Separator for rechargeable lithium battery and rechargebale lithium battery including same
The separator for lithium secondary batteries, with a polyethylene and ceramic coating layer and adhesive layer, addresses safety concerns by maintaining adhesion and permeability, ensuring cycle life and safety during high temperatures.
Patent Information
- Application Number
- KR1020220047170
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-15
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-04-15
AI Technical Summary
Lithium secondary batteries face safety risks due to separator shrinkage and mechanical damage at high temperatures, leading to potential short circuits and ignition.
A separator for lithium secondary batteries comprising a porous substrate with a coating layer containing polyethylene particles and a first ceramic in a specific weight ratio, and an adhesive layer with a second ceramic and a binder, where the ceramics have different average sizes, enhancing adhesion and air permeability.
The separator provides excellent adhesion to electrodes, maintains cycle life characteristics, and ensures safety by preventing ion movement shutdown during high temperature events.
Smart Images

Figure 112022040823915-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The invention relates to a separator for a lithium secondary battery and a lithium secondary battery including the same. Background Technology
[0002] Lithium-ion batteries are attracting attention as power sources for various electronic devices due to their high discharge voltage and high energy density.
[0003] A lithium secondary battery has a structure in which a positive electrode and a negative electrode are arranged facing each other and filled with an electrolyte, and a separator is located between the positive and negative electrodes to prevent a short circuit. The separator may be a porous material capable of permeating ions or an electrolyte.
[0004] If a battery is exposed to a high-temperature environment due to abnormal behavior, the separator may mechanically shrink or be damaged due to its melting characteristics at low temperatures. In this case, the positive and negative electrodes may come into contact, potentially causing the battery to ignite. To address this problem, technology is required to suppress separator shrinkage and ensure battery safety. The problem to be solved
[0005] One embodiment provides a separator for a lithium secondary battery with excellent safety.
[0006] Another embodiment provides a lithium secondary battery comprising the separator. means of solving the problem
[0007] According to one embodiment, the apparatus comprises: a porous substrate; a coating layer located on at least one surface of the porous substrate and comprising polyethylene particles and a first ceramic in a weight ratio of 6:4 to 8:2; and an adhesive layer located on one surface of the coating layer and comprising a second ceramic and a binder in a weight ratio of 7:3 to 5:5. ,The above binder comprises polyvinylidene fluoride and polyvinylidene-hexapropylene copolymer in a weight ratio of 6:4 to 4:6, and provides a separator for a lithium secondary battery in which the average size of the first ceramic and the second ceramic are different.
[0008] The mixing ratio of the second ceramic and the binder may be 6:4 to 5:5 by weight.
[0009] The average size of the first ceramic may be larger than the average size of the second ceramic.
[0010] The average size of the first ceramic may be 550 nm to 750 nm.
[0011] The cross-sectional thickness of the coating layer may be 0.5㎛ to 5㎛.
[0012] The cross-sectional thickness of the adhesive layer may be 0.1㎛ to 4.0㎛.
[0013] The size ratio of the first ceramic and the second ceramic may be 5:1 to 1.5:1.
[0014] The first ceramic or the second ceramic may be identical or different from each other, and is made of Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may be SrTiO3, BaTiO3, Mg(OH)2, boehmite, or a combination thereof.
[0015] In one embodiment, the first ceramic may be boehmite, and the second ceramic may be Al2O3.
[0016] The coating layer may further comprise a vinyl group-containing binder. The vinyl group-containing binder may comprise a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, a second structural unit comprising at least one of a structural unit derived from (meth)acrylic acid, (meth)acrylate, (meth)acrylonitrile, or a combination thereof, and a structural unit derived from (meth)acrylamidosulfonic acid, a (meth)acrylamidosulfonic acid salt, or a combination thereof.
[0017] According to another embodiment, a lithium secondary battery is provided comprising: a cathode comprising a negative electrode active material; a positive electrode comprising a positive electrode active material; a separator located between the cathode and the positive electrode; and a non-aqueous electrolyte.
[0018] Specific details of other embodiments are included in the detailed description below. Effects of the invention
[0019] A separator for a lithium secondary battery according to one embodiment has excellent adhesion to the electrode and can exhibit excellent cycle life characteristics and excellent air permeability characteristics. Brief explanation of the drawing
[0020] FIG. 1 is a simplified drawing of a lithium secondary battery according to one embodiment. Specific details for implementing the invention
[0021] Embodiments of the present invention will be described in detail below. However, these are presented as examples and do not limit the present invention, and the present invention is defined only by the scope of the claims set forth below. The terms used herein are used merely to describe exemplary embodiments and are not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.
[0022] "Combinations of these" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.
[0023] Terms such as "include," "equip," or "have" are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0024] In the drawings, thicknesses have been enlarged to clearly represent various layers and regions, and the same reference numerals have been used for similar parts throughout the specification. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between.
[0025] "Thickness" may be measured, for example, through photographs taken with an optical microscope such as a scanning electron microscope.
[0026] The average size may be the average particle diameter (D50), and unless otherwise defined in this specification, the average particle diameter (D50) refers to the diameter of a particle whose cumulative volume in the particle size distribution is 50 volume%.
[0027] The average particle size (D50) can be measured using methods widely known to those skilled in the art, for example, by using a particle size analyzer, or by using transmission electron microscope (TEM) images or scanning electron microscope (SEM) images. Alternatively, the average particle size (D50) value can be obtained by using a measuring device utilizing dynamic light scattering, performing data analysis to count the number of particles for each particle size range, and then calculating from this.
[0028] One embodiment provides a separator for a lithium secondary battery comprising a porous substrate, a coating layer located on at least one surface of the porous substrate, and an adhesive layer located on one surface of the coating layer.
