excessively, a large amount of brittle MgZn-based compounds may be generated within the plating layer, which can cause a decrease in processability. Therefore, it is preferable that the Mg content be 1.500% or less. The Mg content may be 1.200% or less, 1.000% or less, 0.800% or less, or 0.500% or less.

[0103] [Si: 0 to 1.000%]

[0104] Si is an element effective for improving the corrosion resistance of the plating layer. The Si content may be 0%, but if necessary, Si may be contained in the plating layer in an amount of 0.0001% or more or 0.001% or more. On the other hand, if Si is contained excessively, the adhesion of the plating layer may decrease. Therefore, it is preferable that the Si content be 1.000% or less. The Si content may be 0.800% or less, 0.500% or less, 0.100% or less, or 0.050% or less.

[0105] [Ni: 0 to 1.000%]

[0106] Ni is an element effective for improving the corrosion resistance of the plating layer. The Ni content may be 0%, but to obtain this effect, it is preferable that the Ni content be 0.001% or more. The Ni content may be 0.005% or more, 0.010% or more, or 0.020% or more. On the other hand, if Ni is contained excessively, many intermetallic compounds are formed, which may reduce corrosion resistance. Therefore, it is preferable that the Ni content be 1.000% or less. The Ni content may be 0.800% or less, 0.600% or less, or 0.400% or less.

[0107] [Ca: 0 to 4.000%]

[0108] Ca is an element effective for ensuring the wettability of the plating bath. The Ca content may be 0%, but to obtain this effect, it is preferable that the Ca content be 0.001% or more. The Ca content may be 0.010% or more, 0.100% or more, or 1.000% or more. On the other hand, if Ca is contained excessively, a large amount of hard intermetallic compounds are formed within the plating layer, causing the plating layer to become brittle and potentially reducing adhesion to the steel sheet. Therefore, it is preferable that the Ca content be 4.000% or less. The Ca content may be 3.000% or less, 2.000% or less, or 1.500% or less.

[0109] [Sb: 0 to 0.500%, Pb: 0 to 0.500%, Cu: 0 to 1.000%, Sn: 0 to 1.000%, Ti: 0 to 1.000%, Cr: 0 to 1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0 to 1.000%, Ag: 0 to 1.000%, Li: 0 to 1.000%, La: 0 to 0.500%, Ce: 0 to 0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500% and Sr: 0 to 0.500%]

[0110] Sb, Pb, Cu, Sn, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, La, Ce, B, Y, P, and Sr do not need to be included in the plating layer, but may be present in the plating layer in an amount of 0.0001% or more or 0.001% or more. These elements do not adversely affect the performance of the plated steel sheet as long as they are within a predetermined content range. However, if the content of each element is excessive, it may reduce corrosion resistance. Therefore, it is preferable that the content of Sb, Pb, La, Ce, B, Y, P, and Sr be 0.500% or less, and may be, for example, 0.300% or less, 0.100% or less, or 0.050% or less. Likewise, the content of Cu, Sn, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li is preferably 1.000% or less, and may be, for example, 0.800% or less, 0.500% or less, or 0.100% or less.

[0111] In the plating layer, the remainder other than the above elements consists of Zn and impurities. Impurities in the plating layer refer to components that are incorporated due to various factors of the manufacturing process, including raw materials, when the plating layer is manufactured.

[0112] The chemical composition of the plating layer can be determined by dissolving the plating layer in an acid solution to which an inhibitor that inhibits corrosion of the base steel sheet has been added, and measuring the resulting solution by ICP (inductively coupled plasma) emission spectroscopy.

[0113] As for the plating layer, any plating layer having the chemical composition described above may be used and is not particularly limited, but, for example, it is preferably a hot-dip galvanized (GI) layer. For example, if alloying heat treatment is performed, the Fe content in the plating layer increases, and in the final plating layer, it may not be possible to obtain the desired chemical composition and the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet.” In addition, the thickness of the plating layer may be, for example, 3 to 50 μm. The amount of plating layer applied is not particularly limited, but may be, for example, 10 to 170 g / m² per side. The amount of plating layer applied is determined by dissolving the plating layer in an acid solution to which an inhibitor that inhibits corrosion of the base steel sheet has been added, and by the weight change before and after pickling.

[0114] [Ratio of the area ratio of the η phase in the plating layer of the separation part: 10 to 100%]

[0115] In an embodiment of the present invention, in a plating layer of a separation portion in an area of ​​500 μm from the end of the pressure weld, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%. Since the area of ​​500 μm from the end of the pressure weld corresponds to an area within the heat-affected zone, generally, alloying of Zn is likely to proceed in the plating layer in this area due to the heat input during spot welding. In this regard, the ratio of the Γ phase in the plating layer is high, and the ratio of the η phase, which is mainly Zn (Zn concentration of 97 atomic% or more), is relatively low. However, according to an embodiment of the present invention, compared to the case of spot welding of a conventional Zn-plated steel sheet, a plating layer with a relatively high proportion of the η phase is formed in a separation area immediately outside the welded part, that is, in a separation area of ​​500 μm from the end of the welded part, specifically, a plating layer in which the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10% or more as described above. The fact that the proportion of the η phase is relatively high suggests that the alloying of Zn is not sufficiently progressing even by the heat input of spot welding, that is, it can be said to suggest that direct contact between molten Zn and the base steel sheet is suppressed or reduced. In this regard, since the penetration of molten Zn into the interior of the steel sheet during spot welding is suppressed or reduced, it becomes possible to improve the LME resistance of the resulting welded joint. Therefore, from the perspective of improving the LME resistance of the welded joint and, furthermore, the corrosion resistance of the weldment, the higher the proportion of the η phase in the plating layer in the separation portion immediately outside the pressure weldment, the better. For example, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is preferably 15% or more, more preferably 25% or more, most preferably 40% or more, and may be, for example, 50% or more, 60% or more, or 70% or more.The proportion of the η phase can be increased by increasing the Al content of the entire plating layer and applying the method of manufacturing the plated steel sheet, which will be described in detail later. For example, in order to make the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase 25% or more or 40% or more, it is desirable to make the Al content of the entire plating layer 0.30% or more. Meanwhile, the upper limit can be appropriately set within a range of 100% or less. For example, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase may be 95% or less, 90% or less, 85% or less, or 80% or less. In addition, the structure of the plating layer in the separation portion immediately outside the pressure weld portion is mainly composed of the η phase and the Γ phase. Although not particularly limited, the sum of the area ratios of the η phase and the Γ phase may be 70% or more or 80% or more. Likewise, the sum of the area ratios of the η phase and the Γ phase may be 100% or less, 95% or less, or 90% or less.

