Silicon wafer and epitaxial silicon wafer
By doping 300 mm silicon wafers with phosphorus and carbon, and employing argon annealing, the solution effectively reduces dislocation loop defects and SFs in the epitaxial layer, addressing the challenge of high defect densities in larger silicon wafers for power MOS transistors.
Patent Information
- Application Number
- KR1020250005972
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-21
- Filing Date
- 2025-01-15
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-11-02
AI Technical Summary
Existing silicon wafers with low resistivity, such as 0.9 mΩ·cm or less, experience high stacking fault (SF) densities during epitaxial growth due to dislocation loop defects, particularly in larger 300 mm wafers, which are not effectively addressed by prior methods optimized for smaller 200 mm wafers.
A silicon wafer with a diameter of 300 mm, doped with phosphorus for resistivity of 0.6 to 1.2 mΩ·cm, and incorporating controlled carbon concentrations of 3.5×10⁻⁶ to 5×10⁻¹⁷ atoms/cm³, combined with argon annealing to reduce dislocation loop defects, is used to minimize SFs in the epitaxial layer.
The solution significantly reduces dislocation loop defects and SFs in the epitaxial layer, ensuring low resistivity and improved gettering performance without increasing BMD density, thereby enhancing the quality and reliability of larger silicon wafers for power MOS transistors.
Smart Images

Figure 112025005587938-PAT00005_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to silicon wafers and epitaxial silicon wafers. Background Technology
[0002] Silicon wafers in epitaxial silicon wafers for power MOS transistors have low resistivity before forming the silicon epitaxial layer. These wafers are high-density doped with phosphorus and have a resistivity of 1.2 mΩ·cm or less.
[0003] In recent years, there has been a demand to provide n-type silicon wafers with extremely low resistivity of 0.9 mΩ·cm or less. However, when the resistivity of a silicon wafer is extremely low, stacking faults (SF) may occur in the silicon epitaxial layer when the epitaxial growth process is performed, and therefore, it is necessary to reduce the SF density in the silicon epitaxial layer.
[0004] As described in WO 2014 / 175120, the applicant of the present application has discovered a technique for suppressing the generation of SF in a silicon epitaxial layer (reducing the amount of time spent in the temperature range where SF nuclei are formed) by using a method of adjusting the residence time (thermal history) of a single crystal ingot at 570°C ± 70°C during the growth of a single crystal. In addition, as described in Japanese Patent Publication No. 2014-011293, it has been discovered that the generation of SF in a silicon epitaxial layer can be suppressed by using a method of performing high-temperature heat treatment (argon annealing) before growing the silicon epitaxial layer.
[0005] As described in WO 2014 / 175120, when a silicon wafer is cut from a crystal region having a shortened residence time in a temperature range where SF nuclei are formed (a silicon wafer with few SF nuclei), the SF density in the epitaxial layer can be reduced after growing the silicon epitaxial layer.
[0006] In addition, as described in Japanese Patent Publication No. 2014-011293, the SF density in the epitaxial layer after growing a silicon epitaxial layer can be reduced by performing argon annealing on a silicon wafer (a silicon wafer having many SF nuclei) that is cut from a crystal region having a long residence time in the temperature range where SF nuclei are formed. Although the prior art described in WO 2014 / 175120 and Japanese Patent Publication No. 2014-011293 is effective in suppressing the generation of SF in a silicon epitaxial layer, these publications describe low resistivity results obtained from a silicon wafer with a diameter of 200 mm. More recently, there has been an increasing demand for low-resistivity epitaxial silicon wafers of larger dimensions, such as 300 mm wafers.
[0007] The present invention provides a silicon wafer with a low density of dislocation loop defects that can cause SF, and an epitaxial silicon wafer with low occurrence of SF in the silicon epitaxial layer.
[0008] After active research into the causes of SF generation in silicon epitaxial layers, the inventors of the present invention discovered that a silicon wafer densely doped with phosphorus has two main types of dislocation loop defects (defects in which disturbed parts of the crystal lattice are connected in loops) depending on the thermal history the crystal undergoes during the growth process of a 300 mm single-crystal ingot.
[0009] The details leading to the discovery of dislocation loop-type defects are described below. First, a silicon single-crystal ingot with a diameter of 300 mm is grown in which phosphorus is added at high density as a dopant, and a silicon wafer is produced by cutting from a crystal region having a long residence time in the SF nucleation temperature range (hereinafter referred to as the residence time in the SF nucleation temperature range) and a silicon wafer is produced by cutting from a crystal region having a short residence time in the SF nucleation temperature range.
[0010] Specifically, a silicon wafer having a resistivity of 0.9 mΩ·cm is produced by cutting from the upper side of a straight body of a single-crystal ingot having a residence time of 1,000 minutes or more at 570°C±70°C as a silicon wafer having a long residence time in the SF₆ nucleation temperature range, and a silicon wafer having a resistivity of 0.7 mΩ·cm is produced by cutting from the lower side of a straight body of a single-crystal ingot having a residence time of 50 minutes or less at 570°C±70°C as a silicon wafer having a short residence time in the SF₆ nucleation temperature range. Each silicon wafer is cleaved in the thickness direction, and the cleavage cross-section is observed by a transmission electron microscope (TEM). The results are illustrated in FIGS. 1a and 1b.
[0011] As a result, in a silicon wafer cut from a crystal region (upper crystal region) having a long residence time in the SF nucleation temperature range, large complex dislocation loop defects (2) with overlapping dislocation loops are observed as shown in FIG. 1a, and it is confirmed that there is a high density of large defects with a size exceeding 60 nm. FIG. 1b is a photograph of the complex dislocation loop (2) shown in FIG. 1a taken from a different angle, showing that the complex dislocation loop (2) has a planar shape. Meanwhile, in a silicon wafer cut from a crystal region (lower crystal region) having a short residence time in the SF nucleation temperature range, small dislocation loop defects (4) shown in FIG. 2 are observed, and it is confirmed that there is a low density of large complex dislocation loop defects with a size exceeding 60 nm.
[0012] In addition, it is confirmed that SF occurs in the silicon epitaxial layer originating from large complex dislocation loop defects. Since this suggests that the conditions for SF generation in the silicon epitaxial layer vary depending on the presence or absence of complex dislocation loop defects, the inventors of the present invention have reached the following conclusions by considering the mechanisms that generate dislocation loops.
[0013] The inventors of the present invention made the following assumptions regarding the occurrence of dislocation loop defects. First, during the cooling stage of a silicon single-crystal ingot, interstitial phosphorus present between the lattices within the crystal expels lattice silicon present at lattice positions (driving out lattice silicon), thereby generating interstitial silicon. The generated excess interstitial silicon aggregates to form dislocation loops and separates the interstitial phosphorus from the dislocation loops, causing dislocation loop defects.
[0014] In addition, since it is effective to suppress the aggregation of interstitial silicon to suppress the occurrence of dislocation loop defects, the inventors of the present invention believed that the aggregation of interstitial silicon could be suppressed by intentionally adding an impurity element that can pair with interstitial silicon, and devised the idea of incorporating carbon into the crystal during the single crystal growth stage. When a silicon single crystal ingot is grown by doping (adding) carbon into a silicon melt and the defects formed inside the carbon-doped silicon wafer are evaluated, the inventors of the present invention reached the conclusion that the defect density of large dislocation loops formed inside the silicon wafer is reduced, thereby completing the present invention.
