Method for preparing high specific surface area porous carbons with controlled pore diameter
The chemical stabilization of biomass using phosphorus-containing compounds with amine groups addresses the limitations of existing methods, producing porous carbon with high specific surface area and controlled pore diameter, enhancing adsorption capabilities and environmental safety.
Patent Information
- Application Number
- KR1020230186842
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-12-20
AI Technical Summary
Existing methods for producing porous carbon face challenges in achieving high specific surface area and controlling pore diameter, particularly due to the limitations of physical and chemical activation processes, which are costly, environmentally harmful, and lack control over pore development.
A method involving a chemical stabilization step using phosphorus-containing compounds with amine groups to control biomass grain size, followed by washing, drying, carbonization, and physical activation, enabling precise control of pore diameter to 10 nm or less.
The method produces porous carbon with a high specific surface area and controlled pore diameter, achieving improved adsorption properties and environmental sustainability by using safer, more manageable chemicals.
Smart Images

Figure 112023143074299-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a method for producing high-specific surface area porous carbon capable of controlling pore diameter, and more specifically, to a method for producing porous carbon capable of having a high-specific surface area and controlling the pore diameter to a size of 10 nm or less by effectively controlling the crystal grain size of a biomass precursor to selectively induce an oxidation reaction of the crystal structure. Background Technology
[0002] Based on its high specific surface area and excellent pore characteristics, porous carbon is widely utilized in various fields, including air purifiers, water purification, volatile organic compound (VOC) removal, and energy storage devices. Generally, porous carbon is manufactured from biomass precursors through physical and / or chemical activation processes, and its pore characteristics are known to be influenced by the crystal structure of the precursor, carbonization temperature, and the sequence of activation methods. In particular, the adsorption properties of porous carbon for harmful gases and electrolyte ions do not improve simply with an increase in specific surface area; rather, they depend on the development of micropores and / or mesopores with pore diameters suitable for the size of the substances and / or ions to be adsorbed.
[0003] Against this backdrop, conventional research has been conducted to control the pore characteristics of porous carbon through physical and / or chemical activation processes. While the physical activation process is simple and very inexpensive, it suffers from disadvantages such as low activation yield and difficulty in controlling pore diameter, as pore development occurs through the oxidation of the amorphous or grain edges of the precursor. On the other hand, although the chemical activation process can produce porous carbon with a higher specific surface area compared to the physical process and allows for the control of pore characteristics, it presents various problems, including increased process costs due to the use of chemical activators, wastewater generation from the washing process, and equipment corrosion caused by the activators, and furthermore, it has the disadvantage of causing environmental pollution.
[0004] Phosphoric acid establishes the crystal structure of biomass through dehydration and crosslinking reactions at temperatures of 100 to 400°C, and phosphoric acid-stabilized biomass can be used to produce high-specific-surface-area porous carbon through a physical activation process. However, phosphoric acid is a highly acidic liquid compound, and therefore, the risk of the process increases when large amounts are used in actual industry. Furthermore, while excellent pore characteristics are observed when phosphoric acid-stabilized biomass is produced into high-specific-surface-area porous carbon through a physical activation process, it has the disadvantage of lacking economic feasibility due to the low activation yield.
[0005] Phosphorus-containing compounds containing amine groups, such as (NH4)H2PO4, (NH4)2HPO4, and (NH4)3PO4, are easy to handle in actual processes as they exist in a solid state at room temperature. Furthermore, as the amine groups decompose at temperatures above 150°C, they are compounds capable of causing dehydration and cross-linking reactions in biomass, similar to phosphoric acid. In particular, phosphorus-containing compounds containing amine groups allow for the control of the crystal structure size of biomass during the stabilization phase by controlling the number of bound amine groups. Therefore, there is an urgent need to develop a technology that not only produces porous carbon with a high specific surface area but also allows for easy control of pore diameter by using a chemical stabilization method with phosphorus-containing compounds containing amine groups, which are easier to handle than phosphoric acid and enable control of the crystal structure size of biomass during the stabilization phase. The problem to be solved
[0006] The problem that the present disclosure aims to solve is to provide a method for producing porous carbon with a high specific surface area by effectively controlling the crystal grain size of a biomass precursor using a chemical stabilization method using a phosphorus-containing compound containing an amine group.
[0007] Another problem that the present disclosure aims to solve is to provide a method for producing porous carbon capable of controlling pore diameter, which allows for easy control of pore diameter to 10 nm or less even when using a physical activation process, by selectively inducing an oxidation reaction of the crystal grains of a biomass precursor using a chemical stabilization method using a phosphorus-containing compound containing an amine group.