[0116] [Method for measuring the ratio of the area ratio of the η phase in the plating layer of the separation part]

[0117] The ratio of the η phase in the separation region of 500 μm from the end of the weld is determined as follows. First, a cross-sectional sample of the spot weld is prepared, and then a reflected electron image (BSE image) including the end of the weld is obtained by a scanning electron microscope (SEM-EPMA) equipped with an electron probe microanalyzer, and from the BSE image, the end of the weld of the spot weld and a region of 500 μm extending from the end of the weld toward the separation region (the boundary between the weld and the separation region) are identified. Next, elemental analysis is performed on the identified boundary region to determine the area ratio of the η phase and the area ratio of the Γ phase in the boundary region. Specifically, the η phase is defined as a phase with a Zn concentration of 97 atomic% or more, an Fe concentration of 3 atomic% or less, and other impurities of 3 atomic% or less, and the Γ phase is defined as a phase with a Zn concentration of 87 atomic% or more, an Fe concentration of 8 to 13 atomic%, and other impurities of 3 atomic% or less. The field of view of the SEM image is 100 µm × 100 µm, and similar elemental analysis is performed on five other locations within the boundary region, and the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase in each field of view is calculated. Finally, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is determined by averaging them.

[0118] [Ratio of "Al concentration at the center of the plating layer" / "Al concentration at the location of the plating layer where Fe concentration is 50% of the base steel sheet": 0.10 to 1.50]

[0119] In an embodiment of the present invention, when the plating layer in the separation portion outside the heat-affected zone is measured by glow discharge emission analysis (GDS), it is preferable that the ratio of “Al concentration at the center of the plating layer” to “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” is 0.10 to 1.50. By controlling the ratio of “Al concentration at the center of the plating layer” and “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” measured by GDS to be within this range, the effect of adding Al to the plating layer is fully exerted, and it is assured that during spot welding, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase in the plating layer of the separation portion in the area of ​​500 μm from the end of the pressure weld is controlled to be within the range of 10 to 100%. In a welded joint according to an embodiment of the present invention, the objective of suppressing or reducing the occurrence of LME cracks during spot welding can be achieved by controlling the chemical composition of the plating layer and the ratio of the η phase in the plating layer in the separation portion immediately outside the pressure weld portion within the range described above. Therefore, the above requirement by GDS is not an essential technical feature for achieving the objective of the present invention, but is merely one of the preferred means for reliably controlling the ratio of the η phase in the plating layer of the separation portion within a desired range. Although not particularly limited, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” may be, for example, 0.15 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more. Likewise, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” may be 1.40 or less, 1.30 or less, 1.20 or less, 1.10 or less, or 1.00 or less.

[0120] [Method for measuring the ratio of "Al concentration at the center of the plating layer" / "Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet"]

[0121] The ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel plate” is determined as follows. First, a sample of a plated steel plate is obtained by cutting it to a size of 50 mm × 50 mm from the separation portion outside the heat-affected zone of the weld joint, and then the Al concentration distribution from the surface of the plating layer to a depth of 100 μm is obtained by measuring the said plated steel plate sample by glow discharge emission analysis (GDS). Next, the Al concentration at the depth location where the Fe strength in the GDS measurement is 50% of the Fe strength of the base steel plate (Fe strength at a depth of 100 μm from the surface of the plating layer of the sample) is determined as the “Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel plate,” and the distance from this depth location to the surface is defined as the thickness of the plating layer. The Al concentration by GDS at the 1 / 2 thickness of the plating layer is determined as the “Al concentration at the center of the plating layer,” and finally, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the plating layer position where the Fe concentration is 50% of the base steel sheet” is determined.

[0122] [Base material steel plate]

[0123] In an embodiment of the present invention, the base steel sheet for forming the plating layer is not particularly limited and may be any suitable material, particularly a cold-rolled steel sheet. For example, the base steel sheet may be a material having a chemical composition such that the tensile strength of the plated steel sheet is 780 MPa or higher. Generally, it is known that LME cracking becomes more pronounced when a steel sheet with relatively high strength is spot-welded, and that the susceptibility to LME cracking tends to increase as the strength of the steel sheet increases. Therefore, when a plated steel sheet with a high tensile strength of 780 MPa or higher is used in a welded joint, the effect of suppressing LME cracking becomes particularly pronounced.

[0124] [Desirable Chemical Composition of Base Steel Sheet]

[0125] As described above, the present invention aims to provide a welded joint capable of suppressing or reducing the occurrence of LME cracks during spot welding. This is achieved by making at least one of a plurality of overlapping steel plates into a plated steel plate having a plating layer on a surface corresponding to at least the overlapping surface, controlling the plating layer to have a predetermined chemical composition in the separation portion outside the heat-affected zone, and controlling the ratio of the area ratio of the η phase of the plating layer to the sum of the area ratios of the η phase and the Γ phase in the separation portion of a region of 500 μm from the end of the pressure weld to be within the range of 10 to 100%. Accordingly, it is clear that the chemical composition of the base steel plate having the above plating layer itself is not an essential technical feature for achieving the objective of the present invention. Hereinafter, a preferred chemical composition of a base steel plate is described in detail regarding a plated steel plate useful for use in a welded joint according to an embodiment of the present invention. However, this description is intended to be a simple example of a preferred chemical composition of a base steel plate regarding a plated steel plate having a tensile strength of 780 MPa or more, which is a plated steel plate in which the occurrence of LME becomes significant when spot welded, that is, a plated steel plate having a particularly significant effect in suppressing LME cracking, and it is not intended to limit the present invention to the use of a base steel plate having such a specific chemical composition.

