Negative electrode and rechargeable lithium battery including same

A carbon-based or silicon-based core with a SiO y shell and Li surface layer in the negative electrode active material addresses the challenge of high energy density and fast charging in lithium-ion batteries, enhancing conductivity and cycle life.

KR103047648B1Active Publication Date: 2026-11-11SAMSUNG SDI CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230112990
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-28
Publication Date
2026-11-11
Estimated Expiration
2043-08-28

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in achieving high energy density and fast charging speeds while maintaining excellent cycle life characteristics.

Method used

A negative electrode active material comprising a carbon-based or silicon-based core with a SiO y shell (1≤x≤3, 1≤y≤6) and a surface layer of Li, combined with a cathode, positive electrode, and electrolyte, enhances lithium ion conductivity and charge/discharge efficiency.

Benefits of technology

The solution improves energy density, high-rate charging capabilities, and cycle life characteristics by balancing capacity and conductivity, with the SiO y shell contributing to improved electrical conductivity and reduced irreversible phase reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023094756808-PAT00003_ABST
    Figure 112023094756808-PAT00003_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material and a lithium secondary battery including the same, wherein the negative electrode active material comprises a core comprising at least one of a carbon-based material or a silicon-based material or a combination thereof, and a shell comprising LixSiOy (1≤x≤3, 1≤y≤6) and Si located on the surface of the core.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The invention relates to a negative electrode active material and a lithium secondary battery containing the same. Background Technology

[0002] As the demand for electric vehicles increases, the demand for secondary batteries is also rising rapidly. In particular, there is a growing demand for high energy density and fast charging speeds.

[0003] Lithium-ion batteries are primarily used as such secondary batteries. A lithium-ion battery is a battery comprising a positive electrode, a negative electrode, and an electrolyte, and crystalline carbon, such as graphite, is used as the negative electrode active material. The problem to be solved

[0004] One embodiment provides a negative electrode active material exhibiting excellent cycle life characteristics and rapid charging performance.

[0005] Another embodiment provides a lithium secondary battery comprising the above-mentioned negative electrode active material. means of solving the problem

[0006] One embodiment comprises a core including a carbon-based material or a silicon-based material, or a combination thereof; and Li located on the surface of the core. x SiO y A negative electrode active material comprising a shell containing (1≤x≤3, 1≤y≤6) and Si is provided.

[0007] According to another embodiment, a lithium secondary battery is provided comprising a cathode including the cathode active material; a positive electrode; and an electrolyte. Effects of the invention

[0008] The cathode active material according to one embodiment can exhibit excellent rate characteristics and efficiency. Brief explanation of the drawing

[0009] FIG. 1 is a schematic diagram showing a lithium secondary battery according to one embodiment. Specific details for implementing the invention

[0010] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0011] The terms used herein are for describing exemplary embodiments only and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.

[0012] "Combinations of these" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.

[0013] Terms such as "include," "equip," or "have" are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0014] Throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0015] In the drawings, thicknesses have been enlarged to clearly represent various layers and regions, and the same reference numerals have been used for similar parts throughout the specification. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between.

[0016] In addition, the term "layer" here includes not only the shape formed on the entire surface when viewed in a plan view, but also the shape formed on some surfaces.

[0017] Here, "or" is not interpreted in an exclusive sense; for example, "A or B" is interpreted to include A, B, A+B, etc.

[0018] "Thickness" may be measured, for example, through photographs taken with an optical microscope such as a scanning electron microscope.

[0019] Unless otherwise defined in this specification, the particle size or size may be the average particle size. This average particle size refers to the average particle size (D50) which means the diameter of the particle whose cumulative volume in the particle size distribution is 50 volume%. If the particle is spherical, the diameter may be the particle diameter or the average particle size, and if the particle is not spherical, the diameter may be the major axis length or the average major axis length. The average particle size (D50) may be measured by methods widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope (TEM), a scanning electron microscope (SEM), or a field emission scanning electron microscope (FE-SEM). Alternatively, the average particle size (D50) can be obtained by measuring using a measuring device utilizing dynamic light scattering, performing data analysis to count the number of particles for each particle size range, and then calculating from this. When measuring by laser diffraction, more specifically, the particles to be measured are dispersed in a dispersion medium, then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasound of approximately 28 kHz is irradiated at an output of 60 W, after which the average particle size (D50) at the 50% reference of the particle size distribution in the measuring device can be calculated.

