Positive electrode active material, positive electrode and lithium secondary battery comprising the same

A lithium composite transition metal oxide with a high nickel content and optimized Al/Ni ratio stabilizes the lattice, addressing structural instability and resistance issues, resulting in high capacity and extended lifespan.

KR103047153B1Active Publication Date: 2026-11-11LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020230133819
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-06
Publication Date
2026-11-11
Estimated Expiration
2043-10-06

AI Technical Summary

Technical Problem

Conventional high-nickel cathode active materials for lithium-ion batteries suffer from structural instability, lattice changes, and increased resistance due to high nickel content, leading to reduced capacity and lifespan.

Method used

A positive electrode active material comprising a lithium composite transition metal oxide with a nickel content of 90 mol% or more, a controlled molar ratio of aluminum to nickel (Al/Ni) between 0.015 to 0.034, and a specific crystal structure, which stabilizes the lattice and enhances doping yield.

Benefits of technology

The material achieves high capacity, improved structural stability, and extended lifespan by minimizing volume changes and resistance, while reducing cobalt content for cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023110161425-PAT00001_ABST
    Figure 112023110161425-PAT00001_ABST
Patent Text Reader

Abstract

The present invention provides a positive electrode active material comprising a lithium composite transition metal oxide comprising nickel, cobalt, manganese, and aluminum, wherein the lithium composite transition metal oxide has a nickel content of 90 mol% or more among metals excluding lithium and an Al / Ni molar ratio of aluminum to nickel of 0.015 to 0.034, a positive electrode comprising the positive electrode active material, and a lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a positive electrode active material, a positive electrode containing the same, and a lithium secondary battery. Background Technology

[0002] With the recent rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, the demand for small, lightweight, and relatively high-capacity rechargeable batteries is increasing rapidly. In particular, lithium-ion batteries are gaining prominence as power sources for portable devices due to their lightweight nature and high energy density. Consequently, active research and development efforts are underway to improve the performance of lithium-ion batteries.

[0003] A lithium secondary battery produces electrical energy through oxidation and reduction reactions when lithium ions are inserted into or removed from the positive and negative electrodes, in a state where an organic or polymer electrolyte is charged between a positive electrode and a negative electrode composed of active materials capable of lithium ion intercalation and deintercalation.

[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compounds (LiFePO4) have been used as cathode active materials for lithium secondary batteries. Furthermore, as a method to improve the low thermal stability of LiNiO2 while maintaining its excellent reversible capacity, lithium composite metal oxides (hereinafter simply referred to as 'NCM-based lithium composite transition metal oxides') in which a portion of the nickel (Ni) is substituted with cobalt (Co) and manganese (Mn) have been developed. However, conventionally developed NCM-based lithium composite transition metal oxides had limitations in application due to insufficient capacity characteristics.

[0005] To address these issues, recent research has focused on increasing the Ni content in NCM-based lithium composite transition metal oxides. However, high-nickel cathode active materials with high nickel content generate large amounts of gas during the charge-discharge process due to the high reactivity of nickel. Furthermore, they suffer from significant lattice structural instability caused by cation mixing and oxygen desorption, as well as an increase in the content of residual lithium impurities on the surface.

[0006] Therefore, there is a need to develop cathode materials containing a high nickel content that offer excellent capacity while simultaneously ensuring structural stability. Prior art literature

[0007] (Patent Document 0001) KR 10-2020-0070647 A The problem to be solved

[0008] The present invention aims to provide a positive electrode active material with improved dispersibility, a positive electrode slurry containing the same, a positive electrode, and a lithium secondary battery. means of solving the problem

[0009] The present invention relates to a positive electrode active material comprising a lithium complex transition metal oxide comprising nickel, cobalt, manganese, and aluminum, wherein

[0010] The present invention provides a positive electrode active material in which the content of nickel among the metals excluding lithium in the above lithium composite transition metal oxide is 90 mol% or more, and the molar ratio of aluminum to nickel, Al / Ni, is 0.015 to 0.034.

[0011] In addition, the present invention provides a positive electrode comprising: a positive current collector; and a positive active material layer provided on at least one surface of the positive current collector, wherein the positive active material layer comprises the aforementioned positive active material.

[0012] In addition, the present invention provides a lithium secondary battery comprising the aforementioned positive electrode; a negative electrode comprising a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and an electrolyte. Effects of the invention

[0013] The cathode active material according to the present invention has a high nickel content and excellent capacity, and since the amount of cobalt used can be reduced accordingly, it is advantageous in terms of material supply and price.

[0014] In addition, an optimal Al / Ni molar ratio is provided that can evenly improve doping yield, resistance characteristics, and structural stability in NCMA oxide, and accordingly, a lithium secondary battery with improved charge / discharge capacity and high-temperature life can be provided by including said NCMA oxide. Brief explanation of the drawing

[0015] Figure 1 is a graph showing the change in heat flow rate according to temperature of a positive electrode active material containing a lithium composite transition metal oxide prepared in the examples and comparative examples. Figure 2 is a graph showing the capacity retention rate and resistance increase rate at high temperature of a half cell containing a lithium composite transition metal oxide prepared in the examples and comparative examples as an anode active material. Specific details for implementing the invention

[0016] The present invention will be described in detail below.

