Negative active material and rechargeable lithium battery including same

The combination of boron-doped silicon and amorphous carbon in the cathode active material addresses the challenges of volume expansion, resulting in improved efficiency, capacity, and lifespan for lithium-ion batteries.

KR103047650B1Active Publication Date: 2026-11-11SAMSUNG SDI CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020230092006
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2026-11-11
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in achieving high energy density, capacity, and long lifespan due to the volume expansion of silicon-based cathode active materials during charging and discharging.

Method used

A cathode active material comprising porous silicon secondary particles assembled from boron-doped silicon primary particles and amorphous carbon, which includes a boron-based material to improve conductivity and a carbon coating to suppress volume expansion.

Benefits of technology

The cathode active material exhibits high efficiency, high capacity, and long lifespan characteristics by effectively managing volume expansion and enhancing conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023078000509-PAT00004_ABST
    Figure 112023078000509-PAT00004_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material and a lithium secondary battery including the same, wherein the negative electrode active material comprises porous silicon secondary particles assembled from boron-doped silicon primary particles and amorphous carbon.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The invention relates to a negative electrode active material and a lithium secondary battery containing the same. Background Technology

[0002] With the recent rapid proliferation of electronic devices using batteries, such as mobile phones, laptop computers, and electric vehicles, the demand for lithium-ion batteries—which are small, lightweight, and relatively high-capacity—is rapidly increasing.

[0003] In addition, there is a recent demand for the development of high-energy density electricity, and to this end, high-capacity cathode active materials are required.

[0004] Si-based cathode active materials are being attempted as such high-capacity cathode active materials. The problem to be solved

[0005] One embodiment provides a cathode active material exhibiting high efficiency, high capacity, and long lifespan characteristics.

[0006] Another embodiment provides a lithium secondary battery comprising the above-mentioned negative electrode active material. means of solving the problem

[0007] One embodiment provides a cathode active material comprising porous silicon secondary particles assembled from boron-doped silicon primary particles; and amorphous carbon.

[0008] According to another embodiment, a lithium secondary battery is provided comprising a cathode including the cathode active material; a positive electrode; and an electrolyte. Effects of the invention

[0009] The cathode active material according to one embodiment can exhibit high efficiency, high capacity, and long lifespan characteristics. Brief explanation of the drawing

[0010] FIG. 1 is a schematic diagram showing a lithium secondary battery according to one embodiment. FIG. 2 is a cross-sectional image by secondary ion mass spectroscopy (SIMS) of the cathode active material prepared according to Example 1 (a: silicon elemental mapping analysis result, b: boron elemental mapping analysis result). FIG. 3 is a graph showing the results of internal XPS (X-ray photoelectron spectroscopy) analysis of the cathode active materials prepared according to Examples 1 and 2 and Comparative Example 1. FIG. 4 is a graph showing the X-ray diffraction peak intensity of the negative electrode active material prepared according to Examples 1 and 2 and Comparative Example 1. FIG. 5 is a graph showing the room temperature cycle life characteristics of lithium secondary batteries prepared according to Examples 3 to 5 and Comparative Examples 1 and 2. Specific details for implementing the invention

[0011] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0012] The terms used herein are for describing exemplary embodiments only and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.

[0013] Here, "combinations of these" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.

[0014] The terms "include," "equip," or "have" used herein are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0015] In the drawings, thicknesses have been enlarged to clearly represent various layers and regions, and the same reference numerals have been used for similar parts throughout the specification. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between.

[0016] In addition, the term "layer" here includes not only the shape formed on the entire surface when viewed in a plan view, but also the shape formed on some surfaces.

[0017] Here, "or" is not interpreted in an exclusive sense; for example, "A or B" is interpreted to include A, B, A+B, etc.

[0018] Unless otherwise defined in this specification, the particle size or size may be the average particle size. This average particle size refers to the average particle size (D50) which means the diameter of a particle whose cumulative volume in the particle size distribution is 50% by volume. The average particle size (D50) may be measured by methods widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope (TEM) image or a scanning electron microscope (SEM) image. Alternatively, the average particle size (D50) value may be obtained by measuring using a measuring device utilizing dynamic light-scattering, performing data analysis to count the number of particles for each particle size range, and then calculating from this.

[0019] A negative electrode active material according to one embodiment comprises porous silicon secondary particles assembled from boron-doped silicon primary particles; and amorphous carbon. The negative electrode active material according to one embodiment can be usefully used for a lithium secondary battery.

[0020] In one embodiment, the boron-doped silicon primary particles mean that boron is substituted within the silicon crystal structure, so that boron is located between the silicon lattices.

[0021] The above porous silicon secondary particles may be secondary particles containing pores formed by assembling boron-doped silicon primary particles.

[0022] The above porous silicon secondary particles are formed by assembling silicon primary particles and containing pores inside. Generally, silicon can expand in volume during charging and discharging. Since the porous silicon secondary particles according to one embodiment contain pores inside, they have a buffer function capable of absorbing the volume expansion of these pores, thereby effectively suppressing the problem of the entire negative electrode active material expanding in volume.