[0029] The coating layer may contain polyethylene particles and a first ceramic in a weight ratio of 6:4 to 8:2. In the coating layer, if the weight ratio of the polyethylene particles and the first ceramic deviates from the above range, for example, if an excessive amount of polyethylene particles is used, it is difficult to form the coating layer, the air permeability is reduced and unsuitable, and the adhesion to the porous substrate may be reduced. Furthermore, if an excessive amount of polyethylene particles is used, the safety effect resulting from the use of polyethylene particles cannot be sufficiently obtained. That is, if a small amount of polyethylene particles is used, for example, if an equal amount of polyethylene particles and the first ceramic is used, the coating layer must be formed very thickly to obtain the effect resulting from the use of polyethylene particles. In this case, the separator becomes too thick, deviating from conventional battery specifications, which poses a problem that makes it practically difficult to use in battery manufacturing. If a battery of a conventional size is manufactured using this separator, the size of the positive or negative electrode must be reduced, and consequently, the capacity may be lowered. Alternatively, if a battery is manufactured using this separator and conventional positive and negative electrodes, the final battery thickness increases excessively, making it practically difficult to use.
[0030] The above polyethylene particles are polymer particles having a melting temperature of 80°C to 130°C and may be in the form of wax. At this time, the wax form, that is, polyethylene wax, means that the molecular weight is greater than that of an oligomer and smaller than that of a polymer, and for example, the weight-average molecular weight (Mw) may be 1000 g / mol to 5000 g / mol, 1000 g / mol to 3000 g / mol, or 1500 g / mol to 3000 g / mol.
[0031] The above polyethylene particles do not melt during normal charging and discharging within the battery, but when a high temperature phenomenon occurs within the battery, they melt at a temperature above the melting temperature before the porous substrate, thereby blocking the pores within the porous substrate and blocking the movement of ions, which induces a rapid shutdown function, thereby ensuring the safety of the secondary battery. The average size of the above polyethylene particles may be 0.1㎛ to 3.0㎛. Specifically, the average size of the above polyethylene particles may be 0.1㎛ or more and 2.0㎛ or less, or 0.5㎛ or more and 2.0㎛ or less, for example, 0.5㎛ or more and 1.5㎛, or 1.0㎛ or more and 1.5㎛ or less.
[0032] The above coating layer may further comprise a water-based binder, for example, a vinyl group-containing binder. In this specification, '(meth)acrylic' means acrylic or methacrylic.
[0033] The above vinyl group-containing binder may comprise a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, a second structural unit comprising at least one of a structural unit derived from (meth)acrylic acid, (meth)acrylate, (meth)acrylonitrile, or a combination thereof, and a structural unit derived from (meth)acrylamidosulfonic acid, a (meth)acrylamidosulfonic acid salt, or a combination thereof.
[0034] The first structural unit derived from the above (meth)acrylamide includes an amide functional group (-NH2) within the structural unit. The -NH2 functional group can improve adhesion characteristics with the porous substrate and the electrode, and can more firmly fix the first inorganic particles within the coating layer by forming hydrogen bonds with the -OH functional group of the first inorganic particles described later, thereby enhancing the heat resistance of the separator.
[0035] The structural unit derived from (meth)acrylic acid, (meth)acrylate, (meth)acrylonitrile, or a combination thereof included in the second structural unit above serves to fix polyethylene particles and first ceramic particles onto a porous substrate, and at the same time can provide adhesion so that the coating layer adheres well to the porous substrate and electrode, and can contribute to improving the heat resistance and air permeability of the separator. In addition, by including a carboxyl functional group (-C(=O)O-) within the structural unit, it can contribute to improving the dispersibility of the coating slurry, and by including a nitrile group, it can improve the oxidation resistance of the separator and reduce the moisture content.
[0036] In addition, a structural unit derived from (meth)acrylamidosulfonic acid, (meth)acrylamidosulfonic acid salt, or a combination thereof included in the second structural unit can enhance the heat resistance of the separator by reducing the mobility of the copolymer containing it through the inclusion of a bulky functional group.
[0037] The above vinyl group-containing binder may further improve heat resistance by including a vinyl group-containing copolymer having a glass transition temperature (Tg) of 150°C or higher, and thereby may exhibit excellent heat resistance and air permeability of the separator for a lithium secondary battery by being included in the coating layer together with the first inorganic particles and polyethylene particles.
[0038] The adhesive layer may contain a second ceramic and a binder in a weight ratio of 7:3 to 5:5. In the adhesive layer, if the weight ratio of the second ceramic and the binder falls outside the above range, for example, if an excessive amount of binder is used, the air permeability increases too much, and consequently, the battery resistance may increase, and if a smaller amount of binder is used, the adhesion to the electrode may decrease.
[0039] In one embodiment, the binder may include a polyvinylidene fluoride (PVdF) and polyvinylidene-hexapropylene (PVdF-HFP) copolymer, and in particular, may include the polyvinylidene fluoride (PVdF) and polyvinylidene-hexapropylene (PVdF-HFP) copolymer in a weight ratio of 6:4 to 4:6. If the weight ratio of PVdF and PVdF-HFP as the binder included in the adhesive layer falls outside the above range, both the adhesion strength to the electrode and the air permeability are reduced, making it unsuitable. Thus, the adhesive layer includes an organic binder, and in one embodiment, as the adhesive layer includes an organic binder, the adhesion strength to the electrode can be further improved. In particular, both dry adhesion strength and wet adhesion strength can be improved. Accordingly, the separator according to one embodiment is suitable because it can satisfy both dry adhesion and wet adhesion, which are required as the form of the lithium secondary battery changes from the conventional winding type to the recent stack type.
[0040] The effect of improving dry adhesion and wet adhesion cannot be obtained when using a water-based binder, and especially when using an organic binder, it cannot be obtained when using polyvinylidene fluoride (PVdF) and polyvinylidene-hexapropylene (PVdF-HFP) copolymer in a weight ratio other than 6:4 to 4:6.
[0041] In one embodiment, dry adhesion refers to the adhesion between the separator and the active material layer that occurs when heat and pressure are applied to an electrode assembly (winding type or stack type, regardless of shape) of a positive electrode, a separator, and a negative electrode. Wet adhesion refers to the adhesion between the separator and the active material layer that occurs when heat and pressure are applied after an electrolyte is injected into the electrode assembly.