[0018] In the present invention, the content of each element in the positive electrode active material can be measured by Inductively Coupled Plasma Optical Emission Spectroscopy (ICP-OES). Specifically, this means dissolving 0.03g of the positive electrode active material to be analyzed in 1mL of hydrochloric acid, adding a small amount of hydrogen peroxide and hydrofluoric acid, diluting with 50mL of ultrapure water, and then analyzing using an Avio series (PerkinElmer, Inc) instrument.

[0019] In the present invention, “primary particle” refers to a particle unit in which no grain boundaries appear when observed at a field of view of 5,000 to 20,000 times using a scanning electron microscope.

[0020] In the present invention, “a-axis” and “c-axis” refer to axial directions in the crystal structure of the primary particle. The crystal structure of the primary particle was confirmed through TEM-SAED (Transmission Electron Microscope-Selected Area Electron diffraction) analysis. The length in the c-axis direction and the length in the a-axis direction can be quantitatively analyzed using X-ray diffraction analysis (XRD) by Cu Kα X-rays.

[0021] In the present invention, “X-ray diffraction analysis (XRD)” can be performed by placing a particle to be measured into a holder, irradiating the particle with X-rays, and analyzing the resulting diffraction grating. Sampling was prepared by placing a powder sample of the particle to be measured into a recessed groove in the center of a general powder holder, smoothing the surface using a slide glass, and ensuring the sample height was equal to the edge of the holder. Then, X-ray diffraction analysis was performed using a Bruker D8 Endeavor (light source: Cu Kα, λ=1.54Å) equipped with a LynxEye XE-T position-sensitive detector, under conditions of a step size of 0.02° and a total scan time of approximately 20 minutes for the FDS 0.5°, 2θ=15°~90° region. For the measured data, Rietveld refinement was performed considering the charge at each site (metal ions at transition metal sites are +3, and Ni ions at Li sites are +2) and cation mixing. Instrumental brodadening was considered using the Fundamental Parameter Approach (FPA) implemented in the Bruker TOPAS program, and all peaks of the measurement range were used for fitting. The peak shape was fitted using only the Lorenzian contribution as the First Principle (FP) among the peak types available in TOPAS, and strain was not considered.

[0022] In the present invention, “particle strength” is a value expressed in pressure units (MPa) representing the force at which a particle breaks when a particle is placed in a microcompression testing machine, such as the Anton Paar Step 500, the shape of the particle to be measured is secured using a microscope, and a force is applied to the particle using a tip. Considering the deviation between particles, values ​​measured at least 10 times are mapped, and the average value is used as the particle strength value.

[0023] In the present invention, “D 50 " represents the particle size corresponding to 50% of the volume cumulative particle size distribution of the corresponding particle powder, and can be measured using the laser diffraction method. For example, after dispersing the cathode active material powder in a dispersion medium, it can be introduced into a commercially available laser diffraction particle size measuring device (e.g., Malvern, Mastersizer 3000), irradiated with ultrasound of approximately 28 kHz at an output of 60 W, and then obtained a volume cumulative particle size distribution graph, and the particle size at the point where the volume cumulative amount is 50% can be measured from the obtained volume cumulative particle size distribution graph.

[0025] Hereinafter, each component of the present invention will be described in more detail.

[0027] <Cathode Active Material>

[0028] The present invention relates to a positive electrode active material, specifically a positive electrode active material for a lithium secondary battery.

[0029] The positive electrode active material according to the present invention comprises a lithium composite transition metal oxide comprising nickel, cobalt, manganese, and aluminum, wherein the content of nickel among the metals excluding lithium in the lithium composite transition metal oxide is 90 mol% or more, and the molar ratio of aluminum to nickel, Al / Ni, is 0.015 to 0.034.

[0030] As mentioned above, while increasing the nickel content in lithium composite transition metal oxides can secure high capacity, it leads to a problem of reduced structural stability. Specifically, high-nickel cathode active materials contain a large amount of lithium compounds remaining on the surface, which can cause side reactions during the charging and discharging process, such as generating gas, thereby contributing to reduced stability.

[0031] Furthermore, high-nickel cathode active materials have the disadvantage of undergoing significant changes in lattice constants, specifically volume within the unit cell; these volume changes cause cracks to form within the active material particles. These cracks can lead to the formation of voids within the active material, which can result in a degradation of battery performance.

[0032] Furthermore, due to the high nickel content, cation mixing between lithium and nickel ions occurs frequently; this hinders the movement of lithium ions during battery operation, causing increased battery resistance and degraded lifespan.

[0033] Accordingly, the inventors have resolved the above problem by controlling the ratio of nickel to doping elements—specifically, the molar ratio of Ni and Al in a lithium composite transition metal oxide (hereinafter referred to as NCMA oxide) containing Ni, Co, Mn, and Al—within an optimal range for an ultra-high nickel cathode active material having a nickel content of 90 mol% or more. Al can prevent degradation by reducing volume changes within the unit cell in NCMA oxides having a Ni content of 90 mol% or more, thereby suppressing cracking of active material particles and reducing voids. Therefore, the cathode active material according to the present invention can achieve high capacity while simultaneously exhibiting excellent thermal stability and lifespan characteristics. However, since Al does not contribute to capacity and an excess amount of Al can actually hinder capacity development, it is important to appropriately control the content of Al relative to Ni.