[0015] Meanwhile, Japanese unexamined patent publication No. 2003-505324 describes a method for improving the gettering performance of an epitaxial silicon wafer by adding carbon to the silicon wafer to increase the density of oxygen precipitates (Bulk Micro Defects (BMDs)) formed inside the wafer. Specifically, the invention described in Japanese unexamined patent publication No. 2003-505324 is a technique that attempts to resolve the decrease in gettering performance caused by a decrease in oxygen concentration during the later stages of single-crystal ingot growth by adding carbon. Increasing the BMD density by adding carbon to the silicon crystal to provide an epitaxial wafer with excellent gettering performance is well known beyond Japanese unexamined patent publication No. 2003-505324.
[0016] Generally, it is known that regions containing a high concentration of phosphorus in a silicon wafer act as a getter layer through phosphorus thermal diffusion treatment, phosphorus ion implantation treatment, or the formation of a phosphorus-containing epitaxial layer (also referred to as the phosphorus gettering method). In other words, only the silicon wafer of the present invention, which is doped with phosphorus at a high density to maintain a resistivity of 1.2 mΩ·cm or less, possesses sufficient gettering characteristics due to the presence of a high concentration of phosphorus. Therefore, there is no need to increase the BMD density for the epitaxial wafer of the present invention. Consequently, there is no incentive to add carbon to the silicon wafer of the present invention, which is doped with phosphorus at a high density, in order to improve gettering performance by increasing the BMD density. Furthermore, Japanese unexamined patent publication No. 2003-505324 does not discuss the specific problem of frequent occurrence of SF in a silicon wafer doped with phosphorus at a high density to maintain a substrate resistivity of 1.2 mΩ·cm or less.
[0017] The silicon wafer according to the present invention has a diameter of 300 mm, a dopant of phosphorus, a resistivity of 0.6 mΩ·cm to 1.2 mΩ·cm, and a carbon concentration of 3.5×10⁻⁶ 15 atoms / cm 3 Up to 5×10 17 atoms / cm 3 am.
[0018] The resistivity of a silicon wafer defined by the present invention is a value obtained by measuring the surface of the silicon wafer using a four-point probe method. The carbon concentration of a silicon wafer defined by the present invention is a value obtained by thinning the silicon wafer by polishing and measuring the carbon concentration near the center of the silicon wafer (center-depth position) in the depth direction using a secondary ion mass spectrometer (SIMS). Since it is difficult to accurately measure the carbon concentration on the outermost surface of the silicon wafer due to a large number of noise components, accurate measurement of the carbon concentration is possible when the measurement is performed at a depth of 1 μm or more from the wafer surface to exclude the outermost surface. In the present invention, to obtain a more accurate value, the concentration is defined by the concentration near the center of the silicon wafer in the depth direction.
[0019] In the case of the silicon wafer mentioned above, the oxygen concentration of the silicon wafer is 4.0 × 10⁻⁶ 17 atoms / cm 3 From 10×10 or more 17 atoms / cm 3 The following may be true. The oxygen concentration of a silicon wafer defined by the present invention is a value obtained by thinning the silicon wafer by polishing and then measuring the oxygen concentration near the center of the silicon wafer in the depth direction using SIMS. Since it is difficult to accurately measure the oxygen concentration of the outermost surface of the silicon wafer due to a large number of noise components, accurate measurement of the oxygen concentration is possible when the measurement is performed at a depth of 1 μm or more from the wafer surface to exclude the outermost surface. In the present invention, to obtain a more accurate value, the concentration is defined by the concentration near the center of the silicon wafer in the depth direction.
[0020] Preferably, the silicon wafer mentioned above is substantially free of COPs. In the present invention, "substantially free of COPs" means a silicon wafer in which no COPs are detected by the observation evaluation described below. Specifically, SC-1 cleaning (cleaning using a liquid mixture of ammonia water, hydrogen peroxide, and ultrapure water in a ratio of 1:1:15) is first performed on a silicon wafer cut from a single-crystal silicon ingot grown and processed using the CZ method, and an observation evaluation of the surface of the silicon wafer after cleaning is performed using a SURFSCAN SP-2 manufactured by KLA-Tencor Corporation as a surface defect inspection device, and a light point defect (LPD) presumed to be a surface pit is identified. At that time, the observation mode is set to oblique mode (oblique incidence mode), and the estimation of the surface pit is performed based on the size ratio of the detected wide channel / narrow channel. The LPD specified in this manner is evaluated for the presence of COPs using an Atomic Force Microscope (AFM). In this observational evaluation, a silicon wafer in which no COPs are observed is referred to as a "silicon wafer with no COPs."
[0021] The epitaxial silicon wafer according to the present invention has a diameter of 300 mm, a dopant of phosphorus, a resistivity of 0.6 mΩ·cm to 1.2 mΩ·cm, and a carbon concentration of 3.5×10⁻⁶ 15 atoms / cm 3 Up to 5×10 17 atoms / cm 3 It includes a silicon wafer; and a silicon epitaxial layer on the surface of the silicon wafer.
[0022] The resistivity of the silicon wafer of the epitaxial silicon wafer defined by the present invention is a value obtained by measuring the backside of the silicon wafer using the four-point probe method. In addition, if an oxide film is provided on the backside of the epitaxial silicon wafer, the value is obtained by measuring the backside of the silicon wafer from which the backside oxide film is removed using the four-point probe method. The carbon concentration of the silicon wafer of the epitaxial silicon wafer defined by the present invention is a value obtained by thinning the silicon wafer by polishing and measuring the carbon concentration near the center of the silicon wafer in the depth direction using SIMS.
[0023] When producing an epitaxial silicon wafer, the silicon wafer undergoes high-temperature heat treatment prior to the epitaxial growth process, etc., which causes carbon to diffuse outward and reduce the carbon concentration in the surface layer of the silicon wafer. Therefore, the carbon concentration of the silicon wafer in the epitaxial silicon wafer needs to be measured at a depth where there is no external diffusion of carbon, and accurate measurement of the carbon concentration is possible when measured at a depth of 40 μm or more in the depth direction of the wafer thickness from the wafer surface. In the present invention, to obtain a more accurate value, the concentration is defined by the concentration near the center of the silicon wafer in the depth direction.
[0024] The epitaxial silicon wafer according to the present invention has a diameter of 300 mm, a dopant of phosphorus, a resistivity of 0.6 mΩ·cm to 1.2 mΩ·cm, and a carbon concentration of 3.5×10⁻⁶ 15 atoms / cm 3 Up to 5×10 17 atoms / cm 3The silicon wafer comprises; and a silicon epitaxial layer on the surface of the silicon wafer, wherein the silicon wafer has a low carbon concentration layer on the surface side in contact with the silicon epitaxial layer, the carbon concentration of the low carbon concentration layer is at most 0.9 times the carbon concentration near the center of the silicon wafer in the depth direction, and the depth of the low carbon concentration layer is 5 μm or more and 15 μm or less from the surface of the silicon wafer. That is, the carbon concentration is reduced by at least 10% starting from a depth of the silicon substrate of about 5 μm from the boundary, in the depth direction of the silicon wafer, compared to the carbon concentration at approximately the center. In another embodiment, the carbon concentration is reduced by at least 10% starting from a depth of the silicon substrate of anywhere from 5 μm to 15 μm from the boundary, in the depth direction of the silicon wafer, compared to the carbon concentration at approximately the center.
