Method for manufacturing graphene electronic device precursors
The method addresses contamination and doping issues in 2D material devices by using plasma etching and a protective coating to expose graphene edges for ohmic contact, ensuring stable electrical connectivity and improved device performance.
Patent Information
- Application Number
- KR1020237024543
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-23
- Filing Date
- 2021-12-17
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-12-17
AI Technical Summary
Existing methods for manufacturing electronic devices with 2D materials face issues such as contamination, doping, and performance degradation due to atmospheric interactions, particularly with ohmic contacts, leading to instability and reduced lifespan.
A method involving plasma etching and a plasma-resistant dielectric to expose graphene edges for direct ohmic contact, combined with a protective coating, to prevent doping and contamination while maintaining electrical connectivity.
The method ensures stable and reliable electrical contact with reduced contamination, enhancing the lifespan and performance of 2D material-based devices under various conditions.
Smart Images

Figure 112023078917450-PCT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention provides a method for manufacturing an electronic device precursor. In particular, the method comprises the steps of plasma etching to expose the edge surface of a graphene layer to make direct contact with an ohmic contact, and forming said ohmic contact. Additionally, the present invention provides electronic device precursors, particularly electronic device precursors comprising a graphene layer that makes direct contact with an ohmic contact at the edge portion. Additionally, the electronic device precursor comprises a continuous air-resistant coating layer to protect the edges of the graphene layer. Most preferably, the electronic device precursor is for a Hall effect sensor. Background Technology
[0002] Two-dimensional (2D) materials, particularly graphene, are currently the focus of intensive research and development worldwide. 2D materials have been shown to possess special properties in both theory and practice, leading to a surge in products incorporating these materials, including, to name a few, coatings, batteries, and sensors. Graphene stands out the most, and various potential applications are being investigated. Most notably, graphene is being used in electronic devices and their constituent components, including transistors, LEDs, photovoltaics, Hall-effect sensors, diodes, and similar devices.
[0003] Accordingly, there exist a wide range of electronic devices known in the prior art having integrated graphene layer structures (single-layer or multilayer graphene) and / or other 2D materials as key materials to provide improvements in these devices compared to early devices and electronic products. These include structural improvements through the use of thinner and lighter materials (which may result in flexible electronic devices), as well as performance improvements such as increased electrical and thermal conductivity leading to increased operational efficiencies.
[0004] However, because exposed 2D materials are sensitive to atmospheric interactions and contamination, it is necessary to encapsulate the 2D materials and / or devices containing such materials with protective layers. The inventors have discovered that metals present in ohmic contacts required to form electrical connections to 2D materials can lead to undesirable doping. Doping of 2D materials results in changes to their electronic properties. For devices such as Hall effect sensors (also known as Hall sensors), device operation relies on maintaining charge neutrality within the 2D material as close as possible, making them highly sensitive to changes in their electronic structure. Nevertheless, contamination by atmospheric oxygen or water vapor can cause device performance degradation over time, which is undesirable for customers / consumers who expect electronic devices to maintain a certain level of performance for years after manufacturing. Furthermore, since retroactive replacement of electronic components, particularly microelectronic components, may be impossible or at least very difficult, even minor improvements in lifespan and performance stability are highly valuable.
[0005] During the manufacture of electronic devices, the inventors have discovered that standard lithography processes, such as those using polymer coatings like PMMA to etch desired configurations of underlying 2D materials, have several drawbacks. PMMA coatings can dope 2D materials and may not be suitable for variable temperature applications, or particularly for high or low temperature applications. Standard treatments for removing these polymer coatings by dissolving them in organic solvents can further introduce impurities and contaminants that hinder the manufacture of reliable devices with consistent properties essential for electronic devices, such as microelectronic devices. Nevertheless, it is also known that polymer residues may remain and interfere with subsequent processing steps.
[0006] Alternatively, to avoid contamination, it is known that 2D materials can be simply laser-etched from a substrate without using such photolithographic materials. Such methods involve using a laser beam to ablate the substrate and 2D material outside the active area to leave a patterned 2D material layer. One such disclosure can be found in GB 2570124 A, which discloses using a laser with a wavelength greater than 600 nm and a power of less than 50 watts to selectively remove graphene from a substrate having a thermal resistance greater than that of sapphire. While this process has been found to work well in patterning without damaging the graphene layer structure or the underlying substrate, it can generate large debris particles that may fall onto the surface of the 2D material. The debris acts as a contaminant or prevents the formation of an effective and / or hermetic coating on the 2D material, at least.
[0007] Therefore, it is desirable to manufacture electronic devices containing 2D materials (or, in fact, to produce electronic device precursors for use as electronic devices when providing necessary electrical connections) through methods that involve fewer processing steps and avoid unnecessary and harmful contamination and / or doping. Consequently, there is also a demand for electronic devices and their precursors that provide improvements in long-term stability and / or temperature stability compared to conventional technology. To benefit from the inherent electronic properties of 2D materials, improvements are required to allow the use of 2D material-based devices under extreme conditions.
[0008] The inventors also discovered that contact deposition after device encapsulation prevents the metal from making electrical contact with the 2D material essential for the final electronic device to function. However, contact deposition prior to encapsulation or the coating layer can cause problems due to a height difference between the 2D material and the contacts thereon, leading to a non-shape-following coating that can be more easily damaged.
[0009] CN 103985762 discloses a graphene transistor with ultra-low ohmic contact resistance. The method disclosed herein includes patterning a dielectric layer with a photoresist and etching the dielectric layer using wet chemical techniques (e.g., buffered oxide etch (BOE), or a mixture of nitric acid and hydrogen peroxide (HNO3 + H2O2)).
[0010] "The Dependence of the High-Frequency Performance of Graphene Field-Effect Transistors on Channel Transport Properties", Asad et al. Journal of the Electron Devices Society, 8, 2020, 457-464 discloses a graphene field-effect transistor comprising a patterned Al2O3 dielectric layer using lithography techniques and etching to remove the dielectric from contact regions on graphene.
[0011] There remains a need for a method that allows the fabrication of electronic device precursors comprising a 2D material layer and prevents surface contamination as well as doping by ohmic contact deposition. Additionally, there remains a need for a method that can encapsulate the 2D material while allowing the provision of at least one ohmic contact. The object of the present invention is to provide a method that overcomes or substantially reduces various problems associated with the prior art, or at least provides a commercially useful alternative, and a number of specific embodiments each comprising electronic device precursors obtainable by such methods.
[0012] Accordingly, the inventors have devised a method comprising the step of protecting a graphene layer on a substrate using a plasma-resistant dielectric for both defining an etching pattern of the graphene layer and serving as a protective coating within the final device precursor (and, of course, ultimately within the device). The inventors have discovered that by using a plasma-resistant dielectric to define an etching pattern of a plasma-etchable layer structure containing graphene, this provides an intermediate that leaves only the edges of the graphene layer exposed, and that an ohmic contact can be formed in direct contact with a portion of the exposed edges.
[0013] Accordingly, according to a first aspect of the present invention, a method for manufacturing an electronic device precursor is provided, and the method is:
[0014] (i) providing a plasma-etchable layer structure on a plasma-resistant substrate - the layer structure has an exposed top surface -;
[0015] (ii) patterning a plasma-resistant dielectric on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a layer structure;
[0016] (iii) a step of plasma etching the intermediate—thereby etching away at least one uncovered region of the layer structure to form at least one covered region of the layer structure having an exposed edge surface—; and
[0017] (iv) A step of forming an ohmic contact that is in direct contact with a portion of the exposed edge surface
[0018] A plasma-etchable layer structure comprising one or more graphene layers extending across covered regions of the layer structure to an exposed edge surface.
[0019] The present disclosure will be further explained below. In the following passages, different aspects / exemplars of the present disclosure are defined in more detail. Each aspect / exemplar defined in this way may be combined with any other aspects / exemplars or aspects / exemplars unless clearly indicated otherwise. In particular, any feature indicated as preferred or advantageous may be combined with any other feature or feature indicated as preferred or advantageous.
[0020] Therefore, the method disclosed herein uses a plasma-resistant dielectric to define an etching pattern and protect the surface of a 2D material from being doped by ohmic contacts. This solution is particularly clear because the inventors discovered that charge injection is much greater at the edges of the 2D material layer than at the surface, and thus allows for improved current flow while avoiding doping.