[0008] The problems that the present disclosure aims to solve are not limited to those mentioned above, and any unmentioned problems that the present disclosure aims to solve will be clearly understood by a person skilled in the art to which the present disclosure belongs ("person skilled in the art") from the description below. means of solving the problem
[0009] According to one embodiment of the present disclosure, a method for manufacturing high-specific surface area porous carbon capable of controlling pore diameter may be provided, comprising the following.
[0010] A chemical stabilization step for controlling biomass grain size using a chemical stabilizer;
[0011] A step of washing and drying the above-mentioned biomass with controlled grain size;
[0012] A step of producing carbonized biomass by carbonizing the above-mentioned washed and dried biomass with controlled grain size; and
[0013] An activation step for producing porous carbon from the above carbonized biomass through a physical activation process using an activator.
[0014] For example, the porous carbon may be characterized by having a pore diameter of 10 nm or less.
[0015] For example, the above biomass may be characterized as being a biomass including coconut shells, bamboo, kenaf, etc.
[0016] For example, the chemical stabilization step may be characterized by heating the biomass impregnated with a chemical stabilizer at 150 to 400°C to control the grain size of the biomass.
[0017] For example, the chemical stabilization step may be characterized by heat-treating the biomass impregnated with a chemical stabilizer for 6 to 12 hours.
[0018] For example, the chemical stabilization step may be characterized by being performed in an atmospheric atmosphere composed of inert gases such as N2, Ar, and He.
[0019] For example, the chemical stabilizer may be characterized by comprising one or more active ingredients selected from the group including (NH4)H2PO4, (NH4)2HPO4, and (NH4)3PO4.
[0020] For example, the concentration of the active ingredient may be characterized as being 30 to 90 parts by weight based on 100 parts by weight of the total chemical stabilizer.
[0021] For example, in the above activation step, the activator may be characterized as being one or more selected from the group including H2O, CO2, and air.
[0022] In addition, according to one embodiment of the present disclosure, a high-specific surface area porous carbon having a pore diameter of 10 nm or less can be provided by manufacturing according to the method for manufacturing a high-specific surface area porous carbon capable of controlling the pore diameter. Effects of the invention
[0023] According to the present disclosure, a method for producing porous carbon with a high specific surface area can be provided by effectively controlling the grain size of a biomass precursor using a chemical stabilization method with a phosphorus-containing compound containing an amine group.
[0024] According to the present disclosure, a method for producing porous carbon capable of controlling pore diameter can be provided, which allows for easy control of pore diameter to 10 nm or less even when using a physical activation process by selectively inducing an oxidation reaction of crystal grains of a biomass precursor using a chemical stabilization method using a phosphorus-containing compound containing an amine group.
[0025] The superior and / or useful effects according to the present disclosure are not limited to the effects of the present disclosure described above, and a person skilled in the art will also be able to obviously recognize, based on the disclosure of the present specification, superior and / or useful effects of the present disclosure that are not explicitly disclosed in the present specification, and it should be understood that these are intentionally disclosed by the present specification and are obviously included within the scope of the present disclosure. Brief explanation of the drawing
[0026] FIG. 1 is a schematic diagram illustrating a method for manufacturing porous carbon according to one embodiment of the present disclosure. FIGS. 2 and FIGS. 3 are figures showing the results of an analysis of the pore distribution of porous carbon prepared according to a method for preparing porous carbon according to one embodiment of the present disclosure. Specific details for implementing the invention
[0027] The terms or words used in this specification and claims are not intended to be interpreted as being limited to their commonly accepted dictionary meanings, and a person skilled in the art will clearly understand that said terms or words are used within the scope of conveying what this disclosure means, within the scope of expressing the concept that this specification and claims obviously intend to convey.
[0028] Furthermore, a person skilled in the art will clearly understand that the configurations described in the aspects, modes of embodiment, examples, etc., of the present disclosure described in this specification are merely preferred examples presented at the time to enable a person skilled in the art to understand and reproduce the present disclosure, and are not intended to limit the present disclosure thereto.
[0029] Furthermore, the descriptions and specific embodiments regarding each configuration described in this specification may be obviously applied to the descriptions and specific embodiments of each other configuration. That is, a person skilled in the art will clearly understand that all possible combinations of the various configurations and specific embodiments disclosed in this specification fall within the scope disclosed herein.
[0030] As used herein, the term "and / or" is a term comprising each of the items mentioned and all combinations of two or more. Additionally, where a singular term is used herein, it is disclosed including the plural form unless otherwise noted.
