Co-extruded sheet

A co-extruded sheet with a foamed core and non-foamed skin layers, controlled thickness ratios, and densities addresses thermal expansion issues, enhancing mechanical strength and appearance in polycarbonate resin sheets.

KR103047021B1Active Publication Date: 2026-11-11맥셀 주식회사
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020237044107
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-10-21
Publication Date
2026-11-11
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing co-extruded sheets made of polycarbonate resin face issues with surface bulging and cracking during thermal molding due to thermal expansion of bubbles in the core layer, leading to poor appearance and reduced mechanical strength, especially when heated above 200°C.

Method used

A co-extruded sheet comprising a core layer of foamed resin and two skin layers of non-foamed resin, with controlled thickness ratios and densities, and a specific formula governing the skin layer thickness relative to the total sheet thickness, to suppress thermal expansion and cracking.

Benefits of technology

The solution effectively suppresses surface bulging and cracking during thermal forming, maintains excellent mechanical strength, and ensures lightweight properties, improving the appearance and aesthetic quality of the co-extruded sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023143145186-PCT00002_ABST
    Figure 112023143145186-PCT00002_ABST
Patent Text Reader

Abstract

A co-extruded sheet is provided that can suppress surface bulging or cracking during thermal molding, such as vacuum forming, and can also obtain excellent mechanical strength. The co-extruded sheet (1) comprises a core layer (2) made of a foamed resin, a skin layer (3) made of a non-foamed resin, and a skin layer (4). The skin layer (3) is laminated on one side of the core layer (2), and the skin layer (4) is laminated on the other side of the core layer (2). The co-extruded sheet (1) has a density of 0.4 to 0.9 g / cm³. The co-extruded sheet (1) has a thickness of 1 to 5 mm and satisfies Equation (1) {0.10 ≤ (t1 + t2) / T ≤ 0.5}. In equation (1), t1 represents the thickness of the skin layer (3), t2 represents the thickness of the second skin layer (4), and T represents the thickness of the co-extruded sheet (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a co-extruded sheet comprising an engineering plastic, in particular a polycarbonate resin. Background Technology

[0002] Recently, foamed resins have been attracting attention because they can enhance convenience by lightweighting resin molded bodies and also reduce carbon dioxide emissions. Molding methods for foamed resins include physical foaming and chemical foaming. Chemical foaming utilizes chemical foaming agents. Chemical foaming agents have a high environmental burden and are therefore not preferred from the perspective of global environmental protection. On the other hand, physical foaming utilizes physical foaming agents, such as nitrogen or carbon dioxide, as foaming agents. Physical foaming agents are desirable from the perspective of global environmental protection because they have a low environmental burden. In physical foaming, as a method for foaming high-heat-resistant engineering plastics and super engineering plastics, there is a method in which molten resin of engineering plastics and super engineering plastics is melted by shear-kneading with a high-pressure supercritical fluid.

[0003] Japanese Patent Publication No. 6139038 (Patent Document 1) discloses a method for manufacturing a foamed molded article using a physical foaming agent, such as nitrogen or carbon dioxide, which has a relatively low pressure, rather than a high-pressure supercritical fluid. According to this method, fine foam cells can be formed in a resin molded article through a relatively simple process using a low-pressure physical foaming agent without using a special high-pressure device. In addition, Patent Document 1 discloses a method for molding a foamed molded article by injection molding and extrusion molding.

[0004] Injection molding allows for the production of foamed bodies with complex shapes. However, the molten resin flows within the mold as its surface layer cools and solidifies. Consequently, a relatively thin, non-foamed skin layer is formed on the surface of the foamed body. On the other hand, extrusion molding is suitable for continuously producing foamed bodies of a single shape and thickness, as it has fewer limitations on mold size and load compared to injection molding. Furthermore, sheet-shaped foamed bodies obtained by extrusion molding can be molded into somewhat complex shapes or relatively large sizes by performing vacuum forming or similar processes. However, in extrusion molding, it is difficult to form a skin layer on the surface of the foamed body when the molten resin is discharged from the die outlet and cools and solidifies. As a result, foamed bodies with such a relatively thin skin layer and those without a skin layer have inferior surface aesthetics compared to foamed bodies with a skin layer of sufficient thickness. In addition, foamed molded articles obtained by the extrusion molding method had a problem in that the bubbles were destroyed by the pressure release when the molten resin was discharged from the die outlet, which could cause irregularities on the surface of the foamed article and reduce its aesthetic appearance.

[0005] Furthermore, Patent Document 1 does not examine a foamed molded article of a polycarbonate resin made of a vacuum-moldable amorphous resin, nor does it examine securing the surface smoothness of the foamed molded article when heated at a temperature exceeding the glass transition temperature of the polycarbonate resin. Here, in the case of non-foamed resins, crystalline resins are less likely to undergo significant deformation or dimensional change when heated at a temperature lower than their melting point, even if the temperature is higher than the glass transition temperature. However, in the case of non-foamed resins, amorphous resins are more prone to thermal deformation when heated at a temperature higher than the glass transition temperature (the glass transition temperature of polycarbonate resin is approximately 145°C). Considering this, when a foamed molded article made of an amorphous resin (polycarbonate resin) is heated at a temperature above the glass transition temperature, it becomes more difficult to suppress deformation occurring on its surface, for example, expansion occurring on the surface of the foamed resin due to bubbles formed inside the foamed molded article, or dimensional change of the foamed molded article.

[0006] As a method for forming a skin layer having sufficient thickness, Japanese Patent Publication No. 3654697 (Patent Document 2) discloses a method for manufacturing a thermoplastic resin foam sheet. According to the method for manufacturing a thermoplastic resin foam sheet, a skin layer can be easily formed on the surface of the thermoplastic resin foam sheet by extrusion molding. In addition, Japanese Patent Publication No. 2000-52370 (Patent Document 3) discloses a method for manufacturing a multilayer laminated body. The multilayer laminated body forms a core layer and a skin layer made of foamed resin by co-extrusion molding. The manufacturing method of Patent Document 2 and the manufacturing method of Patent Document 3 utilize general-purpose plastics with relatively low heat resistance and mechanical strength, such as polypropylene or polystyrene, as the main resin material, and do not utilize engineering plastics with excellent heat resistance and mechanical strength, particularly polycarbonate resin. In addition, the manufacturing methods of Patent Document 2 and Patent Document 3 are intended for ease or stability of manufacturing a foamed molded body, and are not intended for improving heat resistance and mechanical strength. Furthermore, if the thickness of the skin layer is too large, that is, if the thickness of the core layer is too small, lightweighting cannot be achieved.

[0007] Japanese Patent Publication No. 3568655 (Patent Document 4) discloses a polycarbonate resin extrusion foam laminated sheet formed by laminating multiple polycarbonate resin extrusion foam sheets. However, the polycarbonate resin extrusion foam laminated sheet of Patent Document 4 manufactures a relatively thick polycarbonate resin foam sheet by cutting and laminating polycarbonate resin extrusion foam sheets, and does not control the skin layer of the surface layer.

[0008] Furthermore, resin molded articles made of foamed resin have a problem in that their mechanical strength decreases due to the low density achieved to improve lightness. In particular, foamed molded articles made of polycarbonate resin, where mechanical strength is required, also have a problem in that their mechanical strength is significantly lower compared to resin molded articles made of non-foamed resin.

