Organic peroxide composition
The use of a moisture-retaining organic peroxide composition in solid form addresses the challenges of melt strength and safety in polypropylene processing, ensuring effective performance and safety under non-inert conditions.
Patent Information
- Application Number
- KR1020240023167
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-21
- Filing Date
- 2024-02-19
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-02-19
AI Technical Summary
Existing methods for improving polypropylene melt strength using peroxides face issues such as decomposition products causing fogging or blooming, safety risks, and handling difficulties, especially under non-inert extrusion conditions.
An organic peroxide composition comprising moisture and a moisture-retaining agent, such as anionic clays or metal phosphates, in solid form, which maintains melt strength and safety under non-inert atmospheres.
The composition produces polypropylene products with excellent melt strength and safety, avoiding decomposition and discoloration, while being easier to handle and use in non-inert extrusion processes.
Smart Images

Figure 112024018565881-PAT00019_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an organic peroxide composition in solid form and its use in a process for manufacturing high melt strength polypropylene (HMS-PP). Background Technology
[0002] Methods for improving the melt strength of polypropylene using peroxides are known in the art. Treatment using peroxides generates long-chain branches. The longer the chain branches, the higher the melt strength.
[0003] For example, WO 99 / 027007 discloses a method comprising the step of heat-treating polypropylene with a percarbonate. Several percarbonates, including dicetyl percarbonate, dimyristyl percarbonate, and di(4-tert-butylcyclohexyl) percarbonate, are disclosed in this specification.
[0004] The advantages of these specific dialkyl percarbonates, apart from their good performance in the relevant method, are their safety mode and ease of handling. All of them are in solid form and—in contrast to many other percarbonates—can be safely stored and handled at room temperature. Additionally, they can be used in extrusion processes.
[0005] High melt strength polypropylene (HMS-PP) is used in food packaging and automotive applications. At higher temperatures, decomposition products of dialkyl peroxides, namely alcohols such as cetyl alcohol, myristyl alcohol, and 4-tert-butylcyclohexanol, tend to evaporate from HMS-PP and condense onto other surfaces, forming a hazy surface with reduced visual transparency. This phenomenon is called fogging.
[0006] For example, as a result of heating HMS-PP-based food packages in a microwave oven, alcohol decomposition products may evaporate and condense on the lid or microwave window of the package, which may negatively affect their transparency.
[0007] HMS-PP used inside vehicles can be heated under warm weather conditions, and alcohol decomposition products can condense on vehicle windows, resulting in clearly undesirable consequences such as reduced visibility.
[0008] The decomposition products of dicetyl and dimyristyl peroxide carbonates also tend to migrate to the surface of modified polypropylene. This phenomenon is called "blooming" and results in the formation of white or glittering particles on the surface, causing an uneven appearance of the polymer surface.
[0009] WO 99 / 36466 and WO 2019 / 038244 disclose methods for increasing the melt strength of polypropylene. As mentioned in WO 2019 / 038244, the use of certain peroxides disclosed herein resulted in higher melt strength than the use of, for example, dicetyl percarbonate, dibenzoyl peroxide, and ortho-substituted dibenzoyl peroxide (as used in WO 99 / 36466). This improvement may be directly attributed to the use of these specific peroxides in combination with an inert atmosphere in the extruder.
[0010] Although the method of WO 2019 / 038244 actually produces polypropylene products with excellent melt strength characteristics, using an inert environment in the extruder is not always practical or desirable. For example, in the recycling of polypropylene plastics, it is desirable to avoid an inert environment (to minimize the overall complexity and cost of the process).
[0011] Through empirical research by the inventors, it was found that switching from an inert atmosphere in the extruder to a non-inert atmosphere (i.e., air instead of an inert atmosphere) while using the organic peroxide of WO 2019 / 038244 still produced polypropylene products having melt strength characteristics superior to those of the organic peroxide used in WO 99 / 36466 (under the same method conditions). However, under non-inert extrusion conditions, the polypropylene products produced were discolored (i.e., yellowed instead of white), showed signs of decomposition, and had inferior melt strength characteristics compared to products produced under an inert atmosphere, none of which were desirable results.
[0012] Furthermore, the preferred organic peroxide formulation used in WO 2019 / 038244 contained a significant amount of moisture. While this organic peroxide formulation is generally safe to use (with proper training), it is not without safety issues. Specifically, when fed into an extruder, there is always a possibility that the formulation may unintentionally leak onto the extruder device. If this occurs, the moisture (sensitizer) evaporates rapidly, increasing the concentration of the peroxide to a point where it becomes sensitive to friction and shock. In the event of such an event, the risk of explosion increases significantly, which must be clearly prevented (especially on an industrial scale). These problems make the handling of the organic peroxide formulation somewhat dangerous and difficult. The problem to be solved
[0013] In this regard, there is a need for an organic peroxide composition that produces polypropylene products under non-inert extrusion conditions while maintaining the excellent polypropylene properties of WO 2019 / 038244 and avoiding the aforementioned safety risks and handling problems. means of solving the problem
[0014] Now, it has been found that these objectives are satisfied by an organic peroxide composition comprising moisture and a moisture retaining agent. Accordingly, the present disclosure can be summarized in the following aspects:
[0015] Mode 1. As an organic peroxide composition in solid form:
[0016] a) At least one organic peroxide of the following formula, wherein
[0017]
[0018] Each R in the formula is an organic peroxide individually selected from C1-5 alkyl groups;
[0019] b) at least one moisture retainer that is solid at room temperature; and
[0020] c) An organic peroxide composition containing moisture.
[0021] Mode 2. An organic peroxide composition, wherein each R is individually selected from methyl, ethyl, n-propyl, i-propyl, n-butyl, secondary-butyl, tertiary-butyl, and tertiary-amyl.
[0022] Mode 3. An organic peroxide composition in embodiment 1 or 2, wherein at least one organic peroxide is di(para-methylbenzoyl) peroxide.
