Method for manufacturing high-purity nickle using nickel carbonyl process
By employing hydrogen reduction and nickel carbonyl reactions, the method produces high-purity nickel efficiently and sustainably, meeting the demand for battery cathode materials and overcoming environmental and domestic production limitations.
Patent Information
- Application Number
- KR1020240030812
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-04
AI Technical Summary
Existing carbon-based oxide smelting methods for producing high-purity nickel are environmentally unsustainable and fail to meet ESG requirements, while current methods for producing Class 1 nickel are insufficient to meet the growing demand for battery cathode materials, and there are limited domestic capabilities for nickel production.
A method using hydrogen as a reducing agent to selectively reduce low-grade nickel oxide ore, followed by a nickel carbonyl reaction to produce high-purity metallic nickel, incorporating a series of steps including calcination, selective reduction, nickel carbonyl reaction, acid leaching, and impurity removal to achieve high-purity nickel MHP.
The method achieves high-purity nickel production with a recovery rate of 98% and purity of 85% or more, addressing environmental concerns and expanding the supply of high-purity nickel for battery companies.
Smart Images

Figure 112024024453255-PAT00004_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for producing high-purity nickel using a nickel carbonyl process, and more specifically, to a method for producing high-purity nickel using a nickel carbonyl process in which low-grade nickel oxide ore of 1.5% or less is selectively reduced using hydrogen, which is more environmentally friendly than carbon, to produce nickel of 25% or more, and then high-purity metallic nickel of 85% or more is produced using a nickel carbonyl reaction. Background Technology
[0002] High-purity nickel is classified into Class 1 (nickel content of 99.8% or more) and Class 2 (less than 99.8%). The demand for Class 1 nickel as a raw material for battery cathode materials is increasing, while Class 2 nickel, which has lower purity than Class 1, is manufactured into ferronickel and is mostly used in stainless steel processes.
[0003] Currently, Class 1 nickel accounts for less than 35% of total nickel production for batteries, but with the significant increase in demand for Class 1 nickel due to the expansion of investment in electric vehicles and batteries in various countries, it is necessary to secure a stable supply chain for nickel.
[0004] In addition, more than 65% of metallic nickel is ferronickel used in the manufacture of stainless steel, and the demand for nickel compounds for batteries is low at about 10%, but due to the recent increase in the adoption and production of electric vehicles, the demand is expected to increase to more than 50% in the future.
[0005] Meanwhile, although small quantities of nickel are produced domestically and nickel sulfate is manufactured by recovering nickel from nickel plating solutions, the proportion is low, resulting in a situation where there are virtually no domestic companies capable of manufacturing nickel using proprietary technology.
[0006] Furthermore, existing carbon-based oxide smelting methods fail to meet ESG (Environmental, Social, Governance) requirements and emit massive amounts of carbon dioxide, necessitating the development of more eco-friendly smelting methods.
[0007] The present invention, described below, is a new technology nickel dry smelting method that uses hydrogen, which is more environmentally friendly than carbon, as a reducing agent to selectively reduce low-grade nickel oxide ore of 1.5% or less to produce nickel of 25% or more, and then uses a nickel carbonyl reaction to produce high-purity metallic nickel of 85% or more.
[0008] High-purity nickel produced using the above hydrogen reduction method and nickel carbonyl method can be used to produce nickel MHP (Ni(OH)2) (hereinafter referred to as MHP) with a purity of 99% or higher through an impurity purification process using a wet leaching method and a selective oxide and sulfide precipitation method, and can be utilized as, for example, a nickel precursor for batteries.
[0009] Meanwhile, prior art patent documents described below include a method for microbial leaching of copper, nickel, and cobalt by iron-oxidizing bacteria from a matte, which is an intermediate product of manganese nodules (Patent Document 1), a method for recovering nickel hydroxide and nickel sulfate from multilayer ceramic capacitor process sludge (Patent Document 2), and a method for extracting and separating copper, zinc, cadmium, and nickel by solvent extraction from a leaching solution of secondary metal resources (Patent Document 3).
[0010] However, the aforementioned prior art differs from the present invention described below, which utilizes a selective hydrogen reduction method and a selective nickel carbonyl reaction.
[0011] In addition, the method of concentrating and recovering ferronickel from a nickel-containing raw material, the method of recovering a nickel concentrate from the concentrated ferronickel, and the method of recycling an iron-containing solution generated in the above method (Patent Document 4) differ from the method of producing ferronickel from low-grade nickel and obtaining high-purity nickel as described below in the present invention.