[0023] The pore volume of the porous silicon secondary particles may be 0.001 cm³ / g to 0.01 cm³ / g, or 0.002 cm³ / g to 0.007 cm³ / g. When the pore volume of the porous silicon secondary particles falls within the above range, the porous silicon secondary particles contain micropores, which further increases the expansion reduction effect, and the structure of the negative electrode active material can be better maintained during charging and discharging, thereby increasing the effects of low expansion and long lifespan.

[0024] The average particle size (D50) of the above silicon primary particles may be 10 nm to 500 nm or 20 nm to 150 nm. In addition, the above secondary particles may have a particle size of 5 µm to 12 µm. The particle size of the above secondary particles may be, for example, 6 µm to 12 µm or 6 µm to 10 µm.

[0025] In addition, porous silicon secondary particles have low conductivity due to their porous structure, but the negative electrode active material according to one embodiment contains boron, and in particular, boron is doped into the silicon primary particles, so conductivity can be improved, and thus battery characteristics such as efficiency, capacity, and lifespan can be improved.

[0026] In one embodiment, the content of boron included in the negative electrode active material may be 0.01 wt% to 5 wt% with respect to 100 wt% of the total negative electrode active material, 0.05 wt% to 2 wt%, or 0.05 wt% to 1 wt%. In one embodiment, the boron content refers to the total content of boron included in the negative electrode active material. When the boron content falls within the above range, the conductivity of the negative electrode active material can be further improved.

[0027] The negative electrode active material according to one embodiment may further include a boron-based material.

[0028] The above boron-based material may be boron oxide, boric acid, MgB2, boron, or a combination thereof. In one embodiment, the above boron-based material may be boron oxide, boric acid, boron, or a combination thereof. Among the boron-based materials, the boron may be elemental boron, that is, boron that is not doped into the silicon primary particle and exists separately from the silicon primary particle or secondary particle.

[0029] Accordingly, it is appropriate for the total content of boron contained in the negative electrode active material according to one embodiment to be within the above range, and there is no need to define the respective content of doped boron and boron contained in the boron-based material. Furthermore, the total content of boron refers to the sum of the content of boron doped in the silicon primary particles and the content of boron contained in the boron-based material located on the surface of the silicon primary particles and / or silicon secondary particles. That is, it refers to the total content of boron present in the negative electrode active material.

[0030] In a negative electrode active material according to one embodiment, it can be confirmed by mapping experiments on the negative electrode active material that boron is doped into silicon primary particles and is also located on the surface of porous silicon secondary particles. In addition, the doping of boron into the silicon primary particles can be measured by XPS experiments.

[0031] In a negative electrode active material according to one embodiment, the amorphous carbon may be located between the silicon primary particles or on the surface of the silicon secondary particles. In a negative electrode active material according to one embodiment, the amorphous carbon may be located on the porous silicon secondary particles and may be included, for example, as a coating layer positioned to cover the secondary particles. Additionally, the amorphous carbon may be located between the primary particles, for example, within the pores of the porous silicon secondary particles.

[0032] In one embodiment, the amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a combination thereof.

[0033] The above amorphous carbon may exist as a coating layer, wherein the thickness may be 1 nm to 2 µm, 1 nm to 500 nm, 10 nm to 300 nm, or 20 nm to 200 nm. When the thickness of the amorphous carbon coating layer falls within the above range, silicon volume expansion during charging and discharging can be effectively suppressed.

[0034] In a negative electrode active material according to one embodiment, the mixing ratio of the silicon and the amorphous carbon may be 55:45 to 70:30 weight ratio and 55:45 to 65:35 weight ratio.

[0035] In the case where the negative electrode active material according to one embodiment further includes a boron-based material, this boron-based material may also be positioned to be covered by the amorphous carbon coating layer.

[0036] The negative electrode active material according to this embodiment may be manufactured using a boron-based material. The addition of the boron-based material may be carried out at any stage during the manufacturing process of the negative electrode active material, prior to the heat treatment process.

[0037] For example, boron-based materials may be used in the porous silicon manufacturing process or in a mixing process with amorphous carbon precursors. The following describes a manufacturing method according to the steps of using boron-based materials.

[0038] 1) Used in the porous silicon manufacturing process

[0039] A silicon dispersion is prepared by mixing micrometer-sized silicon particles with an organic solvent. At this time, the mixing process can be performed as a milling process to reduce the size of the silicon particles from micrometers to nanometers, thereby forming silicon nanoparticles (primary particles). The milling process can be performed using a bead mill or a ball mill.

[0040] As the above organic solvent, alcohols that are easily volatile without oxidizing the silicon particles can be appropriately used, and examples include isopropyl alcohol, ethanol, methanol, butanol, propylene glycol, or combinations thereof.

[0041] The average particle size (D50) of the silicon nanoparticles may be 10 nm to 500 nm, or 20 nm to 150 nm. Additionally, the maximum particle size (Dmax) of the silicon nanoparticles may be 1000 nm or less. When the average particle size (D50) of the silicon nanoparticles falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.

[0042] The mixing ratio of the silicon primary particles and the organic solvent may be 5:95 to 30:70 by weight, or 10:90 to 25:75 by weight. When the mixing ratio of the silicon primary particles and the organic solvent falls within the above range, there may be an advantage in maximizing milling efficiency.

