Photosensitive resin composition, photosensitive element, method for forming resist pattern, and method for producing circuit board

MYPI2025004148A0Undetermined Publication Date: 2024-10-03RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004148
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional photosensitive resin compositions face challenges in achieving high sensitivity, resolution, adhesion, and releasability, particularly in thick film applications for forming resist patterns on wiring boards, which affects production efficiency and pattern quality.

Method used

A photosensitive resin composition incorporating a binder polymer, a photopolymerizable compound, a photopolymerization initiator containing a hexaarylbiimidazole compound and an N-phenylglycine compound, and a sensitizer with an anthracene compound, optimized with specific mass ratios and components to enhance sensitivity, resolution, and releasability.

Benefits of technology

The composition achieves improved sensitivity, resolution, adhesion, and releasability, enabling faster exposure times, efficient resist pattern formation, and effective stripping, suitable for high-density wiring board manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004148_DRAWING_001
    Figure PI2025004148_DRAWING_001
  • Figure PI2025004148_DRAWING_002
    Figure PI2025004148_DRAWING_002
Patent Text Reader

Abstract

A photosensitive resin composition contains a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a sensitizer, in which the photopolymerization initiator contains a hexaarylbiimidazole compound and an N-phenylglycine compound, and the sensitizer contains an anthracene compound.
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive resin composition, photosensitive element, method for forming resist pattern, and method for manufacturing wiring board

[0001] The present disclosure relates to a photosensitive resin composition, a photosensitive element, a method for forming a resist pattern, and a method for producing a wiring board.

[0002] In the field of wiring board manufacturing, photosensitive resin compositions and photosensitive elements comprising a layer formed on a support using the photosensitive resin composition (hereinafter also referred to as a "photosensitive layer") are widely used as resist materials used in etching or plating processes.

[0003] A wiring board is manufactured, for example, by the following procedure. First, a photosensitive layer of a photosensitive element is laminated onto a circuit-forming substrate (photosensitive layer forming step). Next, a predetermined portion of the photosensitive layer is exposed to light to form a photocured portion (exposure step). At this time, the support is peeled off before or after exposure. Thereafter, areas of the photosensitive layer other than the photocured portion are removed from the substrate, and a resist pattern, which is a cured product of the photosensitive resin composition, is formed on the substrate (developing step). Next, the obtained resist pattern is used as a resist and subjected to etching or plating to form a conductor pattern on the substrate (circuit forming step), and finally the resist is peeled off and removed (peeling step).

[0004] As an exposure method, a method of exposing through a photomask using a mercury lamp as a light source has been conventionally known. Recently, a direct imaging exposure method called LDI (Laser Direct Imaging) has been used as an exposure method that does not require a photomask, in which digital data of a pattern is directly written onto a photosensitive layer. This direct imaging exposure method has better alignment accuracy than exposure methods using a photomask and can produce high-resolution patterns, and is therefore being introduced for the production of high-density packaging substrates.

[0005] In general, in the exposure step, it is desirable to shorten the exposure time in order to improve production efficiency. However, in the above-mentioned direct writing exposure method, monochromatic light such as a laser is used as a light source, and actinic rays are irradiated while scanning the substrate, so that the exposure time tends to be longer than that of a conventional exposure method using a photomask. Therefore, in order to shorten the exposure time and improve production efficiency, it is necessary to further improve the sensitivity of the photosensitive resin composition.

[0006] In addition, in the stripping step, it is desirable to shorten the resist stripping time in order to improve production efficiency. Therefore, a photosensitive resin composition that has excellent strippability after curing is required. Furthermore, with the recent trend toward higher density wiring boards, a photosensitive resin composition that can form a resist pattern with excellent resolution and adhesion is also required.

[0007] In response to these demands, various photosensitive resin compositions have been investigated. For example, Patent Document 1 discloses a photosensitive resin composition that is excellent in sensitivity and resolution by using a specific photosensitizer. Patent Document 2 discloses a photosensitive resin composition that is excellent in sensitivity and resolution by using a specific alkali-soluble polymer and a compound having an ethylenic double bond.

[0008] JP 2009-003177 A JP 2013-061556 A

[0009] In recent years, there has been a demand for photosensitive resin compositions that can be used in thick film applications (e.g., forming resist patterns with a thickness of 29 μm or more) to form copper pillars that connect IC chips to wiring substrates for semiconductor packages. The thicker the photosensitive layer formed using the photosensitive resin composition, the more difficult it is to uniformly cure it to the bottom, making it difficult to obtain sufficient resolution and adhesion. Furthermore, the thicker the resist pattern formed, the longer it takes for the stripping solution to penetrate, which can result in longer stripping times. Conventional photosensitive resin compositions have room for further improvement in sensitivity, resolution, adhesion, and strippability.

[0010] An object of the present disclosure is to provide a photosensitive layer resin composition that is excellent in sensitivity, resolution, adhesion, and releasability, as well as a photosensitive element, a method for forming a resist pattern, and a method for producing a wiring board that use the same.

[0011] The present disclosure provides the following photosensitive resin composition, photosensitive element, method for forming a resist pattern, and method for manufacturing a wiring board. [1] A photosensitive resin composition containing a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a sensitizer, wherein the photopolymerization initiator contains a hexaarylbiimidazole compound and an N-phenylglycine compound, and the sensitizer contains an anthracene compound. [2] The photosensitive resin composition according to [1] above, wherein the content of the N-phenylglycine compound is 0.06 parts by mass or less per 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound. [3] The photosensitive resin composition according to [1] or [2] above, wherein the photopolymerizable compound contains a (meth)acrylate compound having an alicyclic structure. [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the photopolymerizable compound contains a polyalkylene glycol di(meth)acrylate compound. [5] The photosensitive resin composition according to [4], wherein the content of the polyalkylene glycol di(meth)acrylate is 8% by mass or more and 30% by mass or less, based on the total amount of the photopolymerizable compound. [6] A photosensitive element comprising a support and a photosensitive layer formed on the support using the photosensitive resin composition according to any one of [1] to [5] above. [7] The photosensitive element according to [6] above, wherein the photosensitive layer has a thickness of 29 μm or more. [8] A method for forming a resist pattern, comprising the steps of forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of [1] to [5] above or the photosensitive element according to [6] or [7] above, photocuring a portion of the photosensitive layer, and removing an uncured portion of the photosensitive layer. [9] A method for producing a wiring board, comprising the step of etching or plating a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to [8] above, to form a conductor pattern.

[0012] According to the present disclosure, it is possible to provide a photosensitive layer resin composition that is excellent in sensitivity, resolution, adhesion, and releasability, as well as a photosensitive element, a method for forming a resist pattern, and a method for producing a wiring board that use the same.

[0013] 1A to 1C are schematic cross-sectional views showing a photosensitive element according to an embodiment of the present invention; 1B to 1C are schematic cross-sectional views showing a method for manufacturing a wiring board according to an embodiment of the present invention;

[0014] Hereinafter, embodiments of the present disclosure will be described in detail. In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended effect of that process is achieved. A numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. The term "layer" encompasses not only a structure that is formed over the entire surface when observed in a plan view, but also a structure that is formed on a portion of the surface. "(Meth)acrylic acid" means at least one of "acrylic acid" and the corresponding "methacrylic acid." The same applies to other similar expressions such as (meth)acrylate.

