Three-color 3D dram stack and methods of making

TWI945285BActive Publication Date: 2026-11-11APPLIED MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
TW111136032
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-28
Filing Date
2022-09-23
Publication Date
2026-11-11
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

The increase in the number of silicon channel and sacrificial layers in 3D DRAM devices beyond the 10 nm node leads to significant wafer bowing due to lattice mismatch-induced stress, which hinders accurate photolithography processes and increases processing complexity and cost.

Method used

A 3-color processing method using film stacks comprising first and second doped SiGe layers and a doped silicon layer, with varying doping amounts and Si:Ge ratios, provides etch selectivity and reduces wafer bow by forming channels through the membrane stack.

Benefits of technology

The method effectively reduces wafer bow to less than 150 µm, enabling precise photolithography and simplifying the processing of 3D DRAM devices with improved etch selectivity and reduced complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920030_001
    Figure TWG2TB001920030_001
  • Figure TWG2TB001920030_002
    Figure TWG2TB001920030_002
  • Figure TWG2TB001920030_003
    Figure TWG2TB001920030_003
Patent Text Reader

Abstract

A method for reducing wafer warping in a 3D DRAM device using a 3-color process is described. A plurality of film stacks are formed on a substrate surface, each film stack comprising two doped SiGe layers and one doped silicon layer, the two doped SiGe layers having different dopant amounts and / or Si:Ge ratios. A 3D DRAM device is also described.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention generally relate to 3D DRAM stacking and methods for forming 3D DRAM devices. In particular, the embodiments of the present invention relate to a method for forming 3D DRAM devices using a 3-color process. Prior Technology

[0002] In the semiconductor manufacturing industry, there is a focus on increasing the bit density of memory devices. One method for manufacturing 3D DRAM devices involves epitaxial growth of a multilayer stack, which includes an epitaxial silicon channel layer and two or more sacrificial epitaxial layers. Subsequent processing steps require the sacrificial layers to be recessed to form access gates and capacitors.

[0003] To extend 3D DRAM density beyond the 10 nm node, the number of silicon channel / sacrificial layer stacks needs to be increased to greater than 100, resulting in 400 epitaxial layers. One problem with increasing the number of layers is wafer warping when the stack size exceeds 150 µm. This wafer warping is believed to be caused by stress induced by lattice mismatch in the silicon channel / sacrificial layer stack. Typically, wafer warping greater than 150 µm can hinder the precise execution of subsequent processes such as lithography.

[0004] During device formation, the sacrificial layer is selectively etched relative to the silicon channels. Conventional processing layer stacking, designed to reduce wafer bending, results in reduced etch selectivity.

[0005] Current technology requires the additional deposition of a stress-relieving film on the back side of the wafer to combat wafer bending. This only partially mitigates the wafer bending problem because bending recurs when the top stack is etched or during thermal processing. Furthermore, removing the back-side film increases processing complexity and cost.

[0006] Therefore, there is a need for 3D DRAM devices with reduced wafer bending and / or improved etch selectivity, and methods for forming 3D DRAM devices. Summary of the Invention

[0007] One or more embodiments of the present invention relate to a method for reducing wafer warping in a 3D DRAM device. A plurality of film stacks are formed on a substrate surface. Each film stack comprises a first doped SiGe layer, a second doped SiGe layer, and a doped silicon layer. The first doped SiGe layer has the experimental formula Si 1-xGe x, where x is in the range >0 to 0.5. The second doped SiGe layer is on top of the first doped SiGe layer and has the experimental formula Si 1-yGe y, where y is in the range >0 to 0.5. The doped silicon layer is on top of the second doped SiGe layer. The first doped SiGe layer and the second doped SiGe layer have one or more different doping amounts or different Si:Ge ratios.