[0012] In addition, a wet smelting recovery method for nickel sulfate (Patent Document 5) has been proposed, but it appears to have little relation to the present invention described below. Prior art literature
[0013] 1. Microbial leaching smelting method of copper, nickel, and cobalt by iron-oxidizing bacteria from a matte, which is an intermediate product of manganese nodules, according to Registered Patent No. 10-0557410 (Registered on February 24, 2006) 2. Method for recovering nickel hydroxide and nickel sulfate from multilayer ceramic condenser process sludge according to Registered Patent No. 10-2496184 (Registered on February 1, 2023) 3. Method for extracting and separating copper, zinc, cadmium, and nickel by solvent extraction from a leaching solution of secondary metal resources according to Registered Patent No. 10-1232199 (Registered on February 5, 2013) 4. Method for concentrating and recovering ferronickel from a nickel-containing raw material, method for recovering a nickel concentrate from the concentrated ferronickel, and method for recycling an iron-containing solution generated in the said method according to Registered Patent No. 10-1203731 (registered November 15, 2012). 5. Wet smelting recovery method of nickel sulfate according to Registered Patent No. 10-2430686 (registered August 4, 2022). The problem to be solved
[0014] The present invention was created to solve the above-mentioned problems, and aims to provide a method for producing high-purity nickel using a nickel-carbonyl process, which selectively reduces low-grade nickel oxide ore of 1.5% or less using hydrogen, which is more environmentally friendly than carbon, to produce nickel of 25% or more, and then produces high-purity metallic nickel of 85% or more using a nickel-carbonyl reaction. means of solving the problem
[0015] The method for producing high-purity nickel using the nickel carbonyl process of the present invention to achieve the above-mentioned purpose is,
[0016] (a) a step of removing moisture (H2O) from the low-grade nickel oxide ore by calcining the low-grade nickel oxide ore;
[0017] (b) a step of producing high-purity metallic nickel by causing a selective reduction reaction of moisture-removed low-grade nickel oxide ore using hydrogen gas as a reducing agent; and
[0018] (c) a step of purifying the above-mentioned metallic nickel into high-purity metallic nickel using a selective nickel-carbonyl reaction;
[0019] (d) a step of liquefying the purified high-purity metallic nickel through acid leaching fixation;
[0020] (e) a step of oxidizing the above liquid high-purity metallic nickel using a predetermined oxidizing agent;
[0021] (f) a step of recovering Ni MHP by removing impurities from oxidized high-purity metallic nickel using a selective hydroxide and selective sulfide precipitation method; characterized by including the above.
[0022] In the present invention, steps (a) and (b) are composed of the following reaction formula 1.
[0023] (Reaction Equation 1)
[0024] NiO + H2 = Ni + H2O
[0025] In paragraph 1,
[0026] In step (c) above, the nickel carbonyl reaction is carried out according to the following reaction scheme 2.
[0027] (Reaction Equation 2)
[0028]
[0029] In the present invention, in step (c), the nickel recovery rate by the nickel carbonyl reaction is 98% or higher, and the purity of the metallic nickel is 85% or higher.
[0030] In the present invention, in step (c), the high-purity metallic nickel is powder nickel.
[0031] In the present invention, in step (f), the Ni MHP is nickel with a purity of 99% or higher. Effects of the invention
[0032] According to an embodiment of the present invention, by using hydrogen, which is more environmentally friendly than carbon, as a reducing agent to selectively reduce low-grade nickel oxide ore of 1.5% or less to produce nickel of 25% or more, and then using a nickel carbonyl reaction, high-purity metallic nickel of 85% or more can be produced.
[0033] In addition, the present invention is a method capable of producing high-purity nickel through a new nickel smelting process that combines the nickel carbonyl reaction method and the wet smelting method.
[0034] Furthermore, the present invention can significantly contribute to expanding the supply of high-purity nickel to battery companies. Brief explanation of the drawing
[0035] FIG. 1 is a flowchart sequentially showing a method for manufacturing high-purity nickel using a nickel carbonyl process according to the present invention. Figure 2 is a schematic diagram of a process for producing high-content nickel using a nickel-carbonyl optimal reaction. Figure 3 is a diagram illustrating the manufacturing process of high-purity nickel MHP by a wet process. Specific details for implementing the invention
[0036] Hereinafter, preferred embodiments according to the present invention will be described in detail with reference to the attached drawings.
[0037] FIG. 1 shows a flowchart sequentially illustrating a method for manufacturing high-purity nickel using the nickel carbonyl method according to the present invention.