[0025] The depth of the low carbon concentration layer is a value based on the carbon concentration profile in the depth direction obtained by SIMS measurement, and refers to the depth position (width) in the depth direction of the silicon wafer from the interface between the epitaxial layer and the silicon wafer.
[0026] In an epitaxial silicon wafer, the resistivity of the silicon wafer is preferably 1.0 mΩ·cm or less.
[0027] In an epitaxial silicon wafer, the carbon concentration of the silicon wafer is preferably 1×10 16 atoms / cm 3 That is all.
[0028] In an epitaxial silicon wafer, the oxygen concentration of the silicon wafer is preferably 4.0 × 10⁻⁶ 17 atoms / cm 3 10×10 17 atoms / cm 3 It is as follows.
[0029] The oxygen concentration of the silicon wafer in an epitaxial silicon wafer defined by the present invention is a value obtained by thinning the silicon wafer by polishing and then measuring the oxygen concentration near the center of the silicon wafer in the depth direction using SIMS. The oxygen concentration of the silicon wafer in an epitaxial silicon wafer needs to be measured at a depth location where there is no external oxygen diffusion, and accurate measurement of the oxygen concentration is possible when measured at a depth location of 150 μm or more in the depth direction of the wafer thickness from the wafer surface. In the present invention, to obtain a more accurate value, the concentration is defined by the concentration near the center of the silicon wafer in the depth direction.
[0030] In an epitaxial silicon wafer, preferably, COPs are not present in the silicon wafer.
[0031] In an epitaxial silicon wafer, an oxide film is preferably provided on the back side of the silicon wafer.
[0032] In an epitaxial silicon wafer, preferably, no oxide film exists on the outer periphery of the ends and back surfaces of the silicon wafer.
[0033] In an epitaxial silicon wafer, the density of LPDs with a size of 0.09 μm or larger observed on the surface of the epitaxial layer is preferably 130 or fewer defects per wafer.
[0034] In an epitaxial silicon wafer, the density of LPDs with a size of 0.09 μm or larger observed on the surface of the epitaxial layer is preferably 100 or fewer defects per wafer. Brief explanation of the drawing
[0035] The present invention is further described in the following detailed description with reference to a plurality of drawings mentioned as non-limiting examples of exemplary embodiments of the present invention, in which like reference numerals indicate similar parts throughout various views of the drawings. Figures 1a and 1b are photographs of complex dislocation loops observed in a silicon wafer cut from a crystal region having a long residence time in the SF nucleation temperature range. Figure 2 is a photograph of a dislocation loop observed in a silicon wafer cut from a crystal region having a short residence time in the SF nucleation temperature range. FIG. 3 is a flowchart illustrating an example of a method for manufacturing an epitaxial silicon wafer according to the present invention. FIGS. 4a and FIGS. 4b are cross-sectional views of an embodiment of an epitaxial silicon wafer according to the present invention. FIGS. 5A and 5B are graphs illustrating the evaluation results for dislocation loops in epitaxial silicon wafers of Example 1 and Comparative Example 1. Figure 6 is a graph illustrating the results of a study on the carbon concentration profiles of epitaxial silicon wafers of Examples 4 and 5. FIGS. 7a to 7d are X-ray topography images of the surfaces of silicon wafers of Examples 6 and 7 and Comparative Examples 4 and 5. Figure 8 is a graph illustrating the relationship between LPD density and resistivity when an epitaxial layer is formed on the surface of each silicon wafer in Examples 8 and 9 and Comparative Examples 6 and 7. Specific details for implementing the invention
[0036] The details set forth in this specification are illustrative and are intended solely for the purpose of illustrative discussion of embodiments of the invention, and are presented to provide what is considered to be the most useful and easily understandable description of the principles and conceptual aspects of the invention. In this regard, there is no attempt to show the structural details of the invention in more detail than is necessary for a basic understanding of the invention, and the description taken together with the drawings makes it clear to those skilled in the art how the forms of the invention can actually be implemented.
[0037] Hereinafter, embodiments of the present invention will be described with reference to the drawings. A silicon wafer according to the present invention has a diameter of 300 mm, is doped with phosphorus, a dopant for adjusting resistivity, has a resistivity of 0.6 mΩ·cm or more and 1.2 mΩ·cm or less, and 3.5×10 15 atoms / cm 3 Up to 5×10 17 atoms / cm 3 It has a carbon concentration of . A silicon wafer having a diameter of 300 mm as defined by the present invention refers to a silicon wafer having a diameter of 300 ± 0.5 mm due to processing errors, etc. In addition, the epitaxial silicon wafer according to the present invention includes a silicon epitaxial layer on the silicon wafer.
[0038] A preferred manufacturing flow for obtaining an epitaxial silicon wafer according to the present invention is illustrated in FIG. 3. This manufacturing flow preferably includes the steps of manufacturing a single crystal ingot (S1), forming an oxide film on the back side (S2), removing the oxide film from the outer periphery (S3), argon annealing (S4), prebaking (S5), and forming an epitaxial layer (S6).
[0039] In the single-crystal ingot manufacturing step (S1), a 300 mm-diameter single-crystal silicon ingot doped with phosphorus as an n-type dopant is manufactured according to the Czochralski (CZ) method using a single-crystal ingot pulling device (not shown), satisfying the following conditions.
[0040] Phosphorus concentration The phosphorus concentration in the single-crystal ingot is 6.0×10 19 atoms / cm 3 1.32×10⁻⁶ 20 atoms / cm 3 By doping with red phosphorus to a value below 0.6 mΩ·cm, a single-crystal ingot having a resistivity of 0.6 mΩ·cm or higher and 1.2 mΩ·cm or lower can be obtained. Wafers of larger dimensions, such as 300 mm wafers, are prone to having more dislocation defects. Furthermore, lowering the resistivity tends to increase the SF density in the wafer. Therefore, for these larger wafers, it is important to reach a specific balance, and a resistivity in the range of 8.0 mΩ·cm to 1.0 mΩ·cm has been determined to be desirable. Preferably, the phosphorus concentration is 8.3 × 10⁻⁶ 19 atoms / cm 3 This concludes the explanation. The phosphorus concentration of the silicon wafer is a value obtained by measuring the phosphorus concentration near the center of the silicon wafer in the depth direction using SIMS. Phosphorus concentration can be determined from the resistivity measured by the four-point probe method using the formula or graph specified by SEMI MF723-0307. If phosphorus is doped before melting the silicon raw material, the phosphorus may evaporate during the melting of the silicon raw material, making it impossible to obtain the desired resistivity. Therefore, it is preferable to dope the silicon melt with red phosphorus after the silicon raw material has been melted.