[0042] The adhesion between the separator and the active material layer must be maintained at an appropriate level so that when the electrode assembly is moved for subsequent battery manufacturing processes, such as electrolyte injection, after manufacturing the electrode assembly, the separator and the active material layer can be moved while attached. However, if the adhesion is too low, the separator and the active material layer may separate, and this problem can occur significantly, especially in stacked types. Furthermore, if appropriate wet adhesion is not maintained during the formation charge / discharge of the final battery after processes such as electrolyte injection, a deformation phenomenon in which the battery swells may occur. Accordingly, for battery application, the dry adhesion must satisfy 90N or more and the wet adhesion must satisfy 600N or more, and the separator of one embodiment is suitable as it can satisfy these physical properties.
[0043] Additionally, the average sizes of the first ceramic and the second ceramic may be different. In one embodiment, the average size of the first ceramic may be larger than the average size of the second ceramic.
[0044] When the average size of the first ceramic is larger than the average size of the second ceramic, the effect of using polyethylene particles in the coating layer can be obtained more fully, and superior cycle life characteristics can be obtained.
[0045] If the average size of the first ceramic is smaller than the average size of the second ceramic, that is, if the second ceramic is larger than the first ceramic, an excessive amount of binder is required, and consequently, the thickness of the adhesive layer increases, the resistance increases, the lifespan may decrease, and there may be problems such as a decrease in energy density.
[0046] The average size of the first ceramic may be 550 nm to 750 nm, 600 nm to 750 nm, or 600 nm to 700 nm. When the average size of the first ceramic falls within the above range, the cycle life characteristics can be improved because there is an appropriate air permeability, for example, 240 sec / 100 cc or less, and excellent adhesion to the porous substrate. The air permeability of the separator should be as low as possible, and is appropriate when it is at most 240 sec / 100 cc or less.
[0047] In addition, the average size of the second ceramic may be 200 nm to 300 nm, or 230 nm to 270 nm. When the average size of the second ceramic falls within the above range, an appropriate specific surface area can be maintained, the binder effect can be appropriately maintained, and the adhesive layer can be formed with an appropriate thickness. If an excessively large second ceramic, for example, one larger than the average size, is used, it is not appropriate because there is a risk that the thickness of the adhesive layer will increase excessively. In one embodiment, the size ratio of the first ceramic to the second ceramic may be 5:1 to 1.5:1, 4:1 to 1.5:1, and also 3.75:1 to 1.8:1.
[0048] The first ceramic or the second ceramic may be identical or different from each other, and is made of Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may be SrTiO3, BaTiO3, Mg(OH)2, boehmite, or a combination thereof. In one embodiment, the first ceramic may be boehmite, and the second ceramic may be Al2O3.
[0049] In addition, the ceramic may be cubic, plate-shaped, spherical, or amorphous, and its shape does not need to be limited.
[0050] The porous substrate has a plurality of pores and may be a substrate typically used in batteries. The porous substrate may include any one polymer selected from the group consisting of polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene oxide, cyclic olefin copolymer, polyphenylene sulfide, polyethylene naphthalate, glass fiber, Teflon, and polytetrafluoroethylene, or a copolymer or mixture of two or more of these.
[0051] In one embodiment, the porous substrate may comprise a polyolefin. Examples of porous substrates comprising a polyolefin include a polyethylene monolayer, a polypropylene monolayer, a polyethylene / polypropylene double layer, a polypropylene / polyethylene / polypropylene triple layer, or a polyethylene / polypropylene / polyethylene triple layer.
[0052] The cross-sectional thickness of the coating layer may be 0.5 μm to 5 μm, and may be, for example, 1 μm to 5 μm, 1 μm to 4 μm, 1 μm to 3 μm, or 1 μm to 2 μm. In one embodiment, the thickness of the coating layer is not limited thereto and can be appropriately adjusted according to the thickness, weight, porosity, etc. of the porous substrate.
[0053] The cross-sectional thickness of the adhesive layer may be 0.1㎛ to 4.0㎛, for example, 0.1㎛ to 3.0㎛, 0.1㎛ to 2.0㎛, 0.1㎛ to 1.0㎛, for example, 0.3㎛ to 1.0㎛, 0.4㎛ to 1.0㎛, 0.4㎛ to 0.9㎛, or 0.5㎛ to 0.9㎛. When the thickness of the adhesive layer falls within the above range, it may exhibit superior cycle life, dry adhesion, and wet adhesion.
[0054] The porous substrate may have a thickness of 1 μm to 40 μm, for example, 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 5 μm to 10 μm.
[0055] As such, a separator according to one embodiment may comprise a coating layer containing polyethylene particles and a first ceramic in a specific weight ratio, and a second ceramic and a binder in a specific weight ratio, wherein the binder comprises polyvinylidene fluoride and a polyvinylidene-hexapropylene copolymer in a specific weight ratio, and the first ceramic and the second ceramic may have different average sizes. A separator having such a combination has excellent adhesion to an electrode and also has excellent air permeability, so that lithium migration can occur easily.
[0056] A separator for a lithium secondary battery according to one embodiment can be manufactured by various known methods. For example, the separator for a lithium secondary battery may form a coating layer by applying a composition for forming a coating layer to one or both sides of a porous substrate and drying it, and then form an adhesive layer by applying a composition for forming an adhesive layer to one side of the coating layer and drying it.
[0057] The above-described composition for forming a coating layer may comprise a first inorganic particle, a polyethylene particle, and a solvent, and may further comprise a vinyl group-containing binder. The solvent is not particularly limited as long as it can dissolve or disperse the first inorganic particle, the polyethylene particle, and the vinyl group-containing binder. In one embodiment, the solvent may be an aqueous solvent comprising water, an alcohol, or a combination thereof. The alcohol may be methyl alcohol, ethyl alcohol, propyl alcohol, or a combination thereof.
[0058] The above coating can be performed, for example, by gravure coating, spin coating, dip coating, bar coating, die coating, slit coating, roll coating, inkjet printing, etc., but is not limited thereto.