[0023] Mode 4. An organic peroxide composition in any one of embodiments 1 to 3, wherein the organic peroxide composition comprises at least one organic peroxide a) in an amount of 40 to 75 weight%, preferably 45 to 70 weight%, more preferably 50 to 65 weight% (weight%) based on the total weight of the organic peroxide composition.
[0024] Mode 5.In any one of embodiments 1 to 4, the organic peroxide composition is an organic peroxide composition that retains 60% or more of the original moisture content of the organic peroxide composition when the organic peroxide composition passes through "Protocol A".
[0025] Mode 6 . An organic peroxide composition in any one of embodiments 1 to 5, wherein at least one moisture retainer comprises one or more anionic clays.
[0026] Mode 7 . An organic peroxide composition in which, in embodiment 6, one or more anionic clays are hydrotalcite.
[0027] Mode 8 . An organic peroxide composition in any one of embodiments 1 to 5, wherein at least one moisture retainer comprises one or more metal phosphates.
[0028] Mode 9 . An organic peroxide composition in which, in embodiment 8, one or more metal phosphates are dical phosphate.
[0029] Mode 10 . An organic peroxide composition in any one of embodiments 1 to 9, wherein the organic peroxide composition comprises at least one moisture retainer b) in an amount of 1 to 30 weight%, preferably 3 to 20 weight%, more preferably 5 to 15 weight% (weight%) based on the total weight of the organic peroxide composition.
[0030] Mode 11 . An organic peroxide composition in any one of embodiments 1 to 10, wherein the organic peroxide composition comprises 5 to 30 weight%, preferably 10 to 25 weight%, more preferably 15 to 20 weight% (weight%) based on the total weight of the organic peroxide composition.
[0031] Mode 12. An organic peroxide composition, wherein in any one of embodiments 1 to 11, one or more stabilizers are additionally included in an amount of preferably 5 to 25 weight% (weight%) based on the total weight of the organic peroxide composition.
[0032] Mode 13 . An organic peroxide composition according to Embodiment 12, wherein one or more stabilizers include or consist of one or more antioxidants.
[0033] Mode 14. An organic peroxide composition in any one of embodiments 1 to 13, wherein the composition is in the form of a compressed solid article, optionally a compressed and shaped solid article.
[0034] Mode 15 . In embodiment 14, the compressed solid article is an organic peroxide composition in which the solid article is a flake or granule.
[0035] Mode 16 A method for improving the melt strength of polypropylene by extruding the polypropylene in an extruder at a temperature of 150°C to 300°C and in the presence of an organic peroxide composition according to any one of embodiments 1 to 13.
[0036] Mode 17 . In embodiment 16, the organic peroxide composition is added to polypropylene before or during extrusion.
[0037] Mode 18 . A method according to embodiment 16 or 17, wherein the amount of organic peroxide composition used is such that the concentration of at least one organic peroxide a) is in the peroxide range of 0.1 to 5.0 g per 100 g of polypropylene, more preferably in the range of 0.5 to 3.0 g per 100 g of polypropylene.
[0038] Mode 19. A method in any one of embodiments 16 to 18, wherein the polypropylene is a homopolymer of propylene or a random, alternating, heteropolymer, or block copolymer or terpolymer of propylene and other olefins.
[0039] Mode 20 . Use of an organic peroxide composition according to any one of embodiments 1 to 15 as an additive for increasing the melt strength of polypropylene and / or for recycling polyolefin plastics. Specific details for implementing the invention
[0040] In a first aspect, the present disclosure relates to an organic peroxide composition in a solid form (preferably in the form of a compressed solid article such as flakes or granules), which:
[0041] a) At least one organic peroxide of the following formula, wherein
[0042]
[0043] In the equation, each R is C 1-5 Organic peroxide individually selected from alkyl groups;
[0044] b) at least one moisture retainer that is solid at room temperature; and
[0045] c) Contains moisture.
[0046] An unexpected finding was that by including moisture and moisture retainers in the organic peroxide composition, it was no longer necessary to use an inert environment in the extruder (i.e., the performance of the peroxide was not affected by the type of atmosphere used). The polypropylene product also showed no apparent signs of polypropylene degradation, and no discoloration of the product was observed (i.e., a white product was obtained). Furthermore, the organic peroxide composition disclosed herein was found to be much safer and easier to handle than the preferred organic peroxide formulation in WO 2019 / 038244. Thus, all the aforementioned technical problems were resolved by the organic peroxide composition disclosed herein. Accordingly, the organic peroxide composition disclosed herein is an excellent candidate for use in the recycling of polypropylene plastics.
[0047] The organic peroxide compositions disclosed herein are in solid form. Many suitable solid forms for organic peroxide compositions exist, for example, powders (e.g., formulations of powder components typically mixed in a conical screw mixer or plugshear mixer), granules, flakes, etc., but are not necessarily limited thereto. As compressed solid articles (e.g., flakes and granules) have been found to be chemically more stable and easier to administer than uncompressed powders, preferably, the organic peroxide composition is compressed (and optionally shaped) into solid articles such as flakes or granules, making it much safer and easier to add to an extruder. An additional unexpected finding was that the MFI was lower when compressed (and optionally shaped) solid articles (e.g., flakes or granules) were used instead of uncompressed powder formulations of the components. Those skilled in the art know how to manufacture compressed (and optionally shaped) solid articles and know of suitable and readily available devices for manufacturing compressed (and optionally shaped) solid articles (e.g., Amandus Kahl pellet mill, Bepex gear pelletizer, etc.).
[0048] The organic peroxide composition comprises, as a first essential component a), at least one organic peroxide selected from organic peroxides of the following chemical formula:
[0049]
[0050] In the formula, each R is located at the para-position of the aromatic ring, and R is C 1-5 It is individually selected from alkyl groups.