[0009] Japanese Patent Publication No. JP 8-174780 (Patent Document 5) discloses a polycarbonate extrusion resin foam laminate sheet with a high foaming ratio manufactured by a co-extrusion molding method. The polycarbonate extrusion resin foam laminate sheet has excellent heat processability, particularly deep drawing processability, and also has excellent appearance and mechanical strength. Patent Document 5 discloses the change in heating dimensions when the polycarbonate extrusion resin foam laminate sheet is heated under a temperature atmosphere of 170°C, which is a relatively low temperature. Prior art literature

[0010] Japanese Patent Publication No. 6139038, Japanese Patent Publication No. 3654697, Japanese Published Patent Application No. 2000-52370, Japanese Patent Publication No. 3568655, Japanese Published Patent Application No. Hei 8-174780

[0011] However, recently, when heat-forming co-extruded sheets into a desired shape using vacuum forming or the like, from the perspective of improving productivity, it is required to be able to form them in a short time from draw-down (a phenomenon where molten resin stretches due to its own weight) and to heat them at a relatively high temperature of 200°C or higher. However, when a co-extruded sheet having a core layer made of foamed resin and a skin layer made of non-foamed resin laminated on the main surface of the core layer is heated at a high temperature of 200°C or higher, the bubbles within the core layer covered by the skin layer tend to expand thermally and coalesce. As a result, there has been a problem in which the appearance and aesthetic quality of the co-extruded sheet deteriorate, such as the skin layer bulging out from the main surface of the co-extruded sheet or cracking occurring in the co-extruded sheet itself.

[0012] Furthermore, co-extrusion molding is an integral molding method in which the core layer and the skin layer are joined within the die during co-extrusion. Consequently, when pressure is released from the die exit, bubbles in the core layer expand, leading to problems with the uniformity of bubble sizes. In particular, when the pressure and concentration of the physical foaming agent are increased, the density of expanding bubbles increases; consequently, the bubble sizes in the core layer of the co-extruded sheet become non-uniform, causing bulging areas to occur in the co-extruded sheet after heating to 200°C or higher.

[0013] In addition, as described in Patent Document 5, a polycarbonate laminated foamed resin sheet with a high foaming ratio can achieve excellent lightness, but there was also a problem that the mechanical strength was reduced compared to a polycarbonate laminated foamed resin sheet with a low foaming ratio.

[0014] The inventors have discovered, as a result of careful consideration, that by controlling the density of the co-extruded sheet and the thickness of the skin layer, it is possible to improve mechanical strength and suppress the deterioration of appearance during vacuum forming in a co-extruded sheet comprising a core layer made of foamed resin intended for lightweighting.

[0015] In addition, Patent Document 5 does not propose improving mechanical strength in terms of the density or thickness of the skin layer of a polycarbonate resin laminated foamed resin sheet and suppressing the deterioration of appearance during vacuum forming.

[0016] The present disclosure aims to provide a co-extruded sheet comprising a polycarbonate resin that can suppress surface bulging or cracking of the co-extruded sheet that occurs during thermal molding such as vacuum forming, and also has excellent mechanical strength.

[0017] To solve the above problem, the present disclosure has devised the following means of solution. That is, the co-extruded sheet related to the present disclosure may include a polycarbonate resin. It may have a core layer made of a foamed resin, a first skin layer made of a non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³, a thickness of 1 to 5 mm, and also satisfy the following formula (1).

[0018] 0.10≤(t1+t2) / T≤0.5···(1)

[0019] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0020] The co-extruded sheet may include a bulge formed on the surface of the co-extruded sheet by heating when heated for 30 minutes in a heating atmosphere of 250°C. The thickness (t3) of the co-extruded sheet including the bulge may be 1.5 times or less of the average thickness (t4) of the co-extruded sheet before heating. The co-extruded sheet after heating may have fewer than one of the above bulges per 100 cm² of its surface.

[0021] The co-extruded sheet may include polycarbonate resin. It may comprise a core layer made of foamed resin, a first skin layer made of non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³ and a thickness of 1 to 5 mm, and may also satisfy the following formula (1).

[0022] 0.10≤(t1+t2) / T≤0.5···(1)

[0023] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0024] When the co-extruded sheet is heated for 30 minutes in a heating atmosphere of 250°C, the average thickness (t5) of the co-extruded sheet after heating may be 1.5 times or less than the average thickness (t4) of the co-extruded sheet before heating.

[0025] The co-extruded sheet may include polycarbonate resin. It may comprise a core layer made of foamed resin, a first skin layer made of non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³ and a thickness of 1 to 5 mm, and may also satisfy the following formula (1).

[0026] 0.10≤(t1+t2) / T≤0.5···(1)

[0027] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0028] The core layer may have a foaming ratio of 1.6 to 3.3 times.

[0029] According to the co-extruded sheet related to the present disclosure, surface bulging or cracking of the co-extruded sheet that occurs during thermal forming such as vacuum forming can be suppressed, and excellent lightness and mechanical strength can also be obtained. Brief explanation of the drawing

[0030] FIG. 1 is a perspective view showing a co-extruded sheet related to an embodiment. FIG. 2 is a cross-sectional view showing the co-extruded sheet shown in FIG. 1. Figure 3 is a cross-sectional view showing a co-extruded sheet after heating. Figure 4 is a cross-sectional view showing a co-extruded sheet after heating. FIG. 5 is a cross-sectional view showing a co-extruded sheet including a decorative film. Specific details for implementing the invention

[0031] To solve the above problem, the present disclosure has devised the following means of solution. That is, the co-extruded sheet related to the present disclosure may include a polycarbonate resin. It may comprise a core layer made of a foamed resin, a first skin layer made of a non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³. The co-extruded sheet may have a thickness of 1 to 5 mm and may also satisfy the following formula (1).

[0032] 0.10≤(t1+t2) / T≤0.5···(1)

[0033] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0034] The co-extruded sheet may include a bulge formed on the surface of the co-extruded sheet by heating when heated for 30 minutes in a heating atmosphere of 250°C. The thickness (t3) of the co-extruded sheet including the bulge may be 1.5 times or less of the average thickness (t4) of the co-extruded sheet before heating. The co-extruded sheet after heating may have fewer than one bulge per 100 cm² of its surface.

[0035] In this way, by controlling the thickness of the skin layer relative to the density and thickness of the co-extruded sheet, surface expansion or cracking occurring during thermal forming, such as vacuum forming, can be suppressed, and excellent lightweight properties and mechanical strength can be obtained. Furthermore, the deterioration of the appearance and aesthetic quality of the co-extruded sheet during thermal forming, such as vacuum forming, can be suppressed.

[0036] The co-extruded sheet may include polycarbonate resin. It may comprise a core layer made of foamed resin, a first skin layer made of non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³ and a thickness of 1 to 5 mm, and may also satisfy the following formula (1).

[0037] 0.10≤(t1+t2) / T≤0.5···(1)

[0038] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0039] When the co-extruded sheet is heated for 30 minutes in a heating atmosphere of 250°C, the average thickness (t5) of the co-extruded sheet after heating may be 1.5 times or less than the average thickness (t4) of the co-extruded sheet before heating. By controlling the thickness of the skin layer relative to the density of the co-extruded sheet and the thickness of the co-extruded sheet, surface expansion or cracking that occurs during thermal forming such as vacuum forming can be suppressed, and excellent lightness and mechanical strength can be obtained. In addition, the deterioration of the appearance of the co-extruded sheet during thermal forming such as vacuum forming can be suppressed.

[0040] The co-extruded sheet may include polycarbonate resin. It may comprise a core layer made of foamed resin, a first skin layer made of non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer. The co-extruded sheet may have a density of 0.4 to 0.9 g / cm³ and a thickness of 1 to 5 mm, and may also satisfy the following formula (1).

[0041] 0.10≤(t1+t2) / T≤0.5···(1)

[0042] In equation (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet.

[0043] The core layer may have a foaming ratio of 1.6 to 3.3 times. By doing so, the deterioration of the appearance of the co-extruded sheet during thermal molding, such as vacuum forming, can be suppressed, and superior lightness and mechanical strength can be obtained.

[0044] The polycarbonate resin included in the first and second skin layers may have a melt volume rate of 1.0 to 5 times with respect to the polycarbonate resin included in the core layer. By doing so, non-uniformity of bubble sizes in the core layer can be suppressed.

[0045] The polycarbonate resin included in the first and second skin layers may have a melt volume rate of 1.5 to 3 times with respect to the polycarbonate resin included in the core layer. By doing so, vacuum formability can be improved.

[0046] The co-extruded sheet may have a density of 0.82 g / cm³ or less. By doing so, superior lightness and mechanical strength can be obtained.

