Positive electrode active material powder and method for preparing thereof

A two-step calcination process for nickel-cobalt-manganese-based lithium transition metal oxide powders addresses particle clumping issues, ensuring uniform particle sizes and reducing performance deviations, thereby enhancing the electrochemical properties of lithium-ion batteries.

KR103047095B1Active Publication Date: 2026-11-11LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020200058470
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-15
Publication Date
2026-11-11
Estimated Expiration
2040-05-15

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode active materials, such as lithium cobalt oxide, face challenges due to particle clumping and aggregation during calcination, leading to uneven particle sizes and performance deviations, which affect the electrochemical properties of the battery.

Method used

A positive electrode active material powder composed of nickel, cobalt, and manganese with controlled crystallite size deviations and uniform particle sizes is manufactured through a two-step calcination process, eliminating the need for grinding and classification, and ensuring uniform washing and coating.

Benefits of technology

The process results in a positive electrode active material powder with reduced performance variations, achieving superior electrochemical properties and stable battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112020049348868-PAT00001_ABST
    Figure 112020049348868-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a positive active material powder for a secondary battery comprising nickel (Ni), cobalt (Co), and manganese (Mn), wherein the standard deviation of the crystallite size of the positive active material constituting the positive active material powder is 5.0 or less and the relative standard deviation is 4.0% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a positive electrode active material powder for a secondary battery and a method for manufacturing the same. Background Technology

[0003] With the recent rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, the demand for small, lightweight, and relatively high-capacity rechargeable batteries is increasing rapidly. In particular, lithium-ion batteries are gaining prominence as power sources for portable devices due to their lightweight nature and high energy density. Consequently, active research and development efforts are underway to improve the performance of lithium-ion batteries.

[0004] In a lithium secondary battery, electrical energy is produced by oxidation and reduction reactions when lithium ions are inserted into or removed from the positive and negative electrodes, which are composed of active materials capable of lithium ion intercalation and deintercalation, with an organic or polymer electrolyte charged between them.

[0005] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compounds (LiFePO4) have been used as cathode active materials for lithium-ion batteries. Among these, lithium cobalt oxide (LiCoO2) is widely used and applied as a cathode active material for high-voltage applications due to its advantages of high operating voltage and excellent capacity characteristics. However, due to the rising price and supply instability of cobalt (Co), there are limitations to its mass use as a power source in fields such as electric vehicles, leading to the emergence of a need for the development of cathode active materials that can replace it.

[0006] Accordingly, a nickel-cobalt-manganese-based lithium transition metal oxide (hereinafter simply referred to as 'NCM-based lithium transition metal oxide') was developed in which a portion of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn). This nickel-cobalt-manganese-based lithium transition metal oxide is generally manufactured by introducing a precursor and a lithium raw material into a crucible of a certain volume and calcining them together at a high temperature. As lithium is inserted into the precursor at a certain temperature, the lithium transition metal oxide is formed. At this time, some unreacted lithium byproducts remain on the surface of the lithium transition metal oxide particles, causing the particles to clump together and aggregate to form an aggregated calcined body. This aggregated calcined body is broken down by grinding during a subsequent process, and after breaking down, it undergoes a washing and / or coating process. At this time, if the disintegration of the aggregated calcined body formed above occurs unevenly, it results in uneven particle size and uneven washing or coating, causing significant deviations in subsequent processes and leading to a problem of significant performance variation in the finally manufactured cathode active material. Prior art literature

[0008] Korean Patent Publication No. 2019-0065963 The problem to be solved

[0009] The present invention aims to provide a positive electrode active material powder for a secondary battery that has excellent electrochemical properties and exhibits small performance deviations by reducing particle size variations caused by non-uniform calcination and disintegration, having uniform particle size and crystal size, and reducing post-processing variations such as non-uniform washing or coating. means of solving the problem

[0011] The present invention provides a positive active material powder for a secondary battery comprising nickel (Ni), cobalt (Co), and manganese (Mn), wherein the standard deviation of the crystallite size of the positive active material constituting the positive active material powder is 5.0 nm or less and the relative standard deviation is 4.0% or less.

[0013] In addition, the present invention provides a method for manufacturing a positive electrode active material powder for a secondary battery, wherein a positive electrode active material precursor comprising nickel (Ni), cobalt (Co), and manganese (Mn) is mixed with a lithium raw material and calcined once to form a first calcined product, and then calcined the first calcined product a second time to form a lithium transition metal oxide.