[0043] A boron-based material is added to the obtained silicon dispersion, and the mixture is spray-dried to produce porous silicon secondary particles. The boron-based material is as described above. According to the spray-drying process, primary particles, which are silicon nanoparticles, are assembled to form secondary particles, and boron oxide is also assembled together in this process. The secondary particles may be spherical, and the average particle size (D50) may be 5 μm to 12 μm.

[0044] The content of the above boron-based material can be controlled to an amount sufficient for boron to be doped into the silicon primary particles. For example, it may be 0.2% to 11% by weight relative to 100% by weight of silicon nanoparticles. When the content of the boron-based material falls within the above range, the formation of by-products (undegraded residues) is reduced, allowing for improved conductivity while maintaining capacity and efficiency.

[0045] The above spray drying process can be carried out at 50°C to 200°C. If the spray drying temperature is carried out within the above temperature and time range, primary particle aggregation can occur effectively and sufficiently.

[0046] The pore volume of the porous silicon secondary particles may be 0.001 cm³ / g to 0.01 cm³ / g, or 0.002 cm³ / g to 0.007 cm³ / g. When the pore volume of the porous silicon secondary particles falls within the above range, the porous silicon secondary particles contain micropores, which further increases the expansion reduction effect, and the structure of the negative electrode active material can be better maintained during charging and discharging, thereby increasing the effects of low expansion and long lifespan.

[0047] A mixture is prepared by mixing porous silicon secondary particles and amorphous carbon precursors produced by the above process.

[0048] The above amorphous carbon precursor may include phenol resin, furan resin, epoxy resin, polyacrylonitrile, polyamide resin, polyimide resin, polyamideimide resin, synthetic pitch, petroleum-based pitch, coal-based pitch, meso pitch, tar, or a combination thereof.

[0049] In addition, the mixing ratio of the porous silicon secondary particles and the amorphous carbon precursor can be adjusted so that the mixing ratio of silicon to amorphous carbon in the final product is 55:45 to 70:30 by weight, and 55:45 to 65:35 by weight.

[0050] Next, the obtained mixture is heat-treated to produce a heat-treated product. This heat treatment process can be carried out at 700°C to 1000°C, for example, 800°C to 1000°C. The heat treatment process can be carried out for 1 hour to 10 hours, or for 1 hour to 8 hours or for 1 hour to 6 hours.

[0051] In addition, the above heat treatment process may be carried out under an N2 or Ar atmosphere.

[0052] According to the above heat treatment process, the amorphous carbon precursor is converted into amorphous carbon to form an amorphous carbon coating layer. Additionally, according to the above heat treatment process, the boron-based material is decomposed to form boron, and this boron is doped into the silicon primary particles, that is, the boron is substituted within the silicon crystal structure, so that the boron is positioned between the silicon lattices. At this time, the decomposed boron may remain without being doped into the silicon primary particles and may be located on the surface of the silicon primary particles and / or the surface of the silicon secondary particles. Furthermore, the boron-based material may not be completely decomposed, and some may remain in an undecomposed state. Such undecomposed boron-based material may be located on the surface of the silicon primary particles and / or the surface of the silicon secondary particles. Such decomposed boron or undecomposed boron-based material may be located continuously in a layered manner on the surface of the silicon primary particles and / or the silicon secondary particles, or discontinuously in an island form.

[0053] 2) Used in the mixing process with amorphous carbon precursors

[0054] First, porous silicon secondary particles containing pores inside are manufactured.

[0055] The above porous silicon secondary particles may be silicon nanoparticles, that is, silicon primary particles assembled therefrom. The average particle size (D50) of the silicon nanoparticles may be 10 nm to 500 nm, or 20 nm to 150 nm. Additionally, the maximum particle size (Dmax) of the silicon nanoparticles may be 1000 nm or less. If the average particle size (D50) of the silicon nanoparticles falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented. The assembly process of the silicon nanoparticles may be carried out as follows. A silicon dispersion is prepared by mixing micrometer-sized silicon particles with an organic solvent. At this time, the mixing process may be performed as a milling process so that the size of the silicon particles is reduced from micrometers to nanometers to become silicon nanoparticles. The milling process may be performed using a bead mill or a ball mill.

[0056] As the above organic solvent, alcohols that are easily volatile without oxidizing the silicon particles can be appropriately used, and examples include isopropyl alcohol, ethanol, methanol, butanol, propylene glycol, or combinations thereof.

[0057] The mixing ratio of the silicon primary particles and the organic solvent may be 5:95 to 30:70 by weight, or 10:90 to 25:75 by weight. When the mixing ratio of the silicon primary particles and the organic solvent falls within the above range, there may be an advantage in maximizing milling efficiency.

[0058] The obtained silicon dispersion is spray-dried to produce porous silicon secondary particles. This spray-drying process can be carried out at a temperature of 50°C to 200°C. Through this spray-drying process, primary particles, which are silicon nanoparticles, are assembled to form secondary particles, thereby producing porous silicon secondary particles. When the spray-drying process is carried out within the above temperature range, the process of primary particles assembling to form secondary particles can be carried out more appropriately.

[0059] The pore volume of the porous silicon secondary particles may be 0.001 cm³ / g to 0.01 cm³ / g, or 0.002 cm³ / g to 0.007 cm³ / g. When the pore volume of the porous silicon secondary particles falls within the above range, the porous silicon secondary particles contain micropores, which further increases the expansion reduction effect, and the structure of the negative electrode active material can be better maintained during charging and discharging, thereby increasing the effects of low expansion and long lifespan.

