Cathode active material for lithium secondary battery, methode of manufacturing the same and lithium secondary battery including the same
A two-step coating process enhances the chemical stability and ion conductivity of high-nickel lithium metal oxide particles, improving the performance of lithium secondary batteries by preventing degradation and maintaining capacity and stability.
Patent Information
- Application Number
- KR1020210177982
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-12-13
AI Technical Summary
High-nickel lithium metal oxide particles in lithium secondary batteries suffer from inferior chemical stability and deteriorating lifespan characteristics during repeated charge-discharge cycles.
A method of manufacturing a positive electrode active material involving a two-step coating process where lithium metal oxide particles are first coated with a first metal and then a second metal, forming a coating layer with a concentration gradient, enhancing chemical stability and ion conductivity.
The coated lithium metal oxide particles improve the capacity, output characteristics, and high-temperature stability of lithium secondary batteries, preventing degradation of lifespan characteristics.
Smart Images

Figure 112021144321619-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery comprising the same. More specifically, the invention relates to a positive electrode active material comprising lithium metal oxide particles having a coating layer formed on a surface, a method for manufacturing the same, and a lithium secondary battery comprising the same. Background Technology
[0002] Rechargeable batteries are batteries capable of repeated charging and discharging, and are widely used as power sources for portable electronic devices such as mobile phones and laptop PCs.
[0003] Examples of secondary batteries include lithium-ion batteries, nickel-cadmium batteries, and nickel-hydrogen batteries; among these, lithium-ion batteries are being actively developed and applied due to their high operating voltage and energy density per unit weight, as well as advantages in charging speed and weight reduction.
[0004] The positive electrode of a lithium secondary battery may include lithium metal oxide particles capable of reversible insertion and extraction of lithium ions as a positive electrode active material.
[0005] For example, the lithium metal oxide particles may include metals such as nickel, cobalt, manganese, and aluminum.
[0006] Meanwhile, as the application range of lithium secondary batteries expands to large devices such as hybrid vehicles, research and development on high-nickel lithium metal oxide particles with increased nickel content are active to secure high capacity.
[0007] However, high-nickel lithium metal oxide particles have inferior chemical stability and suffer from a problem where lifespan characteristics deteriorate during repeated charge-discharge cycles.
[0008] For example, Korean Published Patent Application No. 10-2016-0126840 discloses lithium metal oxide particles having a coating layer formed on a surface to solve the aforementioned problem. Prior art literature
[0009] Korean Patent Publication No. 10-2016-0126840 The problem to be solved
[0010] One objective of the present invention is to provide a positive electrode active material having improved capacity and chemical stability and a method for manufacturing the same.
[0011] One objective of the present invention is to provide a lithium secondary battery having improved capacity, lifespan characteristics, and high-temperature stability. means of solving the problem
[0012] A method for manufacturing a positive electrode active material for a lithium secondary battery according to exemplary embodiments may include the steps of: preparing lithium metal oxide particles; introducing a first coating source containing the lithium metal oxide particles and a first metal into a coating solvent to first coat the lithium metal oxide particles; and introducing a second coating source containing a second metal into the coating solvent while the first coated lithium metal oxide particles are dispersed in the coating solvent to second coat the first coated lithium metal oxide particles.
[0013] In one embodiment, during the first coating step, the first coating source may be added to the coating solvent in a constant amount for a predetermined period of time.
[0014] In one embodiment, during the second coating step, the second coating source may be added to the coating solvent in a constant amount for a predetermined period of time.
[0015] In the above second coating step, the second coating source can be added to the coating solvent in a constant amount for a predetermined period of time.
[0016] In one embodiment, the lithium metal oxide particles may contain 80 mol% or more of nickel relative to the total elements excluding lithium and oxygen.
[0017] In one embodiment, the coating solvent may be deionized water.
[0018] In one embodiment, the first metal and the second metal may independently be any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu.
[0019] In one embodiment, the second metal may be Al.
[0020] In one embodiment, after the step of secondary coating, a step of coating a metalloid may be further included.
[0021] A positive electrode active material for a lithium secondary battery according to exemplary embodiments comprises lithium metal oxide particles; and a coating layer formed on the surface of the lithium metal oxide particles and containing a first metal and a second metal, wherein the coating layer may include a concentration change region having a tendency for the concentration of the first metal to decrease and a tendency for the concentration of the second metal to increase with respect to the radial direction of the lithium metal oxide particles.
[0022] In one embodiment, the coating layer may have a sea shape.
[0023] In one embodiment, the coating layer comprises: a first coating layer formed on the surface of the lithium metal oxide particles; a second coating layer formed on the first coating layer; and an intermediate layer formed between the first coating layer and the second coating layer, wherein in the intermediate layer, the first metal may have a concentration change trend that decreases in the radial direction of the lithium metal oxide particles, and the second metal may have a concentration change trend that increases along the radial direction of the lithium metal oxide particles.
[0024] In one embodiment, the first metal in the first coating layer may have a concentration change trend that increases in the radial direction of the lithium metal oxide particles, and the second metal in the second coating layer may have a concentration change trend that decreases in the radial direction of the lithium metal oxide particles.