[0015] In addition, the present invention provides a positive electrode for a secondary battery and a lithium secondary battery comprising the above positive electrode active material. Effects of the invention

[0017] According to the present invention, it is possible to provide a positive electrode active material powder for a secondary battery that has a small performance variation and excellent electrochemical properties by reducing particle size variation caused by non-uniform calcination and non-uniform disintegration, having uniform particle size and crystal size, and reducing post-process variation such as non-uniform washing or coating. Brief explanation of the drawing

[0019] Figure 1 is a graph showing the crystallite size variation of the positive electrode active material powder according to the examples and comparative examples. Figure 2 is a graph showing the deviation of the a-axis lattice parameter of the positive electrode active material powder according to the examples and comparative examples. Figure 3 is a graph showing the deviation of the c-axis lattice parameter of the positive electrode active material powder according to the examples and comparative examples. Figure 4 is a graph showing the deviation of the weight percentage of lithium byproducts remaining on the surface relative to the weight of the positive electrode active material according to the examples and comparative examples. Figure 5 is a graph showing the discharge capacity variation of the positive electrode active material powder according to the examples and comparative examples. Specific details for implementing the invention

[0020] Hereinafter, the present invention will be described in more detail to aid in understanding the invention. In this case, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0022] <Cathode Active Material Powder>

[0023] The positive active material powder for a secondary battery according to the present invention is a positive active material powder of a lithium transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the standard deviation of the crystallite size of the positive active material constituting the positive active material powder is 5.0 nm or less and the relative standard deviation is 4.0% or less.

[0024] The above lithium transition metal oxide comprises nickel (Ni), cobalt (Co), and manganese (Mn), and more preferably may be a high-nickel (High-Ni) NCM system in which nickel is 70 mol% or more of the total metals excluding lithium, and more preferably may have a nickel (Ni) content of 80 mol% or more. If the nickel (Ni) content of the above lithium transition metal oxide satisfies 70 mol% or more, it may be possible to secure a higher capacity. In addition, the above lithium transition metal oxide may more preferably be an NCMA system in which aluminum (Al) is additionally included in addition to nickel (Ni), cobalt (Co), and manganese (Mn), and likewise may be a high-nickel (High-Ni) NCMA system in which nickel is 70 mol% or more of the total metals excluding lithium.

[0025] More specifically, the lithium transition metal oxide can be represented by the following chemical formula 1.

[0026] [Chemical Formula 1]

[0027] Li a Ni 1-b-c-dCo b Mn c Q d O 2+δ

[0028] In the above chemical formula 1, Q is one or more elements selected from the group consisting of Al, Si, B, W, Mo, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Ta, Sn, Sr, La, Ce, Pr, and Zr, and 1.0≤a≤1.5, 0 <b≤0.5, 0<c≤0.5, 0≤d≤0.1, 0<b+c+d≤0.3, -0.1≤δ≤1.0이다.

[0029] In the lithium transition metal oxide of Chemical Formula 1 above, Li may be included in an amount corresponding to a, i.e., 1.0 ≤ a ≤ 1.5. If a is less than 1.0, there is a risk of reduced capacity, and if it exceeds 1.5, the particles may sinter during the calcination process, making it difficult to manufacture the cathode active material. Considering the balance between the significant effect of improving the capacity characteristics of the cathode active material by controlling the Li content and the sinterability during the manufacture of the active material, the Li may more preferably be included in an amount of 1.03 ≤ a ≤ 1.1.

[0030] In the lithium transition metal oxide of Chemical Formula 1 above, Ni may be included in an amount corresponding to 1-(b+c+d), for example, 0.7 ≤ 1-(b+c+d) < 1. If the composition of the composition in which Ni is present in the lithium composite transition metal oxide of Chemical Formula 1 is 0.7 or higher, a sufficient amount of Ni is secured to contribute to charging and discharging, thereby enabling high capacity. More preferably, Ni may be included in an amount of 0.80 ≤ 1-(b+c+d) ≤ 0.99.

[0031] In the lithium transition metal oxide of Chemical Formula 1 above, Co has an amount corresponding to b, i.e., 0 <b≤0.5로 포함될 수 있다. 상기 화학식 1의 리튬 전이금속 산화물 내 Co의 함량이 0.5를 초과할 경우 비용 증가의 우려가 있다. Co 포함에 따른 용량 특성 개선 효과의 현저함을 고려할 때, 상기 Co는 보다 구체적으로 0.05≤b≤0.2의 함량으로 포함될 수 있다.

[0032] In the lithium transition metal oxide of Chemical Formula 1 above, Mn has an amount corresponding to c, i.e., 0 <c≤0.5의 함량으로 포함될 수 있다. 상기 화학식 1의 리튬 전이금속 산화물 내 c가 0.5을 초과하면 오히려 전지의 출력 특성 및 용량 특성이 저하될 우려가 있으며, 상기 Mn은 보다 구체적으로 0.05≤c≤0.2의 함량으로 포함될 수 있다.

[0033] In the lithium transition metal oxide of Chemical Formula 1 above, Q may be a doping element included in the crystal structure of the lithium transition metal oxide, and Q may be included in an amount corresponding to d, i.e., 0 ≤ d ≤ 0.1. This can be formed by mixing additional doping raw materials. More preferably, Q may include Al.