[0031] As used herein, the terms "comprise" and "comprising" are terms that permit the existence or addition of items other than those mentioned, and as used herein, the terms "consist," "consist," "consisting," and "consisting" are terms that do not permit the existence or addition of items other than those mentioned.
[0032] As used in this specification, the term "to" indicates a numerical range in which the range of values represented by "to" includes the values listed before and after the term as lower and upper values, respectively. Where multiple upper and / or lower values of an arbitrary numerical range are disclosed, the numerical range is disclosed such that any one of the multiple lower values and any one of the multiple upper values are respectively set as the lower and upper values.
[0033] The terms “about” and / or “approximately” as used in this specification refer to a numerical range between a 10% upper limit value and a lower limit value based on the value indicated using “about” and / or “approximately”.
[0034] Terms or words used in this specification and claims should not be interpreted as being limited to their ordinary dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of this disclosure, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention. Accordingly, the configurations described in the embodiments of this specification are merely preferred embodiments of this disclosure and do not represent all of the technical spirit of this disclosure; therefore, it should be understood that various equivalents and modifications that can replace them may exist at the time of filing this application.
[0035] Meanwhile, each description and embodiment disclosed in this specification may also be applied to other descriptions and embodiments. That is, all combinations of the various elements disclosed in this specification fall within the scope of this disclosure, and descriptions omitted in one embodiment may be interpreted in the same manner as described in other embodiments. Furthermore, the scope of this disclosure should not be considered limited by the specific descriptions provided below.
[0036] According to one embodiment of the present disclosure, a method for manufacturing porous carbon may be provided.
[0037] For example, the method for manufacturing the porous carbon described above may be a method for manufacturing high-specific surface area porous carbon capable of controlling pore diameter, comprising the following.
[0038] A chemical stabilization step for controlling biomass grain size using a chemical stabilizer;
[0039] A step of washing and drying the above-mentioned biomass with controlled grain size;
[0040] A step of producing carbonized biomass by carbonizing the above-mentioned washed and dried biomass with controlled grain size; and
[0041] An activation step for producing porous carbon from the above carbonized biomass through a physical activation process using an activator.
[0042] For example, the porous carbon may be characterized by having a pore diameter of 10 nm or less.
[0043] For example, the above biomass may be characterized as being biomass including coconut shells, bamboo, kenaf, etc.
[0044] For example, the chemical stabilization step may be characterized by heating the biomass impregnated with a chemical stabilizer at 150 to 400°C to control the grain size of the biomass.
[0045] For example, the chemical stabilization step may be characterized by heat-treating the biomass impregnated with a chemical stabilizer for 6 to 12 hours.
[0046] For example, the chemical stabilization step may be characterized by being performed in an atmospheric atmosphere composed of inert gases such as N2, Ar, and He.
[0047] For example, the chemical stabilizer may be characterized by comprising one or more active ingredients selected from the group including (NH4)H2PO4, (NH4)2HPO4, and (NH4)3PO4.
[0048] For example, the concentration of the active ingredient may be characterized as being 30 to 90 parts by weight based on 100 parts by weight of the total chemical stabilizer.
[0049] For example, in the above activation step, the activator may be characterized as being one or more selected from the group including H2O, CO2, and air.
[0050] In addition, according to one embodiment of the present disclosure, a high-specific surface area porous carbon having a pore diameter of 10 nm or less can be provided by manufacturing according to the method for manufacturing a high-specific surface area porous carbon capable of controlling the pore diameter.
[0051] The present disclosure is described in more detail below using examples. Process conditions and preparation steps not specified in the following examples may be obvious in the art to which the present disclosure belongs, and a person skilled in the art will be able to select them without difficulty based on the present disclosure and reproduce the problem-solving principles of the present disclosure.
[0052] In addition, regarding the manufacturing method according to the present disclosure, unless otherwise specified, each step constituting the manufacturing method is to be understood as being carried out at room temperature (25°C) and each step is to be performed by means and tools that a person skilled in the art can derive without particular difficulty.
[0053] Preparation Example: Preparation of Biomass and Chemical Stabilizers
[0054] Kenaf was prepared as biomass, and 10g of biomass was dried in a drying oven at 100℃ for 24 hours before use. (NH4)H2PO4 (Daejung Chem, Korea) was used as a chemical stabilizer and was prepared by diluting it in distilled water to a concentration of 40% by weight to make a total of 100ml.