[0020] A negative electrode active material according to one embodiment comprises a core comprising any one of a carbon-based material, a silicon-based material, or a combination thereof; and Li located on the surface of the core. x SiO y It includes a shell containing (1≤x≤3, 1≤y≤6) and Si.

[0021] The negative electrode active material according to one embodiment is Li x SiO y By including a shell containing Si and a silicate compound represented by (1≤x≤3, 1≤y≤6), charge / discharge efficiency can be improved, and lithium ion conductivity can also be improved. In addition, improved energy density and high-rate charging characteristics can be exhibited. When the silicate compound is included in the core, that is, when it is included in the core as well as the shell and distributed throughout the negative electrode active material, electrical conductivity may decrease and cycle life may be reduced.

[0022] The above silicate compound may be Li2SiO3, Li2Si2O5, or a combination thereof.

[0023] According to one embodiment, the shell is SiO z (0 <z≤2)를 더욱 포함할 수도 있다. 상기 쉘이 SiO z (0 <z≤2)를 더욱 포함하는 경우, 에너지 밀도가 증가할 수 있다.

[0024] In one embodiment, the shell may be located in an island-like structure discontinuously on the core surface or in a layer-like structure continuously. That is, a portion of the core surface may not be covered by the shell and may be partially exposed, or the core surface may be entirely covered by the shell and not exposed. In one embodiment, when the shell is in an island-like structure, it exhibits superior cell conductivity, thereby exhibiting superior rate characteristics and efficiency characteristics.

[0025] In one embodiment, the Li x SiO y The weight ratio of (wherein, 1≤x≤3, 1≤y≤6) and Si may be 1:99 to 77:23, 1:99 to 75:25, or 1:99 to 80:20. The above Li x SiO y(Here, 1≤x≤3, 1≤y≤6) and when the weight ratio of Si falls within the above range, there may be an advantage in that high capacity and cycle characteristics can be appropriately balanced.

[0026] In addition, the above Li x SiO y The content of (wherein, 1≤x≤3, 1≤y≤6) may be 0.1 wt% to 15 wt% with respect to 100 wt% of the total cathode active material, 0.1 wt% to 10 wt%, or 0.1 wt% to 5 wt%. The above Li x SiO y When the content of (where 1≤x≤3, 1≤y≤6) is included in the above range, there may be advantages such as high initial efficiency and improved cycle characteristics.

[0027] The thickness of the shell may be 100 nm to 500 nm, 100 nm to 450 nm, or 100 nm to 400 nm. When the thickness of the shell falls within the above range, energy density and high-rate charging capability can be sufficiently improved without reducing electrical conductivity.

[0028] In one embodiment, the shell may be porous. When the shell is porous, there is no irreversible phase that does not react with lithium, and thus, the shell may exhibit advantages in terms of energy density compared to when it is a dense layer.

[0029] In a negative electrode active material according to one embodiment, the core may be a carbon-based material or a silicon-based material, or a combination of the carbon-based material and the silicon-based material. Of course, it may be at least one of these. The carbon-based material may be crystalline carbon. The crystalline carbon may be amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite.

[0030] The silicon-based material may be a Si-C composite. The Si-C composite may comprise silicon particles and a form in which amorphous carbon is coated on the surface of the silicon particles, i.e., silicon particles and an amorphous carbon coating layer coated on the surface of the silicon particles. For example, the silicon-carbon composite may comprise secondary particles assembled from primary silicon particles and an amorphous carbon coating layer located on the surface of the secondary particles. Amorphous carbon may also be located between the primary silicon particles, so that, for example, the primary silicon particles may be coated with amorphous carbon. Additionally, the Si-C composite may comprise a core in which silicon particles are dispersed within an amorphous carbon matrix and an amorphous carbon coating layer coating the surface of the core.

[0031] Since the above secondary particle is located at the center of the Si-C composite, it can be called the core or the center. In addition, the above amorphous carbon coating layer can be called the outer part or the shell.

[0032] The silicon particles or the primary silicon particles may be nano silicon particles. The particle size of the nano silicon particles may be 10 nm to 1,000 nm, and according to another embodiment, 20 nm to 900 nm, 20 nm to 800 nm, 20 nm to 500 nm, 20 nm to 300 nm, or 20 nm to 150 nm. When the average particle size of the silicon particles falls within the above range, excessive volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.

[0033] At this time, the mixing ratio of the silicon particles and amorphous carbon may be 1:99 to 60:40 by weight.