[0015] In this specification, "(poly)oxyethylene group" means an oxyethylene group or a polyoxyethylene group in which two or more ethylene groups are linked by ether bonds. "(poly)oxypropylene group" means an oxypropylene group or a polyoxypropylene group in which two or more propylene groups are linked by ether bonds. "EO-modified" means a compound having a (poly)oxyethylene group. "PO-modified" means a compound having a (poly)oxypropylene group. "EO-PO-modified" means a compound having a (poly)oxyethylene group and / or a (poly)oxypropylene group.

[0016] In this specification, when a composition contains a plurality of substances corresponding to each component, the amount of each component refers to the total amount of the plurality of substances present in the composition, unless otherwise specified. In this specification, the term "solid content" refers to the non-volatile content of the photosensitive resin composition excluding volatile substances. In other words, the term "solid content" refers to components other than the solvent that remain without volatilizing during drying of the photosensitive resin composition, as described below, and includes components that are liquid, syrup-like, or waxy at room temperature (25°C).

[0017] <Photosensitive Resin Composition> The photosensitive resin composition according to this embodiment contains a binder polymer (hereinafter also referred to as "component (A)"), a photopolymerizable compound (hereinafter also referred to as "component (B)"), a photopolymerization initiator (hereinafter also referred to as "component (C)"), and a sensitizer (hereinafter also referred to as "component (D)"). The component (C) contains a hexaarylbiimidazole compound and an N-phenylglycine compound, and the component (D) contains an anthracene compound. By using such a specific photopolymerization initiator and a specific sensitizer in combination, the photosensitive resin composition according to this embodiment has excellent sensitivity, resolution, adhesion, and releasability, and is suitable for use in direct imaging exposure methods and thick film applications. Each component will be described below.

[0018] Component (A): Binder Polymer The photosensitive resin composition contains one or more types of component (A). Examples of component (A) include acrylic resins, styrene resins, epoxy resins, amide resins, amide-epoxy resins, alkyd resins, and phenolic resins.

[0019] From the viewpoint of alkali developability, the component (A) may contain an acrylic resin. The acrylic resin is a resin having structural units (monomer units) derived from a (meth)acryloyl group-containing compound.

[0020] The (meth)acryloyl group-containing compound is a compound containing a (meth)acryloyl group. Examples of the (meth)acryloyl group-containing compound include hydroxyalkyl (meth)acrylate, (meth)acrylic acid, (meth)acrylic acid alkyl ester, (meth)acrylic acid aryl ester, (meth)acrylic acid cycloalkyl ester, acrylamide such as diacetone acrylamide, (meth)acrylic acid tetrahydrofurfuryl ester, (meth)acrylic acid dimethylaminoethyl ester, (meth)acrylic acid diethylaminoethyl ester, (meth)acrylic acid glycidyl ester, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, α-bromoacrylic acid, α-chloroacrylic acid, β-furyl (meth)acrylic acid, and β-styryl (meth)acrylic acid.

[0021] The acrylic resin may be, for example, a polymer (a) having at least one unit selected from the group consisting of a hydroxyalkyl (meth)acrylate unit, a (meth)acrylic acid unit, a (meth)acrylic acid alkyl ester unit, and a (meth)acrylic acid aryl ester unit.

[0022] The hydroxyalkyl (meth)acrylate unit is a structural unit derived from a hydroxyalkyl (meth)acrylate. Examples of the hydroxyalkyl (meth)acrylate include hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, and hydroxyhexyl (meth)acrylate. When the alkyl moiety in the hydroxyalkyl (meth)acrylate unit has 3 or more carbon atoms, the hydroxyalkyl (meth)acrylate unit may have a branched structure.

[0023] When the polymer (a) has a hydroxyalkyl (meth)acrylate unit, the content of the hydroxyalkyl (meth)acrylate unit may be 0.5% by mass or more, 0.75% by mass or more, or 1.0% by mass or more, based on the total amount of monomer units constituting the polymer (a), from the viewpoint of dispersibility, and may be 20% by mass or less, 15% by mass or less, or 8% by mass or less, from the viewpoint of water absorbency.

[0024] The (meth)acrylic acid unit is a structural unit derived from (meth)acrylic acid. When the polymer (a) has the (meth)acrylic acid unit, the content of the (meth)acrylic acid unit may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more, or may be 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, or 30% by mass or less, based on the total amount of the monomer units constituting the polymer (a), from the viewpoints of resolution and adhesion.

[0025] The (meth)acrylic acid alkyl ester unit is a structural unit derived from a (meth)acrylic acid alkyl ester. The alkyl group of the (meth)acrylic acid alkyl ester may be, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, or a structural isomer thereof, or may be an alkyl group having 1 to 4 carbon atoms from the viewpoint of releasability.

[0026] When the polymer (a) has (meth)acrylic acid alkyl ester units, the content of the (meth)acrylic acid alkyl ester units may be 1 mass % or more, 2 mass % or more, 3 mass % or more, or 4 mass % or more, based on the total amount of monomer units constituting the polymer (a), from the viewpoint of releasability, and may be 50 mass % or less, 30 mass % or less, 10 mass % or less, 8 mass % or less, or 6 mass % or less, from the viewpoint of resolution and adhesion.

[0027] The (meth)acrylic acid aryl ester unit is a structural unit derived from a (meth)acrylic acid aryl ester. Examples of the (meth)acrylic acid aryl ester include benzyl (meth)acrylate, phenyl (meth)acrylate, and naphthyl (meth)acrylate. When the polymer (a) has a (meth)acrylic acid aryl ester unit, the content of the (meth)acrylic acid aryl ester unit may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, or 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, 30% by mass or less, or 25% by mass or less, based on the total amount of the monomer units constituting the polymer (a), from the viewpoint of resolution and adhesion.

[0028] The polymer (a) may further have a structural unit derived from a monomer other than the (meth)acryloyl group-containing compound. The other monomer may be one type or two or more types.

[0029] Examples of other monomers include styrene or styrene derivatives, acrylonitrile, vinyl alcohol ethers such as vinyl n-butyl ether, maleic acid, maleic anhydride, maleic acid monoesters such as monomethyl maleate, monoethyl maleate, and monoisopropyl maleate, fumaric acid, cinnamic acid, α-cyanocinnamic acid, itaconic acid, crotonic acid, and propiolic acid. Examples of styrene derivatives include vinyltoluene and α-methylstyrene.

[0030] When the polymer (a) has a structural unit derived from styrene or a styrene derivative (hereinafter also referred to as a "styrene or styrene derivative unit"), the content of the styrene or styrene derivative unit, based on the total amount of the monomer units constituting the polymer (a), may be 40% by mass or more or 45% by mass or more from the viewpoint of resolution, and may be 90% by mass or less, 85% by mass or less, or 80% by mass or less from the viewpoint of developability.