[0126] In an embodiment of the present invention, for example, the base steel sheet is, in mass %,

[0127] C: 0.01 to 0.50%,

[0128] Si: 0.01 to 3.50%,

[0129] Mn: 0.10 to 5.00%,

[0130] P: 0.100% or less,

[0131] S: 0.0300% or less,

[0132] N: 0.0100% or less,

[0133] O: 0 to 0.020%,

[0134] Al: 0 to 1.000%,

[0135] B: 0 to 0.010%,

[0136] Nb: 0 to 0.150%,

[0137] Ti: 0 to 0.20%,

[0138] Mo: 0 to 3.00%,

[0139] Cr: 0 to 2.00%,

[0140] V: 0 to 1.00%,

[0141] Ni: 0 to 2.00%,

[0142] W: 0 to 1.00%,

[0143] Ta: 0 to 0.10%,

[0144] Co: 0 to 3.00%,

[0145] Sn: 0 to 1.00%,

[0146] Sb: 0 to 0.50%,

[0147] Cu: 0 to 2.00%,

[0148] As: 0 to 0.050%,

[0149] Mg: 0 to 0.100%,

[0150] Ca: 0 to 0.100%,

[0151] Zr: 0 to 0.100%,

[0152] Hf: 0 to 0.100%,

[0153] REM: 0 to 0.10, and

[0154] Remainder: Fe and impurities

[0155] It is desirable to have a chemical composition consisting of the following. Each element will be explained in more detail below.

[0156] [C: 0.01 to 0.50%]

[0157] C is an element that increases tensile strength at a low cost and is an important element for controlling the strength of steel. To obtain this effect sufficiently, it is desirable to have a C content of 0.01% or more. The C content may be 0.05% or more, 0.08% or more, 0.09% or more, 0.10% or more, 0.11% or more, 0.12% or more, or 0.15% or more. On the other hand, excessive C content may result in a decrease in elongation. For this reason, it is desirable to have a C content of 0.50% or less. The C content may be 0.40% or less, 0.35% or less, or 0.30% or less.

[0158] [Si: 0.01 to 3.50%]

[0159] Si is an element that acts as a deoxidizer and suppresses the precipitation of carbides during the cooling process in the annealing of cold-rolled sheets. To obtain this effect sufficiently, it is desirable to have a Si content of 0.01% or more. The Si content may be 0.10% or more, 0.12% or more, 0.15% or more, 0.30% or more, or 0.80% or more. On the other hand, if Si is contained excessively, it may result in a decrease in elongation along with an increase in steel strength. For this reason, it is desirable to have a Si content of 3.50% or less. The Si content may be 2.50% or less, 2.00% or less, or 1.50% or less.

[0160] [Mn: 0.10 to 5.00%]

[0161] Mn is an element that influences the ferrite transformation of steel and is effective for increasing strength. To obtain this effect sufficiently, it is desirable to have a Mn content of 0.10% or more. The Mn content may be 0.50% or more, 1.00% or more, or 1.50% or more. On the other hand, if Mn is contained excessively, it may result in a decrease in elongation along with an increase in steel strength. For this reason, it is desirable to have a Mn content of 5.00% or less. The Mn content may be 4.00% or less, 3.00% or less, or 2.50% or less.

[0162] [P: 0.100% or less]

[0163] P is an element that segregates at grain boundaries and promotes the embrittlement of steel. Since a lower P content is desirable, it is ideally 0%. However, an excessive reduction in P content may result in a significant increase in costs. For this reason, the P content may be 0.0001% or more, or 0.001% or more, or 0.005% or more. On the other hand, if P is contained excessively, it may cause embrittlement of steel due to grain boundary segregation as mentioned above. Therefore, it is desirable to keep the P content 0.100% or less. The P content may be 0.050% or less, 0.030% or less, or 0.010% or less.

[0164] [S: 0.0300% or less]

[0165] S is an element that forms non-metallic inclusions, such as MnS, in steel and causes a decrease in the ductility of steel parts. Since a lower S content is desirable, it is ideally 0%. However, excessive reduction of the S content may result in a significant increase in costs. Therefore, the S content may be 0.0001% or more, 0.0002% or more, 0.0010% or more, or 0.0050% or more. On the other hand, excessive S content may cause cracks originating from non-metallic inclusions during cold forming. Therefore, it is desirable to keep the S content 0.0300% or less. The S content may be 0.0200% or less, 0.0150% or less, or 0.0100% or less.

[0166] [N: 0.0100% or less]

[0167] N is an element that forms coarse nitrides in steel sheets and reduces the workability of the steel sheets. Since a lower N content is desirable, it is ideally 0%. However, an excessive reduction in N content may result in a significant increase in manufacturing costs. For this reason, the N content may be 0.0001% or more, 0.0005% or more, or 0.0010% or more. On the other hand, if N is excessively contained, as mentioned above, coarse nitrides may be formed, thereby reducing the workability of the steel sheets. Therefore, it is desirable to keep the N content 0.0100% or less. The N content may be 0.0080% or less, or 0.0050% or less.