[0034] Specifically, Al / Ni, which is the molar ratio of aluminum to nickel, may be 0.015 or higher, 0.021 or higher, or 0.030 or higher, and may be 0.034 or lower, or 0.032 or lower. If Al / Ni is less than 0.015, the lifespan characteristics are degraded due to a rapid volume change within the unit cell caused by an increase in nickel content, and structural instability increases, causing the main peak temperature at which the heat flow is maximum to drop, making it difficult to achieve the aforementioned effects. Conversely, if it exceeds 0.034, the excess amount of Al causes undoped residues to remain on the surface of the active material, hindering the movement of lithium ions, which is undesirable in that surface resistance increases and the capacity developed decreases.

[0036] In one embodiment of the present invention, the content of nickel among the metals excluding lithium in the lithium composite transition metal oxide may be 92 mol% or more, preferably 93 mol% or more, and more preferably 93 mol% to 95 mol%. This is desirable in that it is possible to secure an Al content of at least a certain amount while achieving a high capacity.

[0037] In addition, the content of cobalt among the metals excluding lithium in the lithium composite transition metal oxide may be 0.1 mol% to 1.0 mol%, preferably 0.2 mol% to 0.9 mol%, and more preferably 0.4 mol% to 0.8 mol%. That is, in the present invention, lifespan, resistance, and output characteristics are improved by controlling the Al / Ni molar ratio while minimizing the content of expensive cobalt.

[0038] In addition, the aluminum content among the metals excluding lithium in the lithium composite transition metal oxide may be 1.0 mol% to 5.0 mol%, preferably 1.5 mol% to 4.0 mol%, and more preferably 2.0 mol% to 3.8 mol%. When the aluminum content is within the above range, it is easy to adjust the Al / Ni molar ratio to the optimal range described above in NCMA oxides in which the nickel content is 90 mol% or more.

[0039] Specifically, the lithium composite transition metal oxide may have the composition of Chemical Formula 1 below.

[0040] [Chemical Formula 1]

[0041] Li 1+x (Ni a Co b Mn c Al d M1 e )O2

[0042] In the above chemical formula 1,

[0043] M1 is one or more selected from the group consisting of Ti, Zr, W, Mo, Nb, Cu, Fe, V, Cr, Zn, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Mg, and B, and

[0044] x, a, b, c, d, and e are -0.2≤x≤0.2, 0.90≤a<1, 0, respectively. <b≤0.01, 0<c≤0.05, 0<d≤0.05, 0≤e≤0.05, a+b+c+d+e=1을 만족한다.

[0045] The above 1+x represents the molar ratio of lithium in the lithium composite transition metal oxide, and may be -0.1≤x≤0.2 or 0≤x≤0.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium composite transition metal oxide can be stably formed.

[0046] The above 'a' represents the molar ratio of nickel among all metals excluding lithium in the lithium composite transition metal oxide, and may be 0.920≤a<1, 0.930≤a<1, or 0.930≤a≤0.950. When the molar ratio of nickel satisfies the above range, high energy density is exhibited, making it possible to realize high capacity.

[0047] The above b represents the molar ratio of cobalt among the total metals excluding lithium in the lithium composite transition metal oxide, where 0 <b≤0.009, 0<b≤0.008, 또는 0<b≤0.006일 수 있다. 코발트의 몰비가 상기 범위를 만족할 때, 최소한의 양으로 양호한 저항 특성 및 출력 특성을 구현할 수 있다.

[0048] The above c represents the molar ratio of manganese among the total metals excluding lithium in the lithium composite transition metal oxide, where 0 <c≤0.050, 0<c≤0.040, 또는 0<c≤0.030일 수 있다. 망간의 몰비가 상기 범위를 만족할 때, 양극 활물질의 구조 안정성이 우수하게 나타난다.

[0049] The above d represents the molar ratio of Al among the total metals excluding lithium in the lithium composite transition metal oxide, and the above d may be 0.010≤d≤0.050, 0.015≤d≤0.040, or 0.020≤d≤0.038.

[0050] The above e represents the molar ratio of element M1 among all metals excluding lithium in the lithium composite transition metal oxide, and can be adjusted as needed.

[0052] Meanwhile, the above-mentioned positive electrode active material comprises primary particles and secondary particles formed by the aggregation of the primary particles, and the ratio of the length in the a-axis direction to the length in the c-axis direction of the primary particles, c / a, may be 4.9400 to 4.9500, preferably 4.9400 to 4.9450, and more preferably 4.9405 to 4.9422. A c / a ratio falling within the above range implies that the layered structure of the positive electrode active material is highly complete. Therefore, when the c / a ratio falls within the above range, the movement of lithium ions during charging and discharging is smooth and volume change is minimal, which is effective in improving the characteristics of lifespan degradation due to cycle progression.

[0053] In addition, D of the above positive active material 50The particle size may be 8㎛ to 15㎛, preferably 10㎛ to 13㎛, more preferably 11㎛ to 12㎛, and the average particle size of the primary particle may be 0.3㎛ to 2.0㎛, preferably 0.5㎛ to 1.5㎛, more preferably 0.7㎛ to 1.0㎛, but is not limited thereto.

[0054] Meanwhile, since the bonding energy between Al and O is greater than the bonding energy between Ni and O, the molar ratio of Al / Ni is controlled to the range described above, thereby improving the particle strength. For example, the particle strength of the anode active material may be 142 MPa to 160 MPa, preferably 145 MPa to 155 MPa, and more preferably 150 MPa to 155 MPa. When the particle strength is within the above range, breakage of the anode active material during electrode rolling is minimized, and as side reactions with the electrolyte are reduced, the rate of increase in resistance of the battery can be lowered.