[0034] In one embodiment, the secondary particle or the core may further comprise crystalline carbon. When the silicon-carbon composite further comprises crystalline carbon, the Si-C composite may comprise a silicon primary particle, a secondary particle assembled from crystalline carbon, and an amorphous carbon coating layer formed on the surface of the secondary particle. Additionally, the surface of the silicon primary particle may also be coated with amorphous carbon.

[0035] In addition, when Si-C comprises silicon particles, crystalline carbon, and amorphous carbon, the content of the amorphous carbon may be 30% to 70% by weight with respect to 100% by weight of the total Si-C composite, and the content of the crystalline carbon may be 1% to 20% by weight with respect to 100% by weight of the total Si-C composite. In addition, the content of silicon particles may be 20% to 70% by weight with respect to 100% by weight of the total Si-C composite, and according to one embodiment, may be 30% to 60% by weight.

[0036] The particle size of the above Si-C composite can be appropriately controlled and does not need to be specifically limited.

[0037] When the amorphous carbon is positioned to surround the secondary surface, its thickness can be appropriately controlled, but for example, it may exist with a thickness of 5 nm to 100 nm.

[0038] The above amorphous carbon may be pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a combination thereof. The above crystalline carbon may be amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite.

[0039] In one embodiment, the negative electrode active material may further include an amorphous carbon coating layer located on the shell. When an amorphous carbon coating layer is further included on the shell, electrical conductivity may be further increased. In this case, the thickness of the amorphous carbon coating layer may be 0.1 nm to 50 nm, 0.5 nm to 10 nm, or 1 nm to 5 nm.

[0040] The negative electrode active material according to one embodiment may have a pH of 7 or less, 3 to 7, or 5 to 6. That is, the negative electrode active material according to one embodiment exhibits acidity, and compared to a basic negative electrode active material with a pH exceeding 7, the adhesion strength with the binder during electrode manufacturing may be superior.

[0041] The cathode active material according to this embodiment can be manufactured by the following process.

[0042] After adding a carbon-based material to an acidic solvent, a hydrogen silsesquioxane precursor is added to the resulting mixture.

[0043] The acidic solvent may be hydrochloric acid, sulfuric acid, acetic acid, or a combination thereof. Additionally, the solvent may be an aqueous solution with a concentration of 0.05 M to 0.5 M.

[0044] The amount of the carbon-based material added may be 0.1g to 10g, 0.2g to 10g, or 0.5g to 5g per 10ml of the solvent.

[0045] In addition, after adding the carbon-based material to the acidic solvent, a process of stirring at a speed of 200 rpm to 1000 rpm, 300 rpm to 1000 rpm, or 500 rpm to 1000 rpm for 10 minutes to 1 hour, or 20 minutes to 40 minutes, can be carried out.

[0046] In addition, the process of adding the hydrogen silsesquioxane precursor can be carried out while stirring at a speed of 200 rpm to 1000 rpm, 300 rpm to 1000 rpm, or 500 rpm to 1000 rpm.

[0047] The hydrogen silsesquioxane precursor may be triethoxysilane, trimethoxysilane, nyl trimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, or a combination thereof.

[0048] At this time, the amount of hydrogen silsesquioxane precursor added can be adjusted so that the weight ratio of shell to core in the first heat treatment product is 1:100 to 30:100, 5:100 to 25:100, or 10:100 to 20:100.

[0049] According to the above mixing process, a sol-gel reaction occurs, and a product can be prepared in which a hydrogen silsesquiloxane precursor is coated on the surface of a carbon-based material.

[0050] Next, the obtained product is subjected to a first heat treatment. The first heat treatment process can be carried out by increasing the temperature from 800°C to 1500°C or from 900°C to 1300°C at a heating rate of 1°C / min to 20°C / min or 2°C / min to 15°C, and then maintaining the temperature at this level for 0.5 hours to 5 hours or 0.5 hours to 3 hours. The first heat treatment process can be carried out under an inert atmosphere, and the inert atmosphere may be argon, nitrogen, hydrogen, or a mixture thereof.

[0051] According to the primary heat treatment process, the hydrogen silsesquioxane precursor is decomposed to generate silicon, thereby producing a product comprising a carbon-based material core and a silicon shell located on the surface of the core. Additionally, by controlling the heat treatment temperature in this process, SiO₂ along with silicon z (0 <z≤ 2)을 포함하는 쉘이 생성될 수도 있다.

[0052] The primary heat treatment product and the lithium raw material are mixed. The lithium raw material may be LiH, LiOH, Li2CO3, Li2O, LiCl, or a combination thereof. The mixing ratio of the primary heat treatment product and the lithium raw material can be adjusted so that the Li / Si molar ratio is 1.5 / 1 to 2.0 / 1 or 1.75 / 1 to 2.0 / 1.