[0051] In a preferred embodiment, each R is C 1-5 They are individually selected from alkyl groups. Examples of these groups are methyl, ethyl, n-propyl, i-propyl, n-butyl, secondary-butyl, tertiary-butyl, and tertiary-amyl.
[0052] More preferably, at least one R is methyl.
[0053] Most preferably, the organic peroxide is di(para-methylbenzoyl) peroxide (i.e., each R is methyl).
[0054] Preferably, the organic peroxide composition comprises at least one organic peroxide as described herein in an amount of 40 to 75 weight%, preferably 45 to 70 weight%, more preferably 50 to 65 weight% (weight% based on the total weight of the organic peroxide composition).
[0055] The organic peroxide composition comprises, as a second essential component b), at least one moisture retainer that is solid at room temperature. The term “moisture retainer” has the conventional meaning (in the context of the present art) of a formulation that retains moisture in the organic peroxide composition (i.e., minimizes moisture loss when the composition is compressed), particularly when subjected to compressive force (e.g., through the absorption or adsorption of free moisture in the composition by the “moisture retainer”). Tests to determine whether a formulation is a “moisture retainer” particularly suitable for use in the organic peroxide composition disclosed herein are specified in the following working example (“Protocol A”). “Solid at room temperature” has the conventional meaning, i.e., solid at 25°C and 1 atmosphere. It has been found that the retained moisture in the solid organic peroxide composition is important for successfully producing polypropylene products by extrusion under a non-inert atmosphere, having the same desirable technical characteristics as the polypropylene products produced by the method of WO 2019 / 038244. Moisture retainers suitable for use in chemical compositions are known and are readily available to those skilled in the art. Examples of suitable moisture retainers according to the present invention include, but are not limited to, the following:
[0056] · Anionic clays, e.g., synthetic and natural layered double hydroxides, including but not limited to natural and synthetic hydrotalcites;
[0057] · Moisture-absorbing polymers, e.g., but not limited to, acrylic moisture-absorbing polymers (e.g., poly(meth)acrylic acid, polyacrylamide, etc.), polyvinyl alcohol-based moisture-absorbing polymers, polyethylene glycol-based moisture-absorbing polymers, polysaccharide-based moisture-absorbing polymers (e.g., natural or modified starch-based moisture-absorbing polymers, natural or modified cellulose [particularly carboxymethyl cellulose], natural or modified cyclodextrin, natural or modified guar gum, etc.), polyamide-based moisture-absorbing polymers (e.g., polyaspartic acid);
[0058] · Metal carbonates and metal bicarbonates, e.g., but not limited to, Ca, Mg, Zn, Na, K, or Li carbonates, or Na, K, or Li bicarbonates;
[0059] · Metal oxides, e.g., but not limited to, CaO, MgO, and ZnO;
[0060] · Metal silicates, e.g., but not limited to, calcium silicate or magnesium silicate;
[0061] · Metal phosphates, e.g., but not limited to, dicalcium phosphate;
[0062] · Hydrophilic silica; and
[0063] · Metal sulfide desiccant, e.g., sodium sulfate, barium sulfate, and magnesium sulfate, but not limited thereto.
[0064] A preferred moisture retainer comprises or consists of at least one anionic clay. The anionic clay has a crystal structure comprising a positively charged layer composed of a combination of divalent and trivalent metal hydroxides in which anions and water molecules are present. Hydrotalcite is an example of a naturally occurring anionic clay in which carbonate is the major anion and its layer contains Mg and Al. Various natural, synthetic, and modified forms having other divalent and / or trivalent metals and / or anions (including nitrate anions, organic anions, and pillaring anions) are known and are suitable for use in the compositions disclosed herein. A preferred anionic clay is anionic clay having carbonate or hydroxide anions within the layers. It has been found that anionic clays, such as naturally occurring and synthetic hydrotalcites, such as aluminum magnesium hydroxide carbonate, are particularly effective in the compositions disclosed herein.
[0065] Preferably, the organic peroxide composition contains at least one moisture retainer in an amount of 1 to 30 weight%, preferably 3 to 20 weight%, more preferably 5 to 15 weight% (weight%) based on the total weight of the organic peroxide composition.
[0066] The organic peroxide composition contains water, which is the third essential component c). Preferably, the organic peroxide composition contains water in an amount of 5 to 30 weight%, preferably 10 to 25 weight%, more preferably 15 to 20 weight% (weight%) based on the total weight of the organic peroxide composition.
[0067] Other additives commonly used in organic peroxide compositions may also be included in the organic peroxide composition disclosed herein. These conventional additives typically account for about 5 to 25 weight percent, preferably 5 to 20 weight percent, of the organic peroxide composition. A preferred additive comprises a stabilizer, for example, one or more antioxidants, for example, a primary antioxidant, for example, of the phenol type, and / or a secondary antioxidant, for example, of the phosphite or sulfite type (e.g., Irganox® 1010 [phenol; pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)] and / or Irgafos 168 [phosphite; tris(2,4-di-tert-butylphenyl)-phosphite], or a 1:1 mixture of two antioxidants named Irganox B225 (both of which are available from BASF®) (but are not limited thereto).
[0068] In a preferred embodiment, an organic peroxide composition in solid form (preferably in the form of a compressed solid article such as flakes or granules) comprises the following:
[0069] a) 40 to 75 weight% of at least one organic peroxide of the following formula
[0070]
[0071] (Each R in the equation is C 1-5 Individually selected from alkyl groups);
[0072] b) at least one moisture retainer that is solid at room temperature and satisfies the requirements of “Protocol A” in an amount of 1 to 30 weight%;
[0073] c) 5 to 30 weight percent of moisture; and
[0074] d) Optionally 5 to 25 weight% of at least one antioxidant.