[0055] Meanwhile, when the heat flow of the anode active material is measured using differential scanning calorimetry (DSC), a peak with maximum heat flow may appear at 219°C to 230°C, specifically at 220°C to 230°C, and more specifically at 225°C to 230°C.

[0056] In addition, the maximum heat flow of the anode active material measured in the range of 25°C to 300°C using differential scanning calorimetry (DSC) may be 85.0 W / g or less, 70.0 W / g or less, or 60.0 W / g or less.

[0057] In other words, the positive electrode active material according to the present invention has the advantage of a relatively low risk of explosion even when the internal temperature of the battery rises, because the peak temperature at which the heat flow rate is maximum is relatively high and the maximum value of the heat flow rate is small.

[0059] Meanwhile, the above-mentioned positive electrode active material is subjected to a co-precipitation reaction while supplying a transition metal-containing solution containing a transition metal precursor, an ammonium cation complex forming agent, and a basic compound to a reactor to form a composite transition metal precursor having a nickel content of 90 mol% or more;

[0060] It can be manufactured by a manufacturing method comprising the step of mixing the above-mentioned composite transition metal precursor, lithium raw material, and aluminum raw material, and heat-treating to form an Al-doped lithium composite transition metal oxide.

[0061] At this time, the heat treatment can be performed at 600°C to 900°C, preferably 650°C to 850°C, more preferably 700°C to 800°C for 15 to 24 hours.

[0062] The step of forming the above-mentioned composite transition metal precursor can be prepared, for example, by dissolving each transition metal precursor in a solvent to prepare a transition metal-containing solution, then mixing the transition metal-containing solution, an ammonium cation complex-forming agent, and a basic compound, and then proceeding with a co-precipitation reaction. Additionally, if necessary, an oxidizing agent or oxygen gas may be further introduced during the co-precipitation reaction.

[0063] Meanwhile, the above transition metal precursor may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, etc. of each transition metal.

[0064] Specifically, the nickel precursor may be one or more selected from the group consisting of NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, and nickel sulfide, and the cobalt precursor may be one or more selected from the group consisting of Co(OH)2, Co3O4, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, and Co(SO4)2·7H2O. Additionally, the manganese precursor may be one or more selected from the group consisting of Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halides, and manganese sulfide.

[0065] At this time, the input amount of each of the above transition metal precursors can be determined by considering the molar ratio of the transition metal in the cathode active material to be finally produced.

[0066] Meanwhile, the ammonium cation complex forming agent may include at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3, and may be introduced into a reactor in the form of a solution in which said compound is dissolved in a solvent. At this time, the solvent may be water, or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.).

[0067] The above basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be introduced into the reactor in the form of a solution in which the compound is dissolved in a solvent. In this case, water or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.) may be used as the solvent.

[0068] As described above, when a transition metal-containing solution, an ammonium cation complex-forming agent, and a basic compound are introduced into a reactor and stirred, the transition metals in the transition metal-containing solution co-precipitate, thereby generating precursor particles in the form of transition metal hydroxides.

[0069] At this time, the transition metal-containing solution, ammonium cation complex-forming agent, and basic compound are added in amounts such that the pH of the reaction solution becomes within the desired range.

[0070] When precursor particles are formed in the manner described above, the precursor is obtained by separating them from the reaction solution. For example, the precursor can be obtained by filtering the reaction solution to separate it, and then washing and drying the separated precursor. At this stage, processes such as grinding and / or classification may be performed as necessary.

[0072] A lithium composite transition metal oxide is prepared by mixing the composite transition metal precursor prepared in this manner with a precursor containing a lithium raw material and metal element M1, and heat-treating the mixture.

[0073] As the above lithium raw material, lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or oxyhydroxides may be used, for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or mixtures thereof may be used.

[0074] Meanwhile, the lithium raw material and the composite transition metal precursor can be mixed such that the molar ratio of Li to the total metal in the precursor is 1:1 to 1.2:1, preferably 1:1 to 1.1:1. When the mixing ratio of the lithium raw material and the metal in the precursor satisfies the above range, the layered crystal structure of the lithium composite transition metal oxide is well developed, allowing for the production of a positive electrode active material with excellent capacity characteristics and structural stability.

[0075] In addition, the above aluminum raw material is Al The contained oxides, hydroxides, oxyhydroxides, halides, nitrates, carbonates, acetates, oxalates, citrates, or sulfates may be, for example, Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3 aluminum halides, or combinations thereof. Instead of adding the aluminum raw material together with the lithium raw material during the heat treatment step, it is acceptable to add the aluminum raw material to the transition metal-containing solution during the co-precipitation reaction.

[0076] If additional doping of metal element M1 occurs, the type and amount of metal element M1 added can be controlled by considering the type and content of metal element M1 included in the aforementioned cathode active material.

[0078] <Polar>

[0079] Next, the anode according to the present invention will be described.

[0080] The anode according to the present invention comprises the anode active material. Specifically, the anode according to the present invention comprises an anode current collector; and an anode active material layer provided on at least one surface of the anode current collector, wherein the anode active material layer comprises the anode active material. Since the anode active material is the same as previously described, a detailed description is omitted, and only the remaining components are described in detail below.