[0008] Additional embodiments of the present invention relate to a method of manufacturing a 3D DRAM device. At least 100 film stacks are formed on a substrate surface. Each film stack includes a first doped SiGe layer, a second doped SiGe layer, and a doped silicon layer. The first doped SiGe layer has the experimental formula Si 1-xGe x, where x is in the range >0 to 0.5. The second doped SiGe layer is on the first doped SiGe layer and has the experimental formula Si 1-yGe y, where y is in the range >0 to 0.5. The first doped SiGe layer and the second doped SiGe layer have one or more different doping amounts or different Si:Ge ratios. The doped silicon layer is on the second doped SiGe layer. A channel is formed through the film stack to the substrate. One or more of the first doped SiGe layer or the second doped SiGe layer are selectively removed through this channel.

[0009] Further embodiments of the present invention relate to a method of manufacturing a 3D DRAM device with reduced wafer warp. At least 100 film stacks are formed on a substrate surface. Each film stack comprises an epitaxially grown first doped SiGe layer, an epitaxially grown second doped SiGe layer, and an epitaxially grown doped silicon layer. The epitaxially grown first doped SiGe layer has the experimental formula Si 1-xGe x, where x is in the range >0 to 0.5. The epitaxially grown second doped SiGe layer is on the first doped SiGe layer and has the experimental formula Si 1-yGe y, where y is in the range >0 to 0.5. The first doped SiGe layer and the second doped SiGe layer have one or more different doping amounts or different Si:Ge ratios. The epitaxially grown doped silicon layer is on the second doped SiGe layer. The first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer independently contain a dopant selected from carbon or boron in the range of 0.5-2.5%. The stress in the second doped SiGe layer is more tensile than that in the first doped SiGe layer, and the stress in the first doped SiGe layer is more tensile than that in the Si layer. When using a halide-based etchant, each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer has an etch selectivity greater than 200:1 relative to the other layers. A channel is formed through all the stacks to the substrate surface by photolithography. One or more of the first or second doped SiGe layers are selectively etched from all the film stacks through this channel. Simple Explanation of the Diagram

[0010] A more detailed description of the invention briefly summarized above can be obtained by referring to some of the embodiments illustrated in the accompanying drawings, thereby allowing the features of the invention to be understood in more detail. However, it will be noted that the accompanying drawings illustrate only typical embodiments of the invention and are therefore not intended to limit its scope, as other equivalent embodiments are permissible. The embodiments described herein are illustrated as examples and are not limited to the illustrations in the accompanying drawings; the same element symbols in the accompanying drawings indicate similar elements.

[0011] Figure 1 shows a schematic representation of a 3D DRAM device during formation using a 3-color process according to one or more embodiments of the present invention;

[0012] Figure 2 shows an enlarged view of region II in Figure 1 after the formation of channels through the membrane stack; and

[0013] Figure 3 shows an enlarged view of Figure 2 after selectively removing one of the three colors in a multilayer process. Implementation

[0014] Before describing several exemplary embodiments of the present invention, it will be understood that the invention is not limited to the details of the architecture or processing steps described in the following description. The invention can be other embodiments and can be implemented or performed in various ways.

[0015] As used in this specification and the accompanying claims, the term "substrate" refers to a surface or portion thereof on which processing is performed. Unless the context clearly indicates otherwise, those skilled in the art will understand that "substrate" may also refer to only a portion of a substrate. Furthermore, "deposition on a substrate" may mean both a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0016] As used herein, "substrate" refers to any substrate on which a film treatment is performed during manufacturing processes, or a material surface formed on a substrate. For example, substrate surfaces on which treatments can be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates are not limited to semiconductor wafers. Substrates may be exposed to pretreatment processes for polishing, etching, reduction, oxidation, hydroxylation, annealing, UV curing, electron beam curing, and / or baking of the substrate surface. In addition to film treatments performed directly on the surface of the substrate itself, any film treatment steps disclosed in this invention may also be performed over an underlying layer formed on the substrate, as described in more detail below, and the term "substrate surface" is intended to include this underlying layer as indicated by the context. Therefore, for example, where a film / layer or part of a film / layer has been deposited onto the substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface for further processing.