[0168] The preferred basic chemical composition of the base steel sheet is as described above. In addition, the base steel sheet, if necessary, instead of a portion of the remainder of Fe, comprises: O: 0 to 0.020%, Al: 0 to 1.000%, B: 0 to 0.010%, Nb: 0 to 0.150%, Ti: 0 to 0.20%, Mo: 0 to 3.00%, Cr: 0 to 2.00%, V: 0 to 1.00%, Ni: 0 to 2.00%, W: 0 to 1.00%, Ta: 0 to 0.10%, Co: 0 to 3.00%, Sn: 0 to 1.00%, Sb: 0 to 0.50%, Cu: 0 to 2.00%, As: 0 to 0.050%, Mg: 0 to 0.100%, Ca: 0 to 0.100%, It may contain one or more selected from the group consisting of Zr: 0 to 0.100%, Hf: 0 to 0.100%, and REM: 0 to 0.100%. Each element may be 0.0001% or more, 0.0005% or more, or 0.001% or more.

[0169] In the base steel sheet, the remainder other than the above elements consists of Fe and impurities. Impurities in the base steel sheet refer to components that are incorporated due to various factors of the manufacturing process, including raw materials such as ore or scrap, when the base steel sheet is manufactured industrially.

[0170] The chemical composition of the base steel sheet can be measured by general analytical methods. For example, the chemical composition of the base steel sheet can be measured by first removing the plating layer by mechanical grinding, and then using Inductively Coupled Plasma-Atomic Emission Spectrometry (ICP-AES). C and S can be measured using the combustion-infrared absorption method, N using the inert gas melt-thermal conductivity method, and O using the inert gas melt-non-dispersive infrared absorption method.

[0171] [Thickness of base steel plate]

[0172] The thickness of the base steel sheet is not particularly limited, but may be, for example, 0.2 mm or more, 0.3 mm or more, 0.6 mm or more, 1.0 mm or more, or 2.0 mm or more. Likewise, the thickness of the base steel sheet may be, for example, 6.0 mm or less, 5.0 mm or less, or 4.0 mm or less.

[0173] [Mechanical properties of galvanized steel sheets]

[0174] A plated steel sheet useful for use in a welded joint according to an embodiment of the present invention may have any suitable tensile strength and is not particularly limited, but it is preferable to have a tensile strength of, for example, 780 MPa or more. As mentioned above, LME cracking becomes significant when a steel sheet with relatively high strength is spot welded. For this reason, when the plated steel sheet has a high tensile strength of 780 MPa or more, the effect of suppressing LME cracking becomes particularly significant compared to the case of a conventional plated steel sheet having the same tensile strength. For example, in an embodiment of the present invention, the tensile strength of the plated steel sheet may be 980 MPa or more, 1080 MPa or more, or 1180 MPa or more. Although the upper limit is not particularly limited, for example, the tensile strength of the plated steel sheet may be 2300 MPa or less, 2000 MPa or less, 1800 MPa or less, or 1500 MPa or less. Tensile strength is measured by taking a JIS No. 5 test specimen from a direction in which the longitudinal direction of the test specimen is parallel to the rolling direction of the plated steel sheet, and performing a tensile test in accordance with JIS Z 2241:2011.

[0175] Method for manufacturing galvanized steel sheets

[0176] Next, a preferred method for manufacturing a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention, more specifically, a plated steel sheet having a plating layer in which the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” is 0.10 to 1.50 when measured by glow discharge emission analysis (GDS), will be described. The following description is intended to be an example of a characteristic method for manufacturing the said plated steel sheet, and is not intended to limit the said plated steel sheet to being manufactured by the manufacturing method described below.

[0177] Galvanized steel sheets can be manufactured by performing, for example, a casting process in which molten steel with adjusted chemical composition is cast to form a steel billet; a hot rolling process in which the steel billet is hot-rolled to obtain a hot-rolled steel sheet; a coiling process in which the hot-rolled steel sheet is coiled; a cold rolling process in which the coiled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet; a pretreatment process; an annealing process in which the pretreated cold-rolled steel sheet is annealed; and a plating process in which a plating layer is formed on the obtained base steel sheet. Generally, the cold rolling process may be performed directly after pickling without coiling after the hot rolling process. Each process is described in detail below.

[0178] [Casting Process]

[0179] The conditions of the casting process are not particularly limited. For example, various secondary smelting processes can be performed in addition to the flux from a blast furnace or converter, and then casting can be done using methods such as normal continuous casting or ingot casting.

[0180] [Hot Rolling Process]

[0181] Hot-rolled steel sheets can be obtained by hot-rolling a cast steel billet. The hot-rolling process is carried out by reheating the cast steel billet either directly or after cooling and then hot-rolling it. When reheating is performed, the heating temperature of the steel billet may be, for example, 1100 to 1250°C. In the hot-rolling process, rough rolling and finish rolling are typically performed. The temperature and reduction ratio of each rolling step can be appropriately determined according to the desired metal structure or sheet thickness. For example, the finishing temperature of the finish rolling step may be 900 to 1050°C, and the reduction ratio of the finish rolling step may be 10 to 50%.

[0182] [Winding Process]

[0183] Hot-rolled steel sheets can be coiled at a predetermined temperature. The coiling temperature can be appropriately determined according to the desired metal structure, etc., and, for example, may be 500 to 800°C. Before or after coiling, the hot-rolled steel sheet may be rewound to apply a predetermined heat treatment. Alternatively, the coiling process may be omitted, and the cold rolling process described later may be performed by pickling after the hot rolling process.

[0184] [Cold Rolling Process]

[0185] After performing pickling or the like on a hot-rolled steel sheet, a cold-rolled steel sheet can be obtained by cold-rolling the hot-rolled steel sheet. The reduction ratio of cold rolling can be appropriately determined according to the desired metal structure or sheet thickness, and, for example, may be 20 to 80%. After the cold-rolling process, the sheet may be cooled to room temperature, for example by air cooling.

