A method for recycling carbon fiber composite materials based on microwave heat treatment
Patent Information
- Application Number
- TW114104345
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-02-05
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-02-04
AI Technical Summary
The recycling of carbon fiber composites is challenging due to the difficulty in separating carbon fibers from the resin matrix, and existing methods like high-temperature pyrolysis degrade the mechanical properties of carbon fibers, while current curing processes like autoclave molding are energy-inefficient and have poor process control.
A method utilizing microwave heat treatment for recycling carbon fiber composites involves cutting large sheets into smaller pieces, subjecting them to two-stage microwave pyrolysis in controlled atmospheres, mixing with resin, and then microwave curing to form recycled carbon fiber composite boards, optimizing power density, gas composition, and temperature.
This method efficiently recovers high-value carbon fibers with good mechanical properties, reduces energy consumption, and enables uniform heating, producing recycled composites suitable for various applications.
Smart Images

Figure TWG2TB001920443_001 
Figure TWG2TB001920443_002 
Figure TWG2TB001920443_003
Abstract
Description
Technical Field
[0001] This invention relates to a method for recycling carbon fiber composite materials, and more particularly to a method for recycling carbon fiber composite materials using microwave heat treatment. Prior Technology
[0002] Carbon fiber composites possess advantages such as high strength, ultra-light weight, and resistance to high temperatures and pressures, and are widely used in various fields including construction, medical equipment, sports equipment, transportation, aerospace, defense, and energy. Carbon fiber composites are composed of reinforcing carbon fibers and a resin matrix. Carbon fiber is a crucial component of carbon fiber composites, and large quantities of expensive carbon fiber are found in scraps, defective products, and structural components damaged during use. Furthermore, the strength of carbon fiber composites deteriorates due to resin aging, necessitating their disposal as waste. Carbon fiber recycling and reuse are becoming a critical global issue.
[0003] Due to the good interfacial wettability and tight bonding between carbon fibers and the resin matrix, separation is difficult, making the recycling and reuse of carbon fibers challenging. Traditional methods for carbon fiber recycling and regeneration mainly include mechanical crushing, solvent decomposition, and high-temperature pyrolysis. High-temperature pyrolysis is currently the commercially available method for recycling carbon fiber composites. By degrading the carbon fiber composite at high temperatures, clean carbon fibers are obtained, and some organic liquid fuels can also be recovered. However, due to the high temperatures and surface oxidation, the mechanical properties of carbon fibers decrease significantly, which will affect their reuse.
[0004] In addition, recycled carbon fibers need to be remade into carbon fiber composites to generate new value. Currently, the curing and molding methods for carbon fiber composites include: autoclave molding, resin transfer molding, resin film melt infiltration and compression molding. Among them, the autoclave process is mature and is currently the most widely used process. However, the autoclave process also has certain limitations
[11] : 1. poor process control; 2. long curing time; 3. high energy consumption. Therefore, developing a more energy-efficient curing process is beneficial to reducing the production cost of recycled carbon fiber composites and expanding the application range of recycled carbon fiber composites.
[0005] Microwaves are electromagnetic waves with frequencies ranging from 0.3 to 300 GHz, commonly using frequencies of 2.45 GHz and 0.915 GHz. They possess extremely strong penetrating power, directly dissipating energy within materials. Molecular dipoles rotate at high speeds of hundreds of millions of times per second, performing in-situ energy conversion. This changes the conventional heating process, which requires heat transfer through a temperature gradient, convection through the medium, heat conduction through the container walls, and heat conduction within the sample. Microwave heating has three main characteristics: Instantaneous: High thermal efficiency and short heating time. Selectivity: Different materials exhibit significantly different heating characteristics in a microwave field due to their varying dielectric properties. Penetration: Electromagnetic waves can penetrate the interior of a medium, thus microwaves possess strong penetrating power. Numerous studies have demonstrated that microwave-heated pyrolysis of waste can produce high-quality recyclable materials, achieving the concept of a regenerative circular economy. Domestic and international researchers have also applied microwave heating technology to the curing process of carbon fiber composites, conducting extensive research. Current experiments have proven that carbon fiber is an excellent microwave absorbing material, exhibiting very good heating effects in a microwave field. Compared with traditional heating, microwave heating has a shorter heating time and does not directly contact the heating material, thus improving the problems of high energy consumption and low efficiency of traditional heating.