[0017] According to one or more embodiments, the term "above" for a film or a layer of a film includes the film or layer directly on a surface, such as a substrate surface, and has one or more underlying layers between the film or layer and the surface, such as the substrate surface. Therefore, in one or more embodiments, the phrase "above a substrate surface" is intended to include one or more underlying layers. In other embodiments, the phrase "directly above" refers to a layer or film in contact with a surface, such as a substrate surface, without an intermediate layer. Therefore, the phrase "directly above a substrate surface" refers to a layer in direct contact with a substrate surface without any intermediate layers.

[0018] One or more embodiments of the present invention advantageously provide a three-color method for forming a 3D DRAM device with reduced or neutralized bend in a film stack. When used in this manner, three-color processing refers to having three etch-selective materials used. Some embodiments advantageously provide a 3D DRAM film stack comprising epitaxial silicon (Si) and silicon germanium (SiGe) with reduced or neutralized bend. Some embodiments advantageously provide an epitaxial Si / SiGe stack with reduced bend using carbon (C) or boron (B) doping.

[0019] Referring to Figures 1 to 3, one or more embodiments of the present invention relate to a method for reducing wafer warping in a 3D DRAM device 100 using a 3-color process. A plurality of film stacks 120 are formed on a substrate 100 having a substrate surface 112. The film stacks 120 may also be referred to as 3-color stacks. The embodiment illustrated in Figure 1 shows five film stacks 120 (including film stacks 120a and 120b). Those skilled in the art will recognize that this is merely a representative illustration and that there may be more or fewer film stacks 120. In some embodiments, there are more than 50, 100, 150, or 200 film stacks 120.

[0020] At least some of the film stacks 120, or each of the film stacks 120, includes a first doped SiGe layer 122, a second doped SiGe layer 124, and a doped silicon layer 126. Those skilled in the art will generally recognize that the first doped SiGe layer 122 in the first stack 120a is formed on or directly on the substrate surface 112. The first doped SiGe layer 122 in the subsequent film stack 120b is formed on or directly on the surface 127 of the doped silicon layer 126 of the previous film stack 120a.

[0021] The first doped SiGe layer 122 has the experimental formula Si 1-xGe x. In some embodiments, x is in the range of greater than 0 (>0) to 0.5. In some embodiments, x is in the range of greater than 0 to 0.4, or in the range of greater than 0 to 0.3, or in the range of greater than 0 to 0.2. In some embodiments, x is in the range of 0.05, 0.1, 0.15, 0.2, or 0.25 to 0.5.

[0022] The first doped SiGe layer 122 comprises a dopant having a concentration ranging from 0.5 atomic% to 2.5 atomic%. In some embodiments, the first doped SiGe layer 122 has a dopant concentration ranging from 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5 atomic% to 2.5 atomic%. In some embodiments, the first doped SiGe layer 122 has a dopant concentration ranging from 0.5 atomic% to 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 atomic%.

[0023] The second doped SiGe layer 124 has the experimental formula Si 1-yGe y. In some embodiments, y is in the range greater than 0 to 0.5. In some embodiments, y is in the range greater than 0 to 0.4, or in the range greater than 0 to 0.3, or in the range greater than 0 to 0.2. In some embodiments, x is in the range of 0.05, 0.1, 0.15, 0.2, or 0.25 to 0.5. In some embodiments, the difference between x from the first doped layer 122 and y from the second doped layer 124 is greater than or equal to 0.1, 0.2, 0.3, 0.4, or 0.5. In some embodiments, x is greater than y. In some embodiments, y is greater than x.

[0024] The second doped SiGe layer 124 comprises a dopant having a concentration ranging from 0.5 atomic% to 2.5 atomic%. In some embodiments, the second doped SiGe layer 124 has a dopant concentration ranging from 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5 atomic% to 2.5 atomic%. In some embodiments, the second doped SiGe layer 124 has a dopant concentration ranging from 0.5 atomic% to 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 atomic%.

[0025] The doped silicon layer 126 comprises a dopant having a concentration ranging from 0.5 atomic% to 2.5 atomic%. In some embodiments, the doped silicon layer 126 has a dopant concentration ranging from 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5 atomic% to 2.5 atomic%. In some embodiments, the doped silicon layer 126 has a dopant concentration ranging from 0.5 atomic% to 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5 atomic%.