[0038] Referring to FIG. 1, the method for producing high-purity nickel using the nickel carbonyl process according to the present invention first removes moisture (H2O) from low-grade nickel oxide ore by calcination treatment (step 110).
[0039] Laterite, a representative ore of the above-mentioned low-grade nickel oxide, has a nickel content of only 1.5% or less and contains oxides of iron, silicon, and magnesium.
[0040] As such, low-grade nickel oxide ore has a low nickel content, so excessive acid (e.g., sulfuric acid) is used in the wet leaching process, and leaching residue that cannot be reused is produced.
[0041] Consequently, this causes environmental pollution problems.
[0042] To resolve these problems, an eco-friendly nickel carbonyl method was applied in the present invention.
[0043] In step 110 above, high-purity metallic nickel is produced by selectively reducing the moisture-removed low-grade nickel oxide ore using hydrogen gas as a reducing agent (step 120).
[0044] Steps 110 and 120 above consist of the following reaction scheme 1.
[0045] (Reaction Equation 1)
[0046] NiO + H2 = Ni + H2O
[0047] That is, the above-mentioned low-nickel oxide ore is calcined to remove moisture, and then nickel and iron in a metallic state are produced using hydrogen, an eco-friendly reducing agent. Nickel oxide is easily reduced to a metallic state by hydrogen at a relatively low temperature (reduction is also easy even with hydrogen mixed with a large amount of moisture), and iron oxide is reduced at a relatively high temperature, and iron oxide and metallic iron reach equilibrium even when only 20-30% moisture is mixed (see figure below). Therefore, by controlling the reaction gas hydrogen, the reaction temperature, and the ratio of hydrogen to moisture in the gas, high-purity nickel metal can be obtained through a selective reduction reaction.
[0048] The metallic nickel prepared in Step 120 above is purified into high-purity metallic nickel using a selective nickel-carbonyl reaction (Step 130).
[0049] In step 130 above, the nickel carbonyl reaction is carried out according to the following reaction scheme 2.
[0050] (Reaction Equation 2)
[0051]
[0052] And the above reaction scheme 2 can be represented as a schematic diagram of a high-content nickel manufacturing process using the nickel-carbonyl optimal reaction as shown in Fig. 2.
[0053] If the thermal exchange reaction is subtracted from the above reaction equation 2, it can be expressed as Ni(s) + 4CO(g) = Ni(CO)4(g), and the direction of the reaction changes left and right depending on the temperature.
[0054] Therefore, high-purity Ni is produced through reaction equation 2.
[0055] In the above reaction equation 2, Ni(CO)4 has a melting point of 248K (-25℃) and a boiling point of 316K (43℃), making it very volatile. Furthermore, at 453K (180℃) or higher, it decomposes back into Ni and CO, so this property is utilized to remove CO and other impurities, produce high-purity Ni, and recycle CO gas.
[0056] However, since nickel carbonyl and CO gas are highly toxic gases, measures were taken to prevent them from leaking into the atmosphere.
[0057] Representative processing methods for the above-mentioned low-nickel oxide include the dry reduction method and converter refining method of the ferronickel manufacturing process, but while a nickel-iron alloy with a content of about 20% can be obtained with these methods, high-purity nickel cannot be obtained.
[0058] Therefore, in this invention, a nickel carbonyl method capable of producing eco-friendly and high-purity nickel was applied.
[0059] Meanwhile, it is known that nickel oxide can be easily converted into metallic nickel at lower temperatures and lower hydrogen partial pressures than iron, as shown in the reaction equation below.
[0060] 3H2(g) + 2Ni2SiO4 + 3Na2SO4 = Na6Si2O7 + 4NiO + 3SO2(g) + 3H2O(g)
[0061] H2(g) + NiO = Ni + H2O(g)
[0062] H2(g) + Ni2SiO4 = NiSiO3 + Ni + H2O(g)
[0063] Furthermore, metallic nickel obtained by selective hydrogen reduction can be purified into high-purity nickel through the nickel-carbonyl reaction, which is well known as the carbonyl method or Mond method.
[0064] In the nickel carbonyl process, iron carbonyl is produced at a relatively high temperature, and nickel carbonyl is formed at a temperature of 100°C or lower, so high-purity nickel can be obtained through a selective carbonyl reaction by controlling the reaction temperature.
[0065] The nickel recovery rate by the above nickel-carbonyl reaction is 98% or higher, and the purity of the metallic nickel is 85% or higher.
[0066] And in step 130 above, the high-purity metallic nickel is black powder nickel.