[0075] In a more preferred embodiment, an organic peroxide composition in solid form (preferably in the form of a compressed solid article such as flakes or granules) comprises the following:
[0076] a) 40 to 75 weight% of at least one organic peroxide of the following formula
[0077]
[0078] (Each R in the equation is C 1-5 Individually selected from alkyl groups);
[0079] b) at least one moisture retainer selected from anionic clay, which is solid at room temperature, in an amount of 1 to 30 weight%;
[0080] c) 5 to 30 weight percent of moisture; and
[0081] d) Optionally 5 to 25 weight% of at least one antioxidant (preferably at least one primary antioxidant and / or at least one secondary antioxidant).
[0082] In a more preferred embodiment, an organic peroxide composition in solid form (preferably in the form of a compressed solid article such as flakes or granules) comprises the following:
[0083] a) 40 to 75 weight% of di(para-methylbenzoyl) peroxide;
[0084] b) 1 to 30 weight% of at least one moisture retainer selected from hydrotalcite that is solid at room temperature;
[0085] c) 5 to 30 weight percent of moisture; and
[0086] d) Optionally 5 to 25 weight% of at least one antioxidant (preferably at least one phenol-type antioxidant and / or at least one phosphite-type antioxidant or sulfite-type antioxidant).
[0087] In a further preferred embodiment, an organic peroxide composition in solid form (preferably in the form of a compressed solid article such as flakes or granules) comprises the following:
[0088] a) 40 to 75 weight% of di(para-methylbenzoyl) peroxide;
[0089] b) at least one moisture retainer selected from Mg / Al hydrotalcite, which is solid at room temperature, in an amount of 1 to 30 weight%;
[0090] c) 5 to 30 weight percent of moisture; and
[0091] d) 5 to 25 weight% of at least one antioxidant (preferably at least one phenol-type antioxidant and / or at least one phosphite or sulfite-type antioxidant).
[0092] In a second embodiment, the present invention relates to a method for improving the melt strength of polypropylene by the step of extruding polypropylene from an extruder at a temperature of 150°C to 300°C and in the presence of an organic peroxide composition in solid form as described above.
[0093] An organic peroxide composition is added to polypropylene before or during extrusion. The amount of organic peroxide composition used will vary depending on the desired degree of modification and the type of polypropylene used. Preferably, the amount of organic peroxide composition used is such that the concentration of at least one organic peroxide a) is in the peroxide range of 0.1 to 5.0 g per 100 g of polypropylene, more preferably in the range of 0.5 to 3.0 g per 100 g of polypropylene.
[0094] Preferably, extrusion is performed in a temperature range of 155 to 250°C, more preferably 160 to 240°C.
[0095] Polypropylene may be a homopolymer of propylene or a random, alternating, heteromorphic, or block copolymer or terpolymer of propylene and other olefins. Generally, the propylene copolymer or terpolymer will contain one or more other olefins such as ethylene, butene, pentene, hexene, heptene, or octene, but may also contain styrene or styrene derivatives. The content of olefins other than propylene is preferably 30 weight percent or less of all monomers.
[0096] Polypropylene homopolymers and copolymers of propylene and ethylene are most preferred. It is also possible to use a mixture of polypropylene and polyethylene, such as a polyolefin recycling stream.
[0097] The melting point of commercially available propylene homopolymers is about 160 to 170°C. The melting points of propylene copolymers and terpolymers are generally lower.
[0098] The molecular weight of the polypropylene used can be selected from a wide range. Molecular weight is an indicator of the melt flow index (MFI). The material to be used can be prepared from polypropylene having an MFI of 0.1 to 1000 g / 10 min (230°C, 21.6 N). Preferably, the material to be used is prepared from polypropylene having an MFI of 0.5 to 250 g / 10 min.
[0099] Polypropylene may be branched polypropylene as described in WO 2016 / 126429 and WO 2016 / 126430.
[0100] Extrusion allows the modification of polypropylene to be combined with pelletization. The material is manufactured using a single-screw extruder or a twin-screw extruder. A twin-screw extruder is preferred because it more thoroughly homogenizes peroxides within the polypropylene. The residence time in the extruder is generally about 10 seconds to about 5 minutes.
[0101] The screw speed of the extruder is preferably in the range of 25 to 1000 rpm. The temperature of the extruder must be higher than the melting point of polypropylene.
[0102] The method may be carried out as a batch process, a continuous process, or a combination thereof. A continuous process is preferred.
[0103] During extrusion, a vacuum or atmospheric degassing device may be applied to remove volatile decomposition products and any moisture introduced as part of the peroxide formulation.
[0104] Extrusion may be performed in the presence of auxiliaries to affect the melt flow index of polypropylene and / or improve the degree of deformation. Examples of auxiliaries are TMAIC (trimetallyl isocyanurate), TAIC (triallyl isocyanurate), TAC (triallycianurate), TRIM (trimethylolpropane trimethacrylate), divinylbenzene, HVA-2 (N,N'-phenylene bismaleimide), AMSD (alpha-methyl styrene dimer), and Perkalink 900 (1,3-bis(citraconimidomethyl)benzene).
[0105] Adjuvants are generally understood to be multifunctional reactive additives, such as polyunsaturated compounds, that react rapidly with polymer radicals, overcome steric hindrance, and minimize undesirable side effects. Before or during the method of the present invention, the incorporation of one or more effective amounts of these adjuvants into polypropylene tends to affect the melt flow index and molecular weight of the resulting polypropylene.
[0106] If desired, conventional auxiliary agents known to those skilled in the art, such as antioxidants, UV stabilizers, lubricants, antidegradables, blowing agents, nucleating agents, fillers, pigments, acid capture agents (e.g., calcium stearate), and / or antistatic agents, may be added to the polypropylene. These auxiliary agents may be added to the polypropylene not only before extrusion but also during or after extrusion. For example, a chemical blowing agent (e.g., azodicarbonamide) may be added, or a physical blowing agent (e.g., a gas such as nitrogen, carbon dioxide, butane, or isobutane) may be injected into the extruder to produce foamed polypropylene. The chemical blowing agent is preferably added before or after extrusion; the physical blowing agent is preferably injected during or after extrusion.