[0026] The dopant in any of the first doped SiGe layer 122, the second doped SiGe layer 124, or the doped silicon layer 126 may be any suitable dopant known to those skilled in the art. In some embodiments, the dopant comprises a Group III-V element. In some embodiments, the dopant comprises one or more of carbon or boron. In some embodiments, the dopant is substantially composed of one or more of carbon or boron. When used in this manner, the term "substantially composed of" means that the composition of the subject matter is greater than or equal to 95%, 98%, 99%, or 99.5% of the described material. For example, a dopant substantially composed of carbon and / or boron means that 95% or more of all dopant atoms are carbon or boron. In some embodiments, the dopant comprises carbon or is substantially composed of carbon. In some embodiments, the dopant comprises boron or is substantially composed of boron.

[0027] In some embodiments, the first doped SiGe layer and the second doped SiGe layer independently contain dopant in the range of 0.5-2.5%. In some embodiments, the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer independently contain dopant in the range of 0.5-2.5%. The dopant may be the same or different in the different layers.

[0028] In some embodiments, the x of the first doped SiGe layer 122 and the y of the second doped SiGe layer 124 may be the same or within 0.1 of each other, and the difference in dopant concentration in each of the first doped SiGe layer 122 and the second doped SiGe layer 124 may be greater than or equal to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0 atomic percentage.

[0029] The various layers described can be formed by any suitable technique known to those skilled in the art. For example, one or more of these films can be formed by epitaxial growth, chemical vapor deposition, atomic layer deposition, physical vapor deposition, ion implantation, etc. In some embodiments, each of the first doped SiGe layer 122, the second doped SiGe layer 124, and the doped silicon layer 126 is epitaxially grown. In some embodiments, each of the first doped SiGe layer 122, the second doped SiGe layer 124, and the doped silicon layer 126 is independently grown at a temperature ranging from 500 °C to 800 °C.

[0030] The stress of the film stack 120 is adjusted by doping layers. In some embodiments, the stress of the second doped SiGe layer 124 is more tensile than the stress of the first doped SiGe layer 122. The stress of the film stack 120 is adjusted by doping layers. In some embodiments, the stress of the second doped SiGe layer 124 is more tensile than the stress of the first doped SiGe layer 122, and the stress of the first doped SiGe layer 122 is more tensile than the stress of the doped silicon layer 126. In some embodiments, the stress of the first doped SiGe layer 122 and the second doped SiGe layer 124 is more tensile than the stress of the doped silicon layer 126.

[0031] In some embodiments, the overall wafer curvature is neutralized after the formation of 100 film stacks 120. In some embodiments, the overall wafer curvature is neutralized after the formation of 125, 150, 175, or 200 film stacks 120. When used in this manner, the term "neutralized" means a curvature across the wafer surface of less than or equal to 150 µm, 125 µm, 100 µm, 75 µm, 50 µm, or 25 µm. Some embodiments provide a method of doping epitaxial films in a controlled manner to result in a reduced wafer curvature of ~30 µm for fabricating 5 µm DRAM stacks or potentially larger stacks with a height of 1 µm.

[0032] In the three-color processing illustrated, the first doped SiGe layer 122 and the second doped SiGe layer 124 differ from each other in that they exhibit two different etching selectivity relative to each other. In some embodiments, the first doped SiGe layer 122 and the second doped SiGe layer 124 have similar Si:Ge ratios but different doping levels. In other embodiments, the first doped SiGe layer 122 and the second doped SiGe layer 124 have similar doping levels and different Si:Ge ratios. In other words, in some embodiments, the first doped SiGe layer 122 and the second doped SiGe layer 124 have one or more different doping amounts or different Si:Ge ratios.