[0041] carbon concentration Carbon powder is added to a crucible containing silicon raw material, and the carbon concentration in the single-crystal ingot is 3.5×10 15atoms / cm 3 5.0×10 17 atoms / cm 3 By melting the material to a value below 3.5×10, a single-crystal ingot having a predetermined carbon concentration can be grown. The carbon concentration is 3.5×10 15 atoms / cm 3 By setting it to be greater than or equal to this, the size and density of dislocation loop defects formed inside the silicon wafer can be reduced, and the SF density generated in the epitaxial layer after the epitaxial growth process can be significantly reduced. Preferably, the carbon concentration in the silicon wafer of the present invention is 1×10⁻⁶ 16 atoms / cm 3 The above is the case, and more preferably, the carbon concentration is 3×10 16 atoms / cm 3 That is all.
[0042] On the other hand, the carbon concentration is 5.0×10 17 atoms / cm 3 If it exceeds, the likelihood of dislocations occurring in the single crystal during the single-crystal ingot growth process increases, making it difficult to grow a dislocation-free single-crystal ingot. From the perspective of stabilizing the manufacture of single-crystal ingots, the carbon concentration is more preferably 3.0 × 10⁻⁶. 17 atoms / cm 3 It is as follows.
[0043] Oxygen concentration As mentioned below, if the oxygen concentration of the silicon wafer is high, the device breakdown voltage characteristics tend to deteriorate; therefore, it is desirable to maintain a low oxygen concentration in the single-crystal ingot, and the oxygen concentration is preferably 4.0 × 10⁻⁶. 17 atoms / cm 3 10×10 17 atoms / cm 3 It is within the following range.
[0044] To grow a single-crystal ingot with a low oxygen concentration, it is desirable to apply a magnetic field to the silicon melt, and a well-known horizontal magnetic field or cusp magnetic field may be applied. The oxygen concentration incorporated into the single crystal can be reduced to a desired concentration by slowing down the rotation speed of the crucible storing the silicon melt and by lowering the furnace pressure of the pulling device, etc. The oxygen concentration is 4.0 × 10⁻⁶ 17 atoms / cm 3 If it is less than that, the silicon wafer has low strength, and slip dislocations may occur when the silicon wafer undergoes high-temperature heat treatment. Therefore, the oxygen concentration is preferably 4.0 × 10⁻⁶. 17 atoms / cm 3 That is all.
[0045] Subsequently, a silicon wafer is cut from a single crystal ingot manufactured using the single crystal ingot manufacturing step (S1), and a predetermined process (e.g., grinding, etching, and polishing process) is performed to produce a mirror surface silicon wafer having excellent surface roughness and flatness.
[0046] In the back oxide film formation step (S2), preferably, an oxide film (hereinafter referred to as the back oxide film) is formed on the back side of a silicon wafer using a CVD device within the following condition ranges. Source gas: A mixed gas of monosilane (SiH4) and oxygen (O2) Thickness of back oxide film: 100 nm to 1500 nm Tabernacle temperature: 400℃ to 450℃ Providing this type of back oxide film can suppress auto-doping and suppress resistance fluctuations in the epitaxial layer.
[0047] In the back oxide film formation step (S2), it is difficult to form an oxide film only on the back side of the silicon wafer, and an oxide film formed on the end (chamfered portion) of the silicon wafer after the back oxide film formation step (S2) may be unavoidable. If an epitaxial layer is formed on the surface of the oxide film, nodules (grainy silicon) may appear in the corresponding area, so it is desirable to remove the oxide film formed on the end and the outer periphery of the back side of the silicon wafer.
[0048] Accordingly, in the outer oxide film removal step (S3), the oxide film present on the outer periphery of the back side of the wafer and on the end (chamfered portion) of the silicon wafer can be removed using various methods such as polishing and etching. The oxide film present on the outer periphery of the back side of the wafer is preferably removed over an area of less than 5 mm from the outer edge of the silicon wafer. By removing the end of the silicon wafer and the outer periphery of the back side oxide film in this way, the occurrence of lumps during the growth of the silicon epitaxial layer and the occurrence of particles from the wafer edge can be prevented.
[0049] In the argon annealing step (S4), heat treatment is preferably performed within the following condition ranges. Gas Atmosphere: Argon Gas Heat treatment temperature: 1150℃ to 1250℃ Heat treatment time: 30 to 120 minutes Preferably, a batch furnace (vertical heat treatment device) capable of heat-treating multiple silicon wafers at once is used as a heat treatment device for performing heat treatment.
[0050] By high-concentration carbon doping, the occurrence of large dislocation loop defects in silicon wafers can be suppressed, and by performing argon annealing on silicon wafers, small dislocation loop defects present on silicon wafers can be removed, and the occurrence of SF in epitaxial layers can be reduced as much as possible.
[0051] Additionally, by performing argon annealing on the silicon wafer prior to the epitaxial growth process, carbon diffusion from the silicon wafer to the silicon epitaxial layer occurring during the epitaxial layer formation step (S6) can be reduced. This advantage is described below. FIG. 4a is a schematic diagram illustrating a low-carbon concentration layer formed on the surface layer of a silicon wafer by argon annealing. As shown in FIG. 4a, by performing high-temperature argon annealing on the silicon wafer (11), carbon in the surface layer of the silicon wafer (11) diffuses outward, thereby reducing the carbon concentration of the surface layer. Accordingly, a low-carbon concentration layer (12) is formed on the front and back surfaces of the silicon wafer (11), and this low-carbon concentration layer (12) has a carbon concentration lower than the carbon concentration near the center (C) of the silicon wafer (11) where carbon diffusion outward does not occur.
[0052] FIG. 4b is a schematic diagram illustrating the carbon concentration profile when an epitaxial growth process is performed on a silicon wafer that has undergone argon annealing. As illustrated in FIG. 4b, the carbon concentration after the epitaxial layer formation step (S6) shows a concentration profile in which the carbon concentration in the surface layer of the silicon wafer is reduced. Here, when the region is defined as a low-carbon concentration layer (12) having a carbon concentration 0.9 times or less than the center (C) of the silicon wafer (11) where carbon external diffusion does not occur, the depth (D) of the low-carbon concentration layer (12) formed on the surface of the silicon wafer (11) in contact with the silicon epitaxial layer (13) after the epitaxial growth process may be 5 μm or more and 15 μm or less. That is, the carbon concentration is reduced by more than 10% starting from a depth of the silicon substrate of about 5 μm from the boundary in the depth direction of the silicon wafer compared to the carbon concentration at approximately the center. In another embodiment, the carbon concentration is reduced by more than 10% starting from a depth of the silicon substrate of anywhere from 5 μm to 15 μm from the boundary in the depth direction of the silicon wafer compared to the carbon concentration at approximately the center. By forming a low-carbon concentration layer (12), carbon diffusion from the silicon wafer (11) to the silicon epitaxial layer (13) that occurs during the epitaxial layer formation step (S6) can be further reduced. The thickness of the low-carbon concentration layer (12) can be adjusted as desired by adjusting the heat treatment temperature and time of argon annealing.
[0053] In the prebaking step (S5) in an atmosphere of gases including hydrogen and hydrogen chloride, heat treatment is preferably performed on a silicon wafer in an internal epitaxial device (CENTURA® manufactured by Applied Materials, Inc.) within the following condition ranges. Atmosphere: Hydrogen gas, hydrogen chloride gas Hydrogen gas flow rate: 40L / min Hydrogen chloride gas flow rate: 1L / min Heat treatment temperature: 1150℃ to 1250℃ Heat treatment time: 30 to 300 seconds
[0054] The margin of the surface layer of the silicon wafer obtained as a result of the prebaking step (S5) is preferably 100 nm to 300 nm, more preferably 150 nm ± 10 nm.