[0006] In laboratory-scale studies, carbon fibers can be recycled from waste carbon fiber composites using microwave processes through various techniques, and can also be regenerated into carbon fiber composites. However, these laboratory-scale methods are often complex and unsuitable for industrial-scale production.
[0007] In view of this, it is necessary to propose a rapid and environmentally friendly industrial-scale method for the reuse of carbon fiber composites based on microwave heat treatment. Summary of the Invention
[0008] To address the aforementioned problems, the main objective of this invention is to provide a method for reusing carbon fiber composite materials based on microwave heat treatment, specifically addressing the issues and shortcomings of the existing technology. This method uniformly and efficiently recovers high-value carbon fibers from waste carbon fiber composite materials at relatively low temperatures and ambient pressure, and reuses them as carbon fiber composite materials.
[0009] To achieve the objectives of this invention, a method for reusing carbon fiber composite materials based on microwave heat treatment is provided, the main steps of which include: Step (1): Cut a large sheet of carbon fiber composite material into multiple carbon fiber composite material sheets; Step (2): The carbon fiber composite sheets are subjected to microwave pyrolysis to form a plurality of recycled carbon fiber materials; Step (3): The recycled carbon fiber materials are mixed with a resin to form a prepreg carbon fiber composite material; and Step (4): The preimpregnated carbon fiber composite material is subjected to microwave curing to form a recycled carbon fiber composite board.
[0010] According to one feature of the present invention, step (2) further comprises the following steps: Step (2-1): The carbon fiber composite sheets are subjected to a first microwave pyrolysis treatment in an oxygen-free atmosphere containing inert gas to form a plurality of semi-finished carbon fiber materials. The temperature of the first microwave pyrolysis treatment is between 450 and 600°C, and the time is between 0.2 and 0.8 hours; and Step (2-2): The semi-finished carbon fiber materials are subjected to a second microwave pyrolysis treatment in a low-oxygen atmosphere containing mixed air to form a plurality of recycled carbon fiber materials. The temperature of the second microwave pyrolysis treatment is between 450 and 600°C, and the time is between 0.1 and 0.7 hours.
[0011] According to one feature of the present invention, the microwave power density of the first microwave pyrolysis treatment is between 5 kW / kg and 10 kW / kg, where kg is the unit weight of the carbon fiber composite sheets.
[0012] According to one feature of the present invention, the inert gas system introduced into the first microwave pyrolysis process is nitrogen, and its flow rate is between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute [L / min] and kg is the unit weight of the carbon fiber composite sheets.
[0013] According to one feature of the present invention, the microwave power density of the second microwave pyrolysis treatment is between 3 kW / kg and 8 kW / kg, where kg is the unit weight of the carbon fiber composite sheets.
[0014] According to one feature of the invention, the mixed gas system introduced into the second microwave pyrolysis process contains at least one compressed air with a flow rate between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute [L / min] and kg is the unit weight of the carbon fiber composite sheets.
[0015] According to one feature of the present invention, step (3) further comprises the following step: first crushing the recycled carbon fiber materials to form a plurality of recycled carbon fiber particles.
[0016] According to one feature of the present invention, in step (3), the weight ratio of the recycled carbon fiber material to the resin is between 1:0.5 and 1:2.
[0017] According to one feature of the present invention, step (3) further comprises the following steps:
[0018] The prepreg carbon fiber composite material is placed in a mold to form the prepreg carbon fiber composite material with a specific shape.
[0019] According to one feature of the present invention, in step (4), the temperature of the microwave curing treatment is between 120 and 240°C, and the time is between 0.1 and 3 hours.