[0034] The positive electrode active material powder of the lithium transition metal oxide of the present invention has a crystallite size standard deviation of 5.0 nm or less and a relative standard deviation of 4.0% or less of the positive electrode active material constituting the positive electrode active material powder.

[0035] The lithium transition metal oxide particles of the present invention may be in the form of secondary particles formed by the aggregation of primary particles. In the present invention, 'primary particle' refers to a primary structure of a single particle, and 'secondary particle' refers to an aggregate formed by the aggregation of primary particles through physical or chemical bonding between primary particles without an intentional aggregation or assembly process of the primary particles, i.e., a secondary structure. In the present invention, 'particle' refers to a grain of micro-scale, and when magnified, primary particles of several hundred nanometers in size can be observed. Further magnification reveals distinct regions where atoms form a specific lattice structure; these regions are called 'crystallites,' and their crystallite size can be calculated from XRD measurement data using the Scherrer equation.

[0036] The positive electrode active material powder of the present invention is characterized by having a uniform particle size and crystallite size, with reduced particle size variation due to non-uniform calcination and disintegration. Accordingly, the standard deviation of the crystallite size is 5.0 nm or less, and the relative standard deviation is 4.0% or less. More preferably, the positive electrode active material constituting the positive electrode active material powder may have a crystallite size of 90 to 140 nm, more preferably 100 to 130 nm, and the standard deviation of the crystallite size may be more preferably 0 to 4.5 nm, and even more preferably 0 to 4.3 nm. In addition, the relative standard deviation of the crystallite size of the positive electrode active material constituting the positive electrode active material powder may be more preferably 0 to 3.7%, and even more preferably 0 to 3.5%. In the present invention, the relative standard deviation is a value calculated by dividing the standard deviation by the mean and multiplying by 100. If the standard deviation of the crystallite size of the positive active material constituting the positive active material powder exceeds 5.0 nm or the relative standard deviation exceeds 4.0%, the positive active material particles in the powder will have non-uniform crystallite sizes, and post-processing deviations such as non-uniform washing or coating will increase, resulting in significant performance deviations of the positive active material and potentially deteriorating the electrochemical characteristics of the lithium secondary battery to which it is applied.

[0037] In addition, the standard deviation of the a-axis lattice parameter of the positive active material constituting the positive active material powder of the present invention may be 0.002 Å or less, and the relative standard deviation may be 0.05% or less. More preferably, the positive active material constituting the positive active material powder may have an a-axis lattice parameter standard deviation of 0 to 0.0017 Å, more preferably 0 to 0.0015 Å, and the relative standard deviation may be 0 to 0.045%, more preferably 0 to 0.043%. If the standard deviation of the a-axis lattice parameter of the positive active material constituting the above positive active material powder exceeds 0.002 Å or the relative standard deviation exceeds 0.05%, the positive active material particles in the powder will have a non-uniform crystal structure, and post-processing deviations such as non-uniform washing or coating will increase, resulting in a large deviation in the performance of the positive active material and potentially deteriorating the electrochemical characteristics of the lithium secondary battery to which it is applied.

[0038] In addition, the standard deviation of the c-axis lattice parameter of the positive active material constituting the positive active material powder of the present invention may be 0.003 Å or less, and the relative standard deviation may be 0.03% or less. More preferably, the positive active material constituting the positive active material powder may have a standard deviation of the c-axis lattice parameter of 0 to 0.00295 Å, more preferably 0 to 0.0029 Å, and the relative standard deviation may be 0 to 0.025%, more preferably 0 to 0.023%. If the standard deviation of the c-axis lattice parameter of the positive active material constituting the above positive active material powder exceeds 0.003 Å or the relative standard deviation exceeds 0.03%, the positive active material particles in the powder will have a non-uniform crystal structure, and post-processing deviations such as non-uniform washing or coating will increase, resulting in a large deviation in the performance of the positive active material and potentially deteriorating the electrochemical characteristics of the lithium secondary battery to which it is applied.

[0039] In the present invention, the a-axis lattice parameter and the c-axis lattice parameter of the positive electrode active material are values ​​calculated by indexing XRD measurement data through Rietveld refinement.

[0040] In addition, the standard deviation of the weight percentage of lithium by-products remaining on the surface relative to the weight of the positive active material constituting the positive active material powder of the present invention may be 0.02 weight% or less, and the relative standard deviation may be 3.0% or less. More preferably, the weight percentage of lithium by-products remaining on the surface relative to the weight of the positive active material constituting the positive active material powder may be 0.3 to 0.7 weight%, and even more preferably 0.4 to 0.6 weight%. More preferably, the standard deviation of the weight percentage of lithium by-products remaining on the surface relative to the weight of the positive active material constituting the positive active material powder may be 0 to 0.02 weight%, and even more preferably 0 to 0.015 weight%, and the relative standard deviation may be 0 to 3.0%, and even more preferably 0 to 2.7%. If the standard deviation of the lithium byproduct content remaining on the surface of the positive active material constituting the above positive active material powder exceeds 0.02 weight% or the relative standard deviation exceeds 3.0%, the positive active material particles in the powder are manufactured through a post-process with a large deviation in non-uniform washing or coating, resulting in a large deviation in the performance of the positive active material and potentially deteriorating the electrochemical characteristics of the lithium secondary battery to which it is applied.