[0031] The component (A) may contain a binder polymer other than the polymer (a), or may consist solely of the polymer (a). From the viewpoints of adhesion and resolution, the content of the polymer (a) in the component (A) may be 50 to 100 mass % or 80 to 100 mass % based on the total amount of the component (A).

[0032] The acid value of polymer (a) may be 100 mgKOH / g or more, 120 mgKOH / g or more, 140 mgKOH / g or more, or 150 mgKOH / g or more from the viewpoint of developability, and may be 250 mgKOH / g or less, 240 mgKOH / g or less, or 230 mgKOH / g or less from the viewpoint of adhesion (developer resistance) of the cured product of the photosensitive resin composition. The acid value of polymer (a) can be adjusted by the content of structural units (e.g., (meth)acrylic acid units) constituting polymer (a). When component (A) contains a binder polymer other than polymer (a), the acid value of the other binder polymer may also be within the above range.

[0033] The weight average molecular weight (Mw) of the polymer (a) may be 10,000 or more, 15,000 or more, 20,000 or more, 25,000 or more, 30,000 or more, 35,000 or more, or 40,000 or more from the viewpoint of adhesion (developer resistance) of the cured product of the photosensitive resin composition and ease of forming a thick film resist pattern, and may be 100,000 or less, 80,000 or less, 60,000 or less, or 50,000 or less from the viewpoint of developability. The dispersity (Mw / Mn) of the polymer (a) may be, for example, 1.0 or more or 1.5 or more, and from the viewpoint of adhesion and resolution, may be 3.0 or less or 2.5 or less. When the (A) component contains a binder polymer other than the polymer (a), the Mw of the other binder polymer may also be within the above range.

[0034] The weight average molecular weight and dispersity can be measured, for example, by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene. More specifically, they can be measured under the conditions described in the Examples. For compounds with low molecular weights, if it is difficult to measure the weight average molecular weight using the above-mentioned method, the molecular weight can be measured by another method and the average can be calculated.

[0035] The content of the component (A), based on the total solid content of the photosensitive resin composition, may be 20% by mass or more, 30% by mass or more, or 40% by mass or more from the viewpoint of film formability, and may be 90% by mass or less, 80% by mass or less, 70% by mass or less, or 65% by mass or less from the viewpoint of sensitivity and resolution.

[0036] The content of the (A) component may be 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, 45 parts by mass or more, 50 parts by mass or more, or 55 parts by mass or more, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, from the viewpoint of film formability, and may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, from the viewpoint of sensitivity and resolution.

[0037] Component (B): Photopolymerizable Compound The photosensitive resin composition contains one or more components (B). The component (B) may be any compound that can be polymerized by light, such as a compound having an ethylenically unsaturated bond.

[0038] From the viewpoints of alkaline developability, resolution, and strippability, the component (B) may contain a bisphenol A type (meth)acrylate compound (hereinafter also referred to as "component (b1)"). Examples of the component (b1) include 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolybutoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane. From the viewpoints of resolution and strippability, the component (B) may contain 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane. Examples of 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane include (2,2-bis(4-((meth)acryloxypentaethoxy)phenyl)propane). As the 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, a compound having 10 or more oxyethylene groups may be used, or a compound having less than 10 oxyethylene groups may be used, or a compound having 10 or more oxyethylene groups and a compound having less than 10 oxyethylene groups may be used in combination.

[0039] From the viewpoint of resist resolution, the amount of component (b1) may be 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, or 90 mass % or more, based on the total amount of component (B). Component (B) may consist solely of component (b1).

[0040] From the viewpoints of developability, resolution, adhesion, and releasability, the component (B) may contain a polyalkylene glycol di(meth)acrylate compound (hereinafter also referred to as "component (b2)"; excluding the component (b1) above). Examples of the component (b2) include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and EO-modified polypropylene glycol di(meth)acrylate. The component (b2) may contain EO-modified polypropylene glycol di(meth)acrylate.

[0041] From the viewpoint of developability, the content of the component (b2) may be 8% by mass or more, 10% by mass or more, 12% by mass or more, 14% by mass or more, 16% by mass or more, 18% by mass or more, 20% by mass or more, or 22% by mass or more, based on the total amount of the component (B). From the viewpoints of releasability, adhesion, and resolution, the content of the component (b2) may be 8% by mass or more, 10% by mass or more, 12% by mass or more, 14% by mass or more, 16% by mass or more, or 18% by mass or more, based on the total amount of the component (B), and may be 30% by mass or less, 28% by mass or less, 26% by mass or less, 24% by mass or less, 22% by mass or less, 20% by mass or less, or 19% by mass or less. The content of the component (b2) may be 8% to 30% by mass, based on the total amount of the component (B).

[0042] From the viewpoints of sensitivity, developability, and adhesion, component (B) may contain a compound having three or more (meth)acryloyl groups (hereinafter also referred to as component (b3) (excluding components (b1) and (b2) above). Examples of component (b3) include trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-PO-modified trimethylolpropane tri(meth)acrylate, EO-modified pentaerythritol tetra(meth)acrylate, EO-modified ditrimethylolpropane tetra(meth)acrylate, EO-modified dipentaerythritol hexa(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate. Component (b3) may contain EO-modified trimethylolpropane tri(meth)acrylate. The content of the (b3) component may be 5% by mass or more, 10% by mass or more, or 15% by mass or more, and may be 25% by mass or less, 20% by mass or less, or 18% by mass or less, based on the total amount of the (B) component.

[0043] From the viewpoint of releasability, the component (B) may contain a (meth)acrylate compound having an alicyclic structure (hereinafter also referred to as the "component (b4)"; excluding the components (b1), (b2), and (b3)). Examples of the component (b4) include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, cyclopentanyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. The component (b4) may contain dicyclopentanyl (meth)acrylate. The content of the component (b4) may be 1% by mass or more, 2% by mass or more, 3% by mass or more, 5% by mass or more, or 6% by mass or more, and may be 15% by mass or less, 10% by mass or less, or 8% by mass or less, based on the total amount of the component (B).

[0044] From the viewpoint of peelability and developability, the component (B) may be used in combination with at least one of the components (b2) and (b3) and the component (b4). From the viewpoint of even better peelability, the component (B) may be used in combination with the component (b2) and the component (b4). From the viewpoint of even better sensitivity, developability, and adhesion, the component (B) may be used in combination with the component (b3) and the component (b4). When the component (b2) and the component (b4) are used in combination, the mass ratio of (b2) / (b4) may be 1.5 or more, 2.0 or more, or 2.2 or more. When the component (b3) and the component (b4) are used in combination, the mass ratio of (b3) / (b4) may be 1.5 or more, 2.0 or more, or 2.2 or more.

[0045] The photosensitive resin composition may contain, as the component (B), a photopolymerizable compound other than the above-mentioned components (b1) to (b4).

