Methods of smelting nickel-containing metals and their uses
Patent Information
- Application Number
- LAP847
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-02-28
- Publication Date
- 2026-04-24
AI Technical Summary
The existing technology has problems such as high energy consumption, high smelting temperature, difficulty in separation of slag and poor quality of ferronickel slag when smelting low-grade nickel ore, resulting in low ferronickel production efficiency and high cost.
By oxidizing and roasting low-grade nickel materials with lime, nickel-iron ore is prepared, mixed with a reducing agent and granulated for pre-reduction, and then smelting reduction is performed in an SRV furnace to optimize the smelting process to improve nickel-iron grade and smelting efficiency. .
It achieves low-cost and efficient smelting of ferronickel, reduces energy consumption, improves the grade and smelting efficiency of ferronickel, and the molten ferronickel can be used to prepare high-quality stainless steel, reducing the consumption of alloy elements.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
A smelting method for nickel-containing metal and its application
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 26, 2021, with application number 202110577663.X and invention name "A method for efficiently smelting nickel-containing molten iron using low-grade nickel materials and its application", the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the technical field of molten reduction metallurgy, and specifically relates to a smelting method of nickel-containing metal and its application. Background Art
[0003] Nickel ore resources primarily consist of two types: nickel sulfide ore and laterite nickel ore. With the increasing shortage of nickel sulfide ore, the development and utilization of laterite nickel ore will become the primary source of nickel resources. Laterite nickel ore accounts for 72% of land-based nickel ore resources. As nickel sulfide resources used in electrolytic nickel are increasingly depleted, the production of ferronickel from laterite nickel ore, which in turn is used as a nickel source for stainless steel production, has become an industrial trend.
[0004] Currently, there are three main conventional nickel-iron production processes, namely: the rotary kiln-electric furnace method, the sintering-blast furnace method, and the rotary kiln granular iron method. However, the above three methods generally have problems such as poor raw material adaptability, long process flow, and high energy consumption. In addition, the unit slag discharge of nickel-iron during smelting is nearly 10 times that of ordinary pig iron, and the utilization rate of nickel-iron slag is only 10%, resulting in a large amount of slag accumulation.
[0005] The HIsmelt smelting reduction process, a commercially viable non-blast furnace ironmaking technology, directly utilizes powdered materials and pulverized coal for rapid smelting, boasting wide raw material compatibility and a short process. Because it utilizes a different principle from traditional blast furnaces, HIsmelt avoids the blast furnace smelting process's need to increase coke levels to improve charge permeability, reducing energy consumption. Furthermore, compared to electric furnace smelting, it significantly reduces energy consumption and production costs.
[0006] In traditional technology, researchers have conducted preliminary explorations into the use of HIsmelt for the smelting of iron-containing minerals. For example, patent CN111850218A provides a method for smelting laterite nickel ore to obtain nickel-iron products using the HIsmelt process. This method directly injects laterite nickel ore, coal powder, and dolomite into a furnace to produce nickel-containing molten iron. CN11139330A provides a device for preheating and reducing iron-containing materials. By designing an external device for the smelting reduction furnace, the HIsmelt process is further optimized.
[0007] However, the low-grade nickel-containing ore contains a large amount of physical water and crystallization water, and has the characteristics of low nickel, low iron, high silicon and high magnesium. If the HIsmelt process is used directly for smelting, on the one hand, it will lead to higher smelting temperatures and smelting gas, resulting in a large amount of energy consumption and reduced production efficiency. On the other hand, a large amount of slag will be formed in the furnace, making it difficult to achieve slag and iron separation and continuous smelting. At the same time, the sulfur and arsenic contained in the low-grade nickel-containing ore are difficult to remove, which seriously affects the quality and performance of the subsequent nickel-containing iron water, and it is difficult to obtain high-quality nickel-containing iron water.
[0008] In actual processes, technicians have attempted to use rotary kilns to directly preheat and pre-reduced low-grade nickel-containing ore. However, due to the physical properties of the raw materials, which are low in iron, high in silicon, and high in magnesium, the powdered raw materials form a large amount of high-melting-point substances such as pyroxene and olivine phases in the rotary kiln. Reduction at high temperatures leads to severe ringing in the high-temperature zone of the rotary kiln where nickel and iron grow, hindering continuous production. In addition, this method has poor reduction effects, and the grade of the resulting product is still difficult to meet technical requirements, and the energy consumption and quality issues mentioned above in smelting still exist. If the melt properties during the laterite nickel ore smelting process can be improved, the smelting temperature and slag heat loss can be reduced, it will be important for achieving efficient, low-cost, and continuous industrial operation of low-grade nickel-containing ore.