[0033] The first doped SiGe layer 122, the second doped SiGe layer 124, and the doped silicon layer 126 exhibit etch selectivity relative to each other. In some embodiments, when using a halide-based etchant (e.g., 1% HF, NF3 plasma), the first doped SiGe layer 122 and the doped silicon layer 126 have an etch selectivity greater than 200:1. The halide-based etchant includes wet or vapor-phase etchants. In some embodiments, the halide-based etchant is a vapor-phase etchant containing fluorine atoms. In some embodiments, when using a halide-based etchant, the second doped SiGe layer 124 and the doped silicon layer 126 have an etch selectivity greater than 200:1. In some embodiments, when using a halide-based etchant, the first doped SiGe layer 122 and the second doped SiGe layer 124 have an etch selectivity greater than 200:1. In some embodiments, when a halide-based etchant is used, each of the first doped SiGe layer 122, the second doped SiGe layer 124, and the doped silicon layer 126 has an etch selectivity greater than 200:1 relative to the other layers.

[0034] Although the embodiments and drawings illustrate a 3-color method, those skilled in the art will generally recognize that doped Si and doped SiGe layers can be arranged to provide a 4-color or more color system. By varying the amount of dopant or different Si:Ge ratios, the additional color (SiGe layer) has etch selectivity compared to the first doped SiGe layer 122, the second doped SiGe layer 124, and the doped silicon layer 126.

[0035] Figures 2 and 3 illustrate a portion of the 3D DRAM device 100 in Figure 1 of Region II. In some embodiments of this method, a channel 140 is further included by photolithography to extend through all the film stacks 120 to the substrate surface 112 (or into the substrate 110 by a distance). Those skilled in the art will understand how photolithography is used to form the channel 140. After the formation of the channel 140, one or more of the first doped SiGe layer 122 or the second doped SiGe layer 124 are selectively etched from the film stack 120 through the channel 140. Figure 3 shows the first doped SiGe layer 122 being removed, leaving the second doped SiGe layer 124 and the doped silicon layer 126. Those skilled in the art will understand that the second doped SiGe layer 124 can be removed through the channel 140, while leaving the first doped SiGe layer 122 and the doped silicon layer 126.

[0036] Throughout this specification, references to "one embodiment," "some embodiments," "one or more embodiments," or "an embodiment" indicate that a particular feature, structure, material, or characteristic described with respect to that embodiment is included in at least one embodiment of the invention. Therefore, the appearance of phrases such as "in one or more embodiments," "in some embodiments," "in one embodiment," or "in one embodiment" in various places throughout this specification does not necessarily refer to the same embodiment of the invention. Furthermore, a particular feature, structure, material, or characteristic may be combined in any suitable manner in one or more embodiments.

[0037] Although the invention has been described herein with reference to specific embodiments, those skilled in the art will understand that these embodiments are merely illustrative of the principles and applications of the invention. Various modifications and variations can be made to the methods and apparatus of the invention without departing from the spirit and scope of the invention, as will be apparent to those skilled in the art. Therefore, the invention may include modifications and variations within the scope of the appended claims and their equivalents.

[0038] 100: 3D DRAM device 110:Substrate 112:Substrate surface 120: Membrane stacking 120a: Membrane stacking 120b: Membrane stacking 122: First doped SiGe layer 124: Second doped SiGe layer 126: Doped silicon layer 127: Surface 140: Channel II: Area

[0039] Domestic storage information (please note in order of storage institution, date, and number) none Overseas storage information (please note in the order of storage country, institution, date, and number) none

Claims

1. A method for reducing wafer bending in a 3D DRAM device, the method comprising the steps of: forming a plurality of film stacks on a substrate surface, each of the film stacks comprising: a first doped SiGe layer having an experimental formula Si1-xGex, wherein x is in the range of >0 to 0.5; a second doped SiGe layer on the first doped SiGe layer having an experimental formula Si1-yGey, wherein y is in the range of >0 to 0.5; and a doped silicon layer on the second doped SiGe layer, wherein the first doped SiGe layer and the second doped SiGe layer have one or more of different doping amounts or different Si:Ge ratios.

2. The method as described in claim 1, wherein the first doped SiGe layer contains a dopant in the range of 0.5-2.5 atomic percent.

3. The method as described in claim 2, wherein the dopant is a group III-V element.

4. The method as described in claim 3, wherein the dopant is one or more of carbon or boron.

5. The method as described in claim 1, wherein the second doped SiGe layer contains a dopant in the range of 0.5-2.5 atomic percent.