[0107] HMS-PP may be further processed as known to those skilled in the art. It may be formed directly into the desired end product, processed using an underwater pelletizer, purified, modified, molded, or blended with miscible amounts of other (polymer) materials such as EPM, EPDM, and / or LDPE. Accordingly, there may be variations using other polymers or monomers to improve the compatibility of the end product with other materials.
[0108] Alternatively, HMS-PP may be degraded to increase processability and / or applicability, or may be further processed by, for example, foaming, foam molding, injection molding, blow molding, extrusion coating, profile extrusion, cast film extrusion, blow film extrusion, and / or thermoforming.
[0109] It should be noted that various elements of the present invention, including but not limited to desirable ranges for various parameters, may be combined as long as they are not mutually exclusive.
[0110] Executed examples
[0111] The present invention is illustrated by the following embodiments, but is not limited thereto.
[0113] Melt flow index
[0114] The melt flow index (MFI) was measured using a Goettfert Melt Indexer MI-3 according to ISO 1133 (230°C / 2.16 kg load). MFI is expressed in g / 10 min.
[0115] Melting strength
[0116] Melt strength (MS) was measured using the following configuration and settings in accordance with the manufacturer's instructions, in combination with a Goettfert Rheograph 20 (capillary rheometer) and Goettfert Rheotens 71.97 (in cN):
[0117] Rheograph:
[0118] · Temperature: 220℃
[0119] · Melting time: 10 minutes
[0120] · Die: Capillary tube, length 30 mm, diameter 2 mm
[0121] · Barrel chamber and piston: 15 mm diameter
[0122] · Piston speed: 0.32 mm / sec, 72 seconds -1 Corresponding to the shear rate
[0123] · Melt strand speed (at start): 20 mm / sec
[0124] Rheotens:
[0125] · Wheel (strand) acceleration: 10 mm / sec 2
[0126] · Barrel-to-mid-wheel distance: 100 mm
[0127] · Strand length: 70 mm
[0129] Example 1 (Comparative Example - No moisture retainer b))
[0130] 500 g of polypropylene homopolymer (PP) powder, an organic peroxide formulation, and 0.5 g (0.1 phr) of Irganox® 1010 antioxidant were mixed in a bucket with a spatula and then mixed in a bucket mixer for 10 minutes. The organic peroxide formulation was added in an amount corresponding to the weight percent of pure peroxide presented in Table 1.
[0131] The following organic peroxide formulations were used:
[0132] · Dibenzoyl peroxide, 75% water content (Perkadox® L-W75, Nouryon®)
[0133] · Di(para-methylbenzoyl) peroxide, containing moisture 75% (Perkadox® PM-W75, Nouryon®)
[0134] The compound was extruded on a Haake PolyLab OS RheoDrive 7 system equipped with a Thermo Scientific Haake Rheomex OS PTW16 extruder (co-rotating twin screw, L / D=40) using the following settings:
[0135] · Temperature profile settings: 30°C in the hopper, 160°C in Zone 1, 190°C in Zones 2 to 4, 200°C in Zones 5 and 6, and 210°C in Zones 7 to 10.
[0136] · Screw speed: 280 rpm.
[0137] · Throughput: 1.2 kg / hour, administered by Brabender gravimetric screw feeder type DDW-MD2-DSR28-10.
[0138] · Purging nitrogen from the hopper (3.5 L / min) and the die (9 L / min).
[0139] The extruded material was guided through a water bath for cooling, and the cooled strand was granulated using an automatic granulator.
[0140] The melt flow index (MFI) and melt strength (MS) are directly related to the molecular weight and long-chain branching of the resulting polypropylene structure. A higher MFI indicates polypropylene degradation due to chain cleavage, whereas a lower MFI indicates favorable long-chain branching, which ultimately leads to an increase in MS. The melt flow index (MFI) and melt strength (MS) of the extruded HMS-PP compounds were analyzed as described below. Table 1 lists the corresponding results.
[0141]
[0142] From the above results, it can be seen that the use of an atmospheric environment increases polypropylene decomposition (higher MFI) and reduces melt strength compared to the use of an inert environment.
[0143] In addition, it can be seen that in an inert atmosphere, the best results are achieved when using 1 or 2 wt% of Perkadox PM-W75, i.e., di(para-methylbenzoyl)peroxide [di(4-methylbenzoyl)peroxide] (PTP), rather than using Perkadox L-W75, i.e., dibenzoyl peroxide (BPO).
[0145] Example 2
[0146] A solid form (flake) organic peroxide composition according to the present invention was prepared as follows.
[0147] Step 1: The following ingredients were added sequentially to a 50 L plugshear mixer (Lφdige mixer) and mixed at 60 rpm for 10 minutes: 4.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75), 0.9 kg of Irganox® 1010 (phenolic antioxidant), 0.9 kg of Irgafos 168 (phosphite antioxidant), 1.2 kg of DHT-4V (aluminum hydroxide magnesium carbonate hydrotalcite available from Kisuma Chemicals), followed by 4.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75).
[0148] Step 2: A 500 g batch of the mixture obtained (from Step 1) was compressed using an Alexanderwerk WP50 N / 75 compressor with the following compressor settings: pressure 40 bar, feeder 7.0, roller 1.0.
[0149] Step 3: The compressed product (from Step 2) was granulated using a Frewitt GLA ORV granulator equipped with a 6 mm sieve.
[0150] Step 4: The granulated product (from Step 3) was sieved using a Retsch AS 450 sieving device equipped with 3.15 mm and 1.0 mm sieves. The granulated product was first sieved through a 3.15 mm sieve and then through a 1.0 mm sieve. The fine powder (<1 mm) was returned to a compressor. The final product recovered from the sieve was in the form of solid flakes.