[0021] As described above, the present invention provides a method for manufacturing an electronic device precursor. The precursor is intended to refer to a component that can be installed in an electrical or electronic circuit, typically by wire bonding to an additional circuit, or by other methods known in the art, such as soldering using "flip-chip" style solder bumps as described herein. Accordingly, the electronic device is a functional device that provides current to the precursor when installed and during operation.
[0022] The method comprises a first step of providing a plasma-etchable layer structure on a plasma-resistant substrate, wherein the layer structure has an exposed top surface and the plasma-etchable layer structure comprises one or more graphene layers.
[0023] A plasma-etchable layer structure can be etched during a typical plasma etching step in electronic device manufacturing to remove the layer structure without removing the underlying substrate. Plasma etching is described in more detail herein. In the present invention, the plasma-etchable layer structure comprises one or more graphene layers and preferably consists of them. Preferably, at least the topmost layer of the plasma-etchable layer structure is a graphene layer, thereby ensuring that at least the topmost graphene layer is etched during plasma etching to form an exposed edge surface.
[0024] Preferably, the plasma-etchable layered structure consists of one or more layers of 2D material. 2D materials are widely known in the art and are sometimes referred to as single-layer materials consisting of a single layer of atoms, but materials generally known as transition metal dichalcogenides, including layers of metal atoms interposed between layers of chalcogen atoms (i.e., MX2-type compounds composed of three atomic planes), are also widely known 2D materials. Likewise, graphane (CH) n and graphene oxide are 2D materials, graphene has terminal hydrogen atoms, and graphene oxide has cross-linked oxygen atoms and terminal hydroxyl groups. Silicene is not perfectly flat and is puckered. In all cases, 2D materials can be viewed as sheets or layers of quasi-infinite size in two dimensions and may include, for example, graphene, graphyne, silicene, germanene, borophene, phosphorene, antimonene, hexagonal boron nitride (h-BN), borocarbonitrides, and TMDCs (e.g., MoS2, WS2, MoSe2, WSe2, and MoTe2). Accordingly, in some embodiments, the plasma-etchable layer structure comprises one or more layers of graphene and one or more layers of silicene, germanene, h-BN, boropene, and / or TMDC. In such embodiments, the plasma-etchable layer structure may be referred to as a heterostructure. Much more preferably, the plasma-etchable layer structure comprises one or more layers of graphene, which may be referred to as a graphene layer structure.
[0025] The present invention provides at least one ohmic contact in direct contact with the exposed edge surface of at least one graphene layer of a plasma-etchable layer structure. The plasma-etchable layer structure comprises graphene, and optionally silicene, germanene, boropene, h-BN, and / or TMDC. Accordingly, any reference to graphene in this specification applies equally to other 2D materials unless otherwise specified in the context.
[0026] The layer structure may comprise 1 to 10 individual 2D material layers, at least one of which is a graphene layer. For example, a plasma-etchable layer structure consists of a graphene monolayer. When the layer structure comprises multiple 2D material layers, 2 to 5 layers are preferred, and 2 or 3 layers are much more preferred. Nevertheless, a single layer is also preferred because some of the inherent properties attributable to 2D materials are most pronounced when provided as a monolayer. For example, monolayer graphene is a zero-bandgap semiconductor (i.e., a semi-metal), where the density of states at the Fermi level is zero and lies at the point where the top of the valence band meets the bottom of the conduction band (forming a Dirac cone). Due to the low density of states near the Dirac point, shifts in the Fermi level are particularly sensitive to charge transfer into this pristine graphene. Electronic structures also generate, for example, the quantum Hall effect. Therefore, for certain embodiments, particularly for the Hall sensor configurations described herein, a single layer of graphene is particularly preferred and derives the greatest benefit from the invention. Nevertheless, bilayer or multilayer graphene (so-called graphene layer structures) may be used.
[0027] In the first step of the method, providing a plasma-etchable layer structure of graphene can be achieved by any method known in the art. However, since the plasma-etchable layer structure containing graphene is synthesized directly on the surface of the substrate, it does not involve any physical transfer steps. Preferably, the graphene and any other 2D material layers are formed by CVD or MOCVD growth. It is particularly preferable that the graphene be formed by VPE or MOCVD. MOCVD is a term used to describe a system used in a specific method for depositing layers on a substrate. While the initials stand for metal-organic chemical vapor deposition, MOCVD is a term in the art and is understood to relate to a general process and the apparatus used therefor, and is not necessarily considered to be limited to the use of metal-organic reactants or the manufacture of metal-organic materials, but simply requires the use of a carbon-containing precursor when forming graphene. Instead, the use of these terms indicates a general set of process and device characteristics to a person skilled in the art. MOCVD is further distinguished from CVD technologies due to system complexity and precision. While CVD technologies allow reactions to be carried out with simple stoichiometry and structures, MOCVD allows for the generation of difficult stoichiometry and structures. MOCVD systems are distinguished from CVD systems by at least gas distribution systems, heating and temperature control systems, and chemical control systems. Typically, MOCVD systems cost at least 10 times more than typical CVD systems. MOCVD is particularly desirable for achieving high-quality graphene layer structures.
[0028] MOCVD can also be easily distinguished from atomic layer deposition (ALD) techniques. ALD relies on stepwise reactions of reagents, along with intermediate washing steps used to remove undesirable byproducts and / or excess reagents. It does not rely on the decomposition or dissociation of reagents in the gaseous phase. This is not particularly suitable for the use of reagents with low vapor pressures, such as silanes, which take an excessive amount of time to remove from the reaction chamber. MOCVD growth of graphene is discussed in WO 2017 / 029470, which includes by reference and provides a preferred method.
[0029] The method of WO 2017 / 029470 provides a chamber having a plurality of cooling inlets, wherein, in use, the inlets are arranged to be distributed across the substrate and uniformly separated from the substrate. A flow containing a precursor compound can be provided as a horizontal laminar flow or substantially vertically. Inlets suitable for such reactors are widely known and include Planetary and Showerhead® reactors available from Aixtron®. Other suitable growth chambers include Turbodisc K-series or Propel® MOCVD systems available from Veeco® Instruments Inc.
[0030] Accordingly, in a particularly preferred embodiment, the step of providing a plasma-etchable layer structure on a plasma-resistant substrate is a step of forming a graphene layer structure,
[0031] A step of providing a plasma-resistant substrate on a heated susceptor within a reaction chamber - the chamber has a plurality of cooling inlets, and when in use, the inlets are arranged to be distributed across the substrate and uniformly separated from the substrate -,
[0032] A step of supplying a flow containing a precursor compound into a reaction chamber through inlets to decompose the precursor compound and form graphene on a substrate.
[0033] It includes, wherein the inlets are cooled to less than 100°C, preferably 50°C to 60°C, and the susceptor is heated to a temperature of at least 50°C, which exceeds the decomposition temperature of the precursor.
[0034] This method allows for the production of highly high-quality raw graphene that is scalable for the fabrication of arrays of electronic device precursors and for large-area substrates. As described herein, this raw graphene is advantageous for use in Hall sensor applications due to the resulting quantum Hall effect arising from the intrinsic electronic structure of the raw graphene.
[0035] As described herein, sapphire and silicon are preferred substrates, particularly for graphene prepared by the method of WO 2017 / 029470. As is understandable, silicon substrates may include CMOS substrates, which are silicon-based substrates that allow graphene to be deposited on a silicon surface, but CMOS substrates may include various additional layers or circuits embedded therein. Sapphire is a particularly preferred substrate. R-plane sapphire is most preferred. As is known in the art, the r-plane refers to the crystallographic orientation of the surface of the substrate (i.e., the surface on which graphene is deposited). Such substrates are particularly suitable for providing high-quality graphene, most notably sensors such as Hall effect sensors as described herein. Partially, this is due to the influence of the substrate on the resulting charge carrier density of the graphene deposited thereon. The inventors have found that r-plane sapphire provides a particularly low charge carrier density to the graphene. Preferably, the charge carrier density of one or more graphene layers is 10 12 cm -2Less than, preferably 8×10 11 cm -2 It is less than. For example, when using r-plane sapphire, 6×10 11 cm -2 Less than, preferably 5×10 11 cm -2 A charge carrier density of less than 100% can be obtained.