[0020] The advantages of the present invention's method for reusing carbon fiber composite materials based on microwave heat treatment are: (1) By utilizing the selective heating characteristics of microwaves on carbon fiber composite waste, the interior of the carbon fiber resin matrix composite material is rapidly heated and the whole is heated uniformly, which shortens the processing time and improves the recycling efficiency and effect of carbon fiber; (2) Inert gas or oxygen-containing mixed gas is introduced at different times under normal pressure and a certain temperature is controlled to degrade the resin and then react with oxidation. The carbon fiber does not react, thereby removing the organic matter of the resin and obtaining carbon fiber with good performance, which has a smooth surface and basically no residual resin. (3) The heat released by the oxidation reaction is used for heat preservation, which reduces the energy consumption of microwave power and saves energy significantly. (4) The recycled carbon fiber composite material obtained by microwave curing has excellent mechanical properties and can be combined with various resin matrices to form different carbon fiber reinforced composite materials, which can be applied to different fields. It is a green and environmentally friendly recycling method. Simple Explanation of the Diagram
[0021] To make the above and other objects, features and advantages of the present invention more apparent and understandable, several preferred embodiments are described below in detail with reference to the accompanying drawings. Figure 1 shows a flowchart of a method for reusing carbon fiber composite materials based on microwave heat treatment according to the present invention; Figure 2 shows a flowchart of step (2) of a method for reusing carbon fiber composite materials based on microwave heat treatment according to the present invention. Implementation
[0022] While the present invention may be embodied in various forms, those shown in the accompanying drawings and described herein are preferred embodiments of the invention. Those skilled in the art will understand that the apparatus and methods specifically described herein and illustrated in the drawings are intended as examples of the invention, not limiting illustrative embodiments, and the scope of the invention is defined only by the claims. Features illustrated or described in connection with an illustrative embodiment may be combined with features of other embodiments. Such modifications and variations are included within the scope of the invention.
[0023] Thermal pyrolysis is a thermochemical process that decomposes organic matter into solid substances, condensed liquids, and combustible gases under high temperature, oxygen-free or low-oxygen conditions. To achieve the objectives of this invention, a method for reusing carbon fiber composite materials based on microwave heat treatment is provided.
[0024] Please now refer to Figure 1, which shows a flowchart of a method for reusing carbon fiber composite materials based on microwave heat treatment according to the present invention. The main steps of this method for reusing carbon fiber composite materials based on microwave heat treatment include: Step (1): Cut a large sheet of carbon fiber composite material into multiple carbon fiber composite material sheets; Step (2): The carbon fiber composite sheets are subjected to microwave pyrolysis to form a plurality of recycled carbon fiber materials; Step (3): The recycled carbon fiber materials are mixed with a resin to form a prepreg carbon fiber composite material; and Step (4): The preimpregnated carbon fiber composite material is subjected to microwave curing to form a recycled carbon fiber composite board.
[0025] The carbon fiber in this carbon fiber composite material is one or more of polyacrylonitrile-based carbon fiber, pitch-based carbon fiber, viscose-based carbon fiber, or other carbon fibers. The matrix resin in this carbon fiber composite material is one or more of thermosetting resins or thermoplastic resins. The thermosetting resin includes epoxy resin, unsaturated polyester resin, phenolic resin, urea-formaldehyde resin, vinyl resin, melamine-formaldehyde resin, bismaleimide resin, polyimide resin, polyurethane resin, silicone resin, furan resin, and other thermosetting resins. The thermoplastic resins include polyphenylene sulfide, polyphenylene ether, polytetrafluoroethylene, polyamide, polyetheretherketone, polycarbonate, polyester, nylon, PC / ABS (polycarbonate / acrylonitrile-butadiene-styrene) alloy, polyimide, polyoxymethylene, polypropylene, thermoplastic polyimide, polyethylene, polyarylate, liquid crystal polymer, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polystyrene, and other thermoplastic resins such as acrylonitrile-butadiene-styrene copolymer.