[0151] Based on the solid powder mixed in Step 1, the solid flakes had the following approximate composition:
[0152]
[0154] Example 3
[0155] In this example, polypropylene homopolymer (PP) powder and the solid flakes of Example 2 were fed separately into a twin-screw extruder. Two feeding methods were applied:
[0156] · Closed setting of hopper under nitrogen purge (5 liters / min) having a 1-cm opening for gas release ("inert atmosphere")
[0157] · Opening setting into the funnel under the atmosphere ("Atmosphere")
[0158] The compound was extruded on a Coperion W&P ZSK30 twin-screw extruder (co-rotating twin-screw, L / D=36) using the following settings:
[0159] · Throughput PP: 9.75 kg / hour, administered by Ktron weight loss feeder
[0160] · Organic peroxide formulation throughput: 0.25 kg / hour, administered by a Plasticolor 1500 single-screw feeder (volumetric), placed on a scale to record the administration rate in kg / hour
[0161] · Temperature profile settings: 20℃ in hopper, 160℃ in Zone 1, 190℃ in Zones 2 and 3, 200℃ in Zone 4, 210℃ in Zones 5 and 6 (Zone 6 = Die).
[0162] · Screw speed: 300 rpm
[0163] · Apply a vacuum degassing device at approximately -0.8 bar.
[0164] The extruded material was guided through a water bath for cooling, and the cooled strand was granulated using an automatic granulator.
[0165] As a comparison to demonstrate the beneficial effects of moisture in the flakes, a batch of moisture-free flakes of Example 2 was also tested (i.e., moisture was intentionally removed from the flakes of Example 2 by intentionally drying the flakes before the test). Table 2 shows the corresponding results.
[0166]
[0167] The above results clearly demonstrate the efficacy of the organic peroxide composition of the present invention. Polypropylene products manufactured under an atmospheric atmosphere had essentially the same technical characteristics as those manufactured under an inert atmosphere (i.e., the atmospheric atmosphere did not affect the performance of the peroxide composition). However, moisture-free flakes exhibited a significant loss of performance (polypropylene degradation, product yellowing, and lower melt strength) under an atmospheric atmosphere.
[0168] Therefore, the aforementioned contents can be summarized as follows:
[0169] · Comparative Example 1 - Organic peroxides containing moisture but without moisture retainers exhibit significant performance loss under atmospheric conditions.
[0170] · Comparative Example 3 - Organic peroxides containing moisture retainers but lacking moisture exhibit significant performance loss under atmospheric conditions.
[0171] · Example 3 of the present invention - Moisture retainer and Organic peroxides containing moisture do not exhibit significant performance loss under atmospheric conditions. not .
[0172] From these results, it can be concluded that moisture and moisture retainers act synergistically to produce substantially improved technical results.
[0174] Example 4
[0175] Example 3 was repeated using a polypropylene random copolymer instead of a polypropylene homopolymer. The fine powder sample (from step 4 of Example 2) was also tested by preparing a preliminary mixture with PP powder in a tumble mixer (concrete mill) and feeding the said preliminary mixture through a Ktron feeder at a rate of 10 kg / hour. Table 3 presents the corresponding results, which confirm the aforementioned conclusions.
[0176]
[0178] Example 5 - Moisture retention test (and "Protocol A")
[0179] The following solid composition was prepared by the step of mixing the following components: 80 parts by weight (pbw) of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75), 7.5 pbw of Irganox® 1010 (phenolic antioxidant), 7.5 pbw of Irgafos 168 (phosphorus antioxidant), and 5 pbw of a moisture retainer. The resulting solid composition contained the following components in the following amounts:
[0180]
[0181] Each solid composition was pelletized using a pelletizing press (Herzog HTP 40; press chamber diameter: 25 mm; suction product: 10.0 g; pressure: 20 ± 5 kN (0.4 ± 0.1 ton / cm²) 2 The samples were compressed on the )) and the moisture loss (i.e., moisture lost by pressurizing the tablets under these test conditions) was determined (i.e., the moisture loss % was calculated based on the weight difference between the powder mixture before pressurization and the tablets after pressurization). The moisture loss is recorded as a percentage of the original moisture content. For example, a weight loss of 1 g (i.e., a final weight of 9 g) is equivalent to a 50% loss of the original moisture content (10 g of 20 wt% = 2 g of moisture; therefore, 1 g of moisture leaked out of the tablets under pressurization = 50% moisture loss).
[0182] The following formulations were tested for their water retention capacity:
[0183] · Calcium stearate
[0184] · Lankroflex E2307 (epoxylated soybean oil)
[0185] · DHT-4V (aluminum hydroxide magnesium carbonate hydrotalcite available from Kisuma Chemicals)
[0186] Table 4 below shows the corresponding results.
[0187]
[0188] In the context of the present invention, a moisture retainer particularly suitable for use in the compositions disclosed herein is a retainer that causes the composition containing the aforementioned retains at least 60% of its original moisture content when the composition undergoes the aforementioned specific test conditions (i.e., moisture loss is 40% or less relative to the original moisture content).
[0189] That is, in the context of the present disclosure, the aforementioned formulation is a solid at room temperature and the following experimental protocol (in this application " Protocol A If it meets the requirements of "named as"), the preparation is a particularly suitable "moisture retainer b":
[0190] I. 60 parts by weight (pbw) of di(para-methylbenzoyl) peroxide mixed with 20 pbw of water, 7.5 pbw of pentaerythritol tetrakis(3-(3,5-di-ter-butyl-4-hydroxyphenyl)propionate), 7.5 pbw of tris(2,4-di-ter-butylphenyl)-phosphite, and 5 pbw of a moisture retainer;
[0191] II. Pelletizing Press (Herzog HTP 40; Press chamber diameter: 25 mm; Suction product: 10.0 g; Pressure: 20 ± 5 kN (0.4 ± 0.1 ton / cm²) 2 Compress 10 g of the composition obtained from step I) on ))
[0192] III. Weigh the compressed composition (pellet) obtained from Step II) in g;
[0193] IV. Measure the weight loss due to compression in Step II;
[0194] - That is, 10 g - [weight measured in Step III];
[0195] - Under these specific test conditions, the weight loss corresponds to the weight of the moisture lost as a result of the compressive force applied to the solid composition in Step II;
[0196] V. Calculate moisture loss %;
[0197] - That is, ([Weight loss at Stage IV] / 2)*100);
[0198] VI. Measure the % of the original moisture content retained in the compressed composition;
[0199] - That is, % of the original moisture content = 100% - [% measured in Step V];
[0200] VII. If the % calculated in step VI) is ≥ 60%, the formulation is a particularly suitable moisture retainer b) according to the present disclosure.
