Anion exchange membrane material, manufacturing method thereof, and anion exchange membrane containing the same
By using a polymer solution with distinct solvents and a quaternary ammonium precursor, the method enhances ion conductivity and mechanical stability of anion exchange membranes, addressing the challenges of high IEC and process efficiency.
Patent Information
- Application Number
- KR1020240039722
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Existing anion exchange membranes (AEMs) face challenges in achieving high ion exchange capacity (IEC) while maintaining mechanical stability and process efficiency, often leading to moisture-induced swelling and reduced mechanical properties.
A method involving the preparation of a polymer solution using distinct solvents and a quaternary ammonium precursor to enhance ion conductivity, involving specific chemical formulas and solvent ratios to improve IEC and processability.
The solution results in anion exchange membranes with enhanced ion conductivity, improved mechanical stability, and efficient manufacturing, exhibiting excellent IEC values and reduced moisture absorption.
Smart Images

Figure 112024032409930-PAT00011_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an anion exchange membrane material, and more specifically, to an anion exchange membrane material that can shorten the manufacturing process time, has excellent processability and manufacturing efficiency, and can simultaneously exhibit excellent IEC values, a method for manufacturing the same, and an anion exchange membrane containing the same. Background Technology
[0002] Recently, as research on alkaline anion exchange membrane fuel cells (AEMFCs) has been actively conducted, they are recognized as capable of compensating for and improving upon the shortcomings of conventional proton exchange membrane fuel cells (PEMFCs). For example, while PEMFCs are expensive due to the use of precious metal catalysts, AEMFCs do not use precious metal catalysts and can be manufactured at a low cost by utilizing relatively inexpensive metal catalysts through fast reduction kinetics at the cathode, low corrosion, and high pH process conditions.
[0003] Despite these various advantages, AEMFCs still have performance limitations compared to PECFCs when used as fuel cells, so there is a need to improve the performance of AEMFCs in terms of ion conductivity, chemical stability, mechanical strength, anti-swelling properties, durability, and lifespan stability.
[0004] Among the components constituting the above AEMFC, the anion exchange membrane (AEM) plays an important role in selectively allowing anions to pass through. Unlike the Polymer Electrolyte Membrane (PEM) of PEMFC, which has been actively developed since the beginning, active research and development on anion exchange membranes has only recently begun.
[0005] Many polymers, including poly(ether sulfone), poly(ether ketone), polyimide, poly(phenylene oxide), and hybrid composites containing inorganic materials, have been developed as anion exchange membrane materials to date; however, in water, H + Compared to the mobility of OH - High OH due to the low electrochemical mobility of ions - Currently, it is difficult to develop improvements in the performance of anion exchange membranes (AEMs) due to the inability to achieve ion conductivity. In AEMs, OH - The most direct way to maximize ionic conductivity is to increase the ion exchange capacity (IEC). Ion exchange capacity (IEC) refers to the OH- per gram of a polymer. - Defined as the milliequivalent (meq) of an ion-conducting functional group, increasing the ion exchange capacity (IEC) of the ion exchange membrane itself OH - This means that the ion conductivity increases. However, ion exchange membranes with high ion exchange capacity (IEC) inevitably involve excessive moisture absorption that causes membrane expansion, and the expansion caused by moisture absorption degrades the mechanical properties of the ion exchange membrane and can cause problems such as decomposition of the ion exchange membrane, especially at high temperatures.
[0006] The mechanical properties of such membranes can generally be improved by crosslinking the raw polymer with another polymer having higher mechanical properties; however, this conversely lowers the ion exchange performance, leading to a decrease in the ion conductivity of the polymer membrane. Accordingly, there is a need to develop ion exchange membranes that can satisfy mechanical properties while minimizing the reduction in ion conductivity.