[0009] Summary of the Invention
[0010] According to various embodiments of the present application, on the one hand, the present application provides a method for smelting nickel-containing metal, comprising the following steps:
[0011] Step 1: mixing low-grade nickel material with lime and performing oxidative roasting to obtain nickel iron ore;
[0012] Step 2: After vigorously mixing the nickel iron ore with a first reducing agent, sodium sulfate, water and a binder, granulating to obtain nickel iron ore pellets, adding the nickel iron ore pellets to a rotary kiln, and then mixing with a second reducing agent to perform a pre-reduction treatment to obtain a high-grade nickel iron raw material;
[0013] Step 3: The high-grade nickel-iron raw material is subjected to smelting reduction using an SRV furnace to obtain the nickel-containing iron water.
[0014] It can be understood that the SRV furnace described in this application is the SRV smelting reduction furnace used in the HIsmelt process.
[0015] Furthermore, the conditions for the oxidation roasting in step 1 are: controlling the roasting temperature to be 650° C. to 900° C., the oxygen content to be 30% to 50%, and the time to be 40 to 60 minutes; and / or,
[0016] The amount of lime used is 3% to 10% based on the mass of the low-grade nickel material.
[0017] Optionally, a drying kiln is used to oxidize and roast the low-grade nickel material in step 1. More preferably, the drying kiln is 50 to 100 meters long and the temperature inside the kiln is controlled at 650°C to 900°C.
[0018] Optionally, coal gas, hydrogen, natural gas, high-temperature hot air or other combustible gases are burned in the drying kiln to provide a heat source.
[0019] Furthermore, the low-grade nickel material is selected from one or more of laterite nickel ore, nickel slag, nickel-containing oxide slag and nickel-containing iron filings.
[0020] Preferably, the composition of the low-grade nickel material includes at least 1% to 3% Ni and 20% to 40% Fe in terms of mass percentage.
[0021] More preferably, the composition of the low-grade nickel material includes, by mass percentage, Ni 1% to 3%, Fe 20% to 40%, MgO 5% to 15%, Al2O3 2% to 6%, SiO2 10% to 20%, Cr2O3 0.5% to 3%, and water 25% to 40%.
[0022] Optionally, the water in the above-mentioned low-grade nickel material composition includes physical water and crystal water.
[0023] Under the specific oxidation roasting conditions of step 1, the water in the solid solution of the low-grade nickel material (120-200°C), the iron oxide compound bonded with OH- (about 300°C), the water in the gangue bonded with H2O such as kaolin and beryllite (about 500°C), adsorbed water, goethite crystal water, serpentine structural water, forsterite and other various water can all be effectively removed, so that the final ore moisture content is less than 3%. In addition, the harmful impurities sulfur and arsenic in the material ore undergo the following oxidation reaction in the drying kiln:
[0024] 2FeS2+11 / 2O2=Fe2O3+4SO2(g)
[0025] 4As+3O2=2As2O3(g)
[0026] The harmful gases generated by the above reaction can be exhausted by controlling a negative pressure of 1 to 5 kPa at the tail of the drying kiln. After step one, the sulfur content is removed by up to 70% to 90%, and the arsenic content is removed by up to 50% to 70%. Preferably, the nickel-iron ore obtained after the treatment in step one comprises the following composition by mass percentage: Ni 1.33% to 5.0%, Fe 26% to 75%, MgO 7% to 25%, SiO2 13% to 33%, Cr2O3 0.7% to 5%, and H2O <3%. That is, under the specific treatment conditions of step one, the low-grade nickel material has the effects of dehydration, oxidation and impurity removal, and preliminary enrichment of nickel-iron.
[0027] Furthermore, in the step 2, the amounts of the first reducing agent, sodium sulfate, water and binder are 5% to 15%, 15% to 25%, 1% to 5% and 3% to 5% based on the mass of the ferronickel ore, respectively; and / or,
[0028] The amount of the second reducing agent is 10% to 30% based on the mass of the ferronickel ore; and / or,
[0029] The first reducing agent is selected from one or more of semi-coke powder, bituminous coal and anthracite; and / or,
[0030] The second reducing agent is selected from one or more of semi-coke powder, bituminous coal, anthracite, combustible gas with CO>60% and coal gas with H2>50%.