[0081] The above positive current collector may include a highly conductive metal, and is not particularly limited as long as it facilitates the adhesion of the positive active material layer and is non-reactive within the voltage range of the battery. The above positive current collector may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. Additionally, the above positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive active material. It may be used in various forms, such as films, sheets, foils, nets, porous bodies, foams, and nonwoven fabrics.

[0082] The above anode may be manufactured according to a conventional anode manufacturing method, except for using the above anode active material. Specifically, it may be manufactured by applying an anode slurry containing the above anode active material onto an anode current collector and then drying and rolling, or by casting the above anode slurry onto a separate support and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0083] In one embodiment of the present invention, the anode comprises an anode active material layer formed by coating an anode slurry containing the anode active material onto at least one surface of an anode current collector.

[0084] Meanwhile, the anode slurry may include the anode active material, binder, conductive material, and solvent.

[0085] Specifically, the binder may be one or more selected from the group consisting of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and preferably may be polyvinylidene fluoride.

[0086] The binder may be included in an amount of 0.5% to 3% by weight, preferably 1% to 3% by weight, and more preferably 1.5% to 2.5% by weight, based on the total weight of the solid content in the anode slurry. When the content of the binder is within the above range, sufficient adhesion to the current collector and inter-particle bonding are secured, thereby improving the durability of the anode while maintaining a low initial resistance.

[0087] The conductive material may be one or more selected from the group consisting of graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; carbon-based materials such as carbon fibers or carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and preferably carbon nanotubes or carbon black, most preferably carbon nanotubes.

[0088] The conductive material may be included in an amount of 0.1% to 2.5% by weight, preferably 0.5% to 2% by weight, and more preferably 1% to 2% by weight, based on the total weight of the solid content in the anode slurry. It is desirable that the content of the conductive material be within the above range in that it can reduce the dead volume while maintaining conductivity between active materials.

[0089] In addition, the anode slurry may optionally further include a dispersant, and the dispersant may be hydrogenated nitrile butadiene rubber (HNBR).

[0090] Meanwhile, the solvent of the anode slurry may be a solvent generally used in the relevant technical field, for example, N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), isopropyl alcohol, dimethyl formamide (DMF), acetone, water, or a mixture of two or more of these may be used. The solvent may be used in a way that the aforementioned anode slurry has an appropriate viscosity. For example, the solvent may be included so that the concentration of solids in the anode slurry is 60% by weight or more, preferably 60% to 90% by weight, and more preferably 60% to 80% by weight.

[0092] lithium secondary battery

[0093] Next, a lithium secondary battery according to the present invention will be described.

[0094] Specifically, the above lithium secondary battery comprises a positive electrode, a negative electrode containing a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Since the positive electrode is the same as previously described, a detailed description is omitted, and only the remaining components are described in detail below.

[0095] In addition, the lithium secondary battery may optionally further include a battery container that accommodates the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member that seals the battery container.

[0096] In the above lithium secondary battery, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0097] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 μm to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0098] The above-mentioned cathode active material layer optionally includes a binder and a conductive material together with the cathode active material.

[0099] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ β Examples include metal oxides capable of doping and dedoping lithium, such as (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. The negative electrode active material may be included in an amount of 80% to 99% by weight based on the total weight of the negative electrode active material layer.

[0100] The above binder is a component that assists in the bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1% to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0101] The above conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such conductive material is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; fluorinated carbon; metal powder such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. may be used.

[0102] The above-mentioned cathode active material layer can be manufactured by applying a cathode composite material, prepared by dissolving or dispersing a cathode active material and optionally a binder and a conductive material in a solvent, onto a cathode current collector and drying it, or by casting the cathode composite material onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.

[0103] Meanwhile, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator typically used in lithium secondary batteries may be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0104] In addition, the electrolytes used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing lithium secondary batteries, but are not limited to these.

[0105] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0106] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.

[0107] The above lithium salt may be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, as the anion of the above lithium salt, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may be at least one selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO2, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2, etc., may be used. It is preferable to use the lithium salt within the range of 0.1 to 4.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0108] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the above additives may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.

[0109] The external shape of the lithium secondary battery of the present invention is not particularly limited, but can be a cylindrical shape using a can, a prismatic shape, a pouch shape, or a coin shape.

[0110] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention exhibits stable charge / discharge capacity and lifespan characteristics, it can be used not only as a battery cell used as a power source for small devices such as mobile phones, laptop computers, and digital cameras, but also preferably as a unit cell for a battery module for medium to large devices containing a plurality of battery cells.

[0111] Examples of the above-mentioned medium-to-large devices include power tools, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems, but are not limited to these.

[0112] According to another embodiment of the present invention, a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same are provided.

[0114] The present invention will be explained in more detail below through specific embodiments.

[0116] [Example: Preparation of positive electrode active material]

[0117] Example 1.

[0118] 4 liters of distilled water were added to a co-precipitation reactor (capacity 20 L), and 100 mL of an aqueous ammonia solution with a concentration of 28 wt% was added while maintaining the temperature at 50°C. Then, a transition metal solution mixed with NiSO4, CoSO4, and MnSO4 such that the molar ratio of Ni:Co:Mn was 97.0:0.5:2.5, an aqueous ammonia solution, and a sodium hydroxide solution were added to the co-precipitation reactor, and a co-precipitation reaction was carried out to form a precursor. The precursor particles were separated, washed, and dried in an oven at 130°C to produce the precursor.