[0036] The 2D material of the plasma-etchable layer structure may be a doped 2D material. As merely an example, if the 2D material is graphene and is doped, the graphene is preferably doped with one or more elements selected from the group consisting of silicon, magnesium, zinc, arsenic, oxygen, boron, bromine, and nitrogen. Likewise, the method may next preferably include the step of introducing a doping element into a reaction chamber and selecting the temperature of the substrate, the pressure of the reaction chamber, and the gas flow rate to produce doped graphene. Preferably, the precursor for doped graphene growth comprises the doping element. Alternatively, one or more additional precursors comprising a species (e.g., carbon for graphene growth and silicon for silicine growth) and the doping element are introduced into the substrate within the reaction chamber; the second precursor is a gas or is suspended in the gas to produce doped graphene. The deposition of the plasma-resistant dielectric itself may result in the doping of the 2D material. Therefore, the provision of doped 2D materials can be used to compensate for any doping effects from dielectric patterning.
[0037] A plasma-etchable layer structure is provided on a plasma-resistant substrate. That is, the layer structure is directly on the substrate without an intermediate layer. The layer structure, composed of 2D material layers, provides two opposing surfaces to the layer structure, and the first or bottom surface is the surface in direct contact with the substrate. Thus, the second or top surface is exposed, and preferably, at least this layer is a graphene layer.
[0038] Plasma-resistant substrates are well known in the art. Ceramic materials such as silicon carbide, silicon nitride, and silicon oxide are particularly plasma-resistant. Standard crystalline silicon wafers can be considered as ceramics and are plasma-resistant. Crystalline III-V semiconductors are also plasma-resistant and may be desirable as substrates for certain applications such as LEDs. In a preferred embodiment, the plasma-resistant substrate is sapphire, silicon, silicon dioxide, silicon nitride, silicon carbide, germanium, or III-V semiconductor, much more preferably sapphire or silicon.
[0039] In a preferred embodiment, the etching speed of the layer structure and the substrate is at least 10 times, preferably 10 2 Pear, much more preferably 10 3 There is a difference of several times. Therefore, regardless of the specific resistivity of the substrate for a given plasma treatment, the layer structure is etched significantly faster than the substrate, resulting in complete etching of the exposed layer structure and negligible loss of the substrate surface over the time required for plasma etching.
[0040] Preferably, the plasma-etchable layer structure has an etching rate greater than 0.345 nm per minute. The plasma etching rate can be measured using oxygen plasma etching with 40 W power and an O2 flow of 6 sccm. Thus, a single graphene monolayer (having an ideal thickness of 0.345 nm) will be etched within 1 minute under these conditions. Preferably, the etching rate is greater than 0.5 nm per minute. Therefore, the plasma-resistant substrate can preferably have an etching rate of less than 0.1 nm per minute, preferably less than 0.01 nm per minute.
[0041] The method further comprises the step of patterning a plasma-resistant dielectric on an exposed top surface to form an intermediate having at least one covered region and at least one uncovered region of a layer structure. As described herein in relation to the plasma-resistant substrate, the plasma-resistant dielectric may be any known in the art, and its plasma resistivity is measured by the same parameters (i.e., layer structure and / or etching rate). Typically, this will be an inorganic dielectric such as a ceramic (i.e., one that does not contain carbon-hydrogen bonds). Ceramics may be considered as inorganic oxides, nitrides, carbides, fluorides, or sulfides, and often have a crystalline structure. In a preferred embodiment, the plasma-resistant dielectric is an inorganic oxide, nitride, carbide, fluoride, or sulfide, and preferably is one of alumina (aluminum oxide), silica (silicon dioxide), or silicon nitride.
[0042] Inorganic dielectrics, particularly ceramic dielectrics, are particularly desirable because they provide significantly improved barrier properties compared to organic dielectric materials such as PMMA. Therefore, the dielectric layer can be retained on the final electronic device precursor to provide protection for the layer structure from contamination by atmospheric contaminants, particularly oxygen and water vapor. Such air and moisture-resistant coatings provide a barrier against unintended doping over a significantly longer period, which leads to improved device lifespan. Additionally, inorganic materials such as ceramics can withstand operation at very high temperatures as well as a wide range of temperature fluctuations, and in other cases, allow the electronic device to be used under more extreme conditions without the risk of damage to the layer structure and ultimate contamination, which could eventually lead to drift in device performance (requiring recalibration or simply causing device failure).
[0043] A plasma-resistant dielectric is patterned on the exposed top surface of a plasma-etchable layer structure. That is, the plasma-resistant dielectric is deposited and patterned simultaneously on the exposed top surface of the plasma-etchable layer structure. As described herein, this is particularly preferably achieved by physical vapor deposition (PVD). PVD is a widely known technique. The patterning causes the formation of a dielectric over a portion of the surface, thereby forming one or more covered regions and one or more uncovered regions of the layer structure (providing an intermediate in the manufacture of a device precursor). In a preferred embodiment, the method comprises the step of forming an array of covered regions, each corresponding to an electronic device precursor. Such patterning for forming an array of covered regions may include forming a dielectric in a plurality of regions using a mask (i.e., a shadow mask). The formation of at least one covered region causes the uncovered regions to become the remainder of the layer structure. Accordingly, when an array of covered regions is patterned on a layer structure, this typically provides at least one continuous uncovered region separating the covered regions. In a preferred embodiment, only one uncovered region is formed during the patterning step because the plasma etching step as described herein subsequently causes the formation of a continuous outer edge surface of the layer structure for each electronic device precursor (i.e., the formation of a "filled" "2D shape" having an outer edge). However, in some embodiments, the 2D shape and the patterned dielectric may have an uncovered portion inside that provides an inner and outer edge for the graphene layer after etching.
[0044] Accordingly, in a preferred embodiment, the patterning step comprises forming one or more rectangular shaped regions of the plasma resistive dielectric. Patterning the dielectric, and subsequently the 2D material in this way, implies that the electronic device precursor is particularly desirable for forming a transistor. Next, the electronic device precursor may preferably further include a third contact, i.e., a gate contact. The gate contact may be provided, for example, as a so-called "front gate" on the top of the plasma resistive dielectric or coating (if present), or alternatively as a so-called "back gate" on the bottom of the substrate. When provided on the bottom of the substrate, the 2D material is provided on an insulating region of the substrate surface. Silicon substrates (and silicon nitride equivalents) having SiO2, SiO2 / Si, and "buried" SiO2 regions are exemplary substrates that can be used to manufacture the transistor of the present invention. Alternatively, in a preferred embodiment, the patterning step comprises forming one or more regions, preferably cross-shaped regions, having "Hall-bar" and / or "van der Pauw" geometries of the plasma-resistant dielectric (such geometries or shapes are widely known in the art and include, for example, circles, "clover leaves," squares, rectangles, and cross shapes). Such geometries are widely known in the art for Hall sensors (requiring at least four contacts), and since the cross shape is the most preferred geometry, the electronic device precursor is preferably intended to form a Hall sensor.
[0045] In embodiments comprising forming an array of covered regions, the method preferably further comprises the step of dicing the substrate to separate electronic device precursors from the array. Thus, a plurality of electronic device precursors can be manufactured simultaneously on a single substrate and subsequently diced for individual use. This dicing step is preferably performed near the end of the process.
[0046] In a preferred embodiment of the present invention, the patterning step comprises patterning a plasma-resistant dielectric by physical vapor deposition, such as e-beam evaporation or thermal evaporation. Preferably, e-beam evaporation is used to pattern the plasma-resistant dielectric, and preferably, this is performed using a mask (i.e., a shadow mask). This method is particularly suitable for the deposition of an alumina or silica plasma-resistant dielectric layer on 2D material layers.
[0047] Preferably, the thickness of the patterned dielectric is less than 200 nm, preferably less than 100 nm, more preferably less than 50 nm and / or greater than 1 nm, preferably greater than 3 nm, more preferably greater than 5 nm. Accordingly, the dielectric layer may have a thickness of 1 nm to 200 nm, preferably 3 nm to 100 nm, and much more preferably 5 nm to 50 nm.
[0048] The method further comprises the step of plasma etching an intermediate, thereby etching away at least one uncovered region of the layer structure to form at least one covered region of the layer structure having an exposed edge surface. The plasma etching step results in the etching of all uncovered regions of the plasma-etchable layer structure, thereby exposing the underlying substrate in these regions. The plasma-resistive dielectric prevents etching of the layer structure in the covered regions, and thus the plasma etching results in the formation of an exposed edge of the layer structure that is coterminous with the shape of the patterned dielectric over it. Thus, as described herein, the 2D material layers extend across (and down) the covered regions of the layer structure to the exposed edge surface. Thus, the shape or pattern of the dielectric defines the shape of the etched 2D material layer.