[0031] When preparing nickel-iron ore pellets, sodium sulfate is used as a sulfiding agent to inhibit the reduction of iron oxides, thereby reducing iron oxide reduction and increasing the nickel-iron ratio. Sodium sulfate also disrupts the serpentine structure, releasing nickel and maximizing nickel oxide reduction. The released nickel is then concentrated using metallic iron as a carrier, and the nickel is separated along with the iron during magnetic separation.
[0032] Preferably, when a rotary kiln is used for pre-reduction treatment, the rotary kiln is controlled to operate at a slightly positive pressure (2 to 10 mmH2O) and CO>60%.
[0033] Preferably, the binder is expansive soil.
[0034] Furthermore, in the step 2, the pre-reduction temperature is controlled to be 850-1200° C., and the pre-reduction time is 1-4 hours; and / or the diameter of the nickel-iron ore pellets is 3-8 mm.
[0035] A more effective reduction process is achieved by mixing a portion of the reducing agent with the nickel-iron ore to form pellets, and then feeding the remaining portion of the reducing agent and pellets into a rotary kiln for preheating and pre-reduction. The pelletized first reducing agent and the nickel-iron ore have a larger contact area, allowing for better mixing and enhancing the efficiency of the reduction reaction. The second reducing agent oxidizes CO in the rotary kiln, maintaining a reducing atmosphere and releasing some heat for the pre-reduction process.
[0036] Furthermore, under the specific reduction temperature and treatment time in the rotary kiln, the first reducing agent mixed into the pellets is heated and volatilized, releasing the reduction product CO through reduction. This reducing atmosphere is continuously released from the surface of the material bed, forming a strong reducing atmosphere on the surface of the material bed. This strong reducing atmosphere completely isolates the oxidizing and reducing atmospheres in the free space of the rotary kiln, and the reduction reaction proceeds within the material bed under the conditions of the rotary kiln heating. After step two, the reduction degree of the nickel-iron ore can reach 30% to 60%.
[0037] At the same time, in the prior art, when using a rotary kiln for high-temperature calcination, ring formation is usually caused. The formation of ring formation is the accumulation of sintered solid particles in the material layer. They form a ring along a certain point along the length of the kiln. If the conditions causing overheating persist, the ring formation ring will continue to grow until the inner diameter of the kiln is blocked, so the ring formation phenomenon should be avoided and handled as soon as possible. The current way to handle the ring formation problem is to use burning rings, quenching or scrapers for mechanical treatment. The nickel-iron ore pellet particles made in step 2 have better reduction and movement effects under specific reduction conditions. The better gap between the pellets helps the mixing of the reducing agent and the contact of the reducing gas, which can greatly reduce the occurrence of the ring formation problem. For reduction, the larger gap between the pellets is conducive to the full mixing of the reducing gas and the reducing agent, avoiding the problem of poor reduction conditions and poor reduction effect of the lower material layer during the powder reduction process.
[0038] Alternatively, a continuous horizontal mixer can be used for the intensive mixing step. A continuous horizontal mixer has a mixing rotor with a specific circumferential speed and a specially designed geometry. It rotates closely against the inner wall of the horizontal mixing drum, pumping the mixed material from the bottom to the mixing area at the top of the drum, ensuring mixing intensity and material utilization.
[0039] Optionally, the granulation step utilizes an inclined mixing granulator. The mixing drum in an inclined mixing granulator rotates at a specific inclination, and an eccentrically mounted mixing granulation rotor assists the multifunctional scraper in composite granulation. Fine-grained materials roll and rub in the inclined, high-speed rotating drum under the combined effects of gravity, centrifugal force, and friction, forcefully rolling into balls. This has the advantages of short ball formation time, high ball formation rate, and good strength.
[0040] Preferably, the pre-reduction ferronickel ore comprises the following components by mass: Ni 1.5%-5.6%, T.Fe 32%-80%, MgO 8%-26%, SiO2 15%-30%, and Cr2O3 0.8%-5.5%. However, HIsmelt's original technical requirements were Fe > 55%, moisture < 10%, SiO2 < 4%, and MgO < 3%. Therefore, even after steps 1 and 2, the raw materials still did not meet these requirements, necessitating further adjustments to the smelting process.
[0041] Furthermore, the method further includes the steps of crushing, screening, magnetic separation or flotation of the ferronickel ore and / or the high-grade ferronickel raw material.
[0042] Preferably, the particle size of the material obtained after crushing, screening, magnetic separation or flotation does not exceed 6 mm.