[0201] A desirable moisture retainer b) is that the organic peroxide composition containing formulation b) retains at least 80% of its original moisture content when undergoing Protocol A.
[0203] Example 6
[0204] As previously mentioned, when the preferred organic peroxide formulation used in WO 2019 / 038244 is fed into an extruder, there is always a possibility that the formulation may unintentionally leak onto the extruder device. If this occurs, the moisture (sensitizer) evaporates rapidly, increasing the concentration of the peroxide to a point where the peroxide becomes sensitive to friction and shock. If such an event occurs, the risk of explosion increases significantly, which must be clearly prevented (especially on an industrial scale). These problems make the handling of the organic peroxide formulation somewhat dangerous and difficult. The organic peroxide composition disclosed herein has been found to be much safer and easier to handle than the preferred organic peroxide formulation in WO 2019 / 038244. This finding was based on the following thermal explosion and shock sensitivity safety tests comparing the peroxide composition of Example 2 with the preferred organic peroxide formulation of WO 2019 / 038244.
[0205] Tested composition
[0206] · Peroxide composition of Example 2
[0207] · Dried peroxide composition of Example 2 (simulating the outflow and evaporation of moisture contained in the composition)
[0208] · Perkadox PM-W75 (Preferred organic peroxide formulation of WO 2019 / 038244)
[0209] · Dried Perkadox PM-W75 (simulates the leakage and evaporation of moisture contained in the formulation)
[0210] Safety test method
[0211] Thermal Explosion: Pressure Vessel Testing (PVT)
[0212] Criteria: Explosive - Limit diameter ≥ 9 mm
[0213] Intermediate - Limit diameter ≥ 3.5 mm and < 9 mm
[0214] Low - Limit diameter ≥ 1 mm and < 3.5 mm
[0215] None - Limit diameter < 1 mm
[0216] Reference: UN Manual of Tests and Criteria, 7th revised edition, 2019, Test method E.2
[0218] Impact Sensitivity: BAM Fallhammer
[0219] Criterion: Very High - Shock Sensitivity ≤ 2 J
[0220] High - Shock sensitivity > 2 J and ≤ 7.5 J
[0221] Medium - Shock sensitivity > 7.5 J and ≤ 40 J
[0222] Low - Shock sensitivity > 40 J
[0223] Reference: UN Manual of Tests and Criteria, 7th revised edition, 2019, Test method 3 (a) (ii)
[0224] result
[0225] Table 5 below shows the safety test results.
[0226]
[0227] These results indicate that the organic peroxide composition of the present invention is safer than Perkadox PM-W75 (no thermal explosion) and is much safer than Perkadox PM-W75 in a drying state (e.g., accidental spill near or over an extruder).
[0228] Considering the significantly improved atmosphere performance and significantly improved safety profile, the organic peroxide composition disclosed herein is an excellent candidate for use in polyolefin plastic recycling.
[0230] Example 7
[0231] An organic peroxide composition in solid form (solid granules) according to the present invention was prepared as follows.
[0232] Step 1: The following ingredients were added sequentially to a 10 L Eirich R02 infantary mixer and mixed for 15 minutes: 1.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75), 0.3 kg of Irganox® 1010 (phenolic antioxidant), 0.3 kg of Irgafos 168 (phosphite antioxidant), 0.4 kg of DHT-4V (aluminum hydroxide magnesium carbonate hydrotalcite available from Kisuma Chemicals), followed by 1.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75).
[0233] Step 2: A 4 kg batch of the mixture obtained (from Step 1) was compressed using a manual feed and an Amandus Kahl 14-175 compressor equipped with a 4 mm die plate, using the following compressor settings: 50 rpm; torque maintained at 2.5 to 2.8 kW.
[0234] Step 3: The compressed product (from Step 2) was manually sieved on a 2 mm sieve to remove fine powder. The final product recovered from the sieve was in the form of solid granules (composed mainly of substantially cylindrical granules with a cross-sectional diameter of 4 mm).
[0235] Based on the solid powder mixed in Step 1, the solid granules had the following approximate composition:
[0236]
[0238] Example 8
[0239] An organic peroxide composition in solid form (powder) according to the present invention was prepared by the step of combining the following components: 4.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75), 0.9 kg of Irganox® 1010 (phenolic antioxidant), 0.9 kg of Irgafos 168 (phosphite antioxidant), 1.2 kg of DHT-4V (aluminum hydroxide magnesium carbonate hydrotalcite available from Kisuma Chemicals), followed by 4.5 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75).
[0240] The solid powder had the following approximate composition:
[0241]
[0243] Example 9
[0244] In this embodiment, polypropylene homopolymer (PP) powder and a peroxide composition according to the present invention were individually fed into a twin-screw extruder under an atmospheric environment. The compounds were extruded on a Coperion W&P ZSK30 twin-screw extruder (co-rotating twin-screw, L / D=36) using the following settings:
[0245] · Throughput PP: 9.75 kg / hour (representing 8.78 kg / hour for the CaHPO4-based granules of Example 10), administered by a Ktron weight loss feeder
[0246] · Organic peroxide formulation throughput: 0.25 kg / hour (representing 0.22 kg / hour for the CaHPO4-based granules of Example 10), administered by a Plasticolor 1500 single-screw feeder (volumetric), placed on a balance to record the administration rate in kg / hour.