[0046] Examples of other photopolymerizable compounds include urethane monomers, nonylphenoxy polyethyleneoxy acrylates, phthalic acid compounds, (meth)acrylic acid alkyl esters, and photopolymerizable compounds having at least one cationically polymerizable cyclic ether group in the molecule (such as oxetane compounds). From the viewpoints of resolution, adhesion, resist shape, and removability, the other photopolymerizable compound may be at least one selected from the group consisting of urethane monomers, nonylphenoxy polyethyleneoxy acrylates, and phthalic acid compounds.

[0047] Examples of nonylphenoxy polyethyleneoxyacrylates include nonylphenoxytriethyleneoxyacrylate, nonylphenoxytetraethyleneoxyacrylate, nonylphenoxypentaethyleneoxyacrylate, nonylphenoxyhexaethyleneoxyacrylate, nonylphenoxyheptaethyleneoxyacrylate, nonylphenoxyoctaethyleneoxyacrylate, nonylphenoxynonaethyleneoxyacrylate, nonylphenoxydecaethyleneoxyacrylate, and nonylphenoxyundecaethyleneoxyacrylate.

[0048] Examples of phthalic acid compounds include γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate (also known as 3-chloro-2-hydroxypropyl-2-(meth)acryloyloxyethyl phthalate), β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, and β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate.

[0049] When the component (B) contains other photopolymerizable compounds, the content of the other photopolymerizable compounds may be 1% by mass or more, 3% by mass or more, or 5% by mass or more, and may be 25% by mass or less, 15% by mass or less, or 10% by mass or less, based on the total amount of the component (B), from the viewpoints of resolution, adhesion, resist shape, and removability.

[0050] From the viewpoints of adhesion and resolution, the component (B) may include, among the above-mentioned compounds, a compound having a total of 2 to 40 oxyethylene groups (EO groups) and / or oxypropylene groups (PO groups) in the molecule. From the viewpoints of adhesion and resolution, the total number of EO groups and / or PO groups may be 2 to 40 or 2 to 30.

[0051] The content of the component (B) may be 3% by mass or more, 10% by mass or more, or 25% by mass or more, based on the total solid content of the photosensitive resin composition, from the viewpoint of sensitivity and resolution, and may be 70% by mass or less, 60% by mass or less, or 50% by mass or less, from the viewpoint of film formability.

[0052] Component (C): Photopolymerization Initiator The photosensitive resin composition contains one or more types of component (C). Component (C) contains a hexaarylbiimidazole compound and an N-phenylglycine compound. When a hexaarylbiimidazole compound is used as component (C), the photosensitive resin composition can achieve good resolution and resist pattern formability, but the sensitivity may be reduced. The present inventors have found that by using a hexaarylbiimidazole compound in combination with an N-phenylglycine compound, excellent resolution can be achieved, and sensitivity, adhesion, and releasability can be improved.

[0053] From the viewpoints of sensitivity, resolution, adhesion, and strippability, the hexaarylbiimidazole compound may be a 2,4,5-triarylimidazole dimer. Examples of the 2,4,5-triarylimidazole dimer include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-bis-(m-methoxyphenyl)imidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer.

[0054] From the viewpoints of sensitivity, resolution, adhesion, and releasability, the content of the hexaarylbiimidazole compound may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1.0 parts by mass or more, 3.0 parts by mass or more, 4.0 parts by mass or more, or 4.5 parts by mass or more, relative to 100 parts by mass of the total amount of the component (A) and the component (B), and may be 10 parts by mass or less, 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, or 6 parts by mass or less.

[0055] Examples of the N-phenylglycine compound include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine. From the viewpoints of sensitivity, resolution, adhesion, and strippability, the N-phenylglycine compound may contain N-phenylglycine.

[0056] From the viewpoint of achieving better sensitivity, releasability, and adhesion, the content of the N-phenylglycine compound may be 0.010 parts by mass or more, 0.015 parts by mass or more, 0.020 parts by mass or more, 0.025 parts by mass or more, 0.028 parts by mass or more, or 0.030 parts by mass or more, relative to 100 parts by mass of the total amount of the component (A) and the component (B); from the viewpoint of achieving better resolution, the content of the N-phenylglycine compound may be 0.060 parts by mass or less, 0.055 parts by mass or less, 0.050 parts by mass or less, 0.045 parts by mass or less, 0.040 parts by mass or less, or 0.035 parts by mass or less. From the viewpoints of sensitivity, resolution, adhesion, and releasability, the content of the N-phenylglycine compound may be 0.010 parts by mass to 0.060 parts by mass, 0.015 parts by mass to 0.050 parts by mass, 0.020 parts by mass to 0.040 parts by mass, 0.025 parts by mass to 0.040 parts by mass, or 0.025 parts by mass to 0.035 parts by mass, relative to 100 parts by mass of the total amount of the component (A) and the component (B).

[0057] The component (C) may consist solely of a hexaarylbiimidazole compound and an N-phenylglycine compound, or may further contain a photopolymerization initiator other than a hexaarylbiimidazole compound and an N-phenylglycine compound, as long as the effects of the present disclosure are not impaired.

[0058] The content of the (C) component may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1.0 parts by mass or more, 3.0 parts by mass or more, or 5.0 parts by mass or more, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, and may be 20.0 parts by mass or less, 15.0 parts by mass or less, 10.0 parts by mass or less, 8.0 parts by mass or less, 6.0 parts by mass or less, or 5.5 parts by mass or less.

[0059] Component (D): Sensitizer The photosensitive resin composition contains one or more types of component (D). Component (D) includes an anthracene compound. By including an anthracene compound as component (D), the photosensitive resin composition is particularly suitable for direct writing exposure methods. Examples of the anthracene compound include 1-methylanthracene, 2-methylanthracene, 9-methylanthracene, 2-ethylanthracene, 2-butylanthracene, 9-vinylanthracene, 9-phenylanthracene, 1-aminoanthracene, 2-aminoanthracene, 9-(methylaminomethyl)anthracene, 9-acetylanthracene, 9-anthraldehyde, 9,10-dimethylanthracene, 9,10-dimethoxyanthracene, and 9,10-dipropionanthracene. Examples of anthracene compounds include 9,10-dipentoxyanthracene, anthracene, 9,10-di(2-ethylhexyloxy)anthracene, 2-bromo-9,10-diphenylanthracene, 9-(4-bromophenyl)-10-phenylanthracene, 10-methyl-9-anthraldehyde, 1,4,9,10-tetrahydroxyanthracene, 9,10-dibutoxyanthracene, 9,10-diphenylanthracene, and 9,10-diethoxyanthracene. The anthracene compound may include at least one selected from the group consisting of anthracene compounds having an aryl group and anthracene compounds having an alkoxy group. From the viewpoints of sensitivity, adhesion, resolution, and strippability, the anthracene compound may include 9,10-dibutoxyanthracene. The component (D) may consist solely of an anthracene compound, or may further contain a sensitizer other than an anthracene compound as long as the effects of the present disclosure are not impaired.

[0060] The content of the (D) component may be 0.20 parts by mass or more, 0.30 parts by mass or more, 0.40 parts by mass or more, 0.50 parts by mass or more, 0.55 parts by mass or more, or 0.60 parts by mass or more, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, and may be 1.50 parts by mass or less, 1.00 parts by mass or less, 0.80 parts by mass or less, 0.75 parts by mass or less, or 0.70 parts by mass or less.