[0049] Plasma etching is a typical process used in the manufacture of electronic devices and integrated circuits. Plasma etching involves a plasma flow of a suitable gas mixture across a substrate, and the plasma is typically formed from the application of RF across two electrodes under low pressure. In oxygen plasma etching, RF radiation ionizes the gas to form oxygen radicals that etch the layer structure. By-products, also known in the art as "ash," are removed by a pump, which consists mainly of carbon monoxide and carbon dioxide, when the graphene layer structure is etched by oxygen plasma etching. In a preferred embodiment, plasma etching involves oxygen plasma etching. In a preferred embodiment, oxygen plasma etching involves using RF power of at least 5 W, preferably at least 10 W, more preferably at least 20 W, and preferably less than 200 W, preferably less than 100 W. The flow rate of O2 may be at least 1 sccm, preferably at least 3 sccm and / or less than 50 sccm, preferably less than 30 sccm. Preferably, the chamber pressure is at least 0.1 mbar and / or up to 100 mbar, preferably at least 0.2 mbar and / or up to 10 mbar. Accordingly, the time required for plasma etching may be at least 1 second and / or up to 5 minutes. Preferably, the required time is at least 10 seconds and / or less than 2 minutes.
[0050] Finally, the method of the present invention further comprises the step of forming an ohmic contact (i.e., at least one ohmic contact) that is in direct contact with a portion of the exposed edge surface. Additional contacts may also be formed and may be formed simultaneously. In this case, additional contacts that are in direct contact with the exposed edge surface but separated from any other contacts are also provided (i.e., the contacts do not contact each other). Preferably, one or more ohmic contacts are metal contacts comprising one or more of titanium, aluminum, chromium, and gold. Preferably, the contacts are titanium and / or gold metal contacts. The contacts may preferably be formed by any standard technique, such as electron beam deposition, using a mask.
[0051] The inventors discovered that the dielectric layer not only protects the underlying 2D material from atmospheric contamination but also prevents contacts from forming on the surface of the 2D material. Therefore, since contacts are formed only at exposed edges, the 2D material is substantially protected from metal doping, and improved contact between the ohmic contact and the graphene can be achieved by avoiding wet lithography techniques, including avoiding etchants such as BOE. Furthermore, the inventors discovered that charge injection at the edges of the 2D material is consequently significantly more efficient.
[0052] Although a protective dielectric layer serves to limit contamination of the graphene surface and is nevertheless highly effective, particularly over long periods, the inventors have discovered that exposed edges can provide pathways for contamination and doping of the 2D material over time. While this process is significantly slower than surface doping and may occur only to a limited extent, the inventors have found that stability and lifetime can be further improved by providing an additional protective layer or coating layer that is air (and moisture) resistant. As described herein for devices such as Hall sensors, the functionality of devices based on 2D materials can be highly sensitive to any changes in charge carrier density (i.e., caused by doping by contaminants, primarily oxygen and water vapor, which are atmospheric contaminants). The inventors have found that devices based on shapes with many edges, such as the cross shape of a Hall sensor, are susceptible to contamination and thus benefit greatly from additional coatings. Consequently, the method provides devices that are more robust than those of the prior art.
[0053] Accordingly, the method described herein preferably further comprises the step of forming a coating layer to provide a continuous air-resistant coating on a layer structure (and its patterned dielectric) before or after forming one or more ohmic contacts. Thus, the continuous air-resistant coating coats at least adjacent regions of the layer structure (including etched 2D material layers and a patterned dielectric) and the substrate, surrounding the layer structure and protecting all remaining portions of the exposed edges (i.e., all edges that do not come into direct contact with the ohmic contacts). As described herein, the coating layer may be patterned to leave a portion of the exposed contacts for connection to the circuit. Alternatively, the coating layer may be formed across the substrate to coat the entire substrate, all of the layer structure (and edges), and all of one or more contacts.
[0054] Air-resistant coatings can be referred to as hermetic coatings. The coating is 10 -1 Less than ㎤ / ㎡ / day / atm, preferably 10 -3 Less than ㎤ / ㎡ / day / atm, more preferably 10 -5 It can be characterized by an oxygen permeability of less than ㎤ / m² / day / atm. The air-resistant coating is also 10 -2 Less than g / ㎡ / day, preferably 10 -4 Less than g / ㎡ / day, more preferably 10 -5 It can be characterized by a water vapor transmittance of less than g / m² / day. Such transmittances are generally recognized in the art as necessary for use in electronic devices such as LEDs, where more desirable transmittances are required for OLEDs and Hall sensors.
[0055] The inventors have also discovered that the use of plasma etching to etch a layer structure in uncoated area(s) is particularly advantageous when combined with an additional coating layer. This is because the plasma etching step does not cause deposits to form on the layer structure or substrate, and does not affect the substrate surface roughness (e.g., pitting) that may be caused by alternative techniques such as laser etching. This ultimately leads to a significant improvement in the properties of the coating layer.
[0056] Preferably, the coating layer is an inorganic oxide, nitride, carbide, fluoride, or sulfide, and preferably alumina or silica. Preferably, the thickness of the coating layer is greater than 10 nm, preferably greater than 25 nm, and more preferably greater than 50 nm. Although there is no specific upper limit, a thickness greater than 10 µm or greater than 1 µm simply increases the weight and thickness of the device precursor, while providing only limited additional protective properties. Additionally, for example, deposition rates by ALD can be slow processes, and thicker coatings can make manufacturing times excessively long. Therefore, an ALD layer thickness of up to 500 nm, preferably up to 100 nm, is also desirable.
[0057] The inventors have discovered different solutions to various problems faced during the manufacture of such electronic device precursors including a coating layer, and each solution, such as the one described herein, has its own advantages and disadvantages.
[0058] A preferred embodiment of the present invention includes the step of forming a coating layer after an ohmic contact, so that the ohmic contact is formed on a plasma-resistant substrate. In this embodiment, the coating layer is formed by atomic layer deposition (ALD) across the plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure, the ohmic contact, and the remaining exposed edge surface.
[0059] ALD is a technique known in the art and involves the reaction of at least two precursors in a sequential and self-limiting manner. Repeated cycles for distinct precursors allow for the growth of a thin film in a shape-following manner (i.e., uniform thickness across the entire substrate) due to a layer-by-layer growth mechanism. Alumina is a particularly preferred coating material and can be formed by sequentially exposing trimethylaluminum (TMA) and an oxygen source, preferably water (H2O), O2, and ozone (O3), preferably water. ALD is particularly advantageous because the coating can be reliably formed across the entire substrate (i.e., providing a shape-following coating). However, the inventors have also discovered that while an excellent protective coating layer can be formed by ALD, the entire coating may cause dicing problems when an array of electronic device precursors is fabricated on the substrate. Next, dicing (or cutting) necessarily involves dicing through a coating layer to separate individual device precursors, and this process can easily introduce microcracks into the coating layer.
[0060] This coating layer also coats the entire contact to seal the contact. Nevertheless, the inventors have discovered that wire bonding can be used to penetrate the coating layer to attach a wire to the contact. Accordingly, the method preferably includes the step of wire bonding to the ohmic contacts of the device precursor through the coating layer. Although ALD provides a very uniform protective coating, the coating may be damaged if a hole is drilled to make a wire bond contact.
[0061] Accordingly, the inventors have developed another preferred embodiment in which an ohmic contact is formed before coating and thus formed on a plasma-resistant substrate, but the coating layer is formed by patterning the coating layer on the plasma-resistant substrate, thereby providing a continuous air-resistant coating on at least one covered area of the layer structure and the remaining exposed edge surface.
[0062] The coating layer is preferably patterned using the same technique described herein with respect to dielectric patterning. One difference is that the pattern is geometrically larger, so as to cover the exposed edges of the layer structure and thus cover part of the contact as well as adjacent parts of the substrate, thereby leaving part of the contact exposed. For example, the patterning of the alumina can be performed again using e-beam evaporation.
[0063] Accordingly, this embodiment is advantageous because parts of the substrate (or simply parts of the substrate) between adjacent layer structures of the array remain exposed (which may be referred to as "streets" or "die streets"). Thus, the substrate can be diced without the risk of damaging the coating layer. Additionally, since the contacts remain exposed, the contacts can be wire-bonded without any risk of damage or cracking of the coating layer, or alternatively, solder bumps can be deposited on the contacts.
[0064] Unlike using ALD to provide a shape-following coating across the entire substrate, evaporation is less shape-following and carries the risk of edges remaining exposed. In particular, e-beam evaporation is directional in that shadows, especially those generated by contacts, limit the uniform growth of the coating. However, it is known in the art to rotate the substrate during coating to minimize this effect.