[0025] In one embodiment, the second coating layer comprises a lower coating layer formed on the intermediate layer; and an upper coating layer formed on the lower coating layer, wherein the upper coating layer may contain a second metal and may not contain a first metal.
[0026] In one embodiment, the lithium metal oxide particles may contain 80 mol% or more of nickel relative to the total elements excluding lithium and oxygen.
[0027] In one embodiment, the first metal and the second metal may independently be any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu.
[0028] In one embodiment, a semi-metallic coating layer formed on the coating layer may be further included.
[0029] A lithium secondary battery according to exemplary embodiments may include a positive electrode comprising a positive electrode active material for the lithium secondary battery; and a negative electrode facing the positive electrode. Effects of the invention
[0030] According to the method for manufacturing a positive electrode active material for a lithium secondary battery according to exemplary embodiments, a coating layer can be formed on the surface of lithium metal oxide particles, the coating layer comprising a region in which the first metal and the second metal have a predetermined concentration change tendency, and the first metal and the second metal have a region in which the first metal and the second metal have a predetermined concentration change tendency.
[0031] A positive electrode active material for a lithium secondary battery according to exemplary embodiments may have improved chemical stability, ion conductivity, and low resistance by including the coating layer. In addition, the positive electrode active material may prevent degradation of lifespan characteristics even when including high-nickel (Ni 80 mol% or more) lithium metal oxide particles by including the coating layer.
[0032] A lithium secondary battery according to exemplary embodiments may have improved capacity, output characteristics, lifespan characteristics, and high-temperature stability by including the aforementioned positive electrode active material. Brief explanation of the drawing
[0033] FIG. 1 is a schematic flowchart of a method for manufacturing a positive electrode active material according to an exemplary embodiment. FIG. 2 is a cross-sectional view schematically showing a positive active material particle according to an exemplary embodiment. FIG. 3 is a schematic cross-sectional view of a lithium secondary battery according to an exemplary embodiment. FIG. 4 is a schematic plan view of a lithium secondary battery according to an exemplary embodiment. FIG. 5 is a TEM-EDS line-scanning analysis image measured along a line from the surface of the lithium metal oxide particle to the coating layer in a cross-section of the positive electrode active material particle according to the embodiment. Specific details for implementing the invention
[0034] In this specification, the first metal and the second metal mean different metals.
[0035] Exemplary embodiments of the present invention provide a positive electrode active material for a lithium secondary battery comprising lithium metal oxide particles and a coating layer formed on the surface of the lithium metal oxide particles, a method for manufacturing the same, and a lithium secondary battery comprising the same.
[0036] FIG. 1 is a flowchart schematically illustrating a method for manufacturing a positive electrode active material according to an exemplary embodiment.
[0037] Referring to FIG. 1, lithium metal oxide particles can be prepared (e.g., S10).
[0038] For example, in step S10, metal hydroxide particles are manufactured, said metal hydroxide particles are mixed with a lithium source and calcined to prepare said lithium metal oxide particles.
[0039] For example, in step S10, a reaction solution (e.g., an aqueous solution) comprising a metal salt, a chelating agent, and a co-precipitating agent can be prepared. The metal hydroxide particles can be produced by carrying out a co-precipitation reaction in the reaction solution.
[0040] For example, the metal salt may include metal sulfates, metal nitrates, metal acetates, metal hydroxides, metal carbonates, hydrates thereof, etc.
[0041] For example, the metal salt may include Ni, Co, Mn, Al, Zr, Ti, Cr, B, Mg, Mn, Ba, Si, Y, W, Sr, etc.
[0042] For example, various metal salts can be prepared to satisfy the composition, molar ratio, etc. of the metal described in Chemical Formula 1 below.
[0043] In one embodiment, the metal salt may include Ni.
[0044] In some embodiments, the metal salt may further comprise at least one of Co and Mn. In some embodiments, the metal salt may comprise Ni, Co, and Mn.
[0045] For example, the above co-precipitating agent may include sodium hydroxide, sodium carbonate, etc. For example, the above chelating agent may include water ammonia (e.g., NH3H2O), ammonium carbonate, etc.
[0046] For example, the temperature of the above co-precipitation reaction can be appropriately controlled as known in the art without special limitations.
[0047] For example, the above lithium source may include lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxide, etc.
[0048] In one embodiment, the lithium metal oxide particles may contain Ni.
[0049] In some embodiments, the lithium metal oxide particles may further contain Co, Mn, etc. In some embodiments, the lithium metal oxide particles may contain Ni, Co, and Mn.
[0050] In one embodiment, the lithium metal oxide particles may contain 80 mol% or more of Ni relative to the total elements excluding lithium and oxygen.
[0051] In some embodiments, the lithium metal oxide particles may contain 85 mol% or more, 88 mol% or more, 90 mol% or more, 93 mol% or more, or 95 mol% or more of Ni with respect to the total elements excluding lithium and oxygen. For example, if the lithium metal oxide particles contain nickel at a high concentration, the capacity of the lithium secondary battery may be improved, but the lifespan characteristics and high-temperature stability may be degraded. However, the positive electrode active material according to exemplary embodiments of the present invention may include a coating layer described below to prevent the degradation of lifespan characteristics.
[0052] In one embodiment, the lithium metal oxide particles may be represented by the following chemical formula 1.