[0007] Therefore, there is a need to develop anion exchange membranes that exhibit higher ion exchange capacity and improved mechanical stability. Prior art literature
[0008] Republic of Korea Published Patent No. 10-2016-0143103 (Published Dec. 14, 2016) The problem to be solved
[0009] The present invention was devised to solve the aforementioned problems, and aims to provide an anion exchange membrane material that can shorten the manufacturing process time, has excellent processability and manufacturing efficiency, and simultaneously exhibits excellent IEC values, a method for manufacturing the same, and an anion exchange membrane containing the same. means of solving the problem
[0010] To solve the above-mentioned problem, the present invention provides a method for manufacturing an anion exchange membrane material comprising the steps of: preparing a polymer comprising a compound represented by the following chemical formula 1; preparing a solution by dissolving the polymer in a solvent comprising a first solvent and a second solvent that are different from each other; and preparing a polymer comprising a compound represented by the following chemical formula 2 by adding a quaternary ammonium precursor to the solution.
[0011] [Chemical Formula 1]
[0012]
[0013] [Chemical Formula 2]
[0014]
[0015] In the above chemical formula 1, R 1 to R 4 is a C1-C10 alkyl group, a C6-C20 aryl group, or a C3-C20 heteroaryl group, and R 1 to R 4 At least one of them has a substituent substituted with a halogen element, and
[0016] In the above chemical formula 2, R 5 to R 8 is a C1-C10 alkyl group, a C6-C20 aryl group, or a C3-C20 heteroaryl group, and R 5 to R8 At least one of them is -N + (R 9 Having a substituent substituted with )3, and the above R 9 is hydrogen or a C1 to C3 alkyl group, and
[0017] The above x and y are each independently rational numbers from 1 to 100.
[0018] According to one embodiment of the present invention, the first solvent may include a ring structure within its chemical structure, and the second solvent may not include a ring structure within its chemical structure.
[0019] In addition, the number of methyl groups in the chemical structure of the first solvent and the second solvent may differ from each other.
[0020] In addition, the first solvent may include NMP (N-Methyl-2-pyrrolidone), and the second solvent may include one or more of DMF (Dimethylformamide) and DMSO (Dimethyl Sulfoxide).
[0021] In addition, the above quaternary ammonium precursor may include TMA (Trimethylamine).
[0022] In addition, the step of preparing the above solution can be performed by dissolving a polymer containing a compound represented by Chemical Formula 1 in an amount of 10 to 40 parts by weight per 100 parts by weight of the solvent.
[0023] In addition, the quaternary ammonium precursor may be added in an amount of 3 to 60 parts by weight per 100 parts by weight of a polymer comprising a compound represented by the chemical formula 1.
[0024] In addition, the solvent may contain the first solvent and the second solvent in a weight ratio of 1:0.8 to 1.4.
[0025] In addition, the second solvent may contain the DMF and DMSO in a weight ratio of 1:0.1 to 1:0.5.
[0027] In addition, the present invention provides an anion exchange membrane material comprising a polymer containing a compound represented by the following chemical formula 2, and having an IEC (Ion Exchange Conductivity) of 1.40 to 2.50 as measured by the following measurement method 1.
[0028] [Chemical Formula 2]
[0029]
[0030] In the above chemical formula 2, R 5 to R 8 is a C1-C10 alkyl group, a C6-C20 aryl group, or a C3-C20 heteroaryl group, and R 5 to R 8 At least one of them is -N + (R 9 Having a substituent substituted with )3, and the above R 9 is hydrogen or a C1 to C3 alkyl group, and
[0031] The above x and y are each independently rational numbers from 1 to 100.
[0032] [Measurement Method 1]
[0033] IEC was measured for the manufactured anion exchange membrane using an automatic titration device (848 titrino plus, Metrohm) via an acid-base back titration method.