[0065] Further preferred embodiments include, instead, providing a coating layer before forming contacts and selectively etching away one or more portions of the coating layer to expose corresponding portions of the edge surface. Next, the step of forming contacts includes forming ohmic contacts that are in direct contact with each exposed portion of the edge surface.
[0066] Accordingly, the coating layer can be provided by ALD or e-beam evaporation. Since this embodiment involves forming a coating before any ohmic contacts, a better coating can be achieved with e-beam evaporation, thereby allowing the streets to remain clean. The inventors found that the coating needs to be etched in selective portions to expose corresponding portions of the underlying edge surface to allow for the formation of ohmic contacts. Selective etching is preferably performed using laser etching, reactive ion etching (in so-called "dry etching"), chemical etching (in so-called "wet etching"), and / or photolithography. Since the 2D material is substantially protected from contamination, such methods can be used without serious adverse effects. Nevertheless, laser etching and reactive ion etching are preferred because they are "dry" methods with a reduced risk of doping the 2D material, and reactive ion etching is the most preferred. In some embodiments, selective etching may be performed for a sufficient time to etch and remove the coating layer to expose the corresponding edge surface of the plasma-etchable layer structure.
[0067] Next, this method requires the formation of ohmic contacts that are in direct contact with the edge surfaces exposed by selective etching at each etched portion. Thus, there is an advantage in that the contacts are exposed for connection to an electronic circuit. In particular, the method may further include the step of depositing solder bumps (or solder balls) on the ohmic contacts. This allows the electronic device precursor to be used as a so-called "flip chip." Nevertheless, wire bonding is also preferred. Wire bonding is known in the art and may involve ball bonding, wedge bonding, or compliant bonding.
[0068] However, the inventors found that this embodiment introduces additional complexity to the alignment required for selective etching and contact deposition within the selectively etched portion. Nevertheless, etching also carries the risk of forming cracks in the coating.
[0069] In a second aspect of the present invention, as an electronic device precursor,
[0070] A substrate having a layer structure on top of it - the layer structure is:
[0071] A lower layer on a first region of a substrate - the lower layer comprises one or more graphene layers extending across the lower layer -,
[0072] An upper layer located on a lower layer and formed of a dielectric material
[0073] Includes, and the lower layer and the upper layer share a continuous outer edge surface -;
[0074] An ohmic contact provided on an additional area of the substrate and in direct contact with one or more graphene layers through a continuous outer edge surface; and
[0075] A continuous air-resistant coating layer across a substrate, a layer structure, and at least one ohmic contact
[0076] An electronic device precursor including is provided.
[0077] In a third aspect of the present invention, as an electronic device precursor,
[0078] A substrate having a layer structure on top of it - the layer structure is:
[0079] A lower layer on a first region of a substrate - the lower layer comprises one or more graphene layers extending across the lower layer -,
[0080] An upper layer located on a lower layer and formed of a dielectric material
[0081] Includes, and the lower layer and the upper layer share a continuous outer edge surface -;
[0082] An ohmic contact provided on an additional area of the substrate and in direct contact with one or more graphene layers through a continuous outer edge surface; and
[0083] A continuous air-resistant coating layer surrounding the layered structure
[0084] Provides an electronic device precursor including
[0085] In the fourth aspect of the present invention, as an electronic device precursor,
[0086] A substrate having a layer structure on top of it - the layer structure is:
[0087] A lower layer on a first region of a substrate - the lower layer comprises one or more graphene layers extending across the lower layer -,
[0088] An upper layer located on a lower layer and formed of a dielectric material
[0089] Includes, and the lower layer and the upper layer share a continuous outer edge surface -;
[0090] An ohmic contact in direct contact with one or more graphene layers through a continuous outer edge surface; and
[0091] A continuous air-resistant coating layer surrounding the layered structure
[0092] Provides an electronic device precursor including
[0093] The electronic device precursors of the additional embodiments of the present invention disclosed herein are preferably obtainable by the methods described herein. Accordingly, all features described in relation to the first embodiment can be appropriately applied equally to the additional embodiments of the present invention.
[0094] Consequently, electronic device precursors of additional embodiments of the present invention share the feature of a layered structure comprising a lower layer comprising one or more graphene layers and an upper layer formed of a dielectric material, wherein the lower layer and the upper layer share a continuous outer edge surface. Thus, this provides excellent protection of the graphene from atmospheric contamination, which leads to an extension of the device lifespan and improved stability of device performance over a long period.
[0095] Additionally, ohmic contacts are provided for connection with electronic circuits, and the ohmic contacts make direct contact only with the edges of the graphene layer rather than the upper (or lower) planar surface. Edge contacts provide improved charge injection compared to surface contacts and substantially prevent doping of the graphene. This is particularly useful when the device precursor is intended to be used at high temperatures, where increased temperatures can lead to doping of the 2D material, for example by the metal of the ohmic contacts, after fabrication and during subsequent use.
[0096] In a preferred embodiment of the present invention, the electronic device precursor is for a transistor or a Hall sensor, most preferably for a Hall sensor. Nevertheless, a number of other electronic devices may be manufactured using the method described herein and / or from the electronic device precursor described herein, and include capacitors, diodes, and inductors.
[0097] In a particularly preferred embodiment of the present invention, the method described herein is:
[0098] (i) providing a plasma-etchable layer structure on a plasma-resistant substrate - the layer structure has an exposed top surface -;
[0099] (ii) patterning a plasma-resistant dielectric on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a layer structure;
[0100] (iii) a step of plasma etching the intermediate—thereby etching away at least one uncovered region of the layer structure to form at least one covered region of the layer structure having an exposed edge surface—;
[0101] (iv) forming an ohmic contact by directly contacting a portion of the exposed edge surface on a plasma-resistant substrate; and
[0102] (v) A step of forming a coating layer by ALD across a plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure, an ohmic contact, and the remaining exposed edge surface.
[0103] A plasma-etchable layer structure comprising, wherein, one or more graphene layers extending across the covered regions of the layer structure to an exposed edge surface, or composed thereof. Accordingly, the electronic device precursor of the second embodiment described herein is preferably obtainable by this method, and much more preferably obtained.
[0104] A device precursor of the second embodiment comprises a substrate, a layer structure, and a continuous air-resistant coating layer across at least one ohmic contact, which may also be considered to surround a layer structure according to the third and fourth embodiments disclosed herein.
[0105] In a particularly preferred embodiment of the present invention, the method described herein is:
[0106] (i) providing a plasma-etchable layer structure on a plasma-resistant substrate - the layer structure has an exposed top surface -;
[0107] (ii) patterning a plasma-resistant dielectric on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a layer structure;
[0108] (iii) a step of plasma etching the intermediate—thereby etching away at least one uncovered region of the layer structure to form at least one covered region of the layer structure having an exposed edge surface—;
[0109] (iv) forming an ohmic contact by directly contacting a portion of the exposed edge surface on a plasma-resistant substrate; and
[0110] (v) patterning a coating layer on a plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure and the remaining exposed edge surface.
[0111] A plasma-etchable layer structure comprising, wherein, one or more graphene layers extending across the covered regions of the layer structure to an exposed edge surface, or composed thereof. Accordingly, the electronic device precursors of the third and fourth embodiments described herein are preferably obtainable by this method, and much more preferably obtained.
[0112] In a particularly preferred embodiment of the present invention, the method described herein is:
[0113] (i) providing a plasma-etchable layer structure on a plasma-resistant substrate - the layer structure has an exposed top surface -;
[0114] (ii) patterning a plasma-resistant dielectric on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a layer structure;
[0115] (iii) a step of plasma etching the intermediate—thereby etching away at least one uncovered region of the layer structure to form at least one covered region of the layer structure having an exposed edge surface—;
[0116] (iv) forming a coating layer on a plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure and on the exposed edge surface.
[0117] (v) a step of selectively etching away one or more portions of the coating layer to expose corresponding portions of the edge surface; and
[0118] (vi) A step of forming an ohmic contact that is in direct contact with each exposed portion of the edge surface
[0119] A plasma-etchable layer structure comprising, wherein, one or more graphene layers extending across the covered regions of the layer structure to an exposed edge surface, or composed thereof. Accordingly, the electronic device precursor of the fourth embodiment described herein is preferably obtainable by this method, and much more preferably obtained.