[0041] As such, the anode active material powder according to the present invention reduces particle size variation caused by non-uniform calcination and disintegration, has uniform particle size and crystal size, and reduces post-process variation such as non-uniform washing or coating, resulting in small performance variation and significantly superior electrochemical properties.

[0043] Next, a method for manufacturing a positive electrode active material powder for a secondary battery according to the present invention will be described.

[0044] The positive electrode active material powder for a secondary battery according to the present invention is manufactured by mixing a positive electrode active material precursor comprising nickel (Ni), cobalt (Co), and manganese (Mn) with a lithium raw material, performing a first calcination to form a first calcined product, and then performing a second calcination to form a lithium transition metal oxide.

[0045] The above-mentioned positive active material precursor may be a hydroxide containing nickel (Ni), cobalt (Co), and manganese (Mn), and more preferably, the above-mentioned positive active material precursor may be a high-nickel (High-Ni) NCM system containing nickel (Ni), cobalt (Co), and manganese (Mn) in which nickel is 70 mol% or more of the total metal, and more preferably, the nickel (Ni) content may be 80 mol% or more. If the nickel (Ni) content of the total metal content of the above-mentioned positive active material precursor satisfies 70 mol% or more, the lithium transition metal oxide manufactured using it may be a high-nickel (High-Ni) NCM system lithium transition metal oxide, thereby enabling the securing of a higher capacity. In addition, the above-mentioned positive electrode active material precursor may more preferably be an NCMA system containing aluminum (Al) in addition to nickel (Ni), cobalt (Co), and manganese (Mn), and likewise may be a high-nickel (High-Ni) NCMA system in which nickel is 70 mol% or more of the total metal. However, as in the example above, a lithium transition metal oxide may be formed using a positive electrode active material precursor containing aluminum (Al), or a positive electrode active material that does not contain aluminum (Al) may be used and introduced as a doping source together with the lithium raw material during the calcination process to form a lithium transition metal oxide doped with aluminum (Al), and this is not particularly limited.

[0046] The above lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it is soluble in water. Specifically, the above lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7, and any one or more of these may be used.

[0047] According to a more preferred embodiment of the present invention, the first firing and the second firing are performed in a plurality of crucibles. The first fired product, which is fired in the first firing from the plurality of crucibles, is taken out and collected in a single container. The collected first fired product is then divided again and placed into a plurality of crucibles for second firing. At this time, the first fired product can be naturally mixed through the process of taking out the first fired product and collecting it in a single container. Since the first fired product is collected in a single container and then divided again into a plurality of crucibles to be placed into the first firing, the first fired product is mixed evenly, thereby significantly reducing the deviation within and between crucibles and allowing the second firing to proceed in a uniform state.

[0048] The above primary calcined material may not undergo a grinding and classification step before proceeding with secondary calcination. Conventionally, when primary and secondary calcination are performed, it was common practice to undergo a grinding and classification step of the primary calcined material after the primary calcination and before the secondary calcination. In this case, not only is the process time increased, but the content of magnetic impurities increases due to grinding of the grinder, and there is a possibility that the ground grinder fragments may react with the cathode active material components at high temperatures during secondary calcination, which can adversely affect the final battery performance. Although an iron removal process can be added to eliminate magnetic impurities, there is a problem of additional process time and cost. However, in the case of a preferred embodiment of the present invention, by effectively fine-tuning the oxygen concentration in the RHK kiln, the phenomenon of clumping of the primary calcined product is eliminated to the greatest extent, thereby eliminating the need for grinding and classification after the primary calcination and before the secondary calcination. Furthermore, even after the secondary calcination, post-processing processes including a disintegration process can be facilitated and carried out uniformly, and as a result, a positive electrode active material having uniform particle size and uniform performance can be manufactured.

[0049] The above first calcination may be performed at 500 to 700°C to form a first calcined product, more preferably at 530 to 670°C, and even more preferably at 550 to 650°C. The first calcination is a step of mixing and reacting a positive electrode active material precursor and a lithium raw material, and by calcining at a relatively low temperature of 500 to 700°C, the strength of the calcined body of the first calcined product can be controlled to be low. This is because the lower the temperature at which calcination is performed, the lower the temperature at which lithium by-products on the particle surface are calcined, which may result in a weaker strength of the calcined body. By controlling the strength of the calcined body of the first calcined product to be weak, the strength of the calcined body after the subsequent second calcination can also be controlled to be lower compared to general calcination, and the disintegration process becomes easier, allowing for uniform disintegration.