[0026] In step (1), the large carbon fiber composite material sheet can be a plate structure or an irregularly shaped part. Since carbon fiber composite material is not a homogeneous material, different shapes and structures will affect heat transfer and thus affect the thermal decomposition effect. Therefore, larger carbon fiber composite materials need to be crushed. The crushing method is mechanical processing. The dimensions of these carbon fiber composite material sheets are approximately 2-40 cm in length and 2-20 cm in width.
[0027] Please now refer to Figure 2, which shows a flowchart of step (2) of a method for reusing carbon fiber composite materials based on microwave heat treatment according to the present invention. Step (2) further includes the following steps: Step (2-1): The carbon fiber composite sheets are subjected to a first microwave pyrolysis treatment in an oxygen-free atmosphere containing inert gas to form a plurality of semi-finished carbon fiber materials. The temperature of the first microwave pyrolysis treatment is between 450 and 600°C, and the time is between 0.2 and 0.8 hours; and Step (2-2): The semi-finished carbon fiber materials are subjected to a second microwave pyrolysis treatment in a low-oxygen atmosphere containing mixed air to form a plurality of recycled carbon fiber materials. The temperature of the second microwave pyrolysis treatment is between 450 and 600°C, and the time is between 0.1 and 0.7 hours.
[0028] In step (2), the required microwave power is related to the capacity of the heating cavity and the weight of the carbon fiber composite material being processed. The power of these microwave power sources is adjustable, providing an appropriate power density based on the weight of the heated carbon fiber composite material. Microwaves are electromagnetic waves, using a microwave power at a frequency of either 915MHz or 2450MHz. Microwave heating utilizes the principle of radiation, penetrating the surface of the medium and entering the interior of the carbon fiber composite sheet. The carbon fiber composite sheet absorbs the microwave energy and converts it into heat to achieve the purpose of heating and decomposition.
[0029] In step (2-1), the microwave power density of the first microwave pyrolysis treatment is between 5 kW / kg and 10 kW / kg, where kg is the unit weight of the carbon fiber composite sheets. The inert gas system introduced into the first microwave pyrolysis treatment is nitrogen, and its flow rate is between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute [L / min], and kg is the unit weight of the carbon fiber composite sheets.
[0030] In step (2-1), the oxygen-free condition refers to the absence of oxygen during the microwave heat treatment process. This is achieved by continuously introducing an inert gas, such as nitrogen or argon, to deplete the oxygen within the microwave heating cavity, ensuring no subsequent oxygen replenishment and thus limiting the gas intake design. The inert gas flow rate is directly proportional to the capacity of the heating cavity.
[0031] The first microwave pyrolysis process decomposes the carbon fiber composite sheets into a gaseous substance and the semi-finished carbon fiber material. The gaseous substance is extracted from the microwave heating chamber by an external vacuum device and, after subsequent condensation, separates into a liquid product, namely biogas, and a gaseous product, namely syngas (mainly hydrogen, methane, and carbon monoxide). Both the liquid and gaseous products can be used as energy fuels.
[0032] In step (2-2), the microwave power density of the second microwave pyrolysis treatment is between 3 kW / kg and 8 kW / kg, where kg is the unit weight of the carbon fiber composite sheets. The mixed gas system introduced into the second microwave pyrolysis treatment contains at least one compressed air with a flow rate between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute (L / min) and kg is the unit weight of the carbon fiber composite sheets.
[0033] In step (2-2), the low-oxygen condition refers to the situation where the amount of oxygen in the heating cavity is less than that in ordinary air during microwave heat treatment. This low-oxygen atmosphere can be achieved through a restricted air intake design, meaning that the heating cavity only evacuates air during the reaction process, without any intake. Alternatively, the low-oxygen atmosphere can be achieved by continuously introducing a mixed gas system containing at least compressed air, and then using an external evacuation device to extract the introduced mixed gas from the microwave heating cavity at a gas velocity equal to or greater than the introduced mixed gas. The flow rate of the introduced mixed gas is proportional to the capacity of the heating cavity.