[0059] The above drying may be performed by, for example, natural drying, drying by warm air, hot air or low-humidity air, vacuum drying, or by irradiation by far-infrared rays, electron beams, etc., but is not limited thereto. The above drying process may be performed at a temperature of, for example, 25°C to 120°C.
[0060] The above composition for forming an adhesive layer may include a second ceramic, a binder, and a solvent. The solvent may be an aqueous solvent comprising water, alcohol, or a combination thereof. The alcohol may be methyl alcohol, ethyl alcohol, propyl alcohol, or a combination thereof.
[0061] Another embodiment provides a lithium secondary battery comprising a cathode, a positive electrode, a separator located between the cathode and the positive electrode, and an electrolyte.
[0062] The above separator is a separator according to one embodiment.
[0063] The above-mentioned cathode comprises a current collector and a cathode active material layer formed on the current collector and including the cathode active material.
[0064] The above negative electrode active material may be a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0065] Examples of materials capable of reversibly intercalating / deintercalating the above lithium ions include carbon materials, namely carbon-based negative electrode active materials commonly used in lithium secondary batteries. Representative examples of carbon-based negative electrode active materials include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the above amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0066] As the above lithium metal alloy, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.
[0067] Materials capable of doping and dedoping the above lithium include Si and SiO xExamples include (0 < x < 2), Si-Q alloy (where Q is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Si-carbon composite, Sn, SnO2, Sn-R alloy (where R is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), Sn-carbon composite, etc., and at least one of these may also be mixed with SiO2. The above elements Q and R may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0068] Lithium titanium oxide can be used as the above transition metal oxide.
[0069] A negative electrode active material according to one embodiment may include a Si-C composite comprising a Si-based active material and a carbon-based active material.
[0070] The above Si-based active material is Si, SiO x (0 < x < 2), Si-Q alloy (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si) or a combination thereof.
[0071] The average particle size of the above Si-based active material may be 50 nm to 200 nm.
[0072] When the average particle size of the above Si-based active material falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.
[0073] The above Si-based active material may be included in an amount of 1% to 60% by weight based on the total weight of the Si-C composite, for example, 3 It may be included in an amount of 60% by weight.
[0074] A negative electrode active material according to another embodiment may further include crystalline carbon together with the aforementioned Si-C composite.
[0075] When the above-mentioned cathode active material includes a Si-C composite and crystalline carbon together, the Si-C composite and crystalline carbon may be included in the form of a mixture, in which case the Si-C composite and crystalline carbon may be included in a weight ratio of 1:99 to 50:50. More specifically, the Si-C composite and crystalline carbon may be included in a weight ratio of 5:95 to 20:80.
[0076] The above crystalline carbon may include, for example, graphite, and more specifically, may include natural graphite, artificial graphite, or a mixture thereof.
[0077] The average particle size of the crystalline carbon above may be 5 μm to 30 μm.
[0078] In this specification, the average particle size may be the particle size (D50) at 50% by volume on a cumulative size-distribution curve. The average particle size (D50) may be measured by methods widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope (TEM) image or a scanning electron microscope (SEM) image. Alternatively, the average particle size (D50) value may be obtained by measuring using a dynamic light-scattering device, performing data analysis to count the number of particles for each particle size range, and then calculating from this.
[0079] The above Si-C composite may further include a shell surrounding the surface of the Si-C composite, and the shell may include amorphous carbon. The thickness of the shell may be 5 nm to 100 nm.
[0080] The above amorphous carbon may include soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a mixture thereof.
[0081] The above amorphous carbon may be included in an amount of 1 to 50 parts by weight, for example, 5 to 50 parts by weight, or 10 to 50 parts by weight, per 100 parts by weight of carbon-based active material.
[0082] delete
[0083] The above-mentioned negative electrode active material layer comprises a negative electrode active material and a binder, and may optionally further comprise a conductive material.
[0084] The content of the negative electrode active material in the above negative electrode active material layer may be 95% to 99% by weight based on the total weight of the negative electrode active material layer. The content of the binder in the above negative electrode active material layer may be 1% to 5% by weight based on the total weight of the negative electrode active material layer. Additionally, if a conductive material is further included, the negative electrode active material may be used in an amount of 90% to 98% by weight, the binder in an amount of 1% to 5% by weight, and the conductive material in an amount of 1% to 5% by weight.
[0085] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a water-insoluble binder, a water-soluble binder, or a combination thereof may be used.
[0086] Examples of the above-mentioned water-insoluble binders include ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0087] Examples of the above-mentioned water-soluble binders include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polymers containing ethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or combinations thereof.
[0088] When a water-soluble binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal. The content of such a thickener may be 0.1 to 3 parts by weight per 100 parts by weight of the cathode active material.
[0089] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, Denka black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.
[0090] The above current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0091] The above-mentioned anode comprises a current collector and an anode active material layer formed on the current collector and comprising an anode active material.