[0186] [Pretreatment Process]

[0187] Next, it is effective to perform a predetermined pretreatment process before annealing the cold-rolled steel sheet. Such pretreatment processes may include degreasing treatment and optional grinding treatment. The degreasing treatment may include, for example, passing an electric current through the cold-rolled steel sheet in a solution with a pH of 8.0 or higher (electrolytic treatment). The current density during application may be 1.0 to 8.0 A / dm², and the application time may be 5 to 10 seconds. Meanwhile, optional grinding treatment is preferably performed using a heavy grinding brush. By introducing deformation to the surface of the cold-rolled steel sheet through grinding using a heavy grinding brush, the nucleation of the Fe-Al barrier layer is promoted during the plating process after the annealing process, thereby densifying the Fe-Al barrier layer. Consequently, the growth rate of the Fe-Al barrier layer is slowed down, allowing the thickness to be reduced. As a result, the amount of Al consumed in the formation of the Fe-Al barrier layer can be reduced. Therefore, since the amount of Al in the plating layer other than the Fe-Al barrier layer can be increased, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel sheet” can be increased in the finally obtained plated steel sheet. The grinding treatment is not particularly limited, but can be performed by, for example, using a heavy grinding brush to grind the surface of the cold-rolled steel sheet under conditions of a grinding amount of 10 to 200 g / m². The grinding amount by the heavy grinding brush can be adjusted by any suitable method known to those skilled in the art, and is not particularly limited, but can be adjusted by, for example, appropriately selecting the number of heavy grinding brushes, rotation speed, brush reduction amount, and the coating liquid used.

[0188] [Annealing Process]

[0189] Annealing is performed on a cold-rolled steel sheet that has undergone a pretreatment process. The holding temperature during the annealing process is preferably 700 to 900°C. If the holding temperature during the annealing process exceeds 900°C, an external oxide layer may form on the surface of the steel sheet, potentially leading to a decrease in plating performance. The heating rate to the above holding temperature is not particularly limited, but may be 1 to 10°C / second. The holding time at the above holding temperature is preferably 10 to 300 seconds, and more preferably 80 to 120 seconds. If the holding time exceeds 300 seconds, the external oxide may grow excessively, potentially leading to a decrease in plating performance. The dew point of the atmosphere during the annealing process is preferably -20 to 10°C, and more preferably -10 to 5°C. If the dew point is too low, an external oxide layer may form on the surface of the steel sheet, potentially leading to a decrease in plating performance. On the other hand, if the dew point is too high, Fe oxide may similarly form on the surface of the steel sheet as an external oxide, potentially leading to a decrease in plating performance. In addition, the atmosphere in the annealing process may be a reducing atmosphere, more specifically a reducing atmosphere containing nitrogen and hydrogen, for example, a reducing atmosphere of 1 to 10% hydrogen (for example, 4% hydrogen and nitrogen balance).

[0190] [Plating Process]

[0191] Next, in the plating process, a plating layer having the chemical composition and structure described above is formed on at least one, preferably both, surface of a cold-rolled steel sheet (base steel sheet). More specifically, the plating process is carried out by molten plating using a plating bath whose composition is adjusted so that, for example, the chemical composition of the plating layer is within the range described above. In the plating process, it is very important to first control the time from immersing the steel sheet in the plating bath until the start of cooling to 6 seconds or less, and then to control the average cooling rate from the bath temperature (e.g., 420 to 480°C) to 370°C to 20°C / second or more. By satisfying these requirements, the Fe-Al barrier layer can be thinned, thereby reducing the amount of Al consumed in forming the Fe-Al barrier layer, and thus it becomes possible to secure a sufficient amount of Al present in the plating layer other than the Fe-Al barrier layer. As a result, in the finally obtained plated steel sheet, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel sheet” can be 0.10 or higher. On the other hand, if either of these requirements is not satisfied, that is, if the time from the start of immersion of the steel sheet into the plating bath to the start of cooling exceeds 6 seconds and / or the average cooling rate from the bath temperature to 370°C is less than 20°C / second, a large amount of Al is consumed in the formation of the Fe-Al barrier layer, and the amount of Al in the plating layer other than the Fe-Al barrier layer decreases. As a result, in the finally obtained plated steel sheet, the desired ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of that of the base steel sheet” cannot be obtained.

[0192] From the perspective of further improving the LME resistance of a welded joint, it is desirable that the time from the start of immersion of the steel sheet in the plating bath to the start of cooling be shorter, and the average cooling rate from the bath temperature to 370°C be faster. For example, it is possible to further improve the LME resistance of a welded joint by setting the total Al content of the plating layer to 0.30% or more, the time from the start of immersion of the steel sheet in the plating bath to the start of cooling be 4 seconds or less, and the average cooling rate from the bath temperature to 370°C be 40°C / second or more. In the case where grinding treatment with a heavy grinding brush is performed as the pretreatment process described above, even if the time from the start of immersion of the steel sheet in the plating bath to the start of cooling is 6 seconds or less and the average cooling rate from the bath temperature to 370°C is 20°C / second or more, the same higher LME resistance can be achieved by combining it with the condition that the total Al content of the plating layer is 0.30% or more. Alternatively, it is possible to more significantly improve the LME resistance of the welded joint by setting the total Al content of the plating layer to 0.30% or more, performing grinding treatment with a heavy grinding brush as the pretreatment process described above, and setting the time from the start of immersion of the steel sheet in the plating bath to the start of cooling to 4 seconds or less, and the average cooling rate from the bath temperature to 370°C to 40°C / second or more. The lower limit of the time from the start of immersion of the steel sheet in the plating bath to the start of cooling is not specifically limited, but for example, the time from the start of immersion of the steel sheet in the plating bath to the start of cooling may be 2 seconds or more. Likewise, the upper limit of the average cooling rate from the bath temperature to 370°C is not specifically limited, but for example, the average cooling rate from the bath temperature to 370°C may be 80°C / second or less. Other conditions of the plating process may be appropriately set considering the thickness and amount of the plating layer, etc.For example, by immersing a cold-rolled steel sheet in a plating bath, lifting it, immediately spraying N2 gas or air by a gas wiping method, and then cooling it, the amount of the plating layer can be adjusted to a predetermined range, for example, within a range of 10 to 170 g / m² per side.