[0034] These recycled carbon fiber materials are cooled to below 400°C in a microwave heating chamber under a low-oxygen atmosphere mixed with air, and then fed into a conveyor belt for removal. Once cooled to below 400°C, the recycled carbon fiber materials are fed from below the microwave heating chamber, preventing oxidation and combustion, and accelerating the cooling to room temperature. The carbon fiber materials are then removed from the microwave heating chamber, washed with clean water to remove impurities, and dried to obtain high-quality carbon fiber materials.
[0035] This two-stage microwave pyrolysis process, which includes control methods for different microwave power densities, different heating temperatures, different heating times, different gas compositions and flow rates, and different extraction conditions, effectively yields high-quality recycled carbon fibers.
[0036] Step (3) further includes the following steps: first, crushing the recycled carbon fiber materials to form a plurality of recycled carbon fiber particles.
[0037] In step (3), the weight ratio of the recycled carbon fiber material to the resin is between 1:0.5 and 1:2.
[0038] In step (3), the resin used to pre-impregnate the carbon fiber composite material is one or more of thermosetting resins or thermoplastic resins. The thermosetting resins include epoxy resins, unsaturated polyester resins, phenolic resins, urea-formaldehyde resins, vinyl resins, melamine-formaldehyde resins, bismaleimide resins, polyimide resins, polyurethane resins, silicone resins, furan resins, and other thermosetting resins. The thermoplastic resins include polyphenylene sulfide, polyphenylene ether, polytetrafluoroethylene, polyamide, polyetheretherketone, polycarbonate, polyester, nylon, PC / ABS (polycarbonate / acrylonitrile-butadiene-styrene) alloy, polyamide, polyoxymethylene, polypropylene, thermoplastic polyimide, polyethylene, polyarylate, liquid crystal polymers, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polystyrene, and other thermoplastic resins such as acrylonitrile-butadiene-styrene copolymers.
[0039] Step (3) further includes the following steps: the prepreg carbon fiber composite material is placed in a mold to form the prepreg carbon fiber composite material having a specific shape.
[0040] In step (4), the temperature of the microwave curing treatment is between 120 and 240°C, and the time is between 0.1 and 3 hours. In one embodiment, the heating process of the microwave curing treatment is as follows: first, the temperature is raised to 130°C and held for 30 minutes, then the temperature is raised to 200°C and held for 1.5 hours, with a heating rate of 1.5°C / min and a cooling rate of 1.3°C / min.
[0041] The advantages of the present invention's method for reusing carbon fiber composite materials based on microwave heat treatment are: (1) By utilizing the selective heating characteristics of microwaves on carbon fiber composite waste, the interior of the carbon fiber resin matrix composite material is rapidly heated and the whole is heated uniformly, which shortens the processing time and improves the recycling efficiency and effect of carbon fiber; (2) Inert gas or oxygen-containing mixed gas is introduced at different times under normal pressure and a certain temperature is controlled to degrade the resin and then react with oxidation. The carbon fiber does not react, thereby removing the organic matter of the resin and obtaining carbon fiber with good performance, which has a smooth surface and basically no residual resin. (3) The heat released by the oxidation reaction is used for heat preservation, which reduces the energy consumption of microwave power and saves energy significantly. (4) The recycled carbon fiber composite material obtained by microwave curing has excellent mechanical properties and can be combined with various resin matrices to form different carbon fiber reinforced composite materials, which can be applied to different fields. It is a green and environmentally friendly recycling method.
[0042] Although the present invention has been disclosed with reference to the foregoing preferred embodiments, it is not intended to limit the invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention. As explained above, various modifications and variations can be made without destroying the spirit of the invention. Therefore, the scope of protection of this invention shall be determined by the claims outlined in the appended patent claims.