[0053] [Chemical Formula 1]
[0054] Li x Ni a Co b M c O y
[0055] In Chemical Formula 1, M is at least one of Al, Zr, Ti, B, Mg, Mn, Ba, Si, Y, W, and Sr, and 0.9≤x≤1.2, 1.9≤y≤2.1, 0.8≤a≤1, 0≤(b+c) / a≤0.25, 0 <a+b+c≤1, 0≤b≤0.2, 0≤c≤0.2일 수 있다.
[0056] In some embodiments, 0.85≤a<1, 0.88≤a<1, 0.9≤a<1, 0.93≤a<1, or 0.95≤a<1.
[0057] In some embodiments, step S10 may include the step of doping the lithium metal oxide particles with a doping element. For example, the doping element may be at least one of Al, Ti, Zr, B, Ba, Si, Mg, P, Sr, W, and La.
[0058] Referring to FIG. 1, a coating source containing the lithium metal oxide particles and the first metal can be introduced into a coating solvent and mixed to perform a first wet coating (e.g., S20).
[0059] In one embodiment, the coating solvent may be deionized water.
[0060] In step S20, a first coating layer containing the first metal may be formed on the surface of the lithium metal oxide particles.
[0061] For example, the first coating layer may have a sea shape. For example, the sea shape can be distinguished from the island shape, which is a discontinuous phase, as a continuous phase.
[0062] In one embodiment, the first coating layer may cover an area of 70% or more, 80% or more, or 90% or more of the surface of the lithium metal oxide particles.
[0063] In one embodiment, the first coating layer can substantially cover the entire surface of the lithium metal oxide particle (for example, in EDS analysis, a peak of the first metal is observed over the entire surface area).
[0064] In one embodiment, at step S20, the first coating source may be added to the coating solvent in a constant amount for a predetermined period of time. For example, the addition time and amount may be adjusted according to the desired thickness of the coating layer. Accordingly, a uniform coating layer without defects can be formed.
[0065] Referring to FIG. 1, a second coating source containing a second metal can be added to the coating solvent to perform a second wet coating (e.g., S30).
[0066] Steps S20 and S30 can be performed as an in-situ process. The in-situ process means proceeding with a series of reactions (e.g., first coating and second coating) sequentially without separately extracting an intermediate product (e.g., lithium metal oxide particles with a first coating layer formed). For example, the in-situ process can be performed within the same reactor.
[0067] For example, a second coating source containing a second metal can be introduced into the coating solvent while the lithium metal oxide particles having the first coating layer formed thereon are dispersed in the coating solvent (i.e., without separately filtering or drying the lithium metal oxide particles having the first coating layer formed thereon).
[0068] In one embodiment, at step S30, the second coating source may be added to the coating solvent in a constant amount for a predetermined period of time. For example, the addition time and amount may be adjusted according to the desired thickness of the coating layer. Accordingly, a uniform coating layer without defects can be formed.
[0069] In one embodiment, the timing of the introduction of the first coating source and the timing of the introduction of the second coating source may be separated from each other and may partially overlap.
[0070] By step S30, a second coating layer containing the second metal can be formed on the first coating layer.
[0071] Additionally, by step S30, an intermediate layer may be formed between the first coating layer and the second coating layer, wherein the first metal and the second metal have a predetermined concentration change trend. For example, in the intermediate layer, the first metal may have a concentration change trend that decreases in the radial direction of the lithium metal oxide particles (i.e., from the center of the particles toward the surface), and the second metal may have a concentration change trend that increases in the radial direction of the lithium metal oxide particles.
[0072] For example, the second coating layer and the intermediate layer may have a sea shape.
[0073] The positive electrode active material according to exemplary embodiments includes a first coating layer, a second coating layer, and an intermediate layer (hereinafter abbreviated as coating layer), and may have improved ion conductivity and low resistance, and may suppress adverse reactions with the electrolyte. In addition, even if High-Ni (Ni 80 mol% or more) lithium metal oxide particles are included, the degradation of lifespan characteristics may be prevented by the coating layer described above. Accordingly, a lithium secondary battery containing the positive electrode active material may have improved capacity, output characteristics, lifespan characteristics, and high-temperature stability.
[0074] Meanwhile, when metals are coated (dry or wet) by simultaneously introducing various types of coating sources, the coating layer cannot be formed, and a coating layer in which various types of metals are uniformly dispersed is formed.
[0075] In addition, even if the first coating and the second coating are performed as separate processes, the coating layer (e.g., intermediate layer) cannot be formed.
[0076] In addition, when dry coating is performed, an island-shaped coating layer is formed, making it difficult to effectively passivate lithium metal oxide particles. Furthermore, if wet coating is performed multiple times as a separate process, lithium in the lithium metal oxide particles may be lost, or the crystal structure of the lithium metal oxide particles may be excessively altered, which may result in inferior lifespan characteristics and high-temperature stability of the lithium secondary battery.
[0077] In one embodiment, the first metal and the second metal may independently be any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu.
[0078] In some embodiments, the first metal may be Zr or Ti, and the second metal may be Al.
[0079] In one embodiment, the first coating source may be a coating source solution in which the first metal is dissolved in a solvent in the form of a salt. Likewise, the second coating source may be a coating source solution in which the second metal is dissolved in a solvent in the form of a salt. For example, the solvent may be deionized water.