[0061] (Other Components) The photosensitive resin composition may further contain one or more other components in addition to the components described above. Examples of other components include polymerization inhibitors, hydrogen donors (such as bis[4-(dimethylamino)phenyl]methane and bis[4-(diethylamino)phenyl]methane), tribromophenyl sulfone, thermal color-development inhibitors, plasticizers (such as p-toluenesulfonamide), pigments, fillers, antifoaming agents, flame retardants, stabilizers, adhesion promoters, leveling agents, release promoters, antioxidants, fragrances, imaging agents, and thermal crosslinkers. The content of the other components may be 0.005 parts by mass or more, or 0.01 parts by mass or more, or 20 parts by mass or less, relative to 100 parts by mass of the total amount of component (A) and component (B).

[0062] The photosensitive resin composition may further contain one or more organic solvents from the viewpoint of adjusting the viscosity, such as methanol, ethanol, acetone, methyl ethyl ketone, methyl cellosolve, ethyl cellosolve, toluene, N,N-dimethylformamide, and propylene glycol monomethyl ether.

[0063] The photosensitive resin composition may be in a liquid form or a film form (photosensitive film). The photosensitive resin composition can be used, for example, as a negative photosensitive resin composition. The photosensitive resin composition can be suitably used in the method for forming a resist pattern and the method for manufacturing a wiring board, which will be described later.

[0064] <Photosensitive Element> The photosensitive element according to this embodiment includes a support and a photosensitive layer formed on the support using the above-described photosensitive resin composition. The photosensitive element may further include a protective layer on the photosensitive layer.

[0065] 1 is a schematic cross-sectional view showing a photosensitive element according to one embodiment. As shown in FIG. 1, the photosensitive element 1 includes a support 2, a photosensitive layer 3 provided on the support 2, and a protective layer 4 provided on the side of the photosensitive layer 3 opposite the support 2.

[0066] Examples of materials constituting the support include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene-2,6-naphthalate (PEN), and polyolefins such as polypropylene and polyethylene. The support may have a polyester film or a PET film, from the viewpoint of easily suppressing the occurrence of defects in the resist.

[0067] The haze of the support may be 0.01 to 5.0%, 0.01 to 1.5%, 0.01 to 1.0%, or 0.01 to 0.5%. Haze can be measured using a commercially available haze meter (turbidity meter) in accordance with the method specified in JIS K7105. Haze can be measured, for example, using a commercially available turbidity meter such as NDH-5000 (trade name, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0068] The thickness of the support may be 1 μm or more, 5 μm or more, or 10 μm or more from the viewpoint of easily preventing damage to the support when peeling the support from the photosensitive layer, and may be 100 μm or less, 50 μm or less, 30 μm or less, or 20 μm or less from the viewpoint of easily and suitably performing exposure when exposing through the support.

[0069] The protective layer may be a polymer film having heat resistance and solvent resistance, and for example, a polyolefin film such as a polyethylene film or a polypropylene film can be used. In particular, by using a polyethylene film as the protective layer, misalignment of the photosensitive element during winding can be suppressed, and static electricity is less likely to be generated when the protective layer is peeled off from the photosensitive layer, thereby suppressing damage to the photosensitive layer.

[0070] The thickness of the protective layer may be 1 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more from the viewpoint of easily suppressing damage to the protective layer when the photosensitive layer and the support are laminated onto the substrate while peeling off the protective layer, or may be 100 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less from the viewpoint of easily improving productivity.

[0071] The thickness of the photosensitive layer after drying (after volatilization of the solvent) may be 29 μm to 300 μm. From the viewpoint of forming a resist pattern having a high aspect ratio, the thickness of the photosensitive layer may be 29 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, 55 μm or more, or 60 μm or more, and from the viewpoint of releasability, the thickness may be 300 μm or less, 250 μm or less, 200 μm or less, 150 μm or less, 120 μm or less, 100 μm or less, 80 μm or less, 70 μm or less, or 60 μm or less. The thickness of the photosensitive layer may be the average value of thicknesses at 10 locations.

[0072] The photosensitive element 1 can be obtained, for example, as follows. First, a photosensitive layer 3 is formed on a support 2. The photosensitive layer 3 can be formed, for example, by applying a photosensitive resin composition to form a coating layer and drying the coating layer. Next, a protective layer 4 is coated on the surface of the photosensitive layer 3 opposite the support 2.

[0073] The coating layer is formed by a known method such as roll coating, comma coating, gravure coating, air knife coating, die coating, bar coating, etc. The coating layer is dried, for example, at 70 to 150°C for about 5 to 30 minutes.

[0074] In another embodiment, the photosensitive element may further include other layers such as a cushion layer, an adhesive layer, a light absorbing layer, and a gas barrier layer.

[0075] The photosensitive element 1 may be, for example, in the form of a sheet, or in the form of a photosensitive element roll wound around a core. In the photosensitive element roll, the photosensitive element 1 is preferably wound with the support 2 facing outward. The core is formed of, for example, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, or the like. An end separator may be provided on the end face of the photosensitive element roll from the viewpoint of end face protection, or a moisture-proof end face separator may be provided from the viewpoint of edge fusion resistance. The photosensitive element 1 may be wrapped, for example, in a black sheet with low moisture permeability.

[0076] The photosensitive element according to this embodiment can be suitably used in the method for forming a resist pattern and the method for manufacturing a wiring board, which will be described later.

[0077] <Method of Forming Resist Pattern> The method of forming a resist pattern according to this embodiment includes a step of forming a photosensitive layer on a substrate using the photosensitive resin composition or the photosensitive element (hereinafter also referred to as a "photosensitive layer forming step"), a step of photocuring a portion of the photosensitive layer (hereinafter also referred to as an "exposure step"), and a step of removing an uncured portion of the photosensitive layer (hereinafter also referred to as a "development step"), and may further include other steps as necessary. The resist pattern can also be referred to as a photocured product pattern of the photosensitive resin composition or a relief pattern.

[0078] (Photosensitive layer forming step) In the photosensitive layer forming step, a photosensitive layer is formed on a substrate using a photosensitive resin composition or a photosensitive element. The substrate is not particularly limited, but typically, a circuit-forming substrate having an insulating layer and a conductor layer formed on the insulating layer, or a die pad (substrate for lead frame) such as an alloy substrate is used.

[0079] For example, the photosensitive layer can be formed on the substrate by removing the protective layer from the photosensitive element and then pressing the photosensitive layer of the photosensitive element onto the substrate while heating, thereby obtaining a laminate having the substrate, photosensitive layer, and support in this order.

[0080] The photosensitive layer forming step may be carried out under reduced pressure from the viewpoint of adhesion and followability. Heating during pressure bonding may be carried out at a temperature of 70 to 130°C, and pressure bonding may be carried out at 0.1 to 1.0 MPa (1 to 10 kgf / cm 2 These conditions can be appropriately selected as needed. Note that if the photosensitive layer of the photosensitive element is heated to 70 to 130°C, it is not necessary to preheat the substrate, but the substrate can be preheated in order to further improve the adhesion and followability.