[0035] In addition, the present invention provides an anion exchange membrane comprising the anion exchange membrane material described above. Effects of the invention
[0036] The anion exchange membrane material of the present invention, the method for manufacturing the same, and the anion exchange membrane including the same have excellent ion conductivity, IEC (Ion Exchange Conductivity), and water content characteristics, so they may have excellent heat resistance and chemical resistance, and excellent electrical characteristics. Brief explanation of the drawing
[0037] Figure 1 is a graph of the hydroxide ion conductivity of anion exchange membrane materials according to Example 1, Example 2 and Comparative Example 1 of the present invention at different temperatures. Specific details for implementing the invention
[0038] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0040] The anion exchange membrane material according to the present invention is manufactured through a manufacturing method comprising the steps of: preparing a polymer comprising a compound represented by the following chemical formula 1; preparing a solution by dissolving the polymer in a solvent comprising a first solvent and a second solvent that are different from each other; and preparing a polymer comprising a compound represented by the following chemical formula 2 by adding a quaternary ammonium precursor to the solution.
[0041] [Chemical Formula 1]
[0042]
[0043] [Chemical Formula 2]
[0044]
[0045] In the above chemical formula 1, R 1 to R 4 is a C1 to C10 alkyl group, a C6 to C20 aryl group, or a C3 to C20 heteroaryl group, preferably R 1 to R 4 may be a C1 to C5 alkyl group, and more preferably R 1 to R 4 may be a methyl group, and the above R 1 to R 4 At least one of them has a substituent substituted with a halogen element, and preferably, the R 1 to R 4At least one of them may have a substituent substituted with a Br or Cl element, and more preferably, the R 1 to R 4 At least one of them may have a substituent substituted with Br, and
[0046] In the above chemical formula 2, R 5 to R 8 is a C1 to C10 alkyl group, a C6 to C20 aryl group, or a C3 to C20 heteroaryl group, and preferably, R 5 to R 8 ≡ may be a C1 to C5 alkyl group, and more preferably, R 5 to R 8 can be a methyl group, and the above R 5 to R 8 At least one of them is -N + (R 9 Having a substituent substituted with )3, and the above R 9 is hydrogen or a C1 to C3 alkyl group, and preferably, R 9 may be a C1 to C2 alkyl group, and more preferably, R 9 can be a methyl group, and
[0047] The above x and y are each independently rational numbers from 1 to 100.
[0048] As the compound represented by Chemical Formula 1 and the compound represented by Chemical Formula 2 satisfy the above conditions, it may be more advantageous for achieving the objectives of the present invention.
[0049] First, the step of preparing a polymer comprising a compound represented by the above chemical formula 1 is described.
[0050] A polymer comprising a compound represented by the above chemical formula 1 may be prepared through a known method, and as an example, a polymer comprising a compound represented by the above chemical formula 1 may be prepared by a method including dissolving poly(2,6-dimethyl-1,4-phenylene oxide) in chlorobenzene, adding NBS (N-bromosuccinimide) and AIBN (2,2'-azobisisobutyronitrile), and refluxing at a temperature of 120 to 160 °C for 2.5 to 3.5 hours, but is not limited thereto.
[0052] Next, the steps for preparing the above solution are described.
[0053] The step of preparing the above solution is performed by dissolving the polymer in a solvent containing a first solvent and a second solvent that are different from each other, as described above.
[0054] The first solvent may include a ring structure within its chemical structure, and the second solvent may not include a ring structure within its chemical structure. Accordingly, it may be more advantageous to simultaneously achieve the effects of shortening the manufacturing process time, excellent processability and manufacturing efficiency, and excellent IEC values.
[0055] In addition, the number of methyl groups in the chemical structures of the first solvent and the second solvent may differ from each other. Accordingly, the time of the manufacturing process can be shortened, processability and manufacturing efficiency can be excellent, and it may be more advantageous to simultaneously exhibit all the effects of having an excellent IEC value. Preferably, the first solvent may contain one methyl group, and the second solvent may contain two methyl groups.