[0080] In one embodiment, after step S30, the step of coating the lithium metal oxide particles on which the coating layer is formed may further include a step of coating them with a coating source containing a metalloid. For example, the metalloid coating step may be performed by a dry coating method, a wet coating method, etc.
[0081] In some embodiments, the metalloid coating step may be a wet coating, and the metalloid coating step may also be performed by the in-situ process described above.
[0082] In some embodiments, the metalloid may include boron (B).
[0083] Cathode active material for lithium secondary batteries
[0084] Referring to FIG. 2, a positive electrode active material for a lithium secondary battery according to exemplary embodiments may include lithium metal oxide particles (200); and a coating layer (210, 215, 220) formed on the surface of the lithium metal oxide particles (200) and containing a first metal and a second metal.
[0085] The coating layer may include a concentration change region (e.g., the dotted line region of FIG. 5) in which the concentration of the first metal tends to decrease and the concentration of the second metal tends to increase, based on the radial direction of the lithium metal oxide particles (200) (i.e., from the center of the particle to the surface).
[0086] In one embodiment, the coating layer may include a first coating layer (210) formed on the surface of a lithium metal oxide particle (200); a second coating layer (220) formed on the first coating layer (210); and an intermediate layer (215) formed between the first coating layer (210) and the second coating layer (220).
[0087] In one embodiment, the intermediate layer (215) may include the concentration change region. For example, in the intermediate layer (215), the first metal may have a concentration change trend that decreases in the radial direction of the lithium metal oxide particles (200), and the second metal may have a concentration change trend that increases in the radial direction.
[0088] Whether "concentration tends to decrease (or increase)" or "concentration changes tend to decrease (or increase)" in a specified area is determined by evaluating the area as a whole. Furthermore, even if some areas within the said specified area have values opposite to the overall trend, the overall trend may be maintained as long as the influence is not significant enough to alter the overall trend.
[0089] The positive electrode active material according to the exemplary embodiments may include the coating layer (210, 215, and 220) to have improved ion conductivity and low resistance, and side reactions with the electrolyte may be suppressed. In addition, even if High-Ni (Ni 80 mol% or more) lithium metal oxide particles are included, degradation of life characteristics may be prevented by the coating layer described above. Accordingly, a lithium secondary battery including the positive electrode active material may have improved capacity, output characteristics, life characteristics, and high-temperature stability.
[0090] In one embodiment, the first coating layer (210) contains the first metal and the second metal, and the first metal in the first coating layer (210) may have a tendency for concentration change to increase in the radial direction of the lithium metal oxide particles (200).
[0091] In one embodiment, the second coating layer (220) may contain the first metal and the second metal, and the second metal in the second coating layer (220) may have a tendency of decreasing concentration in the radial direction of the lithium metal oxide particles (200).
[0092] In some embodiments, the second coating layer (220) is formed on the intermediate layer (215) and may include the first metal and a lower coating layer (not shown) containing the first metal and an upper coating layer (not shown) formed on the lower coating layer containing the second metal and not the first metal. For example, by setting the second metal to a metal with excellent passivation performance, the stability of the anode active material can be further improved.
[0093] In one embodiment, the coating layer (210, 215, 220) may have a sea shape rather than an island shape.
[0094] In one embodiment, the first coating layer (210) may cover more than 70%, more than 80%, more than 90% of the surface area of the lithium metal oxide particle (200), or substantially the entire surface. The intermediate layer (215) may cover more than 70%, more than 80%, more than 90% of the surface area of the first coating layer (210), or substantially the entire surface. The second coating layer (220) may cover more than 70%, more than 80%, more than 90% of the surface area of the intermediate layer (2150), or substantially the entire surface. Within the above range, the positive active material may have improved chemical stability.
[0095] For example, the lithium metal oxide particles (200) may have a monolithic form. Alternatively, they may have a secondary particle form in which multiple primary particles are aggregated.
[0096] In one embodiment, the lithium metal oxide particles (200) may contain Ni.
[0097] In some embodiments, the lithium metal oxide particles (200) may further contain Co, Mn, etc. In some embodiments, the lithium metal oxide particles (200) may contain Ni, Co, and Mn.
[0098] In one embodiment, the lithium metal oxide particles (200) may contain 80 mol% or more of Ni with respect to all elements excluding lithium and oxygen.
[0099] In some embodiments, the lithium metal oxide particles (200) may contain at least 85 mol%, at least 88 mol%, at least 90 mol%, at least 93 mol%, or at least 95 mol% of Ni with respect to all elements excluding lithium and oxygen.
[0100] In one embodiment, the lithium metal oxide particles (200) can be represented by the following chemical formula 1.
[0101] [Chemical Formula 1]
[0102] Li x Ni a Co b M c O y
[0103] In Chemical Formula 1, M is at least one of Al, Zr, Ti, B, Mg, Mn, Ba, Si, Y, W, and Sr, and 0.9≤x≤1.2, 1.9≤y≤2.1, 0.8≤a≤1, 0≤(b+c) / a≤0.25, 0 <a+b+c≤1, 0≤b≤0.2, 0≤c≤0.2일 수 있다.