[0067] Next, in step 130 above, the refined high-purity metallic nickel is liquefied through acid leaching fixation (step 140).
[0068] In step 140 above, the liquid high-purity metallic nickel is oxidized using a predetermined oxidizing agent (step 150).
[0069] Ni MHP is recovered by removing impurities from the high-purity metallic nickel oxidized in step 150 using selective hydroxide and selective sulfide precipitation methods (step 160).
[0070] In addition, in step 160 above, nickel with a purity of 99% or higher is recovered from the Ni MHP.
[0071] That is, finally, metallic nickel with a nickel recovery rate of 98% or more and a nickel purity of 85% or more can be obtained through the nickel carbonyl reaction, and the obtained metallic nickel is liquefied through an acid leaching process, and then high-purity nickel MHP is manufactured through an iron removal process.
[0072] In addition, the reaction residue generated after the dry process contains MgO, SiO2, and CaO; however, research has been conducted on utilizing these as fertilizers, steel binders, pig iron substitutes (Remetal), and nickel byproducts, allowing for the reuse (recycling) of the ore without disposal.
[0073] Since the iron ions present as impurities exist in both divalent and trivalent forms, they can be oxidized to trivalent iron using oxidizing agents such as oxygen, hydrogen peroxide, and potassium permanganate, and then easily removed using selective hydroxide and selective sulfide precipitation methods.
[0074] By using a wet purification method to remove impurities such as iron ions and copper (Cu) ions, nickel MHP with a purity of 99% or higher can be obtained.
[0075] Figure 3 is a diagram illustrating the manufacturing process of high-purity nickel MHP by a wet process.
[0076] Meanwhile, there are no domestic companies that produce nickel sulfate from low-grade oxide ore using dry or wet smelting, and there are also no domestic companies that produce high-purity nickel.
[0077] Therefore, it has become possible to produce high-purity nickel through the smelting process of the high-purity nickel manufacturing method using the nickel carbonyl method according to the present invention, which combines the dry selective hydrogen reduction method, the nickel carbonyl reaction method, and the wet smelting method.
[0078] As described above, the present invention has been explained with reference to an embodiment illustrated in the drawings, but this is merely illustrative, and those skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom.
[0079] Therefore, the true scope of protection of the present invention must be determined solely by the appended claims.
Claims
Claim 1 A method for producing high-purity nickel using a nickel-carbonyl process for producing a nickel mixed hydroxide precipitate (hereinafter referred to as "Nickel MHP") from low-grade nickel oxide ore containing 1.5% or less nickel, comprising: (a) a step of calcining the low-grade nickel oxide ore to remove moisture (H2O); (b) a step of selectively reducing the moisture-removed low-grade nickel oxide ore using hydrogen gas as a reducing agent to produce metallic nickel with a nickel content of 25% or more; (c) a step of purifying the metallic nickel by a selective nickel-carbonyl reaction to obtain high-purity metallic nickel with a nickel recovery rate of 98% or more and a purity of 85% or more; (d) a step of liquefying the purified high-purity metallic nickel through an acid leaching process; and (e) a step of oxidizing iron ions in the liquid high-purity metallic nickel with at least one oxidizing agent selected from oxygen, hydrogen peroxide, and potassium permanganate. and (f) a step of recovering nickel MHP with a purity of 99% or higher by removing iron ion and copper (Cu) ion impurities from the oxidized liquid high-purity metallic nickel using a selective hydroxide precipitation method and a selective sulfide precipitation method. A method for producing high-purity nickel using a nickel carbonyl process. Claim 2 A method for producing high-purity nickel using a nickel-carbonyl process according to claim 1, wherein steps (a) and (b) are composed of the following reaction formula 1. (Reaction Formula 1) NiO + H2 = Ni + H2O Claim 3 A method for producing high-purity nickel using a nickel-carbonyl process according to claim 1, wherein in step (c), the nickel-carbonyl reaction is formed by the following reaction formula 2. (Reaction Formula 2) Claim 4 A method for producing high-purity nickel using a nickel carbonyl process, characterized in that, in claim 1, the high-purity metallic nickel obtained in step (c) is powder nickel. Claim 5 A method for producing high-purity nickel using a nickel carbonyl process, characterized in that, in step (c) of claim 1, the oxidizing agent is at least one selected from the group consisting of oxygen, hydrogen peroxide, and potassium permanganate. Claim 6 delete
Citation Information
Patent Citations
Method for recovering nickel and cobalt from nickel, iron and cobalt contaning raw material
KR1020180074569A
Method for Regenerating Nickel from Waste Battery Materials
KR1020230054385A