[0047] When a co-extruded sheet is heated in an atmosphere of 200°C for 30 minutes, the co-extruded sheet may have a dimensional change rate of -5 to 0% in either the extrusion direction or the width direction perpendicular to the extrusion direction in the planar view. By doing so, the dimensional stability of the co-extruded sheet can be ensured during thermal forming such as vacuum forming.

[0048] The co-extruded sheet may have a specific bending modulus of 1.5 GPa·cm³ / g or more. By doing so, the weight of the co-extruded sheet can be reduced, and the mechanical strength can also be improved.

[0049] The co-extruded sheet may have a specific bending modulus of 2 GPa·cm³ / g or more. By doing so, the weight reduction and mechanical strength of the co-extruded sheet can be further improved.

[0050] The co-extruded sheet may further have a decorative film. The decorative film may be laminated on the outer surface of at least one of the first skin layer and the second skin layer. By doing so, a design according to the intended use of the molded product formed by vacuum forming the co-extruded sheet can be provided.

[0051] Hereinafter, embodiments of the co-extruded sheet (1) of the present disclosure will be described in detail using FIGS. 1 to 5. Also, identical and corresponding components in the drawings are given the same reference numerals, and identical descriptions are not repeated. In addition, to make the explanation easier to understand, the components in the drawings referenced below are simplified or schematic, or some components are omitted.

[0052] The co-extruded sheet (1) is made of polycarbonate resin. The co-extruded sheet (1) related to the present embodiment has a sheet shape. The co-extruded sheet (1) is manufactured by co-extruding molten polycarbonate resin. The resin used in the present disclosure may be any engineering plastic that includes polycarbonate resin. The engineering plastic is a thermoplastic resin having a load bending temperature of 100°C or higher. Examples of engineering plastics include, in addition to polycarbonate resin (PC), modified polyphenylene ether (m-PPE), syndiotactic polystyrene (SPS), etc. The resin used in the co-extruded sheet (1) of the present disclosure may include at least one selected from the group consisting of these engineering plastics. Furthermore, the resin material of the co-extruded sheet (1) may be an extrusion-moldable engineering plastic. Additionally, an ultraviolet absorber and an anti-aging agent, etc., may be added to the resin material of the co-extruded sheet (1).

[0053] The co-extruded sheet (1) has a density of 0.4 to 0.9 g / cm³. By making the density of the co-extruded sheet (1) 0.4 to 0.9 g / cm³, it is possible to achieve both lightweighting and increased strength. More preferably, the density of the co-extruded sheet (1) should be 0.4 to 0.82 g / cm³. By doing so, superior lightweighting and mechanical strength can be obtained.

[0054] As shown in FIG. 1, the co-extruded sheet (1) has a core layer (2), a skin layer (3) laminated on one side of the core layer (2), and a skin layer (4) laminated on the other side of the core layer (2). As shown in FIG. 2, the co-extruded sheet (1) has a thickness (T) of 1 to 5 mm.

[0055] The core layer (2) is made of foamed resin. The core layer (2) can be formed by foam molding molten polycarbonate resin. That is, the core layer (2) has a plurality of bubbles. The plurality of bubbles have a roughly elliptical shape that is elongated in the extrusion direction when viewed in a cross-sectional view taken in the thickness direction along the direction of extrusion molding. Among the plurality of bubbles contained in the core layer (2), the bubbles contained near the center in the thickness direction of the core layer (2) have a larger bubble diameter than the bubbles (21) contained near the end in the thickness direction of the core layer (2). The bubble diameter of the plurality of bubbles (21) gradually decreases as it moves from the center in the thickness direction of the core layer (2) toward the end in the thickness direction.

[0056] As shown in FIG. 2, the skin layer (3) is made of a non-foamed resin. That is, the skin layer (3) is not foamed. The skin layer (3) is extruded from the die exit in a non-foamed state by a co-extrusion molding method and laminated integrally with the core layer (2). The skin layer (3) has a thickness t1.

[0057] The skin layer (3) may be made of a thermoplastic resin that can adhere well to the core layer (2). More specifically, it is particularly preferable that the resin material of the skin layer (3) be the same resin material as the core layer (2). In addition, the skin layer (3) may be composed of a reinforcing resin containing an inorganic filler to reinforce the skin layer (3). By composing the skin layer (3) in this way, it is possible to achieve lightweighting and strength enhancement while efficiently improving strength. Inorganic fillers are, for example, glass fibers, carbon fibers, aramid fibers, talc, and mica.

[0058] The skin layer (4) has a thickness t2. The skin layer (4) is identical to the skin layer (3) except that it is laminated on the other side of the core layer (2). Therefore, a detailed description of the skin layer (4) is omitted.

[0059] The thickness (t1) of the skin layer (3) and the thickness (t2) of the skin layer (4) are measured as follows. A cross-section of the co-extruded sheet (1) cut along the width direction in the thickness direction is observed using a microscope. In this disclosure, a KEYENCE model number VHX-60000 is used as the microscope. The magnification of the microscope is sufficient to confirm the diameter of the bubbles at the interface between the skin layer (3) and the core layer (2) of the co-extruded sheet (1). When examining the cross-section of the co-extruded sheet (1), among the numerous bubbles present, 15 bubbles close to the surface of the co-extruded sheet (1) are selected on each virtual boundary line when the cross-section of the co-extruded sheet (1) is divided into 16 equal parts in the width direction, and the bubble closest to the surface of the co-extruded sheet (1) among them is identified. A virtual line is drawn passing over the top of this closest bubble and also perpendicular to the thickness direction. The inner side of the thickness direction relative to the virtual line is designated as the core layer (2), and the outer side of the thickness direction is designated as the skin layer (3). The boundary between the core layer (2) and the skin layer (4) is defined in the same way, and the thickness (t1) of the skin layer (3) and the thickness (t2) of the skin layer (4) are measured. Furthermore, the thickness (t1) of the skin layer (3) and the thickness (t2) of the skin layer (4) are each preferably 0.050 mm or more, from the perspective of making the thickness (T) of the co-extruded sheet (1) as uniform as possible during co-extrusion molding.

[0060] The total thickness of the skin layer, which is the sum of the thickness (t1) of the skin layer (3) and the thickness (t2) of the skin layer (4), is preferably 0.10 to 0.5 with respect to the thickness (T) of the co-extruded sheet (1). That is, the co-extruded sheet (1) satisfies the following formula (1).

[0061] 0.10≤(t1+t2) / T≤0.5···(1)

[0062] If the total thickness (t1+t2) of the skin layer is less than 0.10 relative to the thickness (T) of the co-extruded sheet (1), it is difficult to obtain the reinforcing effect of mechanical strength by the non-foamed resin of the skin layer, and mechanical strength such as non-flexural modulus decreases. On the other hand, if the total thickness (t1+t2) of the skin layer is greater than 0.5 relative to the thickness (T) of the co-extruded sheet (1), the density of the co-extruded sheet (1) increases. As a result, the lightweight properties of the co-extruded sheet (1) due to foaming are compromised. The ratio of the total thickness (t1+t2) of the skin layer to the thickness (T) of the co-extruded sheet (1) is preferably in the range of 0.15 to 0.45, and more preferably in the range of 0.2 to 0.4. By setting the ratio of the total thickness of the skin layer (t1+t2) to the thickness (T) of the co-extruded sheet (1) to this range, it is possible to improve the non-bending elastic modulus while achieving weight reduction through density reduction. Additionally, by setting the ratio of the total thickness of the skin layer (t1+t2) to the thickness (T) of the co-extruded sheet (1) to the range of 0.2 to 0.4, it is possible to improve secondary processing capabilities such as vacuum forming while ensuring the thickness of the core layer (2) that uniformly eliminates irregular bubbles.

[0063] In this way, by controlling the ratio of the thickness (t1+t2) of the skin layer (3) and the skin layer (4) to the density of the co-extruded sheet (1) and the thickness (T) of the co-extruded sheet (1), surface expansion or cracking that occurs during thermal molding, such as vacuum forming, can be suppressed, and excellent lightness and mechanical strength can also be obtained.