[0050] The above first calcination can be carried out under an air or oxygen atmosphere. Calcining under an air or oxygen atmosphere may have the effect of promoting the oxidation reaction of the precursor more than calcining under an inert atmosphere.

[0051] The above secondary calcination may be performed at 700 to 900°C, more preferably at 730 to 870°C, and even more preferably at 750 to 850°C. The above secondary calcination may be performed under an air or oxygen atmosphere. Calcining under an air or oxygen atmosphere may have the effect of promoting the oxidation reaction of the precursor, crystal growth, and phase change compared to calcining under an inert atmosphere.

[0052] Since the second calcination is a step in which a small amount of residual lithium that was not reacted in the first calcination reacts, the strength of the sintered lithium transition metal oxide after the second calcination can be controlled to be lower than that of general calcination, and the disintegration process can be made easier and disintegrated uniformly, thereby obtaining uniform particle size and crystal size, and reducing post-processing deviations such as uneven washing or coating, so that as a result, a positive electrode active material for a secondary battery with small performance deviation and excellent electrochemical properties can be manufactured.

[0053] The lithium transition metal oxide after the above secondary calcination may optionally undergo post-processing steps such as disintegration, washing, and / or coating. The disintegration involves crushing aggregated particles in the form of a calcined body, and specifically, this can be performed using equipment such as an air classifying mill (acm). After disintegration, the high-nickel (High-Ni) NCM-based lithium transition metal oxide with 70 mol% or more nickel may optionally undergo a coating process after a washing process, while the low-nickel (Low-Ni) NCM-based lithium transition metal oxide with less than 70 mol% nickel may optionally undergo a coating process immediately without washing.

[0055] <Cathode and Lithium Secondary Batteries>

[0056] According to another embodiment of the present invention, a cathode for a secondary battery and a lithium secondary battery are provided, comprising a cathode material manufactured as described above.

[0058] Specifically, the positive electrode comprises a positive current collector and a positive active material layer formed on the positive current collector, the positive active material layer comprising the positive active material.

[0059] In the above-mentioned positive electrode, the positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above-mentioned positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the above-mentioned positive current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0061] In addition, the above-mentioned positive active material layer may include a conductive material and a binder along with the positive active material described above.

[0062] At this time, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that possesses electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The conductive material may typically be included in an amount of 1 to 30 weight percent relative to the total weight of the positive electrode active material layer.

[0064] In addition, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.

[0066] The above-described anode may be manufactured according to a conventional anode manufacturing method, except for using the above-described anode active material. Specifically, it may be manufactured by applying a composition for forming an anode active material layer, comprising the above-described anode active material and optionally a binder and a conductive material, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.

[0067] The above solvent may be a solvent commonly used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it is sufficient to dissolve or disperse the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can exhibit excellent thickness uniformity when coated for anode manufacturing thereafter.

[0069] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0071] According to another embodiment of the present invention, an electrochemical device comprising the anode is provided. Specifically, the electrochemical device may be a battery or a capacitor, and more specifically, may be a lithium secondary battery.

[0073] The above lithium secondary battery specifically comprises a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0075] In the above lithium secondary battery, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0076] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0078] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a cathode forming composition comprising a cathode active material and optionally a binder and a conductive material onto a cathode current collector and drying it, or by casting the cathode forming composition onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.

[0080] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ β Examples include metal oxides capable of doping and dedoping lithium, such as (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, low-crystallinity carbon and high-crystallinity carbon may all be used as the carbon material. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0081] In addition, the binder and conductive material mentioned above may be the same as those described above for the anode.

[0083] Meanwhile, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator typically used in lithium secondary batteries may be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0085] In addition, the electrolytes used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing lithium secondary batteries, but are not limited to these.

[0087] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0088] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.

[0090] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0092] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds like difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.

[0094] As described above, since the lithium secondary battery applying the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it is useful in fields such as portable devices like mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0096] Accordingly, according to another embodiment of the present invention, a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same are provided.

[0097] The above battery module or battery pack can be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0099] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0101] Examples 1

[0102] positive electrode active material precursor Ni0 . 88 Co0 . 05 Mn0 .07Al(OH)3, a doping raw material, was added to (OH)2, and LiOH·H2O, a lithium raw material, was added so that the Li / Metal(Ni,Co,Mn,Al) molar ratio was 1.05, and these were mixed. The mixed powder was placed into multiple alumina crucibles for calcination. Subsequently, the mixture was calcined at 620°C under an oxygen atmosphere for 5 hours to form a primary calcined product. Afterward, the primary calcined products from the multiple crucibles were removed and collected into one large container, and the collected primary calcined products were further divided and placed into multiple crucibles. Subsequently, a secondary calcination was performed at 763°C under an oxygen atmosphere for 5 hours to produce a lithium transition metal oxide with a nickel:cobalt:manganese:aluminum molar ratio of 86:5:7:2. Subsequently, 0.1 wt% of H3BO was mixed into the powder that had undergone grinding, washing, and drying processes, and B-coated cathode active material powder was prepared by heat treating it for 5 hours under an air atmosphere at 295°C.