[0053] The above mixing process can be carried out using a ball mill, and zirconia balls may be used with the ball mill, but are not limited thereto.

[0054] Before mixing with the above lithium raw material, a process of forming an amorphous carbon coating layer on the primary heat treatment product may be further carried out.

[0055] The above coating layer formation process can be carried out by mixing a primary heat treatment product and an amorphous carbon precursor and heat treating. The amorphous carbon precursor may be petroleum coke, coal coke, petroleum pitch, coal pitch, pitch carbon, green coke, or a combination thereof.

[0056] The mixing ratio of the above primary heat treatment product and the above amorphous carbon precursor may be a weight ratio of 7:3 to 9.5:0.5.

[0057] The above mixing process may be carried out in a solvent, and the solvent may be tetrahydrofuran, methanol, ethanol, propanol, water, or a combination thereof. In addition, the mixing process may be carried out at 40°C to 80°C or 50°C to 70°C at a speed of 100 rpm to 200 rpm or 110 rpm to 150 rpm so that the solvent is substantially removed.

[0058] After mixing with the above amorphous carbon precursor, heat treatment can be carried out by increasing the temperature to 500°C to 1000°C or 600°C to 900°C at a heating rate of 1°C / min to 10°C / min or 2°C / min to 8°C / min, and then maintaining the temperature for 1 hour to 8 hours or 1 hour to 5 hours.

[0059] The obtained product is subjected to a second heat treatment.

[0060] The above secondary heat treatment process can be carried out by increasing the temperature to 500°C to 1000°C or 600°C to 900°C at a heating rate of 1°C / min to 20°C / min or 2°C / min to 15°C, and then maintaining the temperature at this temperature for 1 hour to 10 hours or 2 hours to 8 hours. The above secondary heat treatment process can be carried out under an inert atmosphere, and the inert atmosphere may be argon, nitrogen, hydrogen, or a mixture thereof.

[0061] In the above secondary heat treatment process, lithium ions generated from the lithium raw material may react with some of the silicon in the silicon shell to form lithium silicates such as Li2SiO3, Li2Si2O5, and Li4SiO4. Additionally, the unreacted remaining silicon may be located on the core, and SiO z (0 <z≤2)이 잔존할 수도 있다.

[0062] In addition, if the process of forming an amorphous carbon coating layer is further carried out, some of the lithium ions generated from the lithium raw material may react with the amorphous carbon to form lithium carbonate (Li2CO3).

[0063] The obtained heat-treated product is cleaned and dried to produce a cathode active material. The cleaning process can be carried out using water or a weakly acidic solvent, and can be carried out using a weakly acidic solvent. The weakly acidic solvent may be phosphoric acid (H3PO4), acetic acid, or a combination thereof.

[0064] By performing a cleaning process, lithium carbonate and Li4SiO4 can be removed. Accordingly, the final negative electrode active material comprises a core containing a carbon-based material and silicate and Si located on the surface of the core.

[0065] Another embodiment provides a lithium secondary battery comprising a negative electrode, a positive electrode, and an electrolyte.

[0066] The above cathode may include a current collector and a cathode active material layer formed on the current collector and comprising the cathode active material according to one embodiment.

[0067] In the above-mentioned negative electrode active material layer, the content of the negative electrode active material may be 95% to 98% by weight with respect to 100% by weight of the entire negative electrode active material layer.

[0068] The above negative electrode active material layer may include a binder and may further include a conductive material. The content of the binder may be 1% to 5% by weight with respect to 100% by weight of the entire negative electrode active material layer. The content of the conductive material may be 1% to 5% by weight with respect to 100% by weight of the entire negative electrode active material layer.

[0069] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a non-aqueous binder, an aqueous binder, or a combination thereof may be used.

[0070] Examples of the above-mentioned non-aqueous binders include ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0071] The above-mentioned water-based binder may be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.

[0072] The above-mentioned cathode binder may include a cellulose-based compound, and the cellulose-based compound may be included together with the above-mentioned aqueous binder. As the above-mentioned cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be used in a mixture. As the above-mentioned alkali metal, Na, K, or Li may be used. The above-mentioned cellulose-based compound may serve as a binder and may also serve as a thickener that imparts viscosity. Accordingly, the content of the cellulose-based compound can be appropriately controlled within the binder content and does not need to be limited, but for example, it may be 0.1 to 3 parts by weight per 100 parts by weight of the cathode active material.