[0064] The melt volume rate (hereinafter referred to as MVR) of the polycarbonate resin included in the skin layer (3) is the same as the MVR of the polycarbonate resin included in the core layer (2), or is higher than the MVR of the polycarbonate resin included in the core layer (2). The MVR of the polycarbonate resin included in the skin layer (3) is 1.0 to 5 times the MVR of the polycarbonate resin included in the core layer (2), and preferably 1.5 to 3 times.

[0065] By making the MVR of the resin included in the skin layer (3) equal to the MVR of the resin included in the core layer (2), or by making it higher than the MVR of the resin included in the core layer (2), the temperature of the resin forming the skin layer (3) can be lowered as much as possible immediately after being discharged from the die exit during extrusion molding. As a result, since the viscosity of the skin layer (3) immediately after being discharged from the die exit can be lowered, swelling or tearing of the surface of the skin layer (3) caused by non-uniformity of bubble sizes included in the core layer (2) can be suppressed. That is, if the ratio of the MVR in the resin included in the skin layer (3) is less than 1.0 times, it becomes difficult to lower the resin temperature, and thus it becomes difficult to suppress swelling or tearing of the surface of the skin layer (3). In addition, if the ratio of MVR in the resin included in the skin layer (3) is 1.5 times or more, it becomes easier to suppress the non-uniformity of the bubble size of the core layer (2) during extrusion molding, and also, the preheating time during vacuum molding can be shortened to improve productivity. On the other hand, if the ratio of MVR in the resin included in the skin layer (3) is greater than 5 times, in order to properly flow the resin forming the skin layer (3) within the die during extrusion molding, it is necessary to drastically lower the MVR of the resin forming the core layer (2). In addition, if the ratio of MVR in the resin included in the skin layer (3) is 3 times or less, the irregular bubbles of the core layer (2) of the co-extruded sheet (1) become more uniform, and the secondary processing capability, such as vacuum molding of the co-extruded sheet (1), can be improved. Therefore, considering that the resin forming the core layer (2) and the skin layer (3) is to be properly fluidized during extrusion molding and also to be controlled to a viscosity that suppresses swelling or tearing of the surface of the skin layer (3), the MVR of the polycarbonate resin included in the skin layer (3) is preferably 1.0 to 5 times, and preferably 1.5 to 3 times, of the MVR of the polycarbonate resin included in the core layer (2).This is also true for the skin layer (4) and the core layer (2).

[0066] In addition, the MVR of the resin contained in the skin layer (3) and the core layer (2) is measured by a plastic flow characteristic test using a capillary rheometer and a slit die rheometer (in accordance with JISK 7199 and ISO 11443). In the present disclosure, the length of the capillary die is 5 mm and the inner diameter is 1 mm, and the measurement is performed at a temperature of 300°C.

[0067] In addition, the core layer (2) of the present disclosure is preferably foam-molded using a physical foaming agent such as nitrogen or carbon dioxide, which has a relatively low pressure, as disclosed in Patent Document 1 above, and among these, nitrogen is more preferable. By doing so, the pressure of the physical foaming agent can be set to a relatively low 1 to 6 MPa, and a large number of fine bubbles can be formed. By doing so, swelling, etc., can be more reliably suppressed when heated at a high temperature during vacuum molding. The average bubble diameter of the bubbles is preferably 0.1 mm or more, 1.0 mm or less, and preferably 0.3 mm or less. In addition, the foaming ratio of the core layer (2) is preferably 1.6 times or more and 3.3 times or less. By doing so, the deterioration of the appearance of the co-extruded sheet during thermal molding such as vacuum molding can be suppressed, and superior lightness and mechanical strength can be obtained. In addition, the foaming ratio of the core layer (2) should be 3.1 times or less. By doing so, better lightness and mechanical strength can be obtained.

[0068] The co-extruded sheet (1) is formed into various shapes by vacuum forming. In vacuum forming, the co-extruded sheet (1) is typically formed by heating to about 200°C, starting the drawdown, and then adhering to a mold or the like and being vacuum-suctioned. That is, it is desirable for the co-extruded sheet (1) to have a small amount of deformation (the rate of change in dimensions before and after heating) relative to the heating temperature during vacuum forming. When the co-extruded sheet (1) is heated for 30 minutes in a 200°C atmosphere, it has a rate of change in dimensions of -5% to 0% in the extrusion direction. Additionally, the co-extruded sheet (1) has a rate of change in dimensions of -5% to 0% in the width direction. That is, the co-extruded sheet (1) has a rate of change in dimensions of -5% to 0% in either the extrusion direction or the width direction. Alternatively, the co-extruded sheet (1) has a dimensional change rate of -5 to 0% in both the extrusion direction and the width direction. The width direction is a direction perpendicular to the extrusion direction described above when viewed in a flat plane. Accordingly, the co-extruded sheet (1) has excellent dimensional stability before and after heating.

[0069] The rate of dimensional change in the extrusion direction can be calculated as follows.

[0070] Dimensional change rate in the extrusion direction (%) = {(Distance between marks in the extrusion direction after heating - Distance between marks in the extrusion direction before heating) / Distance between marks in the extrusion direction before heating} × 100

[0071] Meanwhile, the rate of change in dimensions in the width direction can be calculated as shown in the following formula.

[0072] Percentage of change in width direction (%) = {(Distance between width lines after heating - Distance between width lines before heating) / Distance between width lines before heating} × 100

[0073] The co-extruded sheet (1) has a specific bending modulus of 1.5 GPa·cm³ / g or more, and the specific bending modulus is the value obtained by dividing the bending modulus of the co-extruded sheet (1) by the density of the co-extruded sheet (1). In other words, the greater the specific bending modulus, the better the lightness and mechanical strength. The bending modulus is measured by a three-point bending test (in accordance with ISO 178 or JIS K 7171). At this time, the bending modulus is measured in the atmosphere. The test speed is 10 mm / min.

[0074] The co-extruded sheet (1) is heat-formed into a desired shape, mainly by vacuum forming or the like. When the co-extruded sheet is heated, expansion (bulging) may occur on the surface of the sheet, which can deteriorate the appearance of the sheet surface. Therefore, it is desirable to suppress the occurrence of bulging on the co-extruded sheet (1). As shown in FIG. 3, when the co-extruded sheet (1) is heated for 30 minutes in a heating atmosphere of 250°C, the average thickness (t5) of the co-extruded sheet (1) after heating is 1.5 times or less than the average thickness (t4) of the co-extruded sheet before heating. Also, S, indicated by the dashed line in FIG. 3, is the surface of the co-extruded sheet (1) before heating. That is, the co-extruded sheet (1) can suppress the occurrence of bulging caused by heating, thereby minimizing the change in thickness when comparing before and after heating. By doing so, the co-extruded sheet (1) can improve the appearance and aesthetics during thermal molding, such as vacuum forming.

[0075] In addition, as shown in FIG. 4, the thickness (t3) of the co-extruded sheet including the aforementioned bulging portion (11) is 1.5 times or less of the average thickness (t4) of the co-extruded sheet before heating shown in FIG. 3. The co-extruded sheet (1) after heating has less than one bulging portion (11) per 100 cm² of its surface. That is, according to the co-extruded sheet (1), the height of the bulging portion (11) formed on the surface by heating can be reduced, and the number of bulging portions (11) can be suppressed. By doing so, the co-extruded sheet (1) can improve the appearance and aesthetic qualities during thermal molding, such as vacuum forming. The thermally molded body of the co-extruded sheet is used for applications where appearance and aesthetic qualities are particularly required, such as containers like signboards or suitcases, and interior and exterior materials for vehicles, such as automobiles. Therefore, defects such as expansion in the heat-formed material are not desirable for the listed uses. Accordingly, expansion caused by heating of the co-extruded sheet (1) should be suppressed as much as possible, and specifically, it is preferable that the number of bulging parts (11) be less than one.