[0092] As the above-mentioned cathode active material, a compound capable of reversible intercalation and deintercalation of lithium (a rethated intercalation compound) may be used; specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. As a more specific example, a compound represented by any one of the following chemical formulas may be used. Lia A 1-b X b D2(0.90 ≤ a≤1.8, 0 ≤ b≤ 0.5); Li a A 1-b X b O 2-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a HAVE BEEN 1-b X b O 2-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a HAVE BEEN 2-b X b O 4-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b X c D α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 < α ≤2); Li a Ni 1-b-c Co b X c O 2-α T α (0.90 ≤ a≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 < α < 2); Li a Ni 1-b-c Co b X c O 2-α T2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤0.5, 0 ≤ c ≤ 0.5, 0 < α < 2); Li a Ni 1-b-c Mr b X c D α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 < α ≤2); Li a Ni 1-b-c Mr b X c O2-α T α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 < α < 2); The a Nor 1-b-c Mn b X c O 2-α T2(0.90 ≤ a≤ 1.8, 0 ≤ b ≤0.5, 0 ≤ c ≤0.5, 0 < α < 2); The a Nor b E c G d O2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); The a Nor b Co c Mn d G e O2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); The a NiG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1) Li a CoG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); The a Mn 1-b G b O2(0.90 ≤ a ≤1.8, 0.001 ≤ b ≤ 0.1); The a Mn2G b O4(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); The a Mn 1-g G g PO4(0.90 ≤ a ≤ 1.8, 0 ≤ g ≤ 0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; The (3-f) J2(PO4)3(0 ≤ f ≤2); The (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); The a FePO4(0.90 ≤ to ≤ 1.8)
[0093] In the above chemical formula, A is selected from the group consisting of Ni, Co, Mn, and combinations thereof; X is selected from the group consisting of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, and combinations thereof; D is selected from the group consisting of O, F, S, P, and combinations thereof; E is selected from the group consisting of Co, Mn, and combinations thereof; T is selected from the group consisting of F, S, P, and combinations thereof; G is selected from the group consisting of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, and combinations thereof; Q is selected from the group consisting of Ti, Mo, Mn, and combinations thereof; Z is selected from the group consisting of Cr, V, Fe, Sc, Y, and combinations thereof; and J is selected from the group consisting of V, Cr, Mn, Co, Ni, Cu, and combinations thereof.
[0094] Of course, a coating layer on the surface of this compound may be used, or a mixture of the compound and a compound having a coating layer may be used. This coating layer may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming these coating layers may be amorphous or crystalline. As coating elements included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the art, a detailed explanation will be omitted.
[0095] In the above anode, the content of the anode active material may be 90% to 98% by weight with respect to the total weight of the anode active material layer.
[0096] In one embodiment, the positive active material layer may further include a binder and a conductive material. In this case, the content of the binder and the conductive material may each be 1% to 5% by weight with respect to the total weight of the positive active material layer.
[0097] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0098] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.
[0099] As the current collector mentioned above, aluminum foil, nickel foil, or a combination thereof may be used, but is not limited thereto.
[0100] The above positive active material layer and negative active material layer are formed by preparing an active material composition by mixing an active material, a binder, and optionally a conductive material in a solvent, and applying the active material composition to a current collector. Since such a method for forming active material layers is widely known in the art, a detailed description thereof is omitted in this specification. The solvent may include N-methylpyrrolidone, but is not limited thereto. Additionally, when a water-based binder is used in the negative active material layer, water may be used as the solvent when preparing the negative active material composition.
[0101] The above electrolyte includes a non-aqueous organic solvent and a lithium salt.
[0102] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0103] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.
[0104] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, propylpropionate, decanolide, mevalonolactone, caprolactone, etc. The above ether-based solvents may include dibutyl ether, tetraglame, deglame, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, cyclohexanone, etc. may be used as the ketone-based solvent. In addition, ethyl alcohol, isopropyl alcohol, etc. may be used as the alcohol-based solvent, and as the aprotic solvent, nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc. may be used.
[0105] The above-mentioned non-aqueous organic solvents may be used alone or in a mixture of one or more. When using a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those skilled in the field.
[0106] In addition, for the above carbonate-based solvent, it is preferable to use a mixture of cyclic carbonates and chain carbonates. In this case, using a mixture of cyclic carbonates and chain carbonates in a volume ratio of 1:1 to 1:9 can result in excellent performance of the electrolyte.
[0107] When using the above-mentioned non-aqueous organic solvent in a mixture, a mixed solvent of cyclic carbonate and chain carbonate, a mixed solvent of cyclic carbonate and propionate-based solvent, or a mixed solvent of cyclic carbonate, chain carbonate, and propionate-based solvent may be used. As the propionate-based solvent, methylpropionate, ethylpropionate, propylpropionate, or a combination thereof may be used.
[0108] In this case, when using a mixture of cyclic carbonate and chain carbonate or cyclic carbonate and propionate-based solvent, using a volume ratio of 1:1 to 1:9 may result in superior performance of the electrolyte. Additionally, when using a mixture of cyclic carbonate, chain carbonate, and propionate-based solvent, a volume ratio of 1:1:1 to 3:3:4 may be used. Of course, the mixing ratio of the solvents may also be appropriately adjusted according to the desired physical properties.
[0109] The above-mentioned non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in the above-mentioned carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of 1:1 to 30:1.
[0110] As the above aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound of the following chemical formula 2 may be used.
[0111] [Chemical Formula 2]
[0112]
[0113] (In the above Chemical Formula 2, R1 to R6 are identical or different from each other and are selected from the group consisting of hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.)
[0114] Specific examples of the above aromatic hydrocarbon-based organic solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. It is selected from the group consisting of 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0115] The above electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound of the following chemical formula 3 as a life-enhancing additive to improve battery life.
[0116] [Chemical Formula 3]
[0117]
[0118] (In the above chemical formula 3, R7 and R8 are identical or different from each other and are selected from the group consisting of hydrogen, halogen groups, cyano groups (CN), nitro groups (NO2), and fluorinated alkyl groups having 1 to 5 carbon atoms, and said R7 and R8 At least one of the groups is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, provided that R7 and R8 are not both hydrogen.)
[0119] Representative examples of the above-mentioned ethylene carbonate-based compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. If more of these lifespan-enhancing additives are used, the amount used can be appropriately controlled.
[0120] The above electrolyte may further include vinylethylene carbonate, propane sulfone, succinonitrile, or a combination thereof, and the amount used can be appropriately adjusted.
[0121] The above lithium salt is a material that dissolves in an organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of a lithium secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, and LiN(C x F 2x+1 SO2)(C y F 2y+1The supporting electrolyte comprises one or more selected from the group consisting of SO2)(where x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxalato) phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato) borate (LiBOB), and lithium difluoro(oxalato) borate (LiDFOB). It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0122] FIG. 1 shows an exploded perspective view of a lithium secondary battery according to one embodiment of the present invention. Although the lithium secondary battery according to one embodiment is described as being prismatic, the present invention is not limited thereto and can be applied to various types of batteries such as cylindrical and pouch types.