[0056] In addition, the first solvent may have a molecular weight of 90 to 120 g / mol, and preferably 93 to 110 g / mol. In addition, the second solvent may have a molecular weight of 61 to 88 g / mol, and preferably 65 to 85 g / mol. As the molecular weights of the first solvent and the second solvent satisfy the above ranges, the time of the manufacturing process can be shortened, processability and manufacturing efficiency can be excellent, and it can be more advantageous to simultaneously exhibit all the effects of having an excellent IEC value.
[0057] In addition, the first solvent may have 5 to 7 carbon atoms in its molecule, and preferably 5 to 6 carbon atoms in its molecule. In addition, the second solvent may have 2 to 4 carbon atoms in its molecule, and preferably 2 to 3 carbon atoms in its molecule. As the number of carbon atoms in the molecules of each of the first and second solvents satisfies the above ranges, the time of the manufacturing process can be shortened, processability and manufacturing efficiency can be excellent, and it can be more advantageous to simultaneously exhibit all the effects of having an excellent IEC value.
[0058] In addition, the first solvent may include NMP (N-Methyl-2-pyrrolidone), preferably the first solvent may be NMP, and the second solvent may include one or more of DMF (Dimethylformamide) and DMSO (Dimethyl Sulfoxide), preferably the second solvent may be one or more of DMF (Dimethylformamide) and DMSO (Dimethyl Sulfoxide). Accordingly, it is more advantageous to simultaneously achieve the effects of shortening the manufacturing process time, excellent processability and manufacturing efficiency, and excellent IEC values.
[0059] Meanwhile, the solvent may contain the first solvent and the second solvent in a weight ratio of 1:0.8 to 1.4, and preferably, the first solvent and the second solvent may contain the first solvent and the second solvent in a weight ratio of 1:0.9 to 1.3. If the weight ratio of the first solvent and the second solvent is less than 1:0.8, the manufacturing process time may be long, processability and manufacturing efficiency may be poor, or the IEC value of the manufactured anion exchange membrane may be low. If the weight ratio of the first solvent and the second solvent exceeds 1:1.4, the solubility for the polymer may be low, causing precipitation during the reaction and making it impossible to proceed with the reaction.
[0060] In addition, when the second solvent comprises the DMF (Dimethylformamide) and DMSO, the second solvent may comprise the DMF (Dimethylformamide) and DMSO in a weight ratio of 1:0.1 to 1:0.5, preferably in a weight ratio of 1:0.1 to 1:0.4. When the second solvent comprises the DMF (Dimethylformamide) and DMSO, it may be more advantageous for achieving the objective of the present invention as the DMF (Dimethylformamide) and DMSO satisfy the above weight ratio range.
[0061] Meanwhile, the step of preparing the above solution can be performed by dissolving a polymer containing the compound represented by Chemical Formula 1 in an amount of 10 to 40 parts by weight, preferably 13 to 37 parts by weight, with respect to 100 parts by weight of the solvent. If the amount of the polymer containing the compound represented by Chemical Formula 1 is less than 10 parts by weight with respect to 100 parts by weight of the solvent, there may be a problem where the solid content is low, resulting in reduced productivity or difficulty in meeting process conditions when manufacturing the film, and if the amount exceeds 40 parts by weight, there may be a problem where the solubility of the polymer is low, causing precipitation, or the viscosity becomes very high, making it difficult to perform the film formation process.
[0063] Next, the step of preparing a polymer comprising a compound represented by the above chemical formula 2 is described.
[0064] The step of preparing a polymer comprising a compound represented by the above chemical formula 2 can be performed by adding a quaternary ammonium precursor to the solution.
[0065] The above quaternary ammonium precursor may be used without limitation as long as it is a known quaternary ammonium precursor, but preferably, including TMA (Trimethylamine) may be more advantageous for achieving the purpose of the present invention.