[0076] The co-extruded sheet (1) may contain a plurality of flake-like fillers. The flake-like fillers are inorganic fillers such as, for example, talc, calcium carbonate, mica, clay, boron nitride, wollastonite, potassium titanate, glass flakes, etc. Surface treatments such as silane-based coupling agents, titanate-based coupling agents, phosphate ester-based coupling agents, and fatty acid-based coupling agents may be applied to the flake-like fillers. The flake-like fillers have an aspect ratio of 5 or more. The aspect ratio is calculated by dividing the average particle size of the flake-like fillers by the average thickness (average particle size / average thickness). If the aspect ratio of the flake-like fillers becomes too small, it becomes difficult to achieve excellent surface smoothness. Therefore, the aspect ratio of the flake-like fillers is preferably 10 or more, and more preferably 30 or more. However, if the aspect ratio becomes too large, it becomes difficult to control the flow rate of the mixed molten resin inside the die during the manufacturing process described later, and there is a risk that the surface smoothness will deteriorate. In addition, the increase in viscosity of the mixed molten resin during extrusion molding becomes large, and thermal degradation of the thermoplastic resin may occur due to heat generation within the extrusion molding device described later. Therefore, it is preferable to keep the aspect ratio of the flake-like filler less than 50. It is preferable to have a specific surface area of ​​the flake-like filler of 5 to 20 m² / g. If the specific surface area of ​​the flake-like filler becomes too small, it becomes difficult to achieve surface smoothness due to sliding on the surface by the flake-like filler, and if the specific surface area becomes too large, the resistance of the flake-like filler in the molten resin increases, and as a result, it becomes difficult to properly orient the flake-like filler.

[0077] The core layer (2) may include flake-like fillers oriented approximately parallel to the boundary surface between the core layer (2) and the skin layer (3) in the vicinity of the boundary with the skin layer (3). The vicinity is an area positioned in the thickness direction of the core layer (2) from the boundary surface between the core layer (2) and the skin layer (3) to a thickness of 5% of the core layer thickness. Additionally, the bubbles included in the core layer (2) have a shape that is elongated along the extrusion direction during extrusion molding. Since the flake-like fillers are oriented approximately parallel to the bubble walls of the bubbles extending in the elongation direction, the strength of the bubble walls can be improved. As a result, tearing along the extrusion direction of the co-extruded sheet (1) can be suppressed. In addition, the statement that the flake-like filler is approximately parallel means that in a cross-section obtained by cutting the co-extruded sheet (1) in the thickness direction along the extrusion direction during extrusion molding, the flake-like filler has an inclination of 0° or more and less than 5° with respect to the boundary surface between the core layer (2) and the skin layer (3). In other words, it refers to a state in which the surface (main surface) of the flake-like filler and the boundary surface between the core layer (2) and the skin layer (3) are facing each other so that they are approximately parallel. The same applies to the flake-like filler oriented toward the core layer (2) near the boundary between the core layer (2) and the skin layer (4).

[0078] The orientation state of a plurality of scale-like fillers included in the region near the boundary between the core layer (2) and the skin layer (3) was calculated as follows. First, in a cross-section in the thickness direction following the extrusion direction during extrusion molding, 50 electron microscope images of 150×150 μm were taken at equal intervals from the leading edge to the trailing edge of the extrusion direction in the region near the center of the thickness direction of the region near the core layer (2) and the skin layer (3). Among all the scale-like fillers included in these 50 electron microscope images, scale-like fillers oriented approximately parallel to the boundary surface between the core layer (2) and the skin layer (3) were identified. By doing so, the ratio of scale-like fillers oriented approximately parallel among the plurality of scale-like fillers included in the region near the core layer (2) was calculated.

[0079] The core layer (2) may include flake-like fillers oriented at an angle of 5° to 90° with respect to the surface of the co-extruded sheet (1) in the center region of the thickness direction of the core layer (2). The center region refers to a region with a thickness of 25% from the center of the thickness direction toward the boundary surface between the core layer (2) and the skin layer (3), when the thickness of the core layer (2) is 100%. It is preferable that at least 40% of the flake-like fillers included in the center region are oriented at an angle of 5° to 90° with respect to the surface (S) of the co-extruded sheet (1). By doing so, the moldability of the co-extruded sheet (1) can be improved. More preferably, at least 60%, and even more preferably at least 80%, of the flake-like fillers are oriented at an angle of 5° to 90° with respect to the surface. By doing so, the moldability of the co-extruded sheet (1) can be further improved. Bubbles contained in the central region of the core layer (2) tend to grow larger than the nearby region described above during extrusion molding. This is because the central region is more difficult to cool after extrusion compared to the nearby region. If the bubbles become too large, they become a cause of breakage of the co-extruded sheet (1). As described above, by tilting the flake-shaped filler in the central region and randomly arranging it between the bubbles, the growth of the bubbles in all directions can be suppressed. By doing so, the strength of the co-extruded sheet (1), or the strength during molding, that is, the moldability, can be improved. As a result, when producing a foamed resin molded product by vacuum molding the co-extruded sheet (1) into a material, the bursting of bubbles contained in the co-extruded sheet (1) or the breakage of the co-extruded sheet (1) can be suppressed.

[0080] The orientation state of a plurality of flake-like fillers included in the central region of the core layer (2) can be calculated as follows. First, 50 micrographs are taken at equal intervals at the center of the thickness direction of the core layer (2), just as in the case of the nearby region. Among all the flake-like fillers included in these 50 electron micrographs, the flake-like fillers oriented at an angle of 5° to 90° with respect to the surface of the co-extruded sheet (1) are identified. By doing so, the ratio of flake-like fillers oriented at an angle of 5° to 90° with respect to the surface of the co-extruded sheet (1) among the plurality of flake-like fillers included in the central region is calculated.

[0081] Next, a method for manufacturing a co-extruded sheet (1) will be described (not illustrated). First, resin pellets that serve as the resin material are introduced into the screw cylinder of the main extruder. The resin material is polycarbonate resin. The resin pellets are heated within the screw cylinder to produce molten resin. Next, a foaming agent is injected into the molten resin from a foaming agent injection bomb mounted on the screw cylinder of the main extruder. The foaming agent is dissolved in the molten resin by the screw cylinder described above, and is kneaded to be uniformly dispersed. In this way, a mixed molten resin is produced. The mixed molten resin is discharged from the die outlet to form a core layer (2). At the same time, two molten resins are produced by introducing resin pellets that serve as the resin material into the screw cylinders of two auxiliary extruders and heating and melting them. One of the two molten resins is discharged from the die outlet to form a skin layer (3), and the other is discharged from the die outlet to form a skin layer (4). The mixed molten resin and two molten resins are combined in a die from their respective extruders and discharged from the die outlet so that a skin layer (3) is laminated on one side of the main surface of the core layer (2) and a skin layer (4) is laminated on the other side of the main surface of the core layer (2). The mixed molten resin foams when extruded into the atmosphere from the die outlet. In this way, a co-extruded sheet (1) is manufactured. Furthermore, the foaming method is a physical foaming method that uses an inert gas, such as nitrogen and carbon dioxide, as a foaming agent. The co-extruded sheet (1) extruded in this way is transported to a cutter by a receiving machine. The cutter cuts the co-extruded sheet (1) into a desired shape.

[0082] The co-extruded sheet (1) manufactured in this manner can be used for the following purposes by forming it into a desired shape through vacuum forming, etc. For example, wide products and parts such as mobility materials requiring relatively high strength, such as signboards or automotive exterior materials; products and parts requiring heat resistance, such as batteries or trays for heating elements used in manufacturing processes involving heating processes; or products and parts requiring lightweighting. The co-extruded sheet (1) is suitable as a material for forming such products and parts by foam molding it using a co-extrusion molding method and containing polycarbonate resin.

[0083] Additionally, the co-extruded sheet (1) may have an embellishment film (5) as shown in FIG. 5. The embellishment film (5) is laminated on the outer surface of at least one of the skin layer (3) and the skin layer (4). The outer surface of the skin layer (3) is the surface of the skin layer (3) opposite to the surface facing the core layer (2). The same applies to the outer surface of the skin layer (4). By selecting a desired embellishment film (5) from among a plurality of embellishment films (5) with various designs, the co-extruded sheet (1) can be given an ornament suitable for use in a vacuum-formed molded product. As for the embellishment film (5), although not particularly limited, examples may be used such as a colored film, a film with any shape printed on its surface, a film with a pattern such as a wrinkle grain, wood grain, stone grain, or carbon tone, or a film with a metallic surface gloss imparted by deposition processing. The material of the decorative film (5) is, for example, PC, PMMA, PC / PMMA alloy, ABS, AES, vinyl chloride, copolymer PET, etc. The co-extruded sheet (1) may be composed of three layers: a core layer (2), a skin layer (3), and a skin layer (4), or may be composed by laminating the decorative film (5) onto at least one of the skin layer (3) and the skin layer (4).