[0055] In the epitaxial layer formation step (S6), an epitaxial layer is grown on a silicon wafer that has undergone the prebaking step (S5), preferably within the following ranges of conditions. Dopant gas: Phosphine (PH3) gas Source gas: Trichlorosilane (SiHCl3) gas Carrier gas: Hydrogen gas Growth temperature: 1050℃ to 1150℃ Epitaxial layer thickness: 1㎛ to 10㎛ Epitaxial layer resistivity: 0.01 mΩ·cm to 10 mΩ·cm Phosphorus concentration: 4.44×10⁻⁶ 14 atoms / cm 3 Up to 4.53×10 18 atoms / cm 3 By performing the epitaxial layer formation step (S6), an epitaxial silicon wafer is manufactured in which a silicon epitaxial layer is formed on the surface of the silicon wafer.
[0056] By performing the process flow described above, it is possible to provide a silicon wafer capable of reducing the generation of SF in the epitaxial layer and to provide an epitaxial silicon wafer in which the SF density in the epitaxial layer is reduced. Specifically, a new silicon wafer that did not previously exist is provided, wherein the silicon wafer has a diameter of 300 mm and is phosphorus-added such that its resistivity is 0.6 mΩ·cm to 1.2 mΩ·cm, and the silicon wafer has a carbon concentration of 3.5 × 10⁻⁶ 15 atoms / cm 3 Up to 5×10 17 atoms / cm 3 Carbon is doped at a high density to achieve this.
[0057] Through high-concentration carbon doping, the density of large dislocation loop defects in silicon wafers is reduced. This silicon wafer effectively functions as a bulk wafer for epitaxial growth, capable of reducing the occurrence of epitaxial defects (LPDs or SFs observed on the surface of the epitaxial layer).
[0058] Furthermore, the oxygen concentration of the silicon wafer is 4.0×10 17 atoms / cm 3 Up to 10×10 17 atoms / cm 3 By configuring it to be within the range, poor device internal pressure can be prevented when carbon is doped.
[0059] In addition, by performing argon annealing on the silicon wafer before forming the silicon epitaxial layer, the carbon concentration of the surface layer of the silicon wafer can be reduced, and the amount of carbon diffusion into the silicon epitaxial layer that occurs during the formation of the silicon epitaxial layer can be reduced. By reducing the amount of carbon diffusion into the silicon epitaxial layer, the deterioration of electrical characteristics caused by the occurrence of defects by carbon incorporated into the silicon epitaxial layer can be suppressed during heat treatment in the device process in which a device is manufactured on the epitaxial silicon wafer.
[0060] In the above-mentioned embodiment, the resistivity of the silicon wafer is 0.6 mΩ·cm to 1.2 mΩ·cm. However, as a silicon wafer having better resistivity, the resistivity is preferably 1.0 mΩ·cm or less. As the resistivity decreases, the generation of SF in the epitaxial layer becomes more pronounced, so the effect of carbon doping according to the present invention is more distinct.
[0061] In addition, the silicon wafer according to the present embodiment is manufactured from a single-crystal ingot grown from a silicon melt doped with phosphorus such that the resistivity is 1.2 mΩ·cm or less. Because phosphorus is added at a high density, the OSF ring region, where oxidation-induced stacking faults (OSF) occur during the process of manufacturing the single-crystal ingot, is removed around the ingot, resulting in a crystal region free of COPs. In other words, the silicon wafer according to the present embodiment can be configured as a silicon wafer free of COPs by adding phosphorus at a high density, thereby preventing the occurrence of defects caused by COPs in the epitaxial layer. Examples
[0062] Hereinafter, the experimental conditions and evaluation results of the examples and comparative examples of the present invention are described. <Position Loop Evaluation> Potential loops are evaluated for the following Example 1 and Comparative Example 1. <Example 1> In Example 1, an epitaxial silicon wafer is manufactured within the range of conditions of the manufacturing flow of the epitaxial silicon wafer described with reference to FIG. 3. The growth conditions of the single-crystal ingot are to manufacture the single-crystal ingot by adding carbon powder before melting the silicon raw material so that the resistivity of the upper part of the straight section of the single-crystal ingot becomes 1.0 mΩ·cm, and by adding phosphorus to the silicon melt after melting the silicon raw material. A sample wafer is cut from the position of the ingot on the upper side of the straight section of the carbon-added single-crystal ingot, and a mirror-finish silicon wafer is manufactured by performing a predetermined treatment. When measured by the four-point probe method, the resistivity of the silicon wafer is 0.9 mΩ·cm, and the carbon concentration of the silicon wafer is 1.0 × 10⁻⁶ 16 atoms / cm 3 am.
[0063] <Comparative Example 1> Compared to Example 1 above, a silicon wafer is manufactured under the same manufacturing conditions as in Example 1, except that carbon doping is not performed during the step of growing a single crystal ingot. Similar to Example 1, a sample wafer having a resistivity of 0.9 mΩ·cm is cut, and a mirror-finish silicon wafer is produced by performing a predetermined treatment.
[0064] The silicon wafers of Example 1 and Comparative Example 1 are cleaved in the depth direction, and the cleavage cross-sections are observed by transmission electron microscopy (TEM). Figures 5a and 5b are graphs illustrating the evaluation results for dislocation loops in the silicon wafers of Example 1 and Comparative Example 1. In Figures 5a and 5b, the horizontal axis represents the dislocation loop size, and the vertical axis represents the dislocation loop density. Figure 5a shows the results for the silicon wafer of Comparative Example 1, which is not doped with carbon, and a large number of large dislocation loops with a size exceeding 60 nm were observed because a sample wafer cut from the top side of the crystal having a long residence time in the SF nucleation temperature range was used. Meanwhile, Figure 5b shows the results for the silicon wafer of Example 1, which is doped with carbon at high density. Since a sample wafer cut from the top side of the crystal having a long residence time in the SF nucleation temperature range is used, a large number of small dislocation loops are observed, but it is confirmed that the density of large dislocation loops exceeding 60 nm is significantly reduced. In other words, it is confirmed that the density of large dislocation loops formed on the silicon wafer is reduced by carbon doping.
[0065] [LPD Density Evaluation] When a silicon epitaxial layer is formed using a sample silicon wafer cut from the upper side of a straight body of an ingot having a long residence time in the temperature range where SF nuclei are formed, SF is frequently generated in the epitaxial layer and the LPD density increases. Therefore, in this example, sample silicon wafers for Examples 2 and 3 and Comparative Examples 2 and 3 below, which are cut from the upper side of a straight body, are produced, and the LPD density observed on the surface of the epitaxial layer after the formation of the epitaxial layer is measured.