[0193] Since the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” is controlled to be within the range of 0.10 to 1.50 in the plating steel sheet produced by the present manufacturing method, when used for spot welding, the structure of the initial plating layer changes in the separation area of ​​500 μm from the end of the pressure weld, and a plating layer is formed in which the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%, and in this regard, it is possible to significantly suppress or reduce the penetration of molten Zn into the steel sheet during spot welding.

[0194] [Other steel plates]

[0195] Among the plurality of steel plates used in the welded joint according to the embodiment of the present invention, any suitable steel plate or plated steel plate may be used as a steel plate other than the plated steel plate described above. Such a steel plate may, for example, have a tensile strength of 780 MPa or more, similar to the preferred embodiment of the plated steel plate, or may have a tensile strength of less than 780 MPa. Accordingly, regarding the steel plate other than the plated steel plate described above, a suitable steel plate or plated steel plate may be appropriately selected depending on the application of the welded joint or desired characteristics, such as the desired joint strength.

[0196] Method for manufacturing welded joints

[0197] A welded joint according to an embodiment of the present invention can be manufactured by applying any suitable spot welding method known to those skilled in the art to a plurality of steel plates in which the above-mentioned plated steel plate is used for all steel plates and the steel plates are overlapped, or to a plurality of steel plates in which the above-mentioned plated steel plate is used for one or more steel plates and the plated steel plate is overlapped with another steel plate or another plated steel plate. For example, a welded joint according to an embodiment of the present invention can be manufactured by forming a nugget and a pressure welded portion around it by applying pressure using a pair of opposing electrodes and passing current between the electrodes under normal conditions while applying pressure to the plurality of steel plates overlapped as above. The conditions for spot welding may be any suitable conditions known to those skilled in the art. For example, the welding electrode may be a dome radius type welding electrode with a tip diameter of 6 to 8 mm, the applying force may be 1.5 to 6.0 kN, the current application time may be 0.1 to 1.0 s (5 to 50 cycles, power frequency 50 Hz), the current application current may be 4 to 15 kA, and the angle (the angle formed by the axial direction of the electrode and the direction perpendicular to the surface of the steel plate) may be 0 to 10°.

[0198] According to the weld joint manufactured as described above, the effect of adding Al to the plating layer is fully exerted, allowing the ratio of the η phase in the plating layer in the separation portion outside the pressure weld to be controlled within a desired range, and in this regard, it becomes possible to suppress or reduce the penetration of molten Zn into the steel sheet during spot welding. Therefore, with this weld joint, it is possible to achieve superior LME resistance compared to the case where a conventional plated steel sheet is used with a plating layer having the same chemical composition, more specifically, a Zn-based plating layer having the same Al content, and particularly in use in the automotive field, it can contribute to industrial development by improving collision safety and extending lifespan.

[0199] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to these examples at all.

[0200] Examples

[0201] In the following examples, plated steel sheets were manufactured under various conditions, and the LME resistance of welded joints manufactured by spot welding the manufactured plated steel sheets was investigated.

[0202] [Manufacture of galvanized steel sheets]

[0203] First, molten steel having a chemical composition in mass % consisting of C: 0.15%, Si: 1.00%, Mn: 2.60%, P: 0.010%, S: 0.0020%, N: 0.0100%, Al: 0.020%, and the remainder: Fe and impurities was cast by a continuous casting method to form a steel billet. The steel billet was cooled once, then reheated to 1200°C for hot rolling, and subsequently coiled at 600°C. Hot rolling was performed by carrying out rough rolling and finish rolling, with the finish rolling end temperature being 950°C and the reduction rate of the finish rolling being 30%. Next, the obtained hot-rolled steel sheet was pickled and subsequently cold-rolled at a reduction rate of 50% to obtain a cold-rolled steel sheet having a thickness of 1.6 mm. Next, the obtained cold-rolled steel sheet was subjected to pretreatment by passing current at a current density of 5.0 A / dm² for 8 seconds in a solution of pH 9.2, and subsequently, if necessary, a 2.0% aqueous NaOH solution was applied to the cold-rolled steel sheet, and then the surface of the cold-rolled steel sheet was ground using a heavy grinding brush (Hotani D-100) at a grinding amount of 10 to 200 g / m², a brush reduction amount of 2.0 mm, and a rotational speed of 600 rpm, thereby introducing deformation to the surface of the cold-rolled steel sheet. The presence or absence of grinding by the heavy grinding brush for each cold-rolled steel sheet is shown in Table 1.

[0204] Next, each cold-rolled steel sheet was cut to a size of 100 mm × 200 mm, and then an annealing treatment (annealing atmosphere: 4% hydrogen and nitrogen balance) was performed under conditions of a dew point of 0°C, a holding temperature of 870°C, and a holding time of 100 seconds. For all steel sheet samples, the heating rate during annealing was set to 5°C / second. Next, the cut steel sheet samples were subjected to plating treatment using a molten zinc plating bath having a predetermined bath composition under conditions of the bath temperature shown in Table 1, the time from immersion in the plating bath to the start of cooling, and an average cooling rate from the bath temperature to 370°C, thereby obtaining plated steel sheet samples with plating layers formed on both surfaces of the steel sheet samples. The plating adhesion amount was adjusted to 50 g / m² per side by N2 gas wiping before the start of cooling after lifting the steel sheet samples from the plating bath following immersion. In Comparative Example 28, an alloying heat treatment of 520°C × 10 seconds was performed after the hot-dip galvanizing treatment.

[0205] [Tensile strength of galvanized steel sheets]

[0206] Tensile strength was measured by taking a JIS No. 5 test specimen from a direction in which the longitudinal direction of the test specimen was parallel to the rolling direction of the galvanized steel sheet sample, and performing a tensile test in accordance with JIS Z 2241:2011. As a result, the tensile strength of all galvanized steel sheet samples was 780 MPa or higher.