[0073] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.

[0074] As the above current collector, a material selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof may be used.

[0075] The above anode includes a current collector and an anode active material layer formed on the current collector.

[0076] As the above-mentioned cathode active material, a compound capable of reversible intercalation and deintercalation of lithium (a rethated intercalation compound) may be used. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. As a more specific example, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b X b D 1 2(0.90 ≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 1-b X b O 2-c1 D 1 c1(0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a HAVE BEEN 2-b X b O 4-c1 D 1 c1 (0.90≤a ≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a Ni 1-b-c Co b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li aNi b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1) Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8)

[0077] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; and D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; T is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; Z is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof; L 1 is Mn, Al, or a combination thereof.

[0078] Of course, it is possible to use a compound having a coating layer on its surface, or to use a mixture of the compound and a compound having a coating layer. This coating layer may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming these coating layers may be amorphous or crystalline. As coating elements included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the art, a detailed explanation will be omitted.

[0079] In the above anode, the content of the anode active material may be 90% to 98% by weight with respect to the total weight of the anode active material layer.

[0080] In one embodiment, the positive active material layer may further include a binder and a conductive material. In this case, the content of the binder and the conductive material may each be 1% to 5% by weight with respect to the total weight of the positive active material layer.

[0081] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples of binders include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.

[0082] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.

[0083] Al may be used as the current collector mentioned above, but is not limited thereto.

[0084] The above electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0085] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0086] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.

[0087] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, decanolide, mevalonolactone, caprolactone, etc. The above ether-based solvents may include dibutyl ether, tetraglame, deglame, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, cyclohexanone, etc. may be used as the ketone-based solvent. In addition, ethyl alcohol, isopropyl alcohol, etc. may be used as the alcohol-based solvent, and as the aprotic solvent, nitriles such as R-CN (where R is a hydrocarbon group with a straight, branched, or ring structure having 2 to 20 carbon atoms and may include a double bond, a ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc. may be used.

[0088] The above organic solvents may be used alone or in a mixture of one or more. When used in a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those engaged in the relevant field.

[0089] In addition, for the above carbonate-based solvent, it is preferable to use a mixture of cyclic carbonates and chain carbonates. In this case, using a mixture of cyclic carbonates and chain carbonates in a volume ratio of 1:1 to 1:9 can result in excellent performance of the electrolyte.

[0090] The above organic solvent may further include an aromatic hydrocarbon organic solvent in the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0091] As the above aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound of the following chemical formula 1 may be used.

[0092] [Chemical Formula 1]

[0093]

[0094] (In the above Chemical Formula 1, R1 to R6 are identical or different from each other and are selected from the group consisting of hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.)

[0095] Specific examples of the above aromatic hydrocarbon-based organic solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. It is selected from the group consisting of 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.

[0096] The above electrolyte may further include vinyl ethyl carbonate, vinylene carbonate, or an ethylene carbonate-based compound of the following chemical formula 2 as a life-enhancing additive to improve battery life.

[0097] [Chemical Formula 2]

[0098]

[0099] (In the above chemical formula 2, R7 and R8 are identical or different from each other and are selected from the group consisting of hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, and at least one of R7 and R8 is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, provided that R7 and R8 are not both hydrogen.)

[0100] Representative examples of the above-mentioned ethylene carbonate-based compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. When using more of these lifespan-enhancing additives, the amount used can be appropriately controlled.

[0101] The above lithium salt is a material that dissolves in an organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of a lithium secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, and LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(where x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxolato) phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato) borate (LiBOB) and lithium difluoro(oxalato) borate (LiDFOB)), and one or more selected from the group consisting of these are included as supporting electrolytes. It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0102] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof may be used, and of course, mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators may be used.

[0103] FIG. 1 shows an exploded perspective view of a lithium secondary battery according to one embodiment of the present invention. Although the lithium secondary battery according to one embodiment is described as being prismatic, the present invention is not limited thereto and can be applied to various types of batteries such as cylindrical and pouch types.

[0104] Referring to FIG. 1, a lithium secondary battery (100) according to one embodiment may include an electrode assembly (40) wound with a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown).

[0105] Examples and comparative examples of the present invention are described below. However, the following examples are merely one example of the present invention, and the present invention is not limited to the following examples.