[0055] Example 1: Porous carbon prepared according to the method of the present disclosure
[0056] Kenaf was placed in a graphite crucible, impregnated using the chemical stabilizer prepared in the preparation example, and maintained at room temperature for about 10 minutes. The impregnated kenaf was then placed in a forced-circulation oven under an atmospheric atmosphere, heated to a stabilization temperature of 200°C at a heating rate of 10°C / min, and maintained for 12 hours to decompose the crystal structure of the biomass and establish it through a cross-linking reaction.
[0057] Afterward, the stabilized kenaf was washed five times with distilled water, and the pH was observed to be 6.5. Subsequently, the washed kenaf was dried in an oven at 100°C for 24 hours.
[0058] Washed and dried kenaf was loaded into a reactor under a nitrogen atmosphere (N2, 99.999%, 200cc / min), heated to 700℃ at a heating rate of 10℃ / min, carbonized for 1 hour, left to stand, and then naturally cooled to room temperature.
[0059] Subsequently, the carbonized kenaf was loaded into a reactor under a nitrogen atmosphere (N2, 99.999%, 200 cc / min) and heated to 900°C at a heating rate of 10°C / min. Then, the nitrogen gas was cut off and the atmosphere was switched to a steam atmosphere. Steam was supplied at a flow rate of 0.5 ml / min to activate the mixture for 80 minutes, after which it was naturally cooled to room temperature under a nitrogen atmosphere to produce high-specific-surface-area porous carbon. This was prepared as the porous carbon of Example 1.
[0060] Example 2: Use of different chemical stabilizers
[0061] Porous carbon of Example 2 was prepared by performing the same process as the manufacturing method described in Example 1, except that (NH4)2HPO4 was used as the chemical stabilizer instead of (NH4)H2PO4.
[0062] Example 3: Use of different chemical stabilizers
[0063] Porous carbon of Example 3 was prepared by performing the same process as the manufacturing method described in Example 1, except that (NH4)3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4.
[0064] Example 4: Use of different chemical stabilizers and different stabilization temperatures
[0065] Porous carbon of Example 4 was prepared by performing the same process as the manufacturing method described in Example 1, except that (NH4)3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4 and the stabilization temperature was 250℃ instead of 200℃.
[0066] Example 5: Use of different chemical stabilizers and different stabilization temperatures
[0067] Porous carbon of Example 5 was prepared by performing the same process as the manufacturing method described in Example 1, except that (NH4)3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4 and the stabilization temperature was 300℃ instead of 250℃.
[0068] Example 6: Use of different chemical stabilizers and different stabilization temperatures
[0069] Porous carbon of Example 6 was prepared by performing the same process as the manufacturing method described in Example 1, except that (NH4)3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4 and the stabilization temperature was 350℃ instead of 200℃.
[0070] Comparative Example 1: Use of comparative chemical stabilizers
[0071] Comparative Example 1 porous carbon was prepared by performing the same process as the manufacturing method described in Example 1, except that 85 wt% of H3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4.
[0072] Comparative Example 2: Use of comparative chemical stabilizers and different stabilization temperatures
[0073] Comparative Example 2 porous carbon was prepared by performing the same process as the manufacturing method described in Example 1, except that 85 wt% of H3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4 and the stabilization temperature was 250°C instead of 200°C.
[0074] Comparative Example 3: Use of comparative chemical stabilizers and different stabilization temperatures
[0075] Comparative Example 3 porous carbon was prepared by performing the same process as the manufacturing method described in Example 1, except that 85 wt% of H3PO4 was used as the chemical stabilizer instead of (NH4)H2PO4 and the stabilization temperature was 300°C instead of 200°C.
[0076] Comparative Example 4: Use of commercial porous carbon
[0077] Commercial coconut shell-based porous carbon was prepared as the porous carbon of Comparative Example 4.
[0078] Experimental Example 1: Evaluation of Porous Carbon Porosity Characteristics
[0079] The pore characteristics of the porous carbons in Examples 1 to 6 and Comparative Examples 1 to 4 were evaluated by measuring the specific surface area and activation yield. First, each sample (porous carbon in Examples 1 to 6 and Comparative Examples 1 to 4) was tested at a residual pressure of 10 at 573K. -3After degassing for 6 hours while maintaining a pressure below torr, the amount of nitrogen (N2) gas adsorbed at 77K according to relative pressure (P / P0) was measured using an isothermal adsorption device (BELSORP-max, BEL JAPAN, Japan), and the specific surface area of the porous carbon was calculated. In addition, the yield change of each sample was evaluated by measuring the change in porous carbon mass relative to the biomass precursor used as a percentage. The results are shown in Table 1 below.