[0066] In addition, the quaternary ammonium precursor may be added in an amount of 3 to 60 parts by weight, preferably 5 to 57 parts by weight, per 100 parts by weight of the polymer containing the compound represented by Formula 1. If the quaternary ammonium precursor added to the solution is less than 3 parts by weight per 100 parts by weight of the polymer containing the compound represented by Formula 1, the quaternary ammonium functional group may not be sufficiently introduced, which may result in a problem of reduced electrical performance of the ion exchange membrane. If it is added in an amount exceeding 60 parts by weight, the solubility during the reaction decreases, making it difficult to proceed with the reaction. Furthermore, the use of a large amount of quaternary ammonium precursor increases process costs and generates a large amount of waste liquid, which may have an adverse effect on the environment.
[0068] Meanwhile, the present invention provides an anion exchange membrane material comprising a polymer comprising a compound represented by the above chemical formula 2.
[0069] The above anion exchange membrane material may have an IEC (Ion Exchange Conductivity) of 1.40 to 2.50 as measured by the following measurement method 1, and preferably, the IEC may be 1.60 to 2.30.
[0071] In addition, the present invention provides an anion exchange membrane comprising the anion exchange membrane material described above.
[0072] As the specific description of the above anion exchange membrane may be the same as that known, the present invention does not specifically limit it.
[0074] The anion exchange membrane material of the present invention, the method for manufacturing the same, and the anion exchange membrane including the same have excellent ion conductivity, IEC (Ion Exchange Conductivity), and water content characteristics, so heat resistance and chemical resistance can be improved, and electrical characteristics can be excellent.
[0076] The present invention will be explained more specifically through the following examples, but the following examples are not intended to limit the scope of the invention and should be interpreted as being for the purpose of aiding understanding of the invention.
[0077] [Preparation Example]
[0078] <Preparation Example 1>
[0079] First, a polymer containing a compound represented by the following chemical formula 1 was prepared.
[0080] [Chemical Formula 1]
[0081]
[0082] At this time, in the above Chemical Formula 1, R 1 to R 3 are each methyl groups, and R 4 is a methyl group having a substituent substituted with Br, where x is 31 and y is 69.
[0083] Then, NMP (N-Methyl-2-pyrrolidone), which contains a ring structure in its chemical structure, contains one methyl group, has a molecular weight of 99.13 g / mol, and has five carbon atoms in its molecule, was prepared as a first solvent; DMF (Dimethylformamide), which does not contain a ring structure in its chemical structure, contains two methyl groups, has a molecular weight of 73.09 g / mol, and has three carbon atoms in its molecule, and DMSO (Dimethyl Sulfoxide), which does not contain a ring structure in its chemical structure, contains two methyl groups, has a molecular weight of 78.14 g / mol, and has two carbon atoms in its molecule, were prepared by mixing them (weight ratio of DMF to DMSO 1:0.3); and the first solvent and the second solvent were mixed in a weight ratio of 1:1.3 to prepare a solvent. A solution was prepared by dissolving 19.4 parts by weight of a polymer containing a compound represented by Chemical Formula 1 in 100 parts by weight of the prepared solvent.
[0084] After that, 19 parts by weight of TMA (Trimethylamine) as a quaternary ammonium precursor was added to 100 parts by weight of a polymer containing a compound represented by Chemical Formula 1 to the solution prepared above, and then stirred at room temperature for 20 hours to prepare an anion exchange membrane material containing a polymer containing a compound represented by Chemical Formula 2 below.
[0085] [Chemical Formula 2]
[0086]
[0087] At this time, in the above chemical formula 2, R 5 to R 7 are each methyl groups, and R 8 -N + (R 9 It is a methyl group having a substituent substituted with )3, and the above R 9 Each is a methyl group, and x is 31 and y is 69.
[0088] <Preparation Example 2>
[0089] An anion exchange membrane material was prepared in the same manner as Preparation Example 1, except that NMP (N-Methyl-2-pyrrolidone), which contains a ring structure in its chemical structure, contains one methyl group, has a molecular weight of 99.13 g / mol, and has five carbon atoms in its molecule, was prepared as the first solvent, and DMF (Dimethylformamide), which does not contain a ring structure in its chemical structure, contains two methyl groups, has a molecular weight of 73.09 g / mol, and has three carbon atoms in its molecule, was prepared as the second solvent, and the solvent was prepared by mixing the first solvent and the second solvent in a weight ratio of 1:1.