[0104] In some embodiments, 0.85≤a<1, 0.88≤a<1, 0.9≤a<1, 0.93≤a<1, or 0.95≤a<1.
[0105] In some embodiments, the lithium metal oxide particles (200) may contain a doping element. For example, the doping metal may be at least one of Al, Ti, Zr, B, Ba, Si, Mg, P, Sr, W, and La.
[0106] In one embodiment, the first metal and the second metal may independently be any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu.
[0107] In some embodiments, the first metal may be Zr or Ti, and the second metal may be Al.
[0108] According to some embodiments, the positive active material is formed on the second coating layer (220) and may further include a coating layer (not shown) containing a metalloid. For example, the metalloid may include boron.
[0109] lithium secondary battery
[0110] FIGS. 3 and FIGS. 4 are a schematic plan view and a cross-sectional view, respectively, showing a lithium secondary battery according to exemplary embodiments. FIG. 4 is a cross-sectional view cut along line II' of FIG. 3.
[0111] Referring to FIGS. 3 and 4, a lithium secondary battery may include a positive electrode (100) and a negative electrode (130) facing the positive electrode (100).
[0112] The positive electrode (100) may include a positive electrode current collector (105) and a positive electrode active material layer (110) on the positive electrode current collector (105).
[0113] The positive active material layer (110) may include a positive active material for a lithium secondary battery according to exemplary embodiments, and, if necessary, a positive binder, a conductive material, etc.
[0114] For example, the anode (100) can be manufactured by mixing and stirring an anode active material, an anode binder, a conductive material, a solvent, etc. to produce an anode slurry, and then applying, drying, and rolling the anode slurry onto an anode current collector (105).
[0115] For example, the positive current collector (105) may include stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof.
[0116] For example, the anode binder may include organic binders such as polyvinylidenefluoride (PVDF), vinylidenefluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyacrylonitrile, and polymethylmethacrylate; and water-based binders such as styrene-butadiene rubber (SBR). Additionally, for example, the anode binder may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0117] For example, the conductive material may include carbon-based conductive materials such as graphite, carbon black, graphene, and carbon nanotubes; and metal-based conductive materials such as perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0118] The cathode (130) may include a cathode current collector (125) and a cathode active material layer (120) on the cathode current collector (125).
[0119] For example, the negative electrode active material layer (120) may include a negative electrode active material, a negative electrode binder and a conductive material as needed.
[0120] For example, the cathode (130) can be manufactured by dispersing a cathode active material, a cathode binder, and a cathode conductive material in a solvent to prepare a cathode slurry, and then applying, drying, and rolling the cathode slurry onto a cathode current collector (125).
[0121] For example, the negative current collector (125) may include gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof.
[0122] For example, the above-mentioned negative electrode active material may be a material capable of absorbing and extracting lithium ions. For example, the above-mentioned negative electrode active material may include a lithium alloy, a carbon-based active material, a silicon-based active material, etc., and these may be used alone or in combination of two or more.
[0123] For example, the lithium alloy may include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, indium, etc.
[0124] For example, the carbon-based active material may include crystalline carbon, amorphous carbon, carbon composites, carbon fibers, etc.
[0125] For example, the above amorphous carbon may include hard carbon, coke, mesocarbon micro beads, mesophase pitch-based carbon fibers, etc.
[0126] For example, the crystalline carbon may include natural graphite, artificial graphite, graphitized coke, graphitized MCMB, graphitized MPCF, etc.
[0127] In one embodiment, the negative electrode active material may include a silicon-based active material. For example, the silicon-based active material may be Si, SiO x (0 <x<2), Si / C, SiO / C, Si-Metal 등을 포함할 수 있다. 이 경우, 고용량을 갖는 리튬 이차 전지를 구현할 수 있다.
[0128] The above-described cathode binder and cathode conductive material may be materials substantially identical or similar to the anode binder and conductive material described above. For example, the cathode binder may include a water-based binder such as styrene-butadiene rubber (SBR). Additionally, the cathode binder may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0129] For example, a separator (140) may be interposed between the anode (100) and the cathode (130).
[0130] In some embodiments, the area of the negative electrode (130) may be larger than the area of the positive electrode (100). In this case, lithium ions generated from the positive electrode (100) can move smoothly to the negative electrode (130) without precipitating in the middle.
[0131] For example, the separator (140) may include a porous polymer film made of a polyolefin-based polymer, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. Additionally, for example, the separator (140) may include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0132] For example, an electrode cell may be formed including an anode (100), a cathode (130), and a separator (140).
[0133] For example, a plurality of electrode cells may be stacked to form an electrode assembly (150). For example, the electrode assembly (150) may be formed by winding, lamination, zigzag-folding, etc. of a separator (140).
[0134] A lithium secondary battery according to exemplary embodiments may include a positive electrode lead (107) connected to a positive electrode (100) and protruding outside of a case (160); and a negative electrode lead (127) connected to a negative electrode (130) and protruding outside of a case (160).
[0135] For example, the positive electrode (100) and the positive electrode lead (107) may be electrically connected. Likewise, the negative electrode (130) and the negative electrode lead (127) may be electrically connected.
[0136] For example, the positive lead (107) can be electrically connected to the positive current collector (105). Additionally, the negative lead (130) can be electrically connected to the negative current collector (125).