[0106] (Example 1)

[0107] <Manufacture of Cathode Active Material>

[0108] Step 1)

[0109] 5g of artificial graphite powder was added to 50mL of a 0.1 M aqueous HCl solution and stirred at 700 rpm for 30 minutes to prepare a dispersion. Subsequently, while continuously stirring the dispersion at 700 rpm, triethoxysilane (TES) was added to the dispersion and reacted for 30 minutes.

[0110] The amount of triethoxysilane added was such that the weight ratio of shell to core in the first heat treatment product was 20 / 100 wt%. Subsequently, the obtained product was filtered through a filter to remove the acid solvent, and dried in a convection oven (horizontal oven) at a temperature of 80°C for one day.

[0111] A first heat treatment was performed by using a horizontal furnace to heat the dried powder to 1000°C at a heating rate of 10°C / min under a mixed atmosphere of argon and hydrogen (96 vol% argon and 4 vol% hydrogen) and then maintaining it at 1000°C for 1 hour.

[0112] Subsequently, the powder obtained from the first heat treatment is recovered and ground to obtain a graphite core and silicon and SiO z (0 <z≤2)를 포함하는 쉘을 갖는 생성물을 제조하였다.

[0113] Step 2)

[0114] The above product was mixed with pitch carbon in tetrahydrofuran (THF) in a weight ratio of 9:1, and then stirred at 60°C at a speed of 120 rpm until the solvent was dried.

[0115] After grinding the obtained mixture, the temperature was raised to 800°C at a heating rate of 5°C / min under an argon gas atmosphere, and then heat-treated by maintaining at 800°C for 2 hours to produce a product having an amorphous carbon coating layer.

[0116] Step 3)

[0117] The above product was mixed with LiH powder, and zirconia balls (10 times the amount of the mixed powder) were added to the mixture, followed by shaking and mixing for 30 minutes. At this time, 0.116 g of LiH was used so that the Li / Si molar ratio was 2.0. The obtained mixture was classified using a 500 µm sieve. The classified product was subjected to a secondary heat treatment under an argon atmosphere, heated to 750°C at a heating rate of 10°C / min and held at 750°C for 6 hours, and then ground to obtain a graphite core and silicon oxide (SiO₂). x A shell-structured product containing silicon (Si), lithium silicate (Li2SiO3, Li2Si2O5, Li4SiO4, etc.) was prepared.

[0118] Step 4)

[0119] 1 g of the prepared product was added to 100 mL of distilled water, stirred for 30 minutes, and then filtered using a filter to perform a washing process. Subsequently, the obtained powder was dried in a vacuum oven for one day to remove the Li4SiO4 and Li2CO3 phases, resulting in a graphite core and the Li2SiO3, Li2Si2O5, Si, and SiO located on this graphite core. z (0 <z≤2)를 포함하는 다공성 쉘 및 이 다공성 쉘 상에 위치하는 비정질 탄소층을 포함하는 음극 활물질을 제조하였다.

[0120] In addition, in the manufactured cathode active material, the weight ratio of Li2SiO3 and Li2Si2O5 to Si was 1:99, and the content of Li2SiO3 and Li2Si2O5 was 0.2 wt% with respect to 100 wt% of the total cathode active material. In the manufactured cathode active material, the thickness of the shell was 100 nm to 400 nm, and the thickness of the amorphous carbon layer was 1 nm.

[0121] <Manufacturing of the Cathode>

[0122] A cathode active material layer slurry was prepared by mixing 90 wt% of the manufactured cathode active material, 5 wt% of carboxymethyl cellulose, and 5 wt% of styrene butadiene rubber in a water solvent.

[0123] A cathode was manufactured by coating the above-mentioned cathode active material layer slurry onto a Cu foil current collector, vacuum drying and rolling at 120°C for 2 hours to form a cathode active material layer with a thickness of 30 μm.

[0124] A CR2032 coin battery was manufactured by placing a polyethylene separator between the above-mentioned negative electrode and the lithium metal counter electrode, and then injecting an electrolyte. As the electrolyte, a mixture of ethylene carbonate and ethyl methyl carbonate in which 1M LiPF6 is dissolved was used, comprising 100% by weight of the mixture of ethylene carbonate and ethyl methyl carbonate (mixing ratio of ethylene carbonate to ethyl methyl carbonate = 3:7 by volume) with 2% by weight of fluoroethylene carbonate added.