[0043] Among them, nickel-iron minerals are effectively separated from non-magnetic gangue through magnetic separation, and the gangue components such as silicon, magnesium and aluminum in the magnetic raw materials are significantly reduced. At the same time, part of the lime and non-magnetic substances in the raw materials are removed to further enrich the nickel iron in the nickel iron ore and improve the nickel iron grade.
[0044] Preferably, after crushing, screening and magnetic separation, the high-grade nickel-iron raw material obtained includes the following components in mass percentage:
[0045] Ni 2.0%~6.0%, T.Fe 50%~85%, MgO 1.2%~10%, SiO2 2%~12%, Cr2O3 1.0%~7.6%.
[0046] It can be seen from this that the high-grade nickel-iron raw materials with the above components can meet the original technical requirements of HIsmelt and can be directly put into the SRV smelting reduction furnace for smelting.
[0047] Furthermore, when the SRV furnace is used for smelting reduction in step three, the molten iron level in the furnace is controlled at 1.5-1.8m, the slag thickness is 1.0-1.5m, the spring height in the furnace is 2.5m-3.5m, and the basicity of the slag is controlled at 0.8-1.0.
[0048] Slag is crucial for ensuring smooth smelting operations, the composition and quality of the molten metal, metal recovery rates, and smelting economic indicators. High levels of oxides such as silicon, magnesium, and aluminum in nickel-containing minerals lead to increased slag temperature and slag viscosity, necessitating narrow control of the slag system during the smelting process. Nickel ore smelting produces a significant amount of slag. To ensure the reduction of metal oxides in the slag, while also ensuring a strong bubbling effect and efficient heat transfer within the furnace, the slag thickness is controlled between 1.0 and 1.5 meters, and the bubbling height within the furnace is maintained between 2.5 and 3.5 meters. The slag tapping interval is shortened based on the raw material injection and smelting efficiency.
[0049] Optionally, the slag produced in the furnace is controlled to have a FeO content of 8% to 10%, an Al2O3 content of 6% to 9%, a CaO content of 10% to 23%, a MgO content of 14% to 16%, and a SiO2 content of 24% to 32%.
[0050] Optionally, the slag composition can be adjusted by adding the flux lime; at the same time, 1% to 5% fluorite can be added before slag discharge to improve the slag fluidity and facilitate the slag discharge operation.
[0051] Optionally, lime is added through the lime pipeline to control the quaternary basicity of the slag to 0.8-1.0; the rest are MgO, gangue and other components in the raw materials, forming a low eutectic phase composed of more diopside, ferromagnesian olivine, etc., to improve the fluidity of the slag and lower the melting point.
[0052] Optionally, when adding high-grade ferronickel raw materials to the SRV furnace, the raw material addition rate is controlled to be 130-180 t / h, and the carrier gas pressure of the spray gun is controlled to be 0.5-0.6 MPa.
[0053] Optionally, the smelting pressure in the furnace is controlled by adjusting the flue cone valve. The pressure in the furnace during the smelting process is 80-100 kPa.
[0054] Optionally, the molten pool temperature is controlled at 1450-1550°C.
[0055] Optionally, during the smelting process, the oxygen content of the gas blown into the hot air spray gun is controlled to be 25% to 30%, the hot air temperature is 900 to 1100°C, and the hot air injection volume is controlled to be 160,000 to 200,000m 3 / h.
[0056] On the other hand, the present application also provides nickel-containing molten iron obtained by the above method, wherein the nickel-containing molten iron includes the following components by mass fraction: [C] = 3% to 4%, [P] = 0.01% to 0.015%, [S] = 0.01% to 0.03%, [Ni] = 3% to 7%, and [Cr] = 1.5% to 5.6%.
[0057] On the other hand, the present application also provides a use of nickel-containing molten iron obtained by the above method in smelting nickel-containing stainless steel, wherein the nickel-containing stainless steel is prepared by the following method:
[0058] The nickel-containing molten iron is directly added to an AOD argon oxygen refining furnace for blowing, decarburization and reduction treatment, and alloy components are added according to the requirements of the molten steel composition.
[0059] Furthermore, the blowing and decarburization includes:
[0060] The first stage: Control the ratio of argon and oxygen to 1:3-1:4, blow to C < 0.3%, and the blowing intensity is 1.5-2.5m 3 / (t·min); The second stage: control the ratio of argon and oxygen to 1:1~2:1, blow to C<0.03%, and the blowing intensity is 1.0~1.5m 3 / (t·min), end temperature 1650~1750℃;
[0061] The reduction treatment includes: adding 5-8 kg / t of lime and 1-2 kg / t of fluorite, performing slag refining, and adding one or more of silicon-manganese alloy, silicon-ferroalloy, chromium-ferroalloy and nickel-ferroalloy according to the requirements of molten steel composition.