6. The method as described in claim 5, wherein the dopant is a group III-V element.

7. The method as described in claim 6, wherein the dopant is one or more of carbon or boron.

8. The method as claimed in claim 1, wherein the doped silicon layer comprises a dopant in the range of 0.5-2.5 atomic percent.

9. The method as described in claim 1, wherein each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer is epitaxially grown.

10. The method as claimed in claim 9, wherein each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer is grown independently at a temperature ranging from 500 °C to 800 °C.

11. The method as claimed in claim 1, wherein a stress in the second doped SiGe layer is more tensile than a stress in the first doped SiGe layer, and the stress in the first doped SiGe layer is more tensile than a stress in the doped silicon layer.

12. The method as described in claim 1, wherein when there are 100 film stacks, the wafer bend is less than 150 µm.

13. The method as claimed in claim 1, wherein when a halide-based etchant is used, each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer has an etch selectivity greater than 200:1 relative to the other layers.

14. The method as claimed in claim 1 further comprises the steps of: forming a channel through all of the film stacks to the surface of the substrate by photolithography; and selectively etching one or more of the first doped SiGe layer or the second doped SiGe layer through the channel from all of the film stacks.

15. A method of manufacturing a 3D DRAM device, the method comprising the steps of: forming at least 100 film stacks on a substrate surface, each of the film stacks comprising: a first doped SiGe layer having an experimental formula Si1-xGex, wherein x is in the range of >0 to 0.5; a second doped SiGe layer on the first doped SiGe layer having an experimental formula Si1-yGey, wherein y is in the range of >0 to 0.5, wherein the first doped SiGe layer and the second doped SiGe layer have one or more of different doping amounts or different Si:Ge ratios; a doped silicon layer on the second doped SiGe layer; and forming a channel through the film stacks to the substrate; and selectively removing one or more of the first doped SiGe layer or the second doped SiGe layer through the channel.

16. The method of claim 15, wherein the first doped SiGe layer, the second doped SiGe layer and the doped silicon layer are independently contained in a dopant in the range of 0.5-2.5 atomic percent.

17. The method as described in claim 15, wherein each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer is epitaxially grown.

18. The method as claimed in claim 15, wherein a stress in the second doped SiGe layer is more tensile than a stress in the first doped SiGe layer, and the stress in the first doped SiGe layer is more tensile than a stress in the doped silicon layer.

19. The method as described in claim 1, wherein when there are 100 film stacks, the wafer curvature is less than 150 µm.

20. A method of manufacturing a 3D DRAM device with reduced wafer curvature, the method comprising the steps of: forming at least 100 film stacks on a substrate surface, each of the film stacks comprising: an epitaxially grown first doped SiGe layer having an experimental formula Si1-xGex, wherein x is in the range >0 to 0.5; an epitaxially grown second doped SiGe layer on the first doped SiGe layer, the second doped SiGe layer having an experimental formula Si1-yGey, wherein y is in the range >0 to 0.5, the first doped SiGe layer and the second doped SiGe layer having one or more of different doping amounts or different Si:Ge ratios; and an epitaxially grown doped silicon layer on the second doped SiGe layer, wherein the first doped SiGe layer, the second doped SiGe layer and the doped silicon layer independently contain a dopant selected from carbon or boron in the range of 0.5-2.5 atomic percent. The stress of the second doped SiGe layer is more tensile than that of the first doped SiGe layer, and the stress of the first doped SiGe layer is more tensile than that of the Si layer. Furthermore, when a halide-based etchant is used, each of the first doped SiGe layer, the second doped SiGe layer, and the doped silicon layer has an etch selectivity greater than 200:1 relative to the other layers. A channel is formed by photolithography, the channel passing through all the film stacks to the substrate surface; and one or more of the first doped SiGe layer or the second doped SiGe layer are selectively etched from all the film stacks through the channel.

Citation Information

Patent Citations

  • System comprising a semiconductor device and structure

    TW201937692A

  • Method And Apparatus Providing Improved Thermal Conductivity Of Strain Relaxed Buffer

    US20170125523A1