[0125] (Example 2)

[0126] A negative electrode active material was prepared in the same manner as in Example 1 above, except that in the process of mixing the product and LiH powder, 0.102 g of LiH was used so that the Li / Si molar ratio was 1.75. In the prepared negative electrode active material, the weight ratio of Li2SiO3 and Li2Si2O5 to Si was 2:98, and the content of Li2SiO3 and Li2Si2O5 was 0.4 wt% relative to 100 wt% of the total negative electrode active material. In the prepared negative electrode active material, the thickness of the shell was 100 nm to 400 nm, and the thickness of the amorphous carbon layer was 1 nm.

[0127] A negative electrode and a half-cell were manufactured in the same manner as in Example 1, except that the above negative electrode active material was used.

[0128] (Example 3)

[0129] A negative electrode active material was prepared in the same manner as in Example 1 above, except that in the process of mixing the product and LiH powder, 0.087 g of LiH was used so that the Li / Si molar ratio was 1.5. In the prepared negative electrode active material, the weight ratio of Li2SiO3 and Li2Si2O5 to Si was 3:97, and the content of Li2SiO3 and Li2Si2O5 was 0.6 wt% with respect to 100 wt% of the total negative electrode active material. In the prepared negative electrode active material, the thickness of the shell was 100 nm to 400 nm, and the thickness of the amorphous carbon layer was 1 nm.

[0130] A negative electrode and a half-cell were manufactured in the same manner as in Example 1, except that the above negative electrode active material was used.

[0131] (Comparative Example 1)

[0132] A cathode active material layer slurry was prepared by mixing 97.5 wt% of artificial graphite cathode active material, 1 wt% of carboxymethyl cellulose, and 0.5 wt% of styrene butadiene rubber in a water solvent.

[0133] A cathode was manufactured by coating, drying, and rolling the above cathode active material layer slurry onto a Cu foil current collector to form a cathode active material layer.

[0134] (Comparative Example 2)

[0135] A negative electrode active material was prepared in the same manner as in Example 1 above, except that in the process of mixing the product and LiH powder, 0.058 g of LiH was used so that the Li / Si molar ratio was 1. In the prepared negative electrode active material, the weight ratio of Li2SiO3 and Li2Si2O5 to Si was 76:24, and the content of Li2SiO3 and Li2Si2O5 was 15.2 wt% with respect to 100 wt% of the total negative electrode active material. In the prepared negative electrode active material, the thickness of the shell was 100 nm to 400 nm, and the thickness of the amorphous carbon layer was 1 nm.

[0136] A negative electrode and a half-cell were manufactured in the same manner as in Example 1, except that the above negative electrode active material was used.

[0137] (Comparative Example 3)

[0138] A negative electrode active material was prepared in the same manner as in Example 1, except that in the process of mixing the product and LiH powder, 0.073 g of LiH was used so that the Li / Si molar ratio was 1.25. In the prepared negative electrode active material, the weight ratio of Li2SiO3 and Li2Si2O5 to Si was 59:41, and the content of Li2SiO3 and Li2Si2O5 was 7.4 wt% with respect to 100 wt% of the total negative electrode active material. In the prepared negative electrode active material, the thickness of the shell was 100 nm to 400 nm, and the thickness of the amorphous carbon layer was 1 nm.

[0139] A negative electrode and a half-cell were manufactured in the same manner as in Example 1, except that the above negative electrode active material was used.

[0140] Experimental Example 1) Evaluation of Electrochemical Characteristics

[0141] Half batteries prepared according to Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to five cycles of formation charge-discharge at room temperature (25°C) at 0.1C (1C = 360 mAh / g). After performing the formation charge-discharge, the battery was charged with a constant current of 0.1C until the voltage reached 0.01V, then charged with a constant voltage while maintaining 0.01V in constant voltage mode and cut-off at 0.01C current. Subsequently, it was discharged with a constant current of 0.1C until the voltage reached 2.0V (vs. Li), then charged with a constant current of 0.5C until the voltage reached 0.01V, then charged with a constant voltage while maintaining 0.01V in constant voltage mode and cut-off at 0.05C current. Subsequently, it was discharged with a constant current of 0.5C until the voltage reached 2.0V (vs. Li).

[0142] After measuring the charge capacity and discharge capacity, the initial efficiency (percentage of discharge capacity / charge capacity) was calculated from these results. The results are shown in Table 1 below.