[0119] LiOH as a lithium raw material, the above-prepared precursor, and Al(OH)3 were mixed such that the molar ratio of Li:(Ni+Co+Mn):Al was 1:0.978:0.022, and a lithium composite transition metal oxide was prepared by heat treating at 720°C for 20 hours under an oxygen atmosphere.

[0121] Example 2.

[0122] A precursor was prepared using the same process as in Example 1 above. LiOH, the prepared precursor, and Al(OH)3 were mixed such that the molar ratio of Li:(Ni+Co+Mn):Al was 1:0.968:0.032, and a lithium composite transition metal oxide was prepared by heat treatment at 720°C for 20 hours under an oxygen atmosphere.

[0124] Comparative Example 1.

[0125] A precursor was prepared using the same process as in Example 1 above. LiOH was mixed with the prepared precursor so that the molar ratio of Li:(Ni+Co+Mn) was 1:1, and a lithium composite transition metal oxide was prepared by heat treatment at 720°C for 20 hours under an oxygen atmosphere.

[0127] Comparative Example 2.

[0128] A precursor was prepared using the same process as in Example 1 above. LiOH, the prepared precursor, and Al(OH)3 were mixed such that the molar ratio of Li:(Ni+Co+Mn):Al was 1:0.989:0.011, and a lithium composite transition metal oxide was prepared by heat treatment at 720°C for 20 hours under an oxygen atmosphere.

[0130] Comparative Example 3.

[0131] A precursor was prepared using the same process as in Example 1 above. LiOH, the prepared precursor, and Al(OH)3 were mixed such that the molar ratio of Li:(Ni+Co+Mn):Al was 1:0.964:0.036, and a lithium composite transition metal oxide was prepared by heat treatment at 720°C for 20 hours under an oxygen atmosphere.

[0133] Comparative Example 4.

[0134] 4 liters of distilled water were added to a co-precipitation reactor (capacity 20 L), and 100 mL of an aqueous ammonia solution with a concentration of 28 wt% was added while maintaining the temperature at 50°C. Then, a transition metal solution mixed with NiSO4, CoSO4, and MnSO4 such that the molar ratio of Ni:Co:Mn was 91.0:6.0:3.0, an aqueous ammonia solution, and a sodium hydroxide solution were added to the co-precipitation reactor, and a co-precipitation reaction was carried out to form a precursor. The precursor particles were separated, washed, and dried in an oven at 130°C to produce the precursor.

[0135] LiOH as a lithium raw material, the above-prepared precursor, and Al(OH)3 were mixed such that the molar ratio of Li:(Ni+Co+Mn):Al was 1:0.969:0.031, and a lithium composite transition metal oxide was prepared by heat treating at 720°C for 20 hours under an oxygen atmosphere.

[0137] [Experimental Example]

[0138] Experimental Example 1. Confirmation of Doping Content

[0139] For each of the lithium composite transition metal oxides prepared in Examples 1 and 2 and Comparative Examples 1 to 4 above, the Al content was measured using an inductively coupled plasma emission spectrometer (ICP-OES; Optima 7300DV, PerkinElmer), and the Al content relative to the total weight and total moles of the lithium composite transition metal oxide was calculated and listed in Table 1 below.

[0140] Input composition ratio (mol%) doping yield Al content in oxides Al / Ni mol% ratio Ni Co Mn Al (ppm) (mol%) Example 1 94.9 0.5 2.4 2.2 93% 5,580 2.02 0.021 Example 2 93.9 0.5 2.4 3.2 93% 8,300 2.97 0.032 Comparative Example 1 97.0 0.5 2.5 0.0 - 0 0 0 Comparative Example 2 95.9 0.5 2.5 1.1 93% 2,790 1.01 0.011 Comparative Example 3 93.5 0.5 2.4 3.6 93% 9,300 3.36 0.036 Comparative Example 4 87.9 6.0 3.0 3.1 93% 7,868 2.8 0.032

[0142] Through Table 1 above, it can be seen that doping was performed with a yield of 93% in Examples 1 and 2 and Comparative Examples 2 to 4, and as a result, the lithium composite transition metal oxides prepared in Examples 1 and 2 were confirmed to have a final Al / Ni molar ratio within the range of 0.015 to 0.034. Meanwhile, Comparative Examples 2 and 3 had Al / Ni molar ratios of 0.011 and 0.036, respectively, which fell outside the scope of the present invention, and in the case of Comparative Example 4, which had a Ni content of less than 90 mol%, the Al / Ni molar ratio was measured to be the same as in Example 2.

[0144] Experimental Example 2. XRD Analysis

[0145] For each of the lithium composite transition metal oxides prepared in Examples 1 and 2 and Comparative Examples 1 and 2 above, the results of measuring the c / a ratio using X-ray diffraction analysis (XRD) by Cu Kα X-rays according to the method described above were as follows.

[0146] Example 1 Example 2 Comparative Example 1 Comparative Example 2 c / a 4.9405 4.9422 4.9362 4.9381

[0148] According to Table 2, the lithium composite transition metal oxides of Examples 1 and 2 have a c / a ratio in the range of 4.9400 to 4.9500, which means that lithium composite transition metal oxides with a higher degree of layered structure completeness were prepared compared to Comparative Examples 1 and 2, which did not.