[0062] The beneficial effects of this application include but are not limited to:
[0063] 1. The nickel-containing metal smelting method provided in this application utilizes the HIsmelt smelting reduction technology to smelt low-grade nickel-containing ore, capable of producing nickel-containing molten iron with a nickel content of 4% to 6%, effectively reducing energy consumption and costs, achieving low-cost and efficient smelting of laterite nickel ore and effective utilization of nickel resources;
[0064] 2. The nickel-containing metal smelting method provided in this application optimizes the preheating and pre-reduction processes of the raw materials, making the composition of the raw materials entering the furnace more suitable for the requirements of the HIsmelt reduction technology, especially effectively improving the reduction degree of nickel iron in the raw materials, further improving the smelting efficiency of nickel-containing molten iron;
[0065] 3. The nickel-containing metal smelting method provided in this application, by changing the physical and chemical state of nickel-containing iron ore raw materials and adding them to a rotary kiln in the form of granular pellets for pre-reduction, not only improves the reduction effect of the raw materials and increases the nickel-iron content, but also significantly improves the nickel-iron quality of the raw materials entering the furnace, while avoiding the risk of powdered raw materials forming rings in the rotary kiln, thereby achieving low-cost, high-quality, and continuous smelting of nickel-containing molten iron;
[0066] 4. The nickel-containing molten iron obtained by the nickel-containing metal smelting method provided in this application can be directly used in the AOD refining furnace to smelt high-quality nickel-containing stainless steel, and then the component content can be adjusted according to the standard requirements of stainless steel. This not only reduces the consumption of alloying elements, but also alleviates the alloy dissolution process and improves the smelting efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0068] FIG1 is a flow chart of a smelting process of nickel-containing molten iron and nickel-containing stainless steel provided in one embodiment of the present application;
[0069] FIG2 is a schematic diagram of a production line for implementing the smelting process of nickel-containing molten iron and nickel-containing stainless steel provided in this application.
[0070] Implementation Method
[0071] In order to more clearly illustrate the overall concept of the application, the overall scheme of the application is described in detail below in the form of embodiments. In the description below, a large amount of specific details are provided so that a more thorough understanding of the application is provided. However, it will be apparent to those skilled in the art that the application can be implemented without the need for one or more of these details. In other examples, in order to avoid confusion with the application, some technical features well known in the art are not described.
[0072] Unless otherwise specified, all raw material components in the following examples can be purchased from commercial sources, the experimental instruments used are all experimental instruments known in the art, and the testing methods are all methods known in the art.
[0073] Example 1
[0074] This embodiment provides a method for smelting nickel-containing metal, which comprises the following steps:
[0075] Step 1: Mix laterite nickel ore (composition: Ni 1.5%-2%, Fe 30%-35%, MgO 8%-10%, Al2O3 3%-5%, SiO2 12%-15%, Cr2O3 0.5%-0.8%, physical water and crystal water 30%-40% in total) with 3% lime, and then use a 100m long drying kiln for oxidation roasting, using coal gas as a heat source, using 5kPa negative pressure exhaust at the kiln tail, controlling the kiln temperature at 850°C, and the oxygen content at 40%;
[0076] The dehydrated and oxidized material is crushed, magnetically separated or floated to control the particle size to be less than 6 mm, and lime, gangue and non-magnetic substances in the raw material are removed to avoid back-sulfurization, thereby obtaining a nickel iron ore material, wherein the nickel iron ore material has a composition of Ni=2.5%, Fe=51%, MgO=13%, SiO2=20%, Cr2O3=0.83%, a water content of less than 3%, 80% S removal, and 65% As removal;
[0077] Step 2: Add 15% semi-coke powder, 15% sodium sulfate, 3% water and 4% expansive soil based on the mass of the above-mentioned nickel iron ore, and use a continuous horizontal mixer to vigorously mix. After the mixing degree reaches more than 95%, use an inclined mixing granulator to granulate to obtain granular pellets with a particle size of 5 mm, add the granular pellets to a rotary kiln with a length of 100 m, and then mix 20% bituminous coal for pre-reduction treatment, and control the kiln head of the rotary kiln to maintain a positive pressure of 5 mmH2O. The temperature in the high temperature zone of the kiln is 1000 ° C and the treatment is carried out for 2 hours;
[0078] The preheated and pre-reduced material is crushed and magnetically separated until the particle size is less than 6 mm, and lime, gangue and non-magnetic substances in the raw ore are removed to obtain a high-grade ferronickel raw material, wherein the composition of the high-grade ferronickel raw material is Ni=3.2%, T.Fe=61%, MgO=7%, SiO2=8%, Cr2O3=1.5%, and the degree of reduction is 40%;
[0079] Step 3: Use the HIsmelt process to smelt the above high-grade nickel iron raw materials. The specific steps and parameters are as follows:
[0080] The high-grade nickel iron raw material is passed through the hot ore hopper into the high-temperature ore bin, and is connected to the smelting reduction furnace through a pneumatic conveying pipeline, and is injected into the smelting reduction furnace through the injection pipeline for smelting reduction;
[0081] The addition rate of high-grade nickel iron raw materials is controlled at 150t / h, the carrier gas pressure of the spray gun is 0.6Mpa, and the molten iron level in the furnace is controlled at 1.5-1.8m;
[0082] The pulverized coal enters the smelting reduction furnace through the pulverized coal injection pipeline. In view of the characteristics of nickel iron ore smelting, a lime and fluorite injection system is set up. The system is equipped with a separate conveying control device, and the conveying pipeline is mixed with the material spray gun in front of the furnace.