[0120] In a much more preferred embodiment of the present invention, the method described herein is:
[0121] (i) a step of providing a graphene monolayer on a sapphire substrate by MOCVD - the graphene monolayer has an exposed top surface -;
[0122] (ii) patterning alumina as one or more cross-shaped regions on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a graphene monolayer;
[0123] (iii) a step of etching the intermediate with oxygen plasma—thereby etching away at least one uncovered region of the graphene monolayer to form at least one covered region of the graphene monolayer having an exposed edge surface—;
[0124] (iv) a step of forming four gold ohmic contacts in each cross-shaped region formed in step (ii) on a sapphire substrate - each contact is in direct contact with the distal portion of the exposed edge surface of the four arms of the cross -;
[0125] (v) forming an alumina coating layer by ALD across a sapphire substrate to provide a continuous air-resistant coating on at least one covered region of the monolayer graphene, ohmic contacts, and the remaining exposed edge surfaces.
[0126] It includes, and the graphene monolayer extends across at least one covered area to an exposed edge surface, and the electronic device precursor is intended to form a Hall sensor.
[0127] Therefore, a desirable electronic device precursor is for a Hall sensor, and
[0128] A sapphire substrate having a layer structure on top of it - the layer structure is:
[0129] A graphene monolayer on a first region of a sapphire substrate, and
[0130] Alumina layer on a graphene monolayer
[0131] Includes, and graphene and alumina have a cross-shaped structure and share a continuous outer edge surface -;
[0132] Four gold ohmic contacts - each contact is provided on an additional area of the sapphire substrate and makes direct contact with the distal portion of the exposed edge surface of each of the four cross-shaped arms -; and
[0133] A continuous alumina coating layer across the sapphire substrate, layer structure, and contacts
[0134] Includes
[0135] In another much more preferred embodiment of the present invention, the method described herein is:
[0136] (i) a step of providing a graphene monolayer on a sapphire substrate by MOCVD - the graphene monolayer has an exposed top surface -;
[0137] (ii) patterning alumina as one or more cross-shaped regions on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a graphene monolayer;
[0138] (iii) a step of etching the intermediate with oxygen plasma—thereby etching away at least one uncovered region of the graphene monolayer to form at least one covered region of the graphene monolayer having an exposed edge surface—;
[0139] (iv) a step of forming four gold ohmic contacts in each cross-shaped region formed in step (ii) on a sapphire substrate - each contact is in direct contact with the distal portion of the exposed edge surface of each of the four arms of the cross -;
[0140] (v) patterning an alumina coating layer by e-beam evaporation on a sapphire substrate to provide a continuous air-resistant coating on at least one covered region of the monolayer graphene and the remaining exposed edge surfaces.
[0141] It includes, and the graphene monolayer extends across at least one covered area to an exposed edge surface, and the electronic device precursor is intended to form a Hall sensor.
[0142] Likewise, in another much more preferred embodiment of the present invention, the method described herein is:
[0143] (i) a step of providing a graphene monolayer on a sapphire substrate by MOCVD - the graphene monolayer has an exposed top surface -;
[0144] (ii) patterning alumina as one or more cross-shaped regions on an exposed upper surface to form an intermediate having at least one covered region and at least one uncovered region of a graphene monolayer;
[0145] (iii) a step of etching the intermediate with oxygen plasma—thereby etching away at least one uncovered region of the graphene monolayer to form at least one covered region of the graphene monolayer having an exposed edge surface—;
[0146] (iv) forming an alumina coating layer on a sapphire substrate to provide a continuous air-resistant coating on at least one covered region of the monolayer graphene and on the exposed edge surface.
[0147] (v) a step of selectively laser-etching four portions of an alumina coating layer to expose corresponding portions of the edge surface of a graphene monolayer to expose the distal portions of the edge surface of each of the four cross-shaped arms; and
[0148] (vi) A step of forming four gold ohmic contacts in direct contact with each of the four exposed portions of the edge surface.
[0149] It includes, and the graphene monolayer extends across at least one covered area to an exposed edge surface, and the electronic device precursor is intended to form a Hall sensor.
[0150] Therefore, a desirable electronic device precursor is for a Hall sensor, and
[0151] A sapphire substrate having a layer structure on top of it - the layer structure is:
[0152] A graphene monolayer on a first region of a sapphire substrate, and
[0153] Alumina layer on a graphene monolayer
[0154] Includes, and graphene and alumina have a cross-shaped structure and share a continuous outer edge surface -;
[0155] Four gold ohmic contacts - each contact is provided on an additional area of the sapphire substrate and makes direct contact with the distal portion of the exposed edge surface of each of the four cross-shaped arms -; and
[0156] A continuous alumina coating layer surrounding the layer structure
[0157] Includes
[0158] Accordingly, a preferred electronic device precursor includes an alumina coating layer that encapsulates a layer structure protecting the edges of a graphene monolayer. The contacts of the device precursor are at least partially exposed, that is, they are not coated by the alumina coating layer, as is the case with a sapphire substrate that is at least partially exposed. Typically, at least, regions of the substrate between adjacent device precursors as part of an array allow for dicing of a common substrate to provide multiple device precursors without the risk of damaging the coating during cutting.
[0159] In embodiments that provide such electronic device precursors by first depositing a coating layer and then etching it to expose the edge surface of graphene, the contact will be exposed vertically due to being deposited within the laser-etched opening in the coating.
[0160] In embodiments where the coating layer is patterned after the formation of contacts, partial coating of the contacts during patterning may leave the top surface of the contacts exposed. However, it is also possible to pattern the coating layer over the top surface of the contacts, and at least the edge surface will remain exposed by the patterning of the coating layer. That is, the contacts are not completely encapsulated by the coating layer of the final electronic device precursor, and thus allow for simple wire bonding or soldering for connection to an electronic circuit without the need to puncture the coating layer. Brief explanation of the drawing
[0161] Hereinafter, the present invention will be further described with reference to the following non-limiting drawings: FIG. 1 is a flowchart illustrating the method of the present invention. FIG. 2 is a cross-sectional view of an electronic device precursor according to an embodiment of the present invention. FIG. 3 is a cross-sectional view of another electronic device precursor according to an embodiment of the present invention. FIG. 4 is a plan view of another electronic device precursor according to an embodiment of the present invention. FIG. 5 is a plan view of another electronic device precursor according to an embodiment of the present invention. FIG. 6 is a perspective view of an array of electronic device precursors according to an embodiment of the present invention. Specific details for implementing the invention
[0162] FIG. 1 is a flowchart illustrating a method (100) of the present invention. The method (100) comprises a plurality of essential steps (105, 110, 115 and 120) and may further comprise one of three optional steps (125a, 125b and 125c) representing three alternative preferred specific embodiments of the method (100).
[0163] The method (100) is for forming an electronic device precursor suitable for a Hall sensor and includes a first step (105) of providing a plasma-etchable layer structure on a plasma-resistant substrate. In the exemplary method (100), the plasma-etchable layer structure consists of a graphene monolayer provided directly on a sapphire substrate by MOCVD.
[0164] Next, an additional step (110) involves patterning array cross-shaped regions of alumina on the exposed upper surface of a graphene monolayer by e-beam evaporation to form an array of intermediates. The method will be further described with reference to one intermediate, but it will be understood that all intermediates of the array are processed simultaneously. Step (115) involves etching the exposed graphene monolayer by etching the intermediates with an oxygen plasma, thereby forming an array of cross-shaped regions of alumina-covered graphene, wherein the alumina-covered graphene has a continuously exposed edge surface.
[0165] The method (100) further includes the step (120) of forming a metal ohmic contact that is in direct contact with a portion of the exposed edge surface of the etched graphene monolayer. In particular, four metal contacts are formed at each end of the cross-shaped "arms".
[0166] In a first specific embodiment of the method (100), the method (100) further comprises a step (125a) performed after step (120), which comprises forming a coating layer of alumina by ALD across a sapphire substrate, thereby coating the alumina-coated graphene, ohmic contacts, and exposed substrate with a continuous air-resistant coating.
[0167] In a second specific embodiment, the method (100) further comprises a step (125b) performed after step (120), which involves coating the alumina-coated graphene into a continuous air-resistant coating by patterning an alumina coating layer on a substrate by e-beam evaporation. Thus, the alumina coating provided by step (125b) protects the exposed edge(s) that do not come into contact with the ohmic contacts from atmospheric contamination, and the pattern of the coating has the same geometric cross shape but is geometrically larger. For example, the maximum width and / or maximum height of the shape may be 10% larger or even 20% larger than the patterned alumina of step (110). The patterning step also leaves a portion of each metal contact exposed for connection to an electronic circuit.