[0104] Example 2

[0105] A positive electrode active material powder was prepared by carrying out the same procedure as in Example 1, except that the lithium raw material was added so that the Li / Metal(Ni,Co,Mn,Al) molar ratio was 1.07.

[0107] Comparative example 1

[0108] Positive electrode active material precursor Ni 0.88 Co 0.05 Mn 0.07Al(OH)3, a doping raw material, was added to (OH)2, and the lithium raw material LiOH·H2O was added and mixed so that the Li / Metal(Ni,Co,Mn,Al) molar ratio was 1.05. The mixed powder was placed into multiple alumina crucibles for calcination. Subsequently, the mixture was calcined at 763°C under an oxygen atmosphere for 10 hours to produce a lithium transition metal oxide with a nickel:cobalt:manganese:aluminum molar ratio of 86:5:7:2. After grinding, washing, and drying processes, 0.1 wt% of H3BO3 was mixed into the powder, and the mixture was heat-treated at 295°C under an air atmosphere for 5 hours to produce a B-coated cathode active material powder.

[0110] Comparative example 2

[0111] A positive electrode active material powder was prepared in the same manner as Comparative Example 1, except that a lithium raw material was added so that the Li / Metal(Ni,Co,Mn,Al) molar ratio was 1.07.

[0113] [ Experimental Example 1: Evaluation of Decision Size Deviation]

[0114] In order to verify the crystallite size deviation of the positive active material powders prepared in Examples 1 and 2 and Comparative Examples 1 and 2, a total of 9 powder samples were sampled from each of the 3 crucibles at the upper, middle, and lower positions, and after XRD (Ultima IV) measurement, the average crystallite size was calculated using the Scherrer equation, and the standard deviation and relative standard deviation were calculated, and the results are shown in Table 1 and Figure 1 below.

[0115] Relative standard deviation (%) = Standard deviation / Mean * 100

[0116] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sample 1 (nm) 113.0 111.1 129.0 103.2 Sample 2 (nm) 108.4 116.7 106.0 128.6 Sample 3 (nm) 110.7 118.2 127.7 131.6 Sample 4 (nm) 114.4 122.3 112.4 122.8 Sample 5 (nm) 117.3 121.4 105.3 109.0 Sample 6 (nm) 118.3 118.9 123.3 103.9 Sample 7 (nm) 113.5 109.9 104.5 110.5 Sample 8 (nm) 107.1 113.8 100.1 116.3 Sample 9 (nm) 113.5 116.2 112.5 124.2 Average (nm) 112.9 116.5 113.4 116.7 Standard deviation (nm) 3.4997 4.0337 10.1332 10.0059 Relative standard deviation (%) 3.0995 3.4624 8.9341 8.5756

[0118] Referring to Table 1 and Figure 1 above, in the case of Examples 1 and 2, the standard deviation of the crystal size was small at 5.0 nm or less, and the relative standard deviation was small at 4.0% or less. On the other hand, in the case of Comparative Examples 1 and 2, the standard deviation of the crystal size and the relative standard deviation were significantly larger compared to Examples 1 and 2.

[0120] [Experimental Example 2: Evaluation of a-axis and c-axis lattice constant deviations]

[0121] To verify the deviations in the a-axis and c-axis lattice constants of the cathode active material powders prepared in Examples 1 and 2 and Comparative Examples 1 and 2, a total of 9 powder samples were sampled from each of the three crucibles at the upper, middle, and lower positions, and the average value of each lattice constant was calculated by indexing the XRD (Ultima IV) measurement data through Rietveld refinement, and the standard deviation and relative standard deviation were calculated, and the results are shown in Tables 2 and 3 and Figures 2 and 3 below.

[0122] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sample 1 (Å) 2.8657 2.8505 2.8677 2.8537 Sample 2 (Å) 2.8642 2.8490 2.8692 2.8422 Sample 3 (Å) 2.8673 2.8523 2.8643 2.8573 Sample 4 (Å) 2.8639 2.8493 2.8623 2.8459 Sample 5 (Å) 2.8646 2.8496 2.8657 2.8447 Sample 6 (Å) 2.8664 2.8516 2.8675 2.8514 Sample 7 (Å) 2.8671 2.8522 2.8611 2.8500 Sample 8 (Å) 2.8659 2.8510 2.8698 2.8524 Sample 9 (Å) 2.8668 2.8510 2.8607 2.8523 Average (Å) 2.8658 2.8507 2.8654 2.8500 Standard deviation (Å) 0.0012 0.0011 0.0032 0.0045 Relative standard deviation (%) 0.0418 0.0403 0.1134 0.1594