[0083] Oxygen-rich hot air is blown into the furnace from the top swirl gun to provide heat and oxygen for the reaction in the furnace. The oxygen content of the gas blown into the hot air gun is controlled to be 25%, the hot air temperature is 900℃, and the hot air injection volume is controlled to be 200000m 3 / h;
[0084] Since nickel ore smelting produces a lot of slag, the slag thickness is controlled at 1.0 to 1.3 m to ensure the spring height in the furnace is 2.5 to 3 m.
[0085] The slag produced in the furnace has a controlled FeO content of 8% to 10%, an Al2O3 content of 6% to 9%, a CaO content of 10% to 23%, a MgO content of 14% to 16%, and a SiO2 content of 24% to 32%. The slag composition is adjusted by adding lime flux, which is added through a lime pipeline to control the slag quaternary basicity to 0.8 to 1.0. The remainder is MgO, gangue, and other components in the raw materials, forming a large amount of low-melting-point phases composed of diopside and mafic olivine, thereby improving the slag fluidity and lowering the melting point.
[0086] Adding 1% to 5% fluorite before slag tapping can improve slag fluidity and facilitate slag tapping operations;
[0087] The smelting pressure in the furnace is controlled by adjusting the flue cone valve. The pressure in the furnace during the smelting process is 80-100kPa.
[0088] Control the molten pool temperature at 1450-1550℃;
[0089] The slag and iron in the furnace are separated into layers, the slag is discharged through the slag outlet, and the molten iron is discharged through the lower iron outlet to obtain nickel-containing molten iron.
[0090] Example 2
[0091] The smelting method of this embodiment is substantially the same as that of embodiment 1, with the only difference being that in step 2, the pre-reduction temperature of the rotary kiln is controlled to be 900° C., and the pre-reduction treatment time is 4 hours.
[0092] Example 3
[0093] The smelting method of this embodiment is substantially the same as that of embodiment 1, with the only difference being that in step 2, the pre-reduction temperature of the rotary kiln is controlled to be 1100° C., and the pre-reduction treatment time is 1 hour.
[0094] Example 4
[0095] The smelting method of this embodiment is substantially the same as that of embodiment 1, with the only difference being that the second reducing agent is semi-coke powder, and the amount used is 10% of the mass of the pellets.
[0096] Example 5
[0097] The smelting method of this embodiment is substantially the same as that of embodiment 1, with the only difference being that the second reducing agent is coke oven gas (containing 55% to 60% hydrogen) and the amount used is 30% of the mass of the pellets.
[0098] Comparative Example 1
[0099] The smelting method of this comparative example is substantially the same as that of Example 1, differing only in that the pre-reduction treatment in step 2 is performed by placing the ferronickel ore powder and 35% bituminous coal by mass into a rotary kiln for pre-reduction treatment at 1000°C for 2 hours. In other words, the ferronickel ore and a portion of the reducing agent are not pelletized for pre-reduction.
[0100] The components of the high-grade ferronickel raw materials obtained in the above examples and comparative examples were measured, and the results are shown in Table 1.