[0207] [Measurement of Al concentration distribution in the plating layer]

[0208] First, a plated steel sheet sample was cut to a size of 50 mm × 50 mm, and then the cut plated steel sheet sample was subjected to GDS measurement to obtain the Al concentration distribution from the surface of the plating layer to a depth of 100 μm. Next, the Al concentration at a depth position where the Fe strength in the GDS measurement is 50% of the Fe strength of the base steel sheet (Fe strength at a depth of 100 μm from the surface of the plating layer of the sample) was determined as the “Al concentration at the plating layer position where the Fe concentration is 50% of that of the base steel sheet,” and the distance from this depth position to the surface was defined as the thickness of the plating layer. The Al concentration by GDS at a position halfway the thickness of the plating layer was determined as the “Al concentration at the center of the plating layer,” and finally, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the plating layer position where the Fe concentration is 50% of that of the base steel sheet” was determined. As a result, in the plated steel sheet samples of all embodiments (inventive examples), the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” was controlled within the range of 0.10 to 1.50.

[0209] [Manufacturing of welded joints]

[0210] Among the obtained plated steel sheet samples, a plated steel sheet sample with a size of 100×100 mm was provided for spot welding. Two sheets were prepared by cutting them to a size of 50 mm×100 mm, and a welded joint was manufactured by performing spot welding on these two plated steel sheet samples using a dome radius welding electrode with a tip diameter of 8 mm, with a welding angle of 5°, a pressure of 4.0 kN, a current application time of 0.5 seconds, and a current of 9 kA.

[0211] [Analysis of Chemical Composition of Plating Layer]

[0212] The chemical composition of the plating layer was determined by immersing a 30 mm × 30 mm sample taken from the separation area outside the heat-affected zone of the weld joint in a 10% HCl aqueous solution containing an inhibitor (Evit, manufactured by Asahi Kagaku High School), acid-peeling the plating layer, and then measuring the plating components dissolved in the aqueous solution by ICP emission spectroscopy. The results are shown in Table 1.

[0213] [Measurement of the ratio of the area ratio of the η phase in the plating layer of the separation part]

[0214] The proportion of the η phase in the separation region extending 500 μm from the end of the weld was determined as follows. First, a cross-sectional sample of the spot weld was prepared, and subsequently, a BSE phase including the end of the weld was obtained by SEM-EPMA. From the BSE phase, the end of the weld of the spot weld and a 500 μm region extending from the end of the weld toward the separation region (the boundary between the weld and the separation region) were identified. Next, elemental analysis was performed on the identified boundary region, and the area ratio of the η phase and the area ratio of the Γ phase at the boundary region were determined. Specifically, the η phase was defined as a phase with a Zn concentration of 97 atomic% or more, an Fe concentration of 3 atomic% or less, and other impurities of 3 atomic% or less, and the Γ phase was defined as a phase with a Zn concentration of 87 atomic% or more, an Fe concentration of 8 to 13 atomic%, and other impurities of 3 atomic% or less. The field of view of the SEM image was 100㎛ × 100㎛, and similar elemental analysis was performed on five other locations within the boundary region, and the ratio of the area ratio of phase η to the sum of the area ratios of phase Γ in each field of view was calculated. Finally, the ratio of the area ratio of phase η to the sum of the area ratios of phase Γ was determined by averaging them. In this regard, for the welded joints of all embodiments (inventive examples), the sum of the area ratios of phase η and phase Γ in the separation region of 500㎛ from the end of the pressure weld was 80% or more.

[0215] [Assessment of LME Resistance]

[0216] After cross-sectionally grinding the weld of the manufactured welded joint, it was observed under an optical microscope, the length of the LME cracks formed on the cross-section of the separation area around the pressure weld was measured, and the LME resistance was evaluated as follows.

[0217] AAA: No LME cracks,

[0218] AA: LME crack length greater than 0㎛ to 100㎛,

[0219] A: LME crack length greater than 100㎛ to 500㎛,

[0220] B: LME crack length exceeding 500㎛

[0221] [Evaluation of Corrosion Resistance of Welded Joints]

[0222] Chemical and electrodeposition coatings were applied to the manufactured welded joints, and subjected to a combined cycle corrosion test in accordance with JASO (M609-91) to evaluate the corrosion resistance of the spot welds based on the corrosion conditions of the steel. For each evaluation sample, after the completion of the corrosion test, the corrosion resistance of the welds was evaluated based on the following evaluation criteria, according to the rust formation conditions of the spot welds and each cycle in which red rust occurs.

[0223] AAA: No red-rust formation at over 240 to 360 cycles

[0224] AA: No red-rust formation at over 180 to 240 cycles

[0225] A: No reddish-rust formation in over 90 to 180 cycles

[0226] B: Red-green occurrence at 90 cycles

[0227] The cases of LME resistance AAA, AA, and A were evaluated as weld joints capable of suppressing or reducing the occurrence of LME cracks during spot welding. The results are shown in Table 1 below.

[0228]

[0229] Referring to Table 1, in Comparative Example 26, the Al content of the entire plating layer was low, so the effect of suppressing LME cracking by adding Al could not be fully exerted, and thus the LME resistance was reduced. In Comparative Example 27, the melting point of the plating layer was lowered because the Al content of the entire plating layer was high. As a result, Zn in the plating layer became more prone to melting during spot welding, and thus the LME resistance was reduced. In Comparative Example 28, the Fe content in the plating layer increased due to the alloying heat treatment, so the desired plating chemical composition was not obtained, and the ratio of "Al concentration at the center of the plating layer" to "Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet" also became less than 0.10. In this regard, the ratio of the area ratio of the η phase in the plating layer outside the pressure welding area became 0%. In Comparative Example 28, since the desired ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” was not obtained, it is thought that the direct contact between molten Zn and the base steel sheet during spot welding could not be suppressed or reduced by the Al in the plating layer, and thus the alloying of Zn in the plating layer was promoted. Furthermore, as a result, the LME resistance was reduced. In Comparative Example 29, since the time from immersion in the plating bath to the start of cooling was long, a large amount of Al was consumed in the formation of the Fe-Al barrier layer, and it is thought that the amount of Al in the plating layer other than the Fe-Al barrier layer was reduced. As a result, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” became less than 0.10, and for the same reason as in Comparative Example 28, the ratio of the area ratio of the η phase in the plating layer outside the pressure welding area decreased, and the LME resistance decreased. In Comparative Example 30, because the average cooling rate from the bath temperature to 370°C was slow, a large amount of Al was consumed in the formation of the Fe-Al barrier layer, and it is thought that the amount of Al in the plating layer other than the Fe-Al barrier layer decreased.As a result, the ratio of “Al concentration at the center of the plating layer” / “Al concentration at the location of the plating layer where the Fe concentration is 50% of the base steel sheet” became less than 0.10, and for the same reason as in Comparative Examples 28 and 29, the ratio of the area of ​​the η phase in the plating layer outside the welded part was reduced, and thus the LME resistance was reduced. In addition, in Comparative Examples 26 and 28 to 30, where the ratio of the area of ​​the η phase in the plating layer outside the welded part was low, the corrosion resistance of the welded part was also reduced because the ratio of the η phase, which is mainly Zn, was low.