[0060] A mixture is prepared by mixing the above-mentioned porous silicon secondary particles containing internal pores, an amorphous carbon precursor, and a boron-based material. The boron-based material is as described above.

[0061] The above amorphous carbon precursor is as described above.

[0062] The mixing ratio of the porous silicon secondary particles and the boron-based material may be a weight ratio of 99.8:0.2 to 90:10, a weight ratio of 99.8:0.2 to 98:2, or a weight ratio of 98:2 to 96:4.

[0063] When the mixing ratio of the above porous silicon secondary particles and the above boron-based material falls within the above range, the formation of by-products (undissolved residues) is reduced, allowing for better capacity and efficiency while further improving conductivity.

[0064] In addition, the mixing ratio of the porous silicon secondary particles and the amorphous carbon precursor may be 55:45 to 70:30 weight ratio and 55:45 to 65:45 weight ratio.

[0065] Next, the obtained mixture is heat-treated to produce a heat-treated product. This heat treatment process can be carried out at 700°C to 1000°C, for example, 800°C to 1000°C. The heat treatment process can be carried out for 1 hour to 6 hours, or for 2 hours to 6 hours or for 4 hours to 6 hours.

[0066] In addition, the above heat treatment process may be carried out under an N2 or Ar atmosphere.

[0067] According to the above heat treatment process, the amorphous carbon precursor is converted into amorphous carbon to form an amorphous carbon coating layer. Additionally, according to the above heat treatment process, the boron-based material is decomposed to form boron, and this boron is doped into the silicon primary particles, that is, located between the silicon lattices. At this time, the decomposed boron may remain without being doped into the silicon primary particles and may be located on the surface of the silicon primary particles and / or the surface of the silicon secondary particles. Furthermore, the boron-based material may not be completely decomposed, and some may remain in an undecomposed state. Such undecomposed boron-based material may be located on the surface of the silicon primary particles and / or the surface of the silicon secondary particles. Such decomposed boron or undecomposed boron-based material may be located continuously in a layered manner on the surface of the silicon primary particles and / or the silicon secondary particles, or discontinuously in an island form.

[0068] Another embodiment provides a lithium secondary battery comprising a negative electrode, a positive electrode, and an electrolyte.

[0069] The above cathode may include a current collector and a cathode active material layer formed on the current collector and comprising the cathode active material according to one embodiment.

[0070] A negative electrode active material according to one embodiment may be included as a first negative electrode active material, and crystalline carbon may be included as a second negative electrode active material. In this case, the mixing ratio of the first negative electrode active material and the second negative electrode active material may be included in a weight ratio of 1:99 to 50:50. More specifically, the first negative electrode active material and the second negative electrode active material may be included as negative electrode active materials in a weight ratio of 5:95 to 20:80.

[0071] In the above-mentioned negative electrode active material layer, the content of the negative electrode active material may be 95% to 98% by weight with respect to 100% by weight of the entire negative electrode active material layer.

[0072] The above negative electrode active material layer may include a binder and may further include a conductive material. The content of the binder may be 0.1% to 5% by weight with respect to 100% by weight of the entire negative electrode active material layer. The content of the conductive material may be 0.01% to 5% by weight with respect to 100% by weight of the entire negative electrode active material layer.

[0073] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a non-aqueous binder, an aqueous binder, or a combination thereof may be used.

[0074] Examples of the above-mentioned non-aqueous binders include ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0075] The above-mentioned water-based binder may be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, a polymer containing ethylene oxide, polyvinylpyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.

[0076] A cellulose-based compound may be used as the above-mentioned cathode binder, or a mixture of the above-mentioned cellulose-based compound and the above-mentioned aqueous binder may be used. As the above-mentioned cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal. The above-mentioned cellulose-based compound can act as a binder and may also act as a thickener capable of increasing viscosity. Accordingly, there is no need to separately limit the content of the above-mentioned cellulose-based compound, but for example, the content of the above-mentioned cellulose-based compound may be 0.1 to 3 parts by weight per 100 parts by weight of the cathode active material.

[0077] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.

[0078] The above current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0079] The above anode includes a current collector and an anode active material layer formed on the current collector.

[0080] As the above-mentioned cathode active material, a compound capable of reversible intercalation and deintercalation of lithium (a rethated intercalation compound) may be used. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. As a more specific example, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b X b D 1 2(0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 2-b X b O 4-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a Ni 1-b-c Co b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni1-b-c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1) Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mr 1-b G bO2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8)

[0081] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; and D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; T is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; Z is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof; L 1 is Mn, Al, or a combination thereof.

[0082] Of course, it is possible to use a compound having a coating layer on its surface, or to use a mixture of the compound and a compound having a coating layer. This coating layer may include at least one coating element compound among the oxide of the coating element, the hydroxide of the coating element, the oxyhydroxide of the coating element, the oxycarbonate of the coating element, or the hydroxycarbonate of the coating element. The compounds forming these coating layers may be amorphous or crystalline. As for the coating elements included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the art, a detailed explanation will be omitted.