[0101] Table 1
[0102] Example Ni / %T.Fe / %MgO / %SiO2 / %Cr2O3 / %Reduction degree Example 1 3.26 17.0 8.0 1.5 40% Example 2 2.55 55.09.0 1.2 30% Example 3 2.65 8 6.5 8.4 1.2 33% Example 4 3.15 9 6.37.0 1.4 36% Example 5 3.86 6 4.3 5.2 1.8 50% Comparative Example 1 1.84 5 11.6 13.2 0.7 12%
[0103] It can be seen from the data in Table 1 that compared with Comparative Example 1, the nickel-iron raw materials obtained by the smelting methods provided in Examples 1 to 5 have a significantly improved degree of reduction, and the enrichment effect of nickel-iron is significantly improved. The high-grade nickel-iron raw materials obtained are more suitable for smelting reduction smelting using the HIsmelt process, and can be used to directly prepare high-grade nickel-containing iron water.
[0104] Compared with the comparative example, the smelting method of the embodiment reduces the slag energy loss by 42% to 65% by improving the grade of nickel-iron raw materials and reducing the gangue content, improves the smelting efficiency by 24% to 48% when high-grade raw materials are fed into the furnace, and effectively utilizes the raw materials by more than 30%, thereby realizing the efficient smelting of low-grade nickel-iron raw materials. It plays an important role in the development and utilization of low-grade laterite nickel ore, nickel-containing ore, nickel-containing slag, etc.; at the same time, the enrichment and smelting of metal elements such as Ni and Cr in the raw materials provide higher high-value metal elements for the development of stainless steel products, which can significantly reduce the addition of alloying elements in subsequent processing and reduce production costs.
[0105] Among them, the nickel-containing molten iron obtained by smelting the method provided in Examples 1 to 5 includes the following components by mass fraction: [C] = 3.5% to 4%, [P] = 0.01% to 0.015%, [S] = 0.01% to 0.03%, [Ni] = 3.5% to 5.5%, and [Cr] = 1.8% to 2.6%.
[0106] Example 6
[0107] This embodiment provides a method for preparing nickel-containing stainless steel, comprising the following steps:
[0108] The nickel-containing molten iron having the above mass fraction components prepared by the method provided in the above embodiment is directly added to an AOD argon oxygen refining furnace for blowing, decarburization and reduction treatment to prepare nickel-containing stainless steel water. The preparation process specifically includes:
[0109] Oxidation period: The first stage: control the ratio of argon and oxygen to 1:3-1:4, blow to C<0.3%, and the blowing intensity is 1.5-2.5m 3 / (t·min); The second stage: control the ratio of argon and oxygen to 1:1~2:1, blow to C<0.03%, and the blowing intensity is 1.0~1.5m 3 / (t·min), end temperature 1650~1750℃;
[0110] Reduction period: Add 5-8 kg / t of lime and 1-2 kg / t of fluorite for slag refining, and add one or more of silicon-manganese alloy, ferrosilicon alloy, ferrochrome alloy and nickel-iron alloy according to the requirements of molten steel composition.
[0111] In one embodiment, the nickel-containing molten iron can be used to prepare 201 series, 302 series and 304 series stainless steels. The component content requirements of 201 series, 302 series and 304 series stainless steels are shown in Table 2:
[0112] Table 2
[0113] Example C / %Si / %Mn / %P / %S / %Cr / %Ni / %201 stainless steel ≤0.15 ≤1.0 5.5~7.5 ≤0.06 ≤0.030 16~18 3.5~5.5 302 stainless steel ≤0.15 ≤1.0 ≤2.0 ≤0.035 ≤0.030 17~198~10 304 stainless steel ≤0.08 ≤1.0 ≤2.0 ≤0.045 ≤0.030 18~208~11
[0114] During the reduction phase, ferromanganese and ferrochromium are added to nickel-containing molten iron to adjust the compositional content, resulting in 201 series stainless steel. Ferrochromium and ferronickel are added to nickel-containing molten iron to adjust the compositional content, resulting in 302 series or 304 series stainless steel. For example, the nickel-containing molten iron prepared in Examples 1, 3, and 5 was made into stainless steel #1, stainless steel #2, and stainless steel #3, respectively, which met the compositional requirements for 201 stainless steel, 302 stainless steel, and 304 stainless steel, respectively. The specific results are shown in Table 3:
[0115] Table 3
[0116] Example CSiMnPSCrNi1#(201)0.050.355.100.0100.02116.85.22#(302)0.030.321.320.0120.02317.28.13#(304)0.020.421.350.0150.01818.49.1
[0117] As shown in Table 3, the nickel-containing molten iron produced by the smelting method provided in this application can be directly used to refine and prepare various types of stainless steel. While fully utilizing nickel ore resources, it significantly improves the smelting efficiency and quality of nickel-containing stainless steel, reduces the amount of alloy added, and alleviates the pressure of alloy dissolution. Compared with high alloy addition, to ensure the efficiency and quality of smelting, a separate alloy melting furnace is required, which greatly reduces production costs and process flow.