[0066] The specific conditions for the back oxide film formation step and the epitaxial layer formation step, which are performed as a common process in both the examples and comparative examples, are as follows. [Conditions for Backside Oxide Formation] Under the following conditions, a back oxide film is formed on the back side (the surface opposite to the surface where the epitaxial layer is formed) of each silicon wafer. Source gas: A mixed gas of monosilane (SiH4) and oxygen (O2) Tabernacle Law: CVD Law Tabernacle temperature: 400℃ Thickness of back oxide film: 550 nm The oxide film present on the outer periphery and chamfered portions on the back side of each silicon wafer is removed by an etching process. [Hydrogen Baking Treatment Conditions] Atmosphere: Hydrogen gas Heat treatment temperature: 1200℃ Heat treatment time: 30 seconds [Epitaxial membrane growth conditions] Dopant gas: Phosphine (PH3) gas Source gas: Trichlorosilane (SiHCl3) gas Carrier gas: Hydrogen gas Growth temperature: 1080℃ Epitaxial layer thickness: 4㎛ Resistivity (Epitaxial film resistivity): 0.3 Ω·cm
[0067] <Comparative Example 2> An epitaxial silicon wafer is manufactured without carbon doping by forming a silicon epitaxial layer with a thickness of 4 μm on the surface of the silicon wafer of Comparative Example 1, in which a large number of dislocation loops are observed.
[0068] <Comparative Example 3> An epitaxial silicon wafer is manufactured by performing argon annealing (heat treatment at 1200°C for 30 minutes in an argon gas atmosphere) on the silicon wafer of Comparative Example 1, and then forming a silicon epitaxial layer having a thickness of 4 μm on the surface of the silicon wafer.
[0069] <Example 2> By forming a silicon epitaxial layer with a thickness of 4 μm on the surface of a silicon wafer, an epitaxial silicon wafer is manufactured without performing argon annealing on the silicon wafer of Example 1 in which carbon doping was performed.
[0070] <Example 3> An epitaxial silicon wafer is manufactured by performing argon annealing (heat treatment at 1200°C for 30 minutes in an argon gas atmosphere) on the silicon wafer of Example 1, which has been carbon-doped, and then forming a silicon epitaxial layer having a thickness of 4 μm on the surface of the silicon wafer. The conditions of the epitaxial growth process are the same for Examples 2 and 3 and Comparative Examples 2 and 3.
[0071] The LPD density on the surface of the silicon epitaxial layer of the epitaxial silicon wafer of Comparative Example 2 is measured using a surface defect inspection device (SURFSCAN SP-1 manufactured by KLA-Tencor Corporation). Specifically, the measurement is performed in normal mode (DCN mode), and the density of LPDs with a size of 90 nm or larger observed on the surface of the epitaxial layer is measured. The measurement area is the surface of the epitaxial layer excluding a ring-shaped area from the circumferential edge of the epitaxial silicon wafer up to 3 mm radially from the circumferential edge. The number of counted LPDs can be considered as the number of SFs. As a result, the measurement of the LPDs themselves cannot be performed due to an overflow caused by too many detected numbers (more than 100,000 defects per wafer). In Comparative Example 3, where argon annealing is performed on the silicon wafer, 1,055 LPDs per wafer are observed, although the LPD density may be reduced compared to Comparative Example 2. The following LPD density measurements for each example and each comparative example are performed under the same conditions as in Comparative Example 2.
[0072] When the LPD density on the surface of the silicon epitaxial layer of the epitaxial silicon wafer in Example 2 was measured, the LPD measurement itself could not be performed due to an overflow caused by too many detected defects (the number of defects per wafer was greater than 100,000). This is presumed to be because, although the density of large complex dislocation loops in the silicon wafer is reduced by carbon doping, a large number of small dislocation loops with a size of less than 60 nm are presented.
[0073] In Example 3, where argon annealing is performed on the silicon wafer before the epitaxial growth process, the LPD density on the surface of the epitaxial layer is significantly reduced, and an LPD density of 108 defects per wafer is observed. This is thought to be because small dislocation loops with a size of less than 60 nm present on the surface layer of the silicon wafer are removed by argon annealing.
[0074] Considering the above, it is evident that when carbon is doped into a silicon wafer and argon annealing is performed, the effect of reducing the generation of SF in the silicon epitaxial layer is enhanced, and the LPD density after the formation of the epitaxial layer can be reduced to about one-tenth compared to Comparative Example 3.
[0075] [Carbon Concentration Profile Evaluation] When carbon is doped at a high density, carbon diffusion into the silicon epitaxial layer may occur due to heat treatment during the formation of the silicon epitaxial layer, so the behavior of carbon diffusion into the silicon epitaxial wafer is evaluated. <Example 4> Silicon wafer with high carbon concentration (carbon concentration near the center of the wafer in the depth direction: 3.8×10⁻⁶ 16 atoms / cm 3 ) is prepared, and an epitaxial silicon wafer is manufactured with a silicon epitaxial layer similar to Example 2 formed without performing argon annealing. <Example 5> After performing the same argon annealing as in Example 3 on a silicon wafer similar to Example 4, an epitaxial silicon wafer with a silicon epitaxial layer formed is manufactured.
[0076] Figure 6 is a graph illustrating the results of a study on carbon concentration profiles measured by a secondary ion mass spectrometer for the epitaxial silicon wafers of Examples 4 and 5. The horizontal axis of Figure 6 represents the depth from the surface of the epitaxial silicon wafer, and the vertical axis represents the carbon concentration. There is an interface between the silicon epitaxial layer and the silicon wafer at a depth of 4 μm from the surface of the epitaxial silicon wafer.
[0077] In Example 4, where argon annealing is not performed on the silicon wafer, the width of the low-carbon concentration layer is less than 1 μm. That is, compared to the carbon concentration near the center depth of the silicon wafer, the carbon concentration decreases at a depth within 1 μm from the surface of the silicon wafer. On the other hand, in Example 5, where argon annealing is performed before forming the silicon epitaxial layer, a low-carbon concentration layer having a thickness of 7.6 μm is formed in the depth direction of the wafer from the interface between the silicon epitaxial layer and the silicon wafer, and it was found that the carbon concentration of the silicon epitaxial layer covers almost the entire epitaxial layer except near the interface with the silicon wafer, and the carbon concentration is below the detection limit (2.0 × 10⁻⁶). 15 atoms / cm 3(See below). That is, compared to the carbon concentration near the center depth of the silicon wafer, the carbon concentration is reduced at a depth of within 7.6 μm from the surface of the silicon wafer. The thickness of the low-carbon concentration layer varies depending on the argon annealing conditions. For example, all other conditions are set similarly to those of Example 5, and when the heat treatment conditions are changed to 1150°C for 10 minutes, the thickness is 5.6 μm; when the heat treatment conditions are changed to 1200°C for 10 minutes, it is 7.3 μm; when the heat treatment conditions are changed to 1150°C for 60 minutes, it is 7.3 μm; and when the heat treatment conditions are changed to 1200°C for 60 minutes, it is 9.4 μm. In other words, the thickness of the low-carbon concentration layer can be adjusted as desired by adjusting the heat treatment temperature and time for argon annealing. By forming a low-carbon concentration layer of a predetermined thickness on the surface layer of the silicon wafer, the amount of carbon diffusion from the silicon wafer to the epitaxial layer can be reduced.