[0144] Li / Si molar ratio Charging capacity (mAh / g) Discharge capacity (mAh / g) Initial efficiency (%) Comparative Example 1 - 349 332 95 Comparative Example 2 1.0 372 314 84.6 Comparative Example 3 1.25 393 338 85.9 Example 3 1.5 462 401 86.7 Example 2 1.75 471 410 87.0 Example 1 2.0 483 421 87.2

[0145] As shown in Table 1 above, it can be seen that the batteries of Examples 1 to 3 exhibit appropriate initial efficiency and high charge / discharge capacity. Comparative Example 1 has high initial efficiency but low charge / discharge capacity, and Comparative Examples 2 and 3 both showed lower initial efficiency and charge / discharge capacity than Examples 1 to 3.

[0146] Experimental Example 3) Evaluation of lifespan characteristics

[0147] Half-cells prepared according to Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to 250 charge-discharge cycles at 0.5C, and the ratio of the 250-cycle discharge capacity to the 1-cycle discharge capacity was calculated. The results are shown as capacity retention rates in Table 2 below.

[0148] Experimental Example 4) Evaluation of Coulomb Efficiency

[0149] The half-cells of Examples 1 to 3 and Comparative Examples 1 to 3 were charged and discharged 250 times at 0.1C (36mAh / g) up to the 5th cycle and at 0.5C (180mAh / g) from the 6th cycle onwards, and the Coulomb efficiency was measured. The results are shown in Table 2 below.

[0151] Li / Si molar ratio Capacity retention rate (%) Coulomb efficiency (%) Comparative Example 1 - 94.7 99.9 Comparative Example 2 1.0 96.2 99.8 Comparative Example 3 1.25 97.3 99.9 Example 3 1.5 99.5 99.8 Example 2 1.75 99.3 99.9 Example 1 2.0 99.1 99.9

[0152] As shown in Table 2 above, it can be seen that Examples 1 to 3 exhibit high Coulomb efficiency similar to Comparative Examples 1 to 3, while showing superior capacity retention rates compared to Comparative Examples 1 to 3.

[0153] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.

Claims

Claim 1 A core comprising at least one of a carbon-based material or a silicon-based material, or a combination thereof; and Li located on the surface of the core. x SiO y A negative electrode active material comprising a shell containing (1≤x≤3, 1≤y≤6) and Si, wherein the Li x SiO y (wherein, 1≤x≤3, 1≤y≤6) and the weight ratio of the Si is 1:99 to 3:97, and the cathode active material further comprises an amorphous carbon coating layer located on the shell, wherein the thickness of the amorphous carbon coating layer is 1 nm to 5 nm. Claim 2 In claim 1, the shell is SiO z (0 <z≤2)를 더욱 포함하는 것인 음극 활물질. Claim 3 A negative electrode active material according to claim 1, wherein the shell is located in an island or layered manner on the surface of the core. Claim 4 In paragraph 3, the negative active material wherein the shell is located as an island on the surface of the core. Claim 5 In claim 1, the negative electrode active material is a negative electrode active material having a pH of 7 or less. Claim 6 In claim 1, the carbon-based material is a negative electrode active material that is amorphous carbon, crystalline carbon, or a combination thereof. Claim 7 In claim 1, the silicon-based material is a negative electrode active material that is a Si-C composite. Claim 8 In claim 7, the above Si-C composite is a negative electrode active material comprising silicon particles and an amorphous carbon layer coated on the surface of the silicon particles. Claim 9 A negative electrode active material according to claim 7, wherein the Si-C composite comprises silicon primary particles, secondary particles assembled from crystalline carbon, and an amorphous carbon coating layer formed on the surface of the secondary particles. Claim 10 delete Claim 11 A negative electrode active material according to claim 1, wherein the thickness of the shell is 100 nm to 500 nm. Claim 12 In claim 1, the shell is a porous negative electrode active material. Claim 13 delete Claim 14 delete Claim 15 In paragraph 1, the above Li x SiO y A negative electrode active material in which the content of (wherein, 1≤x≤3, 1≤y≤6) is 0.1% to 15% by weight relative to 100% by weight of the total negative electrode active material. Claim 16 In paragraph 1, the above Li x SiO y A negative electrode active material in which the content of (wherein, 1≤x≤3, 1≤y≤6) is 0.1% to 10% by weight relative to 100% by weight of the total negative electrode active material. Claim 17 A lithium secondary battery comprising a negative electrode comprising a negative electrode active material according to any one of claims 1 to 9, 11, 12, 15 and 16; a positive electrode; and an electrolyte.

Citation Information

Patent Citations

  • Negative electrode active material, negative electrode comprising the negative electrode active material, and lithium secondarty battery comprising the negative electrode

    KR1020190052951A

  • Negative active material for rechargeable lithium battery, and rechargeable lithium battery including same

    KR1020210061009A