[0137] For example, the positive current collector (105) may include a positive tab (106) protruding from one side. A positive active material layer (110) may not be formed on the positive tab (106). The positive tab (106) may be integral with the positive current collector (105) or connected by welding or the like. The positive current collector (105) and the positive lead (107) may be electrically connected through the positive tab (106).
[0138] For example, the negative current collector (125) may include a negative tab (126) protruding from one side. A negative active material layer (120) may not be formed on the negative tab (126). The negative tab (126) may be integral with the negative current collector (125) or connected by welding or the like. The negative current collector (125) and the negative lead (127) may be electrically connected through the negative tab (126).
[0139] For example, the electrode assembly (150) may include a plurality of positive electrodes and a plurality of negative electrodes. For example, each of the plurality of positive electrodes may include a positive electrode tab. For example, each of the plurality of negative electrodes may include a negative electrode tab.
[0140] For example, the anode tabs (or cathode tabs) may be laminated, pressed, and welded to form an anode tab laminate (or cathode tab laminate). For example, the anode tab laminate may be electrically connected to an anode lead (107). For example, the cathode tab laminate may be electrically connected to a cathode lead (127).
[0141] For example, the electrode assembly (150) and the above-described electrolyte can be housed together in a case (160) to form a lithium secondary battery.
[0142] The above lithium secondary battery can be manufactured in, for example, cylindrical, prismatic, pouch, or coin types.
[0143] An electrode assembly (150) can be housed in a case (160) together with an electrolyte to form a lithium secondary battery.
[0144] For example, the above electrolyte may include a lithium salt, an organic solvent, and, if necessary, additives.
[0145] For example, the above lithium salt is Li + X - It can be expressed as.
[0146] For example, the above X - is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It could be any one of them.
[0147] For example, the above lithium salt may include LiBF4, LiPF6, etc.
[0148] For example, the organic solvent may include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, tetrahydrofuran, etc.
[0149] Preferred embodiments and comparative examples of the present invention are described below. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0150] [Example]
[0151] 1. Preparation of positive electrode active material particles
[0152] Lithium metal oxide particles (NCM 811; LiNi) in a reactor 0.8 Co 0.1 Mn 0.1 ) and deionized water were added.
[0153] Zr(SO4)2 dissolved in deionized water (1,500 ppm Zr relative to the weight of lithium metal oxide particles) was continuously introduced into the above reactor for 10 minutes to perform a first wet coating.
[0154] Al2(SO4)3 dissolved in deionized water (1,000 ppm Al relative to the weight of lithium metal oxide particles) was continuously introduced into the reactor for 10 minutes to perform a second wet coating. After performing the first wet coating, the second wet coating was performed without a separate filtering and drying process.
[0155] After the second wet coating, the particles were filtered and dried at 150°C for 12 hours. After drying, the particles were placed in a kiln in an oxygen (O2) atmosphere and calcined at 400°C for 10 hours.
[0156] After calcination, the particles were cooled to room temperature, ground, and classified to produce the positive active material particles of the example.
[0157] 2. Manufacture of lithium secondary batteries
[0158] A positive electrode slurry was prepared by dispersing the positive electrode active material particles of the example, carbon black, and polyvinylidene fluoride in N-methyl-2-pyrrolidone in a weight ratio of 92:5:3.
[0159] The above anode slurry was uniformly applied to an area excluding the protrusion of an aluminum foil (15 μm thick) having a protrusion (anode tab) on one side, and an anode was manufactured by drying and rolling.
[0160] A cathode active material was prepared by mixing artificial graphite and natural graphite in a weight ratio of 7:3, and styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were dispersed in water in a weight ratio of 97:1:2 to prepare a cathode slurry.
[0161] The above cathode slurry was uniformly applied to an area excluding the protrusion of a copper foil (15 μm thickness) having a protrusion (cathode tab) on one side, and the cathode was manufactured by drying and rolling.
[0162] An electrode assembly was formed by interposing a polyethylene separator (thickness 20 μm) between the anode and the cathode. An anode lead and a cathode lead were welded and connected to the anode tab and the cathode tab, respectively.
[0163] After preparing a 1 M LiPF6 solution (30:70 v / v EC / EMC mixed solvent), an electrolyte was prepared by adding 1 wt% FEC (Fluoroethylene carbonate), 0.3 wt% VC (Vinylethylene carbonate), 1 wt% LiPO2F2 (Lithium difluorophosphate), 0.5 wt% PS (1,3-Propane sultone), and 0.5 wt% PRS (Prop-1-ene-1,3-sultone) based on a total electrolyte of 100 wt%.
[0164] The electrode assembly is housed inside a pouch (case) so that a portion of the positive lead and the negative lead are exposed to the outside, and three sides excluding the surface for injecting the electrolyte are sealed.
[0165] A lithium secondary battery sample was manufactured by injecting the above electrolyte into the pouch and sealing the surface of the electrolyte injection area.
[0166] [Comparative Example 1]
[0167] Lithium metal oxide particles (NCM 811; LiNi 0.8 Co 0.1 Mn 0.1 The items were added to deionized water in a 1:1 weight ratio and washed for 20 minutes.