[0123] Referring to FIG. 1, a lithium secondary battery (100) according to one embodiment may include an electrode assembly (40) wound with a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown).
[0124] Examples and comparative examples of the present invention are described below. However, the following examples are merely one example of the present invention, and the present invention is not limited to the following examples.
[0125] (Example 1)
[0126] 1. Separator manufacturing
[0127] 1) Formation of coating layer
[0128] A composition for forming a coating layer was prepared by mixing polyethylene wax with an average size (D50) of 1 μm (melting temperature of polyethylene wax: 110°C, weight-average molecular weight (Mw): 1500 g / mol), boehmite with an average size (D50) of 650 nm, and a methacrylate copolymer binder comprising a first structural unit derived from methacrylic acrylamide and a second structural unit of methacrylic acid in a weight ratio of 56.7 : 37.8 : 5.5 in a water solvent. That is, the mixing ratio of the polyethylene wax and the boehmite was 6 : 4 by weight.
[0129] The above-described composition for forming a coating layer was coated on both sides of a polyethylene single-film substrate with a thickness of 7 μm using a gravure coating method, and dried at 60°C to produce a coating layer with a cross-sectional coating thickness of 2 μm.
[0130] 2) Formation of adhesive layer
[0131] A composition for forming an adhesive layer was prepared by mixing Al2O3 with an average size (D50) of 250 nm, polyvinylidene fluoride (PVdF), and a binder of polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer (PVdF:PVdF-HFP = 5:5 weight ratio) in a 6:4 weight ratio in an N-methylpyrrolidone solvent.
[0132] The above adhesive layer forming composition was applied to the coating layer using a gravure coating method and dried at 70°C to form an adhesive layer with a cross-sectional thickness of 0.7 μm, thereby manufacturing a separator. The resulting separator had a five-layer structure consisting of a porous substrate, coating layers formed on both sides of the substrate, and adhesive layers formed on the coating layers.
[0133] (Examples 2 to 4 and Comparative Examples 1 to 12, Reference Examples 1 to 13)
[0134] A separator was prepared in the same manner as in Example 1, except that the weight ratio of polyethylene wax and boehmite and the average size of boehmite in the composition for forming the coating layer, and the weight ratio of Al2O3 and binder and the average size of Al2O3 and the weight ratio of PVdF:PVdF-HFP in the composition for forming the adhesive layer were changed as shown in Table 1 below.
[0135] coating layer adhesive layer PE Wax: Boehmite (by weight) Average boehmite size (D50, nm) Al2O3: Binder (weight ratio) Al2O3 average size (D50, nm) PVdF:PVdF-HFP (weight ratio) Example 1 6:4 650 6:4 250 5:5 Example 2 8:2 650 6:4 250 5:5 Example 3 6:4 650 5:5 250 5:5 Example 4 8:2 650 5:5 250 5:5 Comparative Example 1 6:4 250 6:4 250 5:5 Comparative Example 2 8:2 250 6:4 250 5:5 Comparative Example 3 6:4 250 5:5 250 5:5 Comparative Example 4 8:2 250 5:5 250 5:5 Comparative Example 5 6:4 650 8:2 250 5:5 Comparative Example 6 8:2 650 8:2 250 5:5 Comparative Example 7 6:4 650 8:2 200 5:5 Comparative Example 8 8:2 650 8:2 200 5:5 Comparative Example 9 6:4 650 8:2 250 4:6 Comparative Example 10 6:4 650 8:2 250 6:4 Comparative Example 11 5:5 650 6:4 250 5:5 Comparative Example 12 9:1 650 6:4 250 5:5 Reference Example 1 6:4 900 6:4 250 5:5 Reference Example 2 8:2 900 6:4 250 5:5 Reference Example 3 6:4 900 5:5 250 5:5 Reference Example 4 8:2 900 5:5 250 5:5 Reference Example 5 6:4 900 5:5 100 5:5 Reference Example 6 6:4 900 5:5 310 5:5 Reference Example 7 8:2 900 5:5 100 5:5 Reference Example 8 8:2 900 5:5 310 5:5 Reference Example 9 6:4 900 5:5 250 3:7 Reference Example 10 6:4 900 5:5 250 7:3 Reference Example 11 8:2 900 5:5 250 3:7 Reference Example 12 8:2 900 5:5 250 7:3 Reference Example 13 6:4 250 6:4 650 5:5
[0136] Experimental Example 1: Air permeability
[0137] During the manufacturing process of Examples 1 to 4, Comparative Examples 1 to 12, and Reference Examples 1 to 13, the air permeability of the porous substrate with the coating layer formed was measured, and the results were shown as the air permeability of the coating layer in Table 2 below. The air permeability test was conducted by measuring the time (in seconds) it takes for 100cc of air to pass through a separator using an air permeability meter (ASAHI-SEICO, TYPE EG01-55-1MR).
[0138] In addition, air permeability was measured in the same manner using separators prepared according to Examples 1 to 4, Comparative Examples 1 to 12, and Reference Examples 1 to 13. The results are shown in Table 2 below.
[0139] Experimental Example 2: Binding strength
[0140] During the manufacturing process of Examples 1 to 4, Comparative Examples 1 and 12, and Reference Examples 1 to 13, a porous substrate with a coating layer formed thereon was cut to a width of 12 mm and a length of 50 mm to produce a sample. A tape attached to a slide glass was applied to the adhesive layer surface of the sample, and the bonding strength was measured while peeling the tape and the adhesive layer using a 180° UTM tensile strength tester. At this time, the peeling speed was set to 10 mm / min, and measurements were taken three times to obtain the average value of the force required to peel 40 mm from the start of peeling. The results are shown in Table 2 below as coating layer results.