[0084] Products and parts made by the co-extruded sheet (1) can reduce the amount of resin used. As a result, the co-extruded sheet (1) related to this embodiment can contribute to improving resource utilization efficiency, reducing transportation burdens, reducing energy consumption, and reducing CO2 emissions. By providing the co-extruded sheet (1) to society, it can contribute to the achievement of Goal 7 (Energy for everyone and cleanly), Goal 9 (Building a foundation for industrial and technological innovation), and Goal 11 (Building sustainable communities) among the 17 goals of the Sustainable Development Goals (SDGs) established by the United Nations.

[0085] Although embodiments have been described above, the present disclosure is not limited to the above embodiments, and various modifications are possible without departing from the spirit thereof.

[0086] (Example)

[0087] As shown in Table 1 below, test specimens of Examples 1 to 10 and Comparative Examples 1 to 6 were prepared, and tests were performed to evaluate the non-bending modulus, the presence or absence of fracture in the Charpy impact test, and the expansion of the test specimens when heated at 250°C for 30 minutes. The resin material used for each of these test specimens is a polycarbonate resin. Furthermore, the present disclosure is not limited to these examples.

[0088]

[0089] (Example 1)

[0090] The test specimen of Example 1 was prepared using a co-extrusion molding method as follows. First, polycarbonate resin was fed into the screw cylinder of a main extruder and shear-mixed while heating at 270°C. Subsequently, N2, a foaming agent, was injected under a pressure of 4 MPa. The polycarbonate resin and foaming agent were heated and melted at 215°C, and a core layer was obtained by setting the die exit temperature to 215°C. Simultaneously, polycarbonate resin was fed into the screw cylinder of a secondary extruder and shear-mixed while heating at 255°C, and two skin layers were obtained by setting the die exit temperature to 215°C. These core layers and skin layers were combined and laminated within the die and discharged from the die exit. In this way, the test specimen of Example 1 was obtained, in which skin layers made of non-foamed resin were laminated on both main surfaces of a core layer made of foamed resin. In addition, the exit gap of the die was set so that the thickness (T) of the test specimen of Example 1 was the value shown in Table 1, and the test specimen of Example 1 was co-extruded with a drawing speed of 0.7 m / min.

[0091] (Examples 2–10)

[0092] The test specimens of Examples 2 to 10 were prepared in the same manner as the test specimen of Example 1, except that the exit gap of the die, the discharge flow rate of the main extruder and auxiliary extruder, and the receiving speed were set so that the respective thickness (T) would be the value shown in Table 1. That is, the test specimens of Examples 1 to 10 have different thicknesses.

[0093] (Comparative Example 1)

[0094] The test specimen of Comparative Example 1 was prepared using a co-extrusion molding method as follows. First, polycarbonate resin was fed into the screw cylinder of a main extruder and shear-mixed while heating at 270°C. Subsequently, isopentane gas, a foaming agent, was injected to achieve a resin content of 0.53 mol / kg. The polycarbonate resin and foaming agent were heated and melted at 215°C, and a core layer was obtained by setting the die exit temperature to 215°C. Simultaneously, polycarbonate resin was fed into the respective screw cylinders of two auxiliary extruders and shear-mixed while heating at 255°C, and two skin layers were obtained by setting the die exit temperature to 215°C. These core layers and skin layers were combined and laminated within the die and discharged from the die exit. In this way, the test specimen of Comparative Example 1 was obtained, in which skin layers made of non-foamed resin were laminated on both main surfaces of a core layer made of foamed resin. In addition, the exit gap of the die was set so that the thickness (T) of the test specimen of Comparative Example 1 was the value shown in Table 1, and the test specimen of Comparative Example 1 was co-extruded with a drawing speed of 6.5 m / min.

[0095] (Comparative Example 2)

[0096] The specimen of Comparative Example 2 was prepared using the extrusion lamination method as follows. First, polycarbonate resin was fed into the screw cylinder of a main extruder and shear-kneaded while heating at 270°C. Subsequently, isopentane gas, a foaming agent, was injected so that the content was 0.53 mol per 1 kg of the fed polycarbonate resin. The polycarbonate resin and the foaming agent were heated and melted at 200°C, and a core layer was obtained by setting the die exit temperature to 200°C. The die exit gap was set so that the thickness (T) of the specimen of Comparative Example 2 was the value shown in Table 1, and the core layer was extruded with a drawing speed of 6.5 m / min. Next, while the extruded core layer was in a molten state, two skin layers made of pre-fabricated polycarbonate resin were laminated by bonding them to the main surfaces of both sides of the core layer.

[0097] (Comparative Example 3)

[0098] The test specimen of Comparative Example 3 was prepared by laminating a core layer and a skin layer by heat pressing. First, a core layer was obtained in the same manner as the test specimen of Comparative Example 2. Next, two skin layers made of pre-fabricated polycarbonate resin were each heat-pressed and laminated onto the main surfaces of both sides of the cooled and solidified core layer.

[0099] (Comparative Example 4)

[0100] The test specimen of Comparative Example 4 was prepared by the injection molding method. Polycarbonate resin was introduced into the screw cylinder of an injection molding machine and shear-mixed while heating at 270°C. Subsequently, nitrogen, which is a foaming agent, was injected under a pressure of 8 MPa, and the polycarbonate resin injected with the foaming agent was filled into the mold. Afterward, the pressure of the mold was released using the core-back method to obtain the test specimen. In addition, the mold was designed so that the thickness of the test specimen was 3 mm.

[0101] The density of the test specimens shown in Table 1 was calculated as follows. A sheet-shaped test specimen was cut to a length of 400 mm in the extrusion direction. The cross-section of the test specimen in the width direction was divided into 11 equal parts in the width direction, and the thickness was measured at 10 points at equal intervals, excluding the ends. The arithmetic mean of these thicknesses was taken as the average thickness of the test specimen. The lengths of each side of the test specimen in the width direction and the extrusion direction were measured using a measuring instrument, and the volume of the test specimen was calculated from the lengths of each side and the average thickness. In addition, the weight of the test specimen was measured using an electronic balance, and the density of the test specimen was obtained by dividing the weight of the test specimen by its volume.

[0102] The dimensional change rate shown in Table 1 was calculated as follows. First, a sample was obtained by cutting a sheet-shaped test specimen to dimensions of 120 mm × 120 mm. At this time, the sample was taken from the center and both ends relative to the total width of the test specimen. The center refers to the part located at half the length of the total width of the test specimen, and both ends refer to parts located 50 mm away from the shortest end of the total width of the test specimen. Each sample was marked in the extrusion direction and the width direction, and a mark was also made in the center of each sample to measure the distance between the marks in the extrusion direction and the width direction. This distance between the marks in the extrusion direction and the width direction was measured using a ruler or a square capable of measuring to a minimum of 0.5 mm. Afterward, a metal container with a PTFE (polytetrafluoroethylene) sheet placed on the inner bottom surface was placed in a dryer, and the temperature of the dryer was adjusted so that the temperature of the metal container was 200 ± 2°C. The specimen was placed in a metal container and heated for 30 minutes. After the heating treatment was completed, the specimen was removed from the metal container and cooled to room temperature, after which the distance between the marks in the extrusion direction and the width direction was measured. Then, the rate of dimensional change was calculated using the formula described above. In addition, for all specimens, the absolute value of the rate of dimensional change in the extrusion direction was greater than the rate of dimensional change in the width direction; therefore, Table 1 shows the rate of dimensional change in the extrusion direction. That is, the rate of dimensional change in the width direction is smaller than the rate of dimensional change in the extrusion direction. Therefore, the dimensions in the width direction were more stable than those in the extrusion direction before and after heating.