[0230] In contrast, in the weld joints according to all embodiments, by having a predetermined plating chemical composition and controlling the ratio of the area ratio of the η phase in the plating layer outside the pressure weld to within the range of 10 to 100%, the effect of adding Al to the plating layer is fully exerted to reliably suppress or reduce LME cracking, and furthermore, because the ratio of the η phase, which is mainly Zn, was high, the corrosion resistance of the weld was also improved. In particular, in Examples 3 to 5, in which the total Al content of the plating layer was 0.30% or more and grinding with a heavy grinding brush was performed as a pretreatment for the annealing process (wherein the time from the start of immersion of the steel plate in the plating bath to the start of cooling was 6 seconds and the average cooling rate from the bath temperature to 370°C was 20°C / second), and in Example 16, in which the total Al content of the plating layer was 0.30% or more, the time from the start of immersion of the steel plate in the plating bath to the start of cooling was 4 seconds and the average cooling rate from the bath temperature to 370°C was 40°C / second (no grinding with a heavy grinding brush), the ratio of the area ratio of the η phase in the plating layer outside the pressure weld was 25% or more, and as a result, the evaluation of LME resistance and weld corrosion resistance was AA, and LME resistance and weld corrosion resistance were improved. In addition, in Examples 6 to 15, 17 and 19 to 25, in which the total Al content of the plating layer is 0.30% or more, grinding with a heavy grinding brush is performed as a pretreatment for the annealing process, and the time from the start of immersion of the steel plate in the plating bath to the start of cooling is 4 seconds, and the average cooling rate from the bath temperature to 370°C is 40°C / second, the ratio of the area ratio of the η phase in the plating layer outside the pressure weld is 40% or more, and as a result, the evaluation of LME resistance and weld corrosion resistance is AAA, and LME resistance and weld corrosion resistance are further improved. Explanation of the symbols

[0231] 1: Welded joint 11: Steel plate 12: Nugget 13: Pressure weld 14: Pressure weld end 15: Heat-affected zone 16: Spot weld 17: Separation Department 18: Plating layer

Claims

Claim 1 A welded joint comprising a plurality of overlapping steel plates, a nugget joining the plurality of steel plates, a spot weld portion having a pressure weld portion and a heat-affected zone formed around the nugget, and a separation portion located around the pressure weld portion; wherein one or more of the plurality of steel plates are plated steel plates having a base steel plate and a plating layer formed on a surface of the base steel plate corresponding to at least the overlapping surface of the plurality of steel plates, and wherein the plating layer in the separation portion outside the heat-affected zone contains, in mass%, Al: 0.10 to 1.50% and Fe: 0.01 to 2.00%, and also Mg: 0 to 1.500%, Si: 0 to 1.000%, Ni: 0 to 1.000%, Ca: 0 to 4.000%, Sb: 0 to 0.500%, Pb: 0 to 0.500%, Cu: 0 to 1.000%, Sn: 0 to 1.000%, Ti: 0 to 1.000%, Cr: 0 to 1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0 to 1.000%, Ag: 0 to 1.000%, Li: 0 to 1.000%, La: 0 to 0.500%, Ce: 0 to 0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500%, and Sr: 0 to 0.500%, with at least one of these totaling 5.A welded joint characterized by having a chemical composition containing 000% or less and the remainder consisting of Zn and impurities, wherein in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 10 to 100%, wherein the η phase refers to a phase in which the Zn concentration is 97 atomic% or more, the Fe concentration is 3 atomic% or less, and other elements are 3 atomic% or less as measured by a scanning electron microscope (SEM-EPMA) equipped with an electron probe microanalyzer, and the Γ phase refers to a phase in which the Zn concentration is 87 atomic% or more, the Fe concentration is 8 to 13 atomic%, and other impurities are 3 atomic% or less as measured by SEM-EPMA, and wherein the plating layer is a hot-dip galvanized (GI) layer. Claim 2 A welded joint according to claim 1, characterized in that the chemical composition contains Al: 0.30 to 1.50% in mass%, and in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 25 to 100%. Claim 3 A welded joint according to claim 1, characterized in that the chemical composition contains Al: 0.30 to 1.50% in mass%, and in the plating layer of the separation portion in an area of ​​500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the sum of the area ratios of the η phase and the Γ phase is 40 to 100%. Claim 4 A welded joint characterized in that, in any one of claims 1 to 3, the plated steel sheet has a tensile strength of 780 MPa or more. Claim 5 delete

Citation Information

Patent Citations

  • Method for producing hot dip galvannealed steel sheet having pure zinc layer

    JP2005248236A

  • Galvanized steel sheet with excellent liquid metal embrittlement resistance and hydrogen embrittlement resistance and method for manufacturing thereof

    KR1020210079054A

  • Process for Producing a Sheet Steel Product Coated with an Anticorrosion System