[0083] In the above anode, the content of the anode active material may be 90% to 98% by weight with respect to the total weight of the anode active material layer.

[0084] In one embodiment, the positive active material layer may further include a binder and a conductive material. In this case, the content of the binder and the conductive material may each be 1% to 5% by weight with respect to the total weight of the positive active material layer.

[0085] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples of binders include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.

[0086] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising mixtures thereof.

[0087] Al may be used as the current collector mentioned above, but is not limited thereto.

[0088] The above electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0089] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0090] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.

[0091] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc., and the above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methylpropionate, ethylpropionate, propylpropionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, etc. The above ether-based solvent may include dibutyl ether, tetraglame, diglame, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc., and the above ketone-based solvent may include cyclohexanone, etc. In addition, the above alcohol-based solvent may include ethyl alcohol, isopropyl alcohol, etc., and the above aprotic solvent may include nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, 1,4-dioxolane, sulfolanes, etc.

[0092] The above organic solvents may be used alone or in a mixture of one or more. When used in a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.

[0093] When using the above-mentioned non-aqueous organic solvent in a mixture, a mixed solvent of cyclic carbonate and chain carbonate, a mixed solvent of cyclic carbonate and propionate-based solvent, or a mixed solvent of cyclic carbonate, chain carbonate, and propionate-based solvent may be used. As the propionate-based solvent, methylpropionate, ethylpropionate, propylpropionate, or a combination thereof may be used.

[0094] In this case, when using a mixture of cyclic carbonate and chain carbonate or cyclic carbonate and propionate-based solvent, mixing them in a volume ratio of 1:1 to 1:9 may be appropriate in terms of electrolyte performance. Additionally, when using a mixture of cyclic carbonate, chain carbonate, and propionate-based solvent, they may be mixed in a volume ratio of 1:1:1 to 3:3:4. Of course, the mixing ratio of the solvents may also be appropriately adjusted according to the desired physical properties.

[0095] The above organic solvent may further include an aromatic hydrocarbon organic solvent in the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0096] As the above aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound of the following chemical formula 1 may be used.

[0097] [Chemical Formula 1]

[0098]

[0099] (In the above Chemical Formula 1, R1 to R6 are identical or different from each other and are selected from the group consisting of hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.)

[0100] Specific examples of the above aromatic hydrocarbon-based organic solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. It is selected from the group consisting of 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.

[0101] The above electrolyte may further include vinyl ethyl carbonate, vinylene carbonate, or an ethylene carbonate-based compound of the following chemical formula 2 as a life-enhancing additive to improve battery life.

[0102] [Chemical Formula 2]

[0103]

[0104] (In the above chemical formula 2, R7 and R8 are identical or different from each other and are selected from the group consisting of hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, and at least one of R7 and R8 is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, provided that R7 and R8 are not both hydrogen.)

[0105] Representative examples of the above-mentioned ethylene carbonate-based compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. When using more of these lifespan-enhancing additives, the amount used can be appropriately controlled.

[0106] The above lithium salt is a material that dissolves in an organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of a lithium secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, and LiN(C x F 2x+1 SO2)(C y F 2y+1SO2)(where x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxolato) phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato) borate (LiBOB)), and lithium difluoro(oxalato) borate (LiDFOB) are included as supporting electrolyte salts, one or more selected from the group consisting of lithium bis(oxalato) borate (LiBOB) and lithium difluoro(oxalato) borate (LiDFOB). It is preferable to use a lithium salt concentration within the range of 0.1 M to 2.0 M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0107] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof may be used, and of course, mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators may be used.

[0108] The above separator may include a porous substrate and a coating layer comprising an organic material, an inorganic material, or a combination thereof located on one or both sides of the porous substrate.

[0109] The porous substrate may be a polymer membrane formed from any one of the following: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene oxide; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; glass fiber; Teflon; and polytetrafluoroethylene, or a copolymer or mixture of two or more of these.

[0110] The porous substrate may have a thickness of about 1 μm to 40 μm, and may have a thickness of, for example, 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 10 μm to 15 μm.

[0111] The above organic material may include a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, and a second structural unit comprising at least one of a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamideidosulfonic acid or its salt.

[0112] The above inorganic materials are Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may include inorganic particles selected from SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof, but is not limited thereto. The average particle size (D) of the inorganic particles 50 ) can be 1 nm to 2000 nm, and, for example, 100 nm to 1000 nm, or 100 nm to 700 nm.

[0113] The above organic and inorganic materials may exist mixed in a single coating layer, or may exist in a stacked form with a coating layer containing organic materials and a coating layer containing inorganic materials.

[0114] The thickness of the coating layer may be 0.5 μm to 20 μm, for example, 1 μm to 10 μm, or 1 μm to 5 μm.

[0115] FIG. 1 shows an exploded perspective view of a lithium secondary battery according to one embodiment of the present invention. Although the lithium secondary battery according to one embodiment is described as being prismatic, the present invention is not limited thereto and can be applied to various types of batteries such as cylindrical and pouch types.

[0116] Referring to FIG. 1, a lithium secondary battery (100) according to one embodiment may include an electrode assembly (40) wound with a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown).

[0117] Examples and comparative examples of the present invention are described below. The following examples are merely embodiments of the present invention, and the present invention is not limited to the following examples.