[0168] In a third specific embodiment, the method (100) further comprises a step (125c) of forming a coating layer prior to step (120). Step (125c) involves forming a coating layer to provide a continuous air-resistant coating of alumina on an alumina-coated graphene monolayer (i.e., thereby coating the exposed edge surface). In this embodiment, step (120) further comprises a step of selectively laser-etching four portions of the coating layer at each end of the lower cross-shaped "arms" to expose corresponding portions of the edge surface of the graphene. As required by the method (100), next, step (120) involves forming metal ohmic contacts in direct contact with the exposed edge surface at each of the selectively etched portions.
[0169] FIG. 2 is a cross-sectional view of an electronic device precursor (200). The precursor (200) can be obtained by the method described herein, which involves forming ohmic contacts and then forming a coating layer by ALD.
[0170] The electronic device precursor (200) is formed from a sapphire substrate (205), and thereon thereis a plasma-etchable 2D material layer (210) containing a graphene layer structure. The 2D material layer (210) has a shape defined by an alumina layer (215) formed thereon. Thus, the 2D material layer and the alumina share a continuous edge surface, where the graphene layer structure extends to this edge.
[0171] The precursor (200) further comprises two ohmic contacts (220a and 220b), each of which is in direct contact with the edge of the 2D material layer (210), and thus the graphene layer structure. Since the alumina and the 2D material share a continuous edge surface and have the same shape, there is no contact material on the surface of the 2D material layer (210). Advantageously, the contacts do not result in any notable doping of the 2D material, as can be observed when contacts are provided on the planar surface of the 2D material. Additionally, the edge contacts provide improved charge injection compared to surface charge injection, thereby improving overall efficiency (e.g., by reducing any electrical losses as heat).
[0172] A continuous air-resistant coating layer of silica is formed on the alumina coating (215), contacts (220a and 220b), and substrate (205). The coating (225) provides excellent protection from atmospheric contamination by preventing the ingress of, for example, oxygen gas and water vapor. The precursor (200) further comprises wires (230a and 230b) wire-bonded to the ohmic contacts (220a and 220b), respectively. The wires (230a and 230b) protrude from the coating layer, providing a means for electrical connection to the ohmic contacts.
[0173] The inventors have discovered that the electronic device precursor (200) provides excellent stability to the electronic device. In particular, the inventors have discovered that a device formed with the precursor (200) exhibits a rate of degradation of less than 0.01% / day (when measured for the initial carrier concentration, and thus the sensitivity of the device and the manufacturing point).
[0174] For comparison, a device formed from a precursor, in which a coating layer (e.g., coating layer (215)) is not provided and instead a ceramic cover is provided, is used to "seal" components (as is widely known in the art and may also be used with the present invention), and it was found that the sensitivity of such a device deteriorates at a rate exceeding 0.5% / day. Likewise, the inventors found that the absence of a coating layer or a ceramic cover is significantly much larger.
[0175] For further comparison, the inventors have found that devices formed using an organic PMMA coating layer provide greater protection against degradation compared to known ceramic covers, and these devices have a degradation rate of 0.03% / day to 0.1% / day.
[0176] The inventors also [described] that when metal contacts are deposited on graphene before patterning the dielectric layer, the metal is 10 12 cm -2 Larger and even 10 13 cm -2 It was discovered that higher concentration doping of larger graphene leads to a significant decrease in sensitivity.
[0177] FIG. 3 is a cross-sectional view of an electronic device precursor (300). The precursor (300) can be obtained by the method described herein, which involves forming a coating layer before the step of forming ohmic contacts.
[0178] The electronic device precursor (300) comprises a sapphire substrate (305) and a plasma-etchable 2D material layer (310) thereon. In this embodiment, the 2D material layer is composed of a double-layer graphene (i.e., a graphene monolayer having two graphene layers). A patterned silica layer (315) is formed thereon, sharing a continuous edge surface with the double-layer graphene (310). A continuous air-resistant coating (325) is deposited on the surface of the patterned silica layer (315). The coating (325) is also deposited on an adjacent portion of the surface of the substrate (305). FIG. 3 is a cross-sectional view of the precursor (300), in which the cross-section bisects two ohmic contacts (320) deposited on the substrate (305). In alternative cross-sections, it will be understood that the coating layer (325) will be continuous.
[0179] The contacts (320) are in direct contact with the edge surface of the double-layer graphene as well as with the silica and alumina coatings thereon. The precursor (300) can be obtained by the method described herein, which includes selectively etching a coating layer formed before forming the ohmic contacts. Thus, the contacts extend from the surface of the substrate (305) exposed during the etching process to the surface of the coating layer (325). In this embodiment, solder balls (or solder bumps) (330) are provided on the exposed portion of the ohmic contacts, thereby the precursor (300) can be described as a "flip-chip".
[0180] FIG. 4 is a top view of an electronic device precursor (400). The precursor (400) is suitable for a Hall sensor and is formed as a 2D material layer under an identically formed / patterned alumina layer (415) which is particularly cross-shaped, all of which are formed on a silicon substrate (405). The ends (i.e., distal portions) of each of the four "arms" of the cross-shaped layer structure of the 2D material and the patterned alumina (415) are in direct contact with each of the four titanium contacts (420a, 420b, 420c, and 420d). A continuous air-resistant alumina coating (425) is provided over the layer structure and portions of each of the contacts in a manner sufficient to encapsulate the edges of the underlying 2D material layer and leave portions of each of the titanium contacts exposed. The coating layer (425) may be provided by e-beam evaporation. In FIG. 4, the coating layer (425) is shown translucent to illustrate the presence of the underlying patterned alumina (415). As can be seen, the 2D material layer has the same shape as the alumina layer (415). The precursor (400) is an individual component obtainable by dicing a substrate formed by an array of equivalent precursors sharing a common substrate. The precursor (400) is advantageous in that dicing does not involve cutting through the coating layer (425), because the coating layer does not extend into the so-called "streets," or parts of the substrate between the array of components being manufactured.
[0181] The inventors used Raman spectra obtained at various locations of the device precursor to confirm the presence (and quality) or absence of graphene. Specifically, the method of the present invention facilitates clean etching of graphene up to the edge of the patterned alumina, thereby allowing ohmic contacts to be provided without the need to remove the protective alumina layer. Additionally, the Raman spectra of the graphene demonstrate that the quality of the graphene near the edge can be maintained to be comparable to the quality of the rest of the underlying and protected portions of the graphene (such as at the point labeled (415) for the stack of graphene and patterned alumina in FIG. 4). Furthermore, the inventors used Raman spectroscopy to demonstrate that there is no graphene outside the patterned dielectric between the coating layer and the substrate (such as at the point labeled (425) for the coating layer in FIG. 4).
[0182] FIG. 5 is a top view of an electronic device precursor (500). The precursor (500) is suitable for a Hall sensor and is formed as a 2D material layer under an identically formed / patterned alumina layer (515) which is particularly cross-shaped, all of which are formed on a sapphire substrate. Separate gold contacts (520) are provided to make direct contact with corresponding edge portions of the lower 2D material layer at four distal portions of the cross shape, specifically at the ends of each arm of the cross shape. A continuous air-resistant coating (525) of silica formed by ALD is coated across the entire substrate and the layer structure of the 2D material and alumina (515) (and thus all edges that do not make direct contact with the contacts (520)), together with all the contacts (520) themselves. As shown in FIG. 4, the coating layer (525) is shown as translucent to show the presence of the underlying patterned alumina (515).
[0183] FIG. 6 is a perspective view of an array (600) of electronic device precursors. The array (600) is formed of four electronic device precursors that can be separated by dicing a substrate along streets (635). Each precursor comprises a portion of a substrate (605a, 605b, 605c, and 605d), and a coating layer (625a, 625b, 625c, and 625d) is formed on each portion to encapsulate layer structures of 2D materials and patterned dielectric layers. Additionally, each precursor comprises two ohmic contacts (620a and 620a'), some of which are not encapsulated by the coating layer (625a).
[0184] 예들
[0185] According to the first example:
[0186] 1. Graphene was grown on a sapphire substrate according to the process of WO2017 / 029470.
[0187] 2. Al2O3 was evaporated onto graphene using thermal evaporation through a shadow mask having cross-shaped apertures. The thickness of the evaporated Al2O3 was 10 nm.
[0188] 3. The graphene in the regions where the graphene remained exposed as the top layer was removed by plasma etching. The settings used for this purpose were 40% power (on a 100W device) with an oxygen flow rate of 6 sccm for 30 seconds.