[0124] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sample 1 (Å) 14.1762 14.1702 14.1761 14.1681 Sample 2 (Å) 14.1783 14.1724 14.1813 14.1513 Sample 3 (Å) 14.1736 14.1678 14.1706 14.1678 Sample 4 (Å) 14.1783 14.1733 14.1783 14.1713 Sample 5 (Å) 14.1729 14.1669 14.1714 14.1801 Sample 6 (Å) 14.1804 14.1740 14.1874 14.1740 Sample 7 (Å) 14.1717 14.1677 14.1687 14.1617 Sample 8 (Å) 14.1759 14.1738 14.1759 14.1751 Sample 9 (Å) 14.1794 14.1744 14.1864 14.1644 Average (Å) 14.1763 14.1712 14.1773 14.1682 Standard deviation (Å) 0.0029 0.0029 0.0063 0.0080 Relative standard deviation (%) 0.0203 0.0202 0.0445 0.0564

[0126] Referring to Tables 2 and 3 and Figures 2 and 3 above, in the case of Examples 1 and 2, the standard deviations of the a-axis and c-axis lattice constants were small, at 0.002 Å and 0.003 Å or less, respectively, and the relative standard deviations were small, at 0.05% and 0.03% or less, respectively. On the other hand, in the case of Comparative Examples 1 and 2, the standard deviations and relative standard deviations of the a-axis and c-axis lattice constants were significantly larger compared to Examples 1 and 2.

[0128] [Experimental Example 3: Evaluation of Deviation in Residual Lithium By-products]

[0129] To determine the deviation in the weight percentage of lithium by-products remaining on the surface of the cathode active material powders prepared in Examples 1 and 2 and Comparative Examples 1 and 2, a total of 9 powder samples were sampled from each of the 3 crucibles at the upper, middle, and lower positions. 5g of each cathode active material powder sample was placed in 100g of distilled water, stirred for 5 minutes, and then filtered. The amount of residual lithium by-products (LiOH, Li2CO3) was calculated by adding a 0.1M HCl aqueous solution to the filtrate and titrating the pH. The average, standard deviation, and relative standard deviation were calculated, and the results are shown in Table 4 and Figure 4 below.

[0130] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sample 1 (wt%) 0.490 0.508 0.488 0.532 Sample 2 (wt%) 0.496 0.509 0.476 0.542 Sample 3 (wt%) 0.510 0.524 0.517 0.519 Sample 4 (wt%) 0.478 0.495 0.458 0.496 Sample 5 (wt%) 0.472 0.519 0.462 0.529 Sample 6 (wt%) 0.485 0.510 0.515 0.483 Sample 7 (wt%) 0.481 0.503 0.531 0.491 Sample 8 (wt%) 0.498 0.514 0.478 0.519 Sample 9 (wt%) 0.502 0.502 0.512 0.500 Average (wt%) 0.490 0.509 0.493 0.512 Standard deviation (wt%) 0.0116 0.0084 0.0249 0.0193 Relative standard deviation (%) 2.3726 1.6453 5.0551 3.7758

[0132] Referring to Table 4 and Figure 4 above, in the case of Examples 1 and 2, the standard deviation of residual lithium byproducts was small at 0.02 wt% or less, and the relative standard deviation was small at 3.0% or less. On the other hand, in the case of Comparative Examples 1 and 2, the standard deviation and relative standard deviation of residual lithium byproducts were significantly larger compared to Examples 1 and 2.

[0134] [ Experimental Example 4: Battery Capacity Variation Evaluation]

[0135] To check the battery capacity variation of the positive electrode active material powders prepared in Examples 1 and 2 and Comparative Examples 1 and 2, a total of 9 powder samples were sampled from each of the 3 crucibles at the upper, middle, and lower positions.

[0136] A positive electrode slurry was prepared by mixing each positive electrode active material powder sample, FX35 conductive material, and KF9700 / BM730H binder in N-methylpyrrolidone (NMP) solvent in a weight ratio of 97.5:1:1.35:0.15. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and then rolled to produce a positive electrode.

[0137] Meanwhile, a Li metal disk was used as the negative electrode active material.

[0138] An electrode assembly was manufactured by interposing a separator between the anode and cathode prepared as described above, and the electrode assembly was placed inside a case, after which an electrolyte was injected into the case to manufacture a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1.0 M concentration lithium hexafluorophosphate (LiPF6) in an organic solvent composed of ethylene carbonate / ethyl methyl carbonate / diethyl carbonate (mixed volume ratio of EC / EMC / DEC = 3 / 3 / 4).

[0139] For each lithium secondary battery half-cell manufactured as described above, a charge-discharge experiment was conducted by charging at 25°C in CCCV mode until it reached 4.25V at 0.1C (termination current 0.05C), and discharging at a constant current of 0.1C until it reached 3.0V. The discharge capacity and discharge capacity deviation were checked, and the results are shown in Table 5 and Figure 5 below.