Claims
1. A method for reusing carbon fiber composite materials based on microwave heat treatment, comprising the following main steps: Step (1): cutting a large sheet of carbon fiber composite material into a plurality of carbon fiber composite material sheets; Step (2): subjecting the carbon fiber composite material sheets to a microwave pyrolysis treatment to form a plurality of recycled carbon fiber materials; Step (3): first crushing the recycled carbon fiber materials to form a plurality of recycled carbon fiber granules, and then mixing them with a resin to form a preimpregnated carbon fiber composite material; and Step (4): subjecting the preimpregnated carbon fiber composite material to a microwave curing treatment to form a recycled carbon fiber composite. Material sheet; wherein step (2) further includes the following steps: Step (2-1): The carbon fiber composite sheet is subjected to a first microwave pyrolysis treatment in an oxygen-free atmosphere containing inert gas to form a plurality of semi-finished carbon fiber materials. The temperature of the first microwave pyrolysis treatment is between 450 and 600°C, the time is between 0.2 and 0.8 hours, the microwave power density is between 5 kW / kg and 10 kW / kg, the inert gas system is nitrogen, and its flow rate is between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute [L / min], and kg is the number of carbon fiber composite sheets. The unit weight of the composite material sheet, and the oxygen-free atmosphere refers to the absence of oxygen in a heating chamber of the first microwave pyrolysis treatment, which is achieved by continuously introducing inert gas to consume all the oxygen in the heating chamber, and without subsequent oxygen replenishment to achieve the oxygen-free atmosphere; and step (2-2): the semi-finished carbon fiber materials are subjected to a second microwave pyrolysis treatment in a low-oxygen atmosphere containing mixed air to form a plurality of recycled carbon fiber materials, the temperature of the second microwave pyrolysis treatment is between 450~600℃, the time is 0.1~0.7 hours, and the microwave power density is between 3kw / kg and 8kw / kg. During the process, the introduced mixed gas system contains at least one compressed air with a flow rate between 10 LPM / kg and 20 LPM / kg, where LPM is liters per minute [L / min], kg is the unit weight of the carbon fiber composite sheets, and the low-oxygen atmosphere refers to the fact that the amount of oxygen in the heating chamber of the second microwave pyrolysis process is less than the amount of oxygen in ordinary air. This low-oxygen atmosphere is achieved by continuously introducing a mixed gas containing at least one compressed air into the heating chamber and extracting the introduced mixed gas from the heating chamber at a gas velocity equal to or greater than that of the introduced mixed gas.
2. A method for reusing carbon fiber composite materials based on microwave heat treatment as described in claim 1, wherein the carbon fiber in the carbon fiber composite material is one or more of other carbon fibers such as polyacrylonitrile-based carbon fiber, pitch-based carbon fiber, or viscose-based carbon fiber.
3. The method for reusing carbon fiber composite materials based on microwave heat treatment as described in claim 1, wherein in step (3), the weight ratio of the recycled carbon fiber materials to the resin is between 1:0.5 and 1:
2.
4. The method for reusing carbon fiber composite material based on microwave heat treatment as described in claim 1, wherein step (3) further comprises the following step: placing the prepreg carbon fiber composite material into a mold to form the prepreg carbon fiber composite material having a specific shape.
5. The method for reusing carbon fiber composite materials based on microwave heat treatment as described in claim 1, wherein in step (4), the temperature of the microwave curing treatment is between 120 and 240°C, and the time is between 0.1 and 3 hours.
Citation Information
Patent Citations
High efficiency carbon fiber recovery method
CN108610507A
Vibration-microwave composite curing forming system and method for composite material component
CN118876467A
Method for manufacturing recycled carbon fiber bundle,recycled carbon fiber, recycled carbon fiber milled, apparatus for producing recycled carbon fiber bundle, method for producing carbon fiber reinforced resin and carbon fiber reinforced resin particle, and recycled carbon fiber bundle
TW201900747A
Methods for preparing composite materials using recycled carbon fibers
TWI719595B