[0080] chemistry stabilizer stabilization temperature (℃) S BET (m 2 / g) V Total (cm 3 / g) V Micro (cm 3 / g) V Meso (cm 3 / g) transference number (%) Example 1 (NH4)H2PO4 200 1950 0.89 0.70 0.19 16.2 Example 2 (NH4)2HPO4 2010 0.93 0.71 0.22 15.8 Example 3 (NH4)3PO4 2100 1.01 0.70 0.31 15.4 Example 4 250 2220 1.10 0.72 0.38 13.7 Example 5 300 2180 1.18 0.69 0.49 12.8 Example 6 350 2090 1.24 0.68 0.56 12.4 Comparative Example 1 H3PO4 200 2020 0.94 0.72 0.22 13.5 Comparative Example 2 250 2050 0.95 0.68 0.27 12.4 Comparative Example 3 300 2150 1.03 0.70 0.33 11.2 Comparative Example 4 - - 1780 0.83 0.70 0.13 -
[0081] As confirmed in Table 1 above, kenaf-based porous carbon chemically stabilized with phosphorus-containing compounds containing amine groups, such as (NH4)H2PO4, (NH4)2HPO4, and (NH4)3PO4, was observed to have a specific surface area similar to that of porous carbon prepared by conventional methods, and the development of a high mesopore volume was confirmed. In particular, the porous carbon of Example 3 was found to have a higher mesopore volume and activation yield at a similar specific surface area.
[0082] Experimental Example 2: Evaluation of Pore Distribution of Porous Carbon
[0083] The pore characteristics of porous carbons in Examples 1 to 6 and Comparative Examples 1 to 4 were evaluated by analyzing the pore distribution. The results of the analysis of porous carbons in Examples 1 to 6 are shown in FIG. 2, and the results of the analysis of porous carbons in Comparative Examples 1 to 4 are shown in FIG. 3.
[0084] As can be seen in FIGS. 2 and 3, when compared to the pore distribution of porous carbon in Examples 1 to 6 and porous carbon in Comparative Examples 1 to 4, it can be confirmed that mesopores with a pore diameter of 2 nm or more are better developed, and as the number of amine groups included in the chemical stabilizer used increases, mesopores with a pore diameter of 2 to 4 nm are better developed, and it was confirmed that control of pore diameter of 10 nm or less was achieved.
[0085] Although preferred embodiments of the present disclosure have been described in detail above, the scope of the present disclosure is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts of the present disclosure as defined in the following claims are also included within the scope of the present disclosure.
Claims
Claim 1 A method for producing high-specific surface area porous carbon capable of controlling pore diameter, comprising: a chemical stabilization step of controlling the grain size of biomass using a chemical stabilizer; a step of washing and drying the biomass with controlled grain size; a step of carbonizing the washed and dried biomass with controlled grain size to produce carbonized biomass; and an activation step of producing porous carbon through a physical activation process using an activator, wherein the porous carbon has a pore diameter of 10 nm or less, the chemical stabilization step controls the grain size of the biomass by heating the biomass impregnated with the chemical stabilizer at 150 to 400°C, the chemical stabilization step heat-treats the biomass impregnated with the chemical stabilizer for 6 to 12 hours, and the chemical stabilizer comprises one or more active ingredients selected from the group including (NH4)H2PO4, (NH4)2HPO4, and (NH4)3PO4. Claim 2 delete Claim 3 A method for producing high-specific surface area porous carbon capable of controlling pore diameter, wherein, in claim 1, the biomass is one or more biomass selected from the group including coconut shells, bamboo, and kenaf. Claim 4 delete Claim 5 delete Claim 6 A method for producing high-specific surface area porous carbon capable of controlling pore diameter, wherein, in claim 1, the chemical stabilization step is performed in an atmospheric atmosphere composed of one or more gases selected from inert gases including N2, Ar, and He. Claim 7 delete Claim 8 A method for manufacturing high-specific surface area porous carbon capable of controlling pore diameter, wherein, in claim 1, the concentration of the active ingredient is 30 to 90 parts by weight based on 100 parts by weight of the total chemical stabilizer. Claim 9 A method for producing high-specific surface area porous carbon capable of controlling pore diameter, wherein, in claim 8, the activator in the activation step is one or more selected from the group including H2O, CO2, and air. Claim 10 High-specific-surface-area porous carbon having a pore diameter of 10 nm or less, manufactured according to any one of the manufacturing methods of claims 1, 3, 6, 8, and 9.
Citation Information
Patent Citations
Method for preparing high specific surface area micropore bamboo fiber base activated carbon fiber
CN104016343A
Activated carbon for automobile canister with low butane retentivity and its manufacturing method