[0189] 4. Ti / Au rod-shaped contacts were evaporated on the ends of the cross arms using a different shadow mask. These were created by evaporating 10 nm of Ti and then evaporating 120 nm of Au. They were positioned relative to the cross arms to contact the edges of the graphene at the ends of the cross arms and to extend laterally from the cross arms.
[0190] 5. A second layer of evaporated Al2O3 was deposited on the first layer in a cross shape larger than the first layer, thereby covering the left portion of the first cross shape and the exposed rod contacts.
[0191] 6. This provided devices on the wafer, which were then processed through standard BEOL processing.
[0192] According to the second example:
[0193] 1. Graphene was grown on a sapphire substrate according to the process of WO2017 / 029470.
[0194] 2. Al2O3 was evaporated onto graphene using thermal evaporation through a shadow mask having cross-shaped apertures. The thickness of the evaporated Al2O3 was 10 nm.
[0195] 3. The graphene in the regions where the graphene remained exposed as the top layer was removed by plasma etching. The settings used for this purpose were 40% power (on a 100W device) with an oxygen flow rate of 6 sccm for 30 seconds.
[0196] 4. Ti / Au rod-shaped contacts were evaporated on the ends of the cross arms using a different shadow mask. These were created by evaporating 10 nm of Ti and then evaporating 120 nm of Au. They were positioned relative to the cross arms to contact the edges of the graphene at the ends of the cross arms and to extend laterally from the cross arms.
[0197] 5. A second layer of Al2O3 was deposited across the entire wafer using ALD. This layer was 65 nm thick.
[0198] 6. This provided devices on the wafer, which were then processed through standard BEOL processing.
[0199] As used herein, the singular forms of "a," "an," and "the" include plural references unless the context clearly indicates otherwise. The use of the term "comprising" is intended to be interpreted as including these features but not excluding other features, and is also intended to include an option of features that are necessarily limited to those described. That is, unless the context clearly indicates otherwise, the term also includes the limitations of "consisting essentially of" (intended to mean that certain additional components may exist so as not to substantially affect the essential nature of the described feature), and "consisting of" (intended to mean that other features may not be included, so that if the components are expressed as percentages according to their proportions, they are summed up to 100% while taking into account any unavoidable impurities).
[0200] It will be understood that while terms such as “first,” “second,” etc., may be used herein to describe various elements, layers, and / or parts, elements, layers, and / or parts should not be limited by these terms. These terms are used solely to distinguish one element, layer, or part from another or additional elements, layers, or parts. It will be understood that the term “on” is intended to mean “directly on,” so as not to have an intermediate layer between one material and another material referred to as being “on” another material. Spatially relative terms such as “below,” “beneath,” “lower,” “above,” “upper,” and similar terms may be used herein for ease of description to explain the relationship of one element or feature to other element(s) or feature(s). It will be understood that spatially relative terms are intended to encompass different orientations of the device during use or operation, in addition to the orientations depicted in the drawings. For example, of the drawings If the device is inverted, elements described as being "below" or "under" other elements or features will be oriented "above" those other elements or features. Accordingly, the exemplary term "below" may encompass both upward and downward orientations. The device may be oriented differently, and spatially relative technical terms used herein are interpreted accordingly.
[0201] The above detailed description is provided for illustrative and illustrative purposes only and is not intended to limit the scope of the appended claims. Many variations of the currently preferred embodiments illustrated herein will be apparent to those skilled in the art and remain within the scope of the appended claims and their equivalents.
Claims
Claim 1 A method for manufacturing an electronic device precursor, comprising: (i) providing a plasma-etchable layer structure on a plasma-resistant substrate, wherein the layer structure has an exposed top surface; (ii) patterning a plasma-resistant dielectric by physical vapor deposition on the exposed top surface to form an intermediate having at least one covered region and at least one uncovered region of the layer structure; (iii) plasma-etching the intermediate, wherein at least one uncovered region of the layer structure is etched away to form at least one covered region of the layer structure having an exposed edge surface; and (iv) forming an ohmic contact in direct contact with a portion of the exposed edge surface, wherein the plasma-etchable layer structure comprises one or more graphene layers extending across the covered regions of the layer structure to the exposed edge surface, and, prior to or after step (iv), the method further comprises (v) forming a coating layer that surrounds the layer structure and protects all remaining portions of the exposed edge surface by providing a continuous air-resistant coating on the covered regions of the layer structure. Claim 2 The method according to claim 1, wherein the plasma-resistant substrate is sapphire, silicon, silicon dioxide, silicon nitride, silicon carbide, germanium, or a III-V semiconductor. Claim 3 A method according to claim 1, wherein at least one of the plasma-resistant dielectric and the coating layer is an inorganic oxide, nitride, carbide, fluoride, or sulfide. Claim 4 A method according to claim 1, wherein the plasma etching comprises oxygen plasma etching. Claim 5 A method according to claim 1, wherein the plasma-etchable layer structure comprises one or more 2D material layers. Claim 6 A method according to claim 5, wherein the plasma-etchable layer structure comprises one or more graphene layers and optionally, at least one layer selected from silicene, germanene, h-BN, borophene, and TMDC. Claim 7 A method according to any one of claims 1 to 6, wherein one or more graphene layers, and, if present, at least one layer selected from silicene, germanene, h-BN, boropene, and TMDC, are each formed by CVD or MOCVD. Claim 8 A method according to claim 1, wherein step (ii) comprises: (i) forming one or more rectangular shaped regions of the plasma resistive dielectric—the electronic device precursor is for forming a transistor—; or (ii) forming one or more cross-shaped regions of the plasma resistive dielectric—the electronic device precursor is for forming a Hall sensor. Claim 9 A method according to claim 1, wherein step (ii) comprises the step of patterning a plasma-resistant dielectric by e-beam evaporation. Claim 10 A method according to any one of claims 1 to 6, 8 and 9, wherein the method comprises the step of forming an array of covered regions corresponding to each electronic device precursor. Claim 11 A method according to claim 1, wherein step (v) is performed after step (iv), and the ohmic contact is formed on the plasma-resistant substrate; and the coating layer is formed by ALD across the plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure, the ohmic contact, and the remaining exposed edge surface. Claim 12 The method of claim 11 further comprises the step of wire-bonding the ohmic contacts of the device precursor through the coating layer. Claim 13 A method according to claim 1, wherein step (v) is performed after step (iv), and the ohmic contact is formed on the plasma-resistant substrate; and the coating layer is formed by patterning a coating layer on the plasma-resistant substrate to provide a continuous air-resistant coating on at least one covered area of the layer structure and the remaining exposed edge surface. Claim 14 In claim 13, the method wherein the coating layer is formed by e-beam evaporation. Claim 15 A method according to claim 1, wherein step (v) is performed prior to step (iv) and includes the step of selectively etching away one or more portions of the coating layer to expose corresponding portions of the edge surface, and step (iv) includes the step of forming an ohmic contact in direct contact with each exposed portion of the edge surface. Claim 16 In paragraph 15, the method wherein selective etching is performed by laser etching or reactive ion etching. Claim 17 A method according to any one of claims 13 to 16, wherein the method further comprises the step of depositing a solder bump on the ohmic contact or wire bonding the ohmic contact. Claim 18 An electronic device precursor for a Hall sensor, wherein the electronic device precursor comprises: a substrate having a layer structure thereon, wherein the layer structure comprises: a lower layer on a first region of the substrate, wherein the lower layer comprises one or more graphene layers extending across the lower layer, and an upper layer formed of a dielectric material on the lower layer, wherein the lower layer and the upper layer share a continuous outer edge surface; an ohmic contact provided on an additional region of the substrate and in direct contact with the one or more graphene layers through a portion of the continuous outer edge surface; and a continuous air-resistant coating layer surrounding the layer structure and protecting all remaining portions of the continuous outer edge surface. Claim 19 An electronic device precursor according to claim 18, wherein the lower layer further comprises at least one layer of silicene, germanene, h-BN, boropene, and TMDC extending across the lower layer. Claim 20 In paragraph 18, the charge carrier density of the one or more graphene layers is 8×10 11 cm -2 Electronic device precursor less than Claim 21 delete Claim 22 delete Claim 23 delete Claim 24 delete
Citation Information
Patent Citations
Ultralow ohmic contact resistance graphene transistor and preparation method thereof
CN103985762A
Compound semiconductor multilayer structure, halldevice, and hall device manufacturing method
KR1020040073568A
Hall sensor manufacturing method, hall sensor, and lens module
KR1020170028378A