[0118] (Example 1)

[0119] Silicon particles with a particle size of several micrometers were mixed with an ethanol solvent in a weight ratio of 85:15, and a silicon nano dispersion was prepared using a bead mill (Netzsch, Germany). In the prepared silicon nano dispersion, the average particle size (D50) of the silicon nanoparticles (primary particles) is 90 nm, and the maximum particle size (Dmax) can be 150 nm.

[0120] The above silicon nano dispersion was spray-dried at 180°C using a spray dryer to produce porous silicon secondary particles. The produced porous silicon secondary particles were formed by assembling primary particles, which are silicon nanoparticles, into spherical secondary particles with an average particle size (D50) of 8 μm, and a pore volume of 0.007 cm³ / g.

[0121] A mixture was prepared by mixing the obtained porous silicon secondary particles, petroleum-based pitch, and boron oxide (B2O3). At this time, the weight ratio of (porous silicon secondary particles and petroleum-based pitch):boron oxide was set to 98:2, and the weight ratio of porous silicon secondary particles:petroleum-based pitch was set to 63.3:36.7.

[0122] The above mixture was heat-treated at 950°C for 2 hours in an N2 atmosphere to produce a negative electrode active material, which is the heat treatment product.

[0123] According to the above heat treatment process, boron oxide is decomposed so that boron is doped into the silicon primary particles, and petroleum pitch is converted into soft carbon, located within the pores of the porous silicon secondary particles, and a soft carbon coating layer is formed on the surface of the porous silicon secondary particles.

[0124] At this time, the boron content contained in the negative electrode active material was 0.7 wt% with respect to 100 wt% of the total negative electrode active material. In addition, the thickness of the soft carbon coating layer was 200 nm.

[0125] In addition, the silicon content constituting the porous silicon secondary particles was 62.9 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 36.4 wt%.

[0126] A cathode active material layer slurry was prepared by mixing 97.5 wt% of the manufactured cathode active material, 1.5 wt% of carboxymethyl cellulose, and 1 wt% of styrene butadiene rubber in a water solvent.

[0127] A cathode was manufactured by coating, drying, and rolling the above cathode active material layer slurry onto a Cu foil current collector to form a cathode active material layer.

[0128] A half-cell was manufactured by a conventional method using the above-described cathode, lithium metal counter electrode, and electrolyte for the half-cell. As the electrolyte for the half-cell, a fluoroethylene carbonate was added to an electrolyte precursor prepared by adding 1.5M LiPF6 to a mixed solvent of ethylene carbonate, ethylmethyl carbonate, and dimethyl carbonate (volume ratio of 2:1:7). At this time, the content of fluoroethylene carbonate was set to 10% by weight relative to 100% by weight of the electrolyte precursor.

[0129] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using a conventional method with an O2 anode and an electrolyte for the full cell. As the electrolyte for the full cell, a fluoroethylene carbonate was added to an electrolyte precursor prepared by adding 1.5M LiPF6 to a mixed solvent (2:1:7 volume ratio) of ethylene carbonate, ethylmethyl carbonate, and dimethyl carbonate. At this time, the content of fluoroethylene carbonate was set to 3.5% by weight relative to 100% by weight of the electrolyte precursor.

[0130] (Example 2)

[0131] A negative electrode active material was prepared in the same manner as in Example 1 above, except that the weight ratio of boron oxide (porous silicon secondary particles and petroleum-based pitch) was 96:4 and the weight ratio of porous silicon secondary particles to petroleum-based pitch was 63.3:36.7.

[0132] The manufactured cathode active material included porous silicon secondary particles assembled from boron-doped silicon primary particles, soft carbon located within the pores of the porous silicon secondary particles, and a soft carbon coating layer located on the surface of the porous silicon secondary particles.

[0133] At this time, the boron content contained in the cathode active material was 1.4 wt% with respect to 100 wt% of the total cathode active material. In addition, the thickness of the soft carbon coating layer was 200 nm.

[0134] In addition, the silicon content constituting the porous silicon secondary particles was 62.4 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 36.2 wt%.

[0135] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0136] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0137] (Example 3)

[0138] Silicon particles with a particle size of several micrometers were mixed with an ethanol solvent in a weight ratio of 85:15, and a silicon nano dispersion was prepared using a bead mill (Netzsch, Germany). In the prepared silicon nano dispersion, the average particle size (D50) of the silicon nanoparticles (primary particles) is 90 nm, and the maximum particle size (Dmax) can be 150 nm.

[0139] Boron oxide (B2O3) was added to the above silicon nano dispersion, and the mixture was spray-dried at 180°C using a spray dryer to produce porous silicon secondary particles. The content of the boron oxide was 2 wt% relative to 100 wt% of the silicon nanoparticles. The produced porous silicon secondary particles were formed by assembling primary particles, which were silicon nanoparticles, into spherical secondary particles with an average particle size (D50) of 8 μm, and the pore volume was 0.007 cm³ / g.

[0140] The obtained porous silicon secondary particles and petroleum-based pitch were mixed, and the mixture was heat-treated at 950°C for 2 hours in an N2 atmosphere to produce a negative electrode active material, which is the heat treatment product. In the above mixing process, the mixing ratio of the porous silicon secondary particles and the petroleum-based pitch was set so that the weight ratio of silicon to petroleum-based pitch was 63.3:36.7.