[0150] Experimental Example 3. Measurement of particle strength

[0151] After taking 3g each of the lithium composite transition metal oxides prepared in Examples 1 and 2 and Comparative Examples 1 and 2 above, the particle strength was measured by applying increasing pressure using a Micro Compression Testing Machine (Shimadzu, MCT-W500) and measuring the pressure at which the particle was destroyed, and the results are listed in Table 3 below.

[0152] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Particle strength (MPa) 145 151 138 140

[0154] Through the results of Table 3 above, it can be confirmed that the lithium composite transition metal oxide prepared in Examples 1 and 2 has much better particle strength compared to the lithium composite transition metal oxide prepared in Comparative Examples 1 and 2.

[0155] This effect is realized because the bonding energy between Al and O is greater than that between Ni and O; such high grain strength is advantageous in that it mitigates grain breakage during the rolling process.

[0157] Experimental Example 4. D 50 measurement

[0158] After dispersing 0.1 g of the lithium composite transition metal oxide powder prepared in Examples 1 and 2 and Comparative Examples 1 to 4 in a dispersion medium, the powder was introduced into a laser diffraction particle size measuring device (Malvern, Mastersizer 3000) and irradiated with ultrasound of approximately 28 kHz at an output of 60 W to measure the D of each cathode material powder 50 ...was measured. The measurement results are shown in Table 4 below.

[0159] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 D 50 (㎛) 11.5 11.6 11.6 11.6 11.6 11.4

[0161] Experimental Example 5. DSC Evaluation

[0162] To evaluate the thermal stability of the lithium composite transition metal oxides prepared in Examples 1 and 2 and Comparative Examples 1 and 2 above, the heat flow was measured using a differential scanning calorimeter (HP-DSC of Setaram), and the results are shown in Fig. 1 and Table 3 below.

[0163] First, a positive electrode slurry was prepared by mixing the respective lithium composite transition metal oxides prepared in Examples 1 and 2 and Comparative Examples 1 and 2 as positive electrode active materials, carbon black (Denka, Li-435) as a conductive material, PVDF (Kureha, KF9709) as a binder, and acrylate (Zeon, BM-730H) as a dispersant in an NMP solvent in a weight ratio of 95.0 : 2.0 : 2.8 : 0.2. The prepared positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and then rolled to produce a positive electrode. An electrode assembly was prepared by interposing a porous polyethylene separator between the prepared positive electrode and a lithium metal anode, and then placed inside a battery case. An electrolyte was then injected into the case to produce a half cell. The above electrolyte was prepared by dissolving 1M concentration of LiPF6 in a mixed organic solvent of ethylene carbonate / dimethyl carbonate / diethyl carbonate in a volume ratio of 3:4:3.

[0164] A manufactured half-cell was charged at 25°C with a constant current of 0.2C until it reached 4.25V, thereby preparing a cell with a 100% SOC. The fully charged cell was disassembled to recover the anode, and the recovered anode was washed with DMC for 30 seconds to remove the electrolyte remaining on the surface, followed by drying. The dried anode was stamped to fit the size of the pan of a differential scanning calorimeter, and then placed into the pan along with 20 µl of the same electrolyte injected into the half-cell, after which the pan was sealed. Subsequently, the heat flow was measured while increasing the temperature from 25°C to 300°C at a rate of 10°C per minute, and the results are shown in Figure 1.

[0165] Meanwhile, the temperature at which the main peak with the maximum heat flow is measured and the maximum heat flow value are listed in Table 5 below.

[0166] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Main peak temperature (°C) 219.4 225.4 215.5 219.1 Maximum heat flow (W / g) 83.1 55.8 83.1 80.7

[0168] Through Table 5 and Figure 1 above, it can be confirmed that when the lithium composite transition metal oxide of Examples 1 and 2, in which the Al / Ni molar ratio is within the range of 0.015 to 0.034 as the positive electrode active material, the main peak with the maximum heat flow is high and the maximum value of the heat flow is low, so the risk of explosion is relatively low even when the internal temperature of the battery rises.

[0169] In particular, Example 2 was found to have the best thermal safety, with a maximum heat flow rate of 60 W / g or less and a main peak temperature of 220°C or higher.

[0171] Experimental Example 6. Evaluation of Dose and Life

[0172] (1) Manufacturing of half cells

[0173] A cathode containing each lithium composite transition metal oxide prepared in the example and comparative example as a cathode active material and a half cell containing the same were prepared in the same manner as Experimental Example 5 above.

[0175] (2) Initial capacity and efficiency measurement

[0176] After performing a formation process on each half cell manufactured in (1) above, the initial charge / discharge capacity and initial efficiency were measured by using a PNE-0506 charge / discharger (manufacturer: PNE Solution Co., Ltd.) to charge the cell to 4.25V at 0.2C (reference capacity 1C = 200mAh / g) at 25℃ under CC-CV conditions and to discharge it to 2.5V at 0.2C, and the results are listed in Table 6 below.

[0178] (3) High temperature life evaluation

[0179] After performing a formation process on each half cell manufactured in (1) above, the cells were charged under CC-CV conditions at 0.33C (reference capacity 1C = 200mAh / g) at 45℃ using a PNE-0506 charge / discharger (manufacturer: PNE Solution Co., Ltd.) to 4.25V, and then CC discharged at 0.33C to 2.5V. This charge / discharge was defined as one cycle, and after one cycle, the initial discharge capacity and initial resistance were measured. Then, the same charge / discharge was repeated up to 30 cycles to measure the capacity and resistance values. Based on this, the capacity retention rate relative to the initial discharge capacity and the resistance increase rate relative to the initial resistance were calculated, and the results are shown in Figure 2 and Table 6.