[0141] Experimental Example 3: Dry Adhesion and Wet Adhesion
[0142] A separator prepared according to Examples 1 to 4, Comparative Examples 1 to 12, and Reference Examples 1 to 12 was cut into 1 cm x 8 cm pieces to prepare two sheets, and two anodes of 3.4 cm x 8 cm were prepared. The prepared anodes, separators, separators, and anodes were laminated, and the laminated product was placed between pouches of 10 cm x 20 cm. Then, a first pressurization was applied for 40 seconds under conditions of a temperature of 75°C and a pressure of 6.84 kgf / ㎠, followed by a second pressurization for 15 seconds under conditions of a temperature of 75°C and a pressure of 11.4 kgf / ㎠, thereby preparing a sample. The above-mentioned anode was prepared by mixing 294 wt% LiCoO2, 3 wt% Ketjen black, and 3 wt% polyvinylidene fluoride in an N-methylpyrrolidone solvent to form an anode active material layer composition, and then applying, drying, and rolling this anode active material layer composition onto a copper current collector. In the lamination process, the adhesive layer of the separator was positioned so as to be in contact with the anode active material layer. .
[0143] Using the above sample, dry adhesive strength was measured in the same manner as the bonding strength test. The results are shown in Table 2 below.
[0144] Separators prepared according to Examples 1 to 4, Comparative Examples 1 to 12, and Reference Examples 1 to 13 were cut into 1 cm x 8 cm pieces to prepare two sheets, and two anodes of 3.4 cm x 8 cm were prepared. The prepared anodes, separators, separators, and anodes were stacked, and this stack was placed between pouches of 10 cm x 20 cm, after which 0.4 g of electrolyte was added to the pouches. Subsequently, a sample was prepared by pressurizing for 60 minutes under conditions of a temperature of 60°C and a pressure of 11.4 kgf / ㎠.
[0145] Wet adhesive strength was measured using the above sample in the same manner as the bonding strength test. The results are shown in Table 2 below.
[0146] coating layer separator Air per 100cc Binding strength (N) Dry adhesion (N) Wet adhesion (N) Air per 100cc Example 1 171 0.72 98 612 215 Example 2 183 0.55 96 600 220 Example 3 171 0.72 102 630 225 Example 4 183 0.55 98 605 236 Comparative Example 1 210 0.61 98 610 274 Comparative Example 2 220 0.59 96 605 288 Comparative Example 3 210 0.61 100 601 286 Comparative Example 4 220 0.59 103 604 290 Comparative Example 5 171 0.72 80 450 219 Comparative Example 6 183 0.55 54 380 224 Comparative Example 7 171 0.72 60 433 235 Comparative Example 8 183 0.55 52 377 240 Comparative Example 9 171 0.72 66 534 206 Comparative Example 10 171 0.72 88 420 204 Comparative Example 11 160 0.75 107 654 199 Comparative Example 12 - - - - - Reference Example 1 156 0.4 84 465 194 Reference Example 2 161 0.36 79 442 200 Reference Example 3 156 0.4 88 478 181 Reference Example 4 161 0.36 80 470 188 Reference Example 5 156 0.4 74 393 203 Reference Example 6 156 0.4 83 494 176 Reference Example 7 161 0.36 70 380 190 Reference Example 8 161 0.36 83 486 171 Reference Example 9 156 0.4 43 846 186 Reference Example 10 156 0.4 116 299 184 Reference Example 11 161 0.36 40 812 196 Reference Example 12 161 0.36 105 280 195 Reference Example 13 210 0.61 115 694 243
[0147] As shown in Table 2 above, in the case of Examples 1 to 4, where the coating layer contains polyethylene wax and boehmite in a weight ratio of 6:4 to 8:2 and the adhesive layer contains Al2O3 and a binder (PVdF and PVdF-HFP) in a weight ratio of 6:4 to 8:2, the average size of the boehmite is larger than the average size of Al2O3, and PVdF and PVdF-HFP are contained in a weight ratio of 6:4 to 4:6, it can be seen that the bonding strength of the coating layer is excellent, and both the dry adhesion and wet adhesion strength of the final separator are excellent. In addition, since Examples 1 to 4 exhibit an air permeability of 240 sec / 100 or less, it can be seen that the air permeability characteristics are excellent.
[0148] Comparative Examples 1 to 4, in which the adhesive layer contains Al2O3 and a binder (PVdF and PVdF-HFP) and uses boehmite and Al2O3 having the same average size, also showed excellent dry and wet adhesion. However, in the case of Comparative Examples 1 to 4, the air permeability exceeds 240 sec / 100cc, indicating that deteriorated air permeability characteristics were exhibited.
[0149] On the other hand, in the case of Comparative Examples 5 to 10, which included alumina and PVdF binder in an 8:2 weight ratio in the adhesive layer, there was a problem in that both dry and wet adhesive strengths did not satisfy the standards of 90N or more and 600N or more.
[0150] In addition, in the case of Comparative Example 11, in which the coating layer contained polyethylene wax and boehmite in a weight ratio of 5:5, the coating layer was not formed well because the polyethylene wax content was low.
[0151] In the case of Comparative Example 12, where the coating layer contained polyethylene wax and boehmite in a weight ratio of 9:1, the ceramic, i.e., boehmite content was too low to be coated, so physical property tests could not be performed.
[0152] In the case of Reference Examples 1 to 12, where the coating layer contains polyethylene wax and boehmite in a weight ratio of 6:4 to 8:2 and the adhesive layer contains Al2O3 and a binder (PVdF and PVdF-HFP) in a weight ratio of 6:4 to 8:2 and PVdF and PVdF-HFP in a weight ratio of 6:4 to 4:6, the average size of the boehmite is too large at 900 μm, and there was a problem that the bonding strength to the porous substrate was very low, and also that the criteria for dry adhesion strength or wet adhesion strength were not satisfied, or that one of them was not satisfied.
[0153] Even though the coating layer contains polyethylene wax and boehmite in a weight ratio of 6:4 to 8:2 and the adhesive layer contains Al2O3 and binder (PVdF and PVdF-HFP) in a weight ratio of 6:4 to 8:2 and PVdF and PVdF-HFP in a weight ratio of 6:4 to 4:6, in the case of Reference Example 13, where the average size of the boehmite is smaller than the average size of the Al2O3, the air permeability was found to be too high at 243 sec / 100cc and was not suitable.