[0081] In the exposure step, the photosensitive layer may be exposed to actinic rays through the support, or the support may be peeled off and then the photosensitive layer may be exposed to actinic rays. As a result, the exposed area irradiated with actinic rays is photocured to form a photocured area (latent image).

[0082] As the exposure method, known exposure methods can be applied, and examples thereof include a method of irradiating an actinic ray in an imagewise manner through a negative or positive mask pattern called artwork (mask exposure method), an LDI exposure method (direct writing exposure), and a method of irradiating an actinic ray projected from a photomask image through a lens in an imagewise manner (projection exposure method). The photosensitive resin composition according to this embodiment can be suitably used for direct writing exposure.

[0083] The light source for actinic rays is not particularly limited as long as it is a commonly used known light source, and examples thereof include those that effectively emit ultraviolet rays, such as carbon arc lamps, mercury vapor arc lamps, ultra-high pressure mercury lamps, high-pressure mercury lamps, xenon lamps, gas lasers such as argon lasers, solid-state lasers such as YAG lasers, and semiconductor lasers such as gallium nitride blue-violet lasers. Among these, from the viewpoint of improving resolution and alignment in a well-balanced manner, light sources capable of emitting monochromatic i-line light with an exposure wavelength of 365 nm, light sources capable of emitting monochromatic h-line light with an exposure wavelength of 405 nm, or light sources capable of emitting actinic rays with exposure wavelengths that are cross-linked with i, h, and g may be used. Examples of light sources capable of emitting monochromatic i-line light with an exposure wavelength of 365 nm include ultra-high pressure mercury lamps. Examples of light sources capable of emitting monochromatic h-line light with an exposure wavelength of 405 nm include blue-violet laser diodes with a wavelength of 405 nm.

[0084] In the method for forming a resist pattern according to this embodiment, from the viewpoint of adhesion, post-exposure baking (PEB) may be performed after the exposure step and before the development step. The temperature when performing PEB may be 50 to 100° C. Heating may be performed using a heater such as a hot plate, a box dryer, or a heating roll.

[0085] (Developing Step) In the developing step, the uncured portions of the photosensitive layer are removed from the substrate. When the photosensitive layer is exposed through the support, the support and the uncured portions of the photosensitive layer are removed from the substrate. In the developing step, a resist pattern consisting of photocured portions of the photosensitive layer is formed on the substrate. The developing method may be wet development or dry development.

[0086] In the case of wet development, development can be carried out by a known wet development method using a developer suitable for the photosensitive resin composition. Examples of wet development methods include dipping, puddling, high-pressure spraying, brushing, scrubbing, and swinging immersion. These wet development methods may be used alone or in combination of two or more methods.

[0087] The developer is appropriately selected depending on the constitution of the photosensitive resin composition, and may be, for example, an alkaline developer or an organic solvent developer.

[0088] From the viewpoints of safety, stability, and ease of use, an alkaline developer may be used as the developer. The alkaline developer may be an aqueous solution containing a base such as an alkali hydroxide such as lithium, sodium, or potassium hydroxide; an alkali carbonate such as lithium, sodium, potassium, or ammonium carbonate or bicarbonate; an alkali metal phosphate such as potassium phosphate or sodium phosphate; an alkali metal pyrophosphate such as sodium pyrophosphate or potassium pyrophosphate; borax; sodium metasilicate; tetramethylammonium hydroxide; ethanolamine; ethylenediamine; diethylenetriamine; 2-amino-2-hydroxymethyl-1,3-propanediol; 1,3-diamino-2-propanol; or morpholine.

[0089] From the viewpoint of environmental friendliness, an inorganic alkaline developer may be used, such as a dilute solution of 0.1 to 5 mass % sodium carbonate, a dilute solution of 0.1 to 5 mass % potassium carbonate, a dilute solution of 0.1 to 5 mass % sodium hydroxide, or a dilute solution of 0.1 to 5 mass % sodium tetraborate.

[0090] The pH of the alkaline developer used for development may be in the range of 9 to 11, and the temperature of the alkaline developer can be adjusted according to the developability of the photosensitive layer. The alkaline developer may contain, for example, a surfactant, an antifoaming agent, or a small amount of an organic solvent to promote development. Examples of organic solvents used in the alkaline developer include 3-acetone alcohol, acetone, ethyl acetate, an alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether.

[0091] Examples of organic solvents used in the organic solvent developer include 1,1,1-trichloroethane, N-methyl-2-pyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone. From the viewpoint of preventing ignition, these organic solvents may be used as the organic solvent developer by adding water in a range of 1 to 20% by mass.

[0092] (Other Steps) In the method for forming a resist pattern according to this embodiment, after removing the uncured portion in the development step, heating at 60 to 250° C. or irradiating with 0.2 to 10 J / cm 2 is performed as necessary. 2 The method may further include a step of further hardening the resist pattern by exposing the resist pattern to light at an exposure dose of 1000 nm or more.

[0093] <Method of manufacturing wiring board> The method of manufacturing a wiring board according to this embodiment includes a step of forming a conductor pattern (wiring layer) by etching or plating a substrate on which a resist pattern has been formed by the above-described method of forming a resist pattern, and may also include other steps such as a resist pattern removal step as necessary.

[0094] In the etching process, a resist pattern formed on a substrate having a conductive layer is used as a mask to etch away the conductive layer of the substrate that is not covered with the resist, thereby forming a conductive pattern.

[0095] The etching method is appropriately selected depending on the conductor layer to be removed. Examples of the etching solution include a cupric chloride solution, a ferric chloride solution, an alkaline etching solution, and a hydrogen peroxide-based etching solution. From the viewpoint of a good etch factor, a ferric chloride solution may be used as the etching solution.

[0096] In the plating process, a resist pattern formed on a substrate having a conductor layer is used as a mask to plate copper, solder, etc. on the conductor layer of the substrate that is not covered with the resist. After the plating process, the resist is removed by removing the resist pattern as described below, and the conductor layer that was covered with the resist is then etched to form the conductor pattern.

[0097] The plating method may be electrolytic plating or electroless plating, and examples thereof include copper plating such as copper sulfate plating and copper pyrophosphate plating; solder plating such as high-throw solder plating; nickel plating such as Watts bath (nickel sulfate-nickel chloride) plating and nickel sulfamate plating; and gold plating such as hard gold plating and soft gold plating.

[0098] After the etching or plating process, the resist pattern on the substrate is removed. The resist pattern can be removed, for example, using an inorganic alkaline stripper or an organic alkaline stripper. Examples of inorganic alkaline stripper solutions that can be used include a 1 to 10 mass % aqueous solution of sodium hydroxide and a 1 to 10 mass % aqueous solution of potassium hydroxide. Examples of organic alkaline stripper solutions that can be used include amine-based strippers such as ethanolamine, ethylenediamine, and diethylenetriamine, and tetramethylammonium hydroxide aqueous solutions. From the viewpoint of the strippability of thick-film resist patterns, organic alkaline stripper solutions may also be used.