[0247] · Temperature profile settings: 20℃ in hopper, 160℃ in Zone 1, 190℃ in Zones 2 and 3, 200℃ in Zone 4, 210℃ in Zones 5 and 6 (Zone 6 = Die).
[0248] · Screw speed: 300 rpm
[0249] · Apply a vacuum degassing device at approximately -0.65 bar.
[0250] The extruded material was guided through a water bath for cooling, and the cooled strands were granulated using an automatic granulator. Table 6 shows the corresponding results.
[0251]
[0252] As expected, the organic peroxide compositions of the present disclosure (Examples 2, 7, and 8) substantially reduced the melt flow index and substantially increased the melt strength. However, an unexpected observation was that the physical form of the organic peroxide compositions appeared to have a performance effect on the MFI: the performance of the compressed compositions (flakes and granules) outperformed that of the equivalent formulations (mixed powders) that did not undergo a compression step. Thus, although the powder form yielded superior results, it was found that these results could be further improved by converting the formulations into compressed articles (e.g., flakes and granules).
[0254] Example 10
[0255] An organic peroxide composition in solid form (solid granules) according to the present invention was prepared as follows. In this example, dicalcium phosphate (CaHPO4.2H2O) was used as a moisture retainer.
[0256] Step 1: The following ingredients were added sequentially to a 10 L Eirich R02 planetary mixer and mixed for 15 minutes: 1.6 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75), 0.8 kg of dicalcium phosphate (CaHPO4.2H2O), followed by 1.6 kg of di(para-methylbenzoyl) peroxide (75% moisture content, Perkadox® PM-W75).
[0257] Step 2: A 4 kg batch of the mixture obtained (from Step 1) was compressed using a manual feed and an Amandus Kahl 14-175 compressor equipped with a 4 mm die plate, using the following compressor settings: 50 rpm; torque maintained at 2.5 to 2.8 kW.
[0258] Step 3: The compressed product (from Step 2) was manually sieved on a 2 mm sieve to remove fine powder. The final product recovered from the sieve was in the form of solid granules (composed mainly of substantially cylindrical granules with a cross-sectional diameter of 4 mm).
[0259] Based on the solid powder mixed in Step 1, the solid granules had the following approximate composition:
[0260]
[0261] Under PP processing conditions equivalent to those of Example 9, the granules exhibited expected performance (reduced MFI, increased melt strength; Table 7 shows the corresponding results).
[0262]
[0264] In this specification, unless expressly otherwise stated, the term “or” is used to mean an operator that returns a real value when either or both of the mentioned conditions are met, in contrast to an operator “exclusive or” which requires only one of the conditions to be met. The word “comprising” is used to mean “consisting of” rather than “constituting.” All prior teachings cited above are incorporated herein by reference. Any acknowledgment of any prior disclosed literature herein shall not be construed as an acknowledgment or representation that such teaching was common knowledge in Europe or elsewhere on the filing date of this application.
Claims
Claim 1 An organic peroxide composition in solid form, comprising: a) at least one organic peroxide of the following formula, wherein In the equation, each R is C 1-5 an organic peroxide individually selected from alkyl groups; b) at least one moisture retainer that is solid at room temperature; and c) an organic peroxide composition comprising moisture. Claim 2 An organic peroxide composition according to claim 1, wherein each R is individually selected from methyl, ethyl, n-propyl, i-propyl, n-butyl, secondary-butyl, tertiary-butyl, and tertiary-amyl. Claim 3 An organic peroxide composition according to claim 1 or 2, wherein at least one organic peroxide is di(para-methylbenzoyl) peroxide. Claim 4 The organic peroxide composition according to claim 1, wherein the organic peroxide composition comprises at least one organic peroxide a) in an amount of 40 to 75 weight% (weight%) based on the total weight of the organic peroxide composition. Claim 5 In claim 1, at least one moisture retainer b) is an organic peroxide composition selected from one or more of: anionic clay; water-absorbing polymer; metal carbonate and metal bicarbonate; metal oxide; metal silicate; metal phosphate; hydrophilic silica; or metal sulfate drying agent. Claim 6 In claim 5, the organic peroxide composition comprising at least one moisture retainer, which includes one or more anionic clays. Claim 7 The organic peroxide composition according to claim 1, wherein the organic peroxide composition comprises at least one moisture retainer b) in an amount of 1 to 30 weight% (weight%) based on the total weight of the organic peroxide composition. Claim 8 The organic peroxide composition according to claim 1, wherein the organic peroxide composition contains 5 to 30 weight% of moisture (weight% based on the total weight of the organic peroxide composition). Claim 9 An organic peroxide composition according to claim 1, further comprising one or more stabilizers. Claim 10 An organic peroxide composition according to claim 9, wherein one or more stabilizers are present in an amount of 5 to 20 weight% (weight%) based on the total weight of the organic peroxide composition. Claim 11 An organic peroxide composition according to claim 9, wherein one or more stabilizers include or consist of one or more antioxidants. Claim 12 A method for improving the melt strength of polypropylene by the step of extruding polypropylene in an extruder at a temperature of 150°C to 300°C in the presence of an organic peroxide composition according to claim 1. Claim 13 In paragraph 12, the organic peroxide composition is added to polypropylene before or during extrusion. Claim 14 A method according to claim 12, wherein the amount of organic peroxide composition used is such that the concentration of at least one organic peroxide a) is in the range of 0.1 to 5.0 g of peroxide per 100 g of polypropylene. Claim 15 In paragraph 12, the polypropylene is a homopolymer of propylene or a random, alternating, heteromorphic, or block copolymer or terpolymer of propylene and other olefins.
Citation Information
Patent Citations
Process for enhancing the melt strength of polypropylene
KR1020170017943A
Process for reducing fogging from high melt strength polypropylene
KR1020180087376A
Method for producing high melt strength polypropylene
KR1020200042520A
Solid organic peroxide composition
KR1020210068519A