[0154] As shown in Table 2 above, in the case of Comparative Examples 5 to 10 and Reference Examples 1 to 9 and 11, the dry adhesive strength was less than 90 N or the wet adhesive strength was less than 600 N, so they could not be used for battery manufacturing, and therefore no further experiments were conducted. In addition, in the case of Reference Example 13, the air permeability was found to be too high, so no further experiments were conducted.
[0155] Experimental Example 4) Dose Retention Rate
[0156] A lithium secondary battery was manufactured by a conventional method using a separator, a cathode, a positive electrode, and an electrolyte prepared according to Examples 1 to 4, Comparative Examples 1 to 4, Comparative Example 11, and Reference Examples 10 and 12.
[0157] The above-mentioned cathode was prepared by mixing 94 wt% artificial graphite, 3 wt% Ketjen black, and 3 wt% polyvinylidene fluoride in an N-methylpyrrolidone solvent to form a cathode active material layer composition, and then applying, drying, and rolling the cathode active material layer composition onto a copper current collector.
[0158] The above anode was prepared by mixing 94 wt% LiCoO2, 3 wt% Ketjen black, and 3 wt% polyvinylidene fluoride in an N-methylpyrrolidone solvent to form an anode active material layer composition, and then applying, drying, and rolling the anode active material layer composition onto a copper current collector.
[0159] As the above electrolyte, a mixed solvent of ethylene carbonate, ethylmethyl carbonate, and dimethyl carbonate (2:1:7 volume ratio) in which 1.5M LiPF6 was dissolved was used.
[0160] The manufactured battery was subjected to 100 charge-discharge cycles at 1.3C at 23℃, and the ratio of the 100-cycle charge capacity to the 1-cycle charge capacity was calculated. The results are shown as the capacity retention rate (%) in Table 3 below.
[0161] Capacity retention rate (%) Example 1 95 Example 2 95 Example 3 92 Example 4 89 Comparative Example 1 75 Comparative Example 2 69 Comparative Example 3 70 Comparative Example 4 65 Comparative Example 11 82 Reference Example 10 54 Reference Example 12 50
[0162] As shown in Table 3 above, it can be seen that the capacity retention rates of Examples 1 to 4 are superior to those of Comparative Examples 1 to 4, Comparative Example 11, and Reference Examples 10 and 12.
[0163] From the above results, it can be seen that Comparative Examples 1 to 4, in which the adhesive layer contains Al2O3 and a binder (PVdF and PVdF-HFP) and uses boehmite and Al2O3 having the same average size, have excellent dry adhesion and wet adhesion, but are not suitable because the capacity retention rate deteriorates.
[0164] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
Claims
Claim 1 A separator for a lithium secondary battery comprising: a porous substrate; a coating layer located on at least one surface of the porous substrate and comprising polyethylene particles and a first ceramic in a weight ratio of 6:4 to 8:2; and an adhesive layer located on one surface of the coating layer and comprising a second ceramic and a binder in a weight ratio of 7:3 to 5:5, wherein the binder comprises polyvinylidene fluoride and a polyvinylidene-hexapropylene copolymer in a weight ratio of 6:4 to 4:6, and the average size of the first ceramic is larger than the average size of the second ceramic. Claim 2 A separator for a lithium secondary battery according to claim 1, wherein the mixing ratio of the second ceramic and the binder is 6:4 to 5:5 by weight. Claim 3 delete Claim 4 A separator for a lithium secondary battery according to claim 1, wherein the average size of the first ceramic is 550 nm to 750 nm. Claim 5 A separator for a lithium secondary battery according to claim 1, wherein the cross-sectional thickness of the coating layer is 0.5㎛ to 5㎛. Claim 6 A separator for a lithium secondary battery according to claim 1, wherein the cross-sectional thickness of the adhesive layer is 0.1 μm to 4.0 μm. Claim 7 A separator for a lithium secondary battery according to claim 1, wherein the size ratio of the first ceramic and the second ceramic is 5:1 to 1.5:
1. Claim 8 In claim 1, the first ceramic or the second ceramic is identical or different from each other, and is Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, A separator for a lithium secondary battery, which is SrTiO3, BaTiO3, Mg(OH)2, boehmite, or a combination thereof. Claim 9 A separator for a lithium secondary battery according to claim 1, wherein the first ceramic is boehmite and the second ceramic is Al2O3. Claim 10 A separator for a lithium secondary battery according to claim 1, wherein the coating layer further comprises a vinyl group-containing binder. Claim 11 A separator for a lithium secondary battery according to claim 10, wherein the vinyl group-containing binder comprises a (meth)acrylic copolymer comprising at least one of a first structural unit derived from (meth)acrylamide, a second structural unit derived from (meth)acrylic acid, (meth)acrylate, (meth)acrylonitrile, or a combination thereof, and a structural unit derived from (meth)acrylamidosulfonic acid, (meth)acrylamidosulfonic acid salt, or a combination thereof. Claim 12 A separator for a lithium secondary battery according to claim 1, wherein the average size of the polyethylene particles is 0.1㎛ to 3.0㎛. Claim 13 A separator for a lithium secondary battery according to claim 1, wherein the weight-average molecular weight (Mw) of the polyethylene is 1000 g / mol to 5000 g / mol. Claim 14 A lithium secondary battery comprising: a cathode comprising a cathode active material; a positive electrode comprising a positive electrode active material; a separator of any one of claims 1, 2 and 4 to 13 located between the cathode and the positive electrode; and a non-aqueous electrolyte.
Citation Information
Patent Citations
A method for manufacturing porous separators for use of secondary cell using nano steam, separators made by the method, and secondary cell
KR1020150001963A
A separator for an electrochemical device comprising a multi-layered porous coating layer and a method for manufacturing the same
KR1020200078416A
Separator for rechargeable lithium battery and rechargeable lithium battery including the same
KR1020200140637A