[0099] Methods for removing the resist pattern include, for example, a dipping method and a spray method, which may be used alone or in combination.

[0100] When the resist pattern is removed after plating, the conductor layer covered with the resist is further etched by etching to form a conductor pattern, thereby manufacturing a desired wiring board. The etching method used in this process is appropriately selected depending on the conductor layer to be removed. For example, the above-mentioned etching solution can be used.

[0101] The method for manufacturing a wiring board according to this embodiment can be applied to the manufacture of not only single-layer wiring boards but also multi-layer wiring boards, and can also be applied to the manufacture of wiring boards having small-diameter through holes.

[0102] The method for manufacturing a wiring board according to this embodiment can be suitably used for manufacturing high-density packaging substrates, particularly for manufacturing wiring boards using a semi-additive process. An example of a manufacturing process for a wiring board using a semi-additive process is shown in FIG.

[0103] In (a) of FIG. 2, a substrate (circuit-forming substrate) is prepared in which a conductor layer 40 is formed on an insulating layer 50. The conductor layer 40 is, for example, a copper layer. In (b) of FIG. 2, the photosensitive layer forming step described above forms a photosensitive layer 30 and a support 20 on the conductor layer 40 of the substrate. In (c) of FIG. 2, the exposure step described above irradiates the photosensitive layer 30 with actinic rays 80 in a desired pattern through the support 20 by a direct writing exposure method, thereby forming photocured portions in the photosensitive layer 30. In (d) of FIG. 2, the development step removes from the substrate areas other than the photocured portions formed in the exposure step, thereby forming a resist pattern 32, which is a photocured portion, on the substrate.

[0104] 2( e), a plating layer 60 is formed on the conductor layer 40 of the substrate that is not covered with resist by a plating process using the resist pattern 32, which is the photocured portion, as a mask. The conductor layer 40 and the plating layer 60 may be made of the same material or different materials. When the conductor layer 40 and the plating layer 60 are made of the same material, the conductor layer 40 and the plating layer 60 may be integrated.

[0105] 2(f), the photocured resist pattern 32 is peeled off and removed using a strong alkaline aqueous solution. The strong alkaline developer may be, for example, a 1 to 10% by mass aqueous sodium hydroxide solution or a 1 to 10% by mass aqueous potassium hydroxide solution. Next, the conductor layer 40 masked by the resist pattern 32 is removed by flash etching, forming a conductor pattern 70 including the etched plating layer 62 and the etched conductor layer 42. The etching solution is appropriately selected depending on the type of conductor layer 40, and may be, for example, a cupric chloride solution, a ferric chloride solution, an alkaline etching solution, a hydrogen peroxide etching solution, or the like. By using the photosensitive element according to this embodiment, a wiring board having a fine conductor pattern can be produced.

[0106] Although the preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments.

[0107] The present disclosure will be explained in more detail below using examples, but the present disclosure is not limited to these examples.

[0108] Synthesis of Component (A) 27 parts by mass of methacrylic acid, 5 parts by mass of methyl methacrylate, 45 parts by mass of styrene, and 23 parts by mass of benzyl methacrylate were mixed with 0.9 parts by mass of azobisisobutyronitrile to prepare solution (a). 0.5 parts by mass of azobisisobutyronitrile was dissolved in 50 parts by mass of a mixed solution (x) of acetone / propylene glycol monomethyl ether (mass ratio: 6 / 1) to prepare solution (b). 500 g of mixed solution (x) was placed in a flask equipped with a stirrer, reflux condenser, thermometer, dropping funnel, and nitrogen gas inlet tube, and the mixture was stirred while blowing nitrogen gas into the flask and heated to 80°C. Solution (a) was added dropwise to the mixed solution in the flask at a constant dropping rate over 4 hours, followed by stirring at 80°C for 2 hours. Next, the solution (b) was added dropwise to the solution in the flask at a constant rate over 10 minutes, and the solution in the flask was stirred at 80°C for 3 hours. The solution in the flask was then heated to 90°C over 30 minutes and maintained at 90°C for 2 hours. The stirring was then stopped and the solution was cooled to room temperature (25°C), yielding a solution of binder polymer A1. The non-volatile content (solid content) of the binder polymer A1 solution was 48% by mass. The weight-average molecular weight of binder polymer A1 was 40,000.

[0109] The weight average molecular weight was measured by gel permeation chromatography (GPC) and calculated by conversion using a calibration curve of standard polystyrene. The GPC conditions are as follows. (GPC conditions) Pump: Hitachi L-6000 type (trade name, manufactured by Hitachi, Ltd.) Column: a total of three columns: Gelpack GL-R420, Gelpack GL-R430, and Gelpack GL-R440 (all manufactured by Resonac Corporation, trade names) Eluent: tetrahydrofuran Measurement temperature: 40°C Flow rate: 2.05 mL / min Detector: Hitachi L-3300 type RI (trade name, manufactured by Hitachi, Ltd.)

[0110] <Preparation of Photosensitive Resin Compositions> Photosensitive resin compositions were prepared by mixing the components shown in Tables 1 and 2 in the amounts (parts by mass) shown in the tables. The amounts (parts by mass) of components other than the solvent shown in Tables 1 and 2 are the masses of non-volatile components (solid content). Details of each component shown in Tables 1 and 2 are as follows.

[0111] (Binder polymer) Polymer A1: Binder polymer A1 synthesized above (Photopolymerizable compound) FA-321M (70): 70% propylene glycol monomethyl ether solution of 2,2-bis(4-(methacryloxyethoxy)phenyl)propane (ethylene oxide adduct of an average of 10 mol) (manufactured by Resonac Co., Ltd.) FA-023M: PO / EO modified dimethacrylate (manufactured by Resonac Co., Ltd., ethylene oxide adduct of an average of 4 mol and propylene oxide adduct of an average of 12 mol (total value)) FA-024M: PO / EO modified dimethacrylate (manufactured by Resonac Co., Ltd., ethylene oxide adduct of an average of 6 mol and propylene oxide adduct of an average of 12 mol (total value)) FA-137M: EO modified trimethylolpropane trimethacrylate (ethylene oxide adduct of an average of 21 mol, manufactured by Resonac Co., Ltd.) UA11: EO-modified urethane methacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) UA13: PO / EO-modified urethane methacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) FA-513AS: dicyclopentanyl acrylate (manufactured by Resonac Corporation) FA-MECH(100): γ-chloro-β-hydroxypropyl-β'-methacryloyloxyethyl-o-phthalate (manufactured by Resonac Corporation) (photopolymerization initiator) N-PG: N-phenylglycine BCIM: 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (manufactured by Hampford Chemical Industries, Ltd.) (sensitizer) DBA: 9,10-dibutoxyanthracene (manufactured by Kawasaki Chemical Industries, Ltd.) EAB: 4,4'-bis(diethylamino)benzophenone (Other ingredients) LCV: Leuco Crystal Violet (Yamada Chemical Co., Ltd.) MKG: Malachite Green (Osaka Organic Chemical Industry Ltd.) LA-7RD: 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl (Adeka Corporation) DIC-TBC-5P: 4-tert-butylcatechol (DIC Corporation) SF-808H: Mixture of carboxybenzotriazole, 5-amino-1H-tetrazole, and methoxypropanol (Sanwa Kasei Co., Ltd.) (Solvents) ACS: Acetone TLS: Toluene MAL: Methanol

[0112] <Preparation of Photosensitive Element> A 16 μm thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name: FB-40) was prepared as a support, and a photosensitive resin composition was applied to the support so as to have a uniform thickness, followed by drying in a hot air convection dryer at 80° C. and 120° C., successively to form a photosensitive layer having a thickness of 40 μm after drying. A polyethylene film (manufactured by Tamapoly Corporation, product name: NF-15) was laminated onto this photosensitive layer as a protective layer, to obtain a photosensitive element in which the support, photosensitive layer, and protective layer were laminated in that order.