[0103] The thickness (T) and specific bending modulus of the test specimens shown in Table 1 were measured according to the measurement method described above. In addition, the MVR ratio shown in Table 1 is the ratio of the MVR of the polycarbonate resin included in the skin layer to the polycarbonate resin included in the core layer, and was measured by the measurement method described above. In addition, regarding the evaluation of the specific bending modulus, the case where the specific bending modulus is greater than 2.0 GPa·cm³ / g was designated as "A", the case where it is greater than 1.5 GPa·cm³ / g and less than or equal to 2.0 GPa·cm³ / g was designated as "B", and the case where it is less than or equal to 1.5 GPa·cm³ / g was designated as "C".

[0104] In Table 1, "Presence or absence of fracture" indicates whether each specimen was fractured by the impact test. In the Charpy impact test (in accordance with ISO 179-1 and JIS K 7111-1), a flat-wise vertical test was performed on each specimen under the condition of no notch, and the presence or absence of fracture was evaluated using a 4J pendulum. A state in which the specimen was only bent without complete fracture, hinge fracture, or partial fracture was evaluated as "A" as not fractured, and all other states were evaluated as fractured as "B".

[0105] In Table 1, "Sheet Expansion / Bulging" indicates the surface expansion after heating for each sheet-shaped test specimen. Surface expansion is the bulging described above. For each test specimen, the presence or absence of sheet expansion was evaluated after heating at a temperature of 250°C for 30 minutes. The specific method is described below. The average thickness of the test specimen before heating was calculated. The cross-section of the test specimen was observed using a micrometer, and the cross-section of the test specimen was divided into 11 equal parts in the width direction. After excluding the ends, the thickness was measured at 10 points at equal intervals, and the arithmetic mean of these thicknesses was taken as the average thickness. The average thickness of the test specimen after heating was calculated in the same manner as the test specimen before heating. In addition, the test specimen after heating was visually inspected to determine the presence or absence of bulging when compared to the surface of the test specimen before heating. When a bulge was visually confirmed, the cross-section including the bulge was observed using a microscope, and the thickness (t3) of the test specimen including the bulge (see FIG. 4) was measured. Surface expansion was defined as the case where the average thickness (t5) of the test specimen after heating was greater than 1.5 times the average thickness (t4) of the test specimen before heating, and the thickness (t3) of the test specimen including the bulge was greater than 1.5 times the average thickness (t4) of the test specimen before heating. The case where there was one or more bulges was evaluated as “C,” the case where there was less than one was evaluated as “B,” and the case where there were none was evaluated as “A.” Additionally, “sheet expansion” in Table 1 was evaluated as “A” when the average thickness (t5) of the test specimen after heating was 1.5 times or less the average thickness (t4) of the test specimen before heating, and “B” when it was greater than 1.5 times. In Table 1, the "bulge" refers to a case where the thickness (t3) of the test specimen including the bulge is greater than 1.5 times the average thickness (t4) of the test specimen before heating, and surface expansion is defined as such. A case with one or more bulges is evaluated as "B," and a case with less than one is evaluated as "A." The heating method of the test specimen is described below. First, a sample was obtained by cutting the test specimen to dimensions of 100 mm × 100 mm.At this time, sample specimens were taken from the center and both ends relative to the full width of the test specimen. The center refers to the portion located at half the length of the full width of the sheet, and both ends refer to portions located 50 mm away from the shortest portion of the full width of the sheet. A metal container with a PTFE (polytetrafluoroethylene) sheet lined on its inner bottom surface was placed in an electric furnace, and the temperature of the furnace was adjusted so that the temperature of the metal container reached 250 ± 2°C. Each cut test specimen was placed in the metal container and heated for 30 minutes. After the heat treatment was completed, the test specimens were removed from the metal container. After cooling the test specimens to room temperature, the condition of the surface of the test specimens was visually inspected.

[0106] (test)

[0107] Regarding the ratio of the total thickness of the skin layer (t1+t2) to the thickness (T) of the co-extruded sheet, in Examples 1 to 10, when the thickness ratio {(t1+t2) / T} is 0.10 to 0.5, an evaluation of “B” or higher can be obtained for any of the “non-bending elastic modulus,” “sheet expansion / bulging part,” and “presence or absence of fracture,” and an evaluation of “A” can be obtained for the “bulging part.” In particular, when the thickness ratio is 0.20 to 0.40 and the density of the test specimen is 0.4 to 0.9 g / cm³, an evaluation of “A” is obtained for the “non-bending elastic modulus” and “presence or absence of fracture.” That is, by controlling the thickness ratio {(t1+t2) / T} of the skin layer (3) and core layer (2) of the co-extruded sheet to 0.20 to 0.40 and controlling the density to 0.4 to 0.9 g / cm³, it was possible to improve lightness and mechanical strength. Regarding the evaluation of "sheet expansion," the proportion of "A" in Examples 1 to 10 was relatively high at 70% or more, indicating that "sheet expansion" could be relatively suppressed in Examples 1 to 10. Furthermore, by keeping the "sheet expansion" at 1.5 times or less, it can be assumed that the co-extruded sheet can obtain excellent appearance and aesthetic qualities after vacuum forming. Additionally, although the test specimen was heated at a temperature of 250°C in the above test, it can be assumed that the evaluation results of the "sheet expansion / bulging part" would be the same even if the test specimen were heated at a temperature of 200°C.

[0108] Next, regarding the MVR ratio of the resin in the skin layer (3) and core layer (2) of the test specimen, in Examples 1 to 7, when the MVR ratio was 1 to 5 times, an evaluation of "B" or higher was obtained for any of the "non-bending elastic modulus," "sheet expansion / bulging part," and "presence or absence of fracture." In particular, when the MVR ratio was 1.5 to 3 times, an evaluation of "A" was obtained for both the "sheet expansion / bulging part" and the "presence or absence of fracture." That is, when the MVR ratio of the resin contained in the skin layer (3) is 1.5 to 3 times, the irregular bubbles in the core layer (2) of the co-extruded sheet (1) tend to become uniform, thereby improving the secondary processing capability, such as vacuum forming of the co-extruded sheet (1). Furthermore, Examples 4 and 5 all obtained an evaluation of "A" for the "non-bending elastic modulus," "sheet expansion / bulging part," and "presence or absence of fracture." That is, it is desirable to have a thickness ratio of 0.20 or more and 0.40 or less, a density of the test specimen (sheet) of 0.6 g / cm³ or more and 0.8 g / cm³ or less, and an MVR ratio of 1.7 times or more and 2.7 times or less. In addition, although the test specimen was heated at a temperature of 250°C in the above test, it can be assumed that the evaluation results of the "sheet expansion / bulging part" would be the same even if the test specimen were heated at a temperature of 200°C.

[0109] In addition, regarding the foaming ratio of the test specimens of Examples 1 to 10, the specific bending modulus of the test specimen of Example 8, which had a foaming ratio of 1.57 times, was lower than that of the other examples. On the other hand, the foaming ratio of Comparative Example 5, which was manufactured by the same co-extrusion as the examples, was 3.42 times, and the specific bending modulus of Comparative Example 5 was 1.38, which was significantly lower. In addition, the test specimen of Comparative Example 6 showed relatively good results with a foaming ratio of 1.63 and a specific bending modulus of 2.00, but the lightness was inferior because the density was 0.96. Therefore, after considering the predetermined thickness ratio {(t1+t2) / T} and density of the co-extruded sheet, it can be considered that the foaming ratio of the co-extruded sheet should be 1.6 to 3.3 times in order to obtain excellent lightness and mechanical strength. In addition, according to the test specimen of Example 2, when the foaming ratio was 3.16 times, the specific bending modulus was 1.75 GPa·cm³ / g, showing a slight downward trend. Therefore, it can be considered more desirable to set the foaming ratio of the co-extruded sheet to 1.6 to 3.1 times.