[0141] According to the above heat treatment process, boron oxide is decomposed, boron is doped into the silicon primary particles, and petroleum pitch is converted into soft carbon, forming a soft carbon coating layer on the surface of the porous silicon secondary particles.

[0142] Accordingly, the manufactured cathode active material included porous silicon secondary particles assembled from boron-doped silicon primary particles, soft carbon located within the pores of the porous silicon secondary particles, and a soft carbon coating layer located on the surface of the porous silicon secondary particles.

[0143] At this time, the boron content contained in the cathode active material was 0.7 wt% with respect to 100 wt% of the total cathode active material. In addition, the thickness of the soft carbon coating layer was 200 nm.

[0144] In addition, the silicon content constituting the porous silicon secondary particles was 62.9 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 36.4 wt%.

[0145] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0146] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0147] (Example 4)

[0148] A negative electrode active material was prepared in the same manner as in Example 3 above, except that boron oxide was used at 4 wt% relative to 100 wt% of silicon nanoparticles.

[0149] The manufactured cathode active material included porous silicon secondary particles assembled from boron-doped silicon primary particles, soft carbon located within the pores of the porous silicon secondary particles, and a soft carbon coating layer located on the surface of the porous silicon secondary particles.

[0150] At this time, the boron content contained in the cathode active material was 1.4 wt% with respect to 100 wt% of the total cathode active material. In addition, the thickness of the soft carbon coating layer was 200 nm.

[0151] In addition, the silicon content constituting the porous silicon was 62.4 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 36.2 wt%.

[0152] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0153] The above cathode, LiNi 0.88 Co0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0154] (Example 5)

[0155] A negative electrode active material was prepared in the same manner as in Example 3 above, except that boron oxide was used at 6 wt% relative to 100 wt% of silicon nanoparticles.

[0156] The manufactured cathode active material included porous silicon secondary particles assembled from boron-doped silicon primary particles, soft carbon located within the pores of the porous silicon secondary particles, and a soft carbon coating layer located on the surface of the porous silicon secondary particles.

[0157] At this time, the boron content contained in the cathode active material was 2.1 wt% with respect to 100 wt% of the total cathode active material. In addition, the thickness of the soft carbon coating layer was 200 nm.

[0158] In addition, the silicon content constituting the porous silicon secondary particles was 62 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 35.9 wt%.

[0159] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0160] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0161] (Comparative Example 1)

[0162] An ethanol solvent and silicon particles with a particle size of several micrometers were mixed in a weight ratio of 8.5:1.5, and a silicon nano dispersion was prepared using a bead mill (Netzsch, Germany). In the prepared silicon nano dispersion, the average particle size (D50) of the silicon nanoparticles (primary particles) can be 90 nm, and the maximum particle size (Dmax) can be 150 nm.

[0163] The above silicon nano dispersion was spray-dried at 180°C using a spray dryer to produce porous silicon secondary particles. The produced porous silicon secondary particles were formed by assembling primary particles, which were silicon nanoparticles, into secondary particles, and had a pore volume of 0.007 cm³ / g.

[0164] The obtained porous silicon secondary particles and petroleum-based pitch were heat-treated at 950°C for 2 hours in an N2 atmosphere to prepare a heat-treated product. The weight ratio of porous silicon secondary particles to petroleum-based pitch was set to 63.3:36.7.

[0165] At this time, the manufactured negative electrode active material included porous silicon secondary particles containing pores inside, a soft carbon coating layer located on the surface of the porous silicon secondary particles, and soft carbon located within the pores. At this time, the silicon content constituting the porous silicon was 63.3 wt% with respect to 100 wt% of the total negative electrode active material, and the content of the soft carbon amorphous carbon was 36.7 wt%.

[0166] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0167] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0168] (Comparative Example 2)

[0169] SiO x A mixture was prepared by mixing (x=1.1) and boron oxide (B2O3) in a weight ratio of 98:2.

[0170] The above mixture was heat-treated at 950°C for 2 hours in an N2 atmosphere to produce a negative electrode active material, which is the heat treatment product.

[0171] The manufactured cathode active material is SiO x and this SiO x Boron doped into and, this SiO x It contained boron located on the surface. At this time, the content of boron contained in the negative electrode active material was 0.7 wt% with respect to 100 wt% of the total negative electrode active material.

[0172] A cathode was manufactured using the above cathode active material, and a half battery was manufactured by a conventional method using this cathode, a lithium metal counter electrode, and the electrolyte for the half battery of Example 1.

[0173] The above cathode, LiNi 0.88 Co 0.1 Al 0.1 A lithium secondary battery in the form of a full cell was manufactured using the O2 anode and the electrolyte for the full cell of Example 1 above by a conventional method.

[0174] Experimental Example 1: SIMS Analysis of Cross-Section of Cathode Active Material

[0175] Secondary Ion Mass Spectroscopy (SIMS) analysis was performed on the cross-section of the negative electrode active material prepared according to Example 1 above. Among the results, the silicon (Si) element mapping analysis results are shown in FIG. 2(a). In addition, the boron element mapping analysis results for the same region as FIG. 2(a) are shown in FIG. 2(b). Referring to FIG. 2, it can be seen that boron is located inside the silicon primary particles.