[0168] After washing, the particles were filtered, dried at 150°C for 12 hours, and placed in a kiln in an oxygen atmosphere and fired at 400°C for 10 hours.
[0169] After calcination, the particles were cooled to room temperature, and then ground and classified to produce the positive active material particles of Comparative Example 1.
[0170] A lithium secondary battery was manufactured in the same manner as the example, except that the positive active material particles of Comparative Example 1 were used.
[0171] [Comparative Example 2]
[0172] Lithium metal oxide particles (NCM 811; LiNi 0.8 Co 0.1 Mn 0.1 The items were added to deionized water in a 1:1 weight ratio and washed for 20 minutes.
[0173] After washing, the particles were filtered and dried at 150°C for 12 hours.
[0174] The cleaned lithium metal oxide particles, ZrO2 (particle size about 100 nm, Zr 1,500 ppm relative to the weight of the lithium metal oxide particles), and Al2O3 (particle size 30 to 70 nm, Al 1,000 ppm relative to the weight of the lithium metal oxide particles) were fed into a dry high-speed mixer and mixed uniformly for 1 minute to prepare a mixture.
[0175] The above mixture was placed in a kiln under an oxygen atmosphere and calcined at 400°C for 10 hours.
[0176] After calcination, the particles were cooled to room temperature, and then ground and classified to produce the positive active material particles of Comparative Example 2.
[0177] A lithium secondary battery was manufactured in the same manner as the example, except that the positive active material particles of Comparative Example 2 were used.
[0178] [Comparative Example 3]
[0179] Lithium metal oxide particles (NCM 811; LiNi) in a reactor 0.8 Co 0.1 Mn 0.1 ) and deionized water were added.
[0180] Zr(SO4)2 dissolved in deionized water (1,500 ppm Zr relative to the weight of lithium metal oxide particles) and Al2(SO4)3 dissolved in deionized water (1,000 ppm Al relative to the weight of lithium metal oxide particles) were simultaneously introduced into the above reactor to perform wet coating.
[0181] After wet coating, the particles were filtered, dried at 150°C for 12 hours, and placed in a kiln in an oxygen (O2) atmosphere and fired at 400°C for 10 hours.
[0182] After calcination, the particles were cooled to room temperature, ground, and classified to produce the positive active material particles of Comparative Example 3.
[0183] A lithium secondary battery was manufactured in the same manner as the example, except that the positive active material particles of Comparative Example 3 were used.
[0184] [Comparative Example 4]
[0185] Lithium metal oxide particles (NCM 811; LiNi) in a reactor 0.8 Co 0.1 Mn 0.1 ) and deionized water were added.
[0186] Zr(SO4)2 dissolved in deionized water (1,500 ppm Zr relative to the weight of lithium metal oxide particles) was continuously introduced into the above reactor for 10 minutes to perform wet coating. After wet coating, the particles were dried at 150°C for 12 hours.
[0187] Wet-coated lithium metal oxide particles and Al2O3 (particle size 30 to 70 nm, Al 1,000 ppm relative to the weight of lithium metal oxide particles) were introduced into a dry high-speed mixer and uniformly mixed for 1 minute to prepare a mixture.
[0188] The above mixture was placed in a kiln under an oxygen atmosphere and calcined at 400°C for 10 hours.
[0189] After calcination, the particles were cooled to room temperature, and then ground and classified to produce the positive active material particles of Comparative Example 4.
[0190] A lithium secondary battery was manufactured in the same manner as the example, except that the positive active material particles of Comparative Example 4 were used.
[0191] Experimental Example 1: TEM-EDS (Morphology and composition analysis of the coating layer)
[0192] The positive electrode active material particles of the example were analyzed using a transmission electron microscope (TEM) and energy-dipersive X-ray spectroscopy (EDS). A Tecnai G2 F30 was used for TEM, and an Oxford Ultim Max TLE was used for EDS.
[0193] For the cross-section of the positive active material particle of the example, TEM-EDS line-scanning analysis (spot size 5 nm) was performed along the radial direction of the particle (from the center to the surface).
[0194] The TEM-EDS line-scanning analysis image is shown in Fig. 5.
[0195] Referring to Fig. 5, it can be seen that within the coating layer, there exists a region with a concentration change trend in which Zr decreases and Al increases, based on the radial direction of the particles (dotted line area in Fig. 5).
[0196] Experimental Example 2: Room Temperature Performance Evaluation
[0197] (1) Initial dose evaluation
[0198] The lithium secondary batteries of the examples and comparative examples were charged at 25°C at a 0.1 C-rate CC / CV rate (4.3V, 0.05C CUT-OFF) and discharged at a 0.1 C-rate CC rate (3.0V CUT-OFF) to measure the single discharge capacity C1.
[0199] (2) Room temperature life (capacity retention rate) evaluation
[0200] The lithium secondary batteries of the examples and comparative examples were charged and discharged 100 times at 25°C, and the 100th discharge capacity C2 was measured.
[0201] The room temperature capacity retention rate was calculated according to the following formula.
[0202] Room temperature capacity retention rate (%) = C2 / C1 × 100
[0203] Experimental Example 3: High-temperature performance evaluation (high-temperature capacity retention rate)
[0204] The lithium secondary batteries of the examples and comparative examples were charged at a high temperature (45°C) using CC / CV charging (0.33C 4.3V 0.05C CUT-OFF) and discharged using CC (0.33C 3.0V CUT-OFF). The above charging and discharging cycles were repeated 100 times, and the discharge capacity C3 of the 100th cycle was measured.