[0180] Room temperature initial charge capacity (mAh / g) Room temperature initial discharge capacity (mAh / g) Initial charge / discharge efficiency at room temperature (%) High temperature capacity retention rate (%) High-temperature resistance increase rate (%) Example 1 248.2 219.3 88.4 93.3 91.5 Example 2 244.8 216.4 88.4 94.8 81.5 Comparative Example 1 254.4 228.1 89.7 91.4 130.2 Comparative Example 2 250.9 224.2 89.4 92.5 119.3 Comparative Example 3 240.2 211.1 87.9 93.4 94.1 Comparative Example 4 236.5 210.6 89.1 94.5 97.5

[0182] Through Table 6 above, it can be confirmed that the cells of Examples 1 and 2, which use a lithium composite transition metal oxide with an Al / Ni molar ratio in the range of 0.015 to 0.034 as the positive electrode active material, both have an initial charge / discharge efficiency of 88% or higher, a high-temperature capacity retention rate of 93% or higher, and a high-temperature resistance increase rate of 92% or lower.

[0183] On the other hand, it can be seen that the cells of Comparative Examples 1 and 2, which used lithium composite transition metal oxides that did not contain Al or had an Al / Ni molar ratio of 0.011 as the positive electrode active material, showed a significant decrease in high-temperature capacity retention rate and high-temperature resistance increase rate. In particular, it can be seen that the high-temperature resistance increase rate was very high, exceeding 110%.

[0184] In addition, it can be confirmed that the cell of Comparative Example 3, which used a lithium composite transition metal oxide with an Al / Ni molar ratio of 0.036 as the cathode active material, showed low initial capacity and efficiency and a high rate of increase in high-temperature resistance.

[0185] In addition, the cathode active material used in Comparative Example 4 differs from the cathode active material used in Example 2 in that the Al / Ni molar ratio is the same, but the nickel content is less than 90 mol%. As a result, it can be confirmed that the initial charge / discharge capacity itself is low and the resistance increase rate at high temperatures has increased significantly.

Claims

Claim 1 A positive electrode active material comprising a lithium composite transition metal oxide containing nickel, cobalt, manganese, and aluminum, wherein the content of nickel among the metals excluding lithium in the lithium composite transition metal oxide is 90 mol% or more, and the molar ratio of aluminum to nickel, Al / Ni, is 0.015 or more and 0.034 or less. Claim 2 A positive active material according to claim 1, wherein the Al / Ni ratio is 0.021 or higher and 0.032 or lower. Claim 3 A positive electrode active material according to claim 1, wherein the nickel content among the metals excluding lithium in the lithium composite transition metal oxide is 93 mol% to 95 mol%. Claim 4 A positive electrode active material according to claim 1, wherein the content of cobalt among the metals excluding lithium in the lithium composite transition metal oxide is 0.1 mol% to 1.0 mol%. Claim 5 A positive electrode active material according to claim 1, wherein the aluminum content among the metals excluding lithium in the lithium composite transition metal oxide is 1.0 mol% to 5.0 mol%. Claim 6 A positive electrode active material according to claim 1, wherein the lithium composite transition metal oxide has the composition of the following chemical formula 1: [Chemical Formula 1]Li 1+x (Ni a Co b Mn c Al d M1 e )O2 In the above chemical formula 1, M1 is one or more selected from the group consisting of Ti, Zr, W, Mo, Nb, Cu, Fe, V, Cr, Zn, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Mg, and B, and x, a, b, c, d, and e are each -0.2≤x≤0.2, 0.90≤a<1, 0 <b≤0.01, 0<c≤0.05, 0<d≤0.05, 0≤e≤0.05, a+b+c+d+e=1을 만족한다. Claim 7 The positive active material of claim 1, wherein the positive active material comprises primary particles and secondary particles formed by aggregating the primary particles, and the ratio of the length in the c-axis direction to the length in the a-axis direction of the primary particles, c / a, is 4.9400 to 4.9500. Claim 8 A positive active material according to claim 1, wherein the particle strength of the positive active material is 142 MPa to 160 MPa. Claim 9 A positive electrode active material according to claim 1, wherein when the heat flow of the positive electrode active material is measured by differential scanning calorimetry (DSC), the peak at which the heat flow is maximum appears at 219°C to 230°C. Claim 10 A positive active material according to claim 1, wherein the maximum heat flow of the positive active material measured in the range of 25°C to 300°C via differential scanning calorimetry (DSC) is 85.0 W / g or less. Claim 11 A positive electrode comprising: a positive current collector; and a positive active material layer provided on at least one surface of the positive current collector, wherein the positive active material layer comprises a positive active material according to claim 1. Claim 12 A lithium secondary battery comprising: a positive electrode according to claim 11; a negative electrode comprising a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

Citation Information

Patent Citations

  • Ultrahigh nickel positive electrode material and preparation method and application thereof

    CN114597372A

  • High-nickel positive electrode active material, producing method thereof, positive electrode and lithium secondary battery comprising the same

    KR1020200070648A

  • Method for producing positive electrode active material for secondary battery

    KR1020200090661A

  • Positive electrode active material and method for manufacturing the same, secondary battery, battery module, battery pack and device

    KR1020230031939A