[0090] <Preparation Example 3>
[0091] An anion exchange membrane material was prepared by carrying out the same procedure as in Preparation Example 1, except that NMP (N-Methyl-2-pyrrolidone), which contains a ring structure in its chemical structure, contains one methyl group, has a molecular weight of 99.13 g / mol, and has five carbon atoms in its molecule, was prepared as the first solvent, and DMF (Dimethylformamide), which does not contain a ring structure in its chemical structure, contains two methyl groups, has a molecular weight of 73.09 g / mol, and has three carbon atoms in its molecule, and IPA (Isopropyl alcohol), which does not contain a ring structure in its chemical structure, contains two methyl groups, has a molecular weight of 60.10 g / mol, and has three carbon atoms in its molecule, were mixed as the second solvent (weight ratio of DMF to IPA 1:0.3), and the solvent was prepared by mixing the first solvent and the second solvent in a weight ratio of 1:1.3. However, precipitation occurred during the reaction, so the process could not proceed further.
[0092] <Comparative Manufacturing Example 1>
[0093] An anion exchange membrane material was prepared in the same manner as in Preparation Example 1, except that NMP (N-Methyl-2-pyrrolidone), which has a ring structure in its chemical structure, contains one methyl group, has a molecular weight of 99.13 g / mol, and has five carbon atoms in its molecule, was used as the solvent.
[0094] [Example]
[0095] <Example 1>
[0096] The anion exchange membrane material of Preparation Example 1 was coated onto a release film using a bar coater, and then dried in an oven at 80 to 100°C for 2 hours to produce a film of 20 to 40 μm.
[0098] <Example 2 and Comparative Example 1>
[0099] A film was prepared by carrying out the same procedure as in Example 1 using the anion exchange membrane material of Preparation Example 2 and Comparative Preparation Example 1.
[0100] The physical properties of the above Example 1, Example 2 and Comparative Example 1 were evaluated and are shown in Table 1 below.
[0101] 1. Particle count evaluation
[0102] For the film prepared using the anion exchange membrane material according to Example 1, Example 2 and Comparative Example 1, 20 x 20 cm 2 The number of particles and foreign substances appearing on the surface area was evaluated visually and is shown in Table 1 below. The better the dispersibility and uniformity of the solution, the fewer or no particles and foreign substances may be present in the manufactured film.
[0103] 2. IEC (Ion Exchange Conductivity) measurement
[0104] For the anion exchange membrane materials according to Example 1, Example 2 and Comparative Example 1, the IEC was measured according to the following measurement method 1 and is shown in Table 1 below. IEC (Ion Exchange capacity) is an indicator representing the amount of conductive groups relative to the mass of the polymer, and a higher IEC means that the amount of conductive groups contained in the same amount of polymer electrolyte membrane is greater.
[0105] [Measurement Method 1]
[0106] IEC was measured for the manufactured anion exchange membrane using an automatic titration device (848 titrino plus, Metrohm) via an acid-base back titration method.
[0107] division Example 1 Example 2 Comparative Example 1 First solvent NMP ○ ○ ○ Second solvent DMF ○ ○ - DMSO ○ - - evaluation Number of particles 0 2 10 IEC(meq / g) 2.03 1.96 1.78
[0108] As shown in Table 1 above, it can be seen that the number of particles in Examples 1 and 2 according to the present invention is significantly improved compared to Comparative Example 1, which uses the first solvent alone, and the IEC is improved by 10.1% to 14.0%.
[0110] 3. Measurement of Ionic Conductivity
[0111] For the anion exchange membrane materials according to Example 1, Example 2 and Comparative Example 1, the ion conductivity was measured according to the following measurement method 2 and is shown in Table 2 and Figure 1 below.