[0078] [Sleep potential assessment] For the following Comparative Examples 4 and 5, and Examples 6 and 7, studies are conducted on whether slip dislocations (defects along the silicon crystal surface) occur based on whether carbon doping or argon annealing was performed. The specifications and conditions shared by Comparative Examples 4 and 5, and Examples 6 and 7 are listed below. Resistivity: 0.91 mΩ·cm Carbon concentration: 3.87×10⁻⁶ 16 atoms / cm 3 In addition, the argon annealing of Comparative Example 5 and Example 7, in which argon annealing is performed, is a heat treatment at 1200°C for 30 minutes in an argon gas atmosphere. Also, in the following descriptions, "heat treatment corresponding to epitaxial layer growth conditions" refers to a heat treatment performed without introducing source gas into an epitaxial device (CENTURA® manufactured by Applied Materials, Inc.) and means a heat treatment at 1150°C for 10 minutes in a hydrogen gas atmosphere. <Comparative Example 4> For a non-carbon-doped silicon wafer, heat treatment corresponding to epitaxial layer growth conditions is performed without performing argon annealing (a silicon epitaxial layer does not grow with heat treatment alone). <Comparative Example 5> Argon annealing is performed on a silicon wafer that is not doped with carbon, and heat treatment corresponding to epitaxial layer growth conditions is performed. <Example 6> For carbon-doped silicon wafers, heat treatment corresponding to epitaxial layer growth conditions is performed without performing argon annealing. <Example 7> Argon annealing is performed on a carbon-doped silicon wafer, and heat treatment corresponding to epitaxial layer growth conditions is performed.
[0079] For each silicon wafer, the presence of slip dislocations observed on the wafer surface is confirmed by X-ray topography. As a result, as shown in Fig. 7, no slip dislocations were found in any of the silicon wafers, and it was also revealed that no slip dislocations occurred even when the silicon wafers were densely doped with carbon.
[0080] [Verification of resistivity, carbon concentration, and LPD density] For the following Comparative Examples 6 and 7, and Examples 8 and 9, silicon wafers are fabricated under various conditions to verify the correlations between resistivity, carbon concentration, and LPD density, an epitaxial layer is formed on the surface of each silicon wafer, and the LPD density observed on the surface of the epitaxial layer is measured. Furthermore, the argon annealing of Comparative Examples 7 and 9 below is a heat treatment at 1200°C for 30 minutes in an argon gas atmosphere. <Comparative Example 6> Without performing carbon doping, phosphorus is doped so that the resistivity of the upper portion of the straight body of the single crystal ingot becomes 1.0 mΩ·cm, and the single crystal ingot is grown to have a resistivity range of 0.6 mΩ·cm to 1.0 mΩ·cm, and a plurality of silicon wafers having different resistivity are manufactured from the single crystal ingot. A silicon epitaxial layer having a thickness of 4 μm is formed without performing argon annealing on any of the silicon wafers. <Comparative Example 7> Similar to Comparative Example 6, carbon doping is not performed, and a single-crystal ingot is grown to have a resistivity range of 0.6 mΩ·cm to 1.0 mΩ·cm, and a plurality of silicon wafers having different resistivity are manufactured from the single-crystal ingot. Without carbon doping, argon annealing is performed on each of the silicon wafers, and then an epitaxial layer having a thickness of 4 μm is formed.
[0081] <Example 8> Similar to Comparative Example 6, a single-crystal ingot having a resistivity range of 0.6 mΩ·cm to 1.0 mΩ·cm was grown, and a plurality of silicon wafers having different resistivity were manufactured from the single-crystal ingot. The carbon concentration at the top of the straight body of the single-crystal ingot was 3.0 × 10⁻⁶ 16 atoms / cm 3 Carbon doping is performed to this extent, but an epitaxial layer with a thickness of 4 μm is formed without performing argon annealing on any of the silicon wafers. <Example 9> Similar to Comparative Example 6, a single-crystal ingot having a resistivity range of 0.6 mΩ·cm to 1.0 mΩ·cm was grown, and a plurality of silicon wafers having different resistivity were manufactured from the single-crystal ingot. The carbon concentration at the top of the straight body of the single-crystal ingot was 3.0 × 10⁻⁶ 16 atoms / cm 3 Carbon doping is performed to this extent, and after argon annealing is performed on each of the silicon wafers, an epitaxial layer with a thickness of 4 μm is formed.
[0082] FIG. 8 is a graph for the epitaxial layers in Examples 8 and 9 and Comparative Examples 6 and 7, illustrating the relationship between the resistivity of the silicon wafer and the LPD density observed on the surface of the epitaxial layer. The horizontal axis of FIG. 8 shows the location where the silicon wafer is cut when the amount of solidification of the entire length of the straight body of the grown ingot is set to 1, using the solidification rate of the straight body of the ingot.
[0083] As shown in FIG. 8, in Example 8, where carbon doping is performed before the epitaxial growth process and argon annealing is not performed, an LPD density of approximately 20,000 defects per wafer is observed in a silicon wafer cut from a position on the straight line of the ingot at a solidification rate of 0.1, which is the upper crystal region, confirming the effect of reducing LPD density. However, in a silicon wafer cut from a position on the straight line of the ingot at a solidification rate of 0.3, the LPD density overflowed. Furthermore, when a silicon wafer cut from the lower crystal region is used, even in the case of a silicon wafer having an extreme resistivity of 0.6 mΩ·cm, the LPD density can be reduced to 130 defects per wafer or less.
[0084] In Example 9, where carbon doping and argon annealing are performed before the epitaxial growth process, the LPD density can be reduced to 100 defects per wafer even when a silicon wafer cut from the upper crystal region is used. This is because the dislocation loop defects are refined by high-concentration carbon doping and the refined dislocation loop defects are removed by performing argon annealing on the silicon wafer, and it was found that the effect of reducing SF through the synergistic effect of high-concentration carbon doping and argon annealing is very significant. Meanwhile, when a silicon wafer cut from the lower crystal region having a short residence time in the SF nucleation temperature range (solidification rate of 0.55 or higher) is used, the LPD density can be reduced to a total of 10 defects per wafer.
[0085] Meanwhile, in Comparative Example 6, where carbon doping and argon annealing are not performed on the silicon wafer, when a silicon wafer cut from the upper crystal region is used, the LPD density overflows, and when a silicon wafer cut from the lower crystal region is used, the LPD density is significantly reduced, but for a silicon wafer having a resistivity of 0.6 mΩ·cm, the LPD density is 250 or more defects per wafer. In addition, in Comparative Example 7, where carbon doping and argon annealing are performed on the silicon wafer before the epitaxial growth process, the LPD density may be reduced compared to Comparative Example 6. However, when a silicon wafer cut from the upper crystal region is used, the LPD density is 500 to 1,100 defects per wafer.
[0086] Based on the results mentioned above, 3.0×10 16 atoms / cm 3By performing the above carbon doping and by performing argon annealing on the silicon wafer prior to the epitaxial growth process, the LPD density observed on the surface of the epitaxial layer in all crystalline regions of the single-crystal ingot can be reduced to at least 100 defects per wafer. Furthermore, even when argon annealing is not performed on the silicon wafer, by performing carbon doping, the LPD density in the crystalline region on the lower side can be reduced to 130 defects or fewer defects per wafer. Although these examples do not disclose all developed experimental examples, the inventors of the present invention [have] at least 3.5 × 10 15 atoms / cm 3 When the above high concentration of carbon is added, the LPD density after the epitaxial growth process can be reduced for a silicon wafer having a resistivity of 0.6 mΩ·cm to 1.2 mΩ·cm compared to the case where no carbon is added.