[0140] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sample 1 (mAh / g) 216.2 215.0 213.3 213.1 Sample 2 (mAh / g) 216.3 215.7 212.3 211.6 Sample 3 (mAh / g) 216.8 216.3 214.8 210.8 Sample 4 (mAh / g) 215.5 216.1 215.1 210.9 Sample 5 (mAh / g) 217.0 215.3 214.8 213.9 Sample 6 (mAh / g) 215.8 215.9 213.7 214.0 Sample 7 (mAh / g) 216.1 215.8 214.9 213.6 Sample 8 (mAh / g) 216.0 216.0 211.7 214.2 Sample 9 (mAh / g) 216.8 215.1 212.3 213.2 Average (mAh / g) 216.3 215.7 213.7 212.8 Standard deviation (mAh / g) 0.4732 0.4306 1.2420 1.2714 Relative standard deviation (%) 0.2188 0.1996 0.5813 0.5974

[0142] Referring to Table 5 and Figure 5 above, in the case of Examples 1 and 2, the standard deviation of the discharge capacity of the lithium secondary battery was small, and the relative standard deviation was also small. On the other hand, in the case of Comparative Examples 1 and 2, the standard deviation and relative standard deviation of the discharge capacity of the lithium secondary battery were significantly larger compared to Examples 1 and 2.

Claims

Claim 1 A positive active material powder for a secondary battery comprising a lithium transition metal oxide containing nickel (Ni), cobalt (Co), and manganese (Mn), wherein the particles of the lithium transition metal oxide are in the form of secondary particles formed by the aggregation of primary particles, and the positive active material constituting the positive active material powder has a crystallite size of 90 to 140 nm, the standard deviation of the crystallite size of the positive active material constituting the positive active material powder is 5.0 nm or less, and the relative standard deviation is 4.0% or less. Claim 2 A positive active material powder for a secondary battery according to claim 1, wherein the standard deviation of the a-axis lattice constant of the positive active material constituting the positive active material powder is 0.002 Å or less and the relative standard deviation is 0.05% or less. Claim 3 A positive active material powder for a secondary battery according to claim 1, wherein the standard deviation of the c-axis lattice constant of the positive active material constituting the positive active material powder is 0.003 Å or less and the relative standard deviation is 0.03% or less. Claim 4 A positive electrode active material powder for a secondary battery according to claim 1, wherein the standard deviation of the weight percentage of lithium byproducts remaining on the surface relative to the weight of the positive electrode active material constituting the positive electrode active material powder is 0.02 wt% or less, and the relative standard deviation is 3.0% or less. Claim 5 In claim 1, the lithium transition metal oxide is a positive electrode active material powder for a secondary battery in which nickel is 70 mol% or more of the total metal excluding lithium. Claim 6 A method for manufacturing a positive electrode active material powder for a secondary battery according to claim 1, comprising mixing a positive electrode active material precursor containing nickel (Ni), cobalt (Co), and manganese (Mn) with a lithium raw material, performing a first calcination to form a first calcined product, and then performing a second calcination to form a lithium transition metal oxide. Claim 7 A method for manufacturing a positive electrode active material powder for a secondary battery according to claim 6, wherein the first calcination and second calcination are performed in a plurality of crucibles, the first calcined product obtained from the first calcination in the plurality of crucibles is taken out and collected in one container, the collected first calcined product is subdivided again and introduced into a plurality of crucibles, and then second calcined. Claim 8 A method for manufacturing a positive electrode active material powder for a secondary battery according to claim 6, wherein a second calcination is performed without the step of crushing and classifying the first calcined product. Claim 9 A method for manufacturing a positive electrode active material powder for a secondary battery, wherein, in claim 6, the first calcination is performed by calcining at 500 to 700°C to form a first calcined product. Claim 10 A method for manufacturing a positive electrode active material powder for a secondary battery, wherein, in claim 6, the secondary calcination is performed at 700 to 900°C. Claim 11 A method for manufacturing a positive electrode active material powder for a secondary battery, wherein the first and second calcination are performed under an air or oxygen atmosphere. Claim 12 A positive electrode for a secondary battery comprising a positive electrode active material according to any one of claims 1 to 5. Claim 13 A lithium secondary battery comprising a positive electrode according to Article 12.

Citation Information

Patent Citations

  • Positive electrode active material for secondary battery, method for producing the same, positive electrode and secondary battery comprising the same

    KR1020180114412A

  • Positive active material for lithium secondary battery, preparing method thereof, and lithium secondary battery comprising positive electrode including positive active material

    KR1020190065963A

  • Positive electrode active material for lithium secondary battery and producing method thereof, positive electrode and lithum secondary battery comprising the same

    KR1020190129615A

  • Positive electrode active material for secondary battery, method for preparing the same and lithium secondary battery comprising the same

    KR1020190131842A