[0112] [Measurement Method 2]
[0113] After immersing the film in a 1M KOH solution for 24 hours, it was washed with triple distilled water, and the ion conductivity was measured using a sheet resistance measuring cell (self-made) and an impedance measuring device (Bio-Logic).
[0114] division Example 1 Example 2 Comparative Example 1 Hydroxide ion conductivity (mS / cm) 20 ℃ 43.51 39.89 37.41 40 ℃ 61.08 50.10 47.21 60 ℃ 94.25 65.47 62.54 80 ℃ 105.46 76.33 73.97
[0115] As shown in Table 2 and Figure 1 above, it can be seen that the hydroxide ion conductivity of Example 1 and Example 2 according to the present invention was higher than that of Comparative Example 1, which uses the first solvent alone, and was improved by 4.7% to 50.7% based on 60°C.
[0117] Although an embodiment of the present invention has been described above, the concept of the present invention is not limited to the embodiments presented in this specification. Those skilled in the art who understand the concept of the present invention may easily propose other embodiments within the scope of the same concept by adding, changing, deleting, or adding components, and such embodiments shall also be considered to fall within the scope of the concept of the present invention.
Claims
Claim 1 A method for manufacturing an anion exchange membrane material comprising the steps of: preparing a polymer comprising a compound represented by the following chemical formula 1; preparing a solution by dissolving the polymer in a solvent comprising different first solvents and second solvents in a weight ratio of 1:0.8 to 1.4; and adding a quaternary ammonium precursor to the solution to prepare a polymer comprising a compound represented by the following chemical formula 2; wherein the first solvent comprises NMP (N-Methyl-2-pyrrolidone) and the second solvent comprises DMF (Dimethylformamide) and DMSO (Dimethyl sulfoxide) in a weight ratio of 1:0.1 to 1:0.5: [Chemical Formula 1] [Chemical Formula 2] In the above chemical formula 1, R 1 to R 4 is a C1-C10 alkyl group, a C6-C20 aryl group, or a C3-C20 heteroaryl group, and R 1 to R 4 At least one of them has a substituent substituted with a halogen element, and in the above chemical formula 2, R 5 to R 8 is a C1-C10 alkyl group, a C6-C20 aryl group, or a C3-C20 heteroaryl group, and R 5 to R 8 At least one of them is -N + (R 9 Having a substituent substituted with )3, and the above R 9 is hydrogen or a C1 to C3 alkyl group, and x and y are each independently rational numbers from 1 to 100. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 In claim 1, the method for manufacturing an anion exchange membrane material comprising the quaternary ammonium precursor TMA (Trimethylamine). Claim 6 A method for manufacturing an anion exchange membrane material according to claim 1, wherein the step of preparing the solution is performed by dissolving a polymer comprising a compound represented by Chemical Formula 1 in an amount of 10 to 40 parts by weight per 100 parts by weight of the solvent. Claim 7 A method for manufacturing an anion exchange membrane material according to claim 1, wherein the quaternary ammonium precursor is added in an amount of 3 to 60 parts by weight per 100 parts by weight of a polymer comprising a compound represented by the chemical formula 1. Claim 8 delete Claim 9 delete Claim 10 delete Claim 11 An anion exchange membrane comprising: an anion exchange membrane material manufactured by the method of any one of claims 1 and 5 to 7.
Citation Information
Patent Citations
Ion Exchange Composite Membrane and Manufacturing Method Thereof
KR101934855B1
Anion-exchange membrane, preparation method thereof and alkaline anion-exchange membrane fuel cell comprising the same
KR1020200126562A
Preparation method of alkaline anion exchange composite membrane having high inorganic matter doping amount
CN107353422A
Anion exchange polymer, ion exchange membrane and preparation method and application thereof
CN117720721A
Anion-exchange membranes for fuel cells and preparation method thereof
KR1020190023249A