[0087] [Evaluation of Device Pressure Resistance Characteristics] Device breakdown voltage characteristics are evaluated. In this example, device breakdown voltage is one of the quality characteristics of a semiconductor device and refers to the voltage at which breakdown occurs when the voltage between the drain and the source is gradually increased while the path between the gate and the source constituting the semiconductor device is short-circuited.
[0088] If oxygen within a silicon wafer diffuses into the epitaxial layer where a semiconductor device is manufactured, there is a concern that the device's breakdown pressure characteristics may be affected. For this reason, the inventors of the present invention prepared silicon wafers with six different levels of oxygen concentration and formed a silicon epitaxial layer on each silicon wafer to investigate whether there were differences in the device's breakdown pressure characteristics based on the difference in oxygen concentration. In addition, studies were also conducted on whether there were differences in the device's breakdown pressure characteristics based on whether the silicon wafer was doped with carbon.
[0089] Specifically, a semiconductor device was manufactured on each of the epitaxial silicon wafers in samples 1 to 12 in Table 1, and a predetermined voltage was applied between the drain and the source while the path between the gate and the source constituting the semiconductor device was short-circuited, and the breakdown voltage characteristics were determined to be "poor" when breakdown occurred, whereas the breakdown voltage characteristics were determined to be "good" when breakdown did not occur.
[0090] The epitaxial silicon wafers in Samples 1 to 6 have a silicon epitaxial layer having a thickness of 4 µm formed on a silicon wafer having a diameter of 300 mm, phosphorus added, and a resistivity of 0.9 mΩ·cm, and this epitaxial layer is a sample wafer formed on each of six carbon-free silicon wafers having six different levels of oxygen concentration. The epitaxial silicon wafers in Samples 7 to 12 have a silicon epitaxial layer having a thickness of 4 µm formed on a silicon wafer having a diameter of 300 mm, phosphorus added, and a resistivity of 0.9 mΩ·cm, similar to Samples 1 to 6, and a carbon concentration of 3.8 × 10⁻⁶ 16 atoms / cm 3 The above epitaxial layer is a sample wafer formed on each of the six silicon wafers having different oxygen concentration levels. The carbon concentration and oxygen concentration are values obtained by thinning the silicon wafer by polishing, and then measuring the concentration near the center of the silicon wafer in the depth direction using SIMS.
[0091]
[0092] As shown in Table 1, it is confirmed that the device internal pressure in samples 7 to 9 is likely to be poor when carbon doping is performed. However, even when carbon doping is performed, the oxygen concentration is 10×10 17 atoms / cm 3It is confirmed that faulty device internal pressure can be prevented by configuring it as follows.
[0093] It should be noted that the foregoing examples are provided for illustrative purposes only and should not be interpreted as limiting the invention. Although the invention has been described with reference to exemplary embodiments, the words used herein are understood to be descriptive and illustrative, not limiting. Within the scope of the appended claims, modifications may be made in aspects of the invention as described and modified, without departing from the scope and spirit of the invention. Although the invention has been described with reference to specific structures, materials, and embodiments herein, the invention is not intended to be limited to the details disclosed herein; rather, the invention extends to all functionally equivalent structures, methods, and uses within the scope of the appended claims.
[0094] The present invention is not limited to the embodiments described above, and various modifications and variations may be possible without departing from the scope of the invention.
Claims
Claim 1 A phosphorus-doped epitaxial wafer having a diameter of 300 mm comprising a silicon substrate having a resistivity in the range of 0.6 mΩ·cm to 1.2 mΩ·cm; an epitaxial layer on the silicon substrate; and a boundary between the epitaxial layer and the silicon substrate; wherein the silicon substrate has a depth of 3.5 × 10⁻⁶ from the center of the silicon substrate in the depth direction. 15 atoms / cm 3 Epitaxial wafer having a carbon concentration of the above. Claim 2 In claim 1, the carbon concentration is 3.5 × 10⁻⁶ at the center of the silicon substrate in the depth direction. 15 atoms / cm 3 Up to 5.0×10 17 atoms / cm 3 Epitaxial wafer within the range of. Claim 3 An epitaxial wafer according to claim 1, wherein the upper surface of the epitaxial layer comprises 130 or fewer light spot defects (LPDs) having a size of 0.09 μm or more. Claim 4 An epitaxial wafer according to claim 1, wherein the upper surface of the epitaxial layer comprises 100 or fewer LPDs having a size of 0.09 μm or more. Claim 5 In claim 1, 4.0×10 within the silicon substrate 17 atoms / cm 3 Up to 10×10 17 atoms / cm 3 Epitaxial wafer additionally containing an oxygen concentration within the range of Claim 6 In claim 1, the silicon substrate is an epitaxial wafer substantially free of crystal-originated particles. Claim 7 As a silicon wafer, phosphorus-doped with a diameter of 300 mm, a resistivity in the range of 0.6 mΩ·cm to 1.2 mΩ·cm, and 3.5 × 10⁻⁶ from the center of the silicon wafer in the depth direction 15 atoms / cm 3 Silicon wafer having a carbon concentration of the above. Claim 8 In claim 7, the carbon concentration is 3.5 × 10⁻⁶ at the center of the silicon wafer in the depth direction. 15 atoms / cm 3 Up to 5.0×10 17 atoms / cm 3 Silicon wafer in the range of. Claim 9 In Paragraph 7, 4.0×10 17 atoms / cm 3 Up to 10×10 17 atoms / cm 3 A silicon wafer additionally containing an oxygen concentration within the range of Claim 10 In paragraph 7, the silicon wafer is a silicon wafer substantially free of crystal-derived particles. Claim 11 A method for manufacturing an epitaxial wafer having a diameter of 300 mm, comprising the steps of: placing a crucible in a furnace; adding phosphorus and carbon to a silicon melt in the crucible; rotaryly pulling a single crystal from the silicon melt with a puller; cutting the single crystal into at least one silicon wafer; and forming an epitaxial layer on the surface of the silicon wafer ― the silicon wafer has a depth of 3.5 × 10⁻⁶ from the center of the silicon wafer in the depth direction 15 atoms / cm 3 A method comprising: having a carbon concentration greater than or equal to the above, wherein the silicon wafer has a resistivity in the range of 0.6 mΩ·cm to 1.2 mΩ·cm. Claim 12 A method according to claim 11, further comprising the step of heating the silicon wafer at a temperature of 1150°C to 1250°C in an atmosphere filled with argon gas. Claim 13 A method according to claim 12, wherein the step of heating the silicon wafer is performed for 30 to 120 minutes. Claim 14 In claim 11, the silicon wafer is 4.0×10 17 atoms / cm 3 Up to 10×10 17 atoms / cm 3 A method further comprising the step of applying a magnetic field to the silicon melt to have an oxygen concentration and controlling the pressure inside the furnace. Claim 15 In paragraph 14, the oxygen concentration is measured from the middle in the depth direction of the silicon wafer. Claim 16 delete Claim 17 delete
Citation Information
Patent Citations
High-resistance silicon wafer and process forproducing the same
KR1020050035862A
Apparatus and method for managing and orchestrating network function virtualization
KR1020180037454A
Method for manufacturing n-type silicon single crystal, ingot of n-type silicon single crystal, silicon wafer and epitaxial silicon wafer
KR1020190126163A
Epitaxial silicon wafer and method for manufacturing same
US20160042974A1