[0113] <Laminate Preparation> A copper-clad laminate (substrate, manufactured by Resonac Corporation, product name: MCL-E-67) comprising a glass epoxy material and copper foil (thickness: 16 μm) arranged on both sides thereof was pickled, rinsed with water, and then dried in an air stream. The copper-clad laminate was then heated to 80°C, and the protective layer was peeled off. The photosensitive element described above was then laminated onto the copper-clad laminate so that the photosensitive layer was in contact with the copper surface, thereby obtaining a laminate comprising, in order, the copper-clad laminate, the photosensitive layer, and the support. Lamination was performed using a 110°C heat roll at a pressure of 0.4 MPa and a roll speed of 1.0 m / min.

[0114] <Evaluation> (Minimum Development Time) The laminate was cut into a square (5 cm x 5 cm) and the support was peeled off to obtain a test piece. Next, the unexposed photosensitive layer of the test piece was spray-developed at a pressure of 0.15 MPa using a 1% by mass aqueous sodium carbonate solution at 30°C. The minimum development time (MD) was determined as the shortest time at which it was visually confirmed that at least 1 mm of the unexposed photosensitive layer had been removed. A full-cone type nozzle was used for spray development. The distance between the test piece and the nozzle tip was 6 cm, and the nozzle was positioned so that the center of the test piece coincided with the center of the nozzle. The shorter the minimum development time (unit: seconds), the better the developability.

[0115] (Sensitivity) After placing a Hitachi 41-step step tablet on the support of the laminate, the photosensitive layer was exposed through the support using a direct imaging exposure machine (manufactured by Via Mechanics Co., Ltd., product name: DE-1UH) with a blue-violet laser diode having a wavelength of 405 nm as a light source, at an exposure amount (amount of irradiation energy) such that the number of remaining steps of the Hitachi 41-step step tablet was 15. The exposure amount at this time (unit: mJ / cm 2 The sensitivity (photosensitivity) was evaluated by the following formula: The lower the exposure amount, the higher the sensitivity.

[0116] (Resolution and Adhesion) Using a drawing pattern in which line width (L) / space width (S) is x / x (x=3 to 30, unit: μm, 1 μm intervals), the photosensitive layer of the laminate was exposed to light with a direct writing exposure machine (manufactured by Via Mechanics Co., Ltd., product name: DE-1UH) using a blue-violet laser diode with a wavelength of 405 nm as a light source, at an exposure amount such that the number of remaining steps on a Hitachi 41-step step tablet was 15.

[0117] After exposure, the support was peeled off from the laminate to expose the photosensitive layer, and the unexposed areas were removed by spraying a 1% by mass aqueous sodium carbonate solution at 30°C for twice the minimum development time. After development, the space areas (unexposed areas) were removed without residue, and the line areas (exposed areas) were formed without meandering or chipping. Resolution was evaluated based on the minimum space width (unit: μm) in the resist pattern, and adhesion was evaluated based on the minimum line width (unit: μm) in the resist pattern. For both resolution and adhesion, the smaller the numerical value, the better the performance.

[0118] (Peeling property) A glass chrome type phototool (having a 40 mm × 60 mm planar pattern) was used as a negative for evaluating peel test on the support of the laminate, and the photosensitive layer was exposed through the support using a direct imaging exposure machine (manufactured by Via Mechanics Co., Ltd., product name: DE-1UH) with a blue-violet laser diode having a wavelength of 405 nm as a light source, at an exposure amount such that the number of remaining steps of a Hitachi 41-step step tablet was 15.

[0119] After exposure, the support was peeled from the laminate to expose the photosensitive layer, and the unexposed areas were removed by spraying a 1% by weight aqueous sodium carbonate solution at 30°C for twice the minimum development time, yielding a substrate on which a cured film had been formed. After leaving this substrate at room temperature for 3 hours, it was immersed in an amine-based stripping solution (aqueous solution of 6% by volume R-100S + 2% by volume R-101, manufactured by Mitsubishi Gas Chemical Company, Inc.) heated to 50°C and stirred at 400 rpm. The time from the start of stirring until the cured film began to peel from the substrate was defined as the peeling start time (unit: seconds, hereinafter also referred to as "T1"), and the time until the cured film was completely removed from the substrate was defined as the peeling end time (unit: seconds, hereinafter also referred to as "T2"). The shorter T1 and T2 values ​​indicate better releasability.

[0120]

[0121]

[0122] DESCRIPTION OF SYMBOLS 1... photosensitive element, 2, 20... support, 3, 30... photosensitive layer, 4... protective layer, 32... resist pattern, 40... conductor layer, 42... conductor layer after etching treatment, 50... insulating layer, 60... plating layer, 62... plating layer after etching treatment, 70... conductor pattern, 80... actinic light.

Claims

1. A photosensitive resin composition comprising a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a sensitizer, wherein the photopolymerization initiator contains a hexaarylbiimidazole compound and an N-phenylglycine compound, and the sensitizer contains an anthracene compound.

2. The photosensitive resin composition according to claim 1, wherein the content of the N-phenylglycine compound is 0.06 parts by mass or less per 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound.

3. The photosensitive resin composition according to claim 1, wherein the photopolymerizable compound comprises a (meth)acrylate compound having an alicyclic structure.

4. The photosensitive resin composition according to claim 1, wherein the photopolymerizable compound comprises a polyalkylene glycol di(meth)acrylate compound.

5. The photosensitive resin composition according to claim 4, wherein the content of the polyalkylene glycol di(meth)acrylate compound is 8% by mass or more and 30% by mass or less, based on the total amount of the photopolymerizable compound.

6. A photosensitive element comprising: a support; and a photosensitive layer formed on the support using the photosensitive resin composition according to any one of claims 1 to 5.

7. The photosensitive element of claim 6, wherein the photosensitive layer has a thickness of 29 μm or greater.

8. A method for forming a resist pattern, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 5; photocuring a portion of the photosensitive layer; and removing an uncured portion of the photosensitive layer.

9. A method for forming a resist pattern, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive element according to claim 6; photocuring a portion of the photosensitive layer; and removing an uncured portion of the photosensitive layer.

10. A method for manufacturing a wiring board, comprising the step of etching or plating a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to claim 8, to form a conductor pattern.