[0118] The foregoing is merely an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application should all be included within the scope of the claims of the present application.
Claims
1. A method for smelting nickel-containing metals, characterized in that: The following steps are involved: Step 1: mixing low-grade nickel material with lime and performing oxidative roasting to obtain nickel iron ore; Step 2: After vigorously mixing the nickel iron ore with a first reducing agent, sodium sulfate, water and a binder, granulating to obtain nickel iron ore pellets, adding the nickel iron ore pellets to a rotary kiln, and then mixing with a second reducing agent to perform a pre-reduction treatment to obtain a high-grade nickel iron raw material; Step 3: The high-grade nickel-iron raw material is subjected to smelting reduction using an SRV furnace to obtain the nickel-containing iron water.
2. The nickel-containing metal smelting method according to claim 1, characterized in that: The conditions of the oxidation roasting in step 1 are: controlling the roasting temperature to be 650° C. to 900° C., the oxygen content to be 30% to 50%, and the time to be 40 to 60 min; and / or, The amount of lime used is 3% to 10% based on the mass of the low-grade nickel material.
3. The method for smelting nickel-containing metal according to claim 1, characterized in that: The low-grade nickel material is selected from one or more of laterite nickel ore, nickel slag, nickel-containing oxide slag and nickel-containing iron filings.
4. The method for smelting nickel-containing metal according to claim 1, characterized in that: In the step 2, the amounts of the first reducing agent, sodium sulfate, water and binder are 5% to 15%, 15% to 25%, 1% to 5% and 3% to 5% based on the mass of the ferronickel ore respectively; and / or, The amount of the second reducing agent is 10% to 30% based on the mass of the ferronickel ore; and / or, The first reducing agent is selected from one or more of semi-coke powder, bituminous coal and anthracite; and / or, The second reducing agent is selected from one or more of semi-coke powder, bituminous coal, anthracite, combustible gas with CO>60% and coal gas with H2>50%.
5. The method for smelting nickel-containing metal according to claim 1, characterized in that: In the step 2, the pre-reduction temperature is controlled to be 850-1200° C. and the pre-reduction time is controlled to be 1-4 hours; and / or, The diameter of the nickel iron ore pellets is 3 to 8 mm.
6. The method for smelting nickel-containing metal according to claim 1, characterized in that: The method further includes the steps of crushing, screening, magnetic separation or flotation of the ferronickel ore and / or the high-grade ferronickel raw material.
7. The method for smelting nickel-containing metal according to claim 1, characterized in that: When the SRV furnace is used for smelting reduction in step three, the molten iron level in the furnace is controlled at 1.5-1.8m, the slag thickness is 1.0-1.5m, the spring height in the furnace is 2.5m-3.5m, and the basicity of the slag is controlled at 0.8-1.
0.
8. Nickel-containing molten iron obtained by the method according to any one of claims 1 to 7, characterized in that The nickel-containing molten iron comprises the following components in mass fractions: [C]=3%-4%, [P]=0.01%-0.015%, [S]=0.01%-0.03%, [Ni]=3%-7%, and [Cr]=1.5%-5.6%.
9. Use of nickel-containing molten iron obtained by the method according to any one of claims 1 to 7 in smelting nickel-containing stainless steel, characterized in that: The nickel-containing stainless steel is prepared by the following method: The nickel-containing molten iron is directly added to an AOD argon oxygen refining furnace for blowing, decarburization and reduction treatment, and alloy components are added according to the requirements of the molten steel composition.
10. The use according to claim 9, characterized in that The blowing decarburization comprises: The first stage: Control the ratio of argon and oxygen to 1:3-1:4, blow to C < 0.3%, and the blowing intensity is 1.5-2.5m 3 / (t·min); The second stage: control the ratio of argon and oxygen to 1:1~2:1, blow to C<0.03%, and the blowing intensity is 1.0~1.5m 3 / (t·min), end temperature 1650~1750℃; The reduction treatment includes: adding 5-8 kg / t of lime and 1-2 kg / t of fluorite, performing slag refining, and adding one or more of silicon-manganese alloy, silicon-ferroalloy, chromium-ferroalloy and nickel-ferroalloy according to the requirements of molten steel composition.