[0110] In addition, when comparing the densities of Example 5 and Examples 8 to 10, in which the thickness ratio {(t1+t2) / T} is 0.37, relatively good results were obtained in Examples 5 and 9, in which the density is 0.82 g / cm³ or less, with a specific bending modulus of 2.00 GPa·cm³ / g or more, whereas in Examples 8 and 10, in which the density is 0.83 g / cm³ or more, the specific bending modulus decreased slightly. Therefore, although it is preferable to set the density of the co-extruded sheet to 0.4 to 0.9 g / cm³, by setting it to 0.82 g / cm³ or less, that is, 0.4 to 0.82 g / cm³, superior lightness and mechanical strength could be obtained.

[0111] Comparative Examples 1 to 3 are low-density polycarbonate laminated resin sheets using isopentane gas as a foaming agent. The density of the test specimens of Comparative Examples 1 to 3 was 0.1 to 0.11, which was less than 0.4. In addition, for the test specimens of Comparative Examples 1 to 3, the ratio of the thickness of the skin layer (t1+t2) to the thickness (T) of the test specimen was less than 0.10.

[0112] In Comparative Examples 1 to 3, the expansion ratio of the specimens increases because organic volatile isopentane gas is used as a blowing agent. Consequently, irregularities resulting from the bursting of bubbles become noticeable on the surface of the specimens after extrusion foam molding. Furthermore, because the shear rate during extrusion molding was set relatively high, the specimens are stretched significantly in the extrusion direction. As a result, the bubbles take on a flat shape that is greatly elongated in the extrusion direction. Due to these factors, when the specimens are heated in an atmosphere above the glass transition temperature of the polycarbonate resin, the bubbles within the specimens tend to shrink. It can be inferred that the dimensional change rate of Comparative Examples 1 to 3 increased due to the significant shrinkage in the extrusion direction. It can be inferred that such greatly elongated, flat bubbles further reduce the density of the specimens, thereby lowering the bending modulus of the specimens and making them prone to fracture. Generally, foamed molded articles made of polycarbonate resin are said to possess excellent lightness and mechanical strength. However, in the tests described above, excellent bending modulus and impact characteristics could not be obtained in the specimens of Comparative Examples 1 to 3. On the other hand, as described above, in the specimens of Examples 1 to 7, by considering the thickness of the skin layer (t1+t2) relative to the thickness (T) of the specimen and further setting the density of the specimen to 0.4 to 0.9 g / cm³, excellent lightness and mechanical strength could be obtained, and the appearance and aesthetics during heating under vacuum forming conditions could also be improved.

[0113] Comparative Example 4 is a sheet-shaped test specimen produced using the injection molding method. In the case of a test specimen produced by the injection molding method, a skin layer is formed on the surface of the test specimen due to the distribution of cooling rates within the mold. In Comparative Example 4, the evaluation of the "sheet expansion / bulging part" was "C," and the evaluation of the "sheet expansion" and "bulging part" was "B." Since the resin forming the skin layer of the test specimen produced by the injection molding method contains a foaming agent, it can be assumed that the foaming agent expands upon heating, causing relatively large and numerous bulging parts to form on the surface of the test specimen. Therefore, the molded body produced by the injection molding method and the co-extruded sheet are differentiated.

[0114] In Comparative Example 5, the evaluation of "non-bending elastic modulus" and "sheet expansion / bulging part" was "C," and the evaluation of "sheet expansion," "bulging part," and "presence or absence of fracture" was "B." In addition, Comparative Example 6 had relatively excellent mechanical strength and appearance when heated under vacuum forming conditions. However, since the density of Comparative Example 6 was greater than 0.9 g / cm³, it was not possible to achieve weight reduction. Explanation of the symbols

[0115] 1 : Co-extruded sheet 2 : Core layer 3: Skin layer 4: Skin layer 5: Artificial film 11: Swelling part T : Thickness t1 : thickness t2 : thickness t3 : thickness t4: Average thickness t5: Average thickness

Claims

Claim 1 A co-extruded sheet comprising a polycarbonate resin, the core layer made of a foamed resin, a first skin layer made of a non-foamed resin laminated on one side of the main surface of the core layer, and a second skin layer laminated on the other side of the main surface of the core layer, wherein the co-extruded sheet has a density of 0.4 to 0.9 g / cm³, the co-extruded sheet has a thickness of 1 to 5 mm, and also satisfies the following equation (1): 0.10 ≤ (t1 + t2) / T ≤ 0.5 ··· (1) (wherein t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet). The co-extruded sheet includes a bulging portion formed on the surface of the co-extruded sheet by heating under a heating atmosphere of 250°C for 30 minutes, and the co-extruded sheet including the bulging portion The thickness (t3) is 1.5 times or less of the average thickness (t4) of the co-extruded sheet before heating, and the co-extruded sheet after heating has less than 1 bulge per 100 cm² of its surface. Claim 2 A co-extruded sheet comprising a polycarbonate resin, the core layer made of a foamed resin, a first skin layer made of a non-foamed resin laminated on one side of the core layer, and a second skin layer laminated on the other side of the core layer, wherein the co-extruded sheet has a density of 0.4 to 0.9 g / cm³, the co-extruded sheet has a thickness of 1 to 5 mm, and also satisfies the following equation (1): 0.10 ≤ (t1 + t2) / T ≤ 0.5 ··· (1) (wherein t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet). When the co-extruded sheet is heated for 30 minutes in a heating atmosphere of 250°C, the average thickness (t5) of the co-extruded sheet after heating is relative to the average thickness (t4) of the co-extruded sheet before heating. Co-extruded sheet with a diameter of 1.5 times or less. Claim 3 A co-extruded sheet comprising a polycarbonate resin, the co-extruded sheet comprises a core layer made of a foamed resin, a first skin layer made of a non-foamed resin laminated on one side of the main surface of the core layer, and a second skin layer laminated on the other side of the main surface of the core layer, wherein the co-extruded sheet has a density of 0.4 to 0.9 g / cm³, the co-extruded sheet has a thickness of 1 to 5 mm, and also satisfies the following equation (1): 0.10 ≤ (t1 + t2) / T ≤ 0.5 ··· (1) (wherein t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the co-extruded sheet). The core layer has a foaming ratio of 1.6 to 3.3 times, and when the co-extruded sheet is heated for 30 minutes in a 200°C atmosphere, the co-extruded sheet is extruded in the extrusion direction and in a planar view. A co-extruded sheet having a dimensional change rate of -5 to 0% in at least one of the width directions perpendicular to the direction. Claim 4 A co-extruded sheet according to any one of claims 1 to 3, wherein the polycarbonate resin included in the first and second skin layers has a melt volume rate of 1.0 to 5 times with respect to the polycarbonate resin included in the core layer. Claim 5 A co-extruded sheet according to any one of claims 1 to 3, wherein the polycarbonate resin included in the first and second skin layers has a melt volume rate of 1.5 to 3 times with respect to the polycarbonate resin included in the core layer. Claim 6 In any one of claims 1 to 3, the co-extruded sheet is a co-extruded sheet having a density of 0.82 g / cm³ or less. Claim 7 A co-extruded sheet according to claim 1 or 2, wherein when the co-extruded sheet is heated in a 200°C atmosphere for 30 minutes, the co-extruded sheet has a dimensional change rate of -5 to 0% in at least one of the extrusion direction and the width direction orthogonal to the extrusion direction in a planar view. Claim 8 In any one of claims 1 to 3, the co-extruded sheet is a co-extruded sheet having a specific bending modulus of 1.5 GPa·cm³ / g or more. Claim 9 In any one of claims 1 to 3, the co-extruded sheet is a co-extruded sheet having a specific bending modulus of 2 GPa·cm³ / g or more. Claim 10 A co-extruded sheet according to any one of claims 1 to 3, wherein the co-extruded sheet further comprises a decorative film, and the decorative film is laminated on the outer surface of at least one of the first skin layer and the second skin layer.

Citation Information

Patent Citations

  • Foam molded article and method for producing the same

    KR1020200067184A

  • Foam composite sheets, adhesive tapes, cushioning materials for electronic components, and adhesive tapes for electronic components