[0205] The high-temperature capacity retention rate was calculated according to the following formula.
[0206] High temperature capacity retention rate (%) = C3 / C1 × 100
[0207] Initial discharge capacity (mAh / g) Efficiency (%) Room temperature capacity retention rate (%) High-temperature capacity retention rate (%) Examples 216.3 94.6 82.1 79.3 Comparative Example 1 213.4 92.1 60.3 51.7 Comparative Example 2 214.2 93.2 69.3 67.4 Comparative Example 3 215.1 93.5 78.1 76.5 Comparative Example 4 214.5 92.9 73.8 70.5
[0208] Referring to Table 1 above, the lithium secondary battery of the example showed improved efficiency, room temperature capacity retention rate, and high temperature capacity retention rate compared to the lithium secondary batteries of the comparative examples. Explanation of the symbols
[0209] 100: Anode 105: Anode current collector 107: Anode Lead 110: Anode Active Material Layer 120: Cathode active material layer 125: Cathode current collector 127: Cathode Lead 130: Cathode 140: Separator 150: Electrode assembly 160: Case 200: Lithium metal oxide particles 210: First coating layer 215: Intermediate layer 220: Second coating layer
Claims
Claim 1 A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising: a step of preparing lithium metal oxide particles; a step of first coating the lithium metal oxide particles by introducing the lithium metal oxide particles and a first coating source containing a first metal into a coating solvent; and a step of second coating the first coated lithium metal oxide particles by continuously introducing a second coating source containing a second metal into the coating solvent without separately filtering or drying, while the first coated lithium metal oxide particles are dispersed in the coating solvent, wherein the first coating step and the second coating step are performed as an in-situ process. Claim 2 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein in the first coating step, a constant amount of the first coating source is added to the coating solvent for a predetermined time, and in the second coating step, a constant amount of the second coating source is added to the coating solvent for a predetermined time. Claim 3 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the lithium metal oxide particles contain 80 mol% or more of nickel with respect to all elements excluding lithium and oxygen. Claim 4 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the coating solvent is deionized water. Claim 5 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the first metal and the second metal are independently any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu. Claim 6 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the second metal is Al. Claim 7 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, further comprising the step of coating a metalloid after the second coating step. Claim 8 A positive electrode active material for a lithium secondary battery comprising: lithium metal oxide particles; and a coating layer formed on the surface of the lithium metal oxide particles and containing a first metal and a second metal, wherein the coating layer includes a concentration change region in which the concentration of the first metal tends to decrease and the concentration of the second metal tends to increase with respect to the radial direction of the lithium metal oxide particles, and wherein the first metal and the second metal are different from each other and are independently any one of Al, Ti, Zr, Mg, Zn, W, Nb, Sr, Ta, and Cu. Claim 9 A positive electrode active material for a lithium secondary battery according to claim 8, wherein the coating layer has a sea shape. Claim 10 A positive electrode active material for a lithium secondary battery according to claim 8, wherein the coating layer comprises: a first coating layer formed on the surface of the lithium metal oxide particles; a second coating layer formed on the first coating layer; and an intermediate layer formed between the first coating layer and the second coating layer, wherein in the intermediate layer, the first metal has a concentration change tendency decreasing in the radial direction of the lithium metal oxide particles, and the second metal has a concentration change tendency increasing in the radial direction of the lithium metal oxide particles. Claim 11 A positive electrode active material for a lithium secondary battery according to claim 10, wherein the first metal in the first coating layer has a concentration change trend that increases in the radial direction of the lithium metal oxide particles, and the second metal in the second coating layer has a concentration change trend that decreases in the radial direction of the lithium metal oxide particles. Claim 12 A positive electrode active material for a lithium secondary battery according to claim 10, wherein the second coating layer comprises a lower coating layer formed on the intermediate layer; and an upper coating layer formed on the lower coating layer, wherein the upper coating layer contains a second metal and does not contain a first metal. Claim 13 A positive electrode active material for a lithium secondary battery according to claim 8, wherein the lithium metal oxide particles contain 80 mol% or more of nickel with respect to all elements excluding lithium and oxygen. Claim 14 delete Claim 15 A positive electrode active material for a lithium secondary battery according to claim 8, further comprising a metalloid coating layer formed on the coating layer. Claim 16 A lithium secondary battery comprising: a positive electrode comprising a positive electrode active material for a lithium secondary battery according to claim 8; and a negative electrode facing the positive electrode.
Citation Information
Patent Citations
Positive electrode active material, preparation method thereof, and positive electrode sheet and lithium battery
CN110620230A
Double-coating-layer modified lithium ion battery positive electrode material and preparation method thereof
CN112349905A
Positive electrode active material, method for producing same, and lithium secondary battery including same
KR101400593B1
Positive electrode active material, manufacturing method thereof, positive electrode, battery, battery pack, electronic device, electric vehicle, power storage device, and power system
KR1020140073423A
Composite cathode active material, Cathode and Lithium battery containing composite cathode active material and Preparation method thereof