[0176] Experimental Example 2: Surface and Internal XPS (X-ray Photoelectron Spectroscopy) Analysis of Cathode Active Material

[0177] The interior of the negative electrode active material prepared according to Examples 1 and 2 and Comparative Example 1 was analyzed by X-ray photoelectron spectroscopy (XPS). The results are shown in Fig. 3. As shown in Fig. 3, it can be seen that Si and elemental boron are present inside the prepared negative electrode active material. In addition, it can be seen that as the amount of boron oxide used increases, the boron peak increases and the Si-Si bond decreases.

[0178] Experimental Example 3) Measurement of X-ray diffraction

[0179] X-ray diffraction peak analysis using CuKα rays was performed on the cathode active materials prepared according to Examples 1 and 2 and Comparative Example 1. The results are shown in Fig. 5. In Fig. 4, the x-axis represented the 2θ value. As shown in Fig. 4, it can be seen that as the amount of boron oxide used increases, the Si peak intensity decreases and shifts in the direction of increasing 2θ. From this result, it can be seen that boron is well doped internally.

[0180] Experimental Example 4) Cycle Life Characteristics

[0181] The lithium secondary batteries prepared according to Examples 1 to 5 and Comparative Examples 1 and 2 were charged and discharged 200 times at room temperature (25°C) under the following conditions, and the discharge capacity at each cycle was determined. Among the results, the results of Comparative Example 1 and Examples 3 to 5 are shown in FIG. 5.

[0182] Charging: 1.0C / Cut-off: 4.0V-0.05C

[0183] Discharge: 1.0C / Cut-off 2.5V

[0184] As shown in FIG. 5, it can be seen that the cycle life characteristics and capacity retention rate of the batteries of Examples 3 to 5 containing boron oxide are superior to those of Comparative Example 1.

[0185] In addition, the ratio of the 200-cycle discharge capacity to the 1-cycle discharge capacity was calculated. Among the results, the results of Comparative Examples 1 and 2 are shown in Table 1 below as capacity retention rates. Furthermore, the ratio of the discharge capacity at each cycle to the 1-cycle discharge capacity was calculated, and the number of cycles at which the capacity ratio drops to less than 80% is indicated in Table 1 below as the point of rapid decline in life.

[0187] Capacity retention rate (%) Point of sharp decline in lifespan Comparative Example 1 86 210 Comparative Example 2 81 300

[0188] As shown in Table 1 above, it can be seen that Comparative Example 2 has a point of rapid decline in lifespan that is equivalent to or slightly later than Comparative Example 1, while the capacity retention rate is much lower than that of Comparative Example 1.

[0189] Looking at the results in Figure 5 and Table 1, Comparative Example 1 has a much lower cycle life and capacity retention rate than Examples 3 to 5, and Comparative Example 2 has a lower capacity retention rate than Comparative Example 1, so it can be seen that Comparative Example 2 exhibits significantly lower life characteristics than Examples 3 to 5.

[0190] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.

Claims

Claim 1 A negative electrode active material comprising: porous silicon secondary particles assembled from boron-doped silicon primary particles; and amorphous carbon, wherein the amorphous carbon is included as a coating layer positioned on the surface of the silicon secondary particles to cover the secondary particles. Claim 2 In claim 1, the content of boron included in the cathode active material is 5 weight%, which is 0.01 weight% with respect to 100 weight% of the total cathode active material. Claim 3 A negative electrode active material according to claim 1, wherein the amorphous carbon is located between the silicon primary particles. Claim 4 A negative electrode active material according to claim 1, wherein the pore volume of the porous silicon secondary particles is 0.001 cm³ / g to 0.01 cm³ / g. Claim 5 In claim 1, the negative electrode active material further comprises a boron-based material. Claim 6 In paragraph 5, the above boron-based material is a negative electrode active material that is boron oxide, boric acid, MgB2, boron, or a combination thereof. Claim 7 In claim 6, the boron-based material is a negative electrode active material which is boron oxide, boric acid, boron, or a combination thereof. Claim 8 In claim 5, the above boron-based material is a negative electrode active material located on the surface of the primary particle and / or the surface of the secondary particle. Claim 9 In claim 1, the amorphous carbon is a negative electrode active material that is soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a combination thereof. Claim 10 A negative electrode active material according to claim 1, wherein the average particle size of the silicon primary particles is 10 nm to 500 nm. Claim 11 A negative electrode active material according to claim 1, wherein the average particle size of the silicon secondary particles is 5㎛ to 12㎛. Claim 12 A negative electrode active material according to claim 1, wherein the amorphous carbon exists with a thickness of 1 nm to 2 μm. Claim 13 A lithium secondary battery comprising a negative electrode active material according to any one of claims 1 to 12 and a negative electrode anode and an electrolyte.

Citation Information

Patent Citations

  • Silicon based negative electrode material for rechargeable battery and method of fabricating the same

    KR101614016B1

  • Negative active material composite for rechargeable lithium battery, method of preparing the same, and negative electrode and rechargeable lithium battery including the same

    KR1020200105402A

  • Negative active material for rechargeable lithium battery, and rechargeable